Cladding material for wire bonding, bonding structure using cladding material for wire bonding, and battery manufacturing method
The use of a cladding material with an Al layer and an Fe layer in wire bonding enhances bonding strength by preventing intermetallic compound formation and ensuring secure contact, addressing the weakness in conventional methods and maintaining performance under load and thermal stress.
Patent Information
- Application Number
- PCT/JP2024/016565
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-04-26
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional wire bonding methods between aluminum-based wires and copper phosphate or nickel-plated steel bus bars often result in the formation of weak intermetallic compounds, leading to reduced bonding strength due to the use of different metals.
A cladding material composed of an Al layer made of pure aluminum or aluminum alloy and an Fe layer made of iron-based alloy, with the Al layer thickness being 20 μm or more, is used to bond the Al-based wire, preventing the formation of fragile intermetallic compounds and enhancing bonding strength by ensuring secure contact and reducing deformation.
The proposed solution significantly improves the bonding strength between the Al-based wire and the cladding material, maintaining high bonding strength even under load and thermal shock conditions, while maintaining conductivity and workability.
Smart Images

Figure JP2024016565_28112024_PF_FP_ABST
Abstract
Description
Clad material for wire bonding, bonded structure using clad material for wire bonding, and method for manufacturing battery
[0001] The present invention relates to a clad material for wire bonding, a joint structure using the clad material for wire bonding, and a method for manufacturing a battery.
[0002] Batteries having a structure in which the battery and a bus bar are joined by wire bonding are known. A battery having such a structure is disclosed in, for example, Japanese Patent Application Laid-Open No. 2010-282811.
[0003] Japanese Patent Application Publication No. 2010-282811 discloses a battery pack consisting of a plurality of unit cells. In this publication, a plurality of unit cells are arranged side by side, and adjacent unit cells are electrically connected by a bus bar (lead plate). In this publication, one end of an aluminum wire is bonded to an end of the unit cell by wire bonding, and the other end of the aluminum wire is bonded to the bus bar by wire bonding, thereby bonding the unit cells and the bus bar together. In this publication, the bus bar is made of copper phosphate or nickel-plated steel sheet.
[0004] JP 2010-282811 A
[0005] In the above-mentioned Japanese Patent Laid-Open No. 2010-282811, since the Al-based wire made of aluminum used for wire bonding and the other member (bus bar) made of copper phosphate or nickel-plated steel sheet to which the wire is bonded are made of different metals, a brittle intermetallic compound may be formed at the bonded portion between the Al-based wire and the other member, which may weaken the bond strength between the wire and the other member. Therefore, there is a demand for improving the bond strength when bonding Al-based wires.
[0006] The present invention has been made to solve the above-mentioned problems, and one object of the present invention is to provide a clad material for wire bonding that can improve the bonding strength when an Al-based wire is bonded by wire bonding, a bonding structure using the clad material for wire bonding, and a method for manufacturing a battery.
[0007] In order to achieve the above object, the inventors of the present application have intensively studied the placement of a clad material between an aluminum wire and another member such as a bus bar, and have found the following configuration: A clad material for wire bonding according to a first aspect of the present invention is a clad material for wire bonding to which an Al-based wire for bonding is bonded by wire bonding, and is composed of an Al layer made of pure aluminum or an aluminum alloy, and an Fe layer made of an iron-based alloy and roll-bonded to the Al layer, the Al layer having a thickness of 20 μm or more, and the Al-based wire for bonding is bonded to the Al layer by wire bonding.
[0008] As described above, the clad material for wire bonding according to a first aspect of the present invention is composed of an Al layer made of pure aluminum or an aluminum alloy and an Fe layer made of an iron-based alloy roll-bonded to the Al layer, the Al layer having a thickness of 20 μm or more, and an Al-based wire for bonding is bonded to the Al layer by wire bonding. Since the Al layer and the Al-based wire are the same metal, the formation of a brittle intermetallic compound at the bonded portion between the Al-based wire and the Al layer can be suppressed during wire bonding. As a result, the bond strength when the Al-based wire is bonded to the clad material for wire bonding can be improved. Furthermore, experiments described below have shown that the thickness of the Al layer of 20 μm or more can improve the bond strength when the Al-based wire is bonded to the Al layer of the clad material for wire bonding.
[0009] In the clad material for wire bonding according to the first aspect, the thickness of the Al layer is preferably 60 μm or less. With this configuration, even when a load is applied when bonding an Al-based wire to the clad material for wire bonding, the Al layer, which is softer than the Fe layer, is thicker, and this prevents the Al layer from significantly deforming and forming a gap between the Al-based wire and the Al layer. By preventing the formation of a gap between the Al-based wire and the Al layer, a load can be applied while the Al-based wire and the Al layer are in reliable contact with each other, resulting in a stronger bond. Furthermore, experiments described below have shown that by setting the thickness of the Al layer to 60 μm or less, the bonding strength when bonding the Al-based wire to the Al layer can be sufficiently increased.
[0010] In the clad material for wire bonding according to the first aspect, the thickness of the Al layer is preferably smaller than the thickness of the Fe layer. With this configuration, the thickness of the Fe layer, which is harder than the Al layer, can be increased, thereby improving the strength of the clad material for wire bonding and suppressing deformation of the clad material for wire bonding even when a load is applied when joining an Al-based wire to the clad material for wire bonding by wire bonding.
[0011] In the clad material for wire bonding according to the first aspect, the Fe layer is preferably made of ferritic stainless steel. By using ferritic stainless steel, which is softer than other stainless steels, the difference in hardness between the Fe layer and the Al layer can be reduced. This allows the Fe layer to be stretched in accordance with the Al layer when the clad material for wire bonding is rolled, thereby suppressing variations in thickness of the Fe layer.
[0012] In this case, the Fe layer is preferably made of SUS 430. By configuring in this manner, the use of SUS 430, which is a versatile ferritic stainless steel with excellent workability, can improve the workability and productivity of the clad material for wire bonding.
[0013] In the wire bonding clad material according to the first aspect, the Al layer is preferably made of A1050. With this configuration, the use of A1050, which has high conductivity, can improve the conductivity of the wire bonding clad material. As a result, when the wire bonding clad material is used between a cell and a bus bar that constitute a battery pack, for example, it is possible to prevent a decrease in conductivity due to the wire bonding clad material compared to when the cell and the bus bar are directly joined.
[0014] A bonding structure using a clad material for wire bonding according to a second aspect of the present invention comprises a clad material for wire bonding including an Al layer made of pure aluminum or an aluminum alloy and an Fe layer made of an iron-based alloy and roll-bonded to the Al layer, the Al layer having a thickness of 20 μm or more, and a plate-like member made of pure aluminum or an aluminum alloy, wherein one end of an Al-based wire for bonding is bonded to the Al layer by wire bonding, and the other end of the Al-based wire is bonded to the plate-like member.
[0015] A bonding structure using a clad material for wire bonding according to a second aspect of the present invention includes, as described above, a clad material for wire bonding including an Al layer made of pure aluminum or an aluminum alloy, the Al layer having a thickness of 20 μm or more, and a plate-shaped member made of pure aluminum or an aluminum alloy. The plate-shaped member may be a bus bar or the like. Since the Al layer and the Al-based wire are the same metal, the formation of a brittle intermetallic compound at the bonded portion between the Al-based wire and the Al layer can be suppressed during bonding. As a result, the bonding strength when the Al-based wire is bonded to the clad material for wire bonding can be improved. Furthermore, experiments described below have shown that a thickness of the Al layer of 20 μm or more can provide a bonding structure with high bonding strength when the Al-based wire is bonded to the Al layer of the clad material for wire bonding.
[0016] In the bonding structure using the clad material for wire bonding according to the second aspect, the bonding strength between the Al-based wire and the Al layer is preferably 9.8 N or more. With this configuration, the bonding strength between the Al-based wire and the clad material for wire bonding can be made sufficiently large for practical use.
[0017] A battery manufacturing method according to a third aspect of the present invention includes the steps of: preparing a clad material for wire bonding by roll-bonding an Al plate material made of pure aluminum or an aluminum alloy with an Fe plate material made of an iron-based alloy, the clad material being composed of an Al layer and an Fe layer, where the Al layer has a thickness of 20 μm or more; bonding a battery terminal member made of an iron-based alloy to the Fe layer; bonding one end of an Al-based wire for bonding to the Al layer by wire bonding; and bonding the other end of the Al-based wire to a bus bar made of pure aluminum or an aluminum alloy.
[0018] A battery manufacturing method according to a third aspect of the present invention includes the steps of preparing a clad material for wire bonding, in which the thickness of the Al layer is 20 μm or more, and joining one end of an Al-based wire for bonding to the Al layer by wire bonding. Because the Al layer and the Al-based wire are the same metal, the formation of a brittle intermetallic compound at the bonded portion between the Al-based wire and the Al layer can be suppressed. As a result, a clad material for wire bonding can be manufactured that can improve the bond strength when the Al-based wire is bonded by wire bonding. Furthermore, the experiment described below has found that the thickness of the Al layer is 20 μm or more, which can improve the bond strength between the Al-based wire and the Al layer of the clad material for wire bonding.
[0019] According to the present invention, it is possible to provide a clad material for wire bonding that can improve the bonding strength when an Al-based wire is bonded by wire bonding, a bonding structure using the clad material for wire bonding, and a method for manufacturing a battery.
[0020] 1A and 1B are diagrams showing a battery pack according to the present embodiment, with FIG. 1A showing a perspective view and FIG. 1B showing a cross-sectional view. FIG. 1B is a diagram showing an example of a clad material for wire bonding according to the present embodiment. FIG. 1C is a diagram showing a state in which a clad material for wire bonding according to the present embodiment and a bus bar are joined by an Al-based wire. FIG. 1D is a diagram showing an example of a unit cell according to the present embodiment. FIG. 1E is a diagram showing a method for manufacturing a clad material for wire bonding according to the present embodiment. FIG. 1F is a diagram for explaining a method for joining a clad material for wire bonding according to the present embodiment to a battery terminal. FIG. 1G is a diagram showing a laser irradiation position when laser welding a clad material for wire bonding according to the present embodiment to a battery terminal. FIG. 1H is a diagram for explaining a wire bonding method according to the present embodiment. FIG. 1I is a graph showing the bonding strength of SUS430 wire-bonded with an Al-based wire and a clad material for wire bonding. FIG. 1J is a graph showing the results of a thermal shock test of SUS430 wire-bonded with an Al-based wire and a clad material for wire bonding.
[0021] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0022] As shown in FIG. 1 , a clad material for wire bonding 1 according to an embodiment of the present invention is used in a battery pack 100. The battery pack 100 is configured by electrically connecting a plurality of lithium-ion secondary batteries 10 via bus bars 20. Note that while the battery pack 100 is depicted in a simplified form in FIG. 1 , the number of lithium-ion secondary batteries 10 constituting the battery pack 100 for automotive use is greater than the number shown in FIG. 1 . The automotive battery pack 100 is a large battery system mounted in an electric vehicle (EV) or a hybrid electric vehicle (HEV). Note that the battery pack 100 is an example of a "battery" as defined in the claims. The bus bars 20 are an example of a "plate-like member" as defined in the claims.
[0023] As shown in Fig. 2, the clad material for wire bonding 1 is composed of an Al layer 1a and an Fe layer 1b. In Fig. 2, the clad material for wire bonding 1 has a circular shape, but the shape of the clad material for wire bonding 1 is not limited to this.
[0024] The Al layer 1a is made of pure aluminum or an aluminum alloy. Pure aluminum has an aluminum content of 99% or more and 100% or less, such as JIS A1000 series aluminum alloys including A1050. Aluminum alloys are alloys in which other elements such as Mn and Mg are added to Al, such as JIS A3000 series aluminum alloys including A3003 and JIS A5000 series aluminum alloys including A5052.
[0025] The Fe layer 1b is made of an iron-based alloy. The iron-based alloy is an alloy in which Fe is the largest component of the metal elements. Among iron-based alloys, those containing approximately 10% by mass or more of Cr are considered to be stainless steel. From the viewpoint of durability, the iron-based alloy constituting the Fe layer 1b is preferably an iron-based stainless steel containing 10% by mass or more of Cr. Furthermore, the iron-based alloy constituting the Fe layer 1b is preferably a ferritic stainless steel, which is a stainless steel that does not contain Ni, in order to reduce the difference in hardness with the Al layer 1a. The ferritic stainless steel is a stainless steel that contains 16% by mass or more and 18% by mass or less of Cr and whose main metal structure at room temperature is a ferrite phase with a body-centered cubic lattice structure, such as SUS430.
[0026] The overall thickness t1 of the wire bonding clad material 1 is 200 μm or more and 400 μm or less. The thickness t2 of the Al layer 1a is 20 μm or more. From the viewpoint of improving the bonding strength with the Al-based wire 2 by wire bonding, the thickness t2 of the Al layer 1a is preferably 60 μm or less. From the viewpoint of improving the strength of the wire bonding clad material 1, the thickness t2 of the Al layer 1a is preferably smaller than the thickness t3 of the Fe layer 1b.
[0027] 3, one end of an Al-based bonding wire 2 is bonded to the Al layer 1a by wire bonding, and the other end of the Al-based bonding wire 2 is bonded to the bus bar 20 by wire bonding. The Al-based wire 2 is made of pure aluminum or an aluminum alloy.
[0028] A terminal (negative electrode terminal or positive electrode terminal) of the lithium ion secondary battery 10 is joined to the Fe layer 1b by, for example, laser welding. In the case of laser welding, the joining is performed by, for example, irradiating a laser from the Al layer 1a side.
[0029] 4 , lithium ion secondary battery 10 includes cylindrical housing 11, lid 12 that seals the opening of housing 11, and power storage element 13 disposed within housing 11. Housing 11 is made of Ni-plated steel sheet and also serves as the negative electrode terminal of lithium ion secondary battery 10.
[0030] The housing 11 contains a storage element 13 and an electrolyte (not shown). The lid member 12 is made of an iron-based alloy and also serves as the positive electrode terminal of the lithium-ion secondary battery 10. The storage element 13 is formed by winding a positive electrode 14, a negative electrode 15, and an insulating separator 16 disposed between the positive electrode 14 and the negative electrode 15. The positive electrode 14 includes a positive electrode current collector (not shown) made of aluminum foil and a positive electrode active material layer (not shown) disposed on the surface of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material such as lithium manganate and a binder formed of a resin material.
[0031] The lithium-ion secondary battery 10 further includes a positive electrode lead material 17 for connecting the positive electrode 14 and the positive electrode terminal (lid material 12), and a negative electrode lead material 18 for connecting the negative electrode 15 and the negative electrode terminal (casing 11). The positive electrode lead material 17 is made of aluminum foil and is joined to the positive electrode current collector of the positive electrode 14 and the lid material 12 by resistance welding or the like. The negative electrode lead material 18 is made of copper foil and is joined to the negative electrode current collector of the negative electrode 15 and the casing 11 by resistance welding or the like.
[0032] As shown in FIG. 1 , the bus bar 20 is made of pure aluminum or an aluminum alloy. In general, a bus bar electrically connects the terminals (negative electrode terminals, positive electrode terminals) of a plurality of unit cells. In this embodiment, the bus bar 20 electrically connects the positive electrode terminals of a plurality of unit cells (lithium ion secondary batteries 10). In this embodiment, the clad material for wire bonding 1 is disposed between the bus bar 20 and the positive electrode terminals of the lithium ion secondary batteries 10. As shown in FIG. 1 , the bus bar 20 has a plate-like shape.
[0033] As shown in FIG. 1 , a recess 20a is provided on the X1 side of the bus bar 20. While FIG. 1 illustrates an example in which the recess 20a is provided on one side (X1 side) in the short direction, the recess 20a may be provided on both sides (X1 side and X2 side) in the short direction. Ends of Al-based wires 2 are bonded to the recess 20a by wire bonding. A single bus bar 20 can simultaneously connect multiple terminals. Although not shown in FIG. 1 , negative electrode terminals are also connected to each other by another bus bar. Laser welding, spot welding, or the like is used to join the negative electrode terminals to the other bus bar. The battery pack 100 illustrated in FIG. 1 is intended to illustrate an example configuration of the portion connecting the positive electrode terminals to each other by the bus bar 20, and other connection portions and the like are omitted. The battery pack may also be configured such that the positive electrode terminals and the negative electrode terminals are joined by a bus bar. The battery pack may also have a configuration in which the positive electrode terminals are connected to each other by a bus bar and the negative electrode terminals are connected to each other by a bus bar, and a configuration in which the positive electrode terminals and the negative electrode terminals are joined by a bus bar.
[0034] (Battery Manufacturing Method) As shown in FIG. 5 , a clad material 1 for wire bonding is prepared by roll-bonding an Al plate 50a and an Fe plate 50b, which are composed of an Al layer 1a and an Fe layer 1b, with the Al layer 1a having a thickness of 20 μm or more. The Al plate 50a is a plate composed of the same pure aluminum or aluminum alloy as the Al layer 1a. The Fe plate 50b is a plate composed of the same iron-based alloy as the Fe layer 1b. In the roll-bonding, the rolling ratio (degree of processing) is set so that the thicknesses of the Al plate 50a and the Fe plate 50b before rolling are the same as the thicknesses of the Al layer 1a and the Fe layer 1b after rolling. Although not shown in FIG. 5 , diffusion annealing may be performed after roll-bonding the Al plate 50a and the Fe plate 50b. Furthermore, softening annealing may be performed before roll-bonding the Al plate 50a and the Fe plate 50b. Furthermore, after the Al plate material 50a and the Fe plate material 50b are roll-bonded, further rolling may be performed to obtain the desired thickness of the Al layer 1a and the desired thickness of the Fe layer 1b. Furthermore, softening annealing may be performed before further rolling. The produced clad material for wire bonding 1 is then processed, for example, into a circular shape. The method for processing into a circular shape may be performed by punching the clad material for wire bonding 1. The diameter of the circularly formed clad material for wire bonding 1 is set to be suitable for the diameter of the terminal to be joined.
[0035] When constructing the battery pack 100 shown in FIG. 1 , the Fe layer 1b of the wire bonding clad material 1 is joined to the battery terminal member as shown in FIG. 6 . In FIG. 6 , the battery terminal member is the lid member 12 (positive electrode terminal). Depending on the configuration of the battery pack, the negative electrode terminal (the outer bottom surface of the housing 11) can also be joined to the Fe layer 1b of the wire bonding clad material 1. A method for joining the Fe layer 1b of the wire bonding clad material 1 to the battery terminal member is, for example, laser welding. In the case of laser welding, a laser irradiation unit 40 is disposed on the Al layer 1a side and laser irradiation is performed. For example, the laser is irradiated so as to form a circular locus along the outer periphery of the circular wire bonding clad material 1, as shown by the dashed line in FIG. 7 .
[0036] After the Fe layer 1b of the wire bonding clad material 1 is joined to the battery terminal member by laser welding or the like, the Al layer 1a of the wire bonding clad material 1 is joined to the bus bar 20. The method of joining the Al layer 1a of the wire bonding clad material 1 to the bus bar 20 is as follows: as shown in Fig. 8 , one end of an Al-based wire 2 for bonding is joined to the Al layer 1a by wire bonding, and the other end of the Al-based wire 2 is joined to the recess 20a of the bus bar 20 by wire bonding.
[0037] Wire bonding can be performed in two ways: by melting one end and the other end of the Al-based wire 2 to form a ball-shaped bond; or by not forming a ball-shaped bond. Methods for bonding one end and the other end of the Al-based wire 2 to the Al layer 1a and the bus bar 20, respectively, include a method using heat, a method using pressure, a method using ultrasound, or a method using a suitable combination of heat, pressure, ultrasound, and the like. When using ultrasound, for example, one end of the wire is pressed against the Al layer 1a of the wire bonding clad material 1 with a tool 50, and ultrasonic vibrations are applied to generate heat internally, melting and bonding the one end of the wire and the vicinity of the surface of the Al layer 1a. This forms a bonded structure consisting of the wire bonding clad material 1 and the bus bar 20. In this case, the bond strength between the Al-based wire 2 and the Al layer 1a of the wire bonding clad material 1 is preferably 9.8 N or more.
[0038] <Effects of this embodiment> In this embodiment, the following effects can be obtained.
[0039] In this embodiment, the wire bonding clad material 1 is composed of an Al layer 1a made of pure aluminum or an aluminum alloy and an Fe layer 1b made of an iron-based alloy and roll-bonded to the Al layer 1a. The thickness t2 of the Al layer 1a is 20 μm or more, and an Al-based wire 2 for bonding is bonded to the Al layer 1a by wire bonding. Since the Al layer 1a and the Al-based wire 2 are made of the same metal, the formation of a brittle intermetallic compound at the bonded portion between the Al-based wire 2 and the Al layer 1a can be suppressed during wire bonding. As a result, the bond strength when the Al-based wire 2 is bonded to the wire bonding clad material 1 can be improved. Furthermore, experiments described below have found that the thickness t2 of the Al layer 1a is 20 μm or more can improve the bond strength when the Al-based wire 2 is bonded to the Al layer 1a of the wire bonding clad material 1.
[0040] Furthermore, in this embodiment, the thickness of the Al layer 1a is 60 μm or less. As a result, even when a load is applied when bonding the Al-based wire 2 to the wire bonding clad material 1 by wire bonding, the Al layer 1a is softer than the Fe layer 1b and has a larger thickness, which prevents the Al layer 1a from significantly deforming and forming a gap between the Al-based wire 2 and the Al layer 1a. By preventing a gap from being formed between the Al-based wire 2 and the Al layer 1a, a load can be applied while the Al-based wire 2 and the Al layer 1a are in reliable contact with each other, resulting in a stronger bond. Furthermore, experiments described below have shown that by setting the thickness of the Al layer 1a to 60 μm or less, the bonding strength when the Al-based wire 2 is bonded to the Al layer 1a can be sufficiently increased.
[0041] In this embodiment, the thickness t2 of the Al layer 1a is smaller than the thickness t3 of the Fe layer 1b. This allows the thickness of the Fe layer 1b, which is harder than the Al layer 1a, to be increased, thereby improving the strength of the wire bonding clad material 1 and preventing deformation of the wire bonding clad material 1 even when a load is applied when joining the Al-based wire 2 to the wire bonding clad material 1 by wire bonding.
[0042] In this embodiment, the Fe layer 1b is made of ferritic stainless steel. By using ferritic stainless steel, which is softer than other stainless steels, the difference in hardness between the Fe layer 1b and the Al layer 1a can be reduced. This allows the Fe layer 1b to be stretched in accordance with the Al layer 1a when the wire bonding clad material 1 is rolled, thereby preventing variations in thickness of the Fe layer 1b.
[0043] In this embodiment, the Fe layer 1b is made of SUS 430. By using SUS 430, which is a versatile ferritic stainless steel with excellent workability, the workability and productivity of the clad material for wire bonding 1 can be improved.
[0044] Furthermore, in this embodiment, the Al layer 1a is made of A1050. Thus, by using A1050, which has high conductivity, it is possible to improve the conductivity of the wire bonding clad material 1. As a result, for example, when the wire bonding clad material 1 is used between the unit cells and the bus bar 20 that constitute the battery pack 100, it is possible to prevent the conductivity from decreasing due to the wire bonding clad material 1 compared to when the unit cells and the bus bar 20 are directly joined.
[0045] Furthermore, the bonded structure using the wire bonding clad material 1 of this embodiment includes the wire bonding clad material 1, which includes the Al layer 1a made of pure aluminum or an aluminum alloy, and the thickness t2 of the Al layer 1a is 20 μm or more, as described above, and the bus bar 20 made of pure aluminum or an aluminum alloy. Because the Al layer 1a and the Al-based wire 2 are made of the same metal, the formation of a brittle intermetallic compound at the bonded portion between the Al-based wire 2 and the Al layer 1a can be suppressed when they are bonded. As a result, the bond strength when the Al-based wire 2 is bonded to the wire bonding clad material 1 can be improved. Furthermore, experiments described below have revealed that a bonded structure with high bond strength can be achieved when the Al-based wire 2 is bonded to the Al layer 1a of the wire bonding clad material 1 by having the Al layer 1a have a thickness of 20 μm or more.
[0046] In this embodiment, the bonding strength between the Al-based wire 2 and the Al layer 1a is 9.8 N or more. This allows the bonding strength between the Al-based wire 2 and the wire bonding clad material 1 to be sufficiently large.
[0047] Furthermore, the battery manufacturing method of this embodiment includes the steps of preparing a clad material for wire bonding 1 having an Al layer 1a with a thickness of 20 μm or more, and joining one end of an Al-based wire 2 for bonding to the Al layer 1a by wire bonding, as described above. Because the Al layer 1a and the Al-based wire 2 are made of the same metal, the formation of a brittle intermetallic compound at the bonded portion between the Al-based wire 2 and the Al layer 1a can be suppressed during bonding. As a result, a clad material for wire bonding 1 can be manufactured that can improve the bond strength when the Al-based wire 2 is bonded by wire bonding. Furthermore, experiments described below have shown that the thickness of the Al layer 1a of 20 μm or more can improve the bond strength between the Al-based wire 2 and the Al layer 1a of the clad material for wire bonding 1.
[0048] [Example] An experiment (example) will be described in which the bonding strength between the Al-based wire 2 and the Al layer 1a of the wire bonding clad material 1 was measured by changing the thickness of the Al layer 1a.
[0049] As the bonded material for Comparative Example 1, in which the thickness of the Al layer 1a to which the Al-based wire 2 was bonded by wire bonding was 0 μm, a plate material made of SUS430, a SUS430 single plate with a plate thickness of 300 μm, was prepared. Furthermore, as the bonded material for Examples 1 to 5 and Comparative Example 2, in which the thickness of the Al layer 1a exceeded 0 μm, a wire-bonding clad material 1 was prepared, which was composed of an Al layer 1a made of A1050 and an Fe layer 1b made of SUS430 and had a total thickness of 300 μm. The bonded materials for Examples 1 to 5 and Comparative Example 2 were wire-bonding clad materials 1 with different ratios (layer thickness ratios) of the thickness of the Al layer 1a to the thickness of the Fe layer 1b, and the thicknesses of the Al layer 1a in each example were 10 μm (Comparative Example 2), 20 μm (Example 1), 40 μm (Example 2), 60 μm (Example 3), 90 μm (Example 4), and 140 μm (Example 5).
[0050] The Al layer 1a of the wire bonding clad material 1 of Examples 1 to 5 and Comparative Example 2 was bonded to one end of an Al-based wire 2 by wire bonding to produce a bonded structure. Also, the SUS430 single plate of Comparative Example 1 was bonded to one end of the Al-based wire 2 by wire bonding to produce a bonded structure. The wire bonding was performed using an Al-based wire 2 with a diameter of 300 μm, with one end of the Al-based wire 2 pressed against the tool 50 to apply a load of 2 N, 3 N, or 4 N, and by oscillating ultrasonic waves with an output of 2 W for 100 ms (milliseconds). The bonded surfaces of the materials to be bonded in Examples 1 to 5 and Comparative Examples 1 and 2 were polished to a mirror finish before wire bonding.
[0051] A wire bond strength evaluation test was performed on each of the bond structures of Examples 1 to 5 and Comparative Examples 1 and 2. A shear test was used for the wire bond strength evaluation test. Specifically, in accordance with JIS Z3198-7 (2003) "Lead-Free Solder Test Methods—Part 7: Shear Test Method for Solder Joints of Chip Components," a shearing jig was applied to the Al-based wire 2, and the shearing jig was moved at a speed of 5 mm / min to 30 mm / min to measure the maximum shear load. The clearance (gap) between the shearing jig and the Al layer 1a of Examples 1 to 5 and Comparative Example 2 was set to 3 μm. Similarly, the clearance (gap) between the shearing jig and the SUS single plate of Comparative Example 1 was set to 3 μm. Furthermore, for Examples 1 to 5 and Comparative Examples 1 and 2, multiple test specimens were prepared for the wire bond strength evaluation test, and the average value of the maximum shear load was calculated to represent the average bond strength. The results of the wire bond strength evaluation test are shown in Table 1 and Fig. 9. In Fig. 9, the average bond strength is plotted as bond strength on the vertical axis, and the thickness of the Al layer 1a is plotted on the horizontal axis. In Fig. 9, the bond strength of the SUS single plate of Comparative Example 1 is plotted at the position where the thickness of the Al layer 1a is 0 µm.
[0052]
[0053] As shown in Table 1, when wire bonding was performed with a load of 2 N using the SUS430 single plate of Comparative Example 1 (the thickness t2 of the Al layer 1a shown in FIG. 2 is 0 μm) as the bonded material, the average bond strength of the bonded structure was 5.8 N. When wire bonding was performed with a load of 3 N, the average bond strength was 8.2 N. When wire bonding was performed with a load of 4 N, the average bond strength was 8.3 N.
[0054] When wire bonding was performed with a load of 2 N using the clad material for wire bonding 1 of Comparative Example 2 having an Al layer 1 a with a thickness t2 of 10 μm as the material to be bonded, the average bond strength of the bonded structure was 9.7 N. When wire bonding was performed with a load of 3 N, the average bond strength was 8.9 N. When wire bonding was performed with a load of 4 N, the average bond strength was 7.9 N.
[0055] When wire bonding was performed with a load of 2 N using the clad material for wire bonding 1 of Example 1 having an Al layer 1 a with a thickness t2 of 20 μm as the bonded material, the average bond strength of the bonded structure was 10.3 N. When wire bonding was performed with a load of 3 N, the average bond strength was 10.6 N. When wire bonding was performed with a load of 4 N, the average bond strength was 11.3 N.
[0056] When wire bonding was performed with a load of 2 N using the clad material for wire bonding 1 of Example 2 having an Al layer 1 a with a thickness t2 of 40 μm as the material to be bonded, the average bond strength of the bonded structure was 10.2 N. When wire bonding was performed with a load of 3 N, the average bond strength was 10.9 N. When wire bonding was performed with a load of 4 N, the average bond strength was 11.2 N.
[0057] When wire bonding was performed with a load of 2 N using the clad material for wire bonding 1 of Example 3 having an Al layer 1 a with a thickness t2 of 60 μm as the material to be bonded, the average bond strength of the bonded structure was 10.6 N. When wire bonding was performed with a load of 3 N, the average bond strength was 11.7 N. When wire bonding was performed with a load of 4 N, the average bond strength was 11.3 N.
[0058] When wire bonding was performed with a load of 2 N using the clad material for wire bonding 1 of Example 4 having an Al layer 1 a with a thickness t2 of 90 μm as the bonded material, the average bond strength of the bonded structure was 7.8 N. When wire bonding was performed with a load of 3 N, the average bond strength was 9.8 N. When wire bonding was performed with a load of 4 N, the average bond strength was 9.6 N.
[0059] Furthermore, when wire bonding was performed with a load of 2 N using the clad material for wire bonding 1 of Example 5 having an Al layer 1 a with a thickness t2 of 140 μm as the material to be bonded, the average bond strength of the bonded structure was 9.0 N. When wire bonding was performed with a load of 3 N, the average bond strength was 9.1 N. When wire bonding was performed with a load of 4 N, the average bond strength was 10.0 N.
[0060] From the above results, the inventors of the present application have found that in the bonded structures using the clad materials for wire bonding 1 of Examples 1 to 5 as the bonded materials, in which the thickness t2 of the Al layer 1a (see FIG. 2) is 20 μm or more, the bond strength (average bond strength) between the bonded materials and the Al-based wire 2 is improved compared to the bonded structure using the SUS430 single plate of Comparative Example 1 as the bonded material, i.e., the bonded structure in which the Al-based wire 2 is directly wire-bonded to the SUS430 single plate. In particular, in the bonded structures using the bonded materials in which the thickness t2 of the Al layer 1a is in the range of 20 μm to 60 μm, the average bond strength of the bonded structures was 9.8 N or more when the load during wire bonding was 4 N or less, i.e., 2 N, 3 N, and 4 N. From this, the inventors of the present application have found that it is preferable to use a clad material for wire bonding 1 in which the thickness t2 of the Al layer 1a is 20 μm or more and 60 μm or less as the material to be joined, because this provides a sufficiently large bonding strength between the material to be joined and the Al-based wire 2. Furthermore, as shown in the graph of Figure 9, the inventors have found that the bonding strength (average bonding strength) is highest when the thickness t2 of the Al layer 1a is 60 μm.
[0061] Next, a thermal shock test was performed on each bond structure for Examples 1 to 5 and Comparative Examples 1 and 2 when wire-bonded under a 3N load. The thermal shock test was conducted in accordance with ISO 16750-4 (Environmental Testing of Automotive Electrical and Electronic Equipment - Mechanical Load), with 1,000 cycles consisting of a high-temperature holding period at 80°C for 20 minutes and a low-temperature holding period at -40°C for 20 minutes. Multiple specimens were prepared for the thermal shock test for Examples 1 to 5 and Comparative Examples 1 and 2, and the average maximum shear load was calculated as described above to represent the average bond strength. The results of the thermal shock test are shown in Table 2 and Figure 10. In Figure 10, the average bond strength is plotted on the vertical axis as bond strength, and the thickness of the Al layer 1a is plotted on the horizontal axis. Also in Figure 10, the bond strength of the SUS single sheet for Comparative Example 1 is plotted at the position where the thickness of the Al layer 1a is 0 μm.
[0062]
[0063] As shown in Table 2, when the SUS430 single plate of Comparative Example 1 (the thickness t2 of the Al layer 1a shown in Figure 2 is 0 μm) was used as the material to be joined, the average joining strength before the thermal shock test (when the number of cycles was 0) was 8.2 N, but after the thermal shock test (when the number of cycles was 1000) it was 10.6 N.
[0064] In addition, when the wire bonding clad material 1 of Comparative Example 2, in which the thickness t2 of the Al layer 1a was 10 μm, was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 8.9 N, but after the thermal shock test (when the number of cycles was 1000) it became 8.8 N.
[0065] In addition, when the wire bonding clad material 1 in Example 1 having an Al layer 1a with a thickness t2 of 20 μm was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 10.6 N, but after the thermal shock test (when the number of cycles was 1000) it became 13.8 N.
[0066] In addition, when the wire bonding clad material 1 of Example 2 having an Al layer 1a with a thickness t2 of 40 μm was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 10.9 N, but after the thermal shock test (when the number of cycles was 1000) it became 13.5 N.
[0067] In addition, when the wire bonding clad material 1 of Example 3 having an Al layer 1a with a thickness t2 of 60 μm was used as the material to be joined, the average bonding strength was 11.7 N before the thermal shock test (when the number of cycles was 0), but it became 13.5 N after the thermal shock test (when the number of cycles was 1000).
[0068] In addition, when the wire bonding clad material 1 of Example 4 having an Al layer 1a with a thickness t2 of 90 μm was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 9.8 N, but after the thermal shock test (when the number of cycles was 1000) it became 11.7 N.
[0069] In addition, when the wire bonding clad material 1 of Example 5, in which the thickness t2 of the Al layer 1a was 140 μm, was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 9.1 N, but after the thermal shock test (when the number of cycles was 1000) it became 11.7 N.
[0070] From the above results, the inventors have found that when the wire bonding clad material 1 in Examples 1 to 5, in which the thickness t2 of the Al layer 1a is 20 μm or more, is used as the bonded material, the average bond strength of the bonded structure after a thermal shock test is improved compared to when the SUS430 single plate in Comparative Example 1 (in which the thickness t2 of the Al layer 1a is 0 μm) is used as the bonded material, i.e., a bonded structure in which the Al-based wire 2 is directly bonded to the SUS430 single plate by wire bonding. In particular, when the thickness t2 of the Al layer 1a is in the range of 20 μm or more and 60 μm or less, the average bond strength after the thermal shock test is 13.5 N or more, and the bond strength of the bonded structure is sufficiently high. As a result, the inventors of the present application have discovered that a bonding structure using a wire bonding clad material 1 in which the thickness t2 of the Al layer 1a as the material to be bonded is 20 μm or more (preferably, the thickness t2 of the Al layer 1a is in the range of 20 μm or more and 60 μm or less) maintains its bonding strength even when repeatedly subjected to thermal shock due to the passage of a large current, etc.
[0071] [Modifications] The embodiments and examples disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is indicated by the claims, not by the description of the embodiments and examples above, and further includes all modifications (modifications) within the meaning and scope equivalent to the claims.
[0072] For example, in the present embodiment, a configuration example in which the clad material for wire bonding 1 is used in the assembled battery 100 has been shown, but the present invention is not limited to this. In the present invention, for example, the clad material for wire bonding 1 may be used in other applications besides the assembled battery 100, such as in electrical and electronic circuit boards for automotive applications.
[0073] Furthermore, in the present embodiment, a configuration example has been shown in which the wire bonding clad material 1 and the lid material 12, which is the positive electrode terminal of the lithium ion secondary battery 10, are laser welded together, and then the wire bonding clad material 1 and the bus bar 20 are joined by wire bonding using an Al-based wire 2, but the present invention is not limited to this. For example, the present invention may be used in a configuration in which the wire bonding clad material 1 and the casing 11, which is the negative electrode terminal of the lithium ion secondary battery 10, are laser welded together, and then the wire bonding clad material 1 and the bus bar 20 are joined by wire bonding using an Al-based wire 2. For example, the present invention may be used in a configuration in which the wire bonding clad material 1 is laser welded to a terminal (positive electrode terminal) of one battery, and another wire bonding clad material 1 is laser welded to a terminal (positive electrode terminal) of the other battery, and then the Al layers 1 a of the one and other wire bonding clad materials 1 are joined together by wire bonding using an Al-based wire 2.
[0074] In the present embodiment, the clad material 1 for wire bonding has a configuration in which the thickness t2 of the Al layer 1a is smaller than the thickness t3 of the Fe layer 1b as shown in Fig. 2, but the present invention is not limited to this. In the present invention, the clad material 1 for wire bonding may have a thickness t2 of the Al layer 1a that is equal to or larger than the thickness t3 of the Fe layer 1b, for example.
[0075] In addition, in the present embodiment, an example of a configuration in which the clad material for wire bonding 1 is used in the cylindrical lithium ion secondary battery 10 shown in Fig. 4 has been shown, but the present invention is not limited to this. In the present invention, the clad material for wire bonding 1 may be used in a prismatic lithium ion secondary battery 10.
[0076] REFERENCE SIGNS LIST 1 Clad material for wire bonding 1a Al layer 1b Fe layer 2 Al-based wire 10 Lithium ion secondary battery 11 Housing (negative electrode terminal) 12 Lid material (positive electrode terminal) 20 Bus bar (plate-shaped member)
Claims
1. A clad material for wire bonding (1) to which an Al-based wire (2) for bonding is bonded by wire bonding, the clad material for wire bonding comprising an Al layer (1a) made of pure aluminum or an aluminum alloy, and an Fe layer (1b) made of an iron-based alloy and roll-bonded to the Al layer, the Al layer having a thickness of 20 μm or more, and an Al-based wire for bonding is bonded to the Al layer by wire bonding.
2. The clad material for wire bonding according to claim 1, wherein the thickness of the Al layer is 60 μm or less.
3. The clad material for wire bonding according to claim 1, wherein the thickness of said Al layer is smaller than the thickness of said Fe layer.
4. The clad material for wire bonding according to claim 1, wherein the Fe layer is made of ferritic stainless steel.
5. The clad material for wire bonding according to claim 4, wherein the Fe layer is made of SUS430.
6. The clad material for wire bonding according to claim 5, wherein the Al layer is made of A1050.
7. A bonding structure using a clad material for wire bonding, comprising: an Al layer (1a) made of pure aluminum or an aluminum alloy; an Fe layer (1b) made of an iron-based alloy and roll-bonded to the Al layer, the Al layer having a thickness of 20 μm or more; and a plate-like member made of pure aluminum or an aluminum alloy, one end of an Al-based wire (2) for bonding is bonded to the Al layer by wire bonding, and the other end of the Al-based wire is bonded to the plate-like member.
8. A bonding structure using the clad material for wire bonding according to claim 7, wherein the bonding strength between the Al-based wire and the Al layer is 9.8 N or more.
9. A method for manufacturing a battery, comprising the steps of: preparing a clad material for wire bonding (1) by roll-bonding an Al plate material (50a) made of pure aluminum or an aluminum alloy and an Fe plate material (50b) made of an iron-based alloy, the clad material being composed of an Al layer (1a) and an Fe layer (1b), the Al layer having a thickness of 20 μm or more; bonding a battery terminal member made of an iron-based alloy to the Fe layer; bonding one end of an Al-based wire (2) for bonding to the Al layer by wire bonding; and bonding the other end of the Al-based wire to a bus bar (20) made of pure aluminum or an aluminum alloy.
Citation Information
Patent Citations
Clad board for bonding pad
JP1988180225U
Electronic circuit unit, ignition device for internal combustion engine and ignition control device for internal combustion engine
JP1993157037A
Sodium sulfur battery module and battery system using it
JP1997270269A
Cladding material for terminal, and terminal for aluminum wire formed using cladding material
JP2005228496A