Method for recovering valuable metals

The method addresses inefficiencies in cobalt and nickel recovery by using cementation and controlled ion exchange to selectively recover these metals from impure solutions, achieving efficient and cost-effective separation and reducing equipment costs.

WO2024241866A1PCT designated stage expired Publication Date: 2024-11-28MITSUBISHI MATERIALS CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016971
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-07
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing methods for recovering cobalt and nickel from solutions containing impurities like iron, copper, and zinc are inefficient, leading to high processing costs and equipment costs due to issues such as co-precipitation, low concentration problems, and the need for multi-stage processing in solvent extraction and ion exchange methods.

Method used

A method involving cementation to precipitate copper and iron ions, followed by pH adjustment, ion exchange using resins with specific groups, and controlled sulfuric acid elution to selectively recover cobalt and nickel, reducing impurity adsorption and enabling efficient separation and recovery without the need for solvent extraction.

Benefits of technology

This method allows for stable and efficient recovery of cobalt and nickel with reduced costs by suppressing impurity adsorption, achieving high purity concentrates and enabling reuse of sulfuric acid, thus lowering overall processing expenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016971_28112024_PF_FP_ABST
    Figure JP2024016971_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A method for recovering valuable metals according to the present invention comprises: a cementation step S01 for adding a metal less noble than copper to a raw solution containing at least one of cobalt and nickel; a pH adjustment step S02 for adjusting the pH of the raw solution to a predetermined range; a first ion exchange step S04 for bringing the raw solution into contact with a first ion exchange resin; a water cleaning step S05 for cleaning the first ion exchange resin with water; a first elution step S06 for bringing the first ion exchange resin into contact with a low-concentration sulfuric acid; and a second elution step S07 for bringing the first ion exchange resin into contact with high-concentration sulfuric acid. When recovering cobalt, an iron removal step S61, a second ion exchange step S62, and a cobalt concentrate recovery step S63 are performed, and when recovering nickel, a nickel concentrate recovery step S71 is performed.
Need to check novelty before this filing date? Find Prior Art

Description

Valuable metal recovery methods

[0001] The present invention relates to a method for recovering valuable metals comprising at least one of cobalt and nickel from a raw solution containing at least one of cobalt and nickel. This application claims priority to Japanese Patent Application No. 2023-085758, filed on May 24, 2023, the contents of which are incorporated herein by reference.

[0002] Valuable metals such as cobalt and nickel are contained in nickel laterite ore leachate, copper raffinate obtained after copper extraction from copper ore leachate, and wastewater generated during the treatment of waste batteries, etc. These leachates, copper raffinate, and wastewater contain impurities such as iron, copper, and zinc in addition to cobalt and nickel. Methods for recovering cobalt and nickel from the above-mentioned leachates and wastewater include a stepwise neutralization method utilizing the difference in solubility products of hydroxides of various metals, a solvent extraction method, and an ion exchange method.

[0003] Patent Document 1 describes a method for obtaining high-purity cobalt salt crystals by utilizing the difference in solubility product of metal hydroxides in a leachate containing cobalt and the like obtained by acid leaching of used lithium-ion batteries, removing impurities through multistage neutralization, recovering cobalt, and further redissolving the precipitate and repeating the multistage neutralization.

[0004] Patent Document 2 describes a method for recovering a metal-containing solution obtained by wet-treating lithium-ion battery waste, in which the solution contains at least one metal ion selected from cobalt ions and nickel ions, and magnesium ions, by using a solvent containing a carboxylic acid extractant in the solution to extract the cobalt ions or nickel ions into the solvent while leaving the magnesium ions in the solution, and then recovering the cobalt ions or nickel ions by back-extraction from the solvent.

[0005] Patent Document 3 describes a method for recovering cobalt and nickel by leaching copper ore and extracting copper ions with a solvent, followed by pretreatment of pH adjustment and iron (III) ion reduction of the copper raffinate solution, and then ion-exchanging the copper with cobalt and nickel, followed by elution with sulfuric acid.

[0006] Patent Document 4 describes a method for separating and recovering nickel and cobalt by solvent extraction from an eluate containing nickel and cobalt obtained by ion exchange.

[0007] Japanese Patent Application Laid-Open No. 2021-139030 Japanese Patent Application Laid-Open No. 2021-172856 International Publication No. 2011 / 100442 Special Publication No. 2008-527164

[0008] However, in the stepwise neutralization method disclosed in Patent Document 1, when a solution contains high concentrations of iron or aluminum as well as cobalt and nickel, the impurities iron and aluminum precipitate (co-precipitate) together with the cobalt and nickel, and therefore cobalt and nickel cannot be selectively precipitated and recovered.

[0009] In the solvent extraction method described in Patent Document 2, when the cobalt-nickel concentration in the solution is low, there is a problem that the solvent loss per recovered amount of cobalt-nickel increases, resulting in an increase in processing costs. Furthermore, when solvent extraction is carried out industrially, a mixer-settler apparatus capable of continuous processing is used, and since solvent extraction of cobalt-nickel requires multistage processing, the apparatus becomes large, which causes problems such as an increase in equipment costs.

[0010] In Patent Document 3, a copper raffinate solution containing various impurities is subjected to appropriate pretreatment, and then cobalt and nickel are adsorbed onto an ion exchange resin. The adsorption resin is eluted with low-concentration sulfuric acid to elute cobalt, and then with high-concentration sulfuric acid to elute nickel. However, this method involves the contamination of nickel, zinc, and iron with cobalt during elution with low-concentration sulfuric acid. Solvent extraction is required to separate these impurities, which, like Patent Document 2, presents challenges such as increased processing costs and increased equipment costs.

[0011] In Patent Document 4, nickel and cobalt are separated and purified from an eluate containing nickel and cobalt obtained by ion exchange, but the method used here is also solvent extraction, which, like Patent Document 2, has problems such as increased processing costs and increased equipment costs.

[0012] As described above, the ion exchange method is suitable as a method for recovering cobalt and nickel from a low-concentration cobalt-nickel-containing solution containing many impurities, but the cobalt-nickel eluate obtained by the ion exchange method has low purity and therefore requires repurification, as described in Patent Document 3 and Patent Document 4. Solvent extraction is used as a repurification method, but as described above, solvent extraction has many problems, particularly when the cobalt and nickel concentrations in the solution are low, and therefore a method for recovering cobalt and nickel without using solvent extraction is desired.

[0013] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a method for recovering valuable metals that can efficiently and stably recover valuable metals consisting of cobalt and nickel from a raw solution that contains impurities such as iron, copper, and zinc in addition to cobalt and nickel.

[0014] In order to solve the above-mentioned problems, a method for recovering valuable metals according to a first aspect of the present invention is a method for recovering valuable metals comprising at least one of cobalt and nickel from a raw solution containing at least one of cobalt and nickel, the method comprising the steps of: a cementation step of adding a metal less noble than copper to the raw solution to precipitate copper ions contained in the raw solution as metallic copper and reducing iron (III) ions contained in the raw solution to iron (II) ions; a pH adjustment step of adjusting the pH of the raw solution after the cementation step to within a range of 1.5 to 5.0; a first ion exchange step of contacting the raw solution after the pH adjustment with a first ion exchange resin having a bispicolylamine group to adsorb at least one of cobalt and nickel in the raw solution onto the first ion exchange resin; a water washing step of washing the first ion exchange resin with water; and % or more and 4.0 vol% or less to elute cobalt from the first ion exchange resin, thereby obtaining a first eluate containing cobalt; and, after the first elution step, a second elution step, after the first elution step, to contact the first ion exchange resin with sulfuric acid having a concentration of 5.0 vol% or more and 50.0 vol% or less to elute nickel from the first ion exchange resin, thereby obtaining a second eluate containing nickel. When recovering cobalt, the process comprises an iron removal step of removing iron ions from the first eluate, a second ion exchange step of contacting the first eluate from which iron has been removed with a second ion exchange resin to adsorb and remove zinc in the first eluate, and a cobalt concentrate recovery step of obtaining a cobalt concentrate from the first eluate from which zinc has been removed. When recovering nickel, the process comprises a nickel concentrate recovery step of obtaining a nickel concentrate from the second eluate.

[0015] According to the method for recovering valuable metals of the present invention, copper ions and iron(III) ions are removed from the raw solution by a cementation step, and the pH is adjusted. The raw solution is then contacted with a first ion exchange resin having bispicolylamine groups to adsorb at least one of cobalt and nickel from the raw solution onto the first ion exchange resin. This prevents copper ions and iron(III) ions from adsorbing onto the first ion exchange resin, allowing at least one of cobalt and nickel to be efficiently adsorbed onto the first ion exchange resin. Furthermore, the pH of the raw solution is adjusted to a range of 1.5 to 5.0 inclusive in the pH adjustment step, preventing cobalt and nickel from precipitating as hydroxides with impurities and allowing the first ion exchange resin to efficiently adsorb cobalt and nickel.

[0016] The method further includes a first elution step of contacting a first ion exchange resin having at least one of cobalt and nickel adsorbed thereon with sulfuric acid having a concentration of 0.5 vol% or more and 4.0 vol% or less to obtain a first eluate containing cobalt, and a second elution step of contacting the first ion exchange resin with sulfuric acid having a concentration of 5.0 vol% or more and 50.0 vol% or less after the first elution step to elute nickel from the first ion exchange resin to obtain a second eluate containing nickel, thereby making it possible to obtain a first eluate containing mainly cobalt and a second eluate containing mainly nickel.

[0017] When recovering cobalt, an iron removal step of removing iron ions from the first eluate, a second ion exchange step of contacting the iron-removed first eluate with a second ion exchange resin to adsorb and remove zinc from the first eluate, and a cobalt concentrate recovery step of obtaining a cobalt concentrate from the zinc-removed first eluate are performed, and when recovering nickel, a nickel concentrate recovery step of obtaining a nickel concentrate from the second eluate are performed. Therefore, cobalt and nickel can be recovered efficiently without using a solvent extraction method. This makes it possible to recover cobalt and nickel at a lower cost than with a solvent extraction method.

[0018] Furthermore, by carrying out the second elution step, the metal adsorbed on the first ion exchange resin can be removed and regenerated, and the first ion exchange step can be carried out again using the used first ion exchange resin. Furthermore, the entire process, including the first elution step and the second elution step, can be performed using a sulfuric acid system, making it easy to treat the wastewater. Furthermore, in the case of a copper raffinate solution obtained after copper extraction from a copper ore leachate, the sulfuric acid-based wastewater can be reused for copper ore leaching, making wastewater treatment unnecessary.

[0019] A valuable metal recovery method according to Aspect 2 of the present invention is the valuable metal recovery method according to Aspect 1, characterized in that in the iron removal step, an oxidizing agent is added to the first eluent to oxidize iron (II) ions to iron (III) ions, the pH is adjusted to 3.0 or more and 5.0 or less using a base, the iron (III) ions are precipitated as iron hydroxide, and solid-liquid separation is performed. According to the valuable metal recovery method according to Aspect 2 of the present invention, an oxidizing agent is added to the first eluent to oxidize iron (II) ions to iron (III) ions, the pH is adjusted to 3.0 or more and 5.0 or less using a base, the iron (III) ions are precipitated as iron hydroxide, and solid-liquid separation is performed. Therefore, iron contained in the first eluent can be efficiently removed, and the amount of iron contained in the cobalt concentrate can be sufficiently reduced.

[0020] A method for recovering valuable metals according to Aspect 3 of the present invention is characterized in that, in the method for recovering valuable metals according to Aspect 1 or Aspect 2, the second ion exchange resin contains at least one of a phosphate group and a phosphonic acid group. According to the method for recovering valuable metals according to Aspect 3 of the present invention, the second ion exchange resin contains at least one of a phosphate group and a phosphonic acid group, so that zinc contained in the first eluate can be efficiently adsorbed onto the second ion exchange resin, and the amount of zinc contained in the cobalt concentrate can be sufficiently reduced.

[0021] A method for recovering valuable metals according to Aspect 4 of the present invention is the method for recovering valuable metals according to any one of Aspects 1 to 3, characterized in that in the cobalt concentrate recovery step, a base is added to the first eluate to adjust the pH to 9.0 or more and 13.0 or less. According to the method for recovering valuable metals according to Aspect 4 of the present invention, a base is added to the first eluate from which iron and zinc have been removed to adjust the pH to 9.0 or more and 13.0 or less, so that a cobalt concentrate can be efficiently recovered from the first eluate.

[0022] A method for recovering valuable metals according to Aspect 5 of the present invention is the method for recovering valuable metals according to any one of Aspects 1 to 3, characterized in that the cobalt in the first eluate is sulfurized in the cobalt concentrate recovery step. According to the method for recovering valuable metals according to Aspect 5 of the present invention, the cobalt in the first eluate from which iron and zinc have been removed is sulfurized, so that the cobalt concentrate can be efficiently recovered from the first eluate.

[0023] A method for recovering valuable metals according to Aspect 6 of the present invention is the method for recovering valuable metals according to any one of Aspects 1 to 5, characterized in that in the nickel concentrate recovery step, a base is added to the second eluent to adjust the pH to 9.0 or more and 13.0 or less. According to the method for recovering valuable metals according to Aspect 6 of the present invention, a base is added to the second eluent to adjust the pH to 9.0 or more and 13.0 or less, so that the nickel concentrate can be efficiently recovered from the second eluent.

[0024] A method for recovering valuable metals according to Aspect 7 of the present invention is the method for recovering valuable metals according to any one of Aspects 1 to 5, characterized in that in the nickel concentrate recovery step, the nickel in the second eluate is sulfurized. According to the method for recovering valuable metals according to Aspect 7 of the present invention, the nickel in the second eluate is sulfurized, so that the nickel concentrate can be efficiently recovered from the second eluate.

[0025] According to the present invention, it is possible to provide a method for recovering valuable metals that can efficiently and stably recover valuable metals such as cobalt and nickel from a raw solution that contains impurities such as iron, copper, and zinc in addition to cobalt and nickel.

[0026] 1 is a flow chart showing a method for recovering valuable metals according to an embodiment of the present invention. 2 is a graph showing the relationship between sulfuric acid concentration and the elution rate of cobalt and nickel in an example.

[0027] An example of an embodiment of the present invention will be described below.

[0028] The method for recovering valuable metals of this embodiment recovers valuable metals consisting of at least one of cobalt and nickel from a raw solution containing at least one of cobalt and nickel, such as a nickel laterite ore leachate, a copper raffinate solution obtained after copper is extracted from a copper ore leachate, or wastewater generated during the treatment of waste batteries, etc. In this embodiment, the raw solution is the copper raffinate solution obtained after copper is extracted from a copper ore leachate, and this raw solution contains cobalt and nickel.

[0029] Here, the valuable metal recovery method of this embodiment will be described using the flow diagram of Figure 1. As shown in Figure 1, the valuable metal recovery method of this embodiment includes a cementation step S01, a pH adjustment step S02, a solid-liquid separation step S03, a first ion exchange step S04, a water washing step S05, a first elution step S06, and a second elution step S07. When cobalt is recovered, an iron removal step S61, a second ion exchange step S62, and a cobalt concentrate recovery step S63 are performed. When nickel is recovered, a nickel concentrate recovery step S71 is performed.

[0030] (Cementation step S01) First, a metal less noble than copper is added to a raw solution containing cobalt and nickel, thereby precipitating copper ions contained in the raw solution as metallic copper and reducing iron (III) ions contained in the raw solution to iron (II) ions. Examples of the metal less noble than copper to be added include iron and aluminum. When iron is added as a metal less noble than copper, the amount of iron added is preferably in the range of 4 g / L to 230 g / L, and when aluminum is added as a metal less noble than copper, the amount of aluminum added is preferably in the range of 2 g / L to 110 g / L.

[0031] (pH Adjustment Step 02) The pH of the raw solution obtained by the cementation step S01 is adjusted to a range of 1.5 to 5.0 using an acid or a base. If the pH of the raw solution exceeds 5.0, cobalt and nickel may precipitate together with impurities. If the pH of the raw solution is less than 1.5, the cobalt and nickel may not be efficiently adsorbed onto the first ion exchange resin in the first ion exchange step S04, which will be described later. Therefore, in this embodiment, the pH of the raw solution is adjusted to a range of 1.5 to 5.0. The pH of the raw solution is preferably 1.5 or higher, and more preferably 2.5 or higher. The pH of the raw solution is preferably 5.0 or lower, and more preferably 3.5 or lower. Examples of acids that can be used include sulfuric acid and nitric acid. Examples of bases that can be used include caustic soda, calcium hydroxide, and magnesium hydroxide.

[0032] (Solid-liquid separation step S03) The pH-adjusted raw solution is subjected to solid-liquid separation. There are no particular limitations on the means of solid-liquid separation, but in this embodiment, suction filtration is performed. In this solid-liquid separation step S03, solids such as precipitates generated in the cementation step S01 and the pH adjustment step S02 are removed from the raw solution.

[0033] (First ion exchange step S04) Next, the raw solution from which the pH has been adjusted and the solid phase has been separated is brought into contact with a first ion exchange resin having bispicolylamine groups, and the cobalt and nickel in the raw solution are adsorbed onto the first ion exchange resin. Here, since the copper ions and iron (III) ions contained in the raw solution have been removed in the cementation step S01, adsorption of the copper ions and iron (III) ions onto the first ion exchange resin can be suppressed in this first ion exchange step S04, and cobalt and nickel can be efficiently adsorbed.

[0034] (Water Washing Step S05) Next, the first ion exchange resin that has adsorbed the cobalt and nickel in the raw solution is washed with pure water to remove impurities such as manganese, aluminum, magnesium, and calcium from the first ion exchange resin.

[0035] (First Elution Step S06) Next, the first ion exchange resin washed with pure water is contacted with sulfuric acid having a concentration of 0.5 vol% to 4.0 vol% to elute cobalt from the first ion exchange resin, thereby obtaining a first eluate containing cobalt. Note that this first eluate will contain impurities other than cobalt, primarily nickel, iron, and zinc. If the sulfuric acid concentration is less than 0.5 vol%, cobalt may not be sufficiently eluted from the first ion exchange resin. On the other hand, if the sulfuric acid concentration exceeds 4.0 vol%, a large amount of nickel may be eluted along with cobalt. For this reason, in this embodiment, the concentration of sulfuric acid used in the first elution step S06 is set to a range of 0.5 vol% to 4.0 vol%. Note that the concentration of sulfuric acid used in the first elution step S06 is preferably 0.5 vol% or higher, and more preferably 1.0 vol% or higher. Furthermore, the concentration of sulfuric acid used in the first elution step S06 is preferably 4.0 vol% or less, and more preferably 2.0 vol% or less. It is also possible that the raw solution contains nickel but not cobalt, or that the raw solution contains nickel and cobalt, but only nickel is to be recovered. In these cases, the first elution step S06 does not need to be performed, or, even if the first elution step S06 is performed, the sulfuric acid concentration may be greater than 4.0 vol%.

[0036] (Second Elution Step S07) Next, after the first elution step S06, the first ion exchange resin is contacted with sulfuric acid having a concentration of 5.0 vol% to 50.0 vol% to elute nickel from the first ion exchange resin, thereby obtaining a second eluate containing nickel. Furthermore, this second elution step S07 regenerates the first ion exchange resin, making it usable again in the first ion exchange step S04. Here, if the sulfuric acid concentration is less than 5.0 vol%, it may be difficult to elute nickel from the first ion exchange resin, and the first ion exchange resin may not be regenerated. On the other hand, if the sulfuric acid concentration exceeds 50.0 vol%, the first ion exchange resin may react with sulfuric acid, making it impossible to reuse the first ion exchange resin. For this reason, in this embodiment, the concentration of sulfuric acid used in the second elution step S07 is set to a range of 5.0 vol% to 50.0 vol%. The concentration of sulfuric acid used in the second elution step S07 is preferably 5.0 vol% or more, and more preferably 10.0 vol% or more. The concentration of sulfuric acid used in the second elution step S07 is preferably 50.0 vol% or less, and more preferably 20.0 vol% or less. It is also possible that the raw solution contains cobalt but not nickel, or that the raw solution contains nickel and cobalt, but only cobalt is to be recovered. In these cases, the second elution step S07 does not need to be performed.

[0037] When cobalt is recovered from the first eluate obtained in the first elution step S06, the following iron removal step S61, second ion exchange step S62, and cobalt concentrate recovery step S63 are carried out.

[0038] (Iron Removal Step S61) In this iron removal step S61, an oxidizing agent is added to the first eluent to oxidize iron (II) ions to iron (III) ions, and a base is used to adjust the pH to 3.0 or higher and 5.0 or lower, thereby precipitating the iron (III) ions as iron hydroxide, followed by solid-liquid separation. By adjusting the pH to 3.0 or higher, the solubility of iron (III) ions is reduced, allowing them to precipitate as iron hydroxide. On the other hand, by adjusting the pH to 5.0 or lower, the precipitation of cobalt and nickel can be suppressed. Examples of the oxidizing agent that can be used include hydrogen peroxide and blown air. Examples of the base that can be used include caustic soda, calcium hydroxide, and magnesium hydroxide.

[0039] (Second ion exchange step S62) Next, the first eluate from which iron has been removed is brought into contact with a second ion exchange resin, and zinc in the first eluate is removed by being adsorbed onto the second ion exchange resin. When bringing the first eluate into contact with the second ion exchange resin, it is preferable to adjust the pH to within a range of 2.0 to 5.0. Here, in this embodiment, it is preferable to use a resin containing at least one of a phosphate group and a phosphonate group as the second ion exchange resin, and specifically, it is preferable to use a resin having an aminomethylphosphonic acid group, a bis-(2,4,4-trimethylpentyl)phosphonic acid group, or a di-(2-ethylhexyl)phosphate group.

[0040] (Cobalt concentrate recovery step S63) Next, a cobalt concentrate is recovered from the first eluate from which zinc has been removed in the second ion exchange step S62. Here, in the cobalt concentrate recovery step S63, a base is added to the first eluate from which iron and zinc have been removed to adjust the pH to 9.0 or more and 13.0 or less, thereby precipitating cobalt, thereby obtaining a cobalt concentrate. Alternatively, the cobalt concentrate can be obtained by sulfiding the cobalt in the first eluate. When sulfiding cobalt, it is preferable to adjust the pH of the first eluate to 3.0 or more and 9.0 or less, and add a sulfiding agent (e.g., sodium sulfide, sodium hydrosulfide, hydrogen sulfide, etc.).

[0041] When nickel is recovered from the second eluate obtained in the second elution step S07, a nickel concentrate recovery step S71 is carried out.

[0042] (Nickel concentrate recovery step S71) A nickel concentrate is recovered from the second eluate obtained in the second elution step S07. Here, in the nickel concentrate recovery step S71, a base is added to the second eluate to adjust the pH to 9.0 or more and 13.0 or less, thereby precipitating nickel, thereby obtaining a nickel concentrate. Alternatively, the nickel concentrate can be obtained by sulfiding the nickel in the second eluate. When sulfiding nickel, it is preferable to adjust the pH of the second eluate to 3.0 or more and 9.0 or less, and add a sulfiding agent (e.g., sodium sulfide, sodium hydrosulfide, hydrogen sulfide, etc.).

[0043] The above-described process makes it possible to efficiently and stably recover valuable metals such as cobalt and nickel from a raw solution containing impurities such as iron, copper, and zinc in addition to cobalt and nickel.

[0044] According to the valuable metal recovery method of this embodiment configured as described above, the cementation step S01, the pH adjustment step S02, and the solid-liquid separation step S03 are performed, and then the first ion exchange step S04 is carried out. Therefore, in this first ion exchange step S04, it is possible to suppress adsorption of copper ions and iron (III) ions onto the first ion exchange resin, and it is possible to efficiently adsorb cobalt and nickel onto the first ion exchange resin.

[0045] The method further includes a first elution step of contacting a first ion exchange resin having at least one of cobalt and nickel adsorbed thereon with sulfuric acid having a concentration of 0.5 vol% or more and 4.0 vol% or less to obtain a first eluate containing cobalt, and a second elution step of contacting the first ion exchange resin with sulfuric acid having a concentration of 5.0 vol% or more and 50.0 vol% or less after the first elution step to elute nickel from the first ion exchange resin to obtain a second eluate containing nickel, thereby making it possible to obtain a first eluate containing mainly cobalt and a second eluate containing mainly nickel.

[0046] When recovering cobalt, an iron removal step of removing iron ions from the first eluate, a second ion exchange step of contacting the iron-removed first eluate with a second ion exchange resin to adsorb and remove zinc from the first eluate, and a cobalt concentrate recovery step of obtaining a cobalt concentrate from the zinc-removed first eluate are performed, and when recovering nickel, a nickel concentrate recovery step of obtaining a nickel concentrate from the second eluate are performed. Therefore, cobalt and nickel can be recovered efficiently without using a solvent extraction method. This makes it possible to recover cobalt and nickel at a lower cost than with a solvent extraction method.

[0047] Furthermore, by carrying out the second elution step, the metal adsorbed on the first ion exchange resin can be removed and regenerated, and the first ion exchange step can be carried out again using the used first ion exchange resin. Furthermore, all processes, including the first elution step and the second elution step, can be configured using a sulfuric acid system, making it easy to treat the effluent. Furthermore, since this embodiment targets the copper raffinate solution obtained after copper is extracted from the copper ore leachate, the sulfuric acid-based effluent can be reused for copper ore leaching, eliminating the need for effluent treatment.

[0048] In this embodiment, when the iron removal step S61 is configured to add an oxidizing agent to the first eluate to oxidize iron (II) ions to iron (III) ions, and then adjust the pH to 3.0 or more and 5.0 or less using a base to precipitate the iron (III) ions as iron hydroxide, followed by solid-liquid separation, the iron contained in the first eluate can be efficiently removed, and a cobalt concentrate with a sufficiently reduced iron content can be recovered from the first eluate.

[0049] In this embodiment, when the second ion exchange resin used in the second ion exchange step S62 contains at least one of a phosphate group and a phosphonate group, the zinc contained in the first eluate can be efficiently adsorbed onto the second ion exchange resin, and it becomes possible to recover a cobalt concentrate with a sufficiently reduced amount of zinc from the first eluate.

[0050] In this embodiment, when the cobalt concentrate recovery step S63 is configured to add a base to the first eluate from which iron and zinc have been removed to adjust the pH to 9.0 or more and 13.0 or less, the cobalt contained in the first eluate can be precipitated, and the cobalt concentrate can be efficiently recovered from the first eluate.

[0051] In this embodiment, when the cobalt concentrate recovery step S63 is configured to sulfide the cobalt in the first eluate from which iron and zinc have been removed, the cobalt contained in the first eluate is converted into sulfide, and the cobalt concentrate can be efficiently recovered from the first eluate.

[0052] In this embodiment, when the nickel concentrate recovery step S71 is configured to add a base to the second eluate to adjust the pH to 9.0 or more and 13.0 or less, the nickel contained in the second eluate can be precipitated, and the nickel concentrate can be efficiently recovered from the second eluate.

[0053] In this embodiment, when the nickel concentrate recovery step S71 is configured to sulfide the nickel in the second eluate, the nickel contained in the second eluate is converted into sulfide, and the nickel concentrate can be efficiently recovered from the second eluate.

[0054] Although the embodiment of the present invention has been described above, the present invention is not limited to this and can be modified as appropriate within the scope of the technical idea of ​​the invention.

[0055] The results of confirmation experiments conducted to confirm the effectiveness of the present invention will be described below.

[0056] Example 1: 1.4 g of iron powder, a metal less noble than copper, was added to 700 mL of copper raffinate obtained after copper extraction from a copper ore leachate, and the mixture was allowed to diffuse for 2.5 hours to allow the cementation reaction to proceed. The composition of the solution before and after cementation was measured by ICP-AES. The measurement results are shown in Table 1.

[0057]

[0058] It was confirmed that the concentrations of copper ions and iron (III) ions were reduced by cementation.

[0059] Next, 80 mL of 5 vol% calcium hydroxide slurry was added to the cemented solution to adjust the pH of the solution from 1.2 to 2.6. The solution was then subjected to suction filtration as a solid-liquid separation step. The solid content (precipitate) obtained here was a mixture of copper precipitated by cementation and calcium sulfate precipitated during the pH adjustment.

[0060] 600 mL of the solution obtained after solid-liquid separation was passed through a column packed with 10 mL of ion exchange resin containing bispicolylamine groups, and cobalt and nickel were adsorbed onto the ion exchange resin. After adsorption, 90 mL of pure water was passed through the column to wash the column and remove impurities. Next, in the first elution step, 120 mL of 1 vol% sulfuric acid was passed through to obtain a first eluate. Then, 120 mL of 20% sulfuric acid was passed through to obtain a second eluate. The liquid compositions of the pure water rinse, the first eluate, and the second eluate were measured by ICP-AES. The iron(II) ion concentration was measured using the 1,10-phenanthroline absorptiometry method specified in JIS K 0400-57-10. The measurement results are shown in Table 2.

[0061]

[0062] The washing solution contains large amounts of impurities such as iron, manganese, aluminum, magnesium, and calcium, and it is confirmed that the impurities can be sufficiently removed by washing with water. The first eluate contains mainly cobalt, and also contains nickel, zinc, and iron as impurities. The second eluate contains mainly nickel, and it is confirmed that it contains almost no impurities.

[0063] Next, 0.45 μL of hydrogen peroxide was added to 300 mL of a simulated solution with the same composition as the first eluent to oxidize iron(II) ions to iron(III) ions. Subsequently, 7.7 mL of 4 M caustic soda was added to neutralize the solution to pH 4, precipitating iron(III) ions as hydroxide. This precipitate was subjected to suction filtration for solid-liquid separation, and iron was removed. 200 mL of the iron-removed solution was passed through 10 mL of ion exchange resin containing bis-(2,4,4-trimethylpentyl)phosphonic acid groups to adsorb zinc. 0.8 mL of 4 M caustic soda was added to 100 mL of this zinc-removed solution to neutralize it to pH 10, precipitating cobalt as hydroxide, and suction filtration was used to recover a cobalt concentrate. The compositions of each solution are shown in Table 3. The composition of the resulting cobalt concentrate is shown in Table 4.

[0064]

[0065]

[0066] It was confirmed that the impurity Fe was removed by the iron removal process. It was also confirmed that the impurity zinc was removed by ion exchange using an ion exchange resin having bis-(2,4,4-trimethylpentyl)phosphonic acid groups. The cobalt concentration in the post-cobalt recovery solution was very low, confirming that cobalt was efficiently recovered. The cobalt concentrate contained mainly cobalt, with traces of nickel. It contained almost no impurities such as iron or aluminum.

[0067] Next, 98 mL of 4 M caustic soda was added to 100 mL of the second eluate to neutralize it to pH 11, and nickel was precipitated as hydroxide, followed by suction filtration to recover a nickel concentrate. The composition of the obtained nickel concentrate is shown in Table 5.

[0068]

[0069] The nickel concentrate mainly contained nickel, with almost no impurities such as iron or aluminum.

[0070] From the above results, it was confirmed that cobalt and nickel can be recovered by the method for recovering valuable metals of the present invention.

[0071] Example 2 In Example 2, a method for recovering a cobalt concentrate from a post-zinc removal solution by sulfurization was evaluated. A solution simulating the post-zinc removal solution obtained in Example 1 above was prepared. 2 mL of a 2 M sodium sulfide solution was added to 200 mL of this solution to precipitate cobalt as sulfide, and the cobalt concentrate was recovered by suction filtration. The compositions of the post-zinc removal solution and the post-sulfurization solution are shown in Table 6. The composition of the obtained cobalt concentrate is shown in Table 7.

[0072]

[0073]

[0074] The cobalt concentration in the post-sulfurization liquid was very low, confirming that cobalt was efficiently recovered by sulfurization. The cobalt concentrate contained mainly cobalt, with traces of nickel. It contained almost no impurities such as iron or aluminum.

[0075] Example 3 In Example 3, the effects of the cementation step and the pH adjustment step were confirmed. Test (1): 5 mL of an ion exchange resin having bispicolylamine groups was added to 50 mL of a copper raffinate solution obtained after copper extraction from a copper ore leachate, and the mixture was stirred for 1 hour. Test (2): 0.3 g of iron powder was added to 100 mL of a copper raffinate solution obtained after copper extraction from a copper ore leachate, and the mixture was stirred for 1 hour. The precipitated copper was filtered by suction to separate the solid and liquid. 50 mL of the resulting solution was then sampled, 5 mL of ion exchange resin was added, and the mixture was stirred for 1 hour. Test (3): 4.2 mL of 4 M caustic soda was added to 100 mL of a copper raffinate solution obtained after copper extraction from a copper ore leachate, and the pH was adjusted from 1.2 to 2.5. 50 mL of the resulting solution was then sampled, 5 mL of ion exchange resin was added, and the mixture was stirred for 1 hour. Test (4): 0.3 g of iron powder was added to 100 mL of copper raffinate obtained after copper extraction from copper ore leachate, and the mixture was stirred for 1 hour. The precipitated copper was filtered off with suction, and 3.3 mL of 4 M caustic soda was added to adjust the pH from 1.2 to 2.5. 50 mL of the resulting solution was taken, to which 5 mL of ion exchange resin was added and stirred for 1 hour. The amounts of cobalt, nickel, and copper adsorbed, determined from the compositions of the solutions before and after adsorption obtained in Tests (1) to (4), are shown in Table 8.

[0076]

[0077] Comparing Tests (1) and (2) in Table 8, it can be seen that removing copper in advance by cementation reduces the amount of copper adsorption, while increasing the amounts of cobalt and nickel adsorption. Comparing Tests (1) and (3) in Table 8 reveals that there is a significant difference in the amount of cobalt and nickel adsorption depending on whether or not pH adjustment is performed. Ion exchange resins containing bispicolylamine groups generally adsorb metals more easily at higher pH levels, so a pH adjustment step is necessary when using low-pH solutions. Comparing Tests (1) to (4) in Table 8 reveals that Test (4) showed the highest amount of cobalt and nickel adsorption, demonstrating that the two steps of cementation and pH adjustment maximize the amount of cobalt and nickel adsorption during ion exchange.

[0078] Example 4 In Example 4, the concentration of sulfuric acid used in the first elution step and the second elution step was investigated. 10 mL of an ion exchange resin having bispicolylamine groups was added to 100 mL of a sulfuric acid solution containing 200 ppm of cobalt, and the mixture was stirred for 30 minutes to obtain a resin with cobalt adsorbed thereto. The adsorbed solution was separated from the cobalt-adsorbed resin, and then the adhering solution was removed by washing with water. 50 mL of 0.5-5 vol% sulfuric acid was added to the washed resin, and the mixture was stirred for 30 minutes. The elution rate (elution rate = amount of cobalt eluted / amount of cobalt adsorbed on the resin) was calculated from the concentration of cobalt dissolved in the solution. A similar test was also performed using a sulfuric acid solution containing 200 ppm of nickel, and the nickel elution rate for 1-10 vol% sulfuric acid was calculated.

[0079] The results are summarized in Figure 2. As can be seen from Figure 2, cobalt can be eluted at a sulfuric acid concentration of 0.5 vol% or higher, but when the sulfuric acid concentration is greater than 4 vol%, 50% or more of nickel is also eluted. Therefore, it was confirmed that by using sulfuric acid with a concentration of 0.5 vol% or higher and 4.0 vol% or lower in the first elution step, cobalt can be eluted while suppressing the elution of nickel, and that by using sulfuric acid with a concentration of 5.0 vol% or higher and 50.0 vol% or lower in the second elution step, nickel can be eluted efficiently.

[0080] (Comparative Experiment) In this comparative experiment, the case where cobalt was recovered without performing the iron removal step and zinc removal step on the first eluate was evaluated. 3.5 mL of 4 M caustic soda was added to 100 mL of the first eluate obtained in Example 1 to neutralize the solution to pH 10, precipitate cobalt as hydroxide, and then suction-filter the solution to recover a cobalt concentrate. The composition of the obtained cobalt concentrate is shown in Table 9. When iron removal and zinc removal are not performed, iron and zinc are mixed in during cobalt recovery, resulting in high iron and zinc concentrations in the cobalt concentrate, making it difficult to sell as an intermediate product.

[0081]

[0082] As a result of the above confirmatory experiments, it was confirmed that the present invention can provide a method for recovering valuable metals that can efficiently and stably recover valuable metals consisting of cobalt and nickel from a raw solution that contains impurities such as iron, copper, and zinc in addition to cobalt and nickel.

Claims

1. A method for recovering valuable metals comprising at least one of cobalt and nickel from a raw solution containing at least one of cobalt and nickel, comprising: a cementation step of adding a metal less noble than copper to the raw solution to precipitate copper ions contained in the raw solution as metallic copper and reduce iron (III) ions contained in the raw solution to iron (II) ions; a pH adjustment step of adjusting the pH of the raw solution after the cementation step to within a range of 1.5 to 5.0; a first ion exchange step of contacting the raw solution after the pH adjustment with a first ion exchange resin having a bispicolylamine group to adsorb at least one of cobalt and nickel in the raw solution onto the first ion exchange resin; a water washing step of washing the first ion exchange resin with water; and a first elution step of contacting the first ion exchange resin after the water washing with sulfuric acid having a concentration of 0.5 vol % to 4.0 vol % to elute cobalt from the first ion exchange resin to obtain a first eluate containing cobalt. a second elution step of contacting the first ion exchange resin with sulfuric acid having a concentration of 5.0 vol% or more and 50.0 vol% or less after the first elution step to elute nickel from the first ion exchange resin and obtain a second eluate containing nickel, wherein when recovering cobalt, an iron removal step of removing iron ions from the first eluate, a second ion exchange step of contacting the first eluate from which iron has been removed with a second ion exchange resin to adsorb zinc in the first eluate and remove it, and a cobalt concentrate recovery step of obtaining a cobalt concentrate from the first eluate from which zinc has been removed are carried out, and when recovering nickel, a nickel concentrate recovery step of obtaining a nickel concentrate from the second eluate is carried out.

2. A method for recovering valuable metals as described in claim 1, characterized in that in the iron removal step, an oxidizing agent is added to the first eluent to oxidize iron (II) ions to iron (III) ions, the pH is adjusted to 3.0 or more and 5.0 or less using a base, the iron (III) ions are precipitated as iron hydroxide, and solid-liquid separation is performed.

3. The method for recovering valuable metals according to claim 1 or 2, characterized in that the second ion exchange resin contains at least one of a phosphate group and a phosphonic acid group.

4. A method for recovering valuable metals as described in claim 1 or 2, characterized in that in the cobalt concentrate recovery step, a base is added to the first eluent to adjust the pH to 9.0 or more and 13.0 or less.

5. A method for recovering valuable metals as described in claim 1 or 2, characterized in that in the cobalt concentrate recovery step, the cobalt in the first eluent is sulfurized.

6. A method for recovering valuable metals as described in claim 1 or 2, characterized in that in the nickel concentrate recovery process, a base is added to the second eluent to adjust the pH to 9.0 or more and 13.0 or less.

7. A method for recovering valuable metals as described in claim 1 or claim 2, characterized in that in the nickel concentrate recovery step, the nickel in the second eluent is sulfurized.

Citation Information

Patent Citations

  • Cobalt recovery

    US20110194999A1

  • Method for treating alloy

    WO2021166755A1