Narrow-groove gas-shielded arc welding method
The three-electrode narrow-gap gas-shielded arc welding method addresses hot cracking issues by controlling current values and electrode arrangements, enhancing welding efficiency and reducing costs for large steel structures.
Patent Information
- Application Number
- PCT/JP2024/010617
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-03-18
- Publication Date
- 2024-11-28
AI Technical Summary
The existing narrow-gap gas-shielded arc welding methods, particularly in multi-electrode welding, face challenges with hot cracking on the weld bead surface during second and subsequent layers, limiting their effectiveness and efficiency.
A three-electrode narrow-gap gas-shielded arc welding method is developed, where the current values for the first and second electrodes are set between 260A to 360A, and the current value of the third electrode is controlled based on the width of the weld bead formed by the previous layer, using a mixed shielding gas with 20% CO2 or more, and specific electrode arrangements to suppress hot cracking.
This method achieves high welding efficiency while effectively suppressing hot cracking, resulting in lower manufacturing costs and improved joint quality, suitable for large and thick steel structures like buildings and bridges.
Smart Images

Figure JP2024010617_28112024_PF_FP_ABST
Abstract
Description
Narrow gap gas shielded arc welding method
[0001] The present invention relates to a gas-shielded arc welding method, and in particular to a narrow-gap gas-shielded arc welding method applicable to steel plates having a thickness of 22 mm or more. The term "narrow groove" as used herein means a groove angle of 25° or less and a minimum groove gap width between steel plates to be welded (base metal) that is 50% or less of the thickness of the steel plates.
[0002] Gas shielded arc welding, which is used for welding steel plates, is a 2 Single gas or Ar and CO 2 The most common type is the consumable electrode type, which uses a mixed gas of argon and argon to shield the molten area, and is widely used in the manufacturing fields of automobiles, construction, bridges, electrical equipment, etc.
[0003] In recent years, as steel structures have become larger and thicker, the amount of welding during the manufacturing process, particularly in butt welding of steel plates, has increased, and the welding work has become more time-consuming, resulting in increased construction costs.
[0004] One possible way to improve this is to apply narrow-gap gas-shielded arc welding, which uses arc welding to multi-layer weld a groove with a gap that is small compared to the plate thickness. Narrow-gap gas-shielded arc welding reduces the cross-sectional area of the weld compared to regular gas-shielded arc welding, which is expected to achieve high welding efficiency and energy savings, and ultimately reduce construction costs.
[0005] Furthermore, recently, a technology has been proposed for performing this narrow-gap gas-shielded arc welding method using multiple electrodes. Multi-electrode welding can increase the amount of deposited metal (metal that melts the welding wire and adheres to the groove) used to fill the groove by the number of electrodes, making it possible to obtain higher welding efficiency than single-electrode welding, and is an effective means for increasing welding efficiency.
[0006] For example, Patent Document 1 discloses a narrow-gap gas-shielded arc welding method for joining steel plates by narrow-gap multi-layer welding. This document describes a first-layer welding method using multi-electrode welding with two or more electrodes, with the first and second electrodes positioned along a predetermined parallel weld line, and the distance between the welding wire tips of the first and second electrodes controlled to a range of 5 mm to 16 mm. Furthermore, the angle of the line connecting the welding wire tips of the first and second electrodes relative to the direction perpendicular to the weld line is controlled to a range of 45° or less. Furthermore, the fusion depth perpendicular to the weld line at the bottom of the steel plate is set to 1.5 mm or more. It is described that these methods result in no welding defects and improved welding efficiency, even when groove preparation such as gas cutting or plasma cutting is performed.
[0007] Patent No. 6137053
[0008] However, the technology described in Patent Document 1 is limited to first layer welding, and in the second layer and subsequent layers, hot cracks C may occur on the weld bead surface as shown in FIG. 3 , making it insufficient as a technology for preventing hot cracks.
[0009] An object of the present invention is to solve the problems of the conventional art and to provide a multi-electrode narrow gap gas-shielded arc welding method that achieves high welding efficiency and can suppress hot cracking.
[0010] In order to achieve the above-mentioned object, the inventors conducted extensive research into three-electrode welding to find a welding method that suppresses hot cracking. As a result, they found that when welding the second and subsequent layers, the current values of the first and second electrodes are set in the range of 260 A to 360 A, and the current value of the third electrode is controlled according to the width of the weld bead formed in the previous welding layer, which becomes the groove gap for the next weld. This method suppresses hot cracking.
[0011] The present invention has been completed based on these findings and further investigations. That is, the gist of the present invention is as follows: [1] A steel plate having a thickness t of 22 mm or more is welded to a steel plate having a groove angle θ of 25° or less and a bottom groove gap G 0A narrow gap gas shielded arc welding method applied to the second layer and thereafter in narrow gap multi-layer welding of 7 mm to 18 mm, in which the multi-layer welding is performed using three electrodes, and the current value I of the first electrode and the second electrode is 1 and I 2 is set in the range of 260 A to 360 A, and the current value I 3 i A narrow gap gas-shielded arc welding method in which [A] is in a range that satisfies the following formula (1): 3 i ≦30×G i-1 -10 ... (1) where I 3 i : Current value [A] of the third electrode of the i-th layer, G i-1 : width [mm] of a weld bead formed by welding the layer immediately before the i-th layer (i-1th layer), where i is a natural number equal to or greater than 2. [2] The narrow gap gas-shielded arc welding method of [1] above, wherein one of the first electrode and the second electrode is a negative wire (positive polarity) and the other is a positive wire (reverse polarity), a distance a between tips of welding wires supplied from power feed tips at the ends of welding torches for the first electrode and the second electrode is in the range of 5 mm to 16 mm, an angle α of a line connecting the welding wire tips of the first electrode and the second electrode with respect to a direction perpendicular to the weld line is 60° or less, diameters of welding wires for all of the electrodes are in the range of 1.0 mm to 1.6 mm, and a distance b between tips of welding wires supplied from power feed tips at the ends of welding torches for the second electrode and the third electrode is in the range of 10 mm to 100 mm. [3] The narrow gap gas-shielded arc welding method according to [1] or [2], wherein the third electrode is disposed in the center of the groove behind the first electrode and the second electrode. [4] In any one of [1] to [3], the shielding gas contains 20% by volume or more of CO 2 [5] The narrow gap gas-shielded arc welding method according to any one of [1] to [4], wherein at least one welding wire used in the positive electrode contains 0.005% to 0.060% by mass of REM (rare earth element).
[0012] According to the present invention, narrow-gap gas-shielded arc welding can be performed with high welding efficiency in the second and subsequent layers while suppressing hot cracking. Furthermore, narrow-gap gas-shielded arc-welded joints obtained by this method can be manufactured at significantly lower costs than conventional welded joints, making them extremely useful for general structures such as buildings, bridges, and ships.
[0013] Fig. 1 is an explanatory diagram showing a typical groove shape targeted by the present invention. (a) is an example in which the weld metal surface is flat, (b) is an example in which the surface is convex, and (c) is an example in which the surface is concave. Fig. 2 is an explanatory diagram showing the procedure for welding with three electrodes. (a) is a front view, and (b) is a top view. Fig. 3 is an explanatory diagram showing a typical example of hot cracking that occurs in a weld metal layer. Fig. 4 is an explanatory diagram showing the relationship between the width of the weld bead and the current value range of the third electrode.
[0014] The present invention will be specifically described below.
[0015] The present invention is directed to a steel plate having a thickness t of 22 mm or more, a groove angle θ of 25° or less, and a bottom groove gap G 0 : A narrow gap gas shielded arc welding method for joining by narrow gap multi-layer welding of 7 mm to 18 mm. Note that the term "steel plate" here includes thick steel material, thick plate steel material, etc.
[0016] [Thickness t of steel plate: 22 mm or more] The thickness t of the steel plate 1 is 22 mm or more. If the thickness t is less than 22 mm, in a conventional V-groove, increasing the groove angle to reduce the groove gap may result in a smaller groove cross-sectional area than the groove targeted by the present invention, and the V-groove may result in highly efficient welding with a smaller deposition amount. Preferably, the thickness t is 30 mm or more.
[0017] Furthermore, since the plate thickness of steel structures, including special structures, is 200 mm or less, in the present invention, it is preferable that the upper limit of the plate thickness t of the steel plate is set to 200 mm.
[0018] The present invention can be applied to various steel plates ranging from mild steel plates to high-tensile steel plates of 780 MPa class. 590 MPa class high-tensile steel plates can also be welded without preheating.
[0019] [Groove angle θ: 25° or less] The groove shape used in the present invention is a V-shaped groove (including an I-shaped groove (θ = 0°)) having a gap at the bottom, and is a narrow groove. An example of the groove shape is shown in FIG. 1. Here, 1 is the steel plate (base material) and 2 is the groove surface. The smaller the groove cross-sectional area of the groove portion of the steel plate, the faster and more efficient welding becomes possible, but defects such as poor fusion are more likely to occur. Furthermore, when the groove angle θ of the groove portion exceeds 25°, it can be performed using conventional construction methods. For this reason, the present invention targets narrow grooves with a groove angle θ of 25° or less, which are difficult to perform using conventional construction methods and are expected to be even more efficient. In a V-shaped groove, when the groove angle θ is 0°, it is called an I-shaped groove, and in terms of the amount of welding, this 0° case is the most efficient. However, since the groove may close during welding due to welding thermal distortion, it is preferable to set the groove angle θ according to the plate thickness t in anticipation of this. When the plate thickness t exceeds 100 mm, the upper limit of the preferable range is preferably 10°. A more preferable range of the included angle θ is 5° to 10°.
[0020] [Bottom groove gap G 0 The smaller the groove of the steel plate, the faster and more efficient the welding becomes, but defects such as insufficient fusion tend to occur. In addition, the bottom groove gap G, which is the gap between the bottoms of the grooves (groove width) before welding begins, 0 Therefore, in the present invention, the bottom groove gap G is set to 18 mm, which is expected to be even more efficient than the conventional welding method. 0 On the other hand, the bottom groove gap G 0 If the gap is less than 7 mm, it may be difficult to perform welding using three electrodes. 0 is in the range of 7 mm to 18 mm, preferably in the range of 8 mm to 12 mm.
[0021] [Multi-layer welding] In the present invention, the first layer and each layer after the second layer are joined by multi-layer welding using three electrodes using the narrow groove described above, and a welding method is provided that is particularly suitable for welding the second layer and beyond. Here, if the number of layers in the multi-layer welding is n, the layers are individually numbered from the first layer (first layer) to the nth layer (final layer), and if an intermediate layer is numbered as number i, the layer immediately before that is number i-1.
[0022] [Electrode Current Value] First, the current value I 1 and the current value I of the second electrode 2 is set to the range of 260 A to 360 A. The current value I of the first electrode and the second electrode 1 and I 2 If the current is less than 260 A, the groove face cannot be sufficiently melted, and there is a high possibility of incomplete fusion. On the other hand, if the current exceeds 360 A, the height of the weld bead increases, resulting in a vertically elongated bead, which increases the risk of hot cracking. Therefore, the current value I of the first electrode 1 and the current value I of the second electrode 2 The range of both is set to 260 A to 360 A. Preferably, it is set to 270 A to 340 A.
[0023] Next, the current value I of the third electrode 3 is controlled for each layer of multi-layer welding based on the relationship with the width of the weld bead of each layer. The inventors have found that this can suppress hot cracking that occurs in each weld layer, which is an object of the present invention. Specifically, the current value I of the third electrode of the i-th layer 3 i is set to a range that satisfies the following formula (1): 3 i ≦30×G i-1 -10 ... (1) where I 3 i : Current value [A] of the third electrode of the i-th layer, G i-1 : Width [mm] of the weld bead formed by welding the layer immediately before the i-th layer (i-1th layer), where i is a natural number of 2 or greater.
[0024] Current value I of the third electrode 3 i When the weld bead width G becomes larger, the height of the weld bead becomes larger and the bead becomes longer, which increases the risk of hot cracking.i is the width G of the weld bead formed by welding one layer before (i-1th layer) i-1 The width of the weld bead increases with the number of layers due to the influence of the current value of the third electrode. Based on this, the relationship between the width of the weld bead and the current value of the third electrode was examined, and it was found that the range shown in Figure 4 is favorable, from which the above formula (1) was derived. In other words, within the range satisfying formula (1), it is possible to suppress the formation of a vertically elongated weld bead, and an excellent effect of preventing hot cracking was obtained.
[0025] [First Layer Welding Conditions] The narrow gap gas-shielded arc welding method according to the present invention is characterized in that the current value for each electrode is controlled as a condition applied to the second layer and thereafter. Therefore, the first layer welding conditions of the welding method according to the present invention are not particularly limited. However, the welding conditions for the second layer and thereafter applied by the present invention can be applied as they are to the welding conditions for the first layer. Furthermore, the current value I of the third electrode in the first layer welding 3 1 , the current value I of the first electrode 1 and the current value I of the second electrode 2 It may be in the same range (260A to 360A).
[0026] The following describes the preferred welding conditions for the second and subsequent layers. The following conditions are also preferred for the first layer.
[0027] [Electrode Polarity] If the first and second electrodes have the same polarity (for example, both the first and second electrodes are wire-positive), the mutual electromagnetic force causes the arcs to be directed inward, concentrating heat at the center of the groove. This results in insufficient melting at the groove surface. On the other hand, if one of the first and second electrodes is wire-negative (positive polarity) and the other is wire-positive (reverse polarity), and the arrangement of the first and second electrodes is appropriately controlled, the magnetic fields generated by the welding currents generate strong outward electromagnetic forces, causing the arcs to repel each other. As a result, sufficient melting depth can be achieved at the groove surface. For these reasons, in the present invention, it is preferable to use wire-negative (positive polarity) and wire-positive (reverse polarity) for one of the first and second electrodes. The polarity of the third electrode 5 is not particularly limited and may be either wire-negative (positive polarity) or wire-positive (reverse polarity).
[0028] [Arrangement of the first and second electrodes] In narrow-gap multi-pass welding, when one pass is performed per layer, welding heat tends to concentrate at the center of the groove with one electrode, resulting in insufficient melting at the groove face of the steel plate, and defects due to incomplete fusion (cold lap) and spatter and slag inclusion on the groove face are likely to occur. In particular, in the first layer welding, the temperature of the steel plate is low and the melting depth is small, so defects due to incomplete fusion are likely to occur. Therefore, in the present invention, as shown in Figure 2, it is preferable to arrange the first electrode 3 and the second electrode 4 of the three electrodes at positions along a predetermined parallel welding line 8. Note that 6 denotes a backing material, 7 denotes a molten pool, and M 1 is the first layer of weld metal (first layer), M 2 is the second layer of weld metal.
[0029] [Distance a between welding wire tips of first electrode and second electrode: 5 mm to 16 mm] The distance a between the tips of welding wires 3 b, 4 b supplied from power feed tips 3 a, 4 a at the tip of each welding torch of first electrode 3 and second electrode 4 (hereinafter also referred to simply as the "distance between first and second electrodes"; see FIG. 2( b)) is preferably adjusted to a range of 5 mm to 16 mm. Note that the "distance between welding wire tips" here refers to the distance between the centers of the welding wire tips of each electrode.
[0030] If the distance a between the first and second electrodes is less than 5 mm, the current (electrons) flowing between the electrodes reduces the heat of the arc itself, preventing sufficient melting of the groove surface 2. On the other hand, if the distance a between the first and second electrodes exceeds 16 mm, the outward electromagnetic force between the electrodes decreases inversely proportional to the distance. This prevents the arc from repelling the inward electromagnetic force generated by the current flowing through the groove surface 2, causing the arcs to turn inward and heat to concentrate at the center of the groove. As a result, sufficient melting of the groove surface 2 is not achieved. Furthermore, in narrow-gap welding, suppressing welding defects caused by spatter adhesion to the groove surface 2 is an issue. However, the first electrode 3 and the second electrode 4 are arranged along predetermined parallel welding lines 8, 8, one of which is wire-negative (positive polarity) and the other is wire-positive (reverse polarity), and the distance a between the first and second electrodes is adjusted to a range of 5 mm to 16 mm. As a result, the spatter is absorbed by the molten metal, and adhesion of spatter to the groove faces is suppressed, resulting in a sound weld. For these reasons, it is preferable to adjust the distance a between the first and second electrodes to the range of 5 mm to 16 mm.
[0031] [Angle α of the Line Connecting the Tips of the Welding Wires of the First and Second Electrodes: 60° or Less] In the present invention, melting of the groove face is ensured by utilizing the repulsion of the arc. However, if the angle α of the line connecting the tips of the welding wires of the first electrode 3 and the second electrode 4 with respect to the direction perpendicular to the weld line exceeds 60°, a sufficient repulsive force of the arc cannot be obtained, and sufficient melting cannot be achieved at the groove face. Therefore, the angle α of the line connecting the tips of the welding wires of the first electrode 3 and the second electrode 4 with respect to the direction perpendicular to the weld line 8 (hereinafter also referred to simply as the "first-second electrode arrangement angle"; see FIG. 2(b)) is preferably 60° or less. More preferably, it is 55° or less. Note that the first-second electrode arrangement angle α may be 0°.
[0032] [Welding wire diameter: 1.0 mm to 1.6 mm] Welding wire for narrow-gap gas-shielded arc welding is generally manufactured with a diameter in the range of 0.6 mm to 2.0 mm. However, when welding with the same current, the thinner the wire diameter, the higher the deposition rate due to Joule heat. Therefore, to achieve highly efficient welding, it is preferable to select a relatively thin wire diameter. On the other hand, if the wire diameter is too thin, the wire will soften due to Joule heat, making the welding unstable. For this reason, the diameter of the welding wire used in the present invention is preferably in the range of 1.0 mm to 1.6 mm.
[0033] [Distance b between welding wire tips of second electrode and third electrode: 10 mm to 100 mm] The distance b between the tips of welding wires 4b, 5b supplied from power feed tips 4a, 5a at the tip of the welding torch of each of second electrode 4 and third electrode 5 (hereinafter also simply referred to as the "second-third electrode distance"; see FIG. 2(b)) is preferably in the range of 10 mm to 100 mm. This is because hot cracking resistance is improved by setting the distance b in this range. More preferably, it is 12 mm to 80 mm.
[0034] [Arrangement of the third electrode] In the first layer welding, the weld buildup height is the bottom groove gap G 0 If the gap exceeds , the risk of hot cracking increases. To avoid this, it is effective to position the third electrode 5 at the center of the groove behind the first electrode 3 and the second electrode 4. This also makes it possible to further reduce the number of layers, greatly reducing the risk of stacking defects in multi-layer welding. Note that the "groove center" here refers to the distance from the center of the groove to the bottom groove gap G 0 A range of ±10% is permitted.
[0035] [Shielding gas: 20% by volume or more of CO 2 The amount of oxygen in the weld metal is also greatly affected by the shielding gas composition. Therefore, the shielding gas used in the narrow gap gas-shielded arc welding according to the present invention is a mixed gas containing CO 2 It is preferable to use a mixed gas containing 20% by volume or more of CO gas and the remainder being an inert gas such as Ar. 2Gas: 100% by volume of a single gas. In the present invention, it is preferable to increase the oxygen concentration in the weld metal, which controls the flow of the weld metal, and direct the convection of the weld metal from the center outward, thereby stably increasing the fusion depth at the bottom of the thick steel plate in the groove.
[0036] [REM Content of Welding Wire: 0.005% by Mass to 0.060% by Mass] REM (rare earth element) is an element effective in reducing the size of inclusions in the weld metal and improving toughness during welding. Furthermore, when welding is performed using a welding wire containing added REM and supplied to a positive electrode, droplet size can be reduced and transfer can be stabilized. This refinement of droplet transfer suppresses the generation of spatter and enables stable gas-shielded arc welding even with a positive electrode. For these reasons, in the present invention, it is preferable to supply a steel wire containing 0.005% by mass to 0.060% by mass of REM (rare earth element) to a positive electrode. Note that elements other than REM (rare earth element) are generally contained in appropriate amounts depending on the grade (steel type) of the welding wire, as specified in JIS Z 3312.
[0037] If the REM (rare earth element) content is less than 0.005% by mass, it is difficult to achieve the above-mentioned droplet refinement and stable transfer. On the other hand, if the REM (rare earth element) content exceeds 0.060% by mass, cracks occur during the wire manufacturing process, making it difficult to manufacture the welding wire. Therefore, the REM (rare earth element) content is preferably in the range of 0.005% to 0.060% by mass. More preferably, it is in the range of 0.010% to 0.055% by mass.
[0038] [Other Welding Conditions] In the present invention, the welding conditions other than those described above do not need to be particularly limited and may be set in accordance with established methods, such as a welding voltage of 32 V to 37 V, a welding speed of 30 cm / min to 90 cm / min, a welding wire extension length of 15 mm to 30 mm, and a welding heat input per pass of 10 kJ / cm to 50 kJ / cm.
[0039] Furthermore, by satisfying the other welding conditions shown below, hot cracking can be further suppressed and welding can be performed more efficiently.
[0040] [Welding wire feed angle φ relative to the bottom groove: 0° to 15° relative to the perpendicular] The arc has directionality and tends to point in the direction that the tip of the electrode (welding wire) points. To effectively utilize this arc direction in melting the groove surface, it is advantageous to point the electrode tip toward the groove surface, and the direction that the electrode tip points varies greatly depending on the feed angle φ of the welding wire supplied from the power feed tip at the tip of the welding torch. The feed angle φ of the welding wire supplied from the power feed tip at the tip of the welding torch relative to the bottom groove is shown in Figure 2(a).
[0041] When the feed angle φ of the welding wires 3b and 4b supplied from the power feed tips 3a and 4a at the tip of the welding torch relative to the bottom groove is less than 0° relative to the vertical, the current flows through a path with less resistance. As a result, the arc creeps up the wire electrode (arc creep), making it difficult to maintain the desired fusion at the groove surface 2, particularly at the bottom. On the other hand, when the feed angle φ of the welding wire supplied from the power feed tip relative to the bottom groove exceeds 15° relative to the vertical, the arc is directed too far toward the groove surface 2, resulting in a convex weld bead shape. This results in insufficient arc melting in the first and subsequent layers of welding, making welding defects more likely to occur. For this reason, the feed angle φ of the welding wires 3b and 4b of the first and second electrodes 3 and 4 relative to the bottom groove is preferably in the range of 0° to 15° relative to the vertical. More preferably, it is 5° to 12°.
[0042] The feed angle φ of the welding wire of the first electrode 3 and the second electrode 4 relative to the bottom groove is the same as the inclination of the power feed tips 3a and 4a, particularly the tip of the power feed tip. Therefore, the feed angle φ of the welding wire can be controlled by the inclination of the tip of the power feed tip. Note that the feed angle φ is defined as positive in the direction toward the groove face. The perpendicular line here refers to the perpendicular line to the bottom groove.
[0043] [Distance d between the side end of the welding wire tip and the bottom groove surface: 0.1 mm to 3.0 mm] As shown in FIG. 2(a), the distance d between the side end of the welding wire tip of the first electrode 3 and the second electrode 4 and the bottom of the groove surface 2 is preferably in the range of 0.1 mm to 3.0 mm. If the distance d between the side end of the tip of the welding wire 3b and 4b at the bottom groove and the bottom groove surface 2 is less than 0.1 mm, an arc will be generated between the top of the wire and the groove surface 2, and the bottom groove surface 2 will not be melted efficiently. On the other hand, if the distance d exceeds 3.0 mm, the arc will be separated from the groove surface 2, and the groove surface 2 will not be melted efficiently. For this reason, the distance d between the side end of the welding wire tip and the bottom groove surface is preferably 0.1 mm to 3.0 mm. More preferably, it is 0.5 mm to 2.0 mm, and even more preferably, it is 0.5 mm to 1.0 mm. The "side end of the tip of the welding wire" refers to the side end of the steel plate bottom that is to be melted by each electrode and that is closer to the groove face 2.
[0044] [Curvature Radius of Welding Wire Feed to Power Feed Tip: 150 mm to 500 mm] In the present invention, a power feed tip with a bent tip is used to control the feed angle φ of the welding wires 3b and 4b fed from the power feed tips 3a and 4a at the welding torch tips of the first electrode 3 and the second electrode 4. In this case, the welding wire passes through the bent power feed tip. To ensure smoother passage, it is preferable to pre-bend the welding wire using a so-called three-point roller or the like. If the curvature radius of the welding wire is less than 150 mm, the wire feed resistance increases, making it difficult to feed the welding wire stably and maintaining an arc. On the other hand, if the curvature radius of the welding wire exceeds 500 mm, the bending of the power feed tip is ineffective in reducing the wire feed resistance, making it difficult to feed the welding wire stably and maintaining an arc. In view of the above, the radius of curvature of the welding wires 3b and 4b fed to the power feed tips 3a and 4a of the first electrode 3 and the second electrode 4 is preferably 150 mm to 500 mm, and more preferably 175 mm to 475 mm.
[0045] The present invention will be further described below with reference to examples. However, the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention.
[0046] Tests were conducted in which grooves were prepared by gas cutting, multi-layer welding was performed on steel plates (base materials) with individual groove shapes, and the groove shapes of each layer from the second layer onwards were measured (Joints No. 1 to 12). Table 1 shows the groove shapes and the welding conditions for each layer from the first electrode to the third electrode from the second layer onwards.
[0047] The weld metal layer was cut at each welded layer, and the cross section of the weld was corroded with nital, after which the occurrence of hot cracking was confirmed for each layer. The results are also shown in Table 1.
[0048] Here, the conditions other than the welding conditions listed in Table 1 are as follows: The steel type (grade) of the steel plate used was 490 MPa class steel to 590 MPa class steel, and the plate thickness t of the steel plate was 30 mm to 100 mm. The steel type (grade) of the welding wire used was YGW18, and the welding wire diameter was 1.2 mm.
[0049] The distance a between the first and second electrodes is 14 mm, the distance b between the second and third electrodes is 16 mm, and the first and second electrode arrangement angle α is 55°.
[0050] The welding speed is 60 cm / min, and the welding heat input is 28 kJ / cm to 41 kJ / cm.
[0051] The REM content of the welding wire used for the negative wire electrode is 0.025 mass % to 0.030 mass %.
[0052] The feed angle φ of the welding wire was 8°, the distance d between the tip end of the welding wire and the groove surface was 0.5 mm, and the radius of curvature of the welding wire was 300 mm.
[0053]
[0054] In all of the inventive examples, no hot cracking was observed even when narrow-gap multi-layer welding was performed using three-electrode welding. On the other hand, in the comparative examples outside the scope of the present invention, hot cracking occurred, and a sound narrow-gap gas-shielded arc-welded joint was not obtained.
[0055] REFERENCE SIGNS LIST 1 Steel plate (base metal) 2 Groove face 3 First electrode 4 Second electrode 5 Third electrode 6 Backing material 3a, 4a, 5a Power contact tip 3b, 4b, 5b Welding wire 7 Welding base 8 Weld line t Plate thickness, θ Groove angle C Hot crack M Weld metal M 1 First layer, M 2 2nd layer, M i-1 The layer immediately before the i-th layer, M i i-th layer G 0 Bottom groove gap, G 1 Width of the first layer weld bead, G i-1 Width of the weld bead of the i-1th layer, G i Width of weld bead of layer i
Claims
1. Steel plate with a thickness of 22 mm or more, groove angle θ of 25° or less, bottom groove gap G 0 A narrow gap gas shielded arc welding method applied to the second layer and thereafter in narrow gap multi-layer welding of 7 mm to 18 mm, in which the multi-layer welding is performed by three electrodes, and the current value I of the first electrode and the second electrode is 1 and I 2 is in the range of 260 A to 360 A, and the current value I 3 i A narrow gap gas-shielded arc welding method in which [A] is in a range that satisfies the following formula (1). 3 i ≦30×G i-1 -10 ... (1) Here, I 3 i : Current value [A] of the third electrode of the i-th layer, G i-1 i: Width [mm] of the weld bead formed by welding the layer before the i-th layer (i-1th layer), where i is a natural number of 2 or more.
2. The narrow gap gas-shielded arc welding method according to claim 1, wherein one of the first electrode and the second electrode is wire negative (positive polarity) and the other is wire positive (reverse polarity), the distance a between the tips of the welding wire supplied from the power feed tips at the tip of the welding torch of the first electrode and the second electrode is in the range of 5 mm to 16 mm, the angle α of a straight line connecting the welding wire tips of the first electrode and the second electrode with respect to a direction perpendicular to the weld line is 60° or less, the diameter of the welding wire of all the electrodes is in the range of 1.0 mm to 1.6 mm, and the distance b between the tips of the welding wire supplied from the power feed tips at the tip of the welding torch of the second electrode and the third electrode is in the range of 10 mm to 100 mm.
3. A narrow gap gas-shielded arc welding method according to claim 1 or 2, wherein the third electrode is positioned in the center of the groove behind the first electrode and the second electrode.
4. Shielding gas containing 20% or more CO by volume 2 The narrow gap gas-shielded arc welding method according to any one of claims 1 to 3, wherein a mixed gas containing a gas is used.
5. A narrow gap gas-shielded arc welding method according to any one of claims 1 to 4, wherein at least one of the welding wires used for the positive electrode contains 0.005% by mass to 0.060% by mass of REM (rare earth element).
Citation Information
Patent Citations
Narrow-gap gas shielded arc welding method
JP6137053B2
Gas shield arc welding of two muliti layer cladded electrodes
JP1999129072A
Tandem welding apparatus, and tandem first pass welding method
JP2011031250A
Narrow groove gas-shield arc-welding method
JP2015223605A