Glass fiber, glass fiber woven fabric, and glass fiber-reinforced resin composition
Glass fibers with specific SiO2, TiO2, and Al2O3 compositions address the heat generation and handling challenges in electronic devices by achieving low dielectric loss tangents and improved handleability, suitable for high-frequency applications.
Patent Information
- Application Number
- PCT/JP2024/013780
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-04-03
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional glass fibers used in electronic devices generate excessive heat due to high dielectric loss, which is a problem exacerbated by increasing alternating current frequencies, and they often lack sufficient handling properties for industrial processing and transportation.
Developing glass fibers with a composition of SiO2, TiO2, and Al2O3, where SiO2 content ranges from 92.50 to 99.99% and TiO2 and Al2O3 content ranges from 0.01 to 5.00% and 0.00 to 2.50% respectively, with specific ratios to achieve a low dielectric loss tangent and improved handling properties, characterized by tensile breaking stress within certain ranges and specific formulas.
The glass fibers exhibit extremely low dielectric loss tangents and excellent handleability, enabling their use in high-frequency electronic devices without heat generation issues and facilitating industrial processing.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Glass fiber, glass fiber fabric, and glass fiber reinforced resin composition
[0001] The present invention relates to a glass fiber, a glass fiber fabric, and a glass fiber reinforced resin composition.
[0002] Conventionally, glass fibers have been widely used in various applications to improve the strength of resin molded products, and the resin molded products are used in components such as housings or printed wiring boards of electronic devices such as servers, smartphones, and laptops.
[0003] Generally, dielectrics such as glass absorb part of the energy of an AC electric field as heat (this is called dielectric loss), and therefore, when the resin molded product is used as a housing or part of the electronic device, there is a problem that the resin molded product generates heat.
[0004] Here, the dielectric loss absorbed by the glass is proportional to the dielectric constant and dielectric loss tangent determined by the components and structure of the glass, and is expressed by the following formula: W = kf × ε 1/2 ×tan δ
[0005] Here, W is the dielectric loss, k is a constant, f is the frequency, ε is the dielectric constant, and tanδ is the dielectric loss tangent. From the above formula, it can be seen that the larger the dielectric constant and the dielectric loss tangent, and the higher the frequency, the larger the dielectric loss and the greater the heat generation of the resin molded product.
[0006] In recent years, as the frequency of the alternating current used in the electronic devices (f in the above formula) has been increasing, there has been a demand for glass fibers used in the housings or parts of the electronic devices to have lower dielectric constants and lower dielectric dissipation factors in order to reduce dielectric loss. Furthermore, compared to the dielectric constant ε, which is raised to the power of 1 / 2 in the above formula, a reduction in the dielectric dissipation factor has a greater impact on reducing dielectric loss energy, and therefore there is a particular demand for achieving a lower dielectric dissipation factor.
[0007] As a glass fiber having an extremely low dielectric tangent, SiO 2 There is known a glass fiber having a silica glass composition in which the content of SiO is 90% by mass or more, particularly 99% by mass or more (see, for example, Patent Document 1). 2As a method for producing glass fibers having a glass composition with a high content of SiO 2 From a mother glass composition containing components that are easily soluble in acid other than SiO 2 A method is known in which components other than the above are dissolved in an acid solution (see, for example, Patent Document 2).
[0008] Here, an extremely low dielectric loss tangent means that the dielectric loss tangent of the glass fiber at a measurement frequency of 28 GHz is less than 0.0010. The dielectric loss tangent of the glass fiber at a measurement frequency of 28 GHz can be measured by the method described below.
[0009] JP 2009-263569 JP 9-169548
[0010] However, the SiO content relative to the total amount of the glass composition obtained by the method of Patent Document 2 is 2 Glass fibers with a high content of do not necessarily have an extremely low dielectric tangent, and even if they have an extremely low dielectric tangent, there is a disadvantage that glass fiber products containing such glass fibers, particularly light, thin, short and small glass fiber products, especially glass fiber woven fabrics, may not have sufficient handleability to withstand industrial processing and transportation.
[0011] An object of the present invention is to eliminate such inconveniences and to provide a glass fiber having an extremely low dielectric tangent and sufficient handleability.
[0012] Another object of the present invention is to provide a glass fiber fabric and a glass fiber reinforced resin composition containing the glass fiber of the present invention.
[0013] To achieve this object, the glass fiber of the present invention contains SiO in the range of 92.50 to 99.99 mass % based on the total amount of the glass composition. 2 and TiO in the range of 0.01 to 5.00 mass%. 2 and Al in the range of 0.00 to 2.50 mass%. 2 O 3 and a glass composition containing the glass fiber, the tensile breaking stress of which is in the range of 1.0 to 100.0 MPa, and SiO 2 The content S of TiO 2The glass fiber is characterized in that the content T of the glass fiber and the tensile breaking stress BS of the glass fiber satisfy the following formula (1): 5.2≦BS×(T / (100−S)) 2 ≦ 33.8 ... (1)
[0014] The glass fiber of the present invention is SiO 2 , TiO 2 and Al 2 O 3 The glass fiber has a glass composition in which the content of each of the above falls within the above range, the tensile breaking stress of the glass fiber falls within the above range, and the S, T, and BS satisfy the formula (1), whereby the glass fiber can have an extremely low dielectric tangent and can be made to have sufficient handleability.
[0015] In addition, it is preferable that the S, T, and BS of the glass fiber of the present invention satisfy the following formula (2): 9.1≦BS×(T / (100−S)). 2 ≦ 33.5 ... (2)
[0016] When the S, T and BS satisfy the formula (2), the glass fiber of the present invention can more reliably have an extremely low dielectric tangent and excellent handleability.
[0017] In addition, it is preferable that the S, T, and BS of the glass fiber of the present invention satisfy the following formula (3): 20.1≦BS×(T / (100−S)). 2 ≦ 33.1 ... (3)
[0018] The glass fiber of the present invention has a particularly extremely low dielectric loss tangent and excellent handleability because S, T, and BS satisfy formula (3). Here, "having a particularly extremely low dielectric loss tangent" means that the dielectric loss tangent of the glass fiber at a measurement frequency of 28 GHz is 0.0005 or less. The dielectric loss tangent of the glass fiber at a measurement frequency of 28 GHz can be measured by the method described below.
[0019] The glass fiber woven fabric of the present invention is characterized by containing the glass fiber of the present invention described above.
[0020] The glass fiber reinforced resin composition of the present invention is characterized by containing the glass fiber of the present invention.
[0021] Next, the embodiment of the present invention will be described in more detail.
[0022] The glass fiber of this embodiment contains SiO in the range of 92.50 to 99.99 mass % based on the total amount of the glass composition. 2 and TiO in the range of 0.01 to 5.00 mass%. 2 and Al in the range of 0.00 to 2.50 mass%. 2 O 3 and a glass composition containing the glass fiber, the tensile breaking stress of which is in the range of 1.0 to 100.0 MPa, and SiO 2 The content S of TiO 2 The glass fiber content T and the tensile breaking stress BS of the glass fiber satisfy the following formula (1): 5.2≦BS×(T / (100−S)). 2 ≦ 33.8 ... (1)
[0023] According to the glass fiber of this embodiment, SiO 2 , TiO 2 and Al 2 O 3 The glass fiber has a glass composition in which the content of each of the above falls within the above range, the tensile breaking stress of the glass fiber falls within the above range, and the S, T, and BS satisfy the formula (1), whereby the glass fiber has an extremely low dielectric tangent and is able to have sufficient handleability, particularly handleability as a glass fiber fabric.
[0024] In the glass composition constituting the glass fiber of this embodiment, SiO 2 If the content of SiO in the glass fiber is less than 92.50 mass %, the dielectric loss tangent of the glass fiber cannot be reduced sufficiently. 2 If the content of exceeds 99.99 mass % based on the total amount of the glass composition, the glass fiber loses its flexibility, and handling properties, particularly handling properties as a glass fiber fabric, deteriorate.
[0025] In the glass composition constituting the glass fiber of this embodiment, from the viewpoint of achieving both a reduction in the dielectric loss tangent of the glass fiber and ease of handling of the glass fiber, SiO 2The content of is preferably in the range of 97.10 to 99.40 mass %, more preferably in the range of 98.10 to 98.90 mass %, based on the total amount of the glass composition.
[0026] In the glass composition constituting the glass fiber of this embodiment, TiO 2 If the content of TiO in the glass fiber is less than 0.01% by mass, the handling of the glass fiber, particularly the handling of the glass fiber fabric, will be deteriorated. 2 If the content of exceeds 5.00 mass % based on the total amount of the glass composition, the dielectric loss tangent of the glass fiber cannot be reduced sufficiently.
[0027] In the glass composition constituting the glass fiber of this embodiment, from the viewpoint of achieving both a reduction in the dielectric loss tangent of the glass fiber and ease of handling of the glass fiber, TiO 2 The content of is preferably in the range of 0.11 to 3.50 mass%, more preferably in the range of 0.31 to 1.94 mass%, even more preferably in the range of 0.51 to 1.80 mass%, particularly preferably in the range of 0.71 to 1.64 mass%, particularly preferably in the range of 0.72 to 1.44 mass%, particularly preferably in the range of 0.73 to 1.20 mass%, and most preferably in the range of 0.75 to 0.99 mass%, based on the total amount of the glass composition.
[0028] In the glass composition constituting the glass fiber of this embodiment, Al is 2 O 3 If the content exceeds 2.50 mass %, the dielectric loss tangent of the glass fiber cannot be reduced sufficiently.
[0029] In the glass composition constituting the glass fiber of this embodiment, from the viewpoint of achieving both a reduction in the dielectric loss tangent of the glass fiber and ease of handling of the glass fiber, Al 2 O 3The content of is preferably in the range of 0.00 to 0.34 mass%, more preferably in the range of 0.00 to 0.24 mass%, even more preferably in the range of 0.00 to 0.20 mass%, particularly preferably in the range of 0.00 to 0.14 mass%, particularly preferably in the range of 0.00 to 0.10 mass%, particularly preferably in the range of 0.00 to 0.09 mass%, and most preferably in the range of 0.01 to 0.09 mass%, based on the total amount of the glass composition.
[0030] The glass composition constituting the glass fiber of the present embodiment may contain, as impurities, oxides of Li, Na, K, Mg, Ca, B, P, Fe, Sn, Sr, Ba, Mn, Co, Ni, Cu, Cr, Mo, W, Ce, Y, La, Bi, Gd, Pr, Sc, or Yb in a range of less than 1.00 mass% in total, preferably less than 0.50 mass% in total, and more preferably less than 0.20 mass% in total, based on the total amount of the glass composition.
[0031] In particular, the glass composition constituting the glass fiber of this embodiment does not contain Li as an impurity. 2 O, Na 2 O.K. 2 O, MgO, CaO, B 2 O 3 , P 2 O 5 , FeO, Fe 2 O 3 , SnO 2 , SrO, BaO, CeO 2 , Y 2 O 3 , La 2 O 3 , Bi 2 O 3 , Gd 2 O 3 , Pr 2 O 3 , Sc 2 O 3 , or Yb 2 O 3When these elements are contained, the contents thereof are preferably each independently in the range of less than 0.40 mass%, more preferably in the range of less than 0.20 mass%, even more preferably in the range of less than 0.10 mass%, particularly preferably in the range of less than 0.05 mass%, particularly preferably in the range of less than 0.03 mass%, and most preferably in the range of less than 0.01 mass%, relative to the total amount of the glass composition.
[0032] The glass composition constituting the glass fiber of this embodiment contains F as an impurity. 2 , Cl 2 , S.O. 3 may be contained independently in a range of less than 0.20 mass%, preferably less than 0.10 mass%, more preferably less than 0.05 mass%, even more preferably less than 0.03 mass%, and most preferably less than 0.01 mass%, relative to the total amount of the glass composition.
[0033] The content of each component in the glass composition constituting the glass fiber of this embodiment can be measured using an ICP optical emission spectrometer for the light element Li, and a wavelength dispersive X-ray fluorescence analyzer for the other elements.
[0034] The measurement method can be as follows: First, glass fibers are pulverized and powdered to obtain glass powder. If organic matter is attached to the surface of the glass fibers, or if the glass fibers are contained in an organic material (resin) mainly as a reinforcing material, the glass fibers are used after removing the organic matter by, for example, heating in a muffle furnace at 300 to 650°C for about 0.5 to 24 hours.
[0035] Next, the light element Li is quantitatively analyzed using an ICP optical emission spectrometer after the glass powder is thermally decomposed with acid. Other elements are quantitatively analyzed using a wavelength-dispersive X-ray fluorescence analyzer after the glass powder is formed into a disk shape using a press. Specifically, quantitative analysis using a wavelength-dispersive X-ray fluorescence analyzer can be performed by preparing a calibration curve sample based on the results measured using the fundamental parameter method and analyzing it using the calibration curve method. The content of each component in the calibration curve sample can be quantitatively analyzed using an ICP optical emission spectrometer. The results of these quantitative analyses are converted into oxides to calculate the content and total amount of each component, and the content (mass %) of each component can be determined from these values.
[0036] In the glass composition constituting the glass fiber of this embodiment, TiO 2 Al content 2 O 3 The ratio of the content of Al 2 O 3 / TiO 2 From the viewpoint of further reducing the dielectric loss tangent of the glass fiber while maintaining the handleability of the glass fiber, particularly the handleability as a glass fiber fabric, Al is preferably in the range of 0.00 to 0.30, more preferably in the range of 0.00 to 0.20, even more preferably in the range of 0.00 to 0.14, and particularly preferably in the range of 0.03 to 0.12. 2 O 3 As the content of Al is lower, the dielectric loss tangent of the glass fiber decreases, but the handleability of the glass fiber tends to deteriorate. 2 O 3 If the content of TiO is low, the high-temperature viscosity of the glass fiber decreases, and the glass fibers tend to fuse together when fired at high temperatures, causing the glass fiber to lose its flexibility. 2 Similarly, as the content of Al is lower, the dielectric loss tangent of the glass fiber decreases, but the handling of the glass fiber tends to deteriorate. However, the degree of the effect of the content of Al on the dielectric loss tangent of the glass fiber and the handling of the glass fiber is 2 O 3That is, TiO 2 If the content of TiO is low, it becomes difficult to suppress the formation of cristobalite crystals in the glass fiber when fired at a high temperature, and the glass fiber becomes brittle. 2 Al content 2 O 3 The ratio of the content of Al 2 O 3 / TiO 2 ) is presumed to represent a ratio suitable for achieving both a reduction in the dielectric tangent of the glass fiber and ease of handling of the glass fiber, particularly ease of handling as a glass fiber fabric, as a combination of these trends.
[0037] In the glass composition constituting the glass fiber of this embodiment, the SiO 2 The content S of TiO in the glass fiber 2 The value of T / (100-S), calculated from the content T, is, for example, in the range of 0.05 to 1.00. From the viewpoint of achieving both a reduction in the dielectric tangent of the glass fiber and ease of handling of the glass fiber, the value of T / (100-S) is preferably in the range of 0.55 to 0.95, more preferably in the range of 0.60 to 0.94, even more preferably in the range of 0.66 to 0.90, particularly preferably in the range of 0.72 to 0.89, and most preferably in the range of 0.78 to 0.88.
[0038] If the tensile breaking stress of the glass fiber of this embodiment is less than 1.0 MPa, it will be difficult to process the glass fiber into glass fiber products such as the glass fiber fabric, etc. If the tensile breaking stress is more than 100.0 MPa, the dielectric loss tangent of the glass fiber will not be sufficiently reduced.
[0039] From the viewpoint of achieving both a reduction in the dielectric tangent of the glass fiber and processability into glass fiber products, the tensile breaking stress of the glass fiber of the present embodiment is preferably in the range of 8.8 to 60.0 MPa, more preferably in the range of 15.0 to 55.0 MPa, and even more preferably in the range of 25.0 to 50.0 MPa.
[0040] The tensile breaking stress of the glass fiber of this embodiment can be measured and calculated by the following method. When the measurement object is a glass fiber fabric made of the glass fiber of this embodiment as a warp, first, four rectangular test pieces, each 200 mm long in the warp direction and 25 mm long in the weft direction, are cut out from the glass fiber fabric. Next, adhesive tape is adhered to both ends of the test piece in the longitudinal direction so that the distance between the tabs is 100 mm, thereby preparing a test piece with tabs.
[0041] Next, the tensile strength of each test piece is measured using a tensile tester (manufactured by Toyo Seiki Seisakusho, Ltd., product name: Stroph VE20D) under conditions in accordance with JIS R 3420:2013, and the average value is calculated. The tensile breaking stress of the glass fiber is calculated using the obtained average tensile strength values by the following formula: Tensile breaking stress = average tensile strength value (unit: N / 25 mm) × density (unit: g / μm 3 ) / Mass per unit length of warp thread (unit: g / μm) / Weave density of warp thread (unit: threads / 25 mm)
[0042] In measuring and calculating the tensile breaking stress of the glass fiber of this embodiment, when the object to be measured is a glass fiber woven fabric having the glass fiber of this embodiment as the weft, the tensile breaking stress is calculated in the same manner as when the object to be measured is a glass fiber woven fabric having the glass fiber of this embodiment as the warp, except that four strip-shaped test pieces having a length of 200 mm in the weft direction and a length of 25 mm in the warp direction are cut out from the glass fiber woven fabric.
[0043] Furthermore, when the object to be measured is a glass fiber woven fabric having the glass fiber of this embodiment as the warp and weft, the tensile breaking stress is calculated in the same manner as when the object to be measured is a glass fiber woven fabric having the glass fiber of this embodiment as the warp. Except for cutting out two strip-shaped test pieces having a length of 200 mm in the warp direction and a length of 25 mm in the weft direction, and two strip-shaped test pieces having a length of 200 mm in the weft direction and a length of 25 mm in the warp direction from the glass fiber woven fabric,
[0044] When the object to be measured is a glass yarn or glass roving made of the glass fiber of this embodiment, the average value of the tensile strength is measured in the same manner as when the object to be measured is a glass fiber woven fabric made of the glass fiber of this embodiment, except that a test piece is used in which tabs are formed by adhering adhesive tape to both ends of the glass yarn or glass roving so that the length between the tabs is 100 mm, and the tensile breaking stress is calculated by the following formula: Tensile breaking stress = average value of tensile strength (unit: N) × density (unit: g / μm 3 ) / Mass per unit length of glass yarn or glass roving (unit: g / μm)
[0045] SiO in the glass composition constituting the glass fiber of this embodiment 2 the content S of TiO in the glass composition 2 The glass fiber content T and the tensile breaking stress BS of the glass fiber satisfy the following formula (1): 5.2≦BS×(T / (100−S)). 2 ≦ 33.8 ... (1)
[0046] In the glass fiber of this embodiment, BS × (T / (100 - S)) 2 If the value of BS×(T / (100−S)) is less than 5.2, the glass fiber will not have an extremely low dielectric tangent or will not have sufficient handleability, particularly handleability as a glass fiber fabric. 2 If the value of exceeds 33.8, the glass fiber of this embodiment cannot have an extremely low dielectric tangent. Here, the expression "the glass fiber of this embodiment has an extremely low dielectric tangent" means that the dielectric tangent of the glass fiber at a measurement frequency of 28 GHz is less than 0.0010.
[0047] The dielectric loss tangent of the glass fiber of this embodiment at a measurement frequency of 28 GHz can be measured by the following method. When the measurement object is a glass fiber fabric made of the glass fiber of this embodiment as warp and weft, two 5 cm x 5 cm test pieces are cut out from positions spaced apart from each other in the glass fiber fabric. Next, each test piece is heated, for example, in a muffle furnace at 300 to 650°C for about 0.5 to 24 hours to remove organic matter such as surface treatment agents containing silane coupling agents and sizing agents adhering to the glass fiber surfaces, as well as moisture.
[0048] Thereafter, the mass per unit area and density of each of the obtained test pieces were measured in accordance with JIS R 3420:2013, and the mass per unit area (unit: g / μm 2 ) / density (unit: g / μm 3 Next, for each test piece, a dielectric constant measuring device (manufactured by Anritsu Corporation, product name: MS46122B) was used to calculate the volume of the test piece using the calculated converted thickness, and the resonance frequency with and without the test piece inserted, as well as the Q value with and without the test piece inserted, were measured eight times at a measurement frequency of 28 GHz, and the average of the obtained measured values was calculated.
[0049] Next, the dielectric loss tangent (where tanδ) of the glass fiber is calculated using the average value of the obtained measured values and the following calculation formula (A) of the cylindrical cavity resonator method. In formula (A), α is a perturbation constant, f L is the resonance frequency when the test piece is inserted, f 0 is the resonant frequency when the test piece is not inserted, V is the volume of the cylindrical cavity resonator, ΔV is the volume of the test piece, and Q L is the Q value when the test piece is inserted, Q 0 means the Q value when the test piece is not inserted.
[0050]
[0051] When the object to be measured is a glass yarn or a glass roving made of the glass fiber of this embodiment, the dielectric loss tangent of a glass fiber fabric obtained by weaving the glass yarn or the glass roving is measured in the same manner as when the object to be measured is a glass fiber fabric made of the glass fiber of this embodiment.
[0052] Furthermore, when the object to be measured is a glass fiber woven fabric containing a glass yarn or glass roving made of the glass fiber of this embodiment as part of the warp or weft, the glass yarn or glass roving made of the glass fiber of this embodiment is extracted from the glass fiber woven fabric to be measured, and the dielectric loss tangent of the extracted glass yarn or glass roving is measured in the same manner as in the case where the object to be measured is a glass yarn or glass roving made of the glass fiber of this embodiment.
[0053] Here, the higher the BS value, the easier it is to handle the glass fiber, particularly as a glass fiber fabric, but the dielectric loss tangent of the glass fiber tends to increase. On the other hand, the lower the BS value, the worse the handleability of the glass fiber, particularly as a glass fiber fabric. On the other hand, the higher the T / (100-S) value, the higher the dielectric loss tangent of the glass fiber tends to increase, and the lower the T / (100-S) value, the lower the dielectric loss tangent of the glass fiber tends to decrease. BS x (T / (100-S)) 2 It is presumed that the value of reflects these trends and indicates the balance between the handleability of the glass fiber, particularly the handleability as a glass fiber fabric, and the dielectric loss tangent of the glass fiber.
[0054] In the glass fiber of this embodiment, it is preferable that S, T, and BS satisfy the following formula (2): 9.1≦BS×(T / (100−S)). 2 ≦ 33.5 ... (2)
[0055] In the glass fiber of the present embodiment, when S, T, and BS satisfy the formula (2), the glass fiber can more reliably have an extremely low dielectric tangent and excellent handleability, particularly handleability as a glass fiber fabric.
[0056] In the glass fiber of this embodiment, it is more preferable that S, T, and BS satisfy the following formula (3): 20.1≦BS×(T / (100−S)). 2 ≦ 33.1 ... (3)
[0057] In the glass fiber of this embodiment, when S, T, and BS satisfy the formula (3), the glass fiber has a particularly extremely low dielectric tangent and excellent handleability, particularly handleability as a glass fiber fabric. Here, the expression "the glass fiber of this embodiment has a particularly extremely low dielectric tangent" means that the dielectric tangent of the glass fiber at a measurement frequency of 28 GHz is 0.0005 or less.
[0058] The glass fiber of this embodiment can be formed, for example, as follows. First, glass raw materials are mixed to obtain a mother glass composition based on the components contained in the ore that will become the glass raw material, the content of each component, and the amount of volatilization of each component during the melting process. In the glass fiber of this embodiment, the mother glass composition contains SiO in the range of 45.0 to 65.0 mass % with respect to the total amount of the glass composition. 2 and Al in the range of 5.0 to 20.0 mass% 2 O 3 and TiO in the range of 0.1 to 3.0 mass%. 2 and a total of 10 to 40 mass% of CaO, MgO, SrO, and B. 2 O 3 and ZrO 2 and CaO, MgO, SrO, B 2 O 3 and ZrO 2 The ratio of the content of CaO to the total content of the above is in the range of 0.10 to 1.00.
[0059] Next, the prepared glass raw material (glass batch) is supplied to a melting furnace and melted at a temperature range of 1000 poise or higher, specifically, at a temperature in the range of 1450 to 1650°C. Next, the glass batch (molten glass) melted at the temperature range is discharged from 10 to 8000 nozzle tips or holes in a bushing controlled at a predetermined temperature. The discharged molten glass is then cooled and solidified while being wound up at high speed and stretched, thereby forming glass single fibers (glass filaments), and these glass filaments are bundled into one or more bundles to obtain a glass fiber bundle (glass strand).
[0060] Next, the obtained glass strands are further subjected to various known processes to obtain glass fiber products having a mother glass composition in various forms such as yarn, woven fabric, knitted fabric, nonwoven fabric including chopped strand mat and multiaxial nonwoven fabric, chopped strand, roving, powder, etc.
[0061] Next, the glass fiber product having the mother glass composition is placed in an acid solution and treated with the acid solution to remove SiO 2 constituting the mother glass composition. 2 The components other than the above are eluted to obtain an acid-eluted glass fiber. Here, the acid solution can be an acid having a pH of 3.0 or less, and examples of such acids include nitric acid, hydrochloric acid, and sulfuric acid. The concentration of the acid solution is preferably 0.2 to 20.0 mass %.
[0062] Furthermore, as a method for treating the glass fiber product with the acid solution, there can be mentioned a method in which the glass fiber product is placed in the acid solution and the acid solution is stirred or circulated. When the acid solution is stirred, the stirring speed is preferably in the range of 0.2 to 20 rps. When the acid solution is circulated, the flow rate is preferably in the range of 0.5 to 50 L / min. When treating the glass fiber product with the acid solution, the ratio of the mass of the glass fiber product to the volume of the acid solution is preferably in the range of 1.0 to 10.0 (g / L).
[0063] The treatment temperature when treating the glass fiber product with the acid solution is preferably in the range of 40 to 95° C. The treatment time when treating the glass fiber product with the acid solution is preferably in the range of 3 to 3,000 minutes.
[0064] The acid-eluted glass fiber is then calcined to obtain the glass fiber of this embodiment. The calcination can be carried out, for example, by placing the acid-eluted glass fiber in a heating device, raising the temperature from room temperature to a calcination temperature in the range of 600 to 1200°C at a temperature increase rate in the range of 1.0 to 100.0°C / min, calcining at the calcination temperature for a calcination time in the range of 0.8 to 80 hours, and then cooling from the calcination temperature to room temperature at a temperature decrease rate in the range of 1.0 to 100.0°C / min.
[0065] In the glass composition constituting the glass fiber of this embodiment, the above-mentioned value of T / (100-S) can be controlled by the base glass composition, the specific surface area of the glass fiber product comprising the base glass composition, and the treatment temperature and treatment time with the acid solution. 2 The content of CaO, MgO, SrO, B in the mother glass composition is increased. 2 O 3 and ZrO 2 The value of T / (100-S) can be increased by, for example, decreasing the ratio of the CaO content to the total content of the glass fiber composite. Furthermore, the value of T / (100-S) can be increased by, for example, decreasing the diameter of the glass filaments constituting the glass fiber product having the mother glass composition and increasing the specific surface area of the glass fiber product. Furthermore, the value of T / (100-S) can be increased by increasing the acid treatment temperature.
[0066] The tensile breaking stress BS of the glass fiber of this embodiment can be controlled by the specific surface area of the glass fiber product having the above-mentioned mother glass composition, the firing temperature and firing time of the firing treatment, and the above-mentioned value of T / (100-S). For example, the tensile breaking stress BS can be reduced by reducing the diameter of the glass filaments constituting the glass fiber product having the above-mentioned mother glass composition and increasing the specific surface area of the glass fiber product. Furthermore, the tensile breaking stress BS can be reduced by increasing the firing temperature and the firing time. Furthermore, the tensile breaking stress BS can be reduced by reducing the value of T / (100-S).
[0067] The glass filaments constituting the glass fiber of this embodiment usually have a true circular cross section and a diameter in the range of 2.0 to 35.0 μm. For applications requiring a low dielectric loss tangent, the glass filaments preferably have a diameter in the range of 2.5 to 9.0 μm, more preferably in the range of 2.8 to 6.0 μm, and even more preferably in the range of 3.0 to 4.5 μm.
[0068] When the glass filaments have an elliptical or oval cross section, the ratio of the major axis to the minor axis of the cross section (major axis / minor axis) is, for example, in the range of 2.0 to 10.0, and the fiber diameter when the cross section is converted into that of a perfect circle (converted fiber diameter) is, for example, in the range of 2.0 to 35.0 μm.
[0069] The glass fiber of this embodiment is typically in the form of a glass fiber bundle (glass strand) in which the glass filaments are bundled in a number ranging from 10 to 8,000, and has a mass per unit length in the range of 0.3 to 10,000.0 tex (g / km). For applications requiring a low dielectric loss tangent, the glass fiber of this embodiment is preferably configured in which the glass filaments are bundled in a number ranging from 20 to 450, and has a mass per unit length in the range of 0.5 to 90.0 tex. Furthermore, the glass fiber of this embodiment is more preferably configured in which the glass filaments are bundled in a number ranging from 35 to 410, and has a mass per unit length in the range of 0.9 to 69.0 tex. Furthermore, the glass fiber of this embodiment is even more preferably configured in which the glass filaments are bundled in a number ranging from 40 to 250, and has a mass per unit length in the range of 1.0 to 15.0 tex. Furthermore, it is particularly preferable that the glass fiber of this embodiment is configured by bundling the glass filaments in a number ranging from 50 to 220, and has a mass per unit length ranging from 1.1 to 7.0 tex.
[0070] The surface of the glass fiber of this embodiment may be coated with an organic substance for the purposes of improving the adhesion between the glass fiber and resin, improving the uniform dispersion of the glass fiber in a mixture of the glass fiber and resin or inorganic material, etc. Examples of such organic substances include starch, urethane resin, epoxy resin, vinyl acetate resin, acrylic resin, modified polypropylene (particularly carboxylic acid-modified polypropylene), and copolymers of (poly)carboxylic acid (particularly maleic acid) and unsaturated monomers. The glass fiber of this embodiment may also be coated with a resin composition containing, in addition to these resins, a silane coupling agent, a lubricant, a surfactant, etc. The glass fiber of this embodiment may also be coated with a treatment composition containing, without the above resins, a silane coupling agent, a surfactant, etc.
[0071] The glass fiber is coated with such a resin composition or treatment composition in a proportion of 0.03 to 2.0 mass % based on the mass of the glass fiber of this embodiment not coated with the resin composition or treatment composition. Coating of glass fiber with an organic substance can be carried out by applying a solution of the resin (hereinafter referred to as a resin solution) or a solution of the resin composition (hereinafter referred to as a resin composition solution) to the glass fiber of this embodiment in a filamentous form such as yarn or roving using a known method such as a roller applicator, and then drying the glass fiber to which the resin solution or the resin composition solution has been applied.
[0072] The coating of the glass fiber with the organic substance can be carried out by immersing the glass fiber of the present embodiment in the form of a woven fabric in a solution of the treatment composition (hereinafter referred to as the treatment composition solution), and then drying the glass fiber to which the treatment composition solution has been applied.
[0073] Furthermore, coating of glass fibers with the organic substance can be carried out by immersing the glass fibers of this embodiment in the form of chopped strands or powder in the resin solution or the resin composition solution, stirring the mixture, and then drying the glass fibers to which the resin solution or the resin composition solution has been applied.
[0074] Furthermore, the coating of glass fiber with the organic substance can be carried out by immersing the glass fiber of this embodiment in the form of a knitted fabric or a nonwoven fabric in the resin solution, the resin composition solution, or the treatment composition solution, and then drying the glass fiber to which the resin solution, the resin composition solution, or the treatment composition solution has been applied.
[0075] Examples of the silane coupling agent include aminosilane, chlorosilane, epoxysilane, mercaptosilane, vinylsilane, and (meth)acrylicsilane. In this embodiment, the silane coupling agents may be used alone or in combination of two or more.
[0076] Examples of aminosilanes include γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-N'-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and γ-anilinopropyltrimethoxysilane.
[0077] Examples of chlorosilane include γ-chloropropyltrimethoxysilane.
[0078] Examples of epoxy silanes include β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and γ-glycidoxypropyltrimethoxysilane.
[0079] Examples of mercaptosilane include γ-mercaptotrimethoxysilane.
[0080] Examples of vinylsilanes include vinyltrimethoxysilane and N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane.
[0081] Examples of (meth)acrylic silanes include γ-methacryloxypropyltrimethoxysilane.
[0082] Examples of lubricants include modified silicone oils, animal oils and their hydrogenated products, vegetable oils and their hydrogenated products, animal waxes, vegetable waxes, mineral waxes, condensates of higher saturated fatty acids and higher saturated alcohols, polyethyleneimines, polyalkylpolyamine alkylamide derivatives, fatty acid amides, and quaternary ammonium salts. In this embodiment, the lubricants may be used alone or in combination of two or more.
[0083] Examples of animal oils include beef tallow.
[0084] Examples of vegetable oils include soybean oil, coconut oil, rapeseed oil, palm oil, castor oil, etc.
[0085] Examples of animal waxes include beeswax and lanolin.
[0086] Examples of vegetable waxes include candelilla wax and carnauba wax.
[0087] Examples of mineral waxes include paraffin wax and montan wax.
[0088] Examples of the condensation products of higher saturated fatty acids and higher saturated alcohols include stearic acid esters such as lauryl stearate.
[0089] Examples of fatty acid amides include dehydration condensates of polyethylene polyamines such as diethylenetriamine, triethylenetetramine, and tetraethylenepentamine with fatty acids such as lauric acid, myristic acid, palmitic acid, and stearic acid.
[0090] Examples of the quaternary ammonium salt include alkyltrimethylammonium salts such as lauryltrimethylammonium chloride.
[0091] Examples of surfactants include nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants. In this embodiment, the surfactants may be used alone or in combination of two or more.
[0092] Examples of nonionic surfactants include ethylene oxide propylene oxide alkyl ethers, polyoxyethylene alkyl ethers, polyoxyethylene-polyoxypropylene block copolymers, alkyl polyoxyethylene-polyoxypropylene block copolymer ethers, polyoxyethylene fatty acid esters, polyoxyethylene fatty acid monoesters, polyoxyethylene fatty acid diesters, polyoxyethylene sorbitan fatty acid esters, glycerol fatty acid ester ethylene oxide adducts, polyoxyethylene castor oil ethers, hydrogenated castor oil ethylene oxide adducts, alkylamine ethylene oxide adducts, fatty acid amide ethylene oxide adducts, glycerol fatty acid esters, polyglycerin fatty acid esters, pentaerythritol fatty acid esters, sorbitol fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, polyhydric alcohol alkyl ethers, fatty acid alkanolamides, acetylene glycol, acetylene alcohol, ethylene oxide adducts of acetylene glycol, and ethylene oxide adducts of acetylene alcohol.
[0093] Examples of cationic surfactants include alkyldimethylbenzylammonium chloride, alkyltrimethylammonium chloride, alkyldimethylethylammonium ethyl sulfate, higher alkylamine salts, ethylene oxide adducts of higher alkylamines, condensates of higher fatty acids and polyalkylenepolyamines, salts of esters of higher fatty acids and alkanolamines, salts of higher fatty acid amides, imidazoline-type cationic surfactants, and alkylpyridinium salts. Examples of higher alkylamine salts include acetates and hydrochlorides.
[0094] Examples of anionic surfactants include higher alcohol sulfates, higher alkyl ether sulfates, α-olefin sulfates, alkylbenzene sulfonates, α-olefin sulfonates, reaction products of fatty acid halides and N-methyltaurine, dialkyl sulfosuccinates, higher alcohol phosphates, and phosphate salts of higher alcohol ethylene oxide adducts.
[0095] Examples of amphoteric surfactants include amino acid-type amphoteric surfactants, betaine-type amphoteric surfactants, and imidazoline-type amphoteric surfactants. Examples of amino acid-type amphoteric surfactants include alkali metal salts of alkylaminopropionic acid. Examples of betaine-type amphoteric surfactants include alkyldimethylbetaine.
[0096] The glass fiber fabric of this embodiment can be obtained by using a glass fiber fabric having the above-mentioned mother glass composition as the glass fiber product having the above-mentioned mother glass composition in the method for obtaining the glass fiber of this embodiment described above.Furthermore, the glass fiber fabric of this embodiment can also be obtained by using a glass yarn having the above-mentioned mother glass composition as the glass fiber product having the above-mentioned mother glass composition in the method for obtaining the glass fiber of this embodiment described above to obtain a glass yarn made of the glass fiber of this embodiment, and using this glass yarn as at least a part of the warp or weft, and weaving with a loom known per se.
[0097] Examples of the loom include a jet loom such as an air jet or water jet loom, a shuttle loom, a rapier loom, etc. In the glass fiber fabric of this embodiment, all of the warp and weft yarns are preferably made of the glass fiber of this embodiment.
[0098] Examples of weaves of the glass fiber fabric of this embodiment include plain weave, satin weave, sieve weave, and twill weave, and plain weave is preferred from the viewpoint of handling of the glass fiber fabric.
[0099] In the glass fiber woven fabric of this embodiment, the glass fiber of this embodiment described above is preferably formed by bundling glass filaments having a filament diameter in the range of 2.5 to 9.0 μm in a number in the range of 35 to 410, having a twist in the range of 0 to 1.0 turns / 25 mm, and having a mass per unit length in the range of 0.9 to 69.0 tex (g / 1000 m).
[0100] In the glass fiber fabric of the present embodiment, when the above-described glass fiber of the present embodiment is contained as a warp or a weft, the warp weave density is preferably in the range of 40 to 130 threads / 25 mm, and the weft weave density is preferably in the range of 40 to 130 threads / 25 mm.
[0101] The glass fiber fabric of this embodiment may be subjected to a surface treatment and a fiber-opening treatment.
[0102] The surface treatment can include a treatment in which the glass fiber fabric is immersed in a solution containing the silane coupling agent or the silane coupling agent and the surfactant, excess water is squeezed out, and the fabric is then heated and dried at a temperature in the range of 80 to 180°C for a time in the range of 1 to 30 minutes.
[0103] Examples of the opening treatment include a treatment for widening the yarn width of the warp and weft yarns by applying a tension in the range of 30 to 200 N to the warp yarns of the glass fiber fabric, such as opening by water jet pressure, opening by high-frequency vibration using a liquid as a medium, opening by pressure of a fluid having a surface pressure, or opening by pressure using a roll.
[0104] The glass fiber woven fabric of this embodiment has a fiber density of 6.0 to 180.0 g / m 2 It is preferable that the glass fiber fabric of this embodiment has a mass in the range of 7.0 to 80.0 g / m and a thickness in the range of 7.0 to 150.0 μm. 2 More preferably, the thickness of the insulating film is in the range of 8.0 to 80.0 μm.
[0105] In the glass fiber fabric of this embodiment, the width of the warp yarns is preferably in the range of 90 to 500 μm, and the width of the weft yarns is preferably in the range of 90 to 500 μm.
[0106] The glass fiber fabric of the present embodiment may have a surface treatment layer containing the silane coupling agent, or the silane coupling agent and the surfactant. When the glass fiber fabric of the present embodiment has the surface treatment layer, the surface treatment layer preferably has a mass of, for example, 0.03 to 1.50 mass% relative to the total mass of the glass fiber fabric including the surface treatment layer.
[0107] The glass fiber reinforced resin composition of this embodiment contains the glass fiber of this embodiment. Specifically, the glass fiber reinforced resin composition of this embodiment contains a thermoplastic or thermosetting resin, glass fiber, and other additives, and contains the glass fiber in a range of 10 to 90 mass% based on the total amount of the glass fiber reinforced resin composition. Furthermore, the glass fiber reinforced resin composition of this embodiment contains a resin in a range of 90 to 10 mass% based on the total amount of the glass fiber reinforced resin composition, and other additives in a range of 0 to 40 mass%.
[0108] Examples of the thermoplastic resin include polyethylene, polypropylene, polystyrene, styrene / maleic anhydride resin, styrene / maleimide resin, polyacrylonitrile, acrylonitrile / styrene (AS) resin, acrylonitrile / butadiene / styrene (ABS) resin, chlorinated polyethylene / acrylonitrile / styrene (ACS) resin, acrylonitrile / ethylene / styrene (AES) resin, acrylonitrile / styrene / methyl acrylate (ASA) resin, styrene / acrylonitrile (SAN) resin, methacrylic resin, polyvinyl chloride (PVC), polyvinylidene chloride (PVDC), polyamide, polyacetal, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polycarbonate, and the like. Examples of suitable polymers include carbonate, polyarylene sulfide, polyethersulfone (PES), polyphenylsulfone (PPSU), polyphenylene ether (PPE), modified polyphenylene ether (m-PPE), polyaryletherketone, liquid crystal polymer (LCP), fluororesin, polyetherimide (PEI), polyarylate (PAR), polysulfone (PSF), polyamideimide (PAI), polyaminobismaleimide (PABM), thermoplastic polyimide (TPI), polyethylene naphthalate (PEN), ethylene / vinyl acetate (EVA) resin, ionomer (IO) resin, polybutadiene, styrene / butadiene resin, polybutylene, polymethylpentene, olefin / vinyl alcohol resin, cyclic olefin resin, cellulose resin, and polylactic acid.
[0109] Examples of polyethylene include high density polyethylene (HDPE), medium density polyethylene, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), and ultra-high molecular weight polyethylene.
[0110] Examples of polypropylene include isotactic polypropylene, atactic polypropylene, syndiotactic polypropylene, and mixtures thereof.
[0111] Examples of polystyrene include general-purpose polystyrene (GPPS), which is an atactic polystyrene having an atactic structure, high impact polystyrene (HIPS), which is GPPS with a rubber component added, and syndiotactic polystyrene having a syndiotactic structure.
[0112] Examples of methacrylic resins include a homopolymer of one of acrylic acid, methacrylic acid, styrene, methyl acrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, and a fatty acid vinyl ester, or a copolymer of two or more of them.
[0113] Examples of polyvinyl chloride include vinyl chloride homopolymers polymerized by conventional methods such as emulsion polymerization, suspension polymerization, microsuspension polymerization, and bulk polymerization; copolymers of vinyl chloride monomers with copolymerizable monomers; and graft copolymers obtained by graft-polymerizing vinyl chloride monomers onto polymers.
[0114] Examples of polyamides include polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polytetramethylene adipamide (nylon 46), polytetramethylene sebacamide (nylon 410), polypentamethylene adipamide (nylon 56), polypentamethylene sebacamide (nylon 510), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polydecamethylene adipamide (nylon 106), and polydecamethylene adipamide (nylon 410). Polyethylene sebacamide (Nylon 1010), polydecamethylene dodecamide (Nylon 1012), polyundecane amide (Nylon 11), polyundecamethylene adipamide (Nylon 116), polydodecanamide (Nylon 12), polyxylene adipamide (Nylon XD6), polyxylene sebacamide (Nylon XD10), polymeta-xylylene adipamide (Nylon MXD6), polypara-xylylene adipamide (Nylon PXD6), polytetramethylene terephthalamide (Nylon 4T), polypentamethylene terephthalamide (nylon 5T), polyhexamethylene terephthalamide (nylon 6T), polyhexamethylene isophthalamide (nylon 6I), polynonamethylene terephthalamide (nylon 9T), polydecamethylene terephthalamide (nylon 10T), polyundecamethylene terephthalamide (nylon 11T), polydodecamethylene terephthalamide (nylon 12T), polytetramethylene isophthalamide (nylon 4I), polybis( Examples of the copolymer include one or a copolymer of two or more of the following components: polybis(3-methyl-4-aminohexyl)methane terephthalamide (nylon PACMT), polybis(3-methyl-4-aminohexyl)methane isophthalamide (nylon PACMI), polybis(3-methyl-4-aminohexyl)methaneandodecamide (nylon PACM12), polybis(3-methyl-4-aminohexyl)methane tetradecamide (nylon PACM14), and the like, as well as mixtures thereof.
[0115] Examples of polyacetals include homopolymers having oxymethylene units as the main repeating units, and copolymers that are mainly composed of oxymethylene units and contain oxyalkylene units having 2 to 8 adjacent carbon atoms in the main chain.
[0116] Examples of polyethylene terephthalate include polymers obtained by polycondensing terephthalic acid or a derivative thereof with ethylene glycol.
[0117] Examples of polybutylene terephthalate include polymers obtained by polycondensing terephthalic acid or a derivative thereof with 1,4-butanediol.
[0118] Examples of polytrimethylene terephthalate include polymers obtained by polycondensing terephthalic acid or a derivative thereof with 1,3-propanediol.
[0119] Examples of polycarbonates include polymers obtained by a transesterification method in which a dihydroxydiaryl compound is reacted with a carbonate ester such as diphenyl carbonate in a molten state, and polymers obtained by a phosgene method in which a dihydroxyaryl compound is reacted with phosgene.
[0120] Examples of polyarylene sulfide include linear polyphenylene sulfide, crosslinked polyphenylene sulfide which has been polymerized and then subjected to a curing reaction to increase the molecular weight, polyphenylene sulfide sulfone, polyphenylene sulfide ether, and polyphenylene sulfide ketone.
[0121] Examples of polyphenylene ethers include poly(2,3-dimethyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-chloromethyl-1,4-phenylene ether), poly(2-methyl-6-hydroxyethyl-1,4-phenylene ether), poly(2-methyl-6-n-butyl-1,4-phenylene ether), poly(2-ethyl-6-isopropyl-1,4-phenylene ether), poly(2-ethyl-6-n-propyl-1,4-phenylene ether), poly(2,3,6-trimethyl-1,4-phenylene ether), poly[2-(4'-methylphenyl)-1,4-phenylene ether], poly(2-bromo-6-phenyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2-phenyl-1,4-phenylene ether), poly(2-chloro-1,4-phenylene ether), poly(2-methyl-1,4-phenylene ether), poly(2-chloro-6-ethyl-1,4-phenylene ether), poly(2-chloro-6-bromo-1,4-phenylene ether), poly(2,6-di-n-propyl-1,4-phenylene ether), poly(2-methyl-6-isopropyl-1,4-phenylene ether), poly(2-chloro-6-methyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2,6-dibromo-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether), poly(2,6-dimethyl-1,4-phenylene ether), and the like.
[0122] Examples of modified polyphenylene ethers include polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and polystyrene, polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and styrene / butadiene copolymer, polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and styrene / maleic anhydride copolymer, polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and polyamide, polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and styrene / butadiene / acrylonitrile copolymer, the polyphenylene ethers in which functional groups such as amino groups, epoxy groups, carboxy groups, and styryl groups have been introduced into the polymer chain terminals, and the polyphenylene ethers in which functional groups such as amino groups, epoxy groups, carboxy groups, styryl groups, and methacrylic groups have been introduced into the polymer chain side chains.
[0123] Examples of polyaryletherketone include polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), and polyetheretherketoneketone (PEEKK).
[0124] Examples of the liquid crystal polymer (LCP) include a (co)polymer, which is a thermotropic liquid crystal polyester, comprising one or more structural units selected from an aromatic hydroxycarbonyl unit, an aromatic dihydroxy unit, an aromatic dicarbonyl unit, an aliphatic dihydroxy unit, an aliphatic dicarbonyl unit, and the like.
[0125] Examples of fluororesins include polytetrafluoroethylene (PTFE), perfluoroalkoxy resin (PFA), fluorinated ethylene propylene resin (FEP), fluorinated ethylene tetrafluoroethylene resin (ETFE), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), and ethylene / chlorotrifluoroethylene resin (ECTFE).
[0126] Examples of ionomer (IO) resins include copolymers of olefin or styrene with unsaturated carboxylic acid, in which a portion of the carboxyl groups is neutralized with metal ions.
[0127] Examples of the olefin / vinyl alcohol resin include an ethylene / vinyl alcohol copolymer, a propylene / vinyl alcohol copolymer, a saponified ethylene / vinyl acetate copolymer, and a saponified propylene / vinyl acetate copolymer.
[0128] Examples of the cyclic olefin resin include monocyclic compounds such as cyclohexene, polycyclic compounds such as tetracyclopentadiene, and polymers of cyclic olefin monomers.
[0129] Examples of polylactic acid include poly-L-lactic acid, which is a homopolymer of the L-form, poly-D-lactic acid, which is a homopolymer of the D-form, and stereocomplex polylactic acid, which is a mixture thereof.
[0130] Examples of the cellulose resin include methyl cellulose, ethyl cellulose, hydroxy cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, cellulose acetate, cellulose propionate, and cellulose butyrate.
[0131] Examples of the thermosetting resin include unsaturated polyester resin, vinyl ester resin, epoxy (EP) resin, melamine (MF) resin, phenolic resin (PF), urethane resin (PU), polyisocyanate, polyisocyanurate, polyimide (PI), urea (UF) resin, silicone (SI) resin, furan (FR) resin, benzoguanamine (BR) resin, alkyd resin, xylene resin, bismaleimide triazine (BT) resin, diallyl phthalate resin (PDAP), thermosetting polyphenylene ether, and thermosetting modified polyphenylene ether.
[0132] Examples of unsaturated polyester resins include resins obtained by esterifying an aliphatic unsaturated dicarboxylic acid with an aliphatic diol.
[0133] Examples of vinyl ester resins include bis-based vinyl ester resins and novolac-based vinyl ester resins.
[0134] Examples of epoxy resins include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol E type epoxy resin, bisphenol S type epoxy resin, bisphenol M type epoxy resin (4,4'-(1,3-phenylenediisopridiene)bisphenol type epoxy resin), bisphenol P type epoxy resin (4,4'-(1,4-phenylenediisopridiene)bisphenol type epoxy resin), bisphenol Z type epoxy resin (4,4'-cyclohexidienebisphenol type epoxy resin), phenol novolac type epoxy resin, cresol novolac type epoxy resin, tetraphenol group ethane type novolac type epoxy resin, and the like. Examples of epoxy resins include epoxy resins, novolac-type epoxy resins having a condensed ring aromatic hydrocarbon structure, biphenyl-type epoxy resins, aralkyl-type epoxy resins such as xylylene-type epoxy resins and phenylaralkyl-type epoxy resins, naphthylene ether-type epoxy resins, naphthol-type epoxy resins, naphthalenediol-type epoxy resins, difunctional to tetrafunctional epoxy-type naphthalene resins, binaphthyl-type epoxy resins, naphthalenearalkyl-type epoxy resins, anthracene-type epoxy resins, phenoxy-type epoxy resins, dicyclopentadiene-type epoxy resins, norbornene-type epoxy resins, adamantane-type epoxy resins, and fluorene-type epoxy resins.
[0135] The melamine resin may be a polymer obtained by polycondensation of melamine (2,4,6-triamino-1,3,5-triazine) and formaldehyde.
[0136] Examples of the phenolic resin include novolac-type phenolic resins such as phenol novolac resin, cresol novolac resin, and bisphenol A-type novolac resin; resole-type phenolic resins such as methylol-type resole resin and dimethylene ether-type resole resin; and aryl alkylene-type phenolic resins, and examples thereof include a single type or a combination of two or more types thereof.
[0137] Urea resins include resins obtained by condensation of urea and formaldehyde.
[0138] The thermoplastic resins or thermosetting resins may be used alone or in combination of two or more.
[0139] Since the glass fiber reinforced resin composition of the present embodiment is used in applications requiring a low dielectric tangent, the resin is preferably an epoxy resin, a modified polyphenylene ether, a thermosetting modified polyphenylene ether, a polybutylene terephthalate, a polypropylene, a fluororesin, or a liquid crystal polymer (LCP).
[0140] Examples of other additives include reinforcing fibers other than glass fibers, fillers other than glass fibers, flame retardants, ultraviolet absorbers, heat stabilizers, antioxidants, antistatic agents, flow improvers, antiblocking agents, lubricants, nucleating agents, antibacterial agents, and pigments.
[0141] Examples of reinforcing fibers other than glass fibers include carbon fibers and metal fibers.
[0142] Examples of fillers other than glass fiber include glass powder, talc, and mica.
[0143] The glass fiber reinforced resin composition of this embodiment may be a prepreg obtained by impregnating the glass fiber fabric of this embodiment with the resin by a method known per se and semi-curing the impregnated resin.
[0144] The glass fiber reinforced resin composition of this embodiment can be molded into various glass fiber reinforced resin molded articles by known molding methods such as injection molding, injection compression molding, two-color molding, blow molding, foam molding (including supercritical fluid), insert molding, in-mold coating molding, extrusion molding, sheet molding, thermoforming, rotational molding, laminate molding, press molding, blow molding, stamping molding, infusion, hand layup, spray-up, resin transfer molding, sheet molding compounding, bulk molding compounding, pultrusion, and filament winding. Furthermore, glass fiber reinforced resin molded articles can also be obtained by curing the prepreg.
[0145] Examples of uses for such molded articles include electronic device housings, electronic components, vehicle exterior and interior components, vehicle engine peripheral components, muffler-related components, and high-pressure tanks.
[0146] Examples of electronic components include printed wiring boards.
[0147] Examples of vehicle exterior members include bumpers, fenders, hoods, air dams, wheel covers, and radomes.
[0148] Examples of vehicle interior materials include door trims and ceiling materials.
[0149] Examples of vehicle engine peripheral components include an oil pan, an engine cover, an intake manifold, and an exhaust manifold.
[0150] Examples of muffler-related members include heat-resistant sound-deadening members, dust-removing filters, catalyst carriers, and the like.
[0151] The glass fiber of this embodiment can be suitably used not only in the glass fiber reinforced resin composition of this embodiment but also as a reinforcing material for inorganic materials such as gypsum, cement, etc. For example, when used as a reinforcing material for gypsum (particularly, a gypsum board having a thickness of 4 to 60 mm), the glass fiber having the glass composition in the above range can be contained in an amount of 0.1 to 4.0 mass% relative to the total mass of the gypsum.
[0152] Next, examples of the present invention and comparative examples will be described.
[0153] [Example 1] First, a glass yarn having composition A shown in Table 1 as a mother glass composition and having 21.0 tex glass yarns formed by bundling 204 glass filaments having a diameter of 7.0 μm was used as warp and weft yarns, and the warp density was 59 threads / 25 mm, the weft density was 57 threads / 25 mm, the thickness was 90 μm, and the mass per unit area was 97 g / m. 2 A glass fiber fabric (hereinafter referred to as glass fiber fabric A) having the following properties was prepared.
[0154] Next, the glass fiber fabric A was placed in a liquid tank containing nitric acid with a concentration of 6.3 mass % as an acid solution, and an acid leaching treatment was carried out while stirring the acid solution at a leaching temperature of 60°C for a leaching time of 180 minutes to obtain an acid-leached glass fiber fabric. The mass ratio of the glass fiber fabric A to the volume of the liquid tank was 5.0 g / L.
[0155] Next, the acid-eluted glass fiber fabric was placed in a muffle furnace, and the temperature was increased from room temperature to the firing temperature of 950°C at a temperature increase rate of 3.3°C / min. After firing at the firing temperature for 24 hours, the temperature was decreased from the firing temperature to room temperature at a temperature decrease rate of 3.3°C / min. Thus, the glass fiber fabric of this example was obtained.
[0156] The obtained glass fiber fabric of this example had glass filaments constituting the warp and weft of 5.8 μm in diameter, a mass per unit length of the warp and weft of 12.0 tex, a warp weave density of 69 threads / 25 mm, a weft weave density of 66 threads / 25 mm, a thickness of 84 μm, and a mass per unit area of 75 g / m 2 It was.
[0157] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this example were measured by the methods described above. The results are shown in Table 2.
[0158] The glass fiber fabric of this example was evaluated for handleability according to the following criteria. When a 10 cm x 10 cm piece of the glass fiber fabric was held at both ends and bent 180° at the center, the glass fiber fabric was rated as A if it returned to its original position. The cut-out glass fiber fabric was rated as B if it did not return to its original position or if it broke at the bent portion after being bent 180° at the center. The cut-out glass fiber fabric was rated as C if it broke before being bent 180° at the center. The results are shown in Table 2.
[0159] [Example 2] The glass fiber fabric of this example was obtained in exactly the same manner as in Example 1, except that the firing temperature when firing the acid-eluted glass fiber fabric was set to 1100°C and the firing time was set to 1 hour.
[0160] The obtained glass fiber woven fabric of this example had glass filaments constituting the warp and weft yarns with a diameter of 5.8 μm, a mass per unit length of the warp and weft yarns of 12.0 tex, a warp weave density of 69 threads / 25 mm, a weft weave density of 66 threads / 25 mm, a thickness of 84 μm, and a mass per unit area of 75 g / m 2 It was.
[0161] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this example were measured by the methods described above. The handleability of the glass fiber was also evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0162] [Example 3] First, a glass fiber having composition A shown in Table 1 as a mother glass composition was used as the warp and weft yarns, and the warp yarn density was 53 threads / 25 mm, the weft yarn density was 53 threads / 25 mm, the thickness was 50 μm, and the mass per unit area was 45 g / m. 2 A glass fiber fabric (hereinafter referred to as glass fiber fabric B) was prepared.
[0163] Next, the glass fiber fabric B was placed in a liquid tank containing nitric acid with a concentration of 6.3 mass % as an acid solution, and an acid leaching treatment was carried out while stirring the acid solution at a leaching temperature of 50°C for 360 minutes to obtain an acid-leached glass fiber fabric. The mass ratio of the glass fiber fabric B to the volume of the liquid tank was 2.5 g / L.
[0164] Next, the acid-eluted glass fiber fabric was placed in a muffle furnace, and the temperature was increased from room temperature to the firing temperature of 900°C at a temperature increase rate of 3.3°C / min. After firing at the firing temperature for 24 hours, the temperature was decreased from the firing temperature to room temperature at a temperature decrease rate of 3.3°C / min. Thus, the glass fiber fabric of this example was obtained.
[0165] The obtained glass fiber woven fabric of this example had glass filaments constituting the warp and weft yarns with a diameter of 4.3 μm, a mass per unit length of the warp and weft yarns of 6.5 tex, a warp weave density of 61 threads / 25 mm, a weft weave density of 61 threads / 25 mm, a thickness of 40 μm, and a mass per unit area of 34 g / m 2 It was.
[0166] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this example were measured by the methods described above. The handleability of the glass fiber was also evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0167] [Example 4] The glass fiber fabric of this example was obtained in exactly the same manner as in Example 3, except that in the acid leaching treatment, the leaching temperature was 60°C, the ratio of the mass of the glass fiber fabric B to the volume of the liquid tank was 5.0 g / L, and the firing temperature when firing the acid leaching-treated glass fiber fabric was 850°C and the firing time was 48 hours.
[0168] The obtained glass fiber woven fabric of this example had glass filaments constituting the warp and weft yarns with a diameter of 4.3 μm, a mass per unit length of the warp and weft yarns of 6.5 tex, a warp weave density of 61 threads / 25 mm, a weft weave density of 61 threads / 25 mm, a thickness of 40 μm, and a mass per unit area of 34 g / m 2 It was.
[0169] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this example were measured by the methods described above. The handleability of the glass fiber was also evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0170] [Example 5] The glass fiber fabric of this example was obtained in exactly the same manner as in Example 3, except that in the acid leaching treatment, the leaching temperature was 60°C, the mass ratio of the glass fiber fabric B to the volume of the liquid tank was 5.0 g / L, and the firing temperature when firing the acid leaching-treated glass fiber fabric was 870°C and the firing time was 48 hours.
[0171] The obtained glass fiber woven fabric of this example had glass filaments constituting the warp and weft yarns with a diameter of 4.3 μm, a mass per unit length of the warp and weft yarns of 6.5 tex, a warp weave density of 61 threads / 25 mm, a weft weave density of 61 threads / 25 mm, a thickness of 40 μm, and a mass per unit area of 34 g / m 2 It was.
[0172] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this example were measured by the methods described above. The handleability of the glass fiber was also evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0173] Example 6 A glass fiber fabric of this example was obtained in exactly the same manner as in Example 1, except that in the acid leaching treatment, the leaching time was 360 minutes and the baking temperature was 900°C.
[0174] The obtained glass fiber fabric of this example had glass filaments constituting the warp and weft of 5.8 μm in diameter, a mass per unit length of the warp and weft of 12.0 tex, a warp weave density of 69 threads / 25 mm, a weft weave density of 66 threads / 25 mm, a thickness of 84 μm, and a mass per unit area of 75 g / m 2 It was.
[0175] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this example were measured by the methods described above. The handleability of the glass fiber was also evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0176] Example 7 A glass fiber fabric of this example was obtained in exactly the same manner as in Example 3, except that the leaching temperature in the acid leaching treatment was set to 60°C.
[0177] The obtained glass fiber woven fabric of this example had glass filaments constituting the warp and weft yarns with a diameter of 4.3 μm, a mass per unit length of the warp and weft yarns of 6.5 tex, a warp weave density of 61 threads / 25 mm, a weft weave density of 61 threads / 25 mm, a thickness of 40 μm, and a mass per unit area of 34 g / m 2 It was.
[0178] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this example were measured by the methods described above. The handleability of the glass fiber was also evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0179] Comparative Example 1 The glass fiber fabric of this comparative example was obtained in exactly the same manner as in Example 4, except that the firing temperature for firing the acid-eluted glass fiber fabric was 800°C and the firing time was 72 hours.
[0180] The obtained glass fiber woven fabric of this comparative example had glass filaments constituting the warp and weft of 4.3 μm in diameter, a mass per unit length of the warp and weft of 6.5 tex, a warp weave density of 61 threads / 25 mm, a weft weave density of 61 threads / 25 mm, a thickness of 40 μm, and a mass per unit area of 34 g / m 2 It was.
[0181] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this comparative example were measured by the methods described above. The handleability of the glass fiber was also evaluated in exactly the same manner as in Example 1. The results are shown in Table 3.
[0182] Comparative Example 2 The glass fiber fabric of this comparative example was obtained in exactly the same manner as in Example 4, except that the firing temperature when firing the acid-eluted glass fiber fabric was 900°C and the firing time was 24 hours.
[0183] The obtained glass fiber woven fabric of this comparative example had glass filaments constituting the warp and weft of 4.3 μm in diameter, a mass per unit length of the warp and weft of 6.5 tex, a warp weave density of 61 threads / 25 mm, a weft weave density of 61 threads / 25 mm, a thickness of 40 μm, and a mass per unit area of 34 g / m 2 It was.
[0184] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this comparative example were measured by the methods described above. The handleability of the glass fiber was also evaluated in exactly the same manner as in Example 1. The results are shown in Table 3.
[0185] Comparative Example 3 A glass fiber fabric of this comparative example was obtained in exactly the same manner as in Example 3, except that the leaching temperature in the acid leaching treatment was 40°C.
[0186] The obtained glass fiber woven fabric of this comparative example had glass filaments constituting the warp and weft of 4.3 μm in diameter, a mass per unit length of the warp and weft of 6.5 tex, a warp weave density of 61 threads / 25 mm, a weft weave density of 61 threads / 25 mm, a thickness of 40 μm, and a mass per unit area of 34 g / m 2 It was.
[0187] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this comparative example were measured by the methods described above. The handleability of the glass fiber was also evaluated in exactly the same manner as in Example 1. The results are shown in Table 3.
[0188] [Comparative Example 4] First, a glass fiber having composition B shown in Table 1 as a mother glass composition, and 22 tex glass yarns formed by bundling 204 glass filaments having a diameter of 7.4 μm, was used as warp and weft yarns, and the warp density was 59 threads / 25 mm, the weft density was 57 threads / 25 mm, the thickness was 90 μm, and the mass per unit area was 101 g / m. 2 A glass fiber fabric (hereinafter referred to as glass fiber fabric C) was prepared.
[0189] Next, the glass fiber fabric C was placed in a liquid tank containing nitric acid with a concentration of 6.3 mass % as an acid solution, and an acid leaching treatment was carried out while stirring the acid solution at a leaching temperature of 60°C for a leaching time of 2,880 minutes to obtain an acid-leached glass fiber fabric. The mass ratio of the glass fiber fabric C to the volume of the liquid tank was 5.0 g / L.
[0190] Next, the acid-eluted glass fiber fabric was placed in a muffle furnace, and the temperature was increased from room temperature to the firing temperature of 900°C at a temperature increase rate of 3.3°C / min. After firing at the firing temperature for 24 hours, the temperature was decreased from the firing temperature to room temperature at a temperature decrease rate of 3.3°C / min. Thus, the glass fiber fabric of this comparative example was obtained.
[0191] The obtained glass fiber woven fabric of this comparative example had glass filaments constituting the warp and weft of 6.3 μm in diameter, a mass per unit length of the warp and weft of 14 tex, a warp weave density of 68 threads / 25 mm, a weft weave density of 65 threads / 25 mm, a thickness of 87 μm, and a mass per unit area of 79 g / m 2 It was.
[0192] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this comparative example were measured by the methods described above. The handleability of the glass fiber was also evaluated in exactly the same manner as in Example 1. The results are shown in Table 3.
[0193] Comparative Example 5 A glass fiber fabric of this comparative example was obtained in exactly the same manner as in Comparative Example 4, except that in the acid leaching treatment, nitric acid with a concentration of 18.0 mass % was used as the acid solution and the leaching time was 360 minutes.
[0194] The obtained glass fiber woven fabric of this comparative example had glass filaments constituting the warp and weft yarns with a diameter of 6.3 μm, a mass per unit length of the warp and weft yarns of 14 tex, a warp weave density of 68 threads / 25 mm, a weft weave density of 65 threads / 25 mm, a thickness of 87 μm, and a mass per unit area of 79 g / m 2 It was.
[0195] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this comparative example were measured by the methods described above. The handleability of the glass fiber was also evaluated in exactly the same manner as in Example 1. The results are shown in Table 3.
[0196] Comparative Example 6 A glass fiber fabric of this comparative example was obtained in exactly the same manner as in Comparative Example 4, except that in the acid leaching treatment, hydrochloric acid with a concentration of 3.6 mass % was used as the acid solution.
[0197] The obtained glass fiber woven fabric of this comparative example had glass filaments constituting the warp and weft of 6.3 μm in diameter, a mass per unit length of the warp and weft of 14 tex, a warp weave density of 68 threads / 25 mm, a weft weave density of 65 threads / 25 mm, a thickness of 87 μm, and a mass per unit area of 79 g / m 2 It was.
[0198] The glass composition, tensile breaking stress, and dielectric loss tangent of the glass fiber fabric of this comparative example were measured by the methods described above. The handleability of the glass fiber was also evaluated in exactly the same manner as in Example 1. The results are shown in Table 3.
[0199]
[0200]
[0201]
[0202] From Table 2, the BS × (T / (100 - S)) 2 The glass fibers of Examples 1 to 7, in which the value of is in the range of 5.2 to 33.8, have a dielectric loss tangent of less than 0.0010 at a measurement frequency of 28 GHz, and it is clear that glass fibers having excellent handleability can be obtained.
[0203] On the other hand, from Table 3, the BS × (T / (100-S)) 2 It is clear that the glass fiber of Comparative Example 1, in which the value of is greater than 33.8, has a dielectric loss tangent of greater than 0.0010 at a measurement frequency of 28 GHz.
[0204] Also, from Table 3, the BS × (T / (100-S)) 2It is clear that the glass fibers of Comparative Examples 2 to 6, in which the value of is less than 5.2, have a dielectric loss tangent of more than 0.0010 at a measurement frequency of 28 GHz, or glass fibers having sufficient handleability cannot be obtained.
Claims
1. Glass fiber having a SiO content in the range of 92.50 to 99.99 mass% based on the total amount of the glass composition. 2 and TiO in the range of 0.01 to 5.00 mass%. 2 and Al in the range of 0.00 to 2.50 mass %. 2 O 3 The glass composition includes a glass fiber having a tensile breaking stress in the range of 1.0 to 100.0 MPa, and the SiO 2 The content S of TiO 2 and the tensile breaking stress BS of the glass fiber satisfy the following formula (1): 5.2≦BS×(T / (100−S)). 2 ≦33.8 ... (1) 2. The glass fiber according to claim 1, wherein the SiO 2 The content S of TiO 2 and the tensile breaking stress BS of the glass fiber satisfy the following formula (2): 9.1≦BS×(T / (100−S)). 2 ≦ 33.5 ... (2) 3. The glass fiber according to claim 1, wherein the SiO 2 The content S of TiO 2 and the tensile breaking stress BS of the glass fiber satisfy the following formula (3): 20.1≦BS×(T / (100−S)). 2 ≦ 33.1 ... (3) 4. A glass fiber fabric comprising the glass fiber according to any one of claims 1 to 3.
5. A glass fiber reinforced resin composition comprising the glass fiber according to any one of claims 1 to 3.
Citation Information
Patent Citations
Highly heat-resistant glass fiber and its production
JP1993178642A
Heat resistant porous glass fiber
JP1997169548A
Heat-resistant glass sliver containing al ▲ lower 2 ▼ lower ▲ lower 3 ▼ with high textile suitability and its product
JP2001525783A
Glass filler, production method therefor, and resin-containing composition comprising glass filler