Laminate, battery, and battery pack

The laminate with inorganic material particles and polymers in the secondary battery separator addresses the limitations of resin film separators by reducing self-discharge and enhancing durability, achieving improved battery performance through controlled particle aggregation and insulation.

WO2024241487A1PCT designated stage expired Publication Date: 2024-11-28KK TOSHIBA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/019140
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional secondary battery separators made of resin films are limited in thickness due to mechanical strength requirements, leading to reduced battery capacity and poor durability, causing decreased cycleability and self-discharge over repeated charging and discharging.

Method used

A laminate is developed with a first film containing inorganic material particles and a polymer, where the median diameter is 0.6 μm or less and the average pore diameter is 0.5 μm or less, satisfying the formula Ra02 / Ra01 ≤ 1.5, which suppresses aggregation of inorganic material particles and maintains insulation properties even at reduced thickness.

Benefits of technology

The laminate effectively reduces self-discharge and enhances durability by preventing the mixing of conductive agents into the film, maintaining insulation and improving cycle life performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023019140_28112024_PF_FP_ABST
    Figure JP2023019140_28112024_PF_FP_ABST
Patent Text Reader

Abstract

According to an embodiment of the present invention, a laminate comprising a first current collector, a first active material-containing layer, and a first film is provided. The first film contains a polymer and inorganic material particles having a median diameter D50 of 0.6 μm or less. The average void diameter of the first film is 0.5 μm or less. The first film satisfies formula (1) below. Ra01 is the distance between Hansen solubility parameter values (HSP values) of the inorganic material particles and n-methyl-2-pyrrolidone. Ra02 is the distance between the Hansen solubility parameter values (HSP values) of the inorganic material particles and the polymer. (1): 0 < Ra02 / Ra01 ≤ 1.5
Need to check novelty before this filing date? Find Prior Art

Description

Laminate, battery, and battery pack

[0001] The embodiments relate to a laminate, a battery, and a battery pack.

[0002] In secondary batteries such as lithium secondary batteries, a porous separator is disposed between the positive electrode and the negative electrode to prevent contact between the two electrodes. The separator is a free-standing membrane separate from the positive electrode and the negative electrode. An example of such a membrane is a microporous membrane made of a polyolefin resin. Such a separator is produced, for example, by extruding a melt containing a polyolefin resin composition into a sheet, extracting and removing substances other than the polyolefin resin, and then stretching the sheet.

[0003] Resin film separators must have sufficient mechanical strength to prevent breakage during battery fabrication, making them difficult to thin beyond a certain level. Because the positive and negative electrodes are stacked or wound with the separator between them, a thick separator limits the number of positive and negative electrode layers that can be accommodated per unit volume of the battery. This results in reduced battery capacity. Furthermore, resin film separators have poor durability, and when used in secondary batteries, the separator deteriorates with repeated charging and discharging, reducing the battery's cycleability.

[0004] In order to reduce the thickness of the separator, it has been considered to integrate a nanofiber membrane or an inorganic material membrane with either the positive electrode or the negative electrode.

[0005] Japanese Patent Application Laid-Open No. 2019-153431

[0006] The present invention provides a laminate including a first film with improved insulating properties, and a battery and a battery pack including the laminate.

[0007] According to an embodiment, a laminate is provided, comprising a first current collector, a first active material-containing layer laminated on at least one surface of the first current collector, and a first film covering at least a portion of the surface of the first active material-containing layer not laminated with the first current collector. The first film contains inorganic material particles and a polymer having a median diameter D50 of 0.6 μm or less. The first film has an average pore size of 0.5 μm or less. The first film satisfies the following formula (1):

[0008] 0<Ra 02 / Ra 01 ≦1.5 (1) However, Ra 01 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and n-methyl-2-pyrrolidone, and Ra 02 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and the polymer.

[0009] Furthermore, according to the embodiment, a battery including the laminate of the embodiment and a battery pack including the laminate of the embodiment are provided.

[0010] FIG. 1 is a cross-sectional view showing an example of a laminate according to an embodiment. FIG. 2 is a perspective view showing a first electrode of the laminate shown in FIG. 1. FIG. 3 is a perspective view showing a second electrode of the laminate shown in FIG. 1. FIG. 4 is a perspective view showing another example of a first electrode. FIG. 5 is a cross-sectional view showing another example of a laminate according to an embodiment. FIG. 6 is a perspective view showing a first electrode of the laminate shown in FIG. 5. FIG. 7 is a perspective view showing another example of a first electrode. FIG. 8 is a cross-sectional view showing yet another example of a laminate according to an embodiment. FIG. 9 is a schematic diagram of one step in a method for producing a laminate according to an embodiment. FIG. 10 is a plan view showing the coating device shown in FIG. 10. FIG. 11 is a schematic diagram of one step in a method for producing a laminate according to an embodiment. FIG. 12 is a partially cutaway perspective view showing an example of a battery according to an embodiment. FIG. 13 is an exploded view of another example of a battery according to an embodiment. FIG. 14 is an exploded perspective view showing an example of a battery pack according to an embodiment. FIG. 15 is a block diagram showing an example of an electrical circuit of the battery pack shown in FIG. 14. Fig. 16 is a schematic diagram showing an example of the relationship between inorganic material particles and polymer Hansen dissolving balls. Fig. 17 is a schematic diagram showing a scanning electron microscope (SEM) image of a cross section of the first film of the laminate of Comparative Example 2 cut along the thickness direction. Embodiment

[0011] Coating the surface of an active material-containing layer of an electrode with an insulating film containing inorganic material particles has been studied. The insulating film containing inorganic material particles is formed, for example, by applying a slurry containing inorganic material particles to the surface of the active material-containing layer and drying it. To increase the density of the film, it is desirable to reduce the particle size of the inorganic material particles. However, it has been found that if the median diameter of the inorganic material particles is reduced to, for example, 0.6 μm or less, the inorganic material particles tend to aggregate, resulting in the generation of many coarse particles with particle diameters of several tens of μm or more, making it impossible to ensure the insulating properties of the film.

[0012] As a result of extensive research, the inventors have found that, among the distances between the Hansen solubility parameters (HSP values) of inorganic material particles, polymers, and solvents (e.g., n-methyl-2-pyrrolidone) contained in a slurry for forming a film, the distance Ra between the HSP values ​​of the inorganic material particles and n-methyl-2-pyrrolidone is 01 The distance Ra between the HSP values ​​of the inorganic material particles and the polymer 02 The ratio (Ra 02 / Ra 01 ) satisfies the following formula (1), the aggregation of inorganic material particles can be suppressed, coarse particles can be sufficiently reduced, and a dense film can be obtained.

[0013] 0<Ra 02 / Ra 01 ≦1.5 (1) The Hansen solubility parameter (HSP) is an index that represents the affinity between two substances (or two components, two materials) and is used to evaluate the dispersibility between the two substances. The distance between the HSP values ​​(Ra) is the distance between the Hansen solubility parameter value (HSP value) of one substance and the Hansen solubility parameter value (HSP value) of the other substance. The larger the distance between the HSP values ​​(Ra), the smaller the affinity between the two substances tends to be. The affinity between polymers and inorganic material particles is determined by a combination of complex factors such as the type of inorganic material particle, the surface condition of the inorganic material particle, the type of polymer, the molecular weight, the functional groups of the polymer, and even the type of dispersion solvent.

[0014] By satisfying the above formula (1), the polymer adsorbs onto the surface of the inorganic material particles, allowing a repulsive force to act between the inorganic material particles. This allows the interaction between the inorganic material particles to become a repulsive force, thereby suppressing aggregation of the inorganic material particles. As a result, the number of coarse particles can be sufficiently reduced. Furthermore, by setting the average pore size of the film containing inorganic material particles to 0.5 μm or less, it is possible to suppress the conductive additive in the active material-containing layer from being mixed into the film, thereby preventing a decrease in the insulating properties of the film.

[0015] (Ra 02 / Ra 01 ) is greater than 1.5, the distance Ra between the HSP values ​​of the inorganic material particles and the polymer 02 Ra 01 Therefore, the affinity between the polymer and the inorganic material particles is small, and the polymer is not adsorbed to the inorganic material particle surface sufficiently, which causes the inorganic material particles to aggregate and result in an increase in coarse particles.

[0016] Therefore, by using a film (hereinafter referred to as the "first film") containing inorganic material particles and polymers with a median diameter D50 of 0.6 μm or less, an average void diameter of 0.5 μm or less, and satisfying formula (1) as the insulating film of an active material-containing layer (hereinafter referred to as the "first active material-containing layer"), it is possible to suppress self-discharge of a battery. Because the first film is highly dense, it can maintain its insulating properties even when its film thickness is thin. Furthermore, it can prevent components such as conductive agents contained in the first active material-containing layer from being mixed into the first film. Therefore, it is possible to maintain the insulating properties between the first electrode and the second electrode with a film thinner than a free-standing film such as a porous resin film.

[0017] The method for measuring the Hansen solubility parameter (HSP) is as follows: Inorganic material particles are added to 10 to 20 types of dispersion media at a concentration of 5% by mass. Furthermore, binder polymer powder is added to each of 10 to 20 types of dispersion media at a concentration of 5% by mass. For each sample obtained in this way, pulsed nuclear magnetic resonance (NMR) measurements are used to determine the relaxation time, which is used to determine whether the inorganic material particles or binder polymer are good or poor solvents for the 10 to 20 types of dispersion media. From these results, the Hansen solubility spheres for the inorganic material particles and binder polymer are calculated. The difference in the center coordinates between these is calculated, and this is taken as the HSP value distance (Ra).

[0018] When the laminate further includes a second active material-containing layer and a second film, and the second active material-containing layer is integrated with the second film, the self-discharge suppression effect can be further enhanced.

[0019] The second film may be integrated with the first film, thereby improving the adhesive strength between the first film and the second film.

[0020] The laminate of the embodiment may further include a first current collector and a first current collecting tab. In this case, a first active material-containing layer is supported on a portion of the first current collector. Furthermore, the first current collector includes the first current collecting tab in another portion not supporting the first active material-containing layer. By covering the portion of the first current collecting tab that includes the boundary with the first active material-containing layer with the first film, it is possible to prevent the first current collecting tab from coming into contact with the counter electrode and causing an internal short circuit. (First Embodiment) The laminate of the first embodiment will be described below.

[0021] The laminate of the first embodiment includes a first electrode and may optionally include a second electrode. The second electrode is the opposite electrode of the first electrode. The first electrode may be a positive electrode and the second electrode may be a negative electrode, or the first electrode may be a negative electrode and the second electrode may be a positive electrode. The first electrode includes a first film and a first active material-containing layer. The first electrode may further include a first current collector and a first current collecting tab. The second electrode includes a second film and a second active material-containing layer. The second electrode may further include a second current collector and a second current collecting tab. The first and second active material-containing layers may be formed on both main surfaces of the first and second current collectors, respectively, or may be formed on only one surface. The first and second electrodes will be described in detail. <First Electrode> <First Film> The first film contains inorganic material particles and polymers having a median diameter D50 of 0.6 μm or less, an average pore diameter of 0.5 μm or less, and satisfies the following formula (1).

[0022] 0<Ra 02 / Ra 01 ≦1.5 (1) However, Ra 01 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and n-methyl-2-pyrrolidone. 02 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and the polymer.

[0023] The first film covers a part or the whole of the surface of the first active material-containing layer that is not covered with the first current collector, and may be fixed to the first active material-containing layer by, for example, adhesion, heat fusion, or the like.

[0024] Examples of inorganic materials include oxides (e.g., Li2O, BeO, BO, Na2O, MgO, Al2O3, SiO2, PO5, CaO, Cr2O3, Fe2O3, ZnO, ZrO2, TiO2, magnesium oxide, silicon oxide, alumina, zirconia, titanium oxide, and other oxides of IIA to VA groups, transition metals, IIIB, and IVB), zeolites (M 2 / n O.Al2O3.xSiO2.yH2O (wherein M is a metal atom such as Na, K, Ca, or Ba, and n is a metal cation M n+where x and y are numbers corresponding to the charge of SiO and HO, and 2≦x≦10, 2≦y), nitrides (e.g., BN, AlN, SiN, and BaN), silicon carbide (SiC), zircon (ZrSiO), carbonates (e.g., MgCO and CaCO), sulfates (e.g., CaSO and BaSO), and composites thereof (e.g., steatite (MgO.SiO), forsterite (2MgO.SiO), and cordierite (2MgO.2AlO.5SiO), which are types of porcelain), tungsten oxide, and mixtures thereof can be mentioned.

[0025] Examples of other inorganic materials include barium titanate, calcium titanate, lead titanate, γ-LiAlO2, LiTiO3, and mullite (3Al 2 O 3 2SiO2), solid electrolytes or mixtures thereof.

[0026] Examples of solid electrolytes include solid electrolytes with no or low lithium ion conductivity and solid electrolytes with lithium ion conductivity. Examples of oxide particles with no or low lithium ion conductivity include lithium aluminum oxide (e.g., LiAlO, Li x Al2O3, where 0<x≦1), lithium silicon oxide, and lithium zirconium oxide.

[0027] Examples of solid electrolytes with lithium ion conductivity include oxide solid electrolytes with a garnet structure. Oxide solid electrolytes with a garnet structure have the advantages of high reduction resistance and a wide electrochemical window. Examples of oxide solid electrolytes with a garnet structure include La 5+x A x La 3-x M2O 12 (A is at least one element selected from the group consisting of Ca, Sr and Ba, M is Nb and / or Ta, and x is preferably in the range of 0.5 or less (including 0)), Li3M 2-x L2O 12 (M is Nb and / or Ta, L is Zr, and x is preferably in the range of 0.5 or less (including 0)), Li 7-3x Al x La3Zr3O12 (x is preferably in the range of 0.5 or less (including 0)), Li7La3Zr2O 12 Among them, Li 6.25 Al 0.25 La3Zr3O 12 , Li 6.4 La3Zr 1.4 Ta 0.6 O 12 , Li 6.4 La3Zr 1.6 Ta 0.6 O 12 , Li7La3Zr2O 12 has high ionic conductivity and is electrochemically stable, and therefore has excellent discharge performance and cycle life performance.

[0028] An example of a solid electrolyte having lithium ion conductivity includes a lithium phosphate solid electrolyte having a NASICON structure. An example of a lithium phosphate solid electrolyte having a NASICON structure includes LiM12(PO4)3, where M1 is one or more elements selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Al. A preferred example is Li 1+x Al x Ge 2-x (PO4)3, Li 1+x Al x Zr 2-x (PO4) 3 , Li 1+x Al x Ti 2-x (PO4)3. Here, in each case, x is preferably in the range of 0 or more and 0.5 or less. Furthermore, each of the exemplified solid electrolytes has high ionic conductivity and high electrochemical stability. Both a lithium phosphate solid electrolyte having a NASICON structure and an oxide solid electrolyte having a garnet structure may be used as the solid electrolyte having lithium ion conductivity.

[0029] Among the types of inorganic material particles described above, particles containing at least one compound selected from the group consisting of titanium oxide, aluminum oxide, and barium sulfate are desirable. By specifying the distance between HSP values ​​as shown in formula (1), aggregation of these inorganic material particles can be suppressed. It is preferable that at least a portion of the titanium oxide particle surface is coated with aluminum oxide. Titanium oxide particles such as titanium dioxide (TiO2) can be adsorbed to polymers through acid-base interactions. By coating at least a portion of the surface of titanium dioxide particles with aluminum oxide particles such as Al2O3, the acid-base properties of the titanium dioxide particle surface can be changed, thereby changing the affinity between the inorganic material particles and polymers, i.e., the distance between HSP values ​​Ra 02 The affinity between the inorganic material particles and the polymer can also be changed by the average molecular weight of the polymer, the units constituting the polymer (homopolymer, copolymer), etc. Examples of titanium oxides are not limited to titanium dioxide. Examples of titanium oxides include lithium titanium oxides (e.g., lithium titanium oxides having a spinel structure or a ramsdellite structure).

[0030] The first film containing particles of at least one inorganic material selected from the above is a porous film composed of an aggregate of inorganic material particles. While there are inorganic materials with lithium ion conductivity, such as solid electrolytes, many inorganic materials have low electronic conductivity or are insulating. Therefore, the first film can function as a partition wall separating the positive electrode and the negative electrode. Furthermore, to suppress the self-discharge rate of a battery including a laminate manufactured by the method described below, it is effective to sufficiently reduce the amount of coarse particles with a particle size of tens of micrometers or more that are formed by aggregation of inorganic material particles in a slurry containing the inorganic material.

[0031] The first membrane can retain the non-aqueous electrolyte in the porous portion, and therefore does not inhibit the permeation of Li ions.

[0032] The shape of the inorganic material particles is not particularly limited, but may be, for example, granular, fibrous, etc. The inorganic material particles are preferably present in the form of primary particles, but may also be present in the form of secondary particles formed by aggregation of primary particles. Both primary and secondary particles of the inorganic material particles may also be present.

[0033] The specific surface area of ​​inorganic material particles is 30 m 2 The lower limit of the specific surface area is 2 m / g or less. 2 / g.

[0034] By setting the median diameter D50 of the inorganic material particles to 0.6 μm or less, the size of the voids can be reduced. The median diameter D50 of the inorganic material particles can be determined as follows: The battery is disassembled to remove the electrode containing the first film. The cross-section of the electrode is processed by ion milling. The cross-section of the cut-out electrode containing the first film is photographed using a scanning electron microscope (SEM) to obtain a cross-sectional SEM image. The obtained image is processed to determine the median diameter D50. Specifically, a line is drawn at any point within the region corresponding to the first film in the cross-sectional SEM image, and the length of overlap between the line and the inorganic material particles is measured. Measurements are taken at any five points, and the median of these lengths is used as the median diameter D50 of the inorganic material particles. By setting the average void diameter of the first film to 0.5 μm or less, it is possible to prevent the conductive additive in the first active material-containing layer from penetrating the first film and reducing the insulating properties of the first film in the manufacturing method described below. A more preferred range for the average void diameter is 0.4 μm or less. The lower limit of the average void diameter can be set to 0.001 μm. The average void diameter can be determined as follows. A scanning electron microscope (SEM) image of the cross section of the electrode including the first film is obtained in the same manner as when measuring the median diameter D50 of the inorganic material particles. A binarization process is performed on the region of the SEM image corresponding to the first film, for example, to make the inorganic material particles white and the voids black. This image is analyzed to obtain the number of voids and the porosity. The porosity A1 (%) is calculated using the following formula (2): A1 (%) = A2 / A3 (2) In formula (2), A2 is the sum of the void areas (μm 2 ), and A3 is the area of ​​the analyzed image (μm 2) Average void area A4 (μm 2 ) is calculated by the following formula (3): A4=A2 / A5 (3) In formula (3), A5 is the total number of voids.

[0035] The average void diameter A6 (μm) is calculated by the following formula (4) assuming that the void shape is a circle. The first film contains a polymer. The polymer may be a binder polymer that functions as a binding agent. Examples of binder polymers include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, or a mixture thereof. The amount of polymer can be 20% by mass or less when the total amount of inorganic material particles and polymer in the first film is 100% by mass. This increases the density of the first film. A more preferable range of the polymer molecular weight is 0.01% by mass or more and 20% by mass or less. The content of the inorganic material in the first film is desirably 80% by mass or more and 99.9% by mass or less. This increases the insulating properties of the first film.

[0036] The first film may contain a solvent such as n-methyl-2-pyrrolidone (NMP). The confirmation method is as follows: Disassemble the battery and remove the electrode containing the first film. Dry the electrode containing the first film to remove any adhering electrolyte. After drying, peel the first film from the electrode containing the first film using tweezers or similar. Peeling the first film off the first electrode reveals inorganic material particles. Measure the mass of the inorganic material particles and define it as W1 (mg). Add acetone to the inorganic material particles and stir while shaking for at least 24 hours. Measure the combined mass of acetone and inorganic material particles and define it as W2 (mg). After shaking well, leave to settle the solids. Then, analyze the supernatant using gas chromatography to quantify the NMP concentration X (μg / mL) in acetone. Calculate the amount of NMP per unit mass N (μg / g) using the following formula: N = X * (W2 - W1) / (0.7908 * W1), where 0.7908 is the density (mg / mL) of acetone at 25°C. The thickness of the first film can be 1 μm or more and 30 μm or less. The thickness of the first film is measured according to the JIS standard (JIS B 7503-1997). Specifically, these thicknesses are measured using a contact-type digital gauge. A sample is placed on a stone surface plate, and a digital gauge fixed to the stone surface plate is used. A flat measuring terminal with a φ5.0 mm tip is used, and the measuring terminal is brought close to the sample from a distance of 1.5 mm or more but less than 5.0 mm above the sample. The distance at which the terminal makes contact with the sample is the sample thickness. <First Active Material-Containing Layer> The first active material-containing layer is laminated on at least one surface of the first current collector. The first active material-containing layer contains a first active material and may optionally contain a binder and a conductive agent.

[0037] The first active material may be a positive electrode active material or a negative electrode active material. Preferably, the first active material is a positive electrode active material. The type of active material may be one or more.

[0038] As the positive electrode active material, for example, a lithium-containing oxide (for example, a lithium transition metal composite oxide) can be used. a CoO 2 (0<a≦1), Li a Ni 1-x Cox O2 (0<a≦1, 0<x≦0.3), Li a Mn x Ni y Co z O2 (0<a≦1, 0<x<0.5, 0<y<0.5, 0≦z<0.5), Li a Mn 2-x M x O4 (0<a≦1, M is at least one element selected from the group consisting of Mg, Co, Al, and Ni, 0<x<0.2), Li a MPO4 (0<a≦1, M is at least one element selected from the group consisting of Fe, Co, and Ni). The type of lithium-containing oxide may be one or more types.

[0039] As the negative electrode active material, carbon materials such as graphite, tin-silicon alloy materials, etc. can be used, but it is preferable to use a titanium-containing oxide. An example of the titanium-containing oxide is lithium titanium oxide having a spinel structure (e.g., Li 4+x TiO 12 (0≦x≦3)), lithium titanium oxide having a ramsdellite structure (e.g., Li 2+y Ti3O7 (0≦y≦3)), metal composite oxides containing Ti and at least one element selected from the group consisting of P, V, Sn, Cu, Ni and Fe, TiNb 2 O 7 and Ti 2 Nb 10 O 19 Examples of metal composite oxides containing Ti and at least one element selected from the group consisting of P, V, Sn, Cu, Ni, and Fe include TiO 2 -P 2 O 5 , TiO 2 -V 2 O 5 , TiO 2 -P 2 O 5 -SnO 2 , TiO 2 -P 2 O 5-MO (wherein M is at least one element selected from the group consisting of Cu, Ni, and Fe). Metal composite oxides and niobium-titanium-containing oxides can be converted into oxides containing lithium by intercalating lithium upon charging.

[0040] The active material may be a single primary particle, a secondary particle formed by aggregation of primary particles, or a mixture of primary and secondary particles.

[0041] The average particle size of the primary particles of the negative electrode active material is preferably in the range of 0.001 to 1 μm. The average particle size can be determined, for example, by observing the negative electrode active material with a SEM. The particle shape may be either granular or fibrous. In the case of fibrous particles, the fiber diameter is preferably 0.1 μm or less. Specifically, the average particle size of the primary particles of the negative electrode active material can be measured from an image observed with an electron microscope (e.g., SEM). When lithium titanium oxide (also known as lithium titanate) with an average particle size of 1 μm or less is used as the negative electrode active material, a negative electrode active material-containing layer with high surface flatness is obtained. Furthermore, when lithium titanium oxide (lithium titanate) is used, the negative electrode potential is more noble than that of lithium-ion secondary batteries using conventional carbon negative electrodes, so lithium metal precipitation does not occur in principle. Negative electrode active materials containing lithium titanium oxide (lithium titanate) exhibit small expansion and contraction during charge and discharge reactions, preventing the collapse of the crystalline structure of the active material.

[0042] Examples of conductive agents include acetylene black, carbon black, graphite, and mixtures thereof. Examples of binders include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-containing rubber, styrene-butadiene rubber, and mixtures thereof. The binder functions to bind the active material and the conductive agent.

[0043] In the positive electrode active material-containing layer, the contents of the active material, conductive agent, and binder are preferably 80% by mass or more and 97% by mass or less, 2% by mass or more and 18% by mass or less, and 1% by mass or more and 17% by mass or less, respectively. In the negative electrode active material-containing layer, the contents of the negative electrode active material, conductive agent, and binder are preferably 70% by mass or more and 98% by mass or less, 1% by mass or more and 28% by mass or less, and 1% by mass or more and 28% by mass or less, respectively.

[0044] The thickness of the first active material-containing layer can be 5 μm or more and 100 μm or less. <First Current Collector> The first current collector can be a conductive sheet. Examples of the conductive sheet include foil made of a conductive material. Examples of the conductive material include aluminum, aluminum alloy, copper, nickel, etc.

[0045] The thickness of the first current collector can be, for example, 5 μm or more and 40 μm or less.

[0046] The first current collector includes a first current collecting tab in a portion of the first current collector that is not supported by the first active material-containing layer. By covering the portion including the boundary between the first current collecting tab and the first active material-containing layer with the first film, it is possible to prevent the first current collecting tab from coming into contact with the counter electrode and causing an internal short circuit. The first current collecting tab may be formed from the same material as the current collector, or a current collecting tab prepared separately from the current collector and connected to the current collector by welding or the like may also be used. <Second Electrode> <Second Active Material-Containing Layer> The second active material-containing layer is laminated on at least one surface of the second current collector. The second active material-containing layer contains a second active material and may optionally contain a binder and a conductive agent.

[0047] The second active material is a positive electrode active material or a negative electrode active material. It is preferable that the second active material is a negative electrode active material. The active material may be one or more types. Examples of the positive electrode active material and the negative electrode active material are the same as those described for the first active material.

[0048] By including a titanium-containing oxide as the active material in the second active material-containing layer, it is possible to prevent lithium dendrites from precipitating in the first film and the second film, thereby improving the charge-discharge cycle life of the secondary battery.

[0049] Examples of the binder and conductive agent include those described for the first active material. <Second Current Collector> The second current collector may be a conductive sheet. Examples of the conductive sheet include those described for the first current collector.

[0050] The thickness of the second current collector can be, for example, 5 μm or more and 40 μm or less.

[0051] The second current collector includes a second current collecting tab in a portion of the second current collector that is not supported by the second active material-containing layer. By covering the portion including the boundary between the second current collecting tab and the second active material-containing layer with the second film, it is possible to prevent the second current collecting tab from coming into contact with the counter electrode, leading to an internal short circuit. The second current collecting tab may be formed from the same material as the current collector, or a current collecting tab prepared separately from the current collector and connected to the current collector by welding or the like may be used. <Second Film> The second film includes organic fibers. The second film may be a porous film in which organic fibers are deposited in a planar direction. The second film has a front surface and a back surface. One of the main surfaces of the second film corresponds to the front surface, and the other main surface corresponds to the back surface. One of the front and back surfaces of the second film contacts the surface of the first film. For example, the second film may be integrated with the surface of the first film or the surface of the second active material-containing layer disposed opposite the first active material-containing layer. There are no particular limitations on how the second film is integrated with the first film or the second active material-containing layer.

[0052] The organic fiber includes at least one organic material selected from the group consisting of polyamideimide, polyamide, polyolefin, polyether, polyimide, polyketone, polysulfone, cellulose, polyvinyl alcohol (PVA), and polyvinylidene fluoride (PVdF). Examples of polyolefin include polypropylene (PP) and polyethylene (PE). The organic fiber may be one or more types. At least one type selected from the group consisting of polyimide, polyamide, polyamideimide, cellulose, PVdF, and PVA is preferred, and at least one type selected from the group consisting of polyimide, polyamide, polyamideimide, cellulose, and PVdF is more preferred.

[0053] Polyimide is insoluble, infusible and does not decompose even at temperatures of 250 to 400° C., so that a second film having excellent heat resistance can be obtained.

[0054] The organic fibers preferably have a length of 1 mm or more and an average diameter of 2 μm or less, more preferably an average diameter of 1 μm or less. Such a second membrane has sufficient strength, porosity, air permeability, pore size, electrolyte resistance, oxidation-reduction resistance, etc., and therefore functions well as a separator. The average diameter of the organic fibers can be measured by observation with a focused ion beam (FIB) device. The length of the organic fibers can be obtained based on the length measurement obtained by observation with the FIB device.

[0055] Since it is necessary to ensure ion permeability and electrolyte retention, it is preferable that 30% or more of the volume of the entire fibers forming the second membrane be organic fibers having an average diameter of 1 μm or less, more preferably organic fibers having an average diameter of 350 nm or less, and even more preferably organic fibers having an average diameter of 50 nm or less.

[0056] Furthermore, it is more preferable that the volume of organic fibers having an average diameter of 1 μm or less (more preferably 350 nm or less, and even more preferably 50 nm or less) accounts for 80% or more of the total volume of the fibers forming the second film. This state can be confirmed by observing the second film with a scanning ion microscope (SIM). It is more preferable that organic fibers having a diameter of 40 nm or less account for 40% or more of the total volume of the fibers forming the second film. A small diameter of the organic fibers means that they have a small effect on hindering ion migration.

[0057] Cation exchange groups are preferably present on at least a portion of the entire surface, including the front and back surfaces, of the organic fibers. The cation exchange groups promote the migration of ions such as lithium ions through the separator, thereby improving the performance of the battery. Specifically, rapid charging and discharging can be performed over a long period of time. The cation exchange groups are not particularly limited, but examples include sulfonic acid groups and carboxylic acid groups. Fibers having cation exchange groups on their surfaces can be formed, for example, by electrospinning using a sulfonated organic material.

[0058] The second membrane has pores, and the average pore size of the pores is preferably 5 nm or more and 10 μm or less. Furthermore, the porosity is preferably 70% or more and 90% or less. Such pores provide a separator with excellent ion permeability and good electrolyte impregnation. The porosity is more preferably 80% or more. The average pore size and porosity of the pores can be confirmed by mercury intrusion porosimetry, calculation from volume and density, SEM observation, SIM observation, and gas desorption / adsorption. The porosity is preferably calculated from the volume and density of the second membrane. Furthermore, the average pore size is preferably measured by mercury intrusion porosimetry or gas adsorption. A high porosity in the second membrane means that it has less of an effect on ion migration.

[0059] The thickness of the second film is preferably in the range of 12 μm or less. The lower limit of the thickness is not particularly limited, but can be 1 μm.

[0060] In the second film, the porosity can be increased by making the organic fibers contained therein sparse, so it is not difficult to obtain a layer with a porosity of, for example, about 90%. However, it is extremely difficult to form a layer with such a high porosity using particles.

[0061] The second membrane is advantageous over the deposit of inorganic fibers in terms of unevenness, susceptibility to cracking, electrolyte content, adhesion, bending properties, porosity, and ion permeability.

[0062] The second film may contain particles of an organic compound, which may be made of the same material as the organic fibers, or may be formed integrally with the organic fibers.

[0063] The second film may be formed on the second active material-containing layer, or may be formed on the first film. Alternatively, the second film may be formed on both the surfaces of the second active material-containing layer and the first film. In either case, it is preferable that one of the front and back surfaces of the second film be in contact with the surface of the first film.

[0064] The second film is formed, for example, by electrospinning. In electrospinning, the first electrode or the second electrode on which the second film is to be formed is grounded to serve as a ground electrode. When forming the second film on the first electrode, the first electrode on which the first film has already been formed is prepared.

[0065] The liquid raw material (e.g., raw material solution) is charged by the voltage applied to the spinning nozzle, and the charge per unit volume of the raw material solution increases due to the evaporation of the solvent from the raw material solution. As the solvent evaporates and the resulting increase in charge per unit volume occurs continuously, the raw material solution ejected from the spinning nozzle stretches longitudinally and deposits as nano-sized organic fibers on the first or second electrode, which serves as the earth electrode. Coulomb force is generated between the organic fibers and the earth electrode due to the potential difference between the nozzle and the earth electrode. Therefore, the nano-sized organic fibers can increase the contact area with the first film, and these organic fibers can be deposited on the first or second electrode due to Coulomb force, thereby increasing the peel strength of the second film from the electrode. The peel strength can be controlled, for example, by adjusting the solution concentration and the sample-to-nozzle distance. If the second film is not formed on the first and second current collecting tabs, it is recommended to mask the first and second current collecting tabs before forming the second film. An example of this is shown in Figure 11. 11 is a perspective view showing a step of forming a second film on the second electrode. As shown in FIG. 11 , the second film 5 is formed directly by depositing organic fibers on the second active material-containing layer 2b and the second current collector tab 2c from a raw material solution ejected from a nozzle N. One side of the second current collector tab 2c and its vicinity are covered with a mask M. Therefore, the second film 5 is a porous film containing organic fibers deposited across the surface of the second active material-containing layer 2b and the portion of the surface of the second current collector tab 2c adjacent to the second active material-containing layer 2b.

[0066] By using the electrospinning method, the second film can be easily formed on the electrode surface. In principle, the electrospinning method forms a single continuous fiber, ensuring resistance to breakage and film cracking due to bending in a thin film. The fact that the organic fibers constituting the second film are continuous and seamless reduces the probability of fraying or partial loss of the second film, which is advantageous in terms of suppressing self-discharge.

[0067] The liquid raw material used in electrospinning is, for example, a raw material solution prepared by dissolving an organic material in a solvent. Examples of organic materials include those listed above for the organic materials constituting organic fibers. The organic material is dissolved in a solvent at a concentration of, for example, about 5 to 60% by mass. The solvent for dissolving the organic material is not particularly limited, and any solvent can be used, such as dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), N,N'-dimethylformamide (DMF), n-methyl-2-pyrrolidone (NMP), water, or alcohols. For organic materials with low solubility, electrospinning is performed while melting a sheet of the organic material using a laser or the like. Additionally, mixing a high-boiling-point organic solvent with a low-melting-point solvent is also acceptable.

[0068] A second film is formed by applying a voltage to the spinning nozzle using a high-pressure generator while discharging the raw material from the spinning nozzle onto the surface of a predetermined electrode. The applied voltage is determined appropriately depending on the solvent / solute species, the boiling point / vapor pressure curve of the solvent, the solution concentration, temperature, nozzle shape, the sample-nozzle distance, etc., and the potential difference between the nozzle and the workpiece can be set to, for example, 0.1 to 100 kV. The feed rate of the raw material is also determined appropriately depending on the solution concentration, solution viscosity, temperature, pressure, applied voltage, nozzle shape, etc. In the case of a syringe type, the feed rate can be set to, for example, approximately 0.1 to 500 μl / min per nozzle. In the case of multiple nozzles or slits, the feed rate can be determined depending on the opening area.

[0069] Because the organic fibers are formed directly on the surface of the electrode in a dry state, the penetration of the solvent contained in the raw materials into the electrode is substantially prevented. The amount of residual solvent inside the electrode is extremely low, at ppm level or less. Residual solvent inside the electrode causes oxidation-reduction reactions, leading to battery loss and reduced battery performance. According to this embodiment, the risk of such problems occurring is minimized, thereby improving battery performance.

[0070] The thickness of the second film is measured according to the JIS standard (JIS B 7503-1997). Specifically, these thicknesses are measured using a contact digital gauge. A sample is placed on a stone surface plate, and a digital gauge fixed to the stone surface plate is used. A flat measuring terminal with a tip of φ5.0 mm is used, and the measuring terminal is brought close to the sample from a distance of 1.5 mm or more but less than 5.0 mm above the sample, and the distance at which it contacts the sample is the thickness of the sample.

[0071] An example of a laminate according to the first embodiment will be described with reference to FIGS. 1 to 8. Common components in each figure are designated by the same reference numerals, and their description will be omitted. FIG. 1 is a cross-sectional view showing an example of a laminate according to the embodiment. In FIG. 1, the thickness direction of the laminate is indicated as the z-axis, the extension direction of the current collecting tab is indicated as the x-axis, and the direction perpendicular to the extension direction of the current collecting tab is indicated as the y-axis. The cross-sectional view in FIG. 1 is a cross-sectional view of the laminate taken along the extension direction of the current collecting tab (x-axis direction). The laminate 100 shown in FIG. 1 includes a first electrode 1, a second electrode 2, and a separator 3. As shown in FIGS. 1 and 2, the first electrode 1 includes a first current collector 1a, a first active material-containing layer 1b having a first front surface 40 and a first back surface 41, and a first current collecting tab 1c. The first current collector 1a is a conductive sheet. The first active material-containing layer 1b is supported on a portion of each of both main surfaces of the first current collector 1a. On each main surface of the first current collector 1a, one side (e.g., a long side or a short side) and its vicinity does not have an active material-containing layer. The portion of the first current collector 1a that does not have an active material-containing layer formed parallel to one side (e.g., a side parallel to the y-axis direction) functions as a first current collecting tab 1c. Of the surfaces of the first active material-containing layer 1b, the surface that is in contact with the first current collector 1a is a first back surface 41.

[0072] As shown in FIG. 3 , the second electrode 2 includes a second current collector 2a, a second active material-containing layer 2b having a second surface 42 and a second back surface 43, and a second current collector tab 2c. The second current collector 2a is a conductive sheet. The second active material-containing layer 2b is supported on a portion of each of both main surfaces of the second current collector 2a. On each main surface of the second current collector 2a, one side and its vicinity are not supported by an active material-containing layer. The active material-containing layer-free portion formed parallel to one side of the second current collector 2a (e.g., a side parallel to the y-axis direction) functions as the second current collector tab 2c. Of the surfaces of the second active material-containing layer 2b, the surface in contact with the second current collector 2a is the second back surface 43.

[0073] The separator 3 includes a first film 4 containing inorganic material particles and a second film 5 containing organic fibers. The first film 4 has a front surface A and a back surface B, and the second film 5 has a front surface C and a back surface D. As shown in FIGS. 1 and 2 , the back surface B of the first film 4 covers the first surface 40 of each of the first active material-containing layers 1b. The method by which the first film 4 is fixed to the first active material-containing layer 1b is not particularly limited, but examples include adhesion and thermal fusion. As shown in FIG. 3 , the second film 5 covers the second surface 42 of each of the second active material-containing layers 2b and four side surfaces 44 perpendicular to the second surface 42, three end faces 45 of the second current collector 2a exposed on the surface of the second electrode 2, and portions 46 including the boundaries with the second active material-containing layer 2b on both main surfaces of the second current collector tab 2c. Therefore, the first active material-containing layer 1b and the second active material-containing layer 2b face each other with the first film 4 and the second film 5 interposed therebetween.

[0074] 1 , it is possible to realize a battery with high energy density and low self-discharge. In addition, since the second film 5 covers one end face 45 of the second current collector 2 a along the y-axis direction and a portion 46 of the surface of the second current collector tab 2 c that includes the boundary with the second active material-containing layer 2 b, internal short circuits due to contact between the first electrode and the second electrode 2 are reduced.

[0075] The first and second current collecting tabs are not limited to the sides of the first and second current collectors that do not support the active material-containing layer. For example, multiple strip-shaped portions protruding from one side of the first and second current collectors can be used as the first and second current collecting tabs. An example of this is shown in FIG. 4. FIG. 4 shows another example of the first electrode 1. As shown in FIG. 4, multiple strip-shaped portions protruding in the x-axis direction from one side of the first current collector 1a along the y-axis direction may be used as the first current collecting tab 1c.

[0076] The first film can be formed only on at least one main surface of the first active material-containing layer, or it can cover at least a portion of the surface of the first current collecting tab. An example of this is shown in Figures 5 and 6. In Figure 5, the thickness direction of the laminate is indicated as the z-axis, the extension direction of the current collecting tab is indicated as the x-axis, and the direction perpendicular to the extension direction of the current collecting tab is indicated as the y-axis. The cross-sectional view in Figure 5 is a cross-sectional view of the laminate 100 cut along the extension direction of the current collecting tab (x-axis direction). For each of the two first active material-containing layers 1b, four side surfaces 47 perpendicular to the main surface are covered with the first film 6. The first film 6 also covers the portions of both main surfaces of the first current collecting tab 1c adjacent to the first active material-containing layer 1b (portions including the boundary with the first active material-containing layer 1b). The first film 6 is provided near the end face of the second electrode opposite the side from which the second current collecting tab 2c extends. The provision of the first film 6 can reduce internal short circuits caused by contact between the first current collecting tab 1c of the first electrode and the end face of the second electrode. When the first current collecting tab 1c is formed of multiple strip-shaped portions protruding from one side of the first current collector 1a along the y-axis direction, as shown in FIG. 7 , it is desirable to cover with the first film 6 portions 48 of each of the four faces of the first current collecting tab 1c adjacent to the first current collector 1a, and end faces 49 of the first current collector 1a located between the first current collecting tabs 1c. This configuration is effective in reducing internal short circuits.

[0077] The second film may be formed on the second electrode, or alternatively, on the first electrode. An example of this is shown in FIG. 8 . In FIG. 8 , the thickness direction of the laminate is indicated as the z-axis, the extension direction of the current collecting tab is indicated as the x-axis, and the direction perpendicular to the extension direction of the current collecting tab is indicated as the y-axis. The cross-sectional view in FIG. 8 is a cross-sectional view of the laminate 100 cut along the extension direction of the current collecting tab (x-axis direction). The second film 7 covers the surface of the first film 4 and all end faces of the first electrode. The second film 7 also covers portions of both main surfaces of the first current collecting tab 1c, including the boundary with the first active material-containing layer 1b.

[0078] The second electrode is disposed such that the second active material-containing layer 2b faces the first active material-containing layer 1b across a separator 3 consisting of a first film 4 and a second film 7. The portion of the main surface of the first current collecting tab 1c adjacent to the first active material-containing layer 1b is covered with the second film 7, and the end face of the first electrode located opposite the side from which the first current collecting tab 1c protrudes is also covered with the second film 7. This configuration suppresses self-discharge and internal short circuits.

[0079] A method for producing the laminate of the embodiment will be described below.

[0080] A slurry containing a first active material (hereinafter referred to as "slurry I") and a slurry containing an inorganic material (hereinafter referred to as "slurry II") are simultaneously coated onto at least one principal surface of a first current collector. An example of the coating process is shown in FIGS. 9 and 10 . A coating device 30 includes a tank 32 for storing slurry I and a tank 33 for storing slurry II, and is configured to simultaneously coat the substrate with slurry I and slurry II. A long first current collector 1a before being cut to a predetermined size is transported to the slurry outlet of the coating device 30 by a transport roller 31. In FIG. 10 , the slurry I outlet 32a is located upstream of the slurry II outlet 33a. Due to this outlet arrangement, the coating device 30 coats the first current collector 1a with slurry I, except for both ends in the short side direction. Next, before the slurry I dries, the slurry II is coated over the first current collector 1a so that it extends beyond the coating area of ​​the slurry I. Since slurry II is applied over slurry I, slurry II can easily conform to the surface shape of slurry I. After that, the slurry is dried, and the dried product is subjected to a roll press and cut to a predetermined size to obtain a first electrode.

[0081] On the other hand, a slurry containing a second active material is applied to a second current collector, the slurry is dried, and the dried material is roll-pressed and cut to a predetermined size to obtain a second electrode. A second film is formed on the second electrode by electrospinning. Pressing may then be performed. The pressing method may be roll pressing or flat plate pressing.

[0082] The first electrode and the second electrode are laminated so that they face each other with the first film and the second film interposed therebetween to obtain the laminate of the embodiment.

[0083] In the above-described manufacturing method, slurry II contains inorganic particles and a polymer having a median diameter D50 of 0.6 μm or less, and has a composition that satisfies formula (1), so that aggregation of the inorganic particles in slurry II can be suppressed, and therefore, when slurry II is overcoated on slurry I, or during the subsequent drying, pressing, or cutting steps, the conductive agent in slurry I can be prevented from being mixed into slurry II.

[0084] The laminate of the first embodiment described above includes a first active material-containing layer and a first film that contains inorganic material particles and a polymer having a median diameter D50 of 0.6 μm or less, has an average void diameter of 0.5 μm or less, and satisfies the following formula (1):

[0085] 0<Ra 02 / Ra 01 ≦1.5 (1) However, Ra 01 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and n-methyl-2-pyrrolidone. 02 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and the polymer.

[0086] The first film can suppress aggregation of inorganic material particles and reduce the generation of coarse particles. As a result, contamination of the first film with the conductive agent in the first active material-containing layer can be suppressed, preventing a decrease in the insulating properties of the first film. Therefore, a battery including this laminate can suppress self-discharge. Furthermore, this battery can improve durability performance, such as cycle life performance. (Second Embodiment) A battery of the second embodiment includes the laminate of the first embodiment. The battery may further include an electrolyte and an exterior member capable of housing the electrolyte and the laminate.

[0087] A plurality of laminates may be used as an electrode group in a battery. A plurality of laminates may be stacked so that the first film and the second film are located between the first active material-containing layer of one laminate and the second active material-containing layer of the laminate adjacent to this laminate. The shape of the electrode group is not limited to this, and one or more laminates wound into a spiral or flat spiral shape may also be used as the electrode group.

[0088] The battery may further include a first electrode terminal electrically connected to the first current collecting tab and a second electrode terminal electrically connected to the second current collecting tab.

[0089] The electrolyte may be, for example, a non-aqueous electrolyte. Examples of the non-aqueous electrolyte include a liquid non-aqueous electrolyte prepared by dissolving an electrolyte in an organic solvent, and a gel non-aqueous electrolyte obtained by combining a liquid electrolyte with a polymer material. The liquid non-aqueous electrolyte can be prepared, for example, by dissolving the electrolyte in an organic solvent at a concentration of 0.5 mol / L or more and 2.5 mol / L or less.

[0090] Examples of the electrolyte include lithium salts such as lithium perchlorate (LiClO), lithium hexafluorophosphate (LiPF), lithium tetrafluoroborate (LiBF), lithium hexafluoroarsenate (LiAsF), lithium trifluoromethasulfonate (LiCFSO), and lithium bistrifluoromethylsulfonylimide [LiN(CFSO)], or mixtures thereof. A material that is resistant to oxidation even at high potentials is preferred, with LiPF being the most preferred.

[0091] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate, chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC), cyclic ethers such as tetrahydrofuran (THF), 2-methyltetrahydrofuran (2MeTHF), and dioxolane (DOX), chain ethers such as dimethoxyethane (DME), and diethoxyethane (DEE), γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents may be used alone or in combination.

[0092] Examples of polymeric materials include polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), and polyethylene oxide (PEO).

[0093] As the non-aqueous electrolyte, a room temperature molten salt containing lithium ions (ionic melt), a polymer solid electrolyte, an inorganic solid electrolyte, or the like may be used.

[0094] As the exterior member, for example, a metal container or a container made of a laminated film can be used.

[0095] The shape of the battery is not particularly limited, and various shapes such as cylindrical, flat, thin, rectangular, and coin shapes can be used.

[0096] FIG. 12 is a partially cutaway perspective view showing an example of a secondary battery according to an embodiment. FIG. 12 is a diagram showing an example of a secondary battery using a laminate film as a casing member. The secondary battery 10 shown in FIG. 12 includes a casing member 11 made of a laminate film, an electrode group 12, a first electrode terminal 13, a second electrode terminal 14, and a nonaqueous electrolyte (not shown). The electrode group 12 includes a plurality of the laminated bodies of the embodiment, and has a structure in which a first electrode and a second electrode are stacked with a separator formed of a first film and a second film interposed therebetween. The nonaqueous electrolyte (not shown) is retained or impregnated in the electrode group 12. The first electrode terminal 13 is electrically connected to a first current collecting tab of the first electrode. The second electrode terminal 14 is electrically connected to a second current collecting tab of the second electrode. As shown in FIG. 12, the first electrode terminal 13 and the second electrode terminal 14 are spaced apart from each other, with their respective tips protruding outward from one side of the casing member 11.

[0097] FIG. 13 is an exploded perspective view showing another example of a secondary battery according to an embodiment. FIG. 13 is a diagram showing an example of a secondary battery using a rectangular metal container as a housing member. The secondary battery shown in FIG. 13 includes a housing member 20, a wound electrode group 21, a lid 22, a first electrode terminal 23, a second electrode terminal 24, and a nonaqueous electrolyte (not shown). The wound electrode group 21 has a structure in which the laminate of the embodiment is wound into a flat spiral shape. In the wound electrode group 21, a first current collecting tab 25 wound into a flat spiral is located on one circumferential end face, and a second current collecting tab 26 wound into a flat spiral is located on the other circumferential end face. The nonaqueous electrolyte (not shown) is retained or impregnated in the electrode group 21. A first electrode lead 27 is electrically connected to the first current collecting tab 25 and also to the first electrode terminal 23. The second electrode lead 28 is electrically connected to the second current collecting tab 26 and also to the second electrode terminal 24. The electrode group 21 is disposed inside the exterior member 20 so that the first electrode lead 27 and the second electrode lead 28 face the main surface side of the exterior member 20. The lid 22 is fixed to the opening 20a of the exterior member 20 by welding or the like. The first electrode terminal 23 and the second electrode terminal 24 are each attached to the lid 22 via an insulating hermetic seal member (not shown).

[0098] According to the battery of the second embodiment described above, since the battery includes the laminate of the embodiment, self-discharge can be suppressed. Furthermore, since the insulating properties can be maintained even when the thickness of the first film is reduced, the thickness of the separator including the first film can be reduced, thereby improving the energy density of the battery. Furthermore, this battery can improve durability performance such as cycle life performance.

[0099] Third Embodiment According to a third embodiment, a battery pack is provided, which includes a battery according to an embodiment.

[0100] The battery pack according to the embodiment may include a plurality of batteries. The plurality of batteries may be electrically connected in series or in parallel. Alternatively, the plurality of batteries may be electrically connected in a combination of series and parallel. That is, the battery pack according to the embodiment may include a battery assembly. The number of battery assemblies may be multiple. The plurality of battery assemblies may be electrically connected in series, in parallel, or in a combination of series and parallel.

[0101] An example of a battery pack according to an embodiment will be described below with reference to Fig. 14 and Fig. 15. Fig. 14 is an exploded perspective view showing an example of a battery pack according to an embodiment. Fig. 15 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 14.

[0102] 14 and 15 includes a plurality of unit cells 51. The unit cells 51 may be, for example, the flat battery 10 according to the embodiment described with reference to FIG.

[0103] A plurality of unit cells 51 are stacked such that the negative electrode terminals (second electrode terminals) 14 and positive electrode terminals (first electrode terminals) 13 extending outward are aligned in the same direction, and are fastened together with adhesive tape 52 to form an assembled battery 53. These unit cells 51 are electrically connected in series with each other as shown in FIG.

[0104] The printed wiring board 54 is disposed so as to face the side surface from which the negative electrode terminal 14 and the positive electrode terminal 13 of the battery 51 extend. As shown in Fig. 15, the printed wiring board 54 is mounted with a thermistor 55, a protection circuit 56, and a terminal 57 for supplying current to an external device. An insulating plate (not shown) is attached to the surface of the printed wiring board 54 facing the battery pack 53 to prevent unnecessary connection with the wiring of the battery pack 53.

[0105] The positive electrode lead 58 is connected to the positive electrode terminal 13 located on the bottom layer of the battery pack 53, and its tip is inserted into and electrically connected to a positive electrode connector 59 on the printed wiring board 54. The negative electrode lead 60 is connected to the negative electrode terminal 14 located on the top layer of the battery pack 53, and its tip is inserted into and electrically connected to a negative electrode connector 61 on the printed wiring board 54. These connectors 59 and 61 are connected to the protection circuit 56 through wires 62 and 63 formed on the printed wiring board 54.

[0106] The thermistor 55 detects the temperature of the cell 51 and transmits the detection signal to the protection circuit 56. The protection circuit 56 can interrupt the positive wiring 64a and the negative wiring 64b between the protection circuit 56 and the power terminal 57 for connecting to an external device under predetermined conditions. One example of the predetermined condition is when the temperature detected by the thermistor 55 exceeds a predetermined temperature. Another example of the predetermined condition is when overcharge, overdischarge, or overcurrent of the cell 51 is detected. This overcharge detection is performed for each cell 51 or the entire battery pack 53. When detecting each cell 51, the battery voltage or the positive or negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 51. In the battery pack 50 shown in FIGS. 14 and 15 , each cell 51 is connected to wiring 65 for voltage detection. A detection signal is transmitted to the protection circuit 56 via these wirings 65.

[0107] Protective sheets 66 made of rubber or resin are disposed on the three sides of the battery pack 53 excluding the sides from which the positive electrode terminal 13 and the negative electrode terminal 14 protrude.

[0108] The battery pack 53 is housed in a container 67 together with the protective sheets 66 and the printed wiring board 54. That is, the protective sheets 66 are arranged on both inner surfaces along the long sides and the inner surface along the short sides of the container 67, and the printed wiring board 54 is arranged on the inner surface along the other short side on the opposite side across the battery pack 53. The battery pack 53 is located in a space surrounded by the protective sheets 66 and the printed wiring board 54. A lid 68 is attached to the top surface of the container 67.

[0109] Heat-shrinkable tape may be used to secure the battery pack 53 instead of the adhesive tape 52. In this case, protective sheets are placed on both sides of the battery pack, and the heat-shrinkable tape is wrapped around the battery pack, and then the heat-shrinkable tape is thermally shrunk to bind the battery pack.

[0110] 14 and 15 show the cells 51 electrically connected in series, they may be electrically connected in parallel to increase the battery capacity. Furthermore, assembled battery packs may be electrically connected in series and / or parallel.

[0111] Furthermore, the configuration of the battery pack according to the embodiment may be appropriately changed depending on the application. The battery pack according to the embodiment is preferably used in applications where cycle performance in large current charging and discharging is desired. Specific applications include power sources for digital cameras and in-vehicle applications such as two- to four-wheel hybrid electric vehicles, two- to four-wheel electric vehicles, and power-assisted bicycles. In-vehicle applications are particularly suitable for the battery pack according to the embodiment.

[0112] The battery pack according to the third embodiment includes the battery according to the embodiment. Therefore, the battery pack according to the embodiment can suppress self-discharge and can increase the energy density and durability.

[0113] Example 1 A secondary battery with a first electrode as a positive electrode and a second electrode as a negative electrode was fabricated by the following method. LiMn2O4 particles were prepared as the positive electrode active material, carbon black as the conductive material, and polyvinylidene fluoride as the binder. These were mixed in a mass ratio of 90:5:5 to obtain a mixture. Next, the obtained mixture was dispersed in n-methyl-2-pyrrolidone (NMP) solvent to prepare slurry I. TiO2 particles (manufactured by Teika Corporation) whose surfaces were coated with Al2O3 particles were prepared as inorganic material particles. The inorganic material particles had a median diameter D50 of 0.3 μm and a specific surface area of ​​12 m 2 / g.

[0114] As a binder polymer, a homopolymer type PVdF (manufactured by Kureha Corporation) having a weight average molecular weight of 500,000 was prepared. PVdF was dissolved in NMP at 10% by mass to prepare a 10% by mass PVdF solution.

[0115] Slurry II was prepared using the following method, with a 4% by mass ratio of PVdF to the inorganic material particles. First, a 10% by mass solution of PVdF was added to NMP solvent and stirred for 10 minutes using a rotor-mounted mixer. The inorganic material particles were gradually added and stirred for 60 minutes. The mixture was then dispersed using a bead mill filled with 1 mm diameter zirconia beads at a filling rate of approximately 50%. The bead mill conditions were a flow rate of 0.1 to 0.5 L / min and a peripheral speed of 5 to 10 m / sec. Grind gauge measurement (JIS K5600-2-5) of Slurry II after dispersion revealed that coarse particles were 20 μm or smaller and few in number. The Hansen solubility parameter (HSP), which indicates the affinity between two components, was measured using the method described below. First, inorganic material particles were added to 10 to 20 different dispersion media, each containing NMP, to a concentration of 5% by mass, to obtain 10 to 20 different samples A. Furthermore, PVdF binder powder was added to each of 10 to 20 types of dispersion media of the same type to a concentration of 5% by mass, to obtain 10 to 20 types of sample B. For the samples A and B thus obtained, pulse NMR measurements were performed to determine the relaxation times, and it was determined whether the inorganic material particles and the PVdF binder were good or poor solvents for the 10 to 20 types of dispersion media, including NMP. From these results, the Hansen spheres were calculated for the inorganic material particles and PVdF. An example is shown in Figure 16. In Figure 16, the Hansen sphere of the inorganic material particles is indicated by H1, and the Hansen sphere of the PVdF is indicated by H2. The difference in the center coordinates between these was calculated, and this was taken as the distance between the HSP values ​​(Ra). The distance between the HSP values ​​(Ra) between NMP and the inorganic material particles was calculated. 01 ) is D1, and the distance between the HSP values ​​of PVdF and inorganic material particles (Ra 02 The distance between the HSP values ​​of PVdF and NMP (Ra) is shown as D2, and the distance between the HSP values ​​of PVdF and NMP (Ra) is shown as D3. D1 was 2.6, D2 was 3.96, and D3 was 2.73. 02 ) / D1(Ra 01The ratio represented by the formula (1) was 1.5. Next, slurry I and slurry II were applied to both sides of a 12 μm thick aluminum foil in this order, with slurry II overflowing. After drying slurry I and slurry II, the dried film was roll-pressed and cut to a predetermined size to obtain a positive electrode, which was the first electrode. A portion not carrying the positive electrode active material-containing layer was provided on one long side of the current collector, and this portion was used as a positive electrode current collecting tab. The thickness of the first film formed from slurry II was 3 μm. The thickness of the positive electrode active material-containing layer was 20 μm.

[0116] On the other hand, a negative electrode, which was a second electrode, was prepared by the following method. 12 Lithium titanate particles having the composition shown in the formula (1), carbon black as a conductive agent, and polyvinylidene fluoride as a binder were prepared. These were mixed in a mass ratio of 90:5:5 to obtain a mixture. The obtained mixture was dispersed in n-methyl-2-pyrrolidone (NMP) solvent to prepare a slurry. The obtained slurry was applied to aluminum foil with a thickness of 12 μm and dried. The dried coating was then pressed to obtain a negative electrode. A portion not carrying the negative electrode active material-containing layer was provided on one long side of the current collector, and this portion served as a negative electrode current collecting tab.

[0117] A second film was formed on the negative electrode by electrospinning, depositing organic fibers. Polyamideimide was used as the organic material. This polyamideimide was dissolved in DMAc as a solvent at a concentration of 20% by mass to prepare a raw material solution as a liquid raw material. The resulting raw material solution was supplied to the surface of the negative electrode from the spinning nozzle at a supply rate of 5 μL / min using a metering pump. A high-voltage generator was used to apply a voltage of 20 kV to the spinning nozzle, and a layer of organic fibers was formed on the negative electrode surface while moving the spinning nozzle over a range of 100 × 200 mm. The electrospinning method was performed with the surface of the negative electrode current collector tab masked, except for a 10 mm portion from the boundary with the negative electrode active material-containing layer on both surfaces (main surfaces) of the negative electrode current collector tab, to obtain a negative electrode having the structure shown in FIG. 3 . That is, the second film covered the surface (main surface) of each negative electrode active material-containing layer, four side surfaces perpendicular to the surface, three end faces of the negative electrode current collector exposed to the negative electrode surface, and a portion of the surface of the negative electrode current collector tab including the boundary with the negative electrode active material-containing layer. The thickness of the negative electrode active material-containing layer was 15 μm. The thickness of the second film was 2 μm.

[0118] The negative electrode was then pressed using a roll press. The second membrane had an average organic fiber diameter of 700 nm, and organic fibers with an average diameter of 1 μm or less accounted for 50% or more of the total volume of the fibers forming the second membrane. The average pore size was 10 μm, and the porosity was 80%.

[0119] Next, a secondary battery was fabricated using the fabricated positive electrode and negative electrode.

[0120] The positive electrode and negative electrode were arranged so that the positive electrode active material-containing layer and the negative electrode active material-containing layer faced each other via the first and second films, and then rolled into a flattened shape to obtain a flat, spirally wound electrode group. After vacuum drying overnight at room temperature, the electrode group was left for one day in a glove box with a dew point of -80°C or less. This was then placed in a metal container together with an electrolyte to obtain the nonaqueous electrolyte battery of Example 1. The electrolyte used was LiPF6 dissolved in ethylene carbonate (EC) and dimethyl carbonate (DMC). The battery was charged to an SOC of 70% and placed in a thermostatic chamber at 25°C to observe the change in voltage over time. As a result, the voltage drop was 0.75 mV / day, indicating that self-discharge was suppressed. (Example 2) A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the first film was prepared by the following method. Barium sulfate (BaSO4) particles (manufactured by Kinseimatec Co., Ltd.) having a median diameter D50 of 0.6 μm were prepared as inorganic material particles.

[0121] The binder polymer used was the same type of PVdF as described in Example 1. 10% by mass of PVdF was dissolved in NMP to prepare a 10% by mass PVdF solution.

[0122] Slurry II was prepared using the following method, so that the PVdF content relative to the inorganic material particles was 4% by mass. First, a 10% by mass solution of PVdF was added to an NMP solvent and stirred for 10 minutes using a stirrer with rotating blades. The inorganic material particles were gradually added and stirred for 60 minutes. The mixture was then dispersed using a bead mill filled with 1 mm diameter zirconia beads at a filling rate of approximately 50%. The bead mill conditions were a flow rate of 0.1 to 0.5 L / min and a peripheral speed of 5 to 10 m / sec. Grind gauge measurement (JIS K5600-2-5) of the dispersed slurry II revealed that the coarse particles were 30 μm or less and were few in number.

[0123] D1 to D3 were determined in the same manner as in Example 1, and D1 was 4.07, D2 was 2.35, and D3 was 2.73. 02 ) / D1(Ra 01The ratio (D50) was calculated to be 0.58. The resulting battery was charged to an SOC of 70% and placed in a thermostatic chamber at 25°C to measure the change in voltage over time. The resulting voltage drop was 0.5 mV / day, indicating that self-discharge was suppressed. (Comparative Example 1) Titania particles (manufactured by Titan Industries) with a median diameter D50 of 0.3 μm were prepared as inorganic material particles. Modified PVdF (manufactured by Solvay) with an average molecular weight of 1,000,000 to 1,200,000 was prepared as a binder polymer. A small amount was dispersed using a benchtop mixer under dispersion conditions equivalent to those in Example 1. A grind gauge revealed numerous coarse particles, indicating that dispersion was not possible. Due to the large number of coarse particles, it was not possible to fabricate an electrode, and therefore a battery. D1 to D3 were calculated in the same manner as in Example 1, yielding D1 of 2.6, D2 of 6.72, and D3 of 4.14. D2 (Ra 02 ) / D1(Ra 01 The ratio (D50) was calculated to be 2.6. (Comparative Example 2) Alumina (Al2O3) particles (manufactured by Nippon Light Metal Co., Ltd.) with a median diameter D50 of 1.1 μm were used as inorganic material particles. The same type of PVdF as in Comparative Example 1 was used as the binder polymer. PVdF was dissolved in NMP at 10% by mass to prepare a 10% by mass PVdF solution.

[0124] Slurry II was prepared by the following method so that the PVdF content was 4% by mass relative to the inorganic material particles. First, a 10% by mass solution of PVdF was added to an NMP solvent and stirred for 10 minutes using a stirrer with rotating blades. The inorganic material particles were gradually added thereto and stirred for 60 minutes. Grind gauge measurement (JIS K5600-2-5) of Slurry II after dispersion revealed poor leveling and indistinguishable results.

[0125] D1 to D3 were determined in the same manner as in Example 1, and D2 (Ra 02 ) / D1(Ra 01 The ratio of 1.7 was calculated.

[0126] A nonaqueous electrolyte battery was fabricated using the same method as in Example 1, except that the first membrane was fabricated using the above method. The average pore diameter of the first membrane was measured using the above method and found to be 0.8 μm. The resulting battery was charged to an SOC of 70% and placed in a thermostatic chamber at 25°C to measure the voltage change over time. The resulting voltage drop was 0.8 mV / day. FIG. 17 shows a schematic SEM image of a cross section of the first membrane of Comparative Example 2 cut along the thickness direction. As shown in FIG. 17, it can be seen that conductive agent 71 is mixed into the voids generated by the aggregation of inorganic material particles 70 in the first membrane 4. The conductive agent 71 is a component of the layer 1b containing the positive electrode active material 72. As a result of the conductive agent 71 being mixed into the first membrane 4, the insulating properties of the first membrane 4 were reduced. (Comparative Example 3) A nonaqueous electrolyte battery was fabricated using the same configuration as in Comparative Example 2, except that the average pore diameter of the first membrane 4 was set to 0.5 μm. The resulting battery was charged to an SOC of 70% and left in a thermostatic chamber at 25° C. to measure the change in voltage over time. As a result, the voltage drop was 0.23 mV / day, and self-discharge was suppressed more than in Comparative Example 3.

[0127] The type of inorganic material, median diameter D50 (μm), and Ra of the inorganic material particles in the examples and comparative examples 02 / Ra 01 The results of the median diameter D50 (μm), the average void diameter (μm), the dispersion evaluation result using a grind gauge, and the self-discharge rate measurement result (mV / day) are shown in Table 1. 02 / Ra 01 The method for measuring the average void diameter (μm) is as described above.

[0128]

[0129] As is clear from Table 1, the batteries of Examples 1 and 2 can suppress self-discharge. Furthermore, the first films of the batteries of Examples 1 and 2 have few coarse particles and are highly dense, so they can maintain insulation properties for a long period of time. Therefore, the batteries of Examples 1 and 2 have excellent life performance.

[0130] On the other hand, the first films of Comparative Examples 2 and 3 both had larger median diameters of inorganic material particles and contained a larger number of coarse particles than those of Examples 1 and 2. In the battery of Comparative Example 3, the average pore diameter of the first film was 0.5 μm or less, and therefore self-discharge was suppressed compared to Comparative Example 2, but the first film was less dense, and therefore the durability of the first film was poor, resulting in a low battery life performance.

[0131] The laminate according to at least one of the embodiments and examples described above includes a first film containing inorganic material particles and a polymer having a median diameter D50 of 0.6 μm or less, an average void diameter of 0.5 μm or less, and satisfying the following formula (1):

[0132] 0<Ra 02 / Ra 01 ≦1.5 (1) However, Ra 01 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and n-methyl-2-pyrrolidone, and Ra 02 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and the polymer.

[0133] The laminate can suppress aggregation of inorganic material particles, thereby increasing the density of the first film, thereby providing a battery with reduced self-discharge and excellent durability.

[0134] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are intended to be included within the scope and spirit of the invention, as well as within the scope of the invention and its equivalents as defined in the claims.

[0135] The following description will be made of embodiments of the present invention. <1> A laminate comprising: a first current collector; a first active material-containing layer laminated on at least one surface of the first current collector; and a first film covering at least a part of the surface of the first active material-containing layer on which the first current collector is not laminated, the first film containing inorganic material particles and a polymer, having a median diameter D50 of 0.6 μm or less, an average void diameter of 0.5 μm or less, and satisfying the following formula (1):

[0136] 0<Ra 02 / Ra 01 ≦1.5 (1) However, Ra 01 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and n-methyl-2-pyrrolidone, and Ra 02 is the distance between the Hansen Solubility Parameters (HSP values) of the inorganic material particles and the polymer. <2> The laminate according to <1>, wherein the first film contains n-methyl-2-pyrrolidone. <3> The specific surface area of ​​the inorganic material particles is 30 m 2 / g or less. <4> The laminate according to any one of <1> to <3>, wherein the inorganic material particles contain at least one compound selected from the group consisting of titanium oxide, aluminum oxide, and barium sulfate. <5> The laminate according to any one of <1> to <4>, wherein the inorganic material particles are at least partially coated with aluminum oxide and include at least one of particles containing titanium oxide and particles containing barium sulfate. <6> The laminate according to any one of <1> to <5>, wherein the amount of the polymer in the first film is 20 mass% or less, when the total amount of the inorganic material particles and the polymer is taken as 100 mass%. <7> The laminate according to any one of <1> to <6>, wherein the polymer is a binder polymer. <8> The laminate according to any one of <1> to <7>, wherein the first active material-containing layer contains a positive electrode active material as an active material. <9> The laminate according to any one of <1> to <8>, further comprising: a second current collector; a second active material-containing layer laminated on at least one surface of the second current collector; and a second film containing organic fibers, the second active material-containing layer and the first film being located between the second active material-containing layer and the first film. <10> A battery comprising the laminate according to any one of <1> to <9>. <11> A battery pack including a battery comprising the laminate according to any one of <1> to <9>.

[0137] REFERENCE SIGNS LIST 1...first electrode, 1a...first current collector, 1b...first active material-containing layer, 1c...first current collecting tab, 2...second electrode, 2a...second current collector, 2b...second active material-containing layer, 2c...second current collecting tab, 3...separator, 4...first film, 5...second film, 6...first film, 7...second film, 10...battery, 11...exterior member, 12...electrode group, 13...first electrode terminal, 13...positive electrode terminal (first electrode terminal), 14...Negative electrode terminal (second electrode terminal), 14...Second electrode terminal, 20...Exterior member, 20a...Opening, 21...Wound electrode group, 22...Lid, 23...First electrode terminal, 24...Second electrode terminal, 25...First current collecting tab, 26...Second current collecting tab, 27...First electrode lead, 28...Second electrode lead, 30...Coating device, 31...Conveyor roller, 32...Tank, 32a...Slurry I discharge port, 33...Tank 33a...slurry II discharge port, 40...first surface, 41...first back surface, 42...second surface, 43...second back surface, 44...four side surfaces, 45...end surface, 45...cross section, 46...portion, 47...four side surfaces, 49...end surface, 50...battery pack, 51...single cell, 52...adhesive tape, 53...battery assembly, 54...printed wiring board, 55...thermistor, 56...protection circuit, 57...current-carrying terminal, 58...positive electrode lead , 59...positive electrode connector, 60...negative electrode lead, 61...negative electrode connector, 62...wiring, 63...wiring, 64a...positive side wiring, 64b...negative side wiring, 65...wiring, 66...protective sheet, 67...storage container, 68...lid, 70...inorganic material particles, 71...conductive agent, 72...positive electrode active material, 100...laminated body, H1...Hansen dissolving bulb for inorganic material particles, H2...Hansen dissolving bulb for NMP solution of PVdF.

Claims

1. A laminate comprising: a first current collector; a first active material-containing layer laminated on at least one surface of the first current collector; and a first film covering at least a portion of the surface of the first active material-containing layer on which the first current collector is not laminated, the first film containing inorganic material particles and polymers having a median diameter D50 of 0.6 μm or less, an average void diameter of 0.5 μm or less, and satisfying the following formula (1): 0<Ra 02 / Ra 01 ≦1.5 (1) However, Ra 01 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and n-methyl-2-pyrrolidone, and Ra 02 is the distance between the Hansen solubility parameters (HSP values) of the inorganic material particles and the polymer.

2. The laminate of claim 1, wherein said first film comprises n-methyl-2-pyrrolidone.

3. The specific surface area of ​​the inorganic material particles is 30 m 2 The laminate according to claim 1, wherein the elastic modulus is 0.1 / g or less.

4. The laminate according to claim 1, wherein said inorganic material particles contain at least one compound selected from the group consisting of titanium oxide, aluminum oxide, and barium sulfate.

5. The laminate according to claim 1, wherein the inorganic material particles include at least one of particles having at least a portion of a surface thereof coated with aluminum oxide and containing titanium oxide or particles containing barium sulfate.

6. The laminate according to claim 1, wherein the amount of the polymer is 20% by mass or less when the total amount of the inorganic material particles and the polymer in the first film is taken as 100% by mass.

7. The laminate according to claim 1, wherein the polymer is a binder polymer.

8. The laminate according to claim 1, wherein the first active material-containing layer contains a positive electrode active material as the active material.

9. The laminate according to claim 1, further comprising: a second current collector; a second active material-containing layer laminated on at least one surface of said second current collector; and a second film containing organic fibers, said second active material-containing layer being positioned between said second active material-containing layer and said first film.

10. A battery comprising the laminate according to any one of claims 1 to 9.

11. A battery pack comprising a battery including the laminate according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Composition for forming porous insulating layer, electrode for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and manufacturing method of electrode for non-aqueous electrolyte secondary battery

    JP2019087523A

  • Laminate and secondary battery

    JP2019153431A

  • Laminate and secondary battery

    JP2019153434A

  • Insulating layer, battery cell sheet, and secondary battery

    JP2019204689A

  • Battery unit and secondary battery

    JP2021048084A