Exterior window film

The external window film, featuring a polyethylene terephthalate base material with a specific hard coat and anchor coat layer composition, addresses adhesion and cracking issues, ensuring enhanced weather resistance and transparency by blocking ultraviolet rays and maintaining performance under outdoor conditions.

WO2024241861A1PCT designated stage expired Publication Date: 2024-11-28LINTEC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016913
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-05-02
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

External window films applied from the outside of windows face issues with adhesion between the base material and hard coat layer, leading to potential cracking and poor weather resistance due to exposure to sunlight, rain, wind, and temperature changes, which affects their transparency and performance.

Method used

The external window film incorporates a polyethylene terephthalate base material with a hard coat layer containing (meth)acrylate resin, urethane (meth)acrylate, hindered amine light stabilizer, and ultraviolet absorbers, along with an anchor coat layer made of thermosetting acrylic resin, to enhance adhesion and prevent cracking when rolled, while the hard coat layer blocks ultraviolet rays to maintain transparency and weather resistance.

Benefits of technology

This configuration improves the adhesion between the base material and hard coat layer, prevents cracking, and ensures excellent weather resistance, maintaining the transparency and performance of the window film even when exposed to harsh outdoor conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016913_28112024_PF_FP_ABST
    Figure JP2024016913_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide an exterior window film which has improved adhesion between a base material and a hard coat layer, prevents the occurrence of cracks in the hard coat layer when wound in a roll shape while ensuring transparency, and has excellent weather resistance. An exterior window film according to the present invention is characterized by comprising: a base material configured from a material containing polyethylene terephthalate; a hard coat layer provided on one surface side of the base material; an anchor coat layer provided between the base material and the hard coat layer; and an adhesive layer disposed on the surface side of the base material opposite to the side on which the hard coat layer is disposed; the hard coat layer is composed of a material containing a (meth)acrylate resin having urethane (meth)acrylate as a constituent component, a hindered amine light stabilizer and a first ultraviolet absorber; and the anchor coat layer is composed of a material containing a thermosetting acrylic resin.
Need to check novelty before this filing date? Find Prior Art

Description

Exterior window film

[0001] The present invention relates to an exterior window film.

[0002] Window films are adhesive films that are applied to the window glass of vehicles such as automobiles, ships, and trains, and buildings such as houses, condominiums, and office buildings. Window films are widely used for purposes such as blocking ultraviolet and / or infrared rays in sunlight, protecting privacy, preventing crime, preventing glass from shattering, and decoration.

[0003] A window film has a configuration including, for example, a transparent substrate, a hard coat layer (hard coat) disposed on one side of the substrate, and a pressure-sensitive adhesive layer disposed on the side of the substrate opposite the side on which the hard coat layer is disposed. Also, window films that can efficiently block ultraviolet rays by incorporating an ultraviolet absorber into the pressure-sensitive adhesive layer are also used (for example, Patent Document 1).

[0004] In interior window films, which are attached to the interior surface of window glass, sunlight hits the window glass / adhesive layer / substrate / hard coat layer / interior in this order. In this case, the adhesive layer can block UV rays before the hard coat layer does, preventing deterioration of the hard coat layer due to UV rays.

[0005] On the other hand, if a building does not have the work space to apply window film to the window glass from the indoor side, the window film will have to be applied to the window glass from the outdoor side. For this reason, there are customers who, due to the structure of the building, want to apply window film to the window glass from the outside. For such customers, exterior window films that can be applied to the outdoor side of the window glass have also been developed.

[0006] In such exterior window films, sunlight hits the film in the following order: hard coat layer, substrate, adhesive layer, window glass, and interior. As a result, the adhesive layer cannot block UV rays before the hard coat layer does, and the hard coat layer is degraded by UV rays.

[0007] Furthermore, in the case of exterior window films, in addition to sunlight, rain, wind, temperature changes, etc. also cause deterioration of the hard coat layer.

[0008] Furthermore, when installing window film on high-placed window glass from the outside, a crane or the like is used, so there is a demand to transport as much window film as possible to the installation location in one operation.

[0009] For this reason, the window film is transported in a rolled state with the hard coat layer facing outwards, and during this process, cracks must not occur in the hard coat layer.

[0010] If cracks occur in the hard coat layer, the transparency of the window film decreases, which may cause problems such as deterioration in the appearance and performance of the window film.

[0011] Furthermore, if the adhesion between the substrate and the hard coat layer is insufficient, the hard coat layer may peel off from the substrate, resulting in problems such as deterioration in the weather resistance and appearance of the window film.

[0012] Re-table 2018 / 173979 publication

[0013] The object of the present invention is to provide an exterior window film having a hard coat layer, which has excellent weather resistance and improves adhesion between the substrate and the hard coat layer while ensuring transparency, and prevents cracks from occurring in the hard coat layer when wound into a roll.

[0014] The above object is achieved by the present invention, which provides an exterior window film comprising: a substrate made of a material containing polyethylene terephthalate, a hard coat layer provided on one side of the substrate, an anchor coat layer provided between the substrate and the hard coat layer, and a pressure-sensitive adhesive layer provided on the side of the substrate opposite to the side on which the hard coat layer is provided, wherein the hard coat layer is made of a material containing a (meth)acrylate resin having a urethane (meth)acrylate as a constituent component, a hindered amine light stabilizer, and a first ultraviolet absorber, wherein the ratio of the hindered amine light stabilizer to 100.0 parts by mass of the (meth)acrylate resin is 2.0 parts by mass or more and 15.0 parts by mass or less, and the ratio of the first ultraviolet absorber is 5.0 parts by mass or more and 30.0 parts by mass or less, and the anchor coat layer is made of a material containing a thermosetting acrylic resin.

[0015] In the present invention, the first ultraviolet absorber preferably contains a compound having a benzophenone structure and a compound having a hydroxyphenyltriazine structure.

[0016] In the present invention, the ratio of the content of the compound having a benzophenone structure to the content of the compound having a hydroxyphenyltriazine structure in the hard coat layer is preferably 1.0:2.0 or more and 2.0:1.0 or less in mass ratio.

[0017] In the present invention, the anchor coat layer preferably contains a second ultraviolet absorber.

[0018] In the present invention, it is preferable that the second ultraviolet absorber contains a compound having a hydroxyphenyltriazine structure.

[0019] In the present invention, the (meth)acrylate resin preferably has a configuration obtained by polymerizing the urethane (meth)acrylate using a photopolymerization initiator.

[0020] In the present invention, the photopolymerization initiator is preferably a triphenylphosphine oxide-based compound, since the ultraviolet absorption wavelength of the photopolymerization initiator is longer than that of the first ultraviolet absorber.

[0021] In the present invention, the thickness of the hard coat layer is preferably 0.1 μm or more and 20 μm or less.

[0022] According to the present invention, it is possible to provide an exterior window film having a hard coat layer, which has excellent weather resistance and which improves adhesion between the substrate and the hard coat layer while ensuring transparency and preventing cracks from occurring in the hard coat layer when wound into a roll.

[0023] FIG. 1 is a cross-sectional view showing an example of the construction of a window film for exterior application according to the present invention.

[0024] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Preferred embodiments of the present invention will now be described in detail. [1] Window Film Fig. 1 is a cross-sectional view showing an example of the construction of a window film for exterior application according to the present invention.

[0025] The exterior window film 1 is an adhesive film that is applied to the window glass of vehicles such as automobiles, ships, and trains, and buildings such as houses, apartment buildings, and office buildings. The exterior window film 1 is used for purposes such as blocking ultraviolet and / or infrared rays in sunlight, protecting privacy, preventing crime, preventing glass from shattering, and providing decoration.

[0026] The exterior window film 1 includes a substrate 2 made of a material containing polyethylene terephthalate, a hard coat layer 3 provided on one side of the substrate 2, an anchor coat layer 4 provided between the substrate 2 and the hard coat layer 3, and a pressure-sensitive adhesive layer 5 provided on the side of the substrate 2 opposite the side on which the hard coat layer 3 is provided. The hard coat layer 3 is made of a material containing a (meth)acrylate resin having a urethane (meth)acrylate as a constituent component, a hindered amine light stabilizer, and a first ultraviolet absorber. Furthermore, the ratio of the hindered amine light stabilizer is 2.0 parts by mass or more and 15.0 parts by mass or less, and the ratio of the first ultraviolet absorber is 5.0 parts by mass or more and 30.0 parts by mass or less, per 100.0 parts by mass of the (meth)acrylate resin. Furthermore, the anchor coat layer 4 is made of a material containing a thermosetting acrylic resin.

[0027] In the hard coat layer 3, the (meth)acrylate resin contains urethane (meth)acrylate as a constituent component, which imparts flexibility to the hard coat layer 3 and contributes to preventing cracks from occurring in the hard coat layer 3 when the exterior window film 1 is wound into a roll.

[0028] Furthermore, the hard coat layer 3 contains a hindered amine light stabilizer, which contributes to improving the weather resistance of the exterior window film 1 and to suppressing a decrease in transparency.

[0029] Furthermore, since the hard coat layer 3 contains the first ultraviolet absorber, ultraviolet rays can be cut in the hard coat layer 3, thereby reducing the proportion of ultraviolet rays in the light transmitted through the exterior window film 1. Furthermore, cutting ultraviolet rays with the hard coat layer 3, which is the outermost layer when the exterior window film 1 is attached to an adherend, can also contribute to suppressing deterioration of the anchor coat layer 4, the substrate 2, and the pressure-sensitive adhesive layer 5.

[0030] The ratio of the hindered amine light stabilizer to 100.0 parts by mass of the (meth)acrylate resin is 2.0 parts by mass or more and 15.0 parts by mass or less, and the ratio of the first ultraviolet absorber is 5.0 parts by mass or more and 30.0 parts by mass or less.

[0031] Furthermore, by containing the hindered amine light stabilizer and the first ultraviolet absorber in a predetermined proportion in the hard coat layer 3, the transparency of the exterior window film 1 is ensured, while preventing cracks from occurring in the hard coat layer 3 when the film is rolled up, thereby improving the weather resistance of the exterior window film 1.

[0032] In addition, an anchor coat layer 4 made of a material containing a thermosetting acrylic resin is provided between the substrate 2 and the hard coat layer 3. This improves the adhesion of the anchor coat layer 4 to both the substrate 2 made of a material containing polyethylene terephthalate and the hard coat layer 3 having the specific composition described above. This improves the adhesion between the substrate 2 and the hard coat layer 3 via the anchor coat layer 4, prevents peeling of the hard coat layer 3 from the substrate 2, and suppresses deterioration in the weather resistance and appearance of the exterior window film 1.

[0033] Furthermore, the anchor coat layer 4 is made of a material containing a thermosetting acrylic resin, which provides the anchor coat layer 4 with sufficient weather resistance and prevents the exterior window film 1 from losing transparency.

[0034] Furthermore, by including a second ultraviolet absorber in the anchor coat layer 4, ultraviolet rays can be cut in the anchor coat layer 4, and the proportion of ultraviolet rays in the sunlight that reaches the substrate 2 can be more reliably reduced.

[0035] The excellent effects of the present invention can be obtained by the exterior window film 1 having the above-mentioned configuration, and cannot be obtained if the exterior window film 1 does not have the above-mentioned configuration.

[0036] For example, if the (meth)acrylate resin constituting the hard coat layer does not contain urethane (meth)acrylate as a constituent component, it will be impossible to sufficiently prevent cracks from occurring in the hard coat layer when the exterior window film is wound into a roll.

[0037] Furthermore, if the hard coat layer does not contain a hindered amine light stabilizer, the weather resistance of the exterior window film will be significantly poor, and the transparency will be significantly reduced.

[0038] Furthermore, even if the hard coat layer contains a hindered amine-based light stabilizer, if the proportion thereof is less than the lower limit, the weather resistance of the exterior window film cannot be sufficiently improved, and the decrease in transparency of the exterior window film cannot be sufficiently suppressed, even if the hard coat layer contains a relatively high content of the first ultraviolet absorber instead.

[0039] Furthermore, if the proportion of the hindered amine light stabilizer in the hard coat layer exceeds the upper limit, the hindered amine light stabilizer may segregate to the surface of the hard coat layer, and the appearance of the exterior window film may be impaired.

[0040] Furthermore, if the hard coat layer does not contain the first ultraviolet absorber, the weather resistance of the exterior window film will be significantly poor.

[0041] Furthermore, even if the hard coat layer contains a first ultraviolet absorber, if the proportion thereof is less than the lower limit, the weather resistance of the exterior window film cannot be sufficiently improved, even if a hindered amine-based light stabilizer is contained in a relatively high content instead.

[0042] Furthermore, if the proportion of the first ultraviolet absorber in the hard coat layer exceeds the upper limit, the ultraviolet light irradiated during the curing reaction of the urethane (meth)acrylate may be excessively absorbed, which may result in poor curing of the urethane (meth)acrylate.

[0043] Furthermore, if the exterior window film does not have an anchor coat layer, the adhesion between the substrate and the hard coat layer cannot be sufficiently improved.

[0044] Furthermore, if the material constituting the anchor coat layer does not contain a thermosetting acrylic resin, the transparency and weather resistance of the exterior window film cannot be sufficiently improved.

[0045] [1-1] Substrate The substrate 2 has the function of supporting the anchor coat layer 4, the hard coat layer 3, and the pressure-sensitive adhesive layer 5. Furthermore, when the exterior window film 1 is attached to an adherend, for example, if the adherend is broken, the substrate 2, together with the pressure-sensitive adhesive layer 5, can hold the broken adherend (e.g., glass, etc.), and can suitably prevent the broken adherend from scattering.

[0046] The substrate 2 is made of a material containing polyethylene terephthalate, and is preferably made mainly of polyethylene terephthalate.

[0047] This improves the handleability of the exterior window film 1 and the workability of attaching the exterior window film 1 to an adherend, etc. Also, the weather resistance of the exterior window film 1 is improved, and the adhesion between the exterior window film 1 and the anchor coat layer 4 and the pressure-sensitive adhesive layer 5, which are made of materials described below, is also improved.

[0048] In this specification, the term "mainly" refers to the constituent material that has the highest content in the target portion.

[0049] In particular, the content of polyethylene terephthalate in the base material 2 is preferably 90% by mass or more, and more preferably 95% by mass or more, so that the above-mentioned effects are more significantly exhibited.

[0050] The substrate 2 may contain components other than those described above, such as colorants, antioxidants, ultraviolet absorbers, light stabilizers, softeners, modifiers, rust inhibitors, fillers, surface lubricants, corrosion inhibitors, heat stabilizers, lubricants, antistatic agents, polymerization inhibitors, crosslinking agents, catalysts, leveling agents, thickeners, and dispersants.

[0051] Among these, it is preferable that the substrate 2 contains an ultraviolet absorber, which can improve the weather resistance of the substrate 2 itself and also improve the weather resistance of the exterior window film 1 as a whole.

[0052] In particular, it is preferable that the base material 2 is mainly made of polyethylene terephthalate and contains an ultraviolet absorber.

[0053] Examples of the ultraviolet absorber include salicylic acid-based ultraviolet absorbers such as p-t-butylphenyl salicylate and p-octylphenyl salicylate; benzophenone-based ultraviolet absorbers such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfobenzophenone, 2,2',4,4'-tetrahydroxybenzophenone and bis(2-methoxy-4-hydroxy-5-benzoylphenyl)methane; and benzotriazole-based ultraviolet absorbers such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol]. Absorbents include cyanoacrylate-based UV absorbers such as ethyl-2-cyano-3,3'-diphenylacrylate; benzoxazinone-based UV absorbers such as 2-p-nitrophenyl-3,1-benzoxazin-4-one, 2-(p-benzoylphenyl)-3,1-benzoxazin-4-one, 2-(2-naphthyl)-3,1-benzoxazin-4-one, 2,2'-(p-phenylene)bis(3,1-benzoxazin-4-one), and 2,2'-(2,6-naphthylene)bis(3,1-benzoxazin-4-one); and inorganic UV absorbers such as titanium dioxide, cerium oxide, zinc oxide, iron oxide, and barium sulfate, and these may be used alone or in combination. Among these, benzoxazinone-based UV absorbers are preferred because they can be melt-mixed with polyethylene terephthalate. Examples of benzoxazinone organic ultraviolet absorbers include 2,2'-(1,4-phenylene)bis[4H-3,1-benzoxazin-4-one] and 2,6-naphthalenebis(1,3-benzoxazin-4-one).

[0054] The substrate 2 may have a substantially uniform composition throughout, or may have regions with different compositions. For example, the substrate 2 may be a laminate including multiple layers with regions with different compositions (including, for example, resin materials with different molecular weights), or may be made of a gradient material whose composition changes gradually along the thickness direction.

[0055] The substrate 2 may be subjected to a surface treatment to enhance adhesion to the anchor coat layer 4 and the pressure-sensitive adhesive layer 5. Examples of such surface treatments include corona treatment and primer treatment (for example, application of an easily adhesive resin).

[0056] Examples of the easily adhesive resin include polyester resin, urethane resin, and acrylic resin.

[0057] The thickness of the substrate 2 is not particularly limited, but is preferably 10 μm to 300 μm, more preferably 15 μm to 200 μm, and even more preferably 20 μm to 100 μm.

[0058] This not only provides weather resistance to the exterior window film 1, but also improves the handleability of the exterior window film 1, facilitating tasks such as application to an adherend. Furthermore, the exterior window film 1 is also improved in conformity to the shape of a curved adherend, effectively preventing wrinkles and the like from forming.

[0059] [1-2] Hard Coat Layer The hard coat layer 3 has better abrasion resistance than the substrate 2, and has the function of improving the abrasion resistance of the exterior window film 1 as a whole, for example.

[0060] This allows the exterior window film 1 to exhibit excellent abrasion resistance after being attached to an adherend. The exterior window film 1 is particularly susceptible to contact and collision with sand, dust, and various flying objects. The hard coat layer 3 is an important component for ensuring that the exterior window film 1 is scratch-resistant and has sufficient weather resistance even in such a usage environment. Furthermore, the hard coat layer 3 can effectively prevent scratches during the process of attaching the exterior window film 1 to an adherend.

[0061] The hard coat layer 3 is composed of a material containing a hindered amine light stabilizer and a first ultraviolet absorber. This blocks ultraviolet rays and reduces the proportion of ultraviolet rays in the light transmitted through the exterior window film 1. Furthermore, the hard coat layer 3, which is the outermost layer when the exterior window film 1 is attached to an adherend, blocks ultraviolet rays. Therefore, the hard coat layer 3 can contribute to suppressing deterioration of the anchor coat layer 4, the pressure-sensitive adhesive layer 5, and the substrate 2, and also has the function of improving the weather resistance of the exterior window film 1.

[0062] [1-2-1] (Meth)acrylate Resin The hard coat layer 3 contains a constituent component, that is, a (meth)acrylate resin having urethane (meth)acrylate as a polymerizable component.

[0063] The (meth)acrylate resin contains urethane (meth)acrylate as a constituent component, thereby imparting flexibility to the hard coat layer 3. In particular, by satisfying a predetermined content relationship between the (meth)acrylate resin and the hindered amine light stabilizer and the first ultraviolet absorber, which will be described in detail later, flexibility can be imparted to the hard coat layer 3, and the occurrence of cracks in the hard coat layer 3 can be suitably prevented.

[0064] Urethane (meth)acrylate is an oligomer having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized and cured by irradiation with energy rays.

[0065] The (meth)acrylate resin constituting the hard coat layer 3 may contain a component other than the urethane (meth)acrylate. Examples of such a component include a (meth)acrylate having no urethane group.

[0066] However, the proportion of urethane (meth)acrylate in the (meth)acrylate resin constituting the hard coat layer 3 is preferably 10.0 mass % or more, more preferably 30.0 mass % or more, and even more preferably 50.0 mass % or more.

[0067] The content of the (meth)acrylate resin in the hard coat layer 3 is preferably 50.0% by mass or more and 93.0% by mass or less, more preferably 60.0% by mass or more and 90.0% by mass or less, and even more preferably 70.0% by mass or more and 86.0% by mass or less.

[0068] When the hard coat layer 3 contains a plurality of types of (meth)acrylate resins, the content of the (meth)acrylate resins in the hard coat layer 3 is the sum of these contents.

[0069] [1-2-2] Hindered Amine Light Stabilizer The hard coat layer 3 contains a hindered amine light stabilizer.

[0070] First, the function of the hindered amine light stabilizer will be described. That is, the hindered amine light stabilizer has the function of returning the energy state of a substance excited by irradiation with ultraviolet light to the ground state and releasing the returned energy as heat.

[0071] Therefore, the hard coat layer 3 containing a hindered amine-based light stabilizer can prevent substances excited by irradiation with ultraviolet rays from causing chemical reactions, and can thus effectively prevent weather resistance deterioration such as yellowing of the exterior window film 1.

[0072] The hindered amine light stabilizer contained in the hard coat layer 3 has the function of improving the weather resistance of the hard coat layer 3 and suppressing deterioration of the properties over time due to light irradiation or the like.

[0073] The hindered amine light stabilizer has at least one group (hindered amine group) represented by the following formula (1) in one molecule.

[0074]

[0075] In formula (1), R 1 represents a hydrogen atom, an alkyl group, or an alkoxy group. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, and a butyl group. Examples of the alkoxy group include a methoxy group and an ethoxy group.

[0076] When there are multiple groups represented by formula (1) in one molecule, R 1 may be the same or different.

[0077] Examples of such hindered amine light stabilizers include dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate, poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene peridinyl)imino}], poly[{6-morpholino-s-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}], N,N',N'',N'''-tetrakis(4,6-bis(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)triazin-2-yl)-4, 7-diazadecane-1,10-diamine, bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butyl malonate, reaction products of cyclohexane with N-butyl 2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine peroxide and 2-aminoethanol, decane Examples of such esters include diacid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidyl) ester, reaction products of 1,1-dimethylethyl hydroperoxide and octane, a mixture of bis(1,2,2,6,6-pentamethyl-piperidyl) sebacate and methyl(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, and bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate. These may be used alone or in combination of two or more.

[0078] Among these, from the viewpoint of excellent performance as a light stabilizer and improving weather resistance, R 1is preferably a tertiary hindered amine group in which the alkyl group is a tertiary hindered amine group. A hindered amine light stabilizer having a tertiary hindered amine group has particularly excellent performance as a light stabilizer. In addition, the above-mentioned effects are more significantly exhibited.

[0079] Examples of such hindered amine light stabilizers include N,N',N'',N'''-tetrakis(4,6-bis(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)triazin-2-yl)-4,7-diazadecane-1,10-diamine, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-piperidyl)sebacate, and a mixture of methyl(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate.

[0080] Such hindered amine light stabilizers are commercially available, for example, from BASF under the trade name "Tinuvin (registered trademark) 292" (a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate).

[0081] As described above, the hindered amine light stabilizer may be contained in the hard coat layer 3 in a proportion of 2.0 parts by mass to 15.0 parts by mass relative to 100.0 parts by mass of the (meth)acrylate resin. However, the proportion of the hindered amine light stabilizer relative to 100.0 parts by mass of the (meth)acrylate resin is preferably 3.0 parts by mass to 14.0 parts by mass, more preferably 4.0 parts by mass to 12.0 parts by mass, and even more preferably 5.0 parts by mass to 10.0 parts by mass. This allows the effects of the present invention to be more significantly exhibited.

[0082] The content of the hindered amine light stabilizer in the hard coat layer 3 is preferably from 1.5% by mass to 12.5% ​​by mass, more preferably from 2.2% by mass to 11.5% by mass, and even more preferably from 4.0% by mass to 8.3% by mass, whereby the effects of the present invention described above are more significantly exhibited.

[0083] When the hard coat layer 3 contains a plurality of types of hindered amine light stabilizers, the content of the hindered amine light stabilizers in the hard coat layer 3 is the sum of the contents of these stabilizers.

[0084] [1-2-3] First Ultraviolet Absorbent The hard coat layer 3 contains a first ultraviolet absorbent.

[0085] The first ultraviolet absorber has the function of absorbing ultraviolet rays and converting them into energy such as heat, thereby preventing the effects of ultraviolet rays on the human body and articles.

[0086] The first ultraviolet absorber preferably has a maximum absorption wavelength of 380 nm or less in the wavelength range of 200 nm or more and 500 nm or less in an acetonitrile solution having a concentration of 0.1% by mass.

[0087] When there are a plurality of absorption maximum wavelengths in the wavelength range of 200 nm or more and 500 nm or less, it is preferable that at least one of the absorption maximum wavelengths is in the above range.

[0088] This allows the acrylic polymer to be sufficiently cured when irradiated with ultraviolet light without being inhibited by the first ultraviolet absorber.

[0089] On the other hand, the lower limit of the absorption maximum wavelength is preferably 280 nm or more from the viewpoint of preventing the effects of ultraviolet rays on the human body and articles.

[0090] Examples of the first ultraviolet absorber include compounds such as benzophenones, benzotriazoles, benzoates, benzoxazinones, triazines, phenyl salicylates, cyanoacrylates, and nickel complex salts, and one type may be used alone or two or more types may be used in combination.

[0091] Among the first ultraviolet absorbents, it is preferable to use a compound having a benzophenone structure or a hydroxyphenyltriazine structure.

[0092] These compounds have excellent compatibility with the above-mentioned (meth)acrylic resins and have a high ultraviolet absorbing function, so that the hard coat layer 3 formed thereon can easily satisfy the above-mentioned optical properties.

[0093] In particular, it is preferable that the hard coat layer 3 contains, as the first ultraviolet absorber, a compound having a benzophenone structure and a compound having a hydroxyphenyltriazine structure, whereby the above-mentioned effects are more significantly exhibited.

[0094] When the hard coat layer 3 contains a compound having a benzophenone structure and a compound having a hydroxyphenyltriazine structure as the first ultraviolet absorber, the ratio of the content of the compound having a benzophenone structure to the content of the compound having a hydroxyphenyltriazine structure in the hard coat layer 3 is preferably 1.0:2.0 or more and 2.0:1.0 or less, more preferably 1.0:1.5 or more and 1.5:1.0 or less, and even more preferably 1.0:1.2 or more and 1.2:1.0 or less, by mass ratio, whereby the above-mentioned effects are more significantly exhibited.

[0095] Specific examples of the first ultraviolet absorber include compounds represented by the following formulas (8) to (12).

[0096]

[0097]

[0098]

[0099] (In formula (11), R is an alkyl group having from 10 to 12 carbon atoms.)

[0100]

[0101] As commercially available products of the above-described first ultraviolet absorber, for example, products under the trade names "Tinuvin (registered trademark) 460," "Tinuvin (registered trademark) 477," and "Tinuvin (registered trademark) 400" are commercially available from BASF, and products under the trade names "Seesorb SB107" and "Seesorb SB106" are commercially available from Shipro Kasei Co., Ltd.

[0102] As described above, the first UV absorber may be contained in the hard coat layer 3 in a proportion of 5.0 parts by mass to 30.0 parts by mass relative to 100.0 parts by mass of the (meth)acrylate resin. However, the proportion of the first UV absorber relative to 100.0 parts by mass of the (meth)acrylate resin is preferably 5.5 parts by mass to 28.0 parts by mass, more preferably 6.0 parts by mass to 25.0 parts by mass, and even more preferably 7.0 parts by mass to 20.0 parts by mass. This allows the effects of the present invention to be more significantly exhibited.

[0103] The content of the first ultraviolet absorber in the hard coat layer 3 is preferably 3.3 mass % or more and 22.7 mass % or less, more preferably 4.0 mass % or more and 21.4 mass % or less, and even more preferably 6.3 mass % or more and 16.0 mass % or less, whereby the above-mentioned effects of the present invention are more significantly exhibited.

[0104] When the hard coat layer 3 contains a plurality of types of first ultraviolet absorbents, the content of the first ultraviolet absorbents in the hard coat layer 3 is the sum of the contents thereof.

[0105] [1-2-4] Other Components The hard coat layer 3 may contain components other than the above-mentioned components. Hereinafter, in this section, such components are also referred to as "other components."

[0106] Examples of such components include resin components other than the (meth)acrylate resin, light stabilizers other than hindered amine light stabilizers, antioxidants, silane coupling agents, leveling agents, antistatic agents, and antifoaming agents.

[0107] However, the proportion of other components in the hard coat layer 3 is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.

[0108] [1-2-5] Other Conditions The thickness of the hard coat layer 3 is not particularly limited, but is preferably 0.1 μm or more and 20 μm or less, more preferably 0.2 μm or more and 15 μm or less, and even more preferably 0.4 μm or more and 10 μm or less.

[0109] This prevents the hard coat layer 3 from becoming excessively hard, while providing even better abrasion resistance and improving the ease of handling of the exterior window film 1. As a result, the workability of attaching the exterior window film 1 to an adherend is improved. In addition, the occurrence of cracks and the like can be suitably prevented.

[0110] [1-3] Anchor Coat Layer The anchor coat layer 4 is provided between the substrate 2 and the hard coat layer 3 and has the function of increasing the adhesion between the substrate 2 and the hard coat layer 3 .

[0111] This prevents the hard coat layer 3 from peeling off from the substrate 2 even in an outdoor environment, and suppresses deterioration in the weather resistance and appearance of the exterior window film 1.

[0112] The anchor coat layer 4 is made of a material containing a thermosetting acrylic resin. The thermosetting acrylic resin contains, for example, a crosslinkable functional group-containing acrylic resin having a crosslinkable functional group capable of reacting with isocyanate, and a polyisocyanate compound as constituent components. The thermosetting acrylic resin forms a crosslinked structure and hardens when heated.

[0113] Examples of crosslinkable functional groups that can react with isocyanate include hydroxyl groups, thiol groups, amino groups, amide groups, carboxyl groups, etc. Among these, hydroxyl groups and carboxyl groups are preferred, and hydroxyl groups are more preferred.

[0114] In the following description, the case where the crosslinkable functional group of the acrylic resin is a hydroxyl group will be mainly described.

[0115] [1-3-1] Hydroxyl-containing acrylic resin The hydroxyl-containing acrylic resin is an acrylic resin having at least one hydroxyl group in one molecule.

[0116] The hydroxyl group-containing acrylic resin can be produced, for example, by copolymerizing a hydroxyl group-containing polymerizable unsaturated monomer with another polymerizable unsaturated monomer copolymerizable with the hydroxyl group-containing polymerizable unsaturated monomer by a known method, such as a solution polymerization method in an organic solvent or an emulsion polymerization method in water.

[0117] The hydroxyl group-containing polymerizable unsaturated monomer is a compound having one or more hydroxyl groups and one or more polymerizable unsaturated bonds in one molecule. Examples of such hydroxyl group-containing polymerizable unsaturated monomers include monoesters of (meth)acrylic acid with dihydric alcohols having from 2 to 8 carbon atoms (preferably from 2 to 4 carbon atoms), such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 7-hydroxyheptyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; ε-caprolactone-modified monoesters of (meth)acrylic acid with dihydric alcohols having from 2 to 8 carbon atoms; N-hydroxymethyl (meth)acrylamide; allyl alcohol; and (meth)acrylates having a polyoxyethylene chain whose molecular terminal is a hydroxyl group. These may be used alone or in combination of two or more.

[0118] In addition, examples of other polymerizable unsaturated monomers copolymerizable with the hydroxyl group-containing polymerizable unsaturated monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and nonyl (meth)acrylate. alkyl or cycloalkyl (meth)acrylates such as tridecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, "isostearyl acrylate" (trade name, manufactured by Osaka Organic Chemical Industry Ltd.), cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, and cyclododecyl (meth)acrylate; polymerizable unsaturated monomers having an isobornyl group such as isobornyl (meth)acrylate; polymerizable unsaturated monomers having an adamantyl group, such as adamantyl (meth)acrylate; vinyl aromatic compounds, such as styrene, α-methylstyrene, and vinyltoluene; polymerizable unsaturated monomers having an alkoxysilyl group, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, γ-(meth)acryloyloxypropyltrimethoxysilane, and γ-(meth)acryloyloxypropyltriethoxysilane; perfluoroalkyl (meth)acrylates, such as perfluorobutylethyl (meth)acrylate and perfluorooctylethyl (meth)acrylate; polymerizable unsaturated monomers having a fluorinated alkyl group, such as fluoroolefin; polymerizable unsaturated monomers having a photopolymerizable functional group, such as a maleimide group; vinyl compounds, such as N-vinylpyrrolidone, ethylene, butadiene, chloroprene, vinyl propionate, and vinyl acetate; carboxyl group-containing polymerizable unsaturated monomers, such as (meth)acrylic acid, maleic acid, crotonic acid, and β-carboxyethyl acrylate;Nitrogen-containing polymerizable unsaturated monomers such as (meth)acrylonitrile, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylamide, and adducts of glycidyl (meth)acrylate and amine compounds; polymerizable unsaturated monomers having two or more polymerizable unsaturated groups in one molecule such as allyl (meth)acrylate and 1,6-hexanediol di(meth)acrylate; epoxy group-containing polymerizable unsaturated monomers such as glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, 3,4-epoxycyclohexylpropyl (meth)acrylate, and allyl glycidyl ether; (meth)acrylates having a polyoxyethylene chain whose molecular terminal is an alkoxy group; 2-acrylamido-2-methylpropanesulfonic acid, allylsulfonic acid, and sodium styrenesulfonate; Polymerizable unsaturated monomers having a sulfonic acid group, such as sulfoethyl methacrylate and its sodium salts and ammonium salts; polymerizable unsaturated monomers having a phosphoric acid group, such as 2-acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, 2-acryloyloxypropyl acid phosphate, and 2-methacryloyloxypropyl acid phosphate; polymerizable unsaturated monomers having an ultraviolet-absorbing functional group, such as 2-hydroxy-4-(3-methacryloyloxy-2-hydroxypropoxy)benzophenone, 2-hydroxy-4-(3-acryloyloxy-2-hydroxypropoxy)benzophenone, 2,2'-dihydroxy-4-(3-methacryloyloxy-2-hydroxypropoxy)benzophenone, 2,2'-dihydroxy-4-(3-acryloyloxy-2-hydroxypropoxy)benzophenone, and 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole;4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, 4-crotonoylamino-2,2,6 Examples of suitable polymerizable unsaturated monomers include ultraviolet-stable polymerizable unsaturated monomers such as 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine and 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine; and polymerizable unsaturated monomer compounds having a carbonyl group such as acrolein, diacetone acrylamide, diacetone methacrylamide, acetoacetoxyethyl methacrylate, formylstyrene, and vinyl alkyl ketones having 4 to 7 carbon atoms (for example, vinyl methyl ketone, vinyl ethyl ketone, vinyl butyl ketone), and the like, and these may be used singly or in combination of two or more types selected from these.

[0119] The hydroxyl value of the hydroxyl-containing acrylic resin is preferably 20 mgKOH / g or more and 100 mgKOH / g or less, and more preferably 30 mgKOH / g or more and 80 mgKOH / g or less.

[0120] This allows the anchor coat layer 4 to have a good balance between coating strength and flexibility.

[0121] In this specification, the term "hydroxyl value" refers to a value determined in accordance with the method specified in "7.1 Neutralization titration method" of JIS K 0070:1992 "Test methods for acid value, saponification value, ester value, iodine value, hydroxyl value and unsaponifiable matter of chemical products." The acid value is also required for calculating the hydroxyl value, and the acid value is also determined in accordance with the method specified in "3.1 Neutralization titration method" of the same JIS standard.

[0122] The weight average molecular weight of the hydroxyl group-containing acrylic resin is, for example, preferably 3,000 or more and 100,000 or less, and more preferably 3,000 or more and 50,000 or less.

[0123] This can further improve the adhesion between the substrate 2 and the hard coat layer 3 via the anchor coat layer 4, and can also make the weather resistance of the anchor coat layer 4 more suitable.

[0124] In this specification, the terms "weight average molecular weight" and "number average molecular weight" are values ​​determined in accordance with the method specified in JIS K 0124-83, and are values ​​calculated from a chromatogram measured by gel permeation chromatography using the molecular weight of standard polystyrene as a reference.

[0125] The glass transition temperature of the hydroxyl group-containing acrylic resin is preferably 20°C or higher and 200°C or lower, more preferably 50°C or higher and 150°C or lower, and even more preferably 70°C or higher and 120°C or lower.

[0126] This makes it possible to improve the coating strength and weather resistance of the anchor coat layer 4 .

[0127] In this specification, the glass transition temperature (°C) refers to the static glass transition temperature, and is a value calculated, for example, as follows. First, using a differential scanning calorimeter "DSC-50Q" (trade name, manufactured by Shimadzu Corporation), a sample is placed in a measuring cup and vacuum suction is applied to completely remove the solvent. Next, the sample is rapidly cooled in a nitrogen stream, and the change in calorific value is measured in the range of -100°C to 100°C at a temperature rise rate of 3°C / min. The first change point in the baseline on the low temperature side is then calculated as the glass transition temperature, and a value is obtained.

[0128] [1-3-2] Polyisocyanate Compound The polyisocyanate compound functions as a crosslinking agent. The isocyanate group of the polyisocyanate compound reacts with the crosslinkable functional group, such as a hydroxyl group, of the crosslinkable functional group-containing acrylic resin to form a crosslinked structure.

[0129] The polyisocyanate compound is a compound having two or more free isocyanate groups in one molecule, and the isocyanate groups are not blocked with a blocking agent.

[0130] Specific examples of the polyisocyanate compound include aliphatic polyisocyanate compounds having 2 to 18 carbon atoms, alicyclic polyisocyanate compounds having 4 to 15 carbon atoms, aromatic aliphatic polyisocyanate compounds having 8 to 15 carbon atoms, aromatic polyisocyanate compounds having 6 to 20 carbon atoms (excluding carbon atoms in NCO groups, the same applies below), compositions thereof, and modified products of these polyisocyanate compounds (e.g., modified products containing urethane groups, carbodiimide groups, allophanate groups, urea groups, biuret groups, uretdione groups, uretoimine groups, isocyanurate groups, and oxazolidone groups). These compounds may be used singly or in combination.

[0131] Examples of the aliphatic polyisocyanate compound include ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl)fumarate, bis(2-isocyanatoethyl)carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate. One or more selected from these compounds may be used alone or in combination.

[0132] Examples of the alicyclic polyisocyanate compound include isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-cyclohexene-1,2-dicarboxylate, and 2,5- and / or 2,6-norbornane diisocyanate. One or more selected from these may be used in combination.

[0133] Examples of the aromatic aliphatic polyisocyanate compound include m- and / or p-xylylene diisocyanate (XDI), α,α,α',α'-tetramethylxylylene diisocyanate (TMXDI), and the like, and one or more selected from these can be used in combination.

[0134] Examples of the aromatic polyisocyanate compound include 1,3- and / or 1,4-phenylene diisocyanate, 2,4- and / or 2,6-tolylene diisocyanate (TDI), 2,4'- and / or 4,4'-biphenylmethane diisocyanate (MDI), 4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatodiphenylmethane, 1,5-naphthylene diisocyanate, 4,4',4''-triphenylmethane triisocyanate, m- and p-isocyanatophenylsulfonyl isocyanate, and the like. One or more selected from these can be used alone or in combination.

[0135] Examples of modified polyisocyanate compounds include modified polyisocyanates such as modified MDI (urethane-modified MDI, carbodiimide-modified MDI, trihydrocarbyl phosphate-modified MDI), urethane-modified TDI, biuret-modified HDI, isocyanurate-modified HDI, and isocyanurate-modified IPDI, and one or more selected from these may be used in combination. More specifically, for example, modified MDI and urethane-modified TDI (isocyanate group-containing prepolymer) may be used in combination.

[0136] In addition to the above polyisocyanate compounds, blocked polyisocyanate compounds in which the isocyanate groups are blocked with a blocking agent can also be used. Examples of blocking agents include phenol compounds, oxime compounds, lactam compounds, alcohol compounds, mercaptan compounds, pyrazole compounds, and active methylene compounds such as diethyl malonate, and one or more selected from these can be used in combination.

[0137] When a blocked polyisocyanate compound is used, it is preferable to use a catalyst for dissociating the blocking agent in combination. An unblocked polyisocyanate compound and a blocked polyisocyanate compound can also be used in combination.

[0138] From the viewpoint of weather resistance, the polyisocyanate compound is preferably an aliphatic polyisocyanate compound or an alicyclic polyisocyanate compound.

[0139] The number average molecular weight of the polyisocyanate compound is not particularly limited, but is preferably 3,000 or less, and more preferably 100 or more and 1,500 or less.

[0140] This can further improve the adhesion between the substrate 2 and the hard coat layer 3 via the anchor coat layer 4, and can also make the flexibility of the anchor coat layer 4 more suitable.

[0141] The ratio of the hydroxyl group-containing acrylic resin to 100 parts by mass of the total solid content of the hydroxyl group-containing acrylic resin and the polyisocyanate compound is preferably 70 parts by mass or more and 97 parts by mass or less, more preferably 75 parts by mass or more and 95 parts by mass or less, and even more preferably 80 parts by mass or more and 93 parts by mass or less.

[0142] This makes it possible to make the stability and curability of the composition for forming the anchor coat layer 4 more favorable.

[0143] Furthermore, the ratio of the polyisocyanate compound to 100 parts by mass of the total solid content of the hydroxyl group-containing acrylic resin and the polyisocyanate compound is preferably 3 parts by mass or more and 30 parts by mass or less, more preferably 5 parts by mass or more and 25 parts by mass or less, and even more preferably 7 parts by mass or more and 20 parts by mass or less.

[0144] This makes it possible to make the stability and curability of the composition for forming the anchor coat layer 4 more favorable.

[0145] The ratio (NCO / OH) of the total amount (mol) of isocyanate groups (NCO) of the polyisocyanate compound contained in the composition for forming the anchor coat layer 4 to the total amount (mol) of hydroxyl groups (OH) of the hydroxyl group-containing acrylic resin contained in the composition is preferably 0.20 or more and 0.80 or less, more preferably 0.30 or more and 0.70 or less, and even more preferably 0.40 or more and 0.65 or less.

[0146] This allows a more appropriate crosslinked structure to be formed between the hydroxyl group-containing acrylic resin, and the adhesion between the substrate 2 and the hard coat layer 3 via the anchor coat layer 4 can be further improved.

[0147] The total amount of isocyanate groups can be calculated from the NCO content, which is the mass ratio (unit: mass%) of isocyanate groups in the polyisocyanate compound contained in the composition, and the mass of the isocyanate compound contained in the composition.

[0148] The total amount of hydroxyl groups can be determined from the hydroxyl value (unit: mgKOH / g) of the entire hydroxyl group-containing acrylic resin contained in the composition.

[0149] [1-3-3] Second UV Absorber The anchor coat layer 4 preferably contains a second UV absorber.

[0150] This allows ultraviolet rays to be cut not only by the hard coat layer 3 but also by the anchor coat layer 4, more reliably reducing the proportion of ultraviolet rays in the light transmitted through the exterior window film 1. Furthermore, cutting ultraviolet rays by the anchor coat layer 4 while the exterior window film 1 is attached to an adherend can also contribute to further suppressing deterioration of the pressure-sensitive adhesive layer 5 and the substrate 2.

[0151] Examples of the second ultraviolet absorber include compounds such as benzophenones, benzotriazoles, benzoates, benzoxazinones, triazines, phenyl salicylates, cyanoacrylates, and nickel complex salts, and one type may be used alone or two or more types may be used in combination.

[0152] More specifically, the second ultraviolet absorber may be any of the ultraviolet absorbers exemplified in [1-2-3] above.

[0153] Among the second ultraviolet absorbents, it is preferable to contain a compound having a hydroxyphenyltriazine structure.

[0154] Compounds having a hydroxyphenyltriazine structure have excellent compatibility with the above-mentioned thermosetting acrylic resins and have high ultraviolet absorption properties, so that the anchor coat layer 4 formed thereon is likely to have the above-mentioned optical properties.

[0155] In the anchor coat layer 4, the second ultraviolet absorber is preferably contained in a proportion of 5.0 parts by mass to 45.0 parts by mass to 100.0 parts by mass of the acrylic resin in a heat-cured state, more preferably 7.0 parts by mass to 42.0 parts by mass, even more preferably 8.0 parts by mass to 37.5 parts by mass, and most preferably 10.0 parts by mass to 30.0 parts by mass, relative to 100.0 parts by mass of the acrylic resin in a heat-cured state. This makes the above-mentioned effects more pronounced.

[0156] The content of the second ultraviolet absorber in the anchor coat layer 4 is preferably 4.1% by mass or more and 34.0% by mass or less, more preferably 5.7% by mass or more and 32.0% by mass or less, and even more preferably 8.3% by mass or more and 24.0% by mass or less, whereby the above-mentioned effects are more significantly exhibited.

[0157] When the anchor coat layer 4 contains a plurality of types of second ultraviolet absorbents, the content of the second ultraviolet absorbents in the anchor coat layer 4 is the sum of these contents.

[0158] [1-3-4] Other Components The anchor coat layer 4 may contain components other than the above-mentioned components. Hereinafter, in this section, such components will also be referred to as "other components."

[0159] Such components include, for example, antifoaming agents, surfactants, curing catalysts, thickeners, preservatives, antifreeze agents, and the like.

[0160] However, the proportion of other components in the anchor coat layer 4 is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.

[0161] [1-3-5] Other Conditions The thickness of the anchor coat layer 4 is not particularly limited, but is preferably 0.05 μm or more and 5.0 μm or less, more preferably 0.1 μm or more and 3.0 μm or less, and even more preferably 0.5 μm or more and 2.0 μm or less.

[0162] This prevents the anchor coat layer 4 from becoming excessively hard, further improving the adhesion between the substrate 2 and the hard coat layer 3 via the anchor coat layer 4, and also improving the ease of handling of the exterior window film 1, improving the workability of attaching the exterior window film 1 to an adherend, etc. This makes it possible to more significantly exhibit the effects of the present invention described above.

[0163] [1-4] Pressure-sensitive adhesive layer The pressure-sensitive adhesive layer 5 generally has excellent flexibility and is the portion that adheres closely to the adherend.

[0164] Examples of adhesives that can be used to form the adhesive layer 5 include acrylic adhesives, natural rubber adhesives, synthetic rubber adhesives, polyvinyl ether adhesives, urethane adhesives, and silicone adhesives.

[0165] Among these, acrylic adhesives, urethane adhesives, and silicone adhesives are particularly suitable from the standpoint of weather resistance and the like.

[0166] Specific examples of synthetic rubber adhesives include styrene-butadiene rubber, polyisobutylene rubber, isobutylene-isoprene, styrene-isoprene block copolymer, styrene-butadiene block copolymer, and styrene-ethylene-butylene block copolymer.

[0167] Specific examples of acrylic pressure-sensitive adhesives include copolymers obtained by polymerizing two or more of various polymerization components such as butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, methyl (meth)acrylate, hydroxyethyl (meth)acrylate, and hydroxybutyl (meth)acrylate.

[0168] Specific examples of polyvinyl ether-based adhesives include polyvinyl ether and polyvinyl isobutyl ether.

[0169] A specific example of the silicone-based adhesive is dimethylpolysiloxane, etc. These adhesives may be used alone or in combination of two or more.

[0170] The adhesive layer 5 only needs to be composed mainly of an adhesive, and may contain components other than the adhesive.

[0171] Examples of such components include ultraviolet absorbers, tackifiers, fillers, softeners, antioxidants, light stabilizers, crosslinking agents, colorants, modifiers, rust inhibitors, flame retardants, hydrolysis inhibitors, surface lubricants, corrosion inhibitors, heat stabilizers, lubricants, antistatic agents, polymerization inhibitors, catalysts, leveling agents, thickeners, dispersants, and antifoaming agents.

[0172] The thickness of the pressure-sensitive adhesive layer 5 is not particularly limited, but is preferably, for example, 1 μm to 100 μm, more preferably 5 μm to 50 μm, and even more preferably 15 μm to 25 μm.

[0173] This not only improves the weather resistance of the exterior window film 1, but also improves the ease of handling of the exterior window film 1, facilitating application (adhesion) to an adherend. Furthermore, the exterior window film 1 is also improved in conformity to the shape of a curved adherend, effectively preventing wrinkles and the like from forming.

[0174] [1-5] Other Conditions The overall thickness of the exterior window film 1 is not particularly limited, but is preferably 11 μm or more and 400 μm or less, more preferably 20 μm or more and 150 μm or less, and even more preferably 30 μm or more and 100 μm or less.

[0175] This improves the weather resistance and UV absorption properties of the exterior window film 1, improves the handling properties of the exterior window film 1, and makes it easier to apply the film to an adherend. Furthermore, the film is also more adaptable to curved surfaces, effectively preventing wrinkles and other imperfections in the exterior window film 1.

[0176] Here, the "total thickness" refers to the overall thickness of the exterior window film 1 when it is attached to an adherend. Therefore, for example, even if a release liner 10 (described below) is disposed on the pressure-sensitive adhesive layer 5 during storage of the exterior window film 1, the thickness of the release liner 10 is not included in the total thickness.

[0177] The exterior window film 1 is preferably transparent so as not to impair the appearance of the adherend.

[0178] In this specification, "transparent" refers to a transmittance in the visible light region of 60% or more (upper limit 100%), and preferably 80% or more (upper limit 100%). The transmittance of the exterior window film 1 can be measured by a method in accordance with JIS A5759:2016 (Architectural Window Films - Visible Light Transmittance Test).

[0179] The exterior window film 1 preferably has a yellowness index (YI) of 4 or less, more preferably 0 or more and 3.5 or less, and even more preferably 0 or more and 2.5 or less.

[0180] This results in an exterior window film 1 with reduced coloration, excellent transparency and colorlessness, and suitable for use as an exterior window film 1.

[0181] The yellowness index (YI) of the exterior window film 1 can be measured by a method in accordance with JIS K 7373:2006.

[0182] The haze of the exterior window film 1, measured in accordance with JIS K 7136:2000, should be close to that of the substrate 2 alone, preferably 2.0% or less, more preferably 1.8% or less, and even more preferably 1.5% or less, which allows the exterior window film 1 to have excellent transparency.

[0183] [2] Release Liner A release liner 10 may be disposed on the pressure-sensitive adhesive layer 5 of the exterior window film 1 .

[0184] The release liner 10 is peeled off from the pressure-sensitive adhesive layer 5 when the exterior window film 1 is to be stuck to an adherend.

[0185] The release liner 10 is not particularly limited and may have a configuration commonly used in the field of window films. For example, the release liner 10 may have a configuration in which a release layer is provided on the surface of a paper substrate or a resin film substrate.

[0186] Examples of materials constituting the resin film substrate include polyethylene terephthalate, polypropylene, etc. Examples of materials constituting the paper substrate include polyethylene-laminated paper, polypropylene-laminated paper, clay-coated paper, resin-coated paper, glassine paper, and fine paper.

[0187] The release layer may be a release layer containing a release agent such as silicone, long-chain alkyl resin, or fluorine-based resin.

[0188] The thickness of the release liner 10 is not particularly limited, but is preferably, for example, 10 μm to 400 μm. If the release layer is provided, the thickness of the release layer is preferably, for example, 0.01 μm to 5 μm.

[0189] [3] Manufacturing Method of Window Film Next, a manufacturing method of the window film for exterior application will be described.

[0190] The exterior window film 1 can be produced, for example, by a method including an anchor coat layer forming step of applying a liquid composition (coating liquid) for forming the anchor coat layer 4 to one surface of the substrate 2 to form the anchor coat layer 4, a hard coat layer forming step of applying a liquid composition (coating liquid) for forming the hard coat layer 3 onto the anchor coat layer 4 to form the hard coat layer 3, and a pressure-sensitive adhesive layer forming step of applying a liquid composition (coating liquid) for forming the pressure-sensitive adhesive layer 5 to the other surface of the substrate 2 to form the pressure-sensitive adhesive layer 5. In such a method, the order of the anchor coat layer forming step, hard coat layer forming step, and pressure-sensitive adhesive layer forming step is not particularly limited.

[0191] [3-1] Anchor Coat Layer Forming Step In the anchor coat layer forming step, a liquid composition (coating liquid) for forming the anchor coat layer 4 is applied to one surface of the substrate 2 to form the anchor coat layer 4.

[0192] From the viewpoint of storage stability, the liquid composition (coating liquid) for forming the anchor coat layer 4 is preferably a multi-component composition containing a main component (liquid A) and a curing agent component (liquid B). Here, the term "multi-component composition" refers to a composition in which two or more components (preferably two components) are mixed together during coating, and is distinguished from a "single-component composition" which is mixed from the beginning of production.

[0193] The main component (liquid A) contains, for example, a hydroxyl group-containing acrylic resin and an ultraviolet absorber, and the curing agent component (liquid B) contains, for example, a polyisocyanate compound.

[0194] When the composition for forming the anchor coat layer 4 is a multi-component composition, the anchor coat layer formation process includes a step of mixing a main component (component A) and a curing agent component (component B) to prepare a liquid composition for forming the anchor coat layer 4.

[0195] Methods for mixing the base component (liquid A) and the curing agent component (liquid B) include mixing in a coating device, mixing in a pipe, and mixing in a storage tank, and any of these methods can be suitably used.

[0196] From the viewpoint of storage stability, the timing for mixing the main component (liquid A) and the curing agent component (liquid B) is, for example, from 0.01 second to 3 months before applying the composition to the substrate 2, preferably from 0.1 second to 10 days before, and more preferably from 0.1 second to 10 hours before.

[0197] The solid content concentration in the liquid composition for forming the anchor coat layer 4 is preferably 10% by mass or more and 60% by mass or less, more preferably 12% by mass or more and 50% by mass or less, and even more preferably 15% by mass or more and 50% by mass or less.

[0198] This makes it possible to make the coating properties of the liquid composition for forming the anchor coat layer 4 more favorable.

[0199] The liquid composition for forming the anchor coat layer 4 thus obtained is applied onto the substrate 2 to obtain an uncured coating film.

[0200] The liquid composition for forming the anchor coat layer 4 can be applied by a known method, such as bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, or air spraying.

[0201] The uncured coating film obtained by applying a liquid composition for forming the anchor coat layer 4 onto the substrate 2 may be preheated (pre-dried) or air-blown under conditions that do not substantially cure the coating film.

[0202] The preheating temperature is preferably 40°C or higher and 100°C or lower, more preferably 50°C or higher and 90°C or lower, and even more preferably 60°C or higher and lower than 80°C.

[0203] The preheating time is preferably 30 seconds or more and 15 minutes or less, and more preferably 1 minute or more and 10 minutes or less.

[0204] The air blowing can be carried out, for example, by blowing air at a temperature of 10° C. or higher and 80° C. or lower onto the coated surface of the composition for 30 seconds or longer and 15 minutes or shorter.

[0205] Next, the uncured coating film is heated to cure the coating film, thereby forming the anchor coat layer 4 .

[0206] The uncured coating film may be heated by a known method, for example, by using hot air heating, infrared heating, high frequency heating, or the like.

[0207] The heating temperature of the uncured coating film is preferably 100°C or higher and 200°C or lower, more preferably 120°C or higher and 180°C or lower, and even more preferably 130°C or higher and 170°C or lower.

[0208] This allows the uncured coating film to be cured more suitably, and the anchor coat layer 4 to be formed more suitably.

[0209] The heating time for the uncured coating film is preferably from 1 second to 10 minutes, more preferably from 10 seconds to 3 minutes, and even more preferably from 30 seconds to 2 minutes.

[0210] This allows the uncured coating film to be cured more suitably, and the anchor coat layer 4 to be formed more suitably.

[0211] [3-2] Hard Coat Layer Forming Step In the hard coat layer forming step, a liquid composition (coating liquid) for forming the hard coat layer 3 is applied onto the anchor coat layer 4 to form the hard coat layer 3 .

[0212] The liquid composition for forming the hard coat layer 3 can be applied by a known method, such as bar coating, knife coating, roll coating, blade coating, die coating, or gravure coating.

[0213] The hard coat layer 3 is formed by curing the liquid composition for forming the hard coat layer 3 that has been applied onto the anchor coat layer 4 .

[0214] The liquid composition for forming the hard coat layer 3 can be cured by, for example, irradiation with energy rays such as ultraviolet rays or electron beams, heating, or the like.

[0215] The liquid composition for forming the hard coat layer 3 preferably further contains a photopolymerization initiator from the viewpoint of shortening the polymerization time by light irradiation and reducing the amount of light irradiation when forming the hard coat layer 3. In other words, the (meth)acrylate resin is preferably configured by polymerizing urethane (meth)acrylate using a photopolymerization initiator.

[0216] Examples of the photopolymerization initiator include triphenylphosphine oxide compounds, α-aminoalkylphenone compounds, benzoin compounds, acetophenone compounds, acylphosphineoxide compounds, titanocene compounds, thioxanthone compounds, peroxide compounds, and further photosensitizers such as amines and quinones. More specific examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzyl phenyl sulfide. tetramethylthiuram monosulfide, azobisisobutyrolnitrile, dibenzyl, diacetyl, 8-chloroanthraquinone, 1-benzoyl-1-hydroxycyclohexyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and the like. One or a combination of two or more selected from these can be used, and among these, triphenylphosphine oxide compounds are preferred.

[0217] The content of the photopolymerization initiator in the liquid composition for forming the hard coat layer 3 is preferably 0.05 parts by mass or more and 15.0 parts by mass or less, more preferably 0.1 parts by mass or more and 10.0 parts by mass or less, and even more preferably 0.3 parts by mass or more and 5.0 parts by mass or less, relative to 100.0 parts by mass of the urethane (meth)acrylate content. This makes it possible to more significantly exhibit the above-mentioned effects.

[0218] If necessary, components other than the above-mentioned components may be contained in the liquid composition for forming the hard coat layer 3. Examples of such components include a thermosetting catalyst and a solvent.

[0219] [3-3] Pressure-sensitive adhesive layer forming step In the pressure-sensitive adhesive layer forming step, a liquid composition (coating liquid) for forming the pressure-sensitive adhesive layer 5 is applied to the other surface side of the substrate 2 to form the pressure-sensitive adhesive layer 5.

[0220] A coating liquid prepared by dissolving or suspending the above-described materials constituting the pressure-sensitive adhesive layer 5 in an appropriate solvent can be used as the liquid composition for forming the pressure-sensitive adhesive layer 5. Examples of the solvent include esters such as ethyl acetate and butyl acetate; ketones such as methyl isobutyl ketone, methyl ethyl ketone and cyclohexanone; and aromatic hydrocarbons such as toluene and xylene, and one or more selected from these can be used in combination.

[0221] The liquid composition for forming the pressure-sensitive adhesive layer 5 may be applied by a known method, for example, a method using various coaters such as an air knife coater, a blade coater, a bar coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Mayer bar coater, or a kiss coater.

[0222] The amount of the liquid composition for forming the pressure-sensitive adhesive layer 5 to be applied may be adjusted as appropriate so that the thickness of the pressure-sensitive adhesive layer 5 after drying falls within the above-mentioned range. The drying conditions for the liquid composition for forming the pressure-sensitive adhesive layer 5 are not particularly limited, but the drying temperature may be, for example, 70°C or higher and 130°C or lower, and the drying time may be, for example, 1 minute or higher and 5 minutes or lower. In this manner, a window film 1 for exterior application can be obtained.

[0223] Furthermore, a release liner 10 may be further laminated on the pressure-sensitive adhesive layer 5 of the exterior window film 1 .

[0224] [4] Adherend Next, an adherend to which the exterior window film 1 is attached will be described.

[0225] The exterior window film 1 is suitably applied to windowpanes of buildings such as houses and offices, and vehicles such as automobiles and trains.

[0226] In particular, the exterior window film 1 of the present invention is attached to the exterior surface of a window glass. With such an exterior window film 1, sunlight strikes in the following order: hard coat layer 3 / anchor coat layer 4 / substrate 2 / adhesive layer 5 / window glass / indoors. Therefore, the hard coat layer 3 and anchor coat layer 4 can block ultraviolet rays, thereby suitably suppressing deterioration of the hard coat layer 3. Deterioration of the substrate 2 and adhesive layer 5 due to ultraviolet rays can also be suitably suppressed. In addition to ultraviolet rays, deterioration of each layer of the exterior window film 1 due to rain, wind, temperature changes, etc. can also be suitably suppressed.

[0227] Furthermore, in the exterior window film 1, the adhesion between the substrate 2 and the hard coat layer 3 is improved via the anchor coat layer 4. Therefore, peeling between the substrate 2 and the hard coat layer 3 is prevented even in an outdoor environment, and deterioration of the hard coat layer 3 can be more effectively prevented.

[0228] As described above, the exterior window film 1 has excellent weather resistance and can therefore be suitably used as an exterior window film, which is placed in a harsher environment than an interior window film.

[0229] [5] Method for Applying Window Film Next, a method for applying the exterior window film 1 will be described.

[0230] When the exterior window film 1 is applied to an adherend such as a window glass, if a release liner 10 is present, the film can be applied by first peeling off the release liner 10 to expose the pressure-sensitive adhesive layer 5 and then adhering the pressure-sensitive adhesive layer 5 to the adherend. Here, application may also be performed by a so-called water application method, in which application is performed at the interface between the pressure-sensitive adhesive layer 5 and the adherend via an application liquid prepared by adding a surfactant to water, and then scraping out the application liquid using a tool called a squeegee.

[0231] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these.

[0232] For example, the exterior window film may have a configuration other than those described above. More specifically, for example, the exterior window film may have at least one intermediate layer between the substrate and the pressure-sensitive adhesive layer, between the substrate and the anchor coat layer, or between the anchor coat layer and the hard coat layer, or may further have at least one coating layer on the outer surface side of the hard coat layer.

[0233] Furthermore, the exterior window film of the present invention may be produced by any method, and the production method is not limited to the above-mentioned production method.

[0234] For example, the window film for exterior application of the present invention may be formed by applying a transfer method in which a composition for forming an adhesive layer is formed on one side of a release liner, and then the release liner with the adhesive layer formed thereon is bonded to a substrate.

[0235] The method for producing an exterior window film may include other steps in addition to the steps described above. Examples of such steps include a pre-treatment step, an intermediate treatment step, and a post-treatment step.

[0236] Furthermore, a step of seasoning the laminate of the substrate and the anchor coat layer may be included between the anchor coat layer forming step and the hard coat layer forming step.

[0237] The present invention will be described in detail below based on specific examples, but the present invention is not limited thereto. In the following examples, treatments and measurements for which temperature conditions are not specified were carried out at room temperature (23°C).

[0238] [6] Manufacturing of exterior window film (Example 1) A liquid composition (coating liquid) for forming an anchor coat layer was prepared using a base material containing a hydroxyl group-containing acrylic resin and Tinuvin 477 (manufactured by BASF) as an ultraviolet absorber, a curing agent containing a polyisocyanate compound, and propylene glycol methyl ether acetate as a solvent. The liquid composition for forming the anchor coat layer was prepared so that the solid content concentration was 20 mass%.

[0239] The hydroxyl group-containing acrylic resin used here contained polymethyl methacrylate resin as a constituent component.

[0240] The proportion of the hydroxyl group-containing acrylic resin in the solid content of the base resin was 76 mass %, the proportion of the ultraviolet absorber was 24 mass %, and the NCO content of the polyisocyanate compound used was 21 mass %.

[0241] The liquid composition for forming the anchor coat layer as described above was applied to one side of the substrate by a bar coating method, adjusting the amount of coating so that the film thickness after curing would be 1.5 μm. This coating film was then subjected to a heat treatment at 120° C. for 1 minute. This formed an anchor coat layer.

[0242] As the substrate, a 50 μm thick polyethylene terephthalate film containing an ultraviolet absorber (manufactured by Toyobo Co., Ltd., Toyobo Ester (registered trademark) film HB3) was used.

[0243] The laminate of the substrate and the anchor coat layer was then seasoned for 4 days in an environment of 23° C. and 50% RH.

[0244] Next, a hard coat layer was formed on the anchor coat layer. A liquid composition (coating liquid) for forming the hard coat layer was prepared using Beamset 575CB (manufactured by Arakawa Chemical Industries, Ltd.) containing urethane acrylate, Tinuvin 292 (manufactured by BASF) as a hindered amine-based light stabilizer, UV-24 (manufactured by Solvay) as a benzophenone-based ultraviolet absorber, Tinuvin 477 (manufactured by BASF) as an ultraviolet absorber, Omnirad 907 (manufactured by IGM Resins) as a photopolymerization initiator, and methyl ethyl ketone as a solvent.

[0245] Tinuvin 292, the structure of which is shown below, is a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate.

[0246]

[0247] UV-24 is 2,2'-dihydroxy-4-methoxybenzophenone, the structure of which is shown below.

[0248]

[0249] Tinuvin 477 is a mixture of a hydroxyphenyltriazine-based ultraviolet absorber and 1-methoxy-2-propyl acetate.

[0250] Also, Omnirad 907 is 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, the structure of which is shown below.

[0251]

[0252] The liquid composition for forming the hard coat layer as described above was applied to one side of the substrate by a bar coating method while adjusting the amount of application so that the film thickness after curing would be 2.5 μm, to obtain a coating film. This coating film was irradiated with an ultraviolet ray irradiator of a high-pressure mercury lamp under a nitrogen atmosphere with an integrated light dose of 200 mJ / cm. 2 The coated film was irradiated with ultraviolet light of 1000 kJ / cm. Thereby, a hard coat layer was formed.

[0253] Next, a solution of an acrylic adhesive (100 parts by weight of a copolymer (weight average molecular weight 600,000) of butyl acrylate / acrylic acid = 90 parts by weight / 10 parts by weight, 1 part by weight of an isocyanate-based crosslinking agent, and 4.3 parts by weight of an ultraviolet absorber) was applied to the surface of the substrate opposite to the surface on which the hard coat layer was provided, so that the thickness after drying would be 25 μm, thereby obtaining a coating film. This coating film was dried at 100 ° C. for 1 minute to form an adhesive layer, and an exterior window film was produced. A release liner having a thickness of 38 μm was laminated onto the adhesive layer of the exterior window film.

[0254] (Examples 2 to 8) Exterior window films were produced in the same manner as in Example 1, except that the amount of each component used in the liquid composition for forming the anchor coat layer and the liquid composition for forming the hard coat layer was changed so that the content of each component in the liquid composition for forming the anchor coat layer satisfied the relationship shown in Table 1.

[0255] Comparative Examples 1 to 9 An attempt was made to manufacture an exterior window film in the same manner as in Example 1, except that the amount of each component used in the liquid composition for forming the anchor coat layer and the liquid composition for forming the hard coat layer was changed so that the content of each component in the liquid composition for forming the anchor coat layer satisfied the relationship shown in Table 2. In Comparative Examples 1 to 8 and 10, exterior window films could be manufactured, but in Comparative Example 9, the hard coat layer did not harden.

[0256] Comparative Example 10 An exterior window film was produced in the same manner as in Example 1, except that a thermosetting polyester resin was used instead of the thermosetting acrylic resin in the liquid composition for forming the anchor coat layer.

[0257] [7] Evaluation of exterior window film The obtained exterior window film was evaluated as follows.

[0258] [7-1] Weather Resistance Test of Hard Coat Layer An accelerated weather resistance test was carried out using a sunshine weather meter.

[0259] The obtained exterior window film was attached to a glass plate, and the glass was placed in a sunshine weather meter. The irradiance was 255 W / m 2 An accelerated weathering test was carried out by exposing the hard coat layer to a black panel temperature of 63°C and a humidity of 50% RH for 2000 hours. The surface of the hard coat layer was visually observed to evaluate the presence or absence of cracks.

[0260] A: No cracks C: Cracks

[0261] [7-2] Adhesion test between substrate and hard coat layer The obtained exterior window film was attached to a glass plate. Then, on the surface on which the hard coat layer was formed, a cross-cut section was made with a cut interval of 1 mm and 10 cut lines x 10 squares, based on the cross-cut method of JIS K 5600-5-6:1999 (ISO 2409:1992), and the adhesion between the substrate and the hard coat layer was evaluated. Cellotape (registered trademark) manufactured by Nichiban Co., Ltd. was attached to the cross-cut section, and after peeling off the tape, the surface of the hard coat layer was visually observed to evaluate whether or not it peeled off.

[0262] A: No peeling B: Slight peeling C: Obvious peeling

[0263] The exterior window film after the accelerated weather resistance test in [7-1] above was also evaluated in the same manner as above.

[0264] [7-3] Crack Resistance Test of Hard Coat Layer The obtained exterior window film was wound into a roll around a cylindrical core having an outer diameter of 20 mm, with the hard coat layer facing outward.

[0265] The core was removed, and a needle was pushed 10 mm into the hard coat layer. The broken surface was visually inspected to evaluate the presence or absence of cracks.

[0266] A: No cracks C: Cracks

[0267] [7-4] Haze of exterior window film The haze of the obtained exterior window film was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., NDH-5000) in accordance with JIS K7136:2000 and evaluated according to the following criteria. The smaller this value, the more excellent the transparency.

[0268] A: Haze is 2.0 or less B: Haze is more than 2.0 and less than 5.0 C: Haze is more than 5.0 and less than 10.0 D: Haze is more than 10.0 and less than 20.0 E: Haze is more than 20.0

[0269] [7-5] Scratch Resistance Test of Hard Coat Layer The obtained exterior window film was set in a Gakushin-type abrasion tester (AB-301 manufactured by Tester Sangyo Co., Ltd.), and the surface of the hard coat layer was rubbed with #0000 steel wool at a load of 50 g / cm. 2 After the friction test, the surface of the hard coat layer was visually observed to evaluate whether or not there were scratches.

[0270] A: No scratches B: A few scratches C: Many scratches

[0271] Tables 1 and 2 summarize the results of the above evaluations for each of the examples and comparative examples, along with the conditions of the compositions used to form the anchor coat layer and hard coat layer. In Tables 1 and 2, the unit of content of each component is parts by mass, and the contents of the hindered amine light stabilizer and ultraviolet absorber are shown as percentages relative to 100.0 parts by mass of urethane acrylate contained in the formed hard coat layer. In Comparative Example 9, the hard coat layer did not harden, so the above evaluations could not be performed.

[0272]

[0273]

[0274] As is clear from Table 1, the examples provided good results in terms of weather resistance, crack resistance, haze, abrasion resistance, and adhesion of the hard coat layer. In contrast, as shown in Table 2, the comparative examples provided unsatisfactory results.

[0275] More specifically, in Comparative Examples 1 to 3 in which no anchor coat layer was formed, and Comparative Example 10 in which a thermosetting polyester resin was used for the anchor coat layer, sufficient adhesion between the substrate and the hard coat layer was not obtained.

[0276] Furthermore, in Comparative Examples 1, 2, and 4, in which the hard coat layer did not contain a hindered amine light stabilizer, cracks occurred after the weather resistance test and the haze was also large. Furthermore, Comparative Example 7, which did not contain an ultraviolet absorber, had significantly poor weather resistance. Furthermore, Comparative Example 1, which did not contain either a hindered amine light stabilizer or an ultraviolet absorber, had even greater haze. Furthermore, Comparative Example 8, which contained both a hindered amine light stabilizer and an ultraviolet absorber but had a low content of ultraviolet absorber, and Comparative Example 5, which contained a low content of hindered amine light stabilizer, showed reduced adhesion after the weather resistance test. Furthermore, Comparative Example 6, which contained a high content of hindered amine light stabilizer, had a high haze.

[0277] In addition, in preparing the liquid composition for forming a hard coat layer, the ratio of the hindered amine light stabilizer and the ratio of the ultraviolet absorber relative to the (meth)acrylate resin in the liquid composition for forming a hard coat layer were variously changed so that, relative to 100.0 parts by mass of the (meth)acrylate resin in the hard coat layer to be formed, the ratios of the hindered amine light stabilizer and the ultraviolet absorber were variously changed within the ranges of 2.0 parts by mass or more and 15.0 parts by mass or less, and the ratio of the ultraviolet absorber was variously changed within the ranges of 5.0 parts by mass or more and 30.0 parts by mass or less. Exterior window films were produced in the same manner as above, and evaluations were performed in the same manner as above, and the same results as above were obtained.

[0278] In addition, window films for exterior application were produced in the same manner as above, except that the mixing ratio of the ultraviolet absorber (UV-24) having a benzophenone structure to the ultraviolet absorber (Tinuvin 477) having a hydroxyphenyltriazine structure in the hard coat layer was variously changed within the range of 1.0:2.0 or more and 2.0:1.0 or less in mass ratio, and the same results were obtained as above when the same evaluations were performed.

[0279] In addition, window films for exterior application were produced in the same manner as above, except that the thickness of the hard coat layer was changed in various ways within the range of 0.1 μm or more and 20 μm or less, and the same evaluations as above were carried out, and the same results as above were obtained.

[0280] According to the present invention, it is possible to provide an exterior window film having a hard coat layer, which has excellent weather resistance and improves adhesion between the substrate and the hard coat layer while ensuring transparency and preventing cracks from occurring in the hard coat layer when wound into a roll. Therefore, the present invention has industrial applicability.

[0281] 1: Window film for exterior application 2: Substrate 3: Hard coat layer 4: Anchor coat layer 5: Pressure-sensitive adhesive layer 10: Release liner

Claims

1. A window film for exterior application comprising a substrate made of a material containing polyethylene terephthalate, a hard coat layer provided on one side of the substrate, an anchor coat layer provided between the substrate and the hard coat layer, and an adhesive layer provided on the side of the substrate opposite the side on which the hard coat layer is provided, wherein the hard coat layer is made of a material containing a (meth)acrylate resin having urethane (meth)acrylate as a constituent component, a hindered amine light stabilizer, and a first ultraviolet absorber, wherein the ratio of the hindered amine light stabilizer is 2.0 parts by mass or more and 15.0 parts by mass or less and the ratio of the first ultraviolet absorber is 5.0 parts by mass or more and 30.0 parts by mass or less relative to 100.0 parts by mass of the (meth)acrylate resin, and the anchor coat layer is made of a material containing a thermosetting acrylic resin.

2. A window film for exterior application as described in claim 1, which contains as the first ultraviolet absorbing agent a compound having a benzophenone structure and a compound having a hydroxyphenyltriazine structure.

3. A window film for exterior application as described in claim 2, wherein the ratio of the content of the compound having the benzophenone structure to the content of the compound having the hydroxyphenyltriazine structure in the hard coat layer is, in mass ratio, 1.0:2.0 or more and 2.0:1.0 or less.

4. A window film for exterior application as described in claim 1 or 2, wherein the anchor coat layer contains a second ultraviolet absorber.

5. The window film for exterior application according to claim 4, wherein the second ultraviolet absorbing agent contains a compound having a hydroxyphenyltriazine structure.

6. The window film for exterior application according to claim 1 or 2, wherein the (meth)acrylate resin is formed by polymerizing the urethane (meth)acrylate using a photopolymerization initiator.

7. The window film for exterior application according to claim 6, wherein the photopolymerization initiator is a triphenylphosphine oxide compound.

8. The window film for exterior application according to claim 1 or 2, wherein the thickness of the hard coat layer is from 0.1 μm to 20 μm.

Citation Information

Patent Citations

  • Laminate

    JP2012081742A

  • Method for manufacturing light control film

    JP2014137575A

  • Laminate

    JP2017165015A

  • Active energy ray-curable resin composition, hard-coated laminated film, and film for attaching to glass exterior

    JP2022174046A