Coated active material, coated active material production method, positive electrode material and battery

The coated active material with a lithium-containing fluoride layer on the positive electrode active material addresses oxidation resistance issues by controlling lithium hydrogen carbonate levels, reducing internal resistance and improving battery performance.

WO2024241817A1PCT designated stage expired Publication Date: 2024-11-28PANASONIC HOLDINGS CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015947
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-04-23
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Batteries using halide solid electrolytes face issues with oxidation resistance, leading to increased internal resistance during charging due to oxidative decomposition of elements like chlorine, bromine, and iodine, and coatings with lithium-containing fluoride can alter the surface chemistry of positive electrode active materials, causing resistance increases during discharge.

Method used

A coated active material is developed with a lithium-containing fluoride coating layer on a positive electrode active material, where lithium hydrogen carbonate is controlled within specific ppm ranges to suppress alkaline component reactions and formation of resistance layers, thereby reducing internal battery resistance.

Benefits of technology

The controlled coating layer improves ionic conductivity and reduces internal battery resistance by preventing oxidative decomposition and surface reactions, enhancing battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015947_28112024_PF_FP_ABST
    Figure JP2024015947_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A coated active material 100 according to the present disclosure comprises: a positive electrode active material 11; lithium hydrogencarbonate present on the surface of the positive electrode active material 11; and a coating layer 12 that coats at least a section of the surface of the positive electrode active material 11. The coating layer 12 contains lithium-containing fluoride. When the mass of the lithium hydrogencarbonate present on the surface of the positive electrode active material 11 is measured by thermogravimetry / mass spectrometry, the ratio R1 of the mass of the lithium hydrogencarbonate to the mass of the positive electrode active material 11 is 130-580 ppm.
Need to check novelty before this filing date? Find Prior Art

Description

Coated active material, method for producing coated active material, positive electrode material, and battery

[0001] The present disclosure relates to a coated active material, a method for manufacturing a coated active material, a positive electrode material, and a battery.

[0002] Patent Document 1 discloses a positive electrode material including a positive electrode active material and a halide solid electrolyte, and the halide solid electrolyte includes lithium, yttrium, and at least one element selected from the group consisting of chlorine, bromine, and iodine.

[0003] International Publication No. 2019 / 135322 International Publication No. 2021 / 187391 International Publication No. 2023 / 037776

[0004] The present disclosure provides a coated active material that can reduce the internal resistance of a battery.

[0005] A coated active material in one aspect of the present disclosure includes: a positive electrode active material; lithium bicarbonate present on a surface of the positive electrode active material; and a coating layer that coats at least a portion of the surface of the positive electrode active material, wherein the coating layer contains a lithium-containing fluoride, and when the mass of the lithium bicarbonate is measured by thermogravimetry-mass spectrometry, a ratio R1 of the mass of the lithium bicarbonate to the mass of the positive electrode active material is 130 ppm or more and 580 ppm or less.

[0006] According to the present disclosure, the internal resistance of a battery can be reduced.

[0007] FIG. 1 is a cross-sectional view showing a schematic configuration of a coated active material 100 according to the first embodiment. FIG. 2 is a flowchart showing a method for manufacturing the coated active material 100. FIG. 3 is a diagram showing a LiNi alloy that has not been subjected to a carbonate annealing treatment. 0.8 Co 0.15 Al 0.05 4 is a cross-sectional view showing a schematic configuration of a positive electrode material 200 according to a second embodiment. FIG. 5 is a cross-sectional view showing a schematic configuration of a battery 300 according to a third embodiment.

[0008] (Findings forming the basis of the present disclosure) Patent Document 1 describes a positive electrode material including a positive electrode active material and a halide solid electrolyte containing lithium, yttrium, and at least one element selected from the group consisting of chlorine, bromine, and iodine.

[0009] However, in batteries using a halide solid electrolyte as the positive electrode material, the halide solid electrolyte undergoes oxidative decomposition during charging. The products of oxidative decomposition function as a resistive layer, increasing the internal resistance of the battery during charging. The increase in the internal resistance of the battery during charging is presumably caused by an oxidation reaction of at least one element selected from the group consisting of chlorine, bromine, and iodine contained in the halide solid electrolyte. Thus, there are issues with the oxidation resistance of halide solid electrolytes.

[0010] Patent Document 2 describes that batteries using a positive electrode active material coated with a material containing a lithium-containing fluoride exhibit excellent oxidation resistance. Such a positive electrode active material can suppress an increase in the internal resistance of the battery during charging. While the details of this mechanism are unclear, it is presumed to be as follows: Fluorine has the highest electronegativity among halogen elements. Therefore, fluorine bonds strongly with cations. Therefore, in lithium-containing fluorides, the oxidation reaction of fluorine, i.e., a side reaction in which electrons are extracted from fluorine, is unlikely to proceed. As a result, a resistance layer is unlikely to be generated due to oxidative decomposition.

[0011] Meanwhile, the present inventors have investigated the resistance of batteries using a positive electrode active material coated with a material containing lithium-containing fluoride. As a result, they have discovered a problem: high output resistance during discharge. While the details of this mechanism are unclear, the following is presumed to be the case. When coating a positive electrode active material with a material containing lithium-containing fluoride, a lithium-containing alkaline component present on the surface of the positive electrode active material may react with the lithium-containing fluoride, resulting in a partial alteration of the coating layer containing lithium-containing fluoride. Here, the lithium-containing alkaline component present on the surface of the positive electrode active material refers to a component that does not function as a positive electrode active material, i.e., a component that does not directly contribute to the absorption and desorption of lithium ions. When the coating layer alters, a resistance layer is formed at the interface between the positive electrode active material and the coating layer. This resistance layer increases the internal resistance of the battery during charge and discharge. Thus, when coating a positive electrode active material with a material containing lithium-containing fluoride, the alteration of the lithium-containing fluoride by the alkaline component on the surface of the positive electrode active material and the resulting increase in battery resistance are issues.

[0012] Patent Document 3 describes that the amount of alkaline components on the surface of a positive electrode active material is reduced by subjecting the positive electrode active material to a cleaning treatment using a water-soluble organic solvent.

[0013] From these findings, the inventors have come up with the technique of the present disclosure.

[0014] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.

[0015] The following descriptions are all comprehensive or provide specific examples. The numerical values, compositions, shapes, thicknesses, electrical properties, secondary battery structures, electrode materials, etc. shown below are merely examples and are not intended to limit the present disclosure. In addition, elements not described in the independent claims showing the most general concepts are optional elements.

[0016] (Embodiment 1) FIG. 1 is a cross-sectional view showing a schematic configuration of a coated active material in embodiment 1. The coated active material 100 in embodiment 1 includes a cathode active material 11, lithium bicarbonate (not shown) present on the surface of the cathode active material 11, and a coating layer 12. The coating layer 12 coats at least a portion of the surface of the cathode active material 11. The coating layer 12 is in direct contact with the cathode active material 11. The coating layer 12 contains a lithium-containing fluoride. When the mass of lithium bicarbonate (LiHCO3) present on the surface of the cathode active material 11 is measured by thermogravimetry-mass spectrometry (TG-MS), the ratio R1 of the mass of lithium bicarbonate to the mass of the cathode active material 11 is 130 ppm or more and 580 ppm or less. In other words, when the mass of the cathode active material 11 is M1 and the mass of the lithium bicarbonate present on the surface of the cathode active material 11 is M2, 10 6 The value calculated by the formula × (M2 / M1) is in the range of 130 or more and 580 or less.

[0017] The alkaline component on the surface of the positive electrode active material 11 is, for example, a strong alkaline component such as lithium hydroxide formed by the adsorption of water onto the residual lithium salt on the surface of the positive electrode active material 11 and the reaction of the residual lithium salt with lithium ions eluted from the positive electrode active material 11 and water. When the strong alkaline component is generated, an exchange of lithium ions with protons occurs on the surface of the positive electrode active material 11, forming a Li-deficient layer (e.g., a NiO layer) on the surface of the positive electrode active material. The presence of the Li-deficient layer is also presumed to affect the output resistance. The strong alkaline component generates lithium carbonates such as lithium bicarbonate by absorbing carbon dioxide from the atmosphere. However, because lithium bicarbonate is an unstable compound, the generation of the strong alkaline component and the formation of the Li-deficient layer are repeated as long as water and carbon dioxide are present. Therefore, by controlling the amount of lithium bicarbonate on the surface of the positive electrode active material 11 to be low, the reaction between lithium ions and water on the surface of the positive electrode active material 11, i.e., the exchange of lithium ions and protons on the surface of the positive electrode active material 11, can be suppressed, and the formation of a Li-deficient layer on the surface of the positive electrode active material 11 can be reduced. Furthermore, by controlling the amount of lithium bicarbonate on the surface of the positive electrode active material 11 to be within the above range, when the surface of the positive electrode active material 11 is coated with the coating layer 12, deterioration of the coating layer 12 due to a reaction between the lithium-containing alkaline component present on the surface of the positive electrode active material 11 and the lithium-containing fluoride contained in the coating layer 12 is suppressed. In other words, the formation of a resistance layer at the interface between the positive electrode active material 11 and the coating layer 12 due to deterioration of the coating layer 12 is suppressed. Therefore, the coated active material 100 can reduce the internal resistance of the battery.

[0018] The ratio R1 may be 140 ppm or more, 150 ppm or more, or 155 ppm or more. The ratio R1 may be 570 ppm or less, 560 ppm or less, 551 ppm or less, 500 ppm or less, or 260 ppm or less. The ratio R1 may be 155 ppm or more and 551 ppm or less. With this configuration, the internal resistance of the battery can be further reduced.

[0019] The amount of lithium bicarbonate present on the surface of the positive electrode active material 11 can be quantified by TG-MS. The gas generated during thermogravimetric analysis (TG) is introduced into a mass spectrometer (MS) to generate an extracted ion chromatogram, and the peak area is normalized. Specifically, a predetermined amount (e.g., 1 g) of calcium oxalate hydrate is first thermally decomposed in a reference gas environment (e.g., 1% argon) to obtain extracted ion chromatograms of argon and carbon dioxide. From the extracted ion chromatograms of argon and carbon dioxide, a sensitivity coefficient is calculated by dividing the carbon dioxide spectral intensity per 1 mol of carbon dioxide by the argon spectral intensity per 1 mol of argon. For example, the sensitivity coefficient is 2.1. Next, a predetermined amount (e.g., 0.1 g) of powder of the positive electrode active material 11 is subjected to TG-MS measurement in an argon gas environment to obtain an ion chromatogram of carbon dioxide. In the obtained carbon dioxide spectrum, the integrated value of the spectrum intensity up to 300°C is considered to correspond to the amount of lithium hydrogen carbonate, and the mass of lithium hydrogen carbonate present on the surface of positive electrode active material 11 is calculated from the value converted using the above-mentioned sensitivity coefficient.

[0020] When the mass of lithium originating from the lithium-containing alkaline component present on the surface of positive electrode active material 11 is measured by neutralization titration, the ratio R2 of the mass of lithium originating from the lithium-containing alkaline component present on the surface of positive electrode active material 11 to the mass of positive electrode active material 11 may be greater than 0.30% and less than or equal to 0.40%. In other words, when the mass of positive electrode active material 11 is M1 and the mass of lithium originating from the lithium-containing alkaline component present on the surface of positive electrode active material 11 is M3, the value calculated by the formula 100 × (M3 / M1) may be greater than 0.30 and less than or equal to 0.40.

[0021] The ratio R2 may be greater than 0.30% and less than or equal to 0.35%. With this configuration, the internal resistance of the battery can be further reduced. The ratio R2 may be greater than or equal to 0.31% and less than or equal to 0.35%.

[0022] The ratio R2 is calculated by the following neutralization titration. Lithium hydroxide (LiOH), lithium carbonate (LiCO) as a lithium carbonate, and a trace amount of lithium bicarbonate (LiHCO) are present as lithium-containing alkaline components on the surface of the positive electrode active material 11. Here, in the neutralization titration, the lithium-containing alkaline component present on the surface of the positive electrode active material 11 is considered to consist only of lithium hydroxide and lithium carbonate, and the mass of the lithium hydroxide and the mass of the lithium carbonate are measured to calculate the ratio R2.

[0023] Neutralization titration can be performed based on the Warder method. A predetermined amount (e.g., 2 g) of powder of the positive electrode active material 11 is added to a predetermined amount (e.g., 200 mL) of ion-exchanged water, stirred thoroughly (e.g., for 30 minutes), and then allowed to stand (e.g., for 10 minutes). Next, the supernatant is filtered through a syringe filter with a pore size of 0.2 μm, and the resulting filtrate is used as the test solution. A phenolphthalein solution is added to the test solution as an indicator, and neutralization titration is performed using a 0.1 mol / L aqueous HCl solution under a nitrogen atmosphere. After the endpoint is detected with phenolphthalein, a methyl orange solution is added to the test solution as an indicator, and neutralization titration is performed using a 0.1 mol / L aqueous HCl solution under a nitrogen atmosphere.

[0024] The mass of lithium hydroxide (LiOH) and the mass of lithium carbonate (Li2CO3) contained in the test solution can be calculated from the amount of HCl required to reach the end point of each reaction. The mass of lithium derived from lithium hydroxide can be calculated from the mass of lithium hydroxide. The mass of lithium derived from lithium carbonate can be calculated from the mass of lithium carbonate. The sum of the mass of lithium derived from lithium hydroxide and the mass of lithium derived from lithium carbonate measured in this way by neutralization titration is taken as the mass of lithium derived from the lithium-containing alkaline component present on the surface of positive electrode active material 11.

[0025] In the present disclosure, the "mass of lithium bicarbonate present on the surface of positive electrode active material 11" essentially means the mass of lithium bicarbonate present in the range extracted by the above method. In the present disclosure, the "mass of lithium derived from the lithium-containing alkaline component present on the surface of positive electrode active material 11" essentially means the mass of lithium derived from the lithium-containing alkaline component present in the range extracted by the above method.

[0026] When the mass of lithium hydroxide (LiOH) present on the surface of positive electrode active material 11 is measured by the neutralization titration, the ratio R3 of the mass of lithium hydroxide to the mass of positive electrode active material 11 may be 1.0% or less. Ratio R3 may be 0.1% or more and 1.0% or less, 0.3% or more and 0.9% or less, 0.4% or more and 0.8% or less, or 0.56% or more and 0.73% or less. This configuration can further reduce the internal resistance of the battery.

[0027] (Coating Layer) Hereinafter, the material that constitutes the coating layer 12 will be referred to as the "coating material." The coated active material 100 contains the positive electrode active material 11 and a coating material. The coating material contains a lithium-containing fluoride.

[0028] The lithium-containing fluoride may be composed of Li, F, and at least one selected from the group consisting of Zr, Ti, and Al. Examples of such lithium-containing fluorides include LiZrF, LiZrF, LiZrF, LiAlF, and LiTiF. This configuration can improve the ionic conductivity of the lithium-containing fluoride. As a result, the internal resistance of the battery can be further reduced.

[0029] The lithium-containing fluoride may contain Li, Me1, Al, and F. Here, Me1 is at least one selected from the group consisting of Ti and Zr. With this configuration, the ionic conductivity of the lithium-containing fluoride can be improved. As a result, the internal resistance of the battery can be further reduced.

[0030] The lithium-containing fluoride may be composed of Li, Me, Al, and F. Here, Me is at least one selected from the group consisting of Ti and Zr. "Composed of Li, Me, Al, and F" means that, except for inevitable impurities, no materials other than Li, Me, Al, and F are intentionally added. This configuration can improve the ionic conductivity of the lithium-containing fluoride. As a result, the internal resistance of the battery can be further reduced.

[0031] The lithium-containing fluoride may be represented by the following composition formula (1): Li6-(m-mx+3x)b(Me1 1-x Me2 x ) b F6 Formula (1) In composition formula (1), Me1 is at least one selected from the group consisting of Ti and Zr, Me2 is at least one selected from the group consisting of Al and Y, m is the valence of Me1, and 0<x<1 and 0<b≦3 are satisfied.

[0032] In the composition formula (1), when Me1 includes a plurality of elements, m is the sum of the products of the composition ratios of the respective elements and the valences of the elements. For example, when Me1 includes an element M1 and an element M2, and the composition ratio of the element M1 is a1 and the valence is m1, and the composition ratio of the element M2 is a2 and the valence of the element M2 is m2, m is expressed as m1a1+m2a2.

[0033] This configuration can improve the ionic conductivity of the lithium-containing fluoride, thereby further reducing the internal resistance of the battery.

[0034] In composition formula (1), 0<x<1 and 0<b≦1.5 may be satisfied, or 0.1≦x≦0.9 and 0.8≦b≦1.2 may be satisfied.

[0035] In the composition formula (1), 0.5≦xb<1 may be satisfied. With this configuration, the ionic conductivity of the lithium-containing fluoride can be improved. As a result, the internal resistance of the battery can be further reduced.

[0036] In the composition formula (1), the following conditions may be satisfied: 2.5≦6−(m−mx+3x)b≦2.9, 0.1≦(1−x)b≦0.5, and 0.5≦xb≦0.9. This configuration can improve the ionic conductivity of the lithium-containing fluoride. As a result, the internal resistance of the battery can be further reduced.

[0037] Me2 may include Al. Me2 may be Al.

[0038] The lithium-containing fluoride may be represented by the following composition formula (2): Li α Me1 β Al γ F6 Formula (2) In composition formula (2), Me1 is at least one selected from the group consisting of Ti and Zr, and α, β, and γ satisfy α+4β+3γ=6 and γ>0.

[0039] In the composition formula (2), γ may satisfy the relationship 0.5≦γ<1. With this configuration, the ionic conductivity of the lithium-containing fluoride can be improved, and as a result, the internal resistance of the battery can be further reduced.

[0040] In the composition formula (2), α, β, and γ may satisfy the following conditions: 2.5≦α≦2.9, 0.1≦β≦0.5, and 0.5≦γ≦0.9. This configuration can improve the ionic conductivity of the lithium-containing fluoride. As a result, the internal resistance of the battery can be further reduced.

[0041] Me1 may be Ti. Me1 may be Zr. With this configuration, the ionic conductivity of the lithium-containing fluoride can be improved. As a result, the internal resistance of the battery can be further reduced.

[0042] The lithium-containing fluoride is Li 2.7 Ti 0.3 Al 0.7 F6 and Li 2.8 Zr 0.2 Al 0.8F6. This configuration can improve the ionic conductivity of the lithium-containing fluoride, thereby further reducing the internal resistance of the battery.

[0043] The lithium-containing fluoride is not limited to one that strictly satisfies the above composition formula, and includes, for example, one that contains a trace amount of impurities other than the constituent elements represented by composition formula (1). For example, in the lithium-containing fluoride, the impurities other than the constituent elements represented by the composition formula may be 10 mass % or less.

[0044] The lithium-containing fluoride may be represented by the following composition formula (3): Li6-(4-x-ny)b(Ti 1-x-y Al x Me3 y ) b F 6-2z O z ...(3)

[0045] Here, Me3 is at least one selected from the group consisting of Zr, Ni, Fe, and Cr, n is the valence of Me3, and 0.1<x<0.9, 0≦y<0.1, 0≦z<0.1, and 0.8<b≦1.2 are satisfied.

[0046] In the composition formula (3), when Me3 includes a plurality of elements, n is the sum of the products of the composition ratios of the respective elements and the valences of the elements. For example, when Me3 includes an element M1 and an element M2, and the composition ratio of the element M1 is a1 and the valence is n1, and the composition ratio of the element M2 is a2 and the valence of the element M2 is n2, n is expressed as n1a1+n2a2.

[0047] The coating material may contain a lithium-containing fluoride as a main component. That is, the coating material may contain, for example, 50% or more of the lithium-containing fluoride in terms of mass ratio relative to the entire coating layer 12.

[0048] The coating material may contain 70% or more of lithium-containing fluoride in terms of mass ratio relative to the entire coating layer 12 .

[0049] The coating material contains a lithium-containing fluoride as a main component, and may further contain unavoidable impurities, or starting materials, by-products, decomposition products, and the like used in synthesizing the lithium-containing fluoride.

[0050] The coating material may, for example, excluding unavoidable impurities, contain 100% lithium-containing fluoride in terms of mass ratio relative to the entire coating layer 12. As described above, the coating material may be composed only of lithium-containing fluoride.

[0051] The coating material may be sulfur-free.

[0052] In the coated active material 100, the ratio of the volume of the coating layer 12 to the total volume of the positive electrode active material 11 and the coating layer 12 may be 1% or more and 10% or less. In other words, the ratio V2 / (V1+V2) of the volume V2 of the coating layer 12 to the sum (V1+V2) of the volume V1 of the positive electrode active material 11 and the volume V2 of the coating layer 12 may be 0.01 or more and 0.1 or less. When the ratio of the volume of the coating layer 12 to the total volume of the positive electrode active material 11 and the coating layer 12 is 1% or more, the surface of the positive electrode active material 11 can be sufficiently covered by the coating layer 12, thereby effectively suppressing the formation of a resistance layer between the positive electrode active material 11 and the coating layer 12. When the ratio of the volume of the coating layer 12 to the total volume of the positive electrode active material 11 and the coating layer 12 is 10% or less, the surface of the positive electrode active material 11 can be prevented from being over-covered by the coating layer 12. As a result, an appropriate electron conduction path is secured between particles of the positive electrode active material 11. The volume V1 of the positive electrode active material 11 means the total volume of the positive electrode active material 11 in the particle group of the coated active material 100. The volume V2 of the coating layer 12 means the total volume of the coating layer 12 in the particle group of the coated active material 100.

[0053] According to the above configuration, the internal resistance of the battery can be further reduced.

[0054] The ratio of the volume of the coating layer 12 to the sum of the volume of the positive electrode active material 11 and the volume of the coating layer 12 can be determined, for example, by determining the volume ratios of 20 arbitrarily selected cross-sectional SEM images of the coated active material 100 obtained by a scanning electron microscope (SEM) and calculating the average value. When the volume of the positive electrode active material 11 is defined as V1, the volume of the coating layer 12 is defined as V2, and the volume of the coated active material 100 is defined as V3, the volume of the coating layer 12 is determined as V3 - V1. Therefore, the ratio of the volume of the coating layer 12 to the sum of the volume of the positive electrode active material 11 and the volume of the coating layer 12 is determined as (V3 - V1) / V3.

[0055] The volume V1 of the positive electrode active material 11 can be calculated by the following method. The area of ​​the positive electrode active material 11 is calculated from the outline of the positive electrode active material 11 extracted from the cross-sectional SEM image. The radius r1 (equivalent circle diameter) of a circle having an area equivalent to this area is calculated. By assuming that the positive electrode active material 11 is a perfect sphere having an equivalent circle diameter r1, the volume V1 of the positive electrode active material 11 can be calculated from the equivalent circle diameter r1. The volume V3 of the coated active material 100 can be calculated by the following method. The area of ​​the coated active material 100 is calculated from the outline of the coated active material 100 extracted from the cross-sectional SEM image. The radius r3 (equivalent circle diameter) of a circle having an area equivalent to this area is calculated. By assuming that the coated active material 100 is a perfect sphere having an equivalent circle diameter r3, the volume V3 of the coated active material 100 can be calculated from the equivalent circle diameter r3. The volume V3 of the coated active material 100 can also be calculated by the following method. The average thickness of the coating layer 12 is added to the equivalent circle diameter r1 of the positive electrode active material 11 calculated from the cross-sectional SEM image, and this is regarded as the equivalent circle diameter r3 of the coated active material 100. The coated active material 100 is regarded as a perfect sphere having the equivalent circle diameter r3, and the volume V3 of the coated active material 100 can be calculated from the equivalent circle diameter r3. The average thickness of the coating layer 12 can be determined, for example, by measuring the thickness of the coating layer 12 at 20 arbitrarily selected points on the cross-sectional SEM image of the coated active material 100 and calculating an average value from these measured values.

[0056] The average thickness of the coating layer 12 may be 1 nm or more and 300 nm or less. When the average thickness of the coating layer 12 is 1 nm or more, the surface of the positive electrode active material 11 can be sufficiently coated with the coating layer 12, thereby efficiently suppressing the formation of a resistance layer between the positive electrode active material 11 and the coating layer 12. When the average thickness of the coating layer 12 is 300 nm or less, the surface of the positive electrode active material 11 can be prevented from being excessively coated with the coating layer 12. As a result, an electron conduction path between particles of the positive electrode active material 11 is appropriately secured.

[0057] According to the above configuration, the internal resistance of the battery can be further reduced.

[0058] The coating of the positive electrode active material 11 with the coating layer 12 suppresses the formation of an oxide film due to oxidative decomposition of another solid electrolyte (e.g., the first solid electrolyte 21 described below) during charging of the battery. Therefore, with the above configuration, the coated active material 100 can reduce the internal resistance of the battery.

[0059] The coated active material 100 has, for example, a particle shape. There are no particular limitations on the particle shape of the coated active material 100. The particle shape of the coated active material 100 is needle-like, scale-like, spherical, or oval-spherical.

[0060] The types and amounts of elements contained in the coated active material 100 can be identified by known chemical analysis methods.

[0061] <Method for Producing Lithium-Containing Fluoride> The lithium-containing fluoride contained in the coating layer 12 can be produced, for example, by the following method.

[0062] Raw material powders are prepared so as to have the desired composition ratio. For example, Li 2.7 Ti 0.3 Al 0.7 When F is produced, LiF, AlF, and TiF are prepared in a molar ratio of 2.7:0.7:0.3. The values ​​"α," "β," and "γ" in the composition formula (2) can be adjusted by adjusting the raw materials, compounding ratio, and synthesis process.

[0063] After mixing the raw material powders, the raw material powders are mixed, pulverized, and reacted with each other using a mechanochemical milling method. Alternatively, after mixing the raw material powders, the mixture may be fired in a vacuum or in an inert atmosphere. For example, firing is performed at a temperature ranging from 100°C to 800°C for one hour or more. This produces a lithium-containing fluoride having the above-described composition.

[0064] The constitution of the crystalline phase (crystal structure) in the lithium-containing fluoride can be determined by adjusting the reaction method and reaction conditions of the raw material powders.

[0065] (Positive Electrode Active Material) The positive electrode active material 11 includes, for example, a material that has the property of absorbing and releasing metal ions such as lithium ions.

[0066] Examples of the positive electrode active material 11 include lithium-containing transition metal oxides, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxysulfides, and transition metal oxynitrides. Examples of polyanionic materials and fluorinated polyanionic materials include LiFePO, LiCoPO, LiCoPOF, LiMnSiO, and LiFeSiO. Examples of lithium-containing transition metal oxides include Li(Ni, Co, Al)O, Li(Ni, Co, Mn)O, and LiCoO, each of which has a layered rock salt structure. Using a lithium-containing transition metal oxide as the positive electrode active material 11 can reduce the manufacturing cost of the positive electrode and increase the average discharge voltage.

[0067] In the present disclosure, when an element in a formula is expressed as "(Ni, Co, Al)," this notation indicates at least one element selected from the group of elements in the parentheses. That is, "(Ni, Co, Al)" is synonymous with "at least one selected from the group consisting of Ni, Co, and Al." The same applies to other elements.

[0068] The positive electrode active material 11 has, for example, a particulate shape.

[0069] The positive electrode active material 11 may contain a lithium-nickel-containing oxide.

[0070] The positive electrode active material 11 may contain lithium nickel cobalt aluminum oxide.

[0071] According to the above configuration, the energy density of the battery can be increased.

[0072] The positive electrode active material 11 may be Li(Ni, Co, Al)O2.

[0073] Li(Ni,Co,Al)O2 includes those containing at least one additional element in addition to Li, Ni, Co, and Al. The additional element may be at least one or more elements selected from boron (B), sodium (Na), magnesium (Mg), silicon (Si), phosphorus (P), sulfur (S), potassium (K), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), copper (Cu), zinc (Zn), gallium (Ga), germanium (Ge), zirconium (Zr), niobium (Nb), molybdenum (Mo), indium (In), tin (Sn), tungsten (W), lanthanum (La), and cerium (Ce).

[0074] <Method for Producing Coated Active Material> The coated active material 100 in the first embodiment can be produced, for example, by the following method.

[0075] 2 is a flowchart showing a method for producing coated active material 100. The method for producing coated active material 100 includes annealing positive electrode active material 11 in a carbon dioxide gas atmosphere at a temperature of 100° C. or higher and 700° C. or lower (step S1), and coating at least a portion of the surface of positive electrode active material 11 with a coating material containing a lithium-containing fluoride (step S4).

[0076] First, the positive electrode active material 11 is annealed in a carbon dioxide gas atmosphere at a temperature of 100° C. or higher and 700° C. or lower (step S1). Hereinafter, the annealing treatment in a carbon dioxide gas atmosphere may be referred to as a "carbonate annealing treatment."

[0077] In step S1, the positive electrode active material 11 is annealed in a carbon dioxide atmosphere to control the amount of alkaline components on the surface of the positive electrode active material 11. The carbonation annealing causes the surface of the positive electrode active material 11 to be coated with a lithium carbonate component, thereby reducing the internal resistance of the battery. The positive electrode active material 11 may be carbonation annealed so that, when the mass of lithium bicarbonate present on the surface of the positive electrode active material 11 is measured by TG-MS, the ratio of the mass of lithium bicarbonate present on the surface of the positive electrode active material 11 to the mass of the positive electrode active material 11 is 130 ppm or more and 580 ppm or less.

[0078] Annealing the positive electrode active material 11 in a carbon dioxide atmosphere controls the alkaline components on the surface of the positive electrode active material 11, reducing the unstable lithium bicarbonate in the lithium carbonate component and stabilizing it as lithium carbonate. This prevents the reaction with water, thereby preventing the intermittent reaction between lithium ions and water on the surface of the positive electrode active material 11. This reduces the exchange of lithium ions and protons on the surface of the positive electrode active material 11, thereby reducing factors that inhibit the absorption and desorption of lithium ions. Furthermore, forming a coating of lithium carbonate components that do not decompose at high potential on the surface of the positive electrode active material 11 enhances oxidation resistance.

[0079] The control of the lithium-containing alkaline component on the surface of the positive electrode active material 11 by the carbonic acid annealing treatment is assumed to be based on the following mechanism. 0.8 Co 0.15 Al 0.05This is an ion chromatogram of water obtained by TG-MS measurement of O2. A change in the spectral shape is observed near 150°C, indicating that water present on the surface of the positive electrode active material 11 begins to be removed in this temperature range. This suggests that the alkaline component on the surface of the positive electrode active material 11 is controlled from this temperature range. The water release behavior converges around 400°C. At temperatures higher than 400°C, almost no water is released from the surface of the positive electrode active material 11. Therefore, the alkalinity on the surface of the positive electrode active material 11 can be controlled by performing the carbonation annealing treatment at 100°C or higher and 700°C or lower. The temperature of the carbonation annealing treatment may be 100°C or higher and 600°C or lower, 150°C or higher and 500°C or lower, or 150°C or higher and 400°C or lower. Step S1 controls the lithium-containing alkaline component present on the surface of the positive electrode active material 11, thereby obtaining a positive electrode active material 11 suitable for reducing the internal resistance of a battery.

[0080] If the temperature of the carbonic acid annealing treatment is 800° C. or higher, the positive electrode active material itself will be altered, and therefore this is not suitable for reducing the internal resistance of the battery.

[0081] The time for the carbonate annealing treatment is not particularly limited. The treatment time can be a time sufficient to control the lithium-containing alkaline component present on the surface of the positive electrode active material 11. The treatment time may be 0.5 hours or more and 10 hours or less.

[0082] The apparatus for performing step S1 is not particularly limited. For example, an electric furnace, a gas furnace, a high-frequency induction heating furnace, or the like can be used.

[0083] After step S1 is completed, the mass of lithium hydrogen carbonate present on the surface of the positive electrode active material 11 may be measured by TG-MS (step S2).

[0084] After completion of step S2, it may be determined whether the ratio of the mass of lithium bicarbonate present on the surface of positive electrode active material 11 to the mass of positive electrode active material 11 is 130 ppm or more and 580 ppm or less (step S3). Steps S1 to S3 may be repeated until the ratio of the mass of lithium bicarbonate present on the surface of positive electrode active material 11 to the mass of positive electrode active material 11 becomes 130 ppm or more and 580 ppm or less.

[0085] After step S3 is completed, at least a portion of the surface of the positive electrode active material 11, in which the mass ratio of lithium bicarbonate present on the surface of the positive electrode active material 11 to the mass of the positive electrode active material 11 is 130 ppm or more and 580 ppm or less, is coated with a coating material containing a lithium-containing fluoride (step S4). Step S4 is performed by combining the positive electrode active material 11 and the coating material. Step S4 forms a coating layer 12 that coats at least a portion of the surface of the positive electrode active material 11. This results in a coated active material 100.

[0086] The positive electrode active material 11 and the coating material are combined by, for example, a dry particle combining method. In the dry particle combining method, the positive electrode active material 11 and the coating material are mixed in an appropriate ratio, milled, and then mechanical energy is applied to the mixture. A mixing device such as a ball mill can be used for the milling. To suppress oxidation of the materials, the milling may be performed in a dry and inert atmosphere.

[0087] The treatment by the dry particle compositing method may include stirring the mixture containing the positive electrode active material 11 and the coating material while applying mechanical energy such as impact, compression, and shear. The dry particle compositing method allows for efficient production of the coated active material 100.

[0088] The device that can be used in step S4 is not particularly limited as long as it is capable of applying mechanical energy such as impact, compression, or shear to the mixture.

[0089] According to the above-described manufacturing method, the ratio of the mass of lithium present on the surface of the positive electrode active material 11 to the mass of the positive electrode active material 11 can be controlled within the above-described range, so that when the surface of the positive electrode active material 11 is coated with a coating material, the lithium-containing alkaline component present on the surface of the positive electrode active material 11 reacts with the lithium-containing fluoride contained in the coating material to prevent the coating layer 12 from deteriorating. That is, the generation of a resistance layer at the interface between the positive electrode active material 11 and the coating layer 12 due to the degeneration of the coating layer 12 is prevented. Therefore, the coated active material 100 manufactured by the above-described manufacturing method can reduce the internal resistance of a battery.

[0090] Second Embodiment Hereinafter, a second embodiment will be described. Descriptions that overlap with the first embodiment will be omitted as appropriate.

[0091] [Positive Electrode Material] FIG. 4 is a cross-sectional view showing a schematic configuration of a positive electrode material 200 according to the second embodiment.

[0092] The positive electrode material 200 of the second embodiment includes the coated active material 100 of the first embodiment and a first solid electrolyte 21. The coated active material 100 can be manufactured by the manufacturing method described above. The first solid electrolyte 21 has, for example, a particulate shape. The first solid electrolyte 21 can achieve high ionic conductivity in the positive electrode material 200.

[0093] (First Solid Electrolyte) The first solid electrolyte 21 includes a solid electrolyte having high ionic conductivity. The first solid electrolyte 21 may include a halide solid electrolyte. The halide solid electrolyte has high ionic conductivity and excellent high potential stability. Furthermore, the halide solid electrolyte has low electronic conductivity and high oxidation resistance, and is therefore less susceptible to oxidative decomposition upon contact with the coated active material 100. Therefore, when the first solid electrolyte 21 includes a halide solid electrolyte, the output characteristics of the battery can be improved.

[0094] Examples of halide solid electrolytes that can be used include Li(Ca, Y, Gd)X, LiMgX, LiFeX, Li(Al, Ga, In)X, Li(Al, Ga, In)X, and LiI. In these halide solid electrolytes, the element X is at least one selected from the group consisting of Cl, Br, and I.

[0095] The halide solid electrolyte may be free of sulfur.

[0096] The first solid electrolyte 21 may include a sulfide solid electrolyte, which has excellent ionic conductivity and flexibility. This configuration can improve the battery characteristics.

[0097] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, and Li 3.25 Ge 0.25 P 0.75 S4, Li 10 GeP2S 12 LiX, LiO, MO, etc. can be used. q , Li p MO q The element X in "LiX" is at least one element selected from the group consisting of F, Cl, Br, and I. q " and "Li p MO q " The element M is at least one element selected from the group consisting of P, Si, Ge, B, Al, Ga, In, Fe, and Zn. q " and "Li p MO q In the above formula, p and q are independent natural numbers.

[0098] The first solid electrolyte 21 may be a sulfide solid electrolyte. That is, the first solid electrolyte 21 may be made of a sulfide solid electrolyte. "Made of a sulfide solid electrolyte" means that, with the exception of inevitable impurities, no materials other than the sulfide solid electrolyte are intentionally added. For example, the sulfide solid electrolyte may contain lithium sulfide and phosphorus sulfide. For example, the sulfide solid electrolyte may be Li2S-P2S5.

[0099] The shape of the first solid electrolyte 21 is not particularly limited and may be, for example, spherical, oval, scale-like, fibrous, or particulate.

[0100] When the first solid electrolyte 21 is particulate (e.g., spherical), the median diameter may be 100 μm or less. When the median diameter is 100 μm or less, the coated active material 100 and the first solid electrolyte 21 can be well dispersed in the positive electrode material 200. As a result, the charge / discharge characteristics of the battery are improved. The median diameter of the first solid electrolyte 21 may be 10 μm or less.

[0101] In this specification, the term "median diameter" refers to the particle size when the cumulative volume in the volume-based particle size distribution is equal to 50%. The volume-based particle size distribution is measured, for example, by a laser diffraction measurement device or an image analysis device.

[0102] The median diameter of the first solid electrolyte 21 may be smaller than the median diameter of the coated active material 100. With this configuration, the coated active material 100 and the first solid electrolyte 21 can be dispersed in the positive electrode material 200 in a more favorable state.

[0103] The median diameter of the coated active material 100 may be 0.1 μm or more and 100 μm or less. When the median diameter of the coated active material 100 is 0.1 μm or more, the coated active material 100 and the first solid electrolyte 21 can form a well-dispersed state in the positive electrode material 200. As a result, the charge / discharge characteristics of the battery are improved. Furthermore, when the median diameter of the coated active material 100 is 100 μm or less, the lithium diffusion rate inside the positive electrode active material 11 is improved. This enables the battery to operate at high power.

[0104] The median diameter of the coated active material 100 may be larger than the median diameter of the first solid electrolyte 21. Even with this configuration, the coated active material 100 and the first solid electrolyte 21 can be well dispersed in the positive electrode material 200.

[0105] In the positive electrode material 200, the first solid electrolyte 21 and the coated active material 100 may be in contact with each other as shown in Fig. 4. In this case, the coating layer 12 and the first solid electrolyte 21 also contact each other. Particles of the first solid electrolyte 21 may fill the spaces between the particles of the coated active material 100.

[0106] In the coated active material 100, the coating layer 12 may uniformly coat the positive electrode active material 11. In other words, the coated active material 100 may be formed by coating the entire surface of the positive electrode active material 11 with the coating layer 12. The coating layer 12 prevents direct contact between the positive electrode active material 11 and the first solid electrolyte 21, and prevents the formation of an oxide film due to oxidative decomposition of the first solid electrolyte 21. Therefore, with this configuration, the internal resistance of the battery is further reduced.

[0107] In the coated active material 100, the coating layer 12 may cover only a portion of the surface of the positive electrode active material 11. In other words, the coated active material 100 may be formed by coating a portion of the surface of the positive electrode active material 11 with the coating layer 12.

[0108] The positive electrode material 200 may include a plurality of first solid electrolytes 21 and a plurality of coated active materials 100 .

[0109] The content of the first solid electrolyte 21 relative to the positive electrode material 200 and the content of the coated active material 100 relative to the positive electrode material 200 may be the same or different.

[0110] <Method for manufacturing the positive electrode material> The positive electrode material 200 is obtained by mixing the coated active material 100 and the first solid electrolyte 21. The method for mixing the coated active material 100 and the first solid electrolyte 21 is not particularly limited. For example, the coated active material 100 and the first solid electrolyte 21 may be mixed using a tool such as a mortar, or the coated active material 100 and the first solid electrolyte 21 may be mixed using a mixing device such as a ball mill. The mixing ratio of the coated active material 100 and the first solid electrolyte 21 is not particularly limited.

[0111] Third Embodiment Hereinafter, a third embodiment will be described. Descriptions that overlap with the first and second embodiments will be omitted as appropriate.

[0112] 5 is a cross-sectional view showing a schematic configuration of a battery 300 according to Embodiment 3. The battery 300 according to Embodiment 3 includes a positive electrode 31, an electrolyte layer 32, and a negative electrode 33. The electrolyte layer 32 is disposed between the positive electrode 31 and the negative electrode 33.

[0113] The positive electrode 31 includes the positive electrode material 200 of the second embodiment. That is, the positive electrode 31 includes the coated active material 100 and the first solid electrolyte 21. The positive electrode 31 includes a material having the property of absorbing and releasing metal ions (e.g., lithium ions).

[0114] According to the above configuration, the charge / discharge efficiency of the battery 300 can be improved.

[0115] The ratio "v1:100-v1" of the volume of the positive electrode active material 11 contained in the positive electrode 31 to the total volume of the coating material and the first solid electrolyte 21 may satisfy 30≦v1≦95. Here, v1 indicates the volume ratio of the positive electrode active material 11 when the total volume of the positive electrode active material 11, coating material, and first solid electrolyte 21 contained in the positive electrode 31 is taken as 100. When 30≦v1 is satisfied, it is easy to ensure a sufficient energy density of the battery 300. When v1≦95 is satisfied, it is easier for the battery 300 to operate at high output.

[0116] The thickness of the positive electrode 31 may be 10 μm or more and 500 μm or less. When the thickness of the positive electrode 31 is 10 μm or more, the energy density of the battery 300 is sufficiently ensured. When the thickness of the positive electrode 31 is 500 μm or less, the battery 300 can operate at high output.

[0117] The electrolyte layer 32 is a layer containing an electrolyte. The electrolyte is, for example, a solid electrolyte. The solid electrolyte contained in the electrolyte layer 32 is called a second solid electrolyte. That is, the electrolyte layer 32 may include a second solid electrolyte layer.

[0118] As the second solid electrolyte, at least one selected from the group consisting of a halide solid electrolyte, a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, and a complex hydride solid electrolyte can be used.

[0119] The second solid electrolyte may include a solid electrolyte having the same composition as the solid electrolyte included in the first solid electrolyte 21 in the second embodiment.

[0120] When the second solid electrolyte includes a halide solid electrolyte, the second solid electrolyte may include a halide solid electrolyte having the same composition as the halide solid electrolyte included in the first solid electrolyte 21 in embodiment 2. That is, the electrolyte layer 32 may include a halide solid electrolyte having the same composition as the halide solid electrolyte included in the first solid electrolyte 21 in embodiment 2. This configuration can further improve the battery characteristics.

[0121] The second solid electrolyte may include a solid electrolyte having a different composition from the solid electrolyte included in first solid electrolyte 21 in the second embodiment.

[0122] When the second solid electrolyte includes a halide solid electrolyte, the second solid electrolyte may include a halide solid electrolyte having a different composition from the halide solid electrolyte included in the first solid electrolyte 21 in embodiment 2. That is, the electrolyte layer 32 may include a halide solid electrolyte having a different composition from the halide solid electrolyte included in the first solid electrolyte 21 in embodiment 2. With such a configuration, the characteristics of the battery 300 can be further improved.

[0123] The second solid electrolyte may include a sulfide solid electrolyte. The second solid electrolyte may include a sulfide solid electrolyte having the same composition as the sulfide solid electrolyte included in the first solid electrolyte 21 of the second embodiment. That is, the electrolyte layer 32 may include a sulfide solid electrolyte having the same composition as the sulfide solid electrolyte included in the first solid electrolyte 21 of the second embodiment. According to the above configuration, since the electrolyte layer 32 includes a sulfide solid electrolyte having excellent reduction stability, a low-potential negative electrode material such as graphite or metallic lithium can be used for the negative electrode 33. This can improve the energy density of the battery 300. Furthermore, when the electrolyte layer 32 includes a sulfide solid electrolyte having the same composition as the sulfide solid electrolyte included in the first solid electrolyte 21 of the second embodiment, the characteristics of the battery 300 can be further improved.

[0124] The second solid electrolyte may include an oxide solid electrolyte, such as a NASICON-type solid electrolyte material represented by LiTi(PO) and its element substitution products, a (LaLi)TiO-based perovskite-type solid electrolyte material, or a Li 14 ZnGeO 16 , LiSiCON-type solid electrolyte materials such as LiSiO, LiGeO and their elemental substitution products, LiLaZrO 12 Garnet-type solid electrolyte materials, such as LiPO and its element substitution products, LiPO and its N-substituted products, glasses based on Li-B-O compounds such as LiBO and LiBO, and glass ceramics to which LiSO, LiCO, etc. are added, can be used.

[0125] The second solid electrolyte may include a polymer solid electrolyte. Examples of the polymer solid electrolyte include a compound of a polymer compound and a lithium salt. The polymer compound may have an ethylene oxide structure. A polymer compound having an ethylene oxide structure can contain a large amount of lithium salt. This can further increase ionic conductivity. Examples of the lithium salt include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), and LiC(SO2CF3)3. The lithium salt may be used alone or in combination.

[0126] The second solid electrolyte may include a complex hydride solid electrolyte, such as LiBH4-LiI or LiBH4-P2S5.

[0127] The electrolyte layer 32 may contain the second solid electrolyte as a main component. That is, the electrolyte layer 32 may contain the second solid electrolyte in a mass ratio of 50% or more (i.e., 50 mass% or more) relative to the entire electrolyte layer 32.

[0128] According to the above configuration, the characteristics of the battery 300 can be further improved.

[0129] The electrolyte layer 32 may contain the second solid electrolyte in a mass ratio of 70% or more (i.e., 70 mass % or more) relative to the entire electrolyte layer 32 .

[0130] According to the above configuration, the characteristics of the battery 300 can be further improved.

[0131] The electrolyte layer 32 contains the second solid electrolyte as a main component, and may further contain unavoidable impurities, or starting materials, by-products, decomposition products, and the like used in synthesizing the second solid electrolyte.

[0132] The electrolyte layer 32 may contain the second solid electrolyte in a mass ratio of 100% (i.e., 100 mass%) relative to the entire electrolyte layer 32, excluding unavoidable impurities. That is, the electrolyte layer 32 may be made of the second solid electrolyte. With the above configuration, the characteristics of the battery 300 can be further improved.

[0133] The electrolyte layer 32 may include two or more of the materials listed as the solid electrolyte as the second solid electrolyte. The two or more solid electrolytes have different compositions. For example, the electrolyte layer 32 may include a halide solid electrolyte and a sulfide solid electrolyte as the second solid electrolyte.

[0134] The thickness of the electrolyte layer 32 may be 1 μm or more and 300 μm or less. When the thickness of the electrolyte layer 32 is 1 μm or more, the possibility of a short circuit between the positive electrode 31 and the negative electrode 33 is reduced. Furthermore, when the thickness of the electrolyte layer 32 is 300 μm or less, the battery 300 can easily operate at high power. In other words, when the thickness of the electrolyte layer 32 is appropriately adjusted, sufficient safety of the battery 300 can be ensured and the battery 300 can be operated at high power.

[0135] The negative electrode 33 includes a material having the property of absorbing and releasing metal ions (e.g., lithium ions) and includes, for example, a negative electrode active material (e.g., negative electrode active material particles).

[0136] The negative electrode active material may be a metal material, a carbon material, an oxide, a nitride, a tin compound, or a silicon compound. The metal material may be a single metal. The metal material may be an alloy. Examples of the metal material include lithium metal or a lithium alloy. Examples of the carbon material include natural graphite, coke, partially graphitized carbon, carbon fiber, spherical carbon, artificial graphite, and amorphous carbon. Examples of the oxide include Li4Ti5O 12 , LiTi2O4, TiO2, etc. From the viewpoint of capacity density, silicon, tin, silicon compounds, or tin compounds can be suitably used.

[0137] The negative electrode 33 may include a solid electrolyte. The solid electrolyte that can be included in the negative electrode 33 is called a third solid electrolyte. That is, the negative electrode 33 may include the third solid electrolyte. With such a configuration, the lithium ion conductivity inside the negative electrode 33 is improved, enabling the battery 300 to operate at high output. As the third solid electrolyte that can be included in the negative electrode 33, the materials listed as examples of the second solid electrolyte of the electrolyte layer 32 can be used.

[0138] The median diameter of the negative electrode active material may be larger than the median diameter of the third solid electrolyte contained in the negative electrode 33. This allows the negative electrode active material and the third solid electrolyte to be well dispersed.

[0139] The ratio "v2:100-v2" of the volume of the negative electrode active material to the volume of the third solid electrolyte contained in the negative electrode 33 may satisfy 30≦v2≦95. Here, v2 indicates the volume ratio of the negative electrode active material when the total volume of the negative electrode active material and the third solid electrolyte contained in the negative electrode 33 is taken as 100. When 30≦v2 is satisfied, it is easy to ensure a sufficient energy density of the battery 300. When v2≦95 is satisfied, it is easier for the battery 300 to operate at high power.

[0140] The thickness of the negative electrode 33 may be 10 μm or more and 500 μm or less. When the thickness of the negative electrode 33 is 10 μm or more, it is easy to ensure a sufficient energy density of the battery 300. When the thickness of the negative electrode 33 is 500 μm or less, it is easier for the battery 300 to operate at high power.

[0141] At least one selected from the group consisting of the positive electrode 31, the electrolyte layer 32, and the negative electrode 33 may contain a binder to improve adhesion between particles. The binder is used to improve the binding of the materials constituting the electrode. Examples of binders include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polyhexyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyhexyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene-butadiene rubber, and carboxymethyl cellulose. The binder may be a copolymer of two or more materials selected from tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene. Alternatively, a mixture of two or more materials selected from these may be used as the binder.

[0142] At least one of the positive electrode 31 and the negative electrode 33 may contain a conductive additive to enhance electronic conductivity. Examples of conductive additives that can be used include graphites such as natural graphite or artificial graphite, carbon blacks such as acetylene black and ketjen black, conductive fibers such as carbon fiber or metal fiber, metal powders such as carbon fluoride and aluminum, conductive whiskers such as zinc oxide or potassium titanate, conductive metal oxides such as titanium oxide, and conductive polymer compounds such as polyaniline, polypyrrole, and polythiophene. Using a carbon conductive additive can reduce the cost of the battery 300.

[0143] The battery 300 can be configured as a battery of various shapes, such as a coin type, a cylindrical type, a square type, a sheet type, a button type, a flat type, or a laminated type.

[0144] The battery 300 can be manufactured, for example, by the following method.

[0145] The cathode material 200, the material for forming the electrolyte layer 32, and the material for forming the anode 33 in the second embodiment are prepared. A laminate in which the cathode 31, the electrolyte layer 32, and the anode 33 are arranged in this order is fabricated by a known method. In this way, the battery 300 is obtained.

[0146] The area of ​​the main surface of the battery 300 is, for example, 1 cm 2 Over 100cm 2 In this case, the battery 300 can be used in portable electronic devices such as smartphones and digital cameras. Alternatively, the area of ​​the main surface of the battery 300 is 100 cm or less. 2 More than 1000cm 2 In this case, the battery 300 can be used as a power source for large mobile equipment such as an electric vehicle. The "main surface" refers to the surface of the battery 300 that has the largest area.

[0147] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.

[0148] (Technology 1) A coated active material comprising: a positive electrode active material; lithium bicarbonate present on a surface of the positive electrode active material; and a coating layer coating at least a portion of the surface of the positive electrode active material, wherein the coating layer contains a lithium-containing fluoride, and when the mass of the lithium bicarbonate is measured by thermogravimetry and mass analysis, a ratio R1 of the mass of the lithium bicarbonate to the mass of the positive electrode active material is 130 ppm or more and 580 ppm or less.

[0149] This configuration can reduce the internal resistance of the battery.

[0150] (Technology 2) The coated active material according to Technology 1, wherein the ratio R1 is 155 ppm or more and 551 ppm or less. With this configuration, the internal resistance of the battery can be further reduced.

[0151] (Technology 3) The coated active material according to Technology 1 or 2, wherein the lithium-containing fluoride contains Li, Me1, Al, and F, and Me1 is at least one selected from the group consisting of Ti and Zr. This configuration can improve the ionic conductivity of the lithium-containing fluoride. As a result, the internal resistance of the battery can be further reduced.

[0152] (Technology 4) The lithium-containing fluoride is represented by the following composition formula (1): Li6-(m-mx+3x)b(Me1 1-x Me2 x ) b F6 ... Formula (1) where Me1 is at least one selected from the group consisting of Ti and Zr, Me2 is at least one selected from the group consisting of Al and Y, m is the valence of Me1, and 0 < x < 1 and 0 < b ≦ 3 are satisfied. This configuration can improve the ionic conductivity of the lithium-containing fluoride. As a result, the internal resistance of the battery can be further reduced.

[0153] (Technology 5) The coated active material according to Technology 4, wherein in the composition formula (1), 0.5≦xb<1 is satisfied. With this configuration, the ionic conductivity of the lithium-containing fluoride can be improved. As a result, the internal resistance of the battery can be further reduced.

[0154] (Technology 6) The coated active material according to Technology 4 or 5, wherein in the composition formula (1), 2.5≦6−(m−mx+3x)b≦2.9, 0.1≦(1−x)b≦0.5, and 0.5≦xb≦0.9 are satisfied. This configuration can improve the ionic conductivity of the lithium-containing fluoride. As a result, the internal resistance of the battery can be further reduced.

[0155] (Technology 7) The coated active material according to any one of Technologies 4 to 6, wherein in the composition formula (1), Me2 is Al. With this configuration, the internal resistance of the battery can be further reduced.

[0156] (Technology 8) The lithium-containing fluoride is Li 2.7 Ti 0.3 Al 0.7 F6 and Li 2.8 Zr 0.2 Al 0.8 The coated active material according to any one of Techniques 1 to 7, wherein the coated active material is at least one selected from the group consisting of F6. According to this configuration, the internal resistance of the battery can be further reduced.

[0157] (Technology 9) The coated active material according to any one of Technologies 1 to 8, wherein the positive electrode active material contains a lithium-nickel-containing oxide. With this configuration, the internal resistance of the battery can be reduced.

[0158] (Technology 10) The coated active material according to any one of Technologies 1 to 9, wherein the positive electrode active material contains lithium nickel cobalt aluminum oxide. With this configuration, the energy density of the battery can be increased.

[0159] (Technology 11) A method for producing a coated active material, comprising: annealing a positive electrode active material at a temperature of 100°C or higher and 700°C or lower in a carbon dioxide gas atmosphere; and coating at least a portion of a surface of the positive electrode active material with a coating material containing a lithium-containing fluoride, wherein the coating is performed by combining the positive electrode active material and the coating material.

[0160] This configuration makes it possible to produce a coated active material that can reduce the internal resistance of the battery.

[0161] (Technology 12) The method for producing a coated active material according to Technology 11, wherein the annealing temperature is 150° C. or more and 400° C. or less. With this configuration, it is possible to produce a coated active material that can further reduce the internal resistance of a battery.

[0162] (Technology 13) The method for producing a coated active material according to Technology 11 or 12, further comprising measuring the mass of lithium bicarbonate present on the surface of the positive electrode active material by thermogravimetry and mass spectrometry between the annealing treatment and the coating. With this configuration, a coated active material capable of reducing the internal resistance of a battery can be produced.

[0163] (Technology 14) The method for producing a coated active material according to Technology 13, further comprising, between the measuring and the coating, determining whether or not a ratio of the mass of the lithium hydrogen carbonate to the mass of the positive electrode active material is 130 ppm or more and 580 ppm or less. With this configuration, it is possible to produce a coated active material that can reduce the internal resistance of a battery.

[0164] (Technology 15) A positive electrode material comprising: the coated active material according to any one of Technologies 1 to 10; and a first solid electrolyte.

[0165] This configuration reduces the internal resistance of the battery.

[0166] (Technology 16) The positive electrode material according to Technology 15, wherein the first solid electrolyte includes a halide solid electrolyte. With this configuration, the internal characteristics of the battery can be improved.

[0167] (Technology 17) The positive electrode material according to Technology 14 or 15, wherein the first solid electrolyte contains a sulfide solid electrolyte. With this configuration, the internal characteristics of the battery can be further improved.

[0168] (Technology 18) A battery comprising a positive electrode containing the positive electrode material according to any one of technologies 15 to 17.

[0169] This configuration can reduce the internal resistance.

[0170] (Technology 19) A battery comprising: a positive electrode containing the positive electrode material according to any one of technologies 15 to 17; a negative electrode; and an electrolyte layer provided between the positive electrode and the negative electrode.

[0171] This configuration can reduce the internal resistance.

[0172] (Technology 20) The battery according to Technology 19, wherein the electrolyte layer includes a second solid electrolyte, and the second solid electrolyte includes a halide solid electrolyte having the same composition as the solid electrolyte included in the first solid electrolyte. With this configuration, output characteristics can be improved.

[0173] (Technology 21) The battery according to Technology 19 or 20, wherein the electrolyte layer includes a second solid electrolyte, and the second solid electrolyte includes a halide solid electrolyte having a different composition from the solid electrolyte included in the first solid electrolyte. With this configuration, output characteristics can be improved.

[0174] (Technology 22) The battery according to any one of claims 19 to 21, wherein the electrolyte layer includes a second solid electrolyte, and the second solid electrolyte includes a sulfide solid electrolyte. With this configuration, output characteristics can be further improved.

[0175] The present disclosure will be described in detail below using examples. The following examples are merely illustrative, and the present disclosure is not limited to the following examples.

[0176] Example 1 Carbonate Annealing of Positive Electrode Active Material Li(Ni, Co, Al)O2 (hereinafter referred to as NCA) with an average particle size of 5 μm was prepared as a positive electrode active material. 500 g of NCA was placed inside a small tubular furnace. The internal temperature of the small tubular furnace was set to 150°C, and carbon dioxide gas was flowed into the small tubular furnace at a rate of 10 mL / min. The NCA was then annealed for 2 hours. This resulted in the positive electrode active material of Example 1.

[0177] [Preparation of Coating Material (Lithium-Containing Fluoride)] In a glove box with an argon atmosphere controlled to a dew point of −60° C. or less and an oxygen value of 5 ppm or less, raw material powders of LiF, AlF, and TiF were weighed out to a molar ratio of LiF:AlF:TiF=2.7:0.7:0.3. These raw material powders were mixed in an agate mortar to obtain a mixture. Next, the mixture was milled using a planetary ball mill (Fritsch, Model P-7) at 500 rpm for 12 hours. This resulted in Li 2.7 Ti 0.3 Al 0.7A compound represented by the formula F6 (hereinafter referred to as LTAF) was obtained. The compound was mixed with an appropriate amount of solvent and milled using a planetary ball mill at 200 rpm for 20 minutes. The solvent was then removed by drying. This resulted in the production of LTAF powder as a coating material (lithium-containing fluoride). The average particle size of the LTAF powder was 0.5 μm.

[0178] The average particle size of LTAF was calculated from a planar SEM image of LTAF taken with a scanning electron microscope (Keyence Corporation, 3D Real Surface View Microscope, VE-8800, magnification 5000). Specifically, the average value of the circle-equivalent diameters of 50 particles randomly selected from the planar SEM image of LTAF was calculated as the average particle size.

[0179] [Preparation of Coated Active Material] Coating of the positive electrode active material of Example 1 with LTAF was carried out using a particle compositing device (Nobilta NOB-MINI, manufactured by Hosokawa Micron Corporation). 48.5 g of positive electrode active material and 1.5 g of LTAF were placed in the NOB-MINI container. The NCA and LTAF were composited under the conditions of a rotation speed of 6000 rpm, an operating time of 60 minutes, and a power value of 550 W to 740 W. This resulted in the production of the coated active material of Example 1. The ratio of the volume of LTAF to the total volume of the NCA and LTAF was 4.6%.

[0180] Example 2 A coated active material of Example 2 was obtained in the same manner as in Example 1, except that the internal temperature of the small tubular furnace was set to 400° C. in the carbonate annealing treatment of the positive electrode active material.

[0181] Comparative Example 1 A coated active material of Comparative Example 1 was obtained in the same manner as in Example 1, except that the internal temperature of the small tubular furnace was set to 800° C. in the carbonate annealing treatment of the positive electrode active material.

[0182] Comparative Example 2 A coated active material of Comparative Example 2 was obtained in the same manner as in Example 1, except that NCA that had not been subjected to the carbonate annealing treatment was coated with LTAF.

[0183] (Measurement of the Mass of Lithium Bicarbonate Present on the Surface of the Cathode Active Material) The following steps were performed on the uncoated cathode active materials of each of the Examples and Comparative Examples. First, 1 g of calcium oxalate hydrate was pyrolyzed by TG-MS in a 1% argon reference gas environment to obtain extracted ion chromatograms of argon and carbon dioxide. From the extracted ion chromatograms, the sensitivity coefficient was calculated by dividing the carbon dioxide spectral intensity per 1 mol of carbon dioxide by the argon spectral intensity per 1 mol of argon. The sensitivity coefficient was 2.1. Next, 0.1 g of powder of each of the uncoated cathode active materials of each of the Examples and Comparative Examples was measured by TG-MS in an argon gas environment to obtain an ion chromatogram of carbon dioxide. In the obtained spectra, the integrated value of the spectral intensity up to 300°C was considered to correspond to the amount of lithium bicarbonate, and the mass of lithium bicarbonate present on the surface of the cathode active material was calculated in molar terms using the sensitivity coefficient described above. From the calculated value, the ratio R1 of the mass of lithium hydrogen carbonate present on the surface of the positive electrode active material to the mass of the positive electrode active material was calculated. The results are shown in Table 1.

[0184] (Measurement of the Mass of Lithium-Containing Alkaline Component Present on the Surface of the Positive Electrode Active Material) The following process was performed on the uncoated positive electrode active materials of each Example and Comparative Example. 2 g of positive electrode active material and 200 mL of ion-exchanged water were placed in a beaker, stirred for 30 minutes, and then allowed to stand for 10 minutes. Next, the supernatant was filtered through a syringe filter with a pore size of 0.2 μm, and the resulting filtrate was used as a test solution. Phenolphthalein solution was added to the test solution as an indicator, and neutralization titration was performed using a 0.1 mol / L aqueous HCl solution under a nitrogen atmosphere. After the endpoint was detected with phenolphthalein, methyl orange solution was added to the test solution as an indicator, and neutralization titration was performed using a 0.1 mol / L aqueous HCl solution under a nitrogen atmosphere. Assuming that lithium hydroxide (LiOH) and lithium carbonate (Li2CO3) were present on the surface of the positive electrode active material, the mass of lithium hydroxide and the mass of lithium carbonate contained in the test solution were calculated from the amount of HCl required to reach the endpoint of each reaction. The mass of this lithium carbonate is the mass of lithium carbonate present on the surface of the positive electrode active material. The mass of lithium derived from lithium carbonate was calculated from the mass of lithium carbonate. The mass of lithium derived from lithium hydroxide was calculated from the mass of lithium hydroxide. The sum of the calculated mass of lithium derived from lithium hydroxide and the mass of lithium derived from lithium carbonate is the mass of lithium derived from the lithium-containing alkaline component present on the surface of the positive electrode active material. From each calculated value and the mass of the positive electrode active material, the ratio R2 of the mass of lithium derived from the lithium-containing alkaline component to the mass of the positive electrode active material, and the ratio R3 of the mass of lithium hydroxide to the mass of the positive electrode active material were calculated. The results are shown in Table 1.

[0185] [Fabrication of Evaluation Batteries] The following steps were carried out using the coated active materials of the examples and comparative examples.

[0186] (Preparation of Positive Electrode Layer Paste) 4.0 g of coated active material, 0.094 g of VGCF as a conductive material, 1.024 g of LiI-LiBr-Li2S-P2S5-based glass ceramic (10LiI 15LiBr 75 (0.75Li2S 0.25P2O5)) as a first solid electrolyte, 0.017 g of butadiene rubber-based binder, and 2.77 g of tetralin were weighed and mixed using an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation). The resulting mixture was used as a positive electrode layer paste. "VGCF" is a registered trademark of Showa Denko KK

[0187] (Preparation of negative electrode layer paste) Li4Ti5O as negative electrode active material 12 3.0 g of particles (density 3.5 g / cc), 0.033 g of conductive carbon (density 2 g / cc), 0.039 g of butadiene rubber binder (density 0.9 g / cc), and 3.71 g of tetralin were weighed and mixed for 30 minutes using an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation). Then, 1.0 g of LiI-LiBr-LiS-P2S5-based glass ceramic (10LiI 15LiBr 75 (0.75LiS 0.25P2O5), density 2 g / cc) was added as a sulfide-based solid electrolyte to the resulting slurry, and the mixture was mixed again for 30 minutes using an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation). The resulting mixture was used as a paste for the negative electrode layer.

[0188] (Preparation of Paste for Electrolyte Layer) Heptane, a heptane solution containing 5% by mass of a butadiene rubber binder, and 1.0 g of a LiI-LiBr-LiS-P2S5-based glass ceramic having an average particle size of 2.5 μm as a second solid electrolyte were added to a polypropylene container and mixed for 30 seconds using an ultrasonic homogenizer (UH-50 manufactured by SMT Corporation). Next, the container was shaken for 3 minutes using a shaker to obtain a paste for a solid electrolyte layer.

[0189] (Preparation of all-solid-state lithium-ion secondary battery) Using an applicator, the paste for the positive electrode layer was applied to a positive electrode current collector (Al foil, thickness 15 μm) by the blade method. After application, the paste was dried on a hot press at 100 ° C. for 30 minutes to obtain a positive electrode having a positive electrode active material layer on the surface of the aluminum foil. Similarly to the positive electrode, the paste for the negative electrode layer was applied to a negative electrode current collector (Ni foil, thickness 22 μm) and dried to obtain a negative electrode having a negative electrode active material layer on the surface of the Ni foil. In all of Examples 1 to 2 and Comparative Examples 1 and 2, the basis weight of the negative electrode active material layer was adjusted so that the charge specific capacity of the negative electrode was 1.15 times that of the charge specific capacity of the positive electrode when the charge specific capacity was 185 mAh / g.

[0190] The positive electrode was pre-pressed. A paste for a solid electrolyte layer was applied to the surface of the positive electrode active material layer of the pre-pressed positive electrode using a die coater, and the paste was dried on a hot plate at 100°C for 30 minutes. Thereafter, a pressure of 2 ton / cm 2 The laminate was roll-pressed at 800 kJ / min to obtain a positive electrode-side laminate having a solid electrolyte layer on the surface of the positive electrode.

[0191] The negative electrode was pre-pressed. A paste for a solid electrolyte layer was applied to the surface of the negative electrode active material layer of the pre-pressed negative electrode using a die coater, and the paste was dried on a hot plate at 100°C for 30 minutes. Thereafter, a pressure of 2 ton / cm 2 The laminate was roll-pressed at 800 kJ / min to obtain a negative electrode-side laminate having a solid electrolyte layer on the surface of the negative electrode.

[0192] The positive electrode side laminate and the negative electrode side laminate were each punched and then laminated together so that the solid electrolyte layers were bonded to each other. Here, the laminates were laminated in a state in which an unpressed solid electrolyte layer (solid electrolyte layer paste) was transferred between the solid electrolyte layer of the positive electrode side laminate and the solid electrolyte layer of the negative electrode side laminate. Thereafter, the laminates were laminated together at 160°C with a pressure of 2 ton / cm. 2 The resulting power generating element was sealed with a laminate and restrained at 0.5 MPa to form an all-solid-state lithium ion secondary battery (battery stack) for evaluation.

[0193] (Evaluation) The test batteries of the Examples and Comparative Examples were evaluated according to the following procedures.

[0194] (Initial Resistance) The secondary battery was placed in a thermostatic chamber at 25°C. The following constant current, constant voltage (CCCV) charging and CCCV discharging were repeated twice. The battery was charged at a constant current of 0.33 C relative to the theoretical capacity of the battery until a voltage of 2.7 V was reached, and then charged at a constant voltage of 2.7 V. Charging was terminated at a current value resulting in a 0.01 C rate. Next, the battery was discharged at a constant current of 0.33 C until a voltage of 1.5 V was reached, and then discharged at a constant voltage of 1.5 V. Discharge was terminated at a current value resulting in a 0.01 C rate.

[0195] Next, the state of charge of the test battery was adjusted by CCCV charging as follows: The battery was charged at a constant current of 0.33 C relative to the theoretical capacity of the battery until the voltage reached 2.0 V, and then the battery was charged at a constant voltage of 2.0 V. Charging was terminated at a current of 0.01 C rate.

[0196] After adjusting the state of charge, 12mA / cm 2 The test battery was discharged for 2 seconds at a current of 0.01 V, and the internal resistance of the battery was determined by dividing the voltage change by the discharge current. The results are shown in Table 1.

[0197]

[0198] (Results) Examples 1 and 2 exhibited reduced resistance compared to Comparative Example 2, in which the positive electrode active material was not subjected to carbonation annealing. Furthermore, Examples 1 and 2 exhibited reduced resistance compared to Comparative Example 1, in which carbonation annealing was performed at 800°C. As described above, water removal from the positive electrode active material begins at 150°C, and it is presumed that the carbonation annealing at 150°C controls the alkaline components on the surface of the positive electrode active material. Furthermore, since water release converges around 400°C, it is presumed that performing the carbonation annealing in a state in which water near the surface has been removed achieves more effective surface control. These effects reduced the internal resistance of the battery. While water release from the surface of the positive electrode active material does not occur at temperatures higher than 400°C, annealing at high temperatures, such as 800°C, is presumed to increase resistance due to changes in the crystalline structure of the NCA itself.

[0199] On the other hand, even if the annealing temperature is in a range higher than 400°C, as long as the change in the crystalline structure of the active material that causes an increase in the battery resistance does not occur, the resistance is 6.8 Ωcm 2 It is believed that it is quite possible to achieve a smaller resistance.

[0200] The battery of the present disclosure can be used, for example, as an all-solid-state lithium secondary battery.

Claims

1. A coated active material comprising a positive electrode active material, lithium hydrogen carbonate present on the surface of the positive electrode active material, and a coating layer covering at least a part of the surface of the positive electrode active material, wherein the coating layer contains a lithium-containing fluoride, and when the mass of the lithium hydrogen carbonate is measured by thermogravimetric-mass spectrometry, the ratio R1 of the mass of the lithium hydrogen carbonate to the mass of the positive electrode active material is 130 ppm or more and 580 ppm or less.

2. The coated active material according to claim 1, wherein the ratio R1 is 155 ppm or more and 551 ppm or less.

3. The coated active material according to claim 1, wherein the lithium-containing fluoride contains Li, Me1, Al, and F, and Me1 is at least one selected from the group consisting of Ti and Zr.

4. The lithium-containing fluoride is represented by the following compositional formula (1): Li6-(m - mx + 3x)b(Me1 1-x Me2 x ). b F6... Formula (1) Here, Me1 is at least one selected from the group consisting of Ti and Zr, Me2 is at least one selected from the group consisting of Al and Y, m is the valence of Me1, 0 < x < 1, and 0 < b ≤ 3 are satisfied. The coated active material according to claim 1.

5. The coated active material according to claim 4, wherein in the composition formula (1), 0.5 ≦ xb < 1 is satisfied.

6. The coated active material according to claim 4, wherein in the composition formula (1), 2.5 ≦ 6-(m - mx + 3x)b ≦ 2.9, 0.1 ≦ (1 - x)b ≦ 0.5, and 0.5 ≦ xb ≦ 0.9 are satisfied.

7. The coated active material according to claim 4, wherein in the composition formula (1), Me2 is Al.

8. The lithium-containing fluoride is Li 2.7 Ti 0.3 Al 0.7 F6 and Li 2.8 Zr 0.2 Al 0.8 F6, and is at least one selected from the group consisting of, the coating active material according to claim 1.

9. The coated active material according to claim 1, wherein the positive electrode active material contains a lithium nickel-containing oxide.

10. The coated active material according to claim 1, wherein the positive electrode active material contains a lithium nickel cobalt aluminum oxide.

11. A method for manufacturing a coated active material, comprising annealing a positive electrode active material at a temperature of 100°C or higher and 700°C or lower in a carbon dioxide atmosphere, and coating at least a part of the surface of the positive electrode active material with a coating material containing a lithium-containing fluoride, wherein the coating is performed by compounding the positive electrode active material and the coating material.

12. The method for manufacturing a coated active material according to claim 11, wherein the temperature of the annealing treatment is 150°C or higher and 400°C or lower.

13. The method for manufacturing a coated active material according to claim 11, comprising measuring the mass of lithium hydrogen carbonate present on the surface of the positive electrode active material by thermogravimetric-mass spectrometry between the annealing and the coating.

14. The method for manufacturing a coated active material according to claim 13, including determining whether the ratio of the mass of lithium hydrogen carbonate to the mass of the positive electrode active material is 130 ppm or more and 580 ppm or less between the measurement and the coating.

15. A positive electrode material comprising the coated active material according to any one of claims 1 to 10 and a first solid electrolyte.

16. The positive electrode material according to claim 15, wherein the first solid electrolyte includes a halide solid electrolyte.

17. The positive electrode material according to claim 15, wherein the first solid electrolyte includes a sulfide solid electrolyte.

18. A battery comprising a positive electrode including the positive electrode material according to claim 15.

19. A battery comprising a positive electrode including the positive electrode material according to claim 15, a negative electrode, and an electrolyte layer provided between the positive electrode and the negative electrode.

20. The battery according to claim 19, wherein the electrolyte layer includes a second solid electrolyte, and the second solid electrolyte includes a halide solid electrolyte having the same composition as the solid electrolyte included in the first solid electrolyte.

21. The battery according to claim 19, wherein the electrolyte layer includes a second solid electrolyte, and the second solid electrolyte includes a halide solid electrolyte having a composition different from that of the solid electrolyte included in the first solid electrolyte.

22. The battery according to claim 19, wherein the electrolyte layer includes a second solid electrolyte, and the second solid electrolyte includes a sulfide solid electrolyte.

Citation Information

Patent Citations

  • Preparation method for lithium ion battery cathode material fluorine-doped lithium vanadate with circulatory stability

    CN105529450A

  • Lithium-rich positive electrode material and preparation method thereof, and secondary lithium battery

    CN108123106A

  • Lithium ion secondary battery

    JP2015095330A

  • Coated active material, method for producing coated active material, positive electrode material and battery

    WO2023037776A1