Charge-transporting varnish

The charge-transporting varnish, composed of surface-treated metal oxide nanoparticles and a polythiophene derivative, addresses the need for improved hole injection materials by forming thin films with superior charge-transporting properties, specifically a deeper HOMO level, enhancing the performance of organic and quantum dot EL devices.

WO2024241889A1PCT designated stage expired Publication Date: 2024-11-28NISSAN CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017192
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-09
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

There is a need for improved wet process materials for hole injection layers in organic electroluminescent (EL) devices and quantum dot EL devices to enhance charge-transporting properties, particularly hole-injecting properties, to achieve better performance and efficiency.

Method used

A charge-transporting varnish containing metal oxide nanoparticles surface-treated with a specific silane coupling agent and a charge-transporting substance, such as a polythiophene derivative, is used to form a thin film with excellent charge-transporting properties, specifically a deeper highest occupied molecular orbital (HOMO) level, improving hole injection properties.

Benefits of technology

The varnish enables the formation of charge-transporting thin films with enhanced hole-injecting properties, suitable for organic EL and quantum dot EL devices, leading to improved performance and efficiency by modifying the HOMO level and enhancing the hole injection property.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017192_28112024_PF_FP_ABST
    Figure JP2024017192_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a charge-transporting varnish that provides a charge-transporting thin film having excellent hole injection properties, the charge-transporting varnish comprising metal oxide nanoparticles each surface-treated with a silane coupling agent represented by formula (S1), a charge-transporting substance and an organic solvent. (Rv1 to Rv3 each independently represent a hydrogen atom, a chlorine atom, a hydroxy group, an alkoxy group optionally having a substituent, or the like, wherein at least one of Rv1 to Rv3 represents a hydrogen atom, a chlorine atom, a hydroxy group, or an alkoxy group optionally having a substituent; L represents a single bond or an alkylene group having 1 to 10 carbon atoms; and Rv4 represents an alkyl group having 1 to 10 carbon atoms and optionally having at least one substituent selected from a halogen atom and others, an alkoxy group having 1 to 10 carbon atoms and optionally having at least one substituent selected from a halogen atom and others, or the like, wherein when Rv4 is an alkyl group having 1 to 10 carbon atoms and optionally having a substituent, L is a single bond.)
Need to check novelty before this filing date? Find Prior Art

Description

Charge-transporting varnish

[0001] The present invention relates to a charge transporting varnish.

[0002] In organic electroluminescence (hereinafter referred to as organic EL) devices, organic functional films made of organic compounds are used as the light-emitting layer and charge injection layer. In particular, the hole injection layer is responsible for transferring charges between the anode and the hole transport layer or light-emitting layer, and plays an important role in achieving low-voltage operation and high brightness of the organic EL device.

[0003] Methods for forming hole injection layers are roughly divided into dry processes, such as vapor deposition, and wet processes, such as inkjet printing and spin coating. Compared to these processes, wet processes are more efficient at producing thin films with high flatness over large areas. Therefore, as organic EL displays are increasingly being manufactured with larger areas, there is a demand for hole injection layers that can be formed by wet processes. A technology related to hole injection materials that can be formed by wet processes has been reported (Patent Document 1).

[0004] Furthermore, in recent years, with the development of display technology, quantum dot electroluminescence (hereinafter referred to as quantum dot EL) devices, which use quantum dot materials as light-emitting layers, have emerged and are showing promise for a wide range of applications. These quantum dot EL devices can be manufactured at low cost using wet processes, and are attracting much attention in fields such as display technology and lighting due to their characteristics, such as controllability of emission wavelength, high color purity, high luminous efficiency, and flexibility.

[0005] Currently, there is a demand for improved performance of organic EL elements and quantum dot EL elements, and improvements are constantly being sought for wet process materials for hole injection layers. In particular, there is an increasing demand for materials that can provide charge transport thin films with high hole injection properties, as these materials can contribute to improving the performance of organic EL elements and quantum dot EL elements, such as the luminance characteristics.

[0006] International Publication No. 2008 / 032616

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a charge transporting varnish that gives a charge transporting thin film that is excellent in charge transporting properties, particularly hole injection properties.

[0008] As a result of extensive research to solve the above-mentioned problems, the present inventors have discovered that by using a charge-transporting varnish containing metal oxide nanoparticles that have been surface-treated with a silane coupling agent having a specific structure, the highest occupied molecular orbital (HOMO) level of the resulting charge-transporting thin film becomes deeper than that of conventional thin films, and a charge-transporting thin film with excellent charge transport properties can be obtained, thereby completing the present invention.

[0009] That is, the present invention provides the following charge transporting varnish: 1. A charge transporting varnish comprising metal oxide nanoparticles that have been surface-treated with a silane coupling agent represented by the following formula (S1), a charge transporting substance, and an organic solvent. (In the formula, R v1 ~R v3 each independently represents a hydrogen atom, a chlorine atom, a hydroxy group, an alkoxy group which may have a substituent, or an alkyl group which may have a substituent; R v1 ~R v3 at least one of the groups represents a hydrogen atom, a chlorine atom, a hydroxy group, or an alkoxy group which may have a substituent; L represents a single bond or an alkylene group having 1 to 10 carbon atoms; R v4 represents an alkyl group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group; an alkoxy group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group; or an aryl group having 6 to 20 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, a hydroxy group, an alkyl group having 1 to 10 carbon atoms, and an alkoxy group having 1 to 10 carbon atoms. v4 is an alkyl group having 1 to 10 carbon atoms which may have a substituent, L is a single bond.) 2. v1 ~R v33. The charge transporting varnish according to 1, wherein R is an alkyl group having 1 to 10 carbon atoms which may have a substituent or an alkoxy group having 1 to 10 carbon atoms which may have a substituent. v4 is an alkyl group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group; or an alkoxy group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group. 4. The charge transport varnish of any of 1 to 3, wherein the charge transport substance is a polythiophene derivative or an amine adduct thereof, or an arylamine derivative. 5. The charge transport varnish of 4, wherein the charge transport substance is a polythiophene derivative or an amine adduct thereof containing a repeating unit represented by the following formula (1): (In the formula, R 1 and R 2 are each independently a hydrogen atom, an alkyl group having 1 to 40 carbon atoms, a fluoroalkyl group having 1 to 40 carbon atoms, an alkoxy group having 1 to 40 carbon atoms, a fluoroalkoxy group having 1 to 40 carbon atoms, an aryloxy group having 6 to 20 carbon atoms, -O-[Z-O] p -R e or a sulfonic acid group, or R 1 and R 2 are bonded to each other, Y is an alkylene group having 1 to 40 carbon atoms which may contain an ether bond and which may be substituted with a sulfonic acid group, Z is an alkylene group having 1 to 40 carbon atoms which may be substituted with a halogen atom, p is an integer of 1 or more, and R e is a hydrogen atom, an alkyl group having 1 to 40 carbon atoms, a fluoroalkyl group having 1 to 40 carbon atoms, or an aryl group having 6 to 20 carbon atoms.) 6. 1 is a sulfonic acid group, and the R 2 is an alkoxy group having 1 to 40 carbon atoms or —O—[Z—O] p -R e or the above R 1 and R 2The charge transport varnish of 5, wherein the bond is -O-Y-O-. 7. The charge transport varnish of any one of 1 to 6, further comprising a dopant substance. 8. The charge transport varnish of 7, wherein the dopant substance comprises at least one selected from the group consisting of arylsulfonic acid compounds and heteropolyacid compounds. 9. The charge transport varnish of any one of 1 to 8, wherein the metal oxide nanoparticles are at least one selected from the group consisting of SiO2, TiO2, and ZrO2. 10. The charge transport varnish of 9, wherein the metal oxide nanoparticles are SiO2. 11. The charge transport varnish of any one of 1 to 10, further comprising one or more amine compounds. 12. The charge transport varnish of 11, wherein the amine compound comprises a tertiary alkylamine compound and an amine compound other than a tertiary alkylamine compound. 13. The charge transport varnish of 12, wherein the amine compound other than a tertiary alkylamine compound is a primary alkylamine compound. 14. A charge transport thin film obtained from the charge transport varnish of any one of 1 to 13. 15. An electronic device comprising the charge transport thin film of 14. 16. The electronic device of 15, wherein the charge transport thin film is a hole injection layer. 17. The electronic device of 16, wherein the electronic device is an organic EL device or a quantum dot EL device.

[0010] By using the charge-transporting varnish of the present invention, a charge-transporting thin film having excellent charge transport properties (particularly, hole injection properties) can be obtained. This charge-transporting thin film can be suitably used as a thin film for electronic devices such as organic EL devices and quantum dot EL devices. In particular, when the charge-transporting varnish of the present invention is used to form a hole-injection layer for an organic EL device or a quantum dot EL device, the resulting hole-injection layer has improved film quality, such as a deeper HOMO level than conventional layers, and the hole injection properties into the hole-transporting layer formed thereon are improved.

[0011] The present invention will be described in more detail below. The charge-transporting varnish according to the present invention is characterized by comprising metal oxide nanoparticles (hereinafter sometimes referred to as surface-treated metal oxide nanoparticles) surface-treated with a silane coupling agent having a specific structure, a charge-transporting substance, and an organic solvent. In the present invention, charge transportability is synonymous with conductivity and hole injection ability. The charge-transporting varnish may itself have charge transportability, or the solid film obtained from it may have charge transportability.

[0012] [1] Surface-treated metal oxide nanoparticles are a characteristic component of the charge-transporting varnish of the present invention, and are metal oxide nanoparticles that have been surface-treated with a silane coupling agent represented by the following formula (S1). Note that nanoparticles refer to fine particles whose primary particle average particle diameter is on the order of nanometers (typically 500 nm or less). Metal oxide nanoparticles refer to metal oxides formed into nanoparticles.

[0013]

[0014] In formula (S1), R v1 ~R v3 each independently represents a hydrogen atom, a chlorine atom, a hydroxy group, an alkoxy group which may have a substituent, or an alkyl group which may have a substituent; R v1 ~R v3 at least one of the groups represents a hydrogen atom, a chlorine atom, a hydroxy group, or an alkoxy group which may have a substituent; L represents a single bond or an alkylene group having 1 to 10 carbon atoms; R v4 represents an alkyl group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group; an alkoxy group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group; or an aryl group having 6 to 20 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, a hydroxy group, an alkyl group having 1 to 10 carbon atoms, and an alkoxy group having 1 to 10 carbon atoms.

[0015] R v1 ~R v3 The alkoxy group may have a linear, branched, or cyclic alkyl group, and specific examples thereof include alkoxy groups having 1 to 10 carbon atoms, such as methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, n-pentoxy, n-hexoxy, n-heptyloxy, n-octyloxy, n-nonyloxy, and n-decyloxy groups. Alkoxy groups having 1 to 5 carbon atoms are preferred, alkoxy groups having 1 to 3 carbon atoms are more preferred, and methoxy and ethoxy groups are even more preferred.

[0016] R v1 ~R v3 The alkyl group may be either linear or branched, and specific examples thereof include alkyl groups having 1 to 10 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl groups, with alkyl groups having 1 to 5 carbon atoms being preferred, alkyl groups having 1 to 3 carbon atoms being more preferred, and methyl and ethyl groups being even more preferred.

[0017] The above R v1 ~R v3 may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, an amino group, and an organosilyl group. v1 ~R v3 When has a substituent, the number of the substituents is preferably 1 to 6, and more preferably 1 to 3.

[0018] Examples of halogen atoms include fluorine, chlorine, bromine and iodine atoms, with fluorine atoms being preferred.

[0019] Examples of organosilyl groups include trialkylsilyl groups in which each alkyl group has 1 to 10 carbon atoms, such as trimethylsilyl group, triethylsilyl group, tripropylsilyl group, tributylsilyl group, tripentylsilyl group, trihexylsilyl group, pentyldimethylsilyl group, hexyldimethylsilyl group, octyldimethylsilyl group, and decyldimethylsilyl group. Other examples include trialkoxysilyl groups in which each alkoxy group has 1 to 10 carbon atoms, such as trimethoxysilyl group, triethoxysilyl group, tri-n-propoxysilyl group, triisopropoxysilyl group, tri-n-butoxysilyl group, tri-s-butoxysilyl group, tri-t-butoxysilyl group, tri-n-pentoxysilyl group, tri-n-hexyloxysilyl group, tri-n-octyloxysilyl group, and tri-n-decyloxysilyl group.

[0020] The alkylene group having 1 to 10 carbon atoms represented by L may be linear, branched, or cyclic. Specific examples thereof include a methylene group, an ethylene group, a propylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, and a decylene group. Among these, an alkylene group having 2 to 5 carbon atoms is preferred, an alkylene group having 2 to 4 carbon atoms is more preferred, and an ethylene group, a trimethylene group, or a tetramethylene group is even more preferred.

[0021] R v4 Examples of the halogen atom include the same as those exemplified above.

[0022] R v4The alkyl group having 1 to 10 carbon atoms may be either linear or branched, and specific examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a cyclopentyl group, a 4-methylpentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, and the like. An alkyl group having 1 to 8 carbon atoms is preferred, an alkyl group having 1 to 6 carbon atoms is more preferred, and a methyl group, an ethyl group, an n-propyl group, or a 4-methylpentyl group is even more preferred.

[0023] R v4 The alkoxy group having 1 to 10 carbon atoms may have a linear, branched, or cyclic alkyl group, and specific examples thereof include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an n-pentoxy group, an n-hexoxy group, an n-heptyloxy group, an n-octyloxy group, an n-nonyloxy group, and an n-decyloxy group. An alkoxy group having 1 to 5 carbon atoms is preferred, an alkoxy group having 1 to 3 carbon atoms is more preferred, and a methoxy group, an ethoxy group, or an n-propoxy group is even more preferred.

[0024] R v4 Examples of the aryl group having 6 to 20 carbon atoms include a phenyl group, a tolyl group, a 1-naphthyl group, a 2-naphthyl group, a 1-anthryl group, a 2-anthryl group, a 9-anthryl group, a 1-phenanthryl group, a 2-phenanthryl group, a 3-phenanthryl group, a 4-phenanthryl group, and a 9-phenanthryl group, with a phenyl group, a tolyl group, and a naphthyl group being preferred.

[0025] R v4 Examples of the alkyl group having 1 to 10 carbon atoms and the alkoxy group having 1 to 10 carbon atoms contained in the aryl group having 6 to 20 carbon atoms include the same groups as those exemplified above.

[0026] The above R v4 When has a substituent, the number of the substituents is preferably 1 to 10, and more preferably 1 to 7.

[0027] However, in the above formula (S1), R v4 When is an alkyl group having 1 to 10 carbon atoms which may have a substituent, L is a single bond.

[0028] As the silane coupling agent represented by the formula (S1), in order to deepen the HOMO level of the resulting charge transporting thin film, v1 ~R v3 is preferably an alkyl group having 1 to 10 carbon atoms which may have a substituent or an alkoxy group having 1 to 10 carbon atoms which may have a substituent. v1 ~R v3 Among these, at least one of which is an alkoxy group having 1 to 10 carbon atoms which may have a substituent, is more preferred, and at least one of which is an alkoxy group having 1 to 5 carbon atoms which may have a substituent, is even more preferred.

[0029] Specific examples of the silane coupling agent include trimethoxy(methyl)silane, trimethoxy(3-methoxypropyl)silane, trimethoxy(propyl)silane, trimethoxy(4-methoxyphenyl)silane, trimethoxyphenylsilane, methoxytrimethylsilane, [3-(1,1,2,3,3,3-hexafluoropropoxy)propyl]trimethoxysilane, trifluoropropyltrimethoxysilane, 1,1,1-trifluoro-2-(trifluoromethyl)-5-(trimethoxysilyl)pentan-2-ol, trimethoxy[3-(perfluorophenyl)propyl]silane, trimethoxyphenylsilane, ethoxytriethylsilane, methoxydimethyl(phenyl)silane, and pentafluorophenylethoxysilane. Examples of suitable silane include dimethylsilane, trimethylethoxysilane, diethoxydimethylsilane, dimethoxydimethylsilane, dimethoxydiphenylsilane, dimethoxymethylphenylsilane, diethoxy(methyl)phenylsilane, triethoxyethylsilane, decyltrimethoxysilane, ethyltrimethoxysilane, hexyltriethoxysilane, hexyltrimethoxysilane, triethoxymethylsilane, n-octyltriethoxysilane, 3-(trihydroxysilyl)-1-propanesulfonic acid, 1,2-bis(trimethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethane, 1,6-bis(trimethoxysilyl)hexane, and 1,6-bis(triethoxysilyl)hexane, but are not limited to these.

[0030] In the present invention, among the above silane coupling agents, trimethoxy(methyl)silane, trimethoxy(3-methoxypropyl)silane, trimethoxy(propyl)silane, trimethoxy(4-methoxyphenyl)silane, trimethoxyphenylsilane, methoxytrimethylsilane, [3-(1,1,2,3,3,3-hexafluoropropoxy)propyl]trimethoxysilane, trifluoropropyltrimethoxysilane, 1,1,1-trifluoro-2-(trifluoromethyl)-5-(trimethoxysilyl)pentan-2-ol, trimethoxysilane, methyltrimethyl ... [3-(perfluorophenyl)propyl]silane is preferred, and trimethoxy(methyl)silane, trimethoxy(3-methoxypropyl)silane, trimethoxy(propyl)silane, methoxytrimethylsilane, [3-(1,1,2,3,3,3-hexafluoropropoxy)propyl]trimethoxysilane, trifluoropropyltrimethoxysilane, 1,1,1-trifluoro-2-(trifluoromethyl)-5-(trimethoxysilyl)pentan-2-ol, and trimethoxy[3-(perfluorophenyl)propyl]silane are more preferred.

[0031] The silane coupling agent may be a commercially available product, or may be obtained by reacting various allyl compounds with a metal catalyst using a known method of hydrosilylation (for example, see Non-Patent Document RSC Adv., 2015, 20603-20616).

[0032] In the present invention, the primary particle size of the metal oxide nanoparticles constituting the surface-treated metal oxide nanoparticles is not particularly limited as long as it is nano-sized, but is usually 5 nm or more, and from the viewpoint of ensuring good particle dispersibility and ease of production, it is usually 200 nm or less, preferably 100 nm or less, and more preferably 30 nm or less.

[0033] The metals constituting the metal oxide nanoparticles include metals in the usual sense as well as metalloids. Metals in the usual sense include, but are not limited to, one or more selected from the group consisting of tin (Sn), titanium (Ti), aluminum (Al), zirconium (Zr), zinc (Zn), niobium (Nb), tantalum (Ta), and tungsten (W). Meanwhile, metalloids refer to elements whose chemical and / or physical properties are intermediate between those of metals and nonmetals. While a universal definition of metalloids has not been established, in the present invention, a total of six elements, namely boron (B), silicon (Si), germanium (Ge), arsenic (As), antimony (Sb), and tellurium (Te), are considered metalloids. These metalloids may be used alone or in combination with two or more of them, or may be used in combination with metals in the usual sense.

[0034] In particular, the metal oxide nanoparticles preferably contain an oxide of one or more metals selected from boron (B), silicon (Si), germanium (Ge), arsenic (As), antimony (Sb), tellurium (Te), tin (Sn), titanium (Ti), aluminum (Al), zirconium (Zr), zinc (Zn), niobium (Nb), tantalum (Ta), and tungsten (W). When two or more metals are used in combination, the metal oxide may be a mixture of oxides of individual metals or a composite oxide containing multiple metals.

[0035] Specific examples of metal oxides include BO, BO, SiO, SiO, GeO, GeO, AsO, AsO, AsO, SbO, SbO, TeO, SnO, ZrO, AlO, and ZnO. However, BO, BO, SiO, SiO, GeO, GeO, AsO, AsO, AsO, SnO, SnO, SbO, TeO, TiO, and mixtures thereof are preferred, SiO, TiO, ZrO, and mixtures thereof are more preferred, and SiO is even more preferred.

[0036] The primary particle diameter of the surface-treated metal oxide nanoparticles is not particularly limited, but is usually 5 nm or more, and from the viewpoint of ensuring good particle dispersibility and ease of production, it is usually 200 nm or less, preferably 100 nm or less, and more preferably 30 nm or less. This particle diameter is the particle diameter at which the cumulative frequency distribution in volume-based particle size distribution measurement by dynamic light scattering method becomes 50% (median diameter D 50 )

[0037] In the surface-treated metal oxide nanoparticles used in the present invention, the amount of silane coupling agent modified on the surface of the metal oxide nanoparticles is not particularly limited. However, from the viewpoint of the dispersibility of the metal oxide nanoparticles and the transparency of the resulting thin film, it is preferred that the amount be 0.1 particles / nm or more and 4.0 particles / nm or less. 2 Preferably, it is less than 0.2 to 3.0 particles / nm 2 More preferably, 0.3 to 2.0 particles / nm 2 It is more preferable that the modification amount X (number / nm 2 ) are the particle size (nm) and specific gravity (g / cm 3 ) The specific surface area SA (nm 2 / g), the total amount of metal oxide particles M (g), the molecular weight Mw of the silane coupling agent, the amount Y (g) of the silane coupling agent, and Avogadro's constant L, and the value is calculated as Y = X * SA * M * Mw / L.

[0038] The amount of surface-treated metal oxide nanoparticles contained in the charge-transporting varnish of the present invention is not particularly limited, but from the viewpoint of improving the hole injection properties of the resulting thin film and increasing the uniformity of the film, the lower limit of the solid content is usually 30 mass %, preferably 40 mass %, and more preferably 50 mass %, and the upper limit is usually 99 mass %, preferably 95 mass %.

[0039] The surface-treated metal oxide nanoparticles used in the present invention may be used in the form of a sol dispersed in a dispersion medium, such as methanol, methyl ethyl ketone, methyl isobutyl ketone, N,N-dimethylacetamide, ethylene glycol, isopropanol, methanol, ethylene glycol monopropyl ether, cyclohexanone, ethyl acetate, toluene, propylene glycol monomethyl ether acetate, or dipropylene glycol monomethyl ether.

[0040] The solids concentration of the sol is not particularly limited, but is preferably 5 to 60% by mass, more preferably 7 to 50% by mass, and even more preferably 10 to 30% by mass. The amount of sol used is determined appropriately taking into account the concentration so that the amount of surface-treated metal oxide nanoparticles ultimately contained in the varnish is the blended amount of metal oxide nanoparticles described above.

[0041] [2] Charge Transporting Substance The charge transporting substance used in the present invention is not particularly limited and can be appropriately selected from charge transporting compounds, charge transporting oligomers, charge transporting polymers, etc. used in the field of organic electroluminescence, etc. Specific examples include various charge transporting compounds and charge transporting oligomers such as arylamine derivatives such as oligoaniline derivatives, N,N'-diarylbenzidine derivatives, and N,N,N',N'-tetraarylbenzidine derivatives, thiophene derivatives such as oligothiophene derivatives, thienothiophene derivatives, and thienobenzothiophene derivatives, pyrrole derivatives such as oligopyrrole, and charge transporting polymers such as polythiophene derivatives, polyaniline derivatives, and polypyrrole derivatives, with polythiophene derivatives being particularly preferred. In a preferred embodiment, the charge transporting substance is a polythiophene derivative containing a repeating unit represented by formula (1) or an amine adduct thereof.

[0042]

[0043] In the formula, R 1 and R 2are each independently a hydrogen atom, an alkyl group having 1 to 40 carbon atoms, a fluoroalkyl group having 1 to 40 carbon atoms, an alkoxy group having 1 to 40 carbon atoms, a fluoroalkoxy group having 1 to 40 carbon atoms, an aryloxy group having 6 to 20 carbon atoms, -O-[Z-O] p -R e or a sulfonic acid group, or R 1 and R 2 are bonded to each other, Y is an alkylene group having 1 to 40 carbon atoms which may contain an ether bond and which may be substituted with a sulfonic acid group, Z is an alkylene group having 1 to 40 carbon atoms which may be substituted with a halogen atom, p is an integer of 1 or more, and R e is a hydrogen atom, an alkyl group having 1 to 40 carbon atoms, a fluoroalkyl group having 1 to 40 carbon atoms, or an aryl group having 6 to 20 carbon atoms.

[0044] The alkyl group having 1 to 40 carbon atoms may be linear, branched, or cyclic, and examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, n-nonadecyl, n-eicosanyl, behenyl, triacontyl, and tetracontyl. In the present invention, alkyl groups having 1 to 18 carbon atoms are preferred, and alkyl groups having 1 to 8 carbon atoms are more preferred.

[0045] The fluoroalkyl group having 1 to 40 carbon atoms is not particularly limited as long as it is an alkyl group having 1 to 40 carbon atoms in which at least one hydrogen atom on a carbon atom is substituted with a fluorine atom, and examples thereof include a fluoromethyl group, a difluoromethyl group, a trifluoromethyl group, a 1-fluoroethyl group, a 2-fluoroethyl group, a 1,2-difluoroethyl group, a 1,1-difluoroethyl group, a 2,2-difluoroethyl group, a 1,1,2-trifluoroethyl group, a 1,2,2-trifluoroethyl group, a 2,2,2-trifluoroethyl group, a 1,1,2,2-tetrafluoroethyl group, a 1,2,2,2-tetrafluoroethyl group, a perfluoroethyl group, a 1-fluoropropyl group, a 2-fluoropropyl group, a 3-fluoropropyl group, a 1,1-difluoropropyl group, a 1,2-difluoropropyl group, a 1,3-difluoropropyl group, a 2,2-difluoropropyl group, a 2,3-difluoropropyl group, a 3,3-difluoropropyl group, a 1,1,2-trifluoropropyl group, a 1,3-trifluoropropyl group, 1,2,3-trifluoropropyl group, 1,3,3-trifluoropropyl group, 2,2,3-trifluoropropyl group, 2,3,3-trifluoropropyl group, 3,3,3-trifluoropropyl group, 1,1,2,2-tetrafluoropropyl group, 1,1,2,3-tetrafluoropropyl group, 1,2,2,3-tetrafluoropropyl group, 1,3,3,3-tetrafluoropropyl group, 2,2,3,3-tetrafluoropropyl group, 2, Examples include a 3,3,3-tetrafluoropropyl group, a 1,1,2,2,3-pentafluoropropyl group, a 1,2,2,3,3-pentafluoropropyl group, a 1,1,3,3,3-pentafluoropropyl group, a 1,2,3,3,3-pentafluoropropyl group, a 2,2,3,3,3-pentafluoropropyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, a perfluorohexyl group, a perfluoroheptyl group, and a perfluorooctyl group.

[0046] The alkoxy group having 1 to 40 carbon atoms may have a linear, branched, or cyclic alkyl group, and examples thereof include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, a c-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentoxy group, an n-hexoxy group, an n-heptyloxy group, an n-octyloxy group, an n-nonyloxy group, an n-decyloxy group, an n-undecyloxy group, an n-dodecyloxy group, an n-tridecyloxy group, an n-tetradecyloxy group, an n-pentadecyloxy group, an n-hexadecyloxy group, an n-heptadecyloxy group, an n-octadecyloxy group, an n-nonadecyloxy group, and an n-eicosanyloxy group.

[0047] The fluoroalkoxy group having 1 to 40 carbon atoms is not particularly limited as long as it is an alkoxy group having 1 to 40 carbon atoms in which at least one hydrogen atom on a carbon atom is substituted with a fluorine atom, and examples thereof include a fluoromethoxy group, a difluoromethoxy group, a trifluoromethoxy group, a 1-fluoroethoxy group, a 2-fluoroethoxy group, a 1,2-difluoroethoxy group, a 1,1-difluoroethoxy group, a 2,2-difluoroethoxy group, a 1,1,2-trifluoroethoxy group, a 1,2, 2-trifluoroethoxy group, 2,2,2-trifluoroethoxy group, 1,1,2,2-tetrafluoroethoxy group, 1,2,2,2-tetrafluoroethoxy group, perfluoroethoxy group, 1-fluoropropoxy group, 2-fluoropropoxy group, 3-fluoropropoxy group, 1,1-difluoropropoxy group, 1,2-difluoropropoxy group, 1,3-difluoropropoxy group, 2,2-difluoropropoxy group, 2,3-difluoropropoxy group, 3,3- Difluoropropoxy group, 1,1,2-trifluoropropoxy group, 1,1,3-trifluoropropoxy group, 1,2,3-trifluoropropoxy group, 1,3,3-trifluoropropoxy group, 2,2,3-trifluoropropoxy group, 2,3,3-trifluoropropoxy group, 3,3,3-trifluoropropoxy group, 1,1,2,2-tetrafluoropropoxy group, 1,1,2,3-tetrafluoropropoxy group, 1,2,2,3-tetrafluoropropoxy group groups, 1,3,3,3-tetrafluoropropoxy groups, 2,2,3,3-tetrafluoropropoxy groups, 2,3,3,3-tetrafluoropropoxy groups, 1,1,2,2,3-pentafluoropropoxy groups, 1,2,2,3,3-pentafluoropropoxy groups, 1,1,3,3,3-pentafluoropropoxy groups, 1,2,3,3,3-pentafluoropropoxy groups, 2,2,3,3,3-pentafluoropropoxy groups, and perfluoropropoxy groups.

[0048] The alkylene group having 1 to 40 carbon atoms may be linear, branched, or cyclic, and examples thereof include a methylene group, an ethylene group, a propylene group, a trimethylene group, a tetramethylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tridecylene group, a tetradecylene group, a pentadecylene group, a hexadecylene group, a heptadecylene group, an octadecylene group, a nonadecylene group, and an eicosanylene group.

[0049] Examples of the aryl group having 6 to 20 carbon atoms include a phenyl group, a tolyl group, a 1-naphthyl group, a 2-naphthyl group, a 1-anthryl group, a 2-anthryl group, a 9-anthryl group, a 1-phenanthryl group, a 2-phenanthryl group, a 3-phenanthryl group, a 4-phenanthryl group, and a 9-phenanthryl group, with a phenyl group, a tolyl group, and a naphthyl group being preferred.

[0050] Examples of the aryloxy group having 6 to 20 carbon atoms include a phenoxy group, an anthracenoxy group, a naphthoxy group, a phenanthrenoxy group, and a fluorenoxy group.

[0051] Halogen atoms include fluorine atoms, chlorine atoms, bromine atoms and iodine atoms.

[0052] In the above formula (1), R 1 and R 2 are each independently a hydrogen atom, a fluoroalkyl group having 1 to 40 carbon atoms, an alkoxy group having 1 to 40 carbon atoms, or —O[C(R a R b )-C(R c R d )-O] p -R e , -OR f , or a sulfonic acid group, or R 1 and R 2 is preferably —O—Y—O—, which is formed by bonding R a ~R dare each independently a hydrogen atom, an alkyl group having 1 to 40 carbon atoms, a fluoroalkyl group having 1 to 40 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and specific examples of these groups are the same as those listed above. a ~R d are each independently preferably a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a fluoroalkyl group having 1 to 8 carbon atoms, or a phenyl group. e is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a fluoroalkyl group having 1 to 8 carbon atoms, or a phenyl group, and is preferably a hydrogen atom, a methyl group, a propyl group, or a butyl group. Furthermore, p is preferably an integer of 1 to 5, and more preferably 1, 2, or 3.

[0053] R f represents a hydrogen atom, an alkyl group having 1 to 40 carbon atoms, a fluoroalkyl group having 1 to 40 carbon atoms, or an aryl group having 6 to 20 carbon atoms, but is preferably a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a fluoroalkyl group having 1 to 8 carbon atoms, or a phenyl group, and more preferably —CHCF.

[0054] In the present invention, R 1 is preferably a hydrogen atom or a sulfonic acid group, more preferably a sulfonic acid group, and R 2 is preferably an alkoxy group having 1 to 40 carbon atoms or —O—[ZO] p -R e , more preferably —O[C(R a R b )-C(R c R d ) -O] p -R e or -OR f , and even more preferably —O[C(R a R b )-C(R c R d ) -O] p -R e , —O—CH2CH2—O—CH2CH2—O—CH3, —O—CH2CH2—O—CH2CH2—OH or —O—CH2CH2—OH, or R 1 and R 2are bonded to each other to form —O—Y—O—.

[0055] For example, the polythiophene derivative according to a preferred embodiment of the present invention may be 1 is a sulfonic acid group, and R 2 contains a repeating unit other than a sulfonic acid group, or R 1 and R 2 Preferably, the polythiophene derivative contains a repeating unit of —O—Y—O— formed by bonding of R 1 is a sulfonic acid group, and R 2 is an alkoxy group having 1 to 40 carbon atoms or —O—[Z—O] p -R e or R 1 and R 2 More preferably, the polythiophene derivative contains a repeating unit of —O—Y—O— formed by bonding of R 1 is a sulfonic acid group, and R 2 is -O[C(R a R b )-C(R c R d ) -O] p -R e or -OR f More preferably, the polythiophene derivative comprises a repeating unit represented by R 1 is a sulfonic acid group, and R 2 is -O[C(R a R b )-C(R c R d ) -O] p -R e or R 1 and R 2 More preferably, the polythiophene derivative contains a repeating unit represented by —O—Y—O— formed by bonding of R 1 is a sulfonic acid group, and R 2 is —O—CH2CH2—O—CH2CH2—O—CH3, —O—CH2CH2—O—CH2CH2—OH, or —O—CH2CH2—OH, or R1 and R 2 are bonded to each other to form repeating units which are groups represented by the following formulae (Y1) and (Y2).

[0056]

[0057] Specific preferred examples of the polythiophene derivative include polythiophenes containing at least one repeating unit represented by the following formulas (1-1) to (1-5).

[0058]

[0059] A suitable structure of the polythiophene derivative is, for example, a polythiophene derivative having a structure represented by the following formula (1a): In the following formula, the units may be bonded randomly or as a block polymer.

[0060]

[0061] In the formula, a to d represent the molar ratio of each unit, and satisfy the following conditions: 0≦a≦1, 0≦b≦1, 0<a+b≦1, 0≦c<1, 0≦d<1, a+b+c+d=1.

[0062] Furthermore, the polythiophene derivatives may be homopolymers or copolymers (including statistical, random, gradient, and block copolymers). As polymers containing monomers A and B, block copolymers include, for example, AB diblock copolymers, A-B-A triblock copolymers, and (AB) m - including multi-block copolymers. Polythiophenes may also contain repeat units derived from other types of monomers, such as thienothiophenes, selenophenes, pyrroles, furans, tellurophenes, anilines, arylamines, and arylenes (such as phenylene, phenylenevinylene, and fluorene).

[0063] In the present invention, the content of the repeating unit represented by formula (1) in the polythiophene derivative is preferably more than 50 mol %, more preferably 80 mol % or more, even more preferably 90 mol % or more, still more preferably 95 mol % or more, and most preferably 100 mol % of all repeating units contained in the polythiophene derivative.

[0064] In the present invention, depending on the purity of the starting monomers used in the polymerization, the polymer formed may contain repeating units derived from impurities. In the present invention, the term "homopolymer" means a polymer containing repeating units derived from one type of monomer, but may also contain repeating units derived from impurities. In the present invention, the polythiophene derivative is preferably a polymer in which essentially all repeating units are repeating units represented by formula (1), and more preferably a polymer containing at least one of repeating units represented by formulas (1-1) to (1-5).

[0065] In the present invention, when the polythiophene derivative contains a repeating unit having a sulfonic acid group, it is preferable to convert the polythiophene derivative into an amine adduct in which an amine compound is added to at least a part of the sulfonic acid groups contained in the polythiophene derivative, from the viewpoint of further improving solubility and dispersibility in organic solvents.

[0066] Examples of amine compounds that can be used to form the amine adduct include methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, s-butylamine, t-butylamine, n-pentylamine, n-hexylamine, n-heptylamine, n-octylamine, 2-ethylhexylamine, n-nonylamine, n-decylamine, n-undecylamine, n-dodecylamine, n-tridecylamine, n-tetradecylamine, n-pentadecylamine, n-hexadecylamine, n-heptadecylamine, and n- monoalkylamine compounds such as octadecylamine, n-nonadecylamine, and n-eicosanylamine; primary amine compounds such as monoarylamine compounds such as aniline, tolylamine, 1-naphthylamine, 2-naphthylamine, 1-anthrylamine, 2-anthrylamine, 9-anthrylamine, 1-phenanthrylamine, 2-phenanthrylamine, 3-phenanthrylamine, 4-phenanthrylamine, and 9-phenanthrylamine; primary amine compounds such as N-ethylmethylamine, N-methyl-n-propylamine, N-methylisopropylamine, N-methyl- n-butylamine, N-methyl-s-butylamine, N-methyl-t-butylamine, N-methylisobutylamine, diethylamine, N-ethyl-n-propylamine, N-ethylisopropylamine, N-ethyl-n-butylamine, N-ethyl-s-butylamine, N-ethyl-t-butylamine, dipropylamine, N-n-propylisopropylamine, N-n-propyl-n-butylamine, N-n-propyl-s-butylamine, diisopropylamine, N-n-butylisopropylamine, N-t-butylisopropylamine, di(n- dialkylamine compounds such as di(butyl)amine, di(s-butyl)amine, diisobutylamine, aziridine (ethyleneimine), 2-methylaziridine (propyleneimine), 2,2-dimethylaziridine, azetidine (trimethyleneimine), 2-methylazetidine, pyrrolidine, 2-methylpyrrolidine, 3-methylpyrrolidine, 2,5-dimethylpyrrolidine, piperidine, 2,6-dimethylpiperidine, 3,5-dimethylpiperidine, 2,2,6,6-tetramethylpiperidine, hexamethyleneimine, heptamethyleneimine, and octamethyleneimine;Diarylamine compounds such as diphenylamine, N-phenyl-1-naphthylamine, N-phenyl-2-naphthylamine, 1,1'-dinaphthylamine, 2,2'-dinaphthylamine, 1,2'-dinaphthylamine, carbazole, 7H-benzo[c]carbazole, 11H-benzo[a]carbazole, 7H-dibenzo[c,g]carbazole, and 13H-dibenzo[a,i]carbazole; N-methylaniline, N-ethylaniline, N-n-propylaniline, N-iso ... secondary amine compounds such as alkylarylamine compounds such as N,N-isopropylaniline, N-n-butylaniline, N-s-butylaniline, N-isobutylaniline, N-methyl-1-naphthylamine, N-ethyl-1-naphthylamine, N-n-propyl-1-naphthylamine, indoline, isoindoline, 1,2,3,4-tetrahydroquinoline, and 1,2,3,4-tetrahydroisoquinoline; Trialkylamine compounds such as N-dimethylisopropylamine, N,N-dimethyl-n-butylamine, N,N-dimethyl-s-butylamine, N,N-dimethyl-t-butylamine, N,N-dimethylisobutylamine, N,N-diethylmethylamine, N-methyldi(n-propyl)amine, N-methyldiisopropylamine, N-methyldi(n-butyl)amine, N-methyldiisobutylamine, triethylamine, N,N-diethyl-n-butylamine, N,N-diisopropylethylamine, N,N-di(n-butyl)ethylamine, tri(n-propyl)amine, tri(i-propyl)amine, tri(n-butyl)amine, tri(i-butyl)amine, 1-methylacetidine, 1-methylpyrrolidine, and 1-methylpiperidine; triarylamine compounds such as triphenylamine; alkyldiarylamine compounds such as N-methyldiphenylamine, N-ethyldiphenylamine, 9-methylcarbazole, and 9-ethylcarbazole;Examples of suitable tertiary amine compounds include dialkylarylamine compounds such as N,N-diethylaniline, N,N-di(n-propyl)aniline, N,N-di(i-propyl)aniline, and N,N-di(n-butyl)aniline. However, taking into consideration the balance between the solubility of the amine adduct and the charge transport properties of the resulting charge-transporting thin film, tertiary amine compounds are preferred, trialkylamine compounds are more preferred, and triethylamine is even more preferred. The amine adduct can be obtained by adding the polythiophene derivative to the amine itself or a solution thereof and stirring thoroughly.

[0067] In the present invention, the polythiophene derivative or its amine adduct may be treated with a reducing agent. In polythiophene derivatives or their amine adducts, some of the repeating units constituting them may have an oxidized chemical structure called a "quinoid structure." The term "quinoid structure" is used in contrast to the term "benzenoid structure." The latter refers to a structure containing an aromatic ring, whereas the former refers to a structure in which a double bond within the aromatic ring moves outside the ring (resulting in the disappearance of the aromatic ring), forming two exocyclic double bonds conjugated with other double bonds remaining within the ring. Those skilled in the art can easily understand the relationship between these two structures from the relationship between the structures of benzoquinone and hydroquinone. Quinoid structures for repeating units of various conjugated polymers are well known to those skilled in the art. As an example, a quinoid structure corresponding to a repeating unit of a polythiophene derivative containing a repeating unit represented by the above formula (1) is shown in the following formula (1').

[0068] (In the formula, R 1 and R 2 is as defined in the above formula (1).

[0069] This quinoid structure is generated by a process in which a polythiophene derivative containing a repeating unit represented by the above formula (1) undergoes an oxidation reaction with a dopant, a so-called doping reaction, and forms part of a structure called a "polaron structure" or a "bipolaron structure" that imparts charge transport properties to the polythiophene derivative. These structures are known. The introduction of a "polaron structure" and / or a "bipolaron structure" is essential in the fabrication of organic EL devices and quantum dot EL devices. In fact, during the fabrication of organic EL devices and quantum dot EL devices, this is achieved by intentionally inducing the above-mentioned doping reaction when a thin film formed from a charge transport varnish is baked. The reason why the polythiophene derivative contains a quinoid structure before the doping reaction is thought to be because the polythiophene derivative underwent an unintended oxidation reaction equivalent to the doping reaction during its manufacturing process (particularly the sulfonation step therein).

[0070] There is a correlation between the amount of quinoid structures contained in the polythiophene derivative and the solubility and dispersibility of the polythiophene derivative in organic solvents; as the amount of quinoid structures increases, the solubility and dispersibility tend to decrease. Therefore, the introduction of quinoid structures after a thin film is formed from a charge-transporting varnish does not cause any problems. However, if an excessive amount of quinoid structures is introduced into the polythiophene derivative due to the unintended oxidation reaction, the production of the charge-transporting varnish may be hindered. Polythiophene derivatives are known to have varying solubility and dispersibility in organic solvents. One of the causes is thought to be that the amount of quinoid structures introduced into the polythiophene due to the unintended oxidation reaction varies depending on the production conditions of each polythiophene derivative. Therefore, when the polythiophene derivative is subjected to a reduction treatment using a reducing agent, even if an excessive amount of quinoid structures is introduced into the polythiophene derivative, the quinoid structures are reduced by reduction, improving the solubility and dispersibility of the polythiophene derivative in organic solvents. This enables the stable production of a good charge-transporting varnish that provides a thin film with excellent uniformity.

[0071] The conditions for the reduction treatment are not particularly limited as long as they can reduce the quinoid structure and appropriately convert it into a non-oxidized structure, i.e., the benzenoid structure (for example, in the case of a polythiophene derivative containing a repeating unit represented by formula (1) above, the quinoid structure represented by formula (1′) is converted into the structure represented by formula (1) above). For example, this treatment can be carried out by simply contacting the polythiophene derivative or the amine adduct with a reducing agent in the presence or absence of a suitable solvent. The reducing agent is also not particularly limited as long as it can appropriately reduce the polythiophene derivative or the amine adduct. Suitable examples of the reducing agent include aqueous ammonia and hydrazine, which are readily available commercially. The amount of the reducing agent cannot be generally specified because it varies depending on the amount of reducing agent used. However, it is usually 0.1 parts by mass or more per 100 parts by mass of the polythiophene derivative or the amine adduct to be treated in order to appropriately reduce the polythiophene derivative or the amine adduct, and 10 parts by mass or less in order to prevent excess reducing agent from remaining.

[0072] In one example of a specific reduction method, the polythiophene derivative or the amine adduct is stirred overnight in 28% aqueous ammonia at room temperature. Reduction under such relatively mild conditions sufficiently improves the solubility and dispersibility of the polythiophene derivative or the amine adduct in organic solvents.

[0073] When an amine adduct of a polythiophene derivative is used in the charge-transporting varnish of the present invention, the reduction treatment may be carried out either before or after the formation of the amine adduct.

[0074] Note that, as a result of this reduction treatment changing the solubility or dispersibility of the polythiophene derivative or its amine adduct in the solvent, the polythiophene derivative or its amine adduct, which was not dissolved in the reaction system at the start of the treatment, may become dissolved by the completion of the treatment. In such cases, the polythiophene derivative or its amine adduct can be recovered by a method such as adding an organic solvent incompatible with the polythiophene derivative or its amine adduct (acetone, isopropyl alcohol, etc., in the case of sulfonated polythiophene) to the reaction system to cause a precipitate of the polythiophene derivative or its amine adduct, and then filtering the precipitate.

[0075] The weight-average molecular weight of the polythiophene derivative or its amine adduct containing the repeating unit represented by formula (1) is preferably about 1,000 to 1,000,000, more preferably about 5,000 to 100,000, and even more preferably about 10,000 to about 50,000. By setting the weight-average molecular weight at or above the lower limit, good conductivity can be obtained with good reproducibility, while by setting it at or below the upper limit, solubility in organic solvents is improved. The weight-average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography.

[0076] The polythiophene derivative or its amine adduct contained in the charge transport varnish of the present invention may be only one type of polythiophene derivative or its amine adduct containing a repeating unit represented by formula (1), or two or more types may be used.In addition, the polythiophene derivative containing a repeating unit represented by formula (1) may be a commercially available product, or may be polymerized by a known method using a thiophene derivative or the like as a starting material.In either case, it is preferable to use a product purified by a method such as reprecipitation or ion exchange.By using a purified product, the properties of an organic EL device or a quantum dot EL device equipped with a thin film obtained from the charge transport varnish of the present invention can be further improved.

[0077] Sulfonation of conjugated polymers and sulfonated conjugated polymers (including sulfonated polythiophenes) are described in U.S. Patent No. 8,017,241 to Seshadri et al., and sulfonated polythiophenes are described in WO 2008 / 073149 and WO 2016 / 171935.

[0078] In the present invention, at least a portion of the polythiophene derivative or its amine adduct containing the repeating unit represented by formula (1) contained in the charge transporting varnish is dissolved in an organic solvent.

[0079] In the present invention, as the charge transport substance, a polythiophene derivative containing a repeating unit represented by formula (1) or an amine adduct thereof may be used in combination with a charge transport substance consisting of another charge transport compound, but it is preferable that only a polythiophene derivative containing a repeating unit represented by formula (1) or an amine adduct thereof is used.

[0080] The content of the charge transporting substance in the charge transporting varnish of the present invention is usually determined appropriately in the range of 1.0 to 70% by mass, preferably 2.0 to 50% by mass, of the solid content, taking into consideration the desired film thickness, the viscosity of the varnish, etc.

[0081] [3] Organic Solvent The organic solvent used in preparing the charge-transporting varnish of the present invention can be a highly polar solvent capable of dissolving the charge-transporting material used. If necessary, a low-polarity solvent may be used because it has better process compatibility than a high-polarity solvent. In the present invention, a low-polarity solvent is defined as one having a dielectric constant of less than 7 at a frequency of 100 kHz, and a high-polarity solvent is defined as one having a dielectric constant of 7 or more at a frequency of 100 kHz.

[0082] Examples of low-polarity solvents include: chlorine-based solvents such as chloroform and chlorobenzene; aromatic hydrocarbon-based solvents such as toluene, xylene, tetralin, cyclohexylbenzene, and decylbenzene; aliphatic alcohol-based solvents such as 1-octanol, 1-nonanol, and 1-decanol; ether-based solvents such as tetrahydrofuran, dioxane, anisole, 4-methoxytoluene, 3-phenoxytoluene, dibenzyl ether, diethylene glycol dimethyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, and triethylene glycol butyl methyl ether; and ester-based solvents such as methyl benzoate, ethyl benzoate, butyl benzoate, isoamyl benzoate, bis(2-ethylhexyl) phthalate, dibutyl maleate, dibutyl oxalate, hexyl acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0083] Examples of highly polar solvents include amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylisobutyramide, N-methylpyrrolidone, and 1,3-dimethyl-2-imidazolidinone; ketone solvents such as ethyl methyl ketone, isophorone, and cyclohexanone; cyano solvents such as acetonitrile and 3-methoxypropionitrile; polyhydric alcohol solvents such as ethylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, 1,3-butanediol, and 2,3-butanediol; monohydric alcohol solvents other than aliphatic alcohols such as diethylene glycol monomethyl ether, diethylene glycol monophenyl ether, triethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, benzyl alcohol, 2-phenoxyethanol, 2-benzyloxyethanol, 3-phenoxybenzyl alcohol, and tetrahydrofurfuryl alcohol; and sulfoxide solvents such as dimethyl sulfoxide.

[0084] [4] Dopant Substance The charge-transporting varnish of the present invention may contain a dopant substance for the purpose of improving the charge transport ability, etc., depending on the application of the resulting thin film. The dopant substance is not particularly limited as long as it is soluble in at least one solvent used in the varnish, and both inorganic and organic dopant substances can be used. Inorganic and organic dopant substances may be used alone or in combination of two or more. The amount of the dopant substance cannot be generally specified because it is determined appropriately taking into account the type of dopant and the desired level of charge transportability, but is typically within the range of 0.0001 to 100.0 parts by mass of the charge-transporting substance per 1 part.

[0085] Examples of inorganic dopant substances include inorganic acids such as hydrogen chloride, sulfuric acid, nitric acid, and phosphoric acid; metal halides such as aluminum(III) chloride (AlCl), titanium(IV) tetrachloride (TiCl), boron tribromide (BBr), boron trifluoride etherate (BF.OEt), iron(III) chloride (FeCl), copper(II) chloride (CuCl), antimony(V) pentachloride (SbCl), antimony(V) pentafluoride (SbF), arsenic(V) pentafluoride (AsF), phosphorus pentafluoride (PF), and tris(4-bromophenyl)aluminum hexachloroantimonate (TBPAH); halogens such as Cl, Br, I, ICl, ICl, IBr, and IF; and heteropolyacids such as phosphomolybdic acid and phosphotungstic acid.

[0086] In addition, examples of organic dopant substances include tetracyanoquinodimethanes such as 7,7,8,8-tetracyanoquinodimethane (TCNQ) and 2,5-difluoro-7,7,8,8-tetracyanoquinodimethane; tetrafluoro-7,7,8,8-tetracyanoquinodimethane (F4TCNQ), tetrachloro-7,7,8,8-tetracyanoquinodimethane, 2-fluoro-7,7,8,8-tetracyanoquinodimethane, 2-chloro-7,7,8,8-tetracyanoquinodimethane, 2,5-difluoro-7,7,8,8-tetracyanoquinodimethane, 2,5- Halotetracyanoquinodimethanes (haloTCNQs) such as dichloro-7,7,8,8-tetracyanoquinodimethane; benzoquinone derivatives such as tetrachloro-1,4-benzoquinone (chloranil) and 2,3-dichloro-5,6-dicyano-1,4-benzoquinone (DDQ); benzenesulfonic acid, tosylic acid, p-styrenesulfonic acid, 2-naphthalenesulfonic acid, 4-hydroxybenzenesulfonic acid, 5-sulfosalicylic acid, p-dodecylbenzenesulfonic acid, dihexylbenzenesulfonic acid, 2,5-dihexylbenzenesulfonic acid, dibutylnaphthalenesulfonic acid, naphthalenesulfonic acid, 6,7-dibutyl-2-naphthalenesulfonic acid, dodecylnaphthalenesulfonic acid, 3-dodecyl-2-naphthalenesulfonic acid, hexylnaphthalenesulfonic acid, 4-hexyl-1-naphthalenesulfonic acid, octylnaphthalenesulfonic acid, 2-octyl-1-naphthalenesulfonic acid, hexylnaphthalenesulfonic acid, 7-hexyl-1-naphthalenesulfonic acid, 6-hexyl-2-naphthalenesulfonic acid, dinonylnaphthalenesulfonic acid, 2,7-dinonyl-4-naphthalenesulfonic acid, dinonylnaphthalenedisulfonic acid, 2,7-di Examples of suitable sulfonic acid compounds include aryl sulfonic acid compounds such as nonyl-4,5-naphthalenedisulfonic acid, 1,4-benzodioxanedisulfonic acid derivatives described in WO 2005 / 000832, arylsulfonic acid derivatives described in WO 2006 / 025342, and dinonylnaphthalenesulfonic acid derivatives described in JP 2005-108828 A; aromatic sulfone compounds such as polystyrene sulfonic acid; fluorinated arylsulfonic acid polymer compounds described in WO 2023 / 008176; and non-aromatic sulfone compounds such as 10-camphorsulfonic acid.These inorganic and organic dopant substances may be used alone or in combination of two or more.

[0087] Among these dopant substances, arylsulfonic acid compounds are suitable for use in the present invention, and may be low molecular weight or high molecular weight. Preferred examples of low molecular weight arylsulfonic acid compounds include arylsulfonic acid compounds represented by formula (H1) or (H2).

[0088]

[0089] A 1 represents O or S, with O being preferred. 2 represents a naphthalene ring or an anthracene ring, with a naphthalene ring being preferred. 3 represents a divalent to tetravalent perfluorobiphenyl group, s represents A 1 and A 3 and is an integer satisfying 2≦s≦4, 3 is a perfluorobiphenyldiyl group, preferably a perfluorobiphenyl-4,4'-diyl group, and s is preferably 2. 2 represents the number of sulfonic acid groups bonded to the hydroxyl group, and is an integer satisfying the relationship 1≦q≦4, with 2 being optimal.

[0090] A 4 ~A 8 are each independently a hydrogen atom, a halogen atom, a cyano group, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, or a halogenated alkenyl group having 2 to 20 carbon atoms; 4 ~A 8 At least three of the groups are halogen atoms.

[0091] Examples of halogenated alkyl groups having 1 to 20 carbon atoms include a trifluoromethyl group, a 2,2,2-trifluoroethyl group, a 1,1,2,2,2-pentafluoroethyl group, a 3,3,3-trifluoropropyl group, a 2,2,3,3,3-pentafluoropropyl group, a 1,1,2,2,3,3,3-heptafluoropropyl group, a 4,4,4-trifluorobutyl group, a 3,3,4,4,4-pentafluorobutyl group, a 2,2,3,3,4,4,4-heptafluorobutyl group, and a 1,1,2,2,3,3,4,4,4-nonafluorobutyl group.

[0092] Examples of halogenated alkenyl groups having 2 to 20 carbon atoms include perfluorovinyl groups, perfluoropropenyl groups (allyl groups), perfluorobutenyl groups, etc. Other examples of halogen atoms and alkyl groups having 1 to 20 carbon atoms include those similar to those mentioned above, but the halogen atom is preferably a fluorine atom.

[0093] Among these, A 4 ~A 8 is a hydrogen atom, a halogen atom, a cyano group, an alkyl group having 1 to 10 carbon atoms, a halogenated alkyl group having 1 to 10 carbon atoms, or a halogenated alkenyl group having 2 to 10 carbon atoms, and A 4 ~A 8 At least three of A are preferably fluorine atoms, and are selected from the group consisting of a hydrogen atom, a fluorine atom, a cyano group, an alkyl group having 1 to 5 carbon atoms, a fluorinated alkyl group having 1 to 5 carbon atoms, and a fluorinated alkenyl group having 2 to 5 carbon atoms, and 4 ~A 8 At least three of A are preferably fluorine atoms, and A is preferably a hydrogen atom, a fluorine atom, a cyano group, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkenyl group having 1 to 5 carbon atoms. 4 , A 5 and A 8 It is more preferable that each of the hydrogen atoms of the alkyl group and the perfluoroalkenyl group is a group in which all of the hydrogen atoms of the alkyl group are substituted with fluorine atoms.

[0094] r represents the number of sulfonic acid groups bonded to the naphthalene ring and is an integer satisfying 1≦r≦4, preferably 2 to 4, and most preferably 2.

[0095] When a low-molecular-weight organic compound is used as the dopant substance, the molecular weight thereof is preferably 3,000 or less, more preferably 2,500 or less, in consideration of solubility in organic solvents. In particular, the molecular weight of the low-molecular-weight arylsulfonic acid compound used as the dopant substance is not particularly limited, but is preferably 2,000 or less, more preferably 1,500 or less, in consideration of solubility in organic solvents.

[0096] In the present invention, examples of arylsulfonic acid compounds that can be suitably used include, but are not limited to, the following compounds:

[0097]

[0098] The amount of the arylsulfonic acid compound used is preferably about 0.01 to 20.0, more preferably about 0.4 to 5.0, in terms of mole ratio per 1 part of the charge transporting substance such as a polythiophene derivative or an arylamine derivative.

[0099] Furthermore, the dopant substance may be a substance whose function as a dopant substance is first exhibited or improved by, for example, a part of its molecule being removed in response to an external stimulus, such as heating during baking, during the process of obtaining a charge-transporting thin film, which is a solid film, from the varnish, for example, an arylsulfonate ester compound protected by a group from which the sulfonic acid group is easily removed.

[0100] The aryl sulfonate ester compound is not particularly limited as long as it has a sulfonate ester group bonded to an aromatic ring. The molecular weight of the aryl sulfonate ester compound is not particularly limited. In a preferred embodiment of the present invention, the molecular weight of the aryl sulfonate ester compound is preferably 100 or more, more preferably 200 or more, and preferably 5,000 or less, more preferably 4,000 or less, even more preferably 3,000 or less, and even more preferably 2,000 or less. In a preferred embodiment of the present invention, the number of sulfonate ester groups in the aryl sulfonate ester compound is preferably 2 or more, more preferably 3 or more, and preferably 6 or less, more preferably 5 or less. In a preferred embodiment of the present invention, the aryl sulfonate ester compound preferably contains an aromatic ring substituted with fluorine.

[0101] Examples of the aryl sulfonate ester compound include the aryl sulfonate ester compounds disclosed in WO 2017 / 217455, the aryl sulfonate ester compounds disclosed in WO 2017 / 217457, and the aryl sulfonate ester compounds described in WO 2019 / 124412. Preferred aryl sulfonate compounds are those represented by the following formula (B1) or (B1′):

[0102]

[0103] In formulas (B1) and (B1′), A 01 is an s-valent hydrocarbon group having 6 to 20 carbon atoms and containing one or more aromatic rings, which may have a substituent, or an s-valent group derived from a compound represented by the following formula (B1a) or (B1b) (i.e., a group obtained by removing s hydrogen atoms on the aromatic rings of a compound represented by the following formula (B1a) or (B1b)):

[0104] (In the formula, W 1 and W 2 are each independently —O—, —S—, —S(O)—, —S(O)—, or —N—, —Si—, —P—, or —P(O)— which may have a substituent.

[0105] An s-valent hydrocarbon group having 6 to 20 carbon atoms and containing one or more aromatic rings is a group obtained by removing s hydrogen atoms from a hydrocarbon having 6 to 20 carbon atoms and containing one or more aromatic rings. Examples of the hydrocarbon containing one or more aromatic rings include benzene, toluene, xylene, biphenyl, naphthalene, anthracene, and pyrene. Of these, groups derived from benzene, biphenyl, etc. are preferred as the s-valent hydrocarbon group.

[0106] The hydrocarbon group may further have some or all of its hydrogen atoms substituted with a substituent, such as a halogen atom (fluorine atom, chlorine atom, bromine atom, or iodine atom), nitro, cyano, hydroxy, amino, silanol, thiol, carboxy, sulfonate ester, phosphoric acid, phosphate ester, ester, thioester, amide, monovalent hydrocarbon, organooxy, organoamino, organosilyl, organothio, acyl, or sulfo group.

[0107] Here, the monovalent hydrocarbon group may be linear, branched, or cyclic, and specific examples thereof include alkyl groups having 1 to 10 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl groups; alkenyl groups having 2 to 10 carbon atoms, such as vinyl, 1-propenyl, 2-propenyl, isopropenyl, 1-methyl-2-propenyl, 1-butenyl, 2-butenyl, 3-butenyl, and hexenyl groups; aryl groups having 6 to 20 carbon atoms, such as phenyl, xylyl, tolyl, 1-naphthyl, and 2-naphthyl groups; and aralkyl groups having 7 to 20 carbon atoms, such as benzyl and phenylethyl groups.

[0108] Specific examples of the organoxy group include alkoxy, alkenyloxy, aryloxy, etc. The alkyl, alkenyl and aryl groups contained therein are the same as those described above.

[0109] Specific examples of the organoamino group include alkylamino groups having 1 to 12 carbon atoms, such as methylamino, ethylamino, propylamino, butylamino, pentylamino, hexylamino, cyclohexylamino, heptylamino, octylamino, nonylamino, decylamino, and dodecylamino groups; dialkylamino groups in which each alkyl group has 1 to 12 carbon atoms, such as dimethylamino, diethylamino, dipropylamino, dibutylamino, dipentylamino, dihexylamino, dicyclohexylamino, diheptylamino, dioctylamino, dinonylamino, and didecylamino groups; and a morpholino group.

[0110] Specific examples of the organosilyl group include trialkylsilyl groups, each of which has 1 to 10 carbon atoms, such as trimethylsilyl, triethylsilyl, tripropylsilyl, tributylsilyl, tripentylsilyl, trihexylsilyl, pentyldimethylsilyl, hexyldimethylsilyl, octyldimethylsilyl, and decyldimethylsilyl. Specific examples of the organothio group include alkylthio groups having 1 to 12 carbon atoms, such as methylthio, ethylthio, propylthio, butylthio, pentylthio, hexylthio, heptylthio, octylthio, nonylthio, decylthio, and dodecylthio. Specific examples of the acyl group include acyl groups having 1 to 10 carbon atoms, such as formyl, acetyl, propionyl, butyryl, isobutyryl, valeryl, isovaleryl, and benzoyl.

[0111] The monovalent hydrocarbon group, organooxy group, organoamino group, organosilyl group, organothio group and acyl group preferably have 1 to 8 carbon atoms.

[0112] Among these substituents, a fluorine atom, a sulfonic acid group, an alkyl group, an organoxy group, and an organosilyl group are more preferred.

[0113] In formula (B1), A 02 is —O—, —S—, or —NH—. Of these, —O— is preferred because it is easy to synthesize.

[0114] In formula (B1), A 03is a (q+1)-valent aromatic group having 6 to 20 carbon atoms. The (q+1)-valent aromatic group is a group obtained by removing (q+1) hydrogen atoms on the aromatic ring from an aromatic compound having 6 to 20 carbon atoms. In the present invention, the aromatic compound means an aromatic hydrocarbon or an aromatic heterocyclic compound. Examples of the aromatic compound include benzene, toluene, xylene, biphenyl, naphthalene, anthracene, pyrene, etc., and among these, A 3 The aromatic group represented by the formula (I) is preferably a group derived from naphthalene or anthracene.

[0115] In formulas (B1) and (B1′), X 1 is an alkylene group having 2 to 5 carbon atoms, and this alkylene group may have -O-, -S- or a carbonyl group between its carbon atoms (carbon-carbon bond), and some or all of its hydrogen atoms may be further substituted with alkyl groups having 1 to 20 carbon atoms. 1 Preferred examples of the alkyl group include ethylene, trimethylene, methyleneoxymethylene, and methylenethiomethylene groups, and some or all of the hydrogen atoms in these groups may be further substituted with an alkyl group having 1 to 20 carbon atoms. Examples of this alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, and bicyclohexyl groups.

[0116] In formulas (B1) and (B1′), X 2 is a single bond, —O—, —S—, or NR—. R is a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. As this monovalent hydrocarbon group, an alkyl group such as a methyl, ethyl, or n-propyl group is preferred. X 2 is preferably a single bond, —O— or —S—, more preferably a single bond or —O—.

[0117] In formulas (B1) and (B1′), X 3is a monovalent hydrocarbon group having 1 to 20 carbon atoms, which may be substituted. This monovalent hydrocarbon group may be linear, branched, or cyclic, and specific examples thereof include alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, and bicyclohexyl groups; vinyl, 1-propenyl, 2-propenyl, isopropenyl, 1-methyl-2-propenyl, and 1-butene. Examples of such groups include alkenyl groups having 2 to 20 carbon atoms, such as phenyl, 2-butenyl, 3-butenyl, and hexenyl; aryl groups having 6 to 20 carbon atoms, such as phenyl, xylyl, tolyl, 1-naphthyl, 2-naphthyl, 1-anthryl, 2-anthryl, 9-anthryl, 1-phenanthryl, 2-phenanthryl, 3-phenanthryl, 4-phenanthryl, 9-phenanthryl, 2-biphenylyl, 3-biphenylyl, and 4-biphenylyl; and aralkyl groups having 7 to 20 carbon atoms, such as benzyl, phenylethyl, and phenylcyclohexyl. Furthermore, some or all of the hydrogen atoms of the monovalent hydrocarbon groups may be further substituted with a substituent. Examples of such substituents include A 01 The same as those mentioned in the description of X. 3 As the alkyl group, an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms is preferred.

[0118] In formulas (B1) and (B1′), s is an integer satisfying 1≦s≦4, preferably 2. q is an integer satisfying 1≦q≦4, preferably 2.

[0119] The arylsulfonate ester compounds represented by formulas (B1) and (B1') exhibit high solubility in a wide range of solvents, including low-polarity solvents, making it possible to adjust the physical properties of the solution using a wide variety of solvents, resulting in excellent coating properties. Therefore, it is preferable to apply the compound in the form of a sulfonate ester and generate sulfonic acid during drying or baking of the coating film. The temperature at which sulfonic acid is generated from the sulfonate ester is preferably stable at room temperature and below the baking temperature, so is preferably 40 to 260°C. Furthermore, considering high stability in the varnish and ease of desorption during baking, a temperature of 80 to 230°C is preferred, and 120 to 180°C is more preferred.

[0120] The arylsulfonic acid ester compound represented by formula (B1) is preferably one represented by any one of the following formulae (B1-1) to (B1-3).

[0121]

[0122] In formula (B1-1), A 11 A is an s-valent group derived from perfluorobiphenyl (i.e., a group obtained by removing s fluorine atoms from perfluorobiphenyl). 12 is —O— or —S—, with —O— being preferred. 13 is a (q+1)-valent group derived from naphthalene or anthracene (i.e., a group obtained by removing (q+1) hydrogen atoms from naphthalene or anthracene), with groups derived from naphthalene being preferred.

[0123] In formula (B1-1), R s1 ~R s4 are each independently a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms, and R s5 is an optionally substituted monovalent hydrocarbon group having 2 to 20 carbon atoms.

[0124] Specific examples of the linear or branched alkyl group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-hexyl, etc. Among these, alkyl groups having 1 to 3 carbon atoms are preferred.

[0125] The monovalent hydrocarbon group having 2 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include alkyl groups such as ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and tert-butyl; and aryl groups such as phenyl, naphthyl, and phenanthryl.

[0126] R s1 ~R s4 Among them, R s1 or R s3 is preferably a linear alkyl group having 1 to 3 carbon atoms, and the remainder is preferably a hydrogen atom. s1 is a linear alkyl group having 1 to 3 carbon atoms, and R s2 ~R s4 is preferably a hydrogen atom. The linear alkyl group having 1 to 3 carbon atoms is preferably a methyl group. s5 As the alkyl group, a linear alkyl group having 2 to 4 carbon atoms or a phenyl group is preferred.

[0127] In formula (B1-1), s is an integer that satisfies 1≦s≦4, and is preferably 2. q is an integer that satisfies 1≦q≦4, and is preferably 2.

[0128] In formula (B1-2), A 14 is an s-valent hydrocarbon group having 6 to 20 carbon atoms and containing one or more aromatic rings, which may be substituted. The s-valent hydrocarbon group is a group obtained by removing s hydrogen atoms from a hydrocarbon having 6 to 20 carbon atoms and containing one or more aromatic rings. Examples of the hydrocarbon include benzene, toluene, xylene, ethylbenzene, biphenyl, naphthalene, anthracene, and phenanthrene.

[0129] In addition, some or all of the hydrogen atoms of the hydrocarbon group may be further substituted with a substituent, and such substituents include halogen atoms (fluorine atom, chlorine atom, bromine atom, iodine atom), nitro, cyano, hydroxy, amino, silanol, thiol, carboxy, sulfonate ester, phosphoric acid, phosphate ester, ester, thioester, amide, monovalent hydrocarbon, organooxy, organoamino, organosilyl, organothio, acyl, and sulfo groups. 14 As the alkyl group, groups derived from benzene, biphenyl, etc. are preferred.

[0130] In formula (B1-2), A 15 is —O— or —S—, with —O— being preferred.

[0131] In formula (B1-2), A 16 is a (q+1)-valent aromatic hydrocarbon group having 6 to 20 carbon atoms. The (q+1)-valent aromatic hydrocarbon group is a group obtained by removing (q+1) hydrogen atoms from the aromatic ring of an aromatic hydrocarbon compound having 6 to 20 carbon atoms. Examples of this aromatic hydrocarbon compound include benzene, toluene, xylene, biphenyl, naphthalene, anthracene, pyrene, etc. Among these, A 16 As the alkyl group, a group derived from naphthalene or anthracene is preferred, and a group derived from naphthalene is more preferred.

[0132] In formula (B1-2), R s6 and R s7 are each independently a hydrogen atom or a linear or branched monovalent aliphatic hydrocarbon group. s8 is a linear or branched monovalent aliphatic hydrocarbon group, provided that R s6 , R s7 and R s8 The total number of carbon atoms in R is 6 or more. s6 , R s7 and R s8 The upper limit of the total number of carbon atoms is not particularly limited, but is preferably 20 or less, and more preferably 10 or less.

[0133] Specific examples of the linear or branched monovalent aliphatic hydrocarbon group include alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-hexyl, n-octyl, 2-ethylhexyl, and decyl groups; and alkenyl groups having 2 to 20 carbon atoms, such as vinyl, 1-propenyl, 2-propenyl, isopropenyl, 1-methyl-2-propenyl, 1-butenyl, 2-butenyl, 3-butenyl, and hexenyl groups.

[0134] R s6 is preferably a hydrogen atom, and R s7 and R s8 is preferably an alkyl group having 1 to 6 carbon atoms. s7 and R s8 may be the same or different.

[0135] In formula (B1-2), s is an integer that satisfies 1≦s≦4, and is preferably 2. q is an integer that satisfies 1≦q≦4, and is preferably 2.

[0136] In formula (B1-3), R s9 ~R s13 are each independently a hydrogen atom, a nitro group, a cyano group, a halogen atom, an alkyl group having 1 to 10 carbon atoms, a halogenated alkyl group having 1 to 10 carbon atoms, or a halogenated alkenyl group having 2 to 10 carbon atoms.

[0137] The alkyl group having 1 to 10 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl groups.

[0138] The halogenated alkyl group having 1 to 10 carbon atoms is not particularly limited as long as it is a group in which some or all of the hydrogen atoms of an alkyl group having 1 to 10 carbon atoms have been substituted with halogen atoms. The halogenated alkyl group may be linear, branched, or cyclic, and specific examples thereof include trifluoromethyl, 2,2,2-trifluoroethyl, 1,1,2,2,2-pentafluoroethyl, 3,3,3-trifluoropropyl, 2,2,3,3,3-pentafluoropropyl, 1,1,2,2,3,3,3-heptafluoropropyl, 4,4,4-trifluorobutyl, 3,3,4,4,4-pentafluorobutyl, 2,2,3,3,4,4,4-heptafluorobutyl, and 1,1,2,2,3,3,4,4,4-nonafluorobutyl groups.

[0139] The halogenated alkenyl group having 2 to 10 carbon atoms is not particularly limited as long as it is a group in which some or all of the hydrogen atoms of an alkenyl group having 2 to 10 carbon atoms have been substituted with halogen atoms. Specific examples thereof include perfluorovinyl, perfluoro-1-propenyl, perfluoro-2-propenyl, perfluoro-1-butenyl, perfluoro-2-butenyl, and perfluoro-3-butenyl groups.

[0140] Of these, R s9 As R, a nitro group, a cyano group, a halogenated alkyl group having 1 to 10 carbon atoms, a halogenated alkenyl group having 2 to 10 carbon atoms, etc. are preferred, a nitro group, a cyano group, a halogenated alkyl group having 1 to 4 carbon atoms, a halogenated alkenyl group having 2 to 4 carbon atoms, etc. are more preferred, and a nitro group, a cyano group, a trifluoromethyl group, a perfluoropropenyl group, etc. are even more preferred. s10 ~R s13 As the atom, a halogen atom is preferable, and a fluorine atom is more preferable.

[0141] In formula (B1-3), A 17 is —O—, —S— or —NH—, with —O— being preferred.

[0142] In formula (B1-3), A 18is a (q+1)-valent aromatic hydrocarbon group having 6 to 20 carbon atoms. The (q+1)-valent aromatic hydrocarbon group is a group obtained by removing (q+1) hydrogen atoms from the aromatic ring of an aromatic hydrocarbon compound having 6 to 20 carbon atoms. Examples of the aromatic hydrocarbon compound include benzene, toluene, xylene, biphenyl, naphthalene, anthracene, and pyrene. Among these, A 18 As the alkyl group, a group derived from naphthalene or anthracene is preferred, and a group derived from naphthalene is more preferred.

[0143] In formula (B1-3), R s14 ~R s17 are each independently a hydrogen atom or a linear or branched monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. The monovalent aliphatic hydrocarbon group may be linear, branched, or cyclic, and specific examples thereof include alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, and n-dodecyl; and alkenyl groups having 2 to 20 carbon atoms, such as vinyl, 1-propenyl, 2-propenyl, isopropenyl, 1-methyl-2-propenyl, 1-butenyl, 2-butenyl, 3-butenyl, and hexenyl. Of these, alkyl groups having 1 to 20 carbon atoms are preferred, alkyl groups having 1 to 10 carbon atoms are more preferred, and alkyl groups having 1 to 8 carbon atoms are even more preferred.

[0144] In formula (B1-3), R s18 represents a linear or branched monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, or OR s19 It is. s19 is an optionally substituted monovalent hydrocarbon group having 2 to 20 carbon atoms.

[0145] R s18 As the linear or branched monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms represented by R s14 ~R s17 Examples include those mentioned in the description of R. s18is a monovalent aliphatic hydrocarbon group, R s18 As the alkyl group, an alkyl group having 1 to 20 carbon atoms is preferable, an alkyl group having 1 to 10 carbon atoms is more preferable, and an alkyl group having 1 to 8 carbon atoms is even more preferable.

[0146] R s19 Examples of the monovalent hydrocarbon group having 2 to 20 carbon atoms represented by the formula (I) include the above-mentioned monovalent aliphatic hydrocarbon groups other than the methyl group, as well as aryl groups such as a phenyl group, a naphthyl group, and a phenanthryl group. s19 is preferably a linear alkyl group having 2 to 4 carbon atoms or a phenyl group. Examples of the substituent that the monovalent hydrocarbon group may have include a fluorine atom, an alkoxy group having 1 to 4 carbon atoms, a nitro group, and a cyano group.

[0147] In formula (B1-3), q is an integer that satisfies 1≦q≦4, and is preferably 2.

[0148] As the arylsulfonic acid ester compound represented by formula (B1-3), those represented by the following formula (B1-3-1) or (B1-3-2) are particularly preferred.

[0149]

[0150] In formulas (B1-3-1) and (B1-3-2), A 17 , A 18 , R s9 ~R s17 , R s19 and q have the same meaning as above. s20 is a linear or branched monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, and specific examples thereof include R s18 Examples of the above-mentioned methods are the same as those described above.

[0151] In the arylsulfonic acid ester compound represented by formula (B1-3-1), R s14 ~R s17 Among them, R s14 or R s16 is preferably a linear alkyl group having 1 to 3 carbon atoms, and the remainder is preferably a hydrogen atom. s14 is a linear alkyl group having 1 to 3 carbon atoms, and Rs15 ~R s17 is preferably a hydrogen atom. As the linear alkyl group having 1 to 3 carbon atoms, a methyl group is preferred. s19 As the alkyl group, a linear alkyl group having 2 to 4 carbon atoms or a phenyl group is preferred.

[0152] In the arylsulfonic acid ester compound represented by formula (B1-3-2), R s14 , R s16 and R s20 The total number of carbon atoms in R is preferably 6 or more. s14 , R s16 and R s20 The upper limit of the total number of carbon atoms in R is preferably 20 or less, more preferably 10 or less. s14 is preferably a hydrogen atom, and R s16 and R s20 is preferably an alkyl group having 1 to 6 carbon atoms. s16 and R s20 may be the same or different from each other.

[0153] The arylsulfonic acid ester compounds represented by formula (B1) may be used singly or in combination of two or more.

[0154] Specific examples of suitable aryl sulfonate compounds include, but are not limited to, those shown below.

[0155]

[0156]

[0157] The amount of the arylsulfonic acid ester compound used is preferably about 0.01 to 20.0, more preferably about 0.05 to 15, in terms of mole ratio per 1 part of the organic functional material such as a polythiophene derivative or an arylamine derivative.

[0158] The dopant material may also be a fluorinated aryl sulfonic acid polymer compound.

[0159] The fluorinated arylsulfonic acid polymer compound is characterized by containing a repeating unit represented by the following formula (F1):

[0160]

[0161] In formula (F1), Ar F represents a fluorinated arylene group. F The fluorinated arylene group of the formula (I) is not particularly limited as long as at least one hydrogen atom on the arylene group is substituted with a fluorine atom, but it is preferable that at least one of the remaining hydrogen atoms is substituted with an electron-withdrawing group other than a sulfo group. Examples of the electron-withdrawing group include halogen atoms such as fluorine atom, chlorine atom, bromine atom, and iodine atom; nitro group; cyano group; acyl group; carboxy group; carboxylic acid ester group; and acyl groups such as formyl group and acetyl group. In particular, Ar F The fluorinated arylene group is preferably an arylene group substituted with two or more fluorine atoms, and more preferably a perfluoroarylene group.

[0162] Ar F There is no particular limitation on the number of carbon atoms in the arylene group constituting Ar, but the number of carbon atoms is preferably 6 to 20, and more preferably 6 to 16. Specific examples thereof include 1,4-phenylene, 1,3-phenylene, 1,2-phenylene, 1,5-naphthylene, 1,7-naphthylene, 1,8-naphthylene, 2,6-naphthylene, 2,7-naphthylene, 4,4'-biphenylylene, and anthracenyl groups, with a phenylene group being preferred and a 1,4-phenylene group being more preferred. Therefore, Ar F As the alkyl group, a tetrafluorophenylene group is preferred, and a 2,3,5,6-tetrafluoro-1,4-phenylene group is more preferred.

[0163] X represents O, S, NH, CONH or NHCO, with O and S being preferred, and O being more preferred.

[0164] A preferred fluorinated arylsulfonic acid polymer compound of the present invention is one represented by the following formula (F1-1):

[0165] (In the formula, n1 represents an integer of 1 to 4.)

[0166] More preferred fluorinated arylsulfonic acid polymer compounds include those represented by the following formula (F1-2).

[0167] (In the formula, n1 represents an integer of 1 to 4.)

[0168] A more suitable fluorinated arylsulfonic acid polymer compound is one represented by the following formula (F1-3).

[0169]

[0170] Ar S has at least one SO3R on the ring w represents an aryl group having a group, and R w represents a hydrogen atom or an alkali metal atom such as Li, Na, or K, and is preferably a hydrogen atom. S There is no particular limitation on the number of carbon atoms in the aryl group constituting Ar, but it is preferably 6 to 30 carbon atoms, more preferably 6 to 20 carbon atoms, and even more preferably 6 to 12 carbon atoms. Specific examples thereof include phenyl, 1-naphthyl, 2-naphthyl, 1-anthryl, 2-anthryl, 9-anthryl, 1-phenanthryl, 2-phenanthryl, 3-phenanthryl, 4-phenanthryl, and 9-phenanthryl groups, with naphthyl groups being preferred, and 1-naphthyl groups being more preferred. S The number of SO3R groups contained in Ar may be one or more, but is preferably 2 to 4, and more preferably 2. S As the compound represented by the following formula (Ar S -1) to (Ar S -6).

[0171] (In the formula, R w represents the same meaning as above. n2 represents an integer of 2 to 4.

[0172] (In the formula, R w has the same meaning as above.)

[0173] (In the formula, R w has the same meaning as above.)

[0174] (In the formula, R w has the same meaning as above.)

[0175] The fluorinated arylsulfonic acid polymer compound of the present invention may be a polymer containing only a repeating unit represented by the above formula (1). However, from the viewpoint of increasing solubility in organic solvents, a polymer further containing a repeating unit represented by the following formula (F2) is preferred.

[0176]

[0177] In formula (F2), R' represents a monovalent organic group. Examples of this monovalent organic group include a monovalent hydrocarbon group, a heteroaryl group, and a -COOR" group (wherein R" represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms). There are no particular restrictions on the number of carbon atoms in the monovalent hydrocarbon group, but a carbon number of 1 to 20 is preferred, a carbon number of 6 to 20 is more preferred, and a carbon number of 6 to 10 is even more preferred. Specific examples thereof include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; and aryl groups such as phenyl, 1-naphthyl, 2-naphthyl, 1-anthryl, 2-anthryl, 9-anthryl, 1-phenanthryl, 2-phenanthryl, 3-phenanthryl, 4-phenanthryl, and 9-phenanthryl.

[0178] Specific examples of heteroaryl groups include heteroaryl groups having 2 to 20 carbon atoms, such as 2-thienyl, 3-thienyl, 2-furanyl, 3-furanyl, 2-oxazolyl, 4-oxazolyl, 5-oxazolyl, 3-isoxazolyl, 4-isoxazolyl, 5-isoxazolyl, 2-thiazolyl, 4-thiazolyl, 5-thiazolyl, 3-isothiazolyl, 4-isothiazolyl, 5-isothiazolyl, 2-imidazolyl, 4-imidazolyl, 2-pyridyl, 3-pyridyl, and 4-pyridyl groups.

[0179] Examples of the alkyl group having 1 to 10 carbon atoms for R″ include the same groups as those exemplified above, and among these, alkyl groups having 1 to 5 carbon atoms are preferred.

[0180] In addition, the monovalent hydrocarbon group, heteroaryl group, and alkyl group having 1 to 10 carbon atoms represented by R" may have some or all of their hydrogen atoms substituted with a substituent. Examples of such a substituent include a halogen atom, a cyano group, a nitro group, a carboxy group, a sulfo group, and a hydroxyl group. Examples of the halogen atom include the same atoms as those exemplified above.

[0181] Among these, in consideration of improving the device characteristics and life characteristics of an organic EL device obtained by using the fluorinated arylsulfonic acid polymer compound of the present invention as a dopant substance, R' is preferably an aryl group substituted with a halogen atom, more preferably a fluorinated aryl group, and even more preferably a perfluoroaryl group. In particular, R' is preferably a phenyl group substituted with a halogen atom, more preferably a fluorinated phenyl group, and even more preferably a perfluorophenyl group.

[0182] When the fluorinated arylsulfonic acid polymer compound of the present invention contains a repeating unit represented by formula (F2), the content ratio of the unit of formula (F1) to the unit of formula (F2) is not particularly limited. However, in consideration of improving device characteristics when used as a dopant substance, the molar ratio of formula (F1):formula (F2) is preferably from 10:1 to 1:10, more preferably from 5:1 to 1:5, even more preferably from 3:1 to 1:3, and still more preferably 1:1.

[0183] The molecular weight of the fluorinated arylsulfonic acid polymer compound of the present invention is not particularly limited, but from the viewpoint of improving heat resistance and ensuring solubility in solvents, the weight average molecular weight Mw is preferably 1,000 to 50,000, more preferably 1,500 to 10,000, and even more preferably 2,000 to 10,000. The molecular weight distribution (Mw / Mn) is preferably 1 to 3, more preferably 1 to 2. The weight average molecular weight is a value measured by gel permeation chromatography (GPC) using polyethylene oxide as a standard sample.

[0184] The fluorinated arylsulfonic acid polymer compound of the present invention can be obtained by polymerizing a monomer represented by the following formula (F1A) and, if necessary, a monomer represented by the following formula (F2A) in the presence of a solvent and a radical polymerization initiator by a known radical polymerization method. In this case, two or more types of monomers represented by formula (F1A) may be used in combination, and two or more types of monomers represented by formula (F2A) may be used in combination.

[0185] (In the formula, Ar F , Ar S , X and R f1 has the same meaning as above.)

[0186] Heteropolyacids can also be suitably used as dopant substances. Heteropolyacids are polyacids that have a structure in which a heteroatom is located at the center of the molecule, typically represented by a Keggin-type chemical structure shown in formula (D1) or a Dawson-type chemical structure shown in formula (D2), and are formed by condensing an isopolyacid, which is an oxyacid of vanadium (V), molybdenum (Mo), tungsten (W), or the like, with an oxyacid of a different element. Examples of such oxyacids of different elements include oxyacids of silicon (Si), phosphorus (P), and arsenic (As).

[0187]

[0188] Specific examples of heteropolyacids include phosphomolybdic acid, silicomolybdic acid, phosphotungstic acid, silicotungstic acid, and phosphotungstomolybdic acid, which may be used alone or in combination of two or more. The heteropolyacids used in the present invention are commercially available or can be synthesized by known methods. In particular, when only one type of heteropolyacid is contained, it is preferable that the one type of heteropolyacid contains tungsten. That is, phosphotungstic acid, silicotungstic acid, phosphotungstomolybdic acid, and the like are preferred, with phosphotungstic acid and silicotungstic acid being more preferred.

[0189] In addition, heteropolyacids can be used in the present invention even if they have a large or small number of elements in the structure represented by the general formula in quantitative analysis such as elemental analysis, as long as they are commercially available or appropriately synthesized according to a known synthesis method. That is, for example, phosphotungstic acid is generally represented by the chemical formula H3(PW 12 O 40 )·nHO, but whether the number of P (phosphorus), O (oxygen), or W (tungsten) in this formula is large or small in quantitative analysis, it can be used in the present invention as long as it is commercially available or appropriately synthesized according to a known synthesis method. In this case, the mass of the heteropolyacid specified in the present invention does not refer to the mass of pure phosphotungstic acid (phosphotungstic acid content) in a synthesized or commercially available product, but rather refers to the total mass, including water of hydration and other impurities, in a form available as a commercially available product or in a form that can be isolated by a known synthesis method.

[0190] The amount of heteropolyacid used can be about 0.001 to 50.0 parts by mass per 1 part of the charge transporting substance such as a polythiophene derivative or an arylamine derivative, but is preferably about 0.01 to 20.0 parts, and more preferably about 0.1 to 10.0 parts.

[0191] [5] Amine Compound The charge-transporting varnish of the present invention may contain an amine compound for the purpose of improving the dispersibility or solubility of the charge-transporting substance, such as a polythiophene derivative or its amine adduct. Such an amine compound is not particularly limited as long as it is soluble in at least one solvent used in the varnish, and one type may be used alone, or two or more types may be used.

[0192] Specific examples of the primary amine compound include methylamine, ethylamine, n-propylamine, isopropylamine, 3-ethoxypropylamine, n-butylamine, isobutylamine, s-butylamine, t-butylamine, n-pentylamine, n-hexylamine, n-heptylamine, n-octylamine, 2-ethylhexylamine, n-nonylamine, n-decylamine, n-undecylamine, n-dodecylamine, n-tridecylamine, n-tetradecylamine, and n-pentadecylamine. monoalkylamine compounds such as aniline, n-hexadecylamine, n-heptadecylamine, n-octadecylamine, n-nonadecylamine, and n-eicosanylamine; and monoarylamine compounds such as aniline, tolylamine, 1-naphthylamine, 2-naphthylamine, 1-anthrylamine, 2-anthrylamine, 9-anthrylamine, 1-phenanthrylamine, 2-phenanthrylamine, 3-phenanthrylamine, 4-phenanthrylamine, and 9-phenanthrylamine.

[0193] Specific examples of secondary amine compounds include N-ethylmethylamine, N-methyl-n-propylamine, N-methylisopropylamine, N-methyl-n-butylamine, N-methyl-s-butylamine, N-methyl-t-butylamine, N-methylisobutylamine, diethylamine, N-ethyl-n-propylamine, N-ethylisopropylamine, N-ethyl-n-butylamine, N-ethyl-s-butylamine, N-ethyl-t-butylamine, dipropylamine, N-n-propylisopropylamine, and N-n-propyl N-n-butylamine, N-n-propyl-s-butylamine, diisopropylamine, N-n-butylisopropylamine, N-t-butylisopropylamine, di(n-butyl)amine, di(s-butyl)amine, diisobutylamine, aziridine (ethyleneimine), 2-methylaziridine (propyleneimine), 2,2-dimethylaziridine, azetidine (trimethyleneimine), 2-methylazetidine, pyrrolidine, 2-methylpyrrolidine, 3-methylpyrrolidine, 2,5-dimethylpyrrolidine, piperidine, 2,6-di Dialkylamine compounds such as methylpiperidine, 3,5-dimethylpiperidine, 2,2,6,6-tetramethylpiperidine, hexamethyleneimine, heptamethyleneimine, and octamethyleneimine; diphenylamine, N-phenyl-1-naphthylamine, N-phenyl-2-naphthylamine, 1,1'-dinaphthylamine, 2,2'-dinaphthylamine, 1,2'-dinaphthylamine, carbazole, 7H-benzo[c]carbazole, 11H-benzo[a]carbazole, 7H-dibenzo[c,g]carbazole, 13H-di Examples thereof include diarylamine compounds such as benzo[a,i]carbazole; and alkylarylamine compounds such as N-methylaniline, N-ethylaniline, N-n-propylaniline, N-isopropylaniline, N-n-butylaniline, N-s-butylaniline, N-isobutylaniline, N-methyl-1-naphthylamine, N-ethyl-1-naphthylamine, N-n-propyl-1-naphthylamine, indoline, isoindoline, 1,2,3,4-tetrahydroquinoline, and 1,2,3,4-tetrahydroisoquinoline.

[0194] Specific examples of the tertiary amine compound include N,N-dimethylethylamine, N,N-dimethyl-n-propylamine, N,N-dimethylisopropylamine, N,N-dimethyl-n-butylamine, N,N-dimethyl-s-butylamine, N,N-dimethyl-t-butylamine, N,N-dimethylisobutylamine, N,N-diethylmethylamine, N-methyldi(n-propyl)amine, N-methyldiisopropylamine, N-methyldi(n-butyl)amine, N-methyldiisobutylamine, triethylamine, N,N-diethyl-n-butylamine, N,N-diisopropylethylamine, and N,N-di(n-butyl)ethylamine. trialkylamine compounds such as tri(n-propyl)amine, tri(i-propyl)amine, tri(n-butyl)amine, tri(i-butyl)amine, 1-methylacetidine, 1-methylpyrrolidine, and 1-methylpiperidine; triarylamine compounds such as triphenylamine; alkyldiarylamine compounds such as N-methyldiphenylamine, N-ethyldiphenylamine, 9-methylcarbazole, and 9-ethylcarbazole; and dialkylarylamine compounds such as N,N-diethylaniline, N,N-di(n-propyl)aniline, N,N-di(i-propyl)aniline, and N,N-di(n-butyl)aniline.

[0195] In particular, when the charge-transporting varnish of the present invention contains an amine compound, the amine compound preferably contains a primary amine compound, and more preferably contains a monoalkylamine, particularly a monoalkylamine having from 2 to 20 carbon atoms, because this has an excellent ability to improve the dispersibility and solubility of the charge-transporting substance, such as the polythiophene derivative or its amine adduct, used in the present invention.

[0196] When the charge-transporting varnish of the present invention contains an amine compound, the content thereof is usually about 10 times or less by mass relative to the charge-transporting substance such as the polythiophene derivative or its amine adduct used in the present invention.

[0197] [6] Charge-Transporting Varnish and Charge-Transporting Thin Film The viscosity of the charge-transporting varnish is determined appropriately depending on the thickness of the thin film to be produced and the solid content concentration, but is typically 1 to 50 mPa·s at 25°C. In the present invention, the solid content refers to the components contained in the charge-transporting varnish other than the solvent. The solid content concentration of the charge-transporting varnish is determined appropriately taking into account the viscosity and surface tension of the varnish, the thickness of the thin film to be produced, and the like, but is typically about 0.1 to 10.0% by mass. In consideration of improving the coatability of the varnish, it is preferably about 0.5 to 5.0% by mass, and more preferably about 1.0 to 4.0% by mass.

[0198] The method for preparing the charge-transporting varnish is not particularly limited, but examples include a method in which a charge-transporting substance and, if necessary, a dopant substance are dissolved in a high-polarity solvent, and then a low-polarity solvent and surface-treated metal oxide nanoparticles are added thereto; and a method in which a high-polarity solvent and a low-polarity solvent are mixed, and then a charge-transporting substance and, if necessary, a dopant substance are dissolved therein, and then surface-treated metal oxide nanoparticles are added thereto.

[0199] In particular, when preparing a charge-transporting varnish, from the viewpoint of obtaining a thin film with higher flatness with good reproducibility, it is desirable to dissolve the charge-transporting substance and, if necessary, the dopant substance in an organic solvent, and then filter the resulting solution using a filter on the order of submicrometers before use.

[0200] The charge-transporting varnish described above can be used to easily produce a charge-transporting thin film, and is therefore suitable for use in producing electronic devices, particularly organic EL devices and quantum dot EL devices. In this case, the charge-transporting thin film can be formed by applying the charge-transporting varnish described above to a substrate and baking it. The method for applying the varnish is not particularly limited, and examples include dipping, spin coating, transfer printing, roll coating, brush coating, inkjet coating, spraying, and slit coating. It is preferable to adjust the viscosity and surface tension of the varnish depending on the application method.

[0201] Furthermore, the atmosphere in which the charge-transporting varnish is baked after application is not particularly limited, and a thin film with a uniform film surface and high charge transport properties can be obtained not only in an air atmosphere but also in an inert gas such as nitrogen or in a vacuum. However, depending on the type of dopant substance used, a thin film with charge transport properties can sometimes be reproducibly obtained by baking the varnish in an air atmosphere.

[0202] The baking temperature is appropriately determined within a range of about 100 to 260° C., taking into consideration the use of the resulting thin film, the degree of charge transport property to be imparted to the resulting thin film, the type and boiling point of the solvent, etc. For example, when the resulting thin film is used as a hole injection layer of an organic EL device or a quantum dot EL device, the baking temperature is preferably about 140 to 250° C., and more preferably about 145 to 240° C. During baking, the temperature may be changed in two or more stages for the purpose of achieving more uniform film formation or promoting a reaction on the substrate, and heating may be performed using an appropriate device such as a hot plate or an oven.

[0203] The thickness of the charge transport thin film is not particularly limited, but is preferably 5 to 300 nm when used as a functional layer provided between an anode and a light-emitting layer, such as a hole injection layer, hole transport layer, or hole injection transport layer, of an organic EL device or a quantum dot EL device. Methods for changing the film thickness include changing the solids concentration in the varnish or changing the amount of solution on the substrate during application.

[0204] [7] Organic EL Devices and Quantum Dot EL Devices When the above-described charge transport thin film is applied to an organic EL device or a quantum dot EL device, the organic EL device or the quantum dot EL device can be configured to include the above-described charge transport thin film between a pair of electrodes constituting the organic EL device or the quantum dot EL device. Representative configurations of organic EL devices or quantum dot EL devices include, but are not limited to, the following (a) to (f). In the configurations described below, an electron blocking layer or the like can be provided between the light-emitting layer and the anode, and a hole blocking layer or the like can be provided between the light-emitting layer and the cathode, as necessary. Furthermore, the hole injection layer, the hole transport layer, or the hole injection transport layer may also function as an electron blocking layer, and the electron injection layer, the electron transport layer, or the electron injection transport layer may also function as a hole blocking layer. Furthermore, an optional functional layer can be provided between each layer as necessary. (a) anode / hole injection layer / hole transport layer / light-emitting layer / electron transport layer / electron injection layer / cathode (b) anode / hole injection layer / hole transport layer / light-emitting layer / electron injection transport layer / cathode (c) anode / hole injection transport layer / light-emitting layer / electron transport layer / electron injection layer / cathode (d) anode / hole injection transport layer / light-emitting layer / electron injection transport layer / cathode (e) anode / hole injection layer / hole transport layer / light-emitting layer / cathode (f) anode / hole injection transport layer / light-emitting layer / cathode

[0205] The terms "hole injection layer," "hole transport layer," and "hole injection transport layer" refer to layers formed between the light-emitting layer and the anode, which have the function of transporting holes from the anode to the light-emitting layer. When only one layer of a hole-transporting material is provided between the light-emitting layer and the anode, it is the "hole injection transport layer." When two or more layers of a hole-transporting material are provided between the light-emitting layer and the anode, the layer closest to the anode is the "hole injection layer," and the remaining layers are "hole transport layers." In particular, the hole injection (transport) layer is a thin film that is excellent not only in the ability to accept holes from the anode but also in the ability to inject holes into the hole transport (light-emitting) layer.

[0206] The terms "electron injection layer," "electron transport layer," and "electron injection transport layer" refer to layers formed between the light-emitting layer and the cathode, which transport electrons from the cathode to the light-emitting layer. When only one layer of an electron-transporting material is provided between the light-emitting layer and the cathode, it is the "electron injection transport layer." When two or more layers of an electron-transporting material are provided between the light-emitting layer and the cathode, the layer closest to the cathode is the "electron injection layer," and the remaining layers are "electron transport layers." The term "light-emitting layer" refers to an organic layer that emits light. When a doping system is employed, it contains a host material and a dopant material. In this case, the host material primarily promotes the recombination of electrons and holes and confines excitons within the light-emitting layer, while the dopant material efficiently emits the excitons obtained by recombination. In the case of phosphorescent devices, the host material primarily confines excitons generated by the dopant within the light-emitting layer.

[0207] The charge-transporting thin film of the present invention can be used as a functional layer provided between an anode and an emitting layer in an organic EL device or a quantum dot EL device, and is suitable as a hole-injection layer, a hole-transport layer, or a hole-injection-transport layer, more suitable as a hole-injection layer or a hole-transport layer, and even more suitable as a hole-injection layer.

[0208] Materials and methods for producing an EL device using the charge-transport varnish of the present invention include, but are not limited to, those listed below. An example of a method for producing an OLED device having a hole-injection layer made of a thin film obtained from the charge-transport varnish of the present invention is as follows. It is preferable to preliminarily clean the electrodes with alcohol, pure water, or the like, or to perform surface treatments such as UV ozone treatment or oxygen-plasma treatment, to the extent that they do not adversely affect the electrodes. A hole-injection layer made of the charge-transport thin film of the present invention is formed on an anode substrate by the above-described method. This substrate is then introduced into a vacuum deposition apparatus, and a hole-transport layer, a light-emitting layer, an electron-transport layer, an electron-transport layer / hole-blocking layer, and a cathode metal are sequentially deposited by vapor deposition. Alternatively, instead of forming the hole-transport layer and the light-emitting layer by vapor deposition in this method, these layers are formed by a wet process using a hole-transport layer-forming composition containing a hole-transport polymer and a light-emitting layer-forming composition containing a light-emitting polymer. If necessary, an electron-blocking layer may be provided between the light-emitting layer and the hole-transport layer.

[0209] Examples of anode materials include transparent electrodes such as indium tin oxide (ITO) and indium zinc oxide (IZO), and metal anodes made of metals such as aluminum or alloys thereof, preferably those that have undergone planarization. Polythiophene derivatives and polyaniline derivatives with high charge transport properties can also be used. Other metals that can be used to make metal anodes include, but are not limited to, gold, silver, copper, indium, and alloys thereof.

[0210] Examples of materials for forming the hole transport layer include triarylamines such as (triphenylamine) dimer derivatives, [(triphenylamine) dimer] spiro dimer, N,N'-bis(naphthalen-1-yl)-N,N'-bis(phenyl)-benzidine (α-NPD), 4,4',4"-tris[3-methylphenyl(phenyl)amino]triphenylamine (m-MTDATA), and 4,4',4"-tris[1-naphthyl(phenyl)amino]triphenylamine (1-TNATA), and oligothiophenes such as 5,5"-bis-{4-[bis(4-methylphenyl)amino]phenyl}-2,2':5',2"-terthiophene (BMA-3T).

[0211] Examples of materials for forming the light-emitting layer include, but are not limited to, low-molecular-weight light-emitting materials such as metal complexes (e.g., aluminum complexes of 8-hydroxyquinoline), metal complexes of 10-hydroxybenzo[h]quinoline, bisstyrylbenzene derivatives, bisstyrylarylene derivatives, metal complexes of (2-hydroxyphenyl)benzothiazole, and silole derivatives; and systems in which a light-emitting material and an electron transfer material are mixed with a polymer compound (e.g., poly(p-phenylenevinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene], poly(3-alkylthiophene), or polyvinylcarbazole. Furthermore, when the light-emitting layer is formed by vapor deposition, it may be co-deposited with a light-emitting dopant. Examples of light-emitting dopants include, but are not limited to, metal complexes (e.g., tris(2-phenylpyridine)iridium(III) (Ir(ppy)), naphthacene derivatives (e.g., rubrene), quinacridone derivatives, and fused polycyclic aromatic rings (e.g., perylene).

[0212] Examples of materials for forming the electron transport layer / hole blocking layer include, but are not limited to, oxydiazole derivatives, triazole derivatives, phenanthroline derivatives, phenylquinoxaline derivatives, benzimidazole derivatives, and pyrimidine derivatives.

[0213] Materials for forming the electron injection layer include, but are not limited to, metal oxides such as lithium oxide (LiO), magnesium oxide (MgO), and alumina (AlO), and metal fluorides such as lithium fluoride (LiF) and sodium fluoride (NaF). Cathode materials include, but are not limited to, aluminum, magnesium-silver alloys, and aluminum-lithium alloys. Materials for forming the electron blocking layer include, but are not limited to, tris(phenylpyrazole)iridium.

[0214] Examples of hole transporting polymers include poly[(9,9-dihexylfluorenyl-2,7-diyl)-co-(N,N'-bis{p-butylphenyl}-1,4-diaminophenylene)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(N,N'-bis{p-butylphenyl}-1,1'-biphenylene-4,4-diamine)], poly[(9,9-bis{1'-penten-5'-yl}fluorenyl-2,7-diyl)-co-(N,N'-bis{p-butylphenyl}-1,4-diaminophenylene)], and poly[N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)-benzidine]-endcapped with Examples of the polysilcisquinoxane include poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'(N-(4-sec-butylphenyl)diphenylamine)], poly(9-vinylcarbazole), and poly(4-butyl-N,N-diphenylaniline).

[0215] Examples of the light-emitting polymer include polyfluorene derivatives such as poly(9,9-dialkylfluorene) (PDAF), polyphenylenevinylene derivatives such as poly(2-methoxy-5-(2'-ethylhexoxy)-1,4-phenylenevinylene) (MEH-PPV), polythiophene derivatives such as poly(3-alkylthiophene) (PAT), and polyvinylcarbazole (PVCz).

[0216] The quantum dot material may include at least one semiconductor material selected from the group consisting of II-VI semiconductors, III-V semiconductors, I-III-VI semiconductors, IV semiconductors, and I-II-IV-VI semiconductors. Specific examples of the semiconductor material include CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, and CdHgZnT. e, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe; GaN, GaP, GaAs, G aSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, Ga InNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb; SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnS Examples of suitable gallium arsenide include, but are not limited to, Cu ...

[0217] As described above, the charge-transporting varnish of the present invention is suitably used for forming functional layers such as a hole injection layer, a hole transport layer, and a hole injection transport layer that are provided between an anode and a light-emitting layer in an organic EL device or a quantum dot EL device. However, it can also be used for forming charge-transporting thin films in electronic devices such as organic photoelectric conversion devices, organic thin-film solar cells, organic perovskite photoelectric conversion devices, organic integrated circuits, organic field-effect transistors, organic thin-film transistors, organic light-emitting transistors, organic optical inspectors, organic photoreceptors, organic field quenching devices, light-emitting electrochemical cells, quantum lasers, organic laser diodes, and organic plasmon light-emitting devices.

[0218] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The apparatus used is as follows.

[0219] (1) Application of charge transport ink: Spin coater MS-A100 manufactured by Mikasa Co., Ltd. (2) 1 H-NMR: AVANCE III HD 500MHz Nuclear Magnetic Resonance Spectrometer manufactured by Bruker (3) Measurement of ionization potential of charge transport thin film: AC-3 manufactured by Riken Keiki Co., Ltd. (4) Fabrication of hole-only device (HOD): C-E2L1G1-N Multifunctional Vapor Deposition System manufactured by Choshu Sangyo Co., Ltd. (5) Measurement of electrical properties of hole-only device (HOD): Multi-channel IVL measurement device manufactured by EHC Co., Ltd.

[0220] [1] Synthesis of Compounds [Synthesis Example 1] According to the methods described in Production Examples 2-1 and 2-2 of WO 2020 / 203407, an amine adduct of a polythiophene derivative, which is a polymer containing a repeating unit represented by the following formula (1a), was synthesized.

[0221] (wherein a to d are the same as above.)

[0222] Synthesis Example 2 An arylsulfonic acid compound represented by formula (b-1) was synthesized according to the method described in WO 2006 / 025342.

[0223]

[0224] [Synthesis Example 3]: [3-(1,1,2,3,3,3-hexafluoropropoxy)propyl]trimethoxysilane

[0225] A 50 mL flask was charged with (2H-perfluoropropyl)-2-propenyl ether (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (2 g, 9.61 mmol). The atmosphere in the flask was replaced with N2, and then toluene (20 g) and 1,3-divinyltetramethyldisiloxane platinum(0) complex (2% toluene solution, manufactured by Sigma-Aldrich) (0.37 g, 0.019 mmol) were added and stirred. The solution was then cooled to 0°C, and trimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) (1.29 g, 0.011 mol) was added dropwise. The mixture was stirred at room temperature for 24 hours. After stirring, activated carbon (1.5 g) was added to the reaction mixture, which was stirred for 1 hour and then filtered. The toluene was distilled off from the resulting filtrate to obtain the target compound as a brown liquid (0.94 g, 2.85 mmol, yield 30%). 1 The H-NMR spectrum is shown below. 1 H-NMR (300MHz, CDCl3) δ4.80-4.72 (m, 1H), 3.97 (t, J = 6.5Hz, 2H), 3.58 (s, 9H), 1.81-1.76 (m, 2H), 0.69 (t, J = 8.3Hz, 2H).

[0226] [Synthesis Example 4]: 1,1,1-trifluoro-2-(trifluoromethyl)-5-(trimethoxysilyl)pentan-2-ol

[0227] A 50 mL flask was charged with 1,1,1-trifluoro-2-(trifluoromethyl)-4-penten-2-ol (Tokyo Chemical Industry Co., Ltd.) (2 g, 9.61 mmol). The atmosphere in the flask was replaced with N2, and then toluene (20 g) and 1,3-divinyltetramethyldisiloxane platinum(0) complex (2% toluene solution, Sigma-Aldrich) (0.37 g, 0.019 mmol) were added and stirred. The solution was then cooled to 0°C, and trimethoxysilane (Tokyo Chemical Industry Co., Ltd.) (1.29 g, 0.011 mol) was added dropwise, followed by stirring at room temperature for 24 hours. After stirring was completed, activated carbon (1.5 g) was added to the reaction mixture, which was stirred for 1 hour and then filtered. The toluene was distilled off from the resulting filtrate to obtain the target compound as a brown liquid (1.28 g, 3.87 mmol, 40% yield). 1 The H-NMR spectrum is shown below. 1 H-NMR (300MHz, CDCl3) δ4.42 (brs, 1H), 3.60 (s, 9H), 2.01 (t, J=7.8Hz, 2H), 1.76-1.70 (m, 2H), 0.76 (t, J=7.5Hz, 2H).

[0228] [2] Production of Surface-Treated Silica Sol [Production Example 1] 100 g of ST-OS (manufactured by Nissan Chemical Industries, Ltd.), which is a water-dispersed silica sol, and dipropylene glycol monomethyl ether (manufactured by Kanto Chemical Co., Ltd.; the same applies hereinafter) were placed in a recovery flask, and the water contained in the ST-OS was solvent-substituted with dipropylene glycol monomethyl ether using an evaporator, thereby obtaining a dipropylene glycol monomethyl ether-dispersed silica sol (solid content concentration: 15.9% by mass).

[0229] [Production Example 2] 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether were placed in a reaction vessel, and the solid content concentration was adjusted to 10.0 mass%. 0.34 g (2.5 mmol) of trimethoxy(methyl)silane (manufactured by Tokyo Chemical Industry Co., Ltd., the same applies hereinafter) was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 μm to obtain surface-treated silica sol A [solid content (surface-treated silica) concentration 10.6 mass%].

[0230] [Production Example 3] 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether were placed in a reaction vessel, and the solid content concentration was adjusted to 10.0 mass%. 0.49 g (2.5 mmol) of trimethoxy(3-methoxypropyl)silane (manufactured by Gelest, Inc.) was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 μm to obtain surface-treated silica sol B [solid content (surface-treated silica) concentration 10.9 mass%].

[0231] [Production Example 4] 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether were placed in a reaction vessel, and the solid content concentration was adjusted to 10.0 mass%. 0.41 g (2.5 mmol) of trimethoxy(propyl)silane (manufactured by Tokyo Chemical Industry Co., Ltd., the same applies hereinafter) was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 μm to obtain surface-treated silica sol C [solid content (surface-treated silica) concentration 10.7 mass%].

[0232] [Production Example 5] 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether were placed in a reaction vessel, and the solid content concentration was adjusted to 10.0 mass%. 0.57 g (2.5 mmol) of trimethoxy(4-methoxyphenyl)silane (Tokyo Chemical Industry Co., Ltd.) was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 μm to obtain surface-treated silica sol D [solid content (surface-treated silica) concentration 11.0 mass%].

[0233] [Production Example 6] 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether were placed in a reaction vessel, and the solid content concentration was adjusted to 10.0 mass%. 0.50 g (2.5 mmol) of trimethoxyphenylsilane (Tokyo Chemical Industry Co., Ltd.) was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 µm to obtain surface-treated silica sol E [solid content (surface-treated silica) concentration 10.9 mass%].

[0234] [Production Example 7] 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether were placed in a reaction vessel, and the solid content concentration was adjusted to 10.0 mass%. 0.26 g (2.5 mmol) of methoxytrimethylsilane (Tokyo Chemical Industry Co., Ltd.) was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 μm to obtain surface-treated silica sol F [solid content (surface-treated silica) concentration 10.4 mass%].

[0235] [Production Example 8] A reaction vessel was charged with 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether, and the solid content concentration was adjusted to 10.0 mass%. 0.83 g (2.5 mmol) of [3-(1,1,2,3,3,3-hexafluoropropoxy)propyl]trimethoxysilane obtained in Synthesis Example 3 was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 μm to obtain surface-treated silica sol G [solid content (surface-treated silica) concentration 11.5 mass%].

[0236] [Production Example 9] 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether were placed in a reaction vessel, and the solid content concentration was adjusted to 10.0 mass%. 0.55 g (2.5 mmol) of trifluoropropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-7103) was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 μm to obtain surface-treated silica sol H [solid content (surface-treated silica) concentration 11.0 mass%].

[0237] [Production Example 10] A reaction vessel was charged with 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether, and the solid content concentration was adjusted to 10.0 mass%. 0.82 g (2.5 mmol) of 1,1,1-trifluoro-2-(trifluoromethyl)-5-(trimethoxysilyl)pentan-2-ol obtained in Synthesis Example 4 was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 µm to obtain surface-treated silica sol I [solid content (surface-treated silica) concentration 11.4 mass%].

[0238] [Production Example 11] 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether were placed in a reaction vessel, and the solids concentration was adjusted to 10.0 mass%. 0.83 g (2.5 mmol) of trimethoxy[3-(perfluorophenyl)propyl]silane (manufactured by Gelest, Inc.) was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 μm to obtain surface-treated silica sol J [solids concentration (surface-treated silica) 11.5 mass%].

[0239] [Production Example 12] 31.4 g of the dipropylene glycol monomethyl ether-dispersed silica sol obtained in Production Example 1 and 18.6 g of dipropylene glycol monomethyl ether were placed in a reaction vessel, and the solid content concentration was adjusted to 10.0 mass%. 0.73 g (2.5 mmol) of dodecyltrimethoxysilane (Tokyo Chemical Industry Co., Ltd.) was added thereto, and the mixture was stirred at 60°C under nitrogen for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 μm to obtain surface-treated silica sol K [solid content (surface-treated silica) concentration 11.3 mass%].

[0240] [3] Preparation of composition for preparing varnish [Preparation Example 1] 1.0 g of the polythiophene derivative amine adduct obtained in Synthesis Example 1 was added to 16.9 g of 1,3-dimethyl-2-imidazolidinone (manufactured by Kanto Chemical Co., Ltd.; the same applies hereinafter) and 2.1 g of 3-ethoxypropylamine (manufactured by Tokyo Chemical Industry Co., Ltd.), and the mixture was stirred at 80°C for 3 hours using a hot stirrer to obtain a dark blue mixed solution.

[0241] Preparation Example 2 A 1,3-dimethyl-2-imidazolidinone solution containing 10% by mass of the arylsulfonic acid compound obtained in Synthesis Example 2 was prepared by stirring using a hot stirrer at 400 rpm and 50°C for 1 hour.

[0242] [4] Preparation of Silica Sol-Containing Charge-Transporting Varnish [Example 1-1] 1.98 g of 1,3-dimethyl-2-imidazolidinone, 3.37 g of dipropylene glycol (manufactured by Junsei Chemical Co., Ltd., the same applies hereinafter), and 1.35 g of dipropylene glycol monomethyl ether were placed in a recovery flask and stirred at room temperature for 30 minutes using a stirrer. Then, 0.45 g of the 1,3-dimethyl-2-imidazolidinone solution of the arylsulfonic acid compound obtained in Preparation Example 2 was added, and the mixture was stirred at room temperature for 30 minutes using a stirrer. Then, 0.6 g of the mixed solution obtained in Preparation Example 1 was added, and the mixture was stirred at room temperature for 30 minutes. Next, 2.25 g of the surface-treated silica sol A produced in Preparation Example 2 was added to the resulting mixed solution, and the mixture was stirred at room temperature for 30 minutes. The resulting mixture was filtered through a PP syringe filter with a pore size of 0.2 μm to obtain a charge-transporting varnish (solids concentration: 3.1% by mass).

[0243] Examples 1-2 to 1-10 Charge-transporting varnishes (solid content concentration: 3.1 to 3.3% by mass) were obtained in the same manner as in Example 1-1, except that the surface-treated silica sols B to J produced in Production Examples 3 to 11 were used instead of the surface-treated silica sol A produced in Production Example 2.

[0244] Comparative Example 1-1: 1.98 g of 1,3-dimethyl-2-imidazolidinone, 3.37 g of dipropylene glycol, and 2.18 g of dipropylene glycol monomethyl ether were placed in a recovery flask and stirred at room temperature for 30 minutes using a stirrer. Then, 0.45 g of the 1,3-dimethyl-2-imidazolidinone solution of the arylsulfonic acid compound obtained in Preparation Example 2 was added, and the mixture was stirred at room temperature for 30 minutes using a stirrer. Then, 0.6 g of the mixed solution obtained in Preparation Example 1 was added, and the mixture was stirred at room temperature for 30 minutes. Next, 1.42 g of the dipropylene glycol monomethyl ether-dispersed silica sol produced in Preparation Example 1 was added to the resulting mixed solution, and the mixture was stirred at room temperature for 30 minutes. The resulting mixture was filtered through a PP syringe filter with a pore size of 0.2 μm to obtain a charge-transporting varnish (solids concentration: 3.0% by mass).

[0245] Comparative Example 1-2: 1.98 g of 1,3-dimethyl-2-imidazolidinone, 3.37 g of dipropylene glycol (manufactured by Junsei Chemical Co., Ltd., the same applies hereinafter), and 1.35 g of dipropylene glycol monomethyl ether were placed in a recovery flask and stirred at room temperature for 30 minutes using a stirrer. Then, 0.45 g of the 1,3-dimethyl-2-imidazolidinone solution of arylsulfonic acid compound A obtained in Preparation Example 2 was added, and the mixture was stirred at room temperature for 30 minutes using a stirrer. Then, 0.6 g of the mixed solution obtained in Preparation Example 1 was added, and the mixture was stirred at room temperature for 30 minutes. Next, 2.25 g of the surface-treated silica sol K produced in Preparation Example 12 was added to the resulting mixed solution. However, a precipitate formed, and a uniform charge-transporting varnish could not be obtained.

[0246] [5] Preparation of Charge-Transporting Thin Film and Evaluation of Ionization Potential [Example 2-1] The charge-transporting varnish obtained in Example 1-1 was applied to an ITO substrate using a spin coater and then baked in air at 120°C for 1 minute. The substrate was then baked in air at 230°C for 15 minutes to form a uniform thin film with a thickness of 65 nm on the ITO substrate. The ITO substrate used was a 25 mm x 25 mm x 0.7 mm glass substrate with a 50 nm thick pattern of indium tin oxide (ITO) on the glass substrate. Surface impurities were removed using an O2 plasma cleaning device (150 W, 30 seconds) before use.

[0247] [Examples 2-2 to 2-10] A uniform thin film having a thickness of 65 nm was formed on an ITO substrate in the same manner as in Example 2-1, except that the charge-transporting varnish in Example 2-1 was changed to the charge-transporting varnish obtained in Examples 1-2 to 1-10.

[0248] Comparative Example 2-1 A uniform thin film having a thickness of 65 nm was formed on an ITO substrate in the same manner as in Example 2-1, except that the charge-transporting varnish in Example 2-1 was changed to the charge-transporting varnish obtained in Comparative Example 1-1.

[0249] The ionization potential (IP) of the thin film surface was measured using a photoelectron spectrometer (AC-3) for the charge-transporting thin films on the ITO substrates formed in Examples 2-1 to 2-10 and Comparative Example 2-1. The measurements were performed under conditions of a light intensity of 20 nW and a measurement range of 4.8 to 7.0 eV, and the ionization potential value was calculated from the threshold energy of electron emission. The values ​​(ΔIP) of (IP of Examples 2-1 to 2-10) minus (IP of Comparative Example 1-1) are shown in Table 1.

[0250]

[0251] As shown in Table 1, the thin films formed from the charge-transporting varnish using the surface-treated silica sol of the present invention (Examples 2-1 to 2-10) exhibited higher IP than the thin film formed from the charge-transporting varnish using the surface-treated silica sol (Comparative Example 2-1). Generally, the IP of an organic semiconductor material corresponds to the HOMO level. Therefore, it can be said that the thin films formed from the charge-transporting varnish using the surface-treated silica sol have a deeper HOMO than those formed from the surface-untreated silica sol. This is thought to be due to the fact that the use of the surface-treated silica sols exemplified in Production Examples 2 to 11 changes the interaction between the silica sol and the charge-transporting material and / or the dispersibility of the silica sol, resulting in a different surface state for the resulting charge-transporting thin film compared to the case where a surface-unmodified silica sol is used.

[0252] [6] Fabrication and Evaluation of Hole-Only Device (HOD) [Example 3-1] The charge-transporting varnish obtained in Example 1-1 was applied to an ITO substrate using a spin coater and then dried at 120°C for 1 minute in an air atmosphere. The substrate was then baked at 230°C for 15 minutes in an air atmosphere to form a uniform 65 nm thin film (hole injection layer) on the ITO substrate. A 25 mm x 25 mm x 0.7 mm glass substrate with a patterned 50 nm thick ITO film formed on its surface was used as the ITO substrate. Prior to use, impurities on the surface were removed using an O2 plasma cleaning device (150 W, 30 seconds). Next, onto the ITO substrate on which the thin film had been formed, an ink prepared by dissolving TFB (poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4′(N-(4-sec-butylphenyl)diphenylamine)]) (manufactured by Sigma-Aldrich), a common hole transport material, in dehydrated xylene (manufactured by Kanto Chemical Co., Inc.) to a solids concentration of 1.5% by mass was applied using a spin coater, and the ink was then dried at 120° C. for 1 minute under a nitrogen atmosphere. The ink was then baked at 200° C. for 30 minutes under a nitrogen atmosphere to form a uniform thin film (hole transport layer) with a thickness of 50 nm on the hole injection layer. The ITO substrate after the film formation was then subjected to a vacuum deposition apparatus (vacuum degree 1.0×10 -5A hole-only device was fabricated by forming a cathode by vapor deposition of aluminum using a vacuum evaporation system (Pa). The deposition was carried out at a deposition rate of 0.2 nm / sec to a thickness of 80 nm.

[0253] To prevent deterioration of characteristics due to the influence of oxygen, water, etc. in the air, the hole-only device was sealed with a sealing substrate before its characteristics were evaluated. Sealing was performed as follows. In a nitrogen atmosphere with an oxygen concentration of 2 ppm or less and a dew point of -76°C or less, the organic EL element was placed between sealing substrates, and the sealing substrates were bonded together with an adhesive (Moresco Moisture Cut WB90US(P) manufactured by MORESCO Corporation). At this time, a moisture scavenger (HD-071010W-40 manufactured by DYNIC Corporation) was placed inside the sealing substrate together with the organic EL element. The bonded sealing substrates were irradiated with UV light (wavelength: 365 nm, irradiation dose: 6,000 mJ / cm). 2 ) and then annealed at 80°C for 1 hour to harden the adhesive.

[0254] Examples 3-2 to 3-10 Hole-only devices were fabricated in the same manner as in Example 3-1, except that the charge-transporting varnish in Example 3-1 was changed to the charge-transporting varnishes obtained in Examples 1-2 to 1-10.

[0255] Comparative Example 3-1 A hole-only device was fabricated in the same manner as in Example 3-1, except that the charge-transporting varnish in Example 3-1 was changed to the charge-transporting varnish obtained in Comparative Example 1-1.

[0256] The current-voltage characteristics were evaluated for each of the devices of Examples 3-1 to 3-10 and Comparative Example 3-1. Specifically, the current density (mA / cm) was measured when a voltage was applied to the hole-only device from −5 V to +5 V in 0.25 V increments. 2 The current densities when a voltage of +5 V was applied to the elements of Examples 3-1 to 3-10 and Comparative Example 3-1 are shown in Table 2.

[0257]

[0258] As shown in Table 2, the current density when a voltage of +5 V was applied to the hole-only devices of Examples 3-1 to 3-10 all exhibited values ​​higher than the current density of the hole-only device prepared in Comparative Example 3-1. One of the reasons for this is considered to be that the thin film formed from the charge-transporting varnish using the surface-treated silica sol of the present invention has a deeper HOMO film surface than the thin film formed from the charge-transporting varnish using the non-surface-treated silica sol, which improves hole injection properties into the hole-transporting layer formed on top.

[0259] [7] Production of Surface-Treated Zirconia Sol [Production Example 13] 26 g of HZ-400M7 (manufactured by Nissan Chemical Industries, Ltd.), which is a zirconia sol dispersed in methanol, and dipropylene glycol monomethyl ether (manufactured by Kanto Chemical Co., Ltd.; the same applies hereinafter) were placed in a recovery flask, and the methanol contained in HZ-400M7 was solvent-substituted with dipropylene glycol monomethyl ether using an evaporator, thereby obtaining a zirconia sol dispersed in dipropylene glycol monomethyl ether (solid content concentration: 20.0 mass %).

[0260] [Production Example 14] 5.0 g of the zirconia sol dispersed in dipropylene glycol monomethyl ether obtained in Production Example 13 and 0.1 g (0.73 mmol) of trimethoxy(methyl)silane (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to a reaction vessel and stirred under nitrogen at 60°C for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 µm to obtain surface-treated zirconia sol A [solid content (surface-treated zirconia) concentration 22.0 mass%].

[0261] [Production Example 15] 5.0 g of the dipropylene glycol monomethyl ether-dispersed zirconia sol obtained in Production Example 13 and 0.1 g (0.61 mmol) of trimethoxy(propyl)silane (Tokyo Chemical Industry Co., Ltd.) were added to a reaction vessel and stirred under nitrogen at 60°C for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 µm to obtain surface-treated zirconia sol B [solid content (surface-treated zirconia) concentration 22.0 mass%].

[0262] [8] Preparation of Zirconia Sol-Containing Charge-Transporting Varnish [Example 4-1] 1.98 g of 1,3-dimethyl-2-imidazolidinone, 3.37 g of dipropylene glycol, and 2.47 g of dipropylene glycol monomethyl ether were placed in a recovery flask and stirred at room temperature for 30 minutes using a stirrer. Then, 0.45 g of the 1,3-dimethyl-2-imidazolidinone solution of the arylsulfonic acid compound obtained in Preparation Example 2 was added, and the mixture was stirred at room temperature for 30 minutes using a stirrer. Then, 0.6 g of the mixed solution obtained in Preparation Example 1 was added, and the mixture was stirred at room temperature for 30 minutes. Next, 1.13 g of the surface-treated zirconia sol A produced in Preparation Example 14 was added to the resulting mixed solution, and the mixture was stirred at room temperature for 30 minutes. The resulting mixture was filtered through a PP syringe filter with a pore size of 0.2 μm to obtain a charge-transporting varnish (solids concentration: 3.2% by mass).

[0263] Example 4-2: 1.98 g of 1,3-dimethyl-2-imidazolidinone, 3.37 g of dipropylene glycol, and 2.47 g of dipropylene glycol monomethyl ether were placed in a recovery flask and stirred at room temperature for 30 minutes using a stirrer. Then, 0.45 g of the 1,3-dimethyl-2-imidazolidinone solution of the arylsulfonic acid compound obtained in Preparation Example 2 was added, and the mixture was stirred at room temperature for 30 minutes using a stirrer. Then, 0.6 g of the mixed solution obtained in Preparation Example 1 was added, and the mixture was stirred at room temperature for 30 minutes. Next, 1.13 g of the surface-treated zirconia sol B produced in Preparation Example 15 was added to the resulting mixed solution, and the mixture was stirred at room temperature for 30 minutes. The resulting mixture was filtered through a PP syringe filter with a pore size of 0.2 μm to obtain a charge-transporting varnish (solids concentration: 3.2% by mass).

[0264] Comparative Example 4-1: 1.98 g of 1,3-dimethyl-2-imidazolidinone, 3.37 g of dipropylene glycol, and 2.18 g of dipropylene glycol monomethyl ether were placed in a recovery flask and stirred at room temperature for 30 minutes using a stirrer. Then, 0.45 g of the 1,3-dimethyl-2-imidazolidinone solution of the arylsulfonic acid compound obtained in Preparation Example 2 was added, and the mixture was stirred at room temperature for 30 minutes using a stirrer. Then, 0.6 g of the mixed solution obtained in Preparation Example 1 was added, and the mixture was stirred at room temperature for 30 minutes. Next, 1.13 g of the dipropylene glycol monomethyl ether-dispersed zirconia sol produced in Preparation Example 13 was added to the resulting mixed solution, and the mixture was stirred at room temperature for 30 minutes. The resulting mixture was filtered through a PP syringe filter with a pore size of 0.2 μm to obtain a charge-transporting varnish (solids concentration: 3.0% by mass).

[0265] [9] Preparation of Charge-Transporting Thin Film and Evaluation of Ionization Potential [Examples 5-1 to 5-2] A uniform thin film with a thickness of 65 nm was formed on an ITO substrate in the same manner as in Example 2-1, except that the charge-transporting varnish in Example 2-1 was changed to the charge-transporting varnish obtained in Examples 4-1 and 4-2.

[0266] Comparative Example 5-1 A uniform thin film having a thickness of 65 nm was formed on an ITO substrate in the same manner as in Example 2-1, except that the charge-transporting varnish in Example 2-1 was changed to the charge-transporting varnish obtained in Comparative Example 4-1.

[0267] The ionization potential (IP) of the thin film surface was measured using a photoelectron spectrometer (AC-3) for the charge-transporting thin films on the ITO substrates formed in Examples 5-1 and 5-2 and Comparative Example 5-1. The measurements were performed under conditions of a light intensity of 20 nW and a measurement range of 4.8 to 7.0 eV, and the ionization potential value was calculated from the threshold energy of electron emission. The values ​​(ΔIP) of (IP of Examples 5-1 and 5-2) minus (IP of Comparative Example 5-1) are shown in Table 3.

[0268]

[0269] As shown in Table 3, the thin film formed from the charge-transporting varnish using the surface-treated zirconia sol of the present invention exhibited a higher IP than the thin film formed from the charge-transporting varnish using the surface-treated zirconia sol. The same effect was obtained as when the surface-treated silica sol was used. It is believed that the use of the surface-treated zirconia sol changes the interaction between the sol and the charge-transporting substance and the dispersibility of the sol itself, resulting in a different surface state of the charge-transporting thin film obtained from the case where untreated zirconia sol is used.

[0270]

[10] Fabrication and Evaluation of Hole-Only Devices (HODs) [Examples 6-1 to 6-2] Hole-only devices were fabricated in the same manner as in Example 3-1, except that the charge-transporting varnish in Example 3-1 was changed to the charge-transporting varnishes obtained in Examples 4-1 and 4-2.

[0271] Comparative Example 6-1 A hole-only device was fabricated in the same manner as in Example 3-1, except that the charge-transporting varnish in Example 3-1 was changed to the charge-transporting varnish obtained in Comparative Example 4-1.

[0272] The current-voltage characteristics were evaluated for each of the devices of Examples 6-1 and 6-2 and Comparative Example 6-1. Specifically, the current density (mA / cm) was measured when a voltage of −5 V to +5 V was applied in 0.25 V increments to the hole-only devices. 2 The current densities when a voltage of +5 V was applied to the elements of Examples 6-2 to 6-2 and Comparative Example 6-1 are shown in Table 4.

[0273]

[0274] As shown in Table 4, when a voltage of +5 V was applied to the hole-only devices of Examples 6-1 and 6-2, the current density was higher than that of the hole-only device prepared in Comparative Example 6-1. It is believed that one of the reasons for this is that the thin film formed from the charge-transporting varnish using the surface-treated zirconia sol of the present invention has a deeper HOMO film surface than the thin film formed from the charge-transporting varnish using the non-surface-treated zirconia sol, thereby improving hole injection properties into the hole-transporting layer formed on top. It was shown that similar effects can be obtained not only when using surface-treated silica sol but also when using surface-treated zirconia sol.

[0275]

[11] Production of Surface-Treated Titania Sol [Production Example 16] 15.8 g of HT-R305M7-20 (manufactured by Nissan Chemical Industries, Ltd.), which is a titania sol dispersed in methanol, and dipropylene glycol monomethyl ether were placed in a recovery flask, and the methanol contained in HT-R305M7-20 was solvent-substituted with dipropylene glycol monomethyl ether using an evaporator, thereby obtaining a titania sol dispersed in dipropylene glycol monomethyl ether (solid content concentration 10.0 mass%).

[0276] [Production Example 17] 8.0 g of the dipropylene glycol monomethyl ether-dispersed titania sol obtained in Production Example 16 and 0.08 g (0.59 mmol) of trimethoxy(methyl)silane were added to a reaction vessel, and the mixture was stirred under nitrogen at 60°C for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 µm to obtain surface-treated titania sol A [solid content (surface-treated titania) concentration 10.9 mass%].

[0277] [Production Example 18] 8.0 g of the dipropylene glycol monomethyl ether-dispersed titania sol obtained in Production Example 16 and 0.08 g (0.49 mmol) of trimethoxy(propyl)silane were added to a reaction vessel, and the mixture was stirred under nitrogen at 60°C for 3 hours. After cooling to room temperature, the mixture was filtered through a PTFE filter with a pore size of 1.0 µm to obtain surface-treated titania sol B [solid content (surface-treated titania) concentration 10.9 mass%].

[0278]

[12] Preparation of Titania Sol-Containing Charge-Transporting Varnish [Example 7-1] 1.98 g of 1,3-dimethyl-2-imidazolidinone, 3.37 g of dipropylene glycol, and 1.35 g of dipropylene glycol monomethyl ether were placed in a recovery flask and stirred at room temperature for 30 minutes using a stirrer. Then, 0.45 g of the 1,3-dimethyl-2-imidazolidinone solution of the arylsulfonic acid compound obtained in Preparation Example 2 was added, and the mixture was stirred at room temperature for 30 minutes using a stirrer. Then, 0.6 g of the mixed solution obtained in Preparation Example 1 was added, and the mixture was stirred at room temperature for 30 minutes. Next, 2.25 g of the surface-treated titania sol A produced in Preparation Example 17 was added to the resulting mixed solution, and the mixture was stirred at room temperature for 30 minutes. The resulting mixture was filtered through a PP syringe filter with a pore size of 0.2 μm to obtain a charge-transporting varnish (solids concentration: 3.2% by mass).

[0279] Example 7-2: 1.98 g of 1,3-dimethyl-2-imidazolidinone, 3.37 g of dipropylene glycol, and 1.35 g of dipropylene glycol monomethyl ether were placed in a recovery flask and stirred at room temperature for 30 minutes using a stirrer. Then, 0.45 g of the 1,3-dimethyl-2-imidazolidinone solution of the arylsulfonic acid compound obtained in Preparation Example 2 was added, and the mixture was stirred at room temperature for 30 minutes using a stirrer. Then, 0.6 g of the mixed solution obtained in Preparation Example 1 was added, and the mixture was stirred at room temperature for 30 minutes. Next, 2.25 g of the surface-treated titania sol B produced in Preparation Example 18 was added to the resulting mixed solution, and the mixture was stirred at room temperature for 30 minutes. The resulting mixture was filtered through a PP syringe filter with a pore size of 0.2 μm to obtain a charge-transporting varnish (solids concentration: 3.2% by mass).

[0280] Comparative Example 7-1: 1.98 g of 1,3-dimethyl-2-imidazolidinone, 3.37 g of dipropylene glycol, and 1.35 g of dipropylene glycol monomethyl ether were placed in a recovery flask and stirred at room temperature for 30 minutes using a stirrer. Then, 0.45 g of the 1,3-dimethyl-2-imidazolidinone solution of the arylsulfonic acid compound obtained in Preparation Example 2 was added, and the mixture was stirred at room temperature for 30 minutes using a stirrer. Then, 0.6 g of the mixed solution obtained in Preparation Example 1 was added, and the mixture was stirred at room temperature for 30 minutes. Next, 2.25 g of the titania sol produced in Preparation Example 16 was added to the resulting mixed solution, and the mixture was stirred at room temperature for 30 minutes. The resulting mixture was filtered through a PP syringe filter with a pore size of 0.2 μm to obtain a charge-transporting varnish (solids concentration: 3.0% by mass).

[0281]

[13] Preparation of Charge-Transporting Thin Film and Evaluation of Ionization Potential [Examples 8-1 to 8-2] A uniform thin film with a thickness of 65 nm was formed on an ITO substrate in the same manner as in Example 2-1, except that the charge-transporting varnish in Example 2-1 was changed to the charge-transporting varnish obtained in Examples 7-1 and 7-2.

[0282] Comparative Example 8-1 A uniform thin film having a thickness of 65 nm was formed on an ITO substrate in the same manner as in Example 2-1, except that the charge-transporting varnish in Example 2-1 was changed to the charge-transporting varnish obtained in Comparative Example 7-1.

[0283] The ionization potential (IP) of the thin film surface was measured using a photoelectron spectrometer (AC-3) for the charge-transporting thin films on the ITO substrates formed in Examples 7-1 and 7-2 and Comparative Example 7-1. The measurements were performed under conditions of a light intensity of 20 nW and a measurement range of 4.8 to 7.0 eV, and the ionization potential value was calculated from the threshold energy of electron emission. The values ​​(ΔIP) of (IP of Examples 7-1 and 7-2) minus (IP of Comparative Example 7-1) are shown in Table 5.

[0284]

[0285] As shown in Table 5, the thin film formed from the charge-transporting varnish using the surface-treated titania sol of the present invention exhibited a higher IP than the thin film formed from the charge-transporting varnish using the surface-treated titania sol. The same effect was obtained as when the surface-treated silica sol was used. It is believed that the use of the surface-treated titania sol changes the interaction between the sol and the charge-transporting material and the dispersibility of the sol itself, resulting in a different surface condition for the resulting charge-transporting thin film compared to when the untreated titania sol was used.

[0286]

[14] Fabrication and Evaluation of Hole-Only Devices (HOD) [Examples 9-1 to 9-2] Hole-only devices were fabricated in the same manner as in Example 3-1, except that the charge-transporting varnish in Example 3-1 was changed to the charge-transporting varnish obtained in Examples 7-1 and 7-2. In order to stably evaluate the devices, the thickness of the hole-transporting layer (TFB) was set to 65 nm.

[0287] [Comparative Example 9-1] A hole-only device was fabricated in the same manner as in Example 3-1, except that the charge-transporting varnish in Example 3-1 was changed to the charge-transporting varnish obtained in Comparative Example 7-1. From the viewpoint of stable evaluation of the device, the thickness of the hole-transporting layer (TFB) was set to 65 nm.

[0288] The current-voltage characteristics were evaluated for each of the devices of Examples 9-1 and 9-2 and Comparative Example 9-1. Specifically, the current density (mA / cm) was measured when a voltage was applied to the hole-only device from −5 V to +5 V in 0.25 V increments. 2 Table 6 shows the current densities when a voltage of +5 V was applied to the devices of Examples 9-1 and 9-2 and Comparative Example 9-1.

[0289]

[0290] As shown in Table 6, when a voltage of +5 V was applied to the hole-only devices of Examples 9-1 and 9-2, the current density was higher than that of the hole-only device prepared in Comparative Example 9-1. It is believed that one of the reasons for this is that the thin film formed from the charge-transporting varnish using the surface-treated titania sol of the present invention has a deeper HOMO film surface than the thin film formed from the charge-transporting varnish using the non-surface-treated titania sol, thereby improving hole injection properties into the hole-transporting layer formed on top. It was shown that similar effects can be obtained not only when using surface-treated silica sol but also when using surface-treated titania sol.

Claims

1. A charge transporting varnish comprising metal oxide nanoparticles surface-treated with a silane coupling agent represented by the following formula (S1), a charge transporting substance, and an organic solvent. (In the formula, R v1 ~R v3 each independently represents a hydrogen atom, a chlorine atom, a hydroxyl group, an alkoxy group which may have a substituent, or an alkyl group which may have a substituent; R v1 ~R v3 at least one of the groups represents a hydrogen atom, a chlorine atom, a hydroxyl group, or an alkoxy group which may have a substituent; L represents a single bond or an alkylene group having 1 to 10 carbon atoms; R v4 represents an alkyl group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group; an alkoxy group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group; or an aryl group having 6 to 20 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, a hydroxy group, an alkyl group having 1 to 10 carbon atoms, and an alkoxy group having 1 to 10 carbon atoms. v4 is an alkyl group having 1 to 10 carbon atoms which may have a substituent, L is a single bond.

2. The above R v1 ~R v3 2. The charge transporting varnish according to claim 1, wherein is an optionally substituted alkyl group having 1 to 10 carbon atoms or an optionally substituted alkoxy group having 1 to 10 carbon atoms.

3. R v4 is an alkyl group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group; or an alkoxy group having 1 to 10 carbon atoms which may have at least one substituent selected from the group consisting of a halogen atom, a sulfo group, and a hydroxy group.

4. The charge transporting varnish according to claim 1, wherein the charge transporting substance is a polythiophene derivative or an amine adduct thereof, or an arylamine derivative.

5. The charge transporting varnish according to claim 4, wherein the charge transporting substance is a polythiophene derivative containing a repeating unit represented by the following formula (1) or an amine adduct thereof. (In the formula, R 1 and R 2 are each independently a hydrogen atom, an alkyl group having 1 to 40 carbon atoms, a fluoroalkyl group having 1 to 40 carbon atoms, an alkoxy group having 1 to 40 carbon atoms, a fluoroalkoxy group having 1 to 40 carbon atoms, an aryloxy group having 6 to 20 carbon atoms, -O-[Z-O] p -R e or a sulfonic acid group, or R 1 and R 2 is bonded to each other, Y is an alkylene group having 1 to 40 carbon atoms which may contain an ether bond and which may be substituted with a sulfonic acid group, Z is an alkylene group having 1 to 40 carbon atoms which may be substituted with a halogen atom, p is an integer of 1 or more, R e is a hydrogen atom, an alkyl group having 1 to 40 carbon atoms, a fluoroalkyl group having 1 to 40 carbon atoms, or an aryl group having 6 to 20 carbon atoms.

6. R above 1 is a sulfonic acid group, and the R 2 is an alkoxy group having 1 to 40 carbon atoms or -O-[Z-O] p -R e or the above R 1 and R 2 6. The charge transporting varnish according to claim 5, wherein the bond is --O--Y--O--.

7. The charge transporting varnish of claim 1 further comprising a dopant material.

8. The charge transporting varnish according to claim 7, wherein said dopant substance comprises at least one substance selected from the group consisting of arylsulfonic acid compounds and heteropolyacid compounds.

9. The charge transporting varnish according to claim 1, wherein the metal oxide nanoparticles are at least one selected from the group consisting of SiO2, TiO2 and ZrO2.

10. The charge transporting varnish according to claim 9, wherein said metal oxide nanoparticles are SiO2.

11. The charge transporting varnish of claim 1, further comprising one or more amine compounds.

12. The charge transporting varnish according to claim 11, wherein the amine compound comprises a tertiary alkylamine compound and an amine compound other than a tertiary alkylamine compound.

13. The charge transporting varnish according to claim 12, wherein the amine compound other than the tertiary alkylamine compound is a primary alkylamine compound.

14. A charge-transporting thin film obtained from the charge-transporting varnish according to any one of claims 1 to 13.

15. An electronic device comprising the charge transporting thin film according to claim 14.

16. The electronic device according to claim 15, wherein said charge transporting thin film is a hole injection layer.

17. The electronic device according to claim 16, which is an organic EL device or a quantum dot EL device.

Citation Information

Patent Citations

  • Charge transporting thin film

    JP2019009468A

  • Charge-transporting varnish and charge-transporting thin film

    WO2019124413A1

  • Charge-transporting composition

    WO2020009138A1