Non-magnetic austenitic steel, and magnetic field confinement-type nuclear fusion device comprising same

A non-magnetic austenitic steel alloy with specific elemental composition addresses the need for improved resistance in fusion devices, providing stable operation and reduced magnetic interference by forming a dense oxide film, enhancing oxidation and mechanical strength.

WO2024241943A1PCT designated stage expired Publication Date: 2024-11-28HELICAL FUSION CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017632
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-13
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Magnetic confinement fusion devices require non-magnetic materials with improved oxidation resistance, neutron radiation resistance, and mechanical strength to maintain stable operation and prevent magnetic interference with plasma confinement.

Method used

A non-magnetic austenitic steel alloy with a composition of 28-32% Mn, 5-7% Al, 0.5-2% Si, and 0-0.3% C, optionally containing Y2O3, which forms a dense oxide film for enhanced corrosion resistance and mechanical strength, is developed for use in fusion device components.

Benefits of technology

The austenitic steel exhibits superior oxidation resistance, mechanical strength, and neutron irradiation resistance, ensuring stable operation and minimizing magnetic interference in magnetic confinement fusion devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017632_28112024_PF_FP_ABST
    Figure JP2024017632_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A magnetic field confinement-type nuclear fusion device (1) comprises a first component (e.g., a blanket 20) including non-magnetic austenitic steel. The non-magnetic austenitic steel contains 28–31 mass% of Mn, 5–7 mass% of Al, 0.5–2 mass% of Si, 0–0.3 mass% of C, and 0–1.5 mass% of Y2O3, with the balance consisting of Fe and inevitable impurities.
Need to check novelty before this filing date? Find Prior Art

Description

Non-magnetic austenitic steel and magnetic confinement fusion device containing the same

[0001] The present invention relates to a non-magnetic austenitic steel and a magnetic confinement nuclear fusion device including the same.

[0002] Japanese Patent Application Laid-Open No. 2021-133804 (Patent Document 1) describes the use of low-activation ferritic steel (e.g., F82H) as a housing material for a nuclear fusion blanket.

[0003] Japanese Patent Application Laid-Open No. 2021-133804

[0004] A magnetic confinement fusion device is a device that uses magnetic field lines to confine plasma and generate a sustained fusion reaction. For this reason, it is preferable to use non-magnetic materials for the components and members incorporated into a magnetic confinement fusion device. However, in addition to being non-magnetic, materials for fusion devices must also have improved properties such as oxidation resistance, neutron radiation resistance, and mechanical strength.

[0005] An object of the present invention is to provide a non-magnetic austenitic steel suitable as a material for use in a magnetic confinement fusion device, and a magnetic confinement fusion device using the same.

[0006] The non-magnetic austenitic steel according to one embodiment contains 28% by mass or more and 32% by mass or less of Mn, 5% by mass or more and 7% by mass or less of Al, 0.5% by mass or more and 2% by mass or less of Si, 0% by mass or more and 0.3% by mass or less of C, and Y. 2 O 3 (Yttrium oxide) is contained in an amount of 0 mass % or more and 1.5 mass % or less, with the remainder being Fe and unavoidable impurities.

[0007] Another embodiment of a magnetic confinement fusion device includes a first component including a non-magnetic austenitic steel, the non-magnetic austenitic steel containing 28% by mass or more and 32% by mass or less of Mn, 5% by mass or more and 7% by mass or less of Al, 0.5% by mass or more and 2% by mass or less of Si, 0% by mass or more and 0.3% by mass or less of C, and Y. 2 O 3 contains 0 mass % or more and 1.5 mass % or less, and the balance is Fe and unavoidable impurities.

[0008] Exemplary embodiments of the present invention provide austenitic steels suitable for inclusion in magnetic confinement fusion devices.

[0009] FIG. 1 is a cutaway perspective view showing an example of the configuration of a magnetic confinement fusion device according to one embodiment; FIG. 2 is a diagram showing mass gain curves for Example 1 and Comparative Example 1; FIG. 3 is a diagram showing an image of a sample of Example 1 observed by a scanning transmission electron microscope (STEM); FIG. 4 is a diagram showing an image of a sample of Example 1 observed by an energy dispersive X-ray analyzer (EDS); FIG. 5 is an explanatory diagram showing a forged austenitic steel produced as Example 2; FIG. 6 is an explanatory diagram showing the results of X-ray crystal structure analysis of test specimens of the austenitic steel of Example 2 after thermal aging tests at 700°C for 10 hours, 100 hours, and 1000 hours; FIG. 7 is an explanatory diagram showing the results of X-ray crystal structure analysis of test specimens of the austenitic steel of Example 2 before thermal aging tests; FIG. 8 is an explanatory diagram showing the results of analysis by an electron probe microanalyzer (EMPA) of test specimens of the austenitic steel of Example 2 after thermal aging tests at 700°C for 10 hours, 100 hours, and 1000 hours. 1 is an explanatory diagram showing the evaluation results of nanoindentation hardness in the austenitic steels of Example 2 and Comparative Example 2. FIG. 2 is an explanatory diagram showing the evaluation results of elastic modulus in the austenitic steels of Example 2 and Comparative Example 2. FIG. 3 is an explanatory diagram showing the results of X-ray crystal structure analysis in each of six regions extending from the circumference toward the center in the forged material of the austenitic steel of Example 2. FIG. 4 is an explanatory diagram showing the results of a tensile strength test for the austenitic steels of Example 3 and Comparative Example 3.

[0010] The inventors of the present application are conducting research and development of a nuclear fusion device that causes a nuclear fusion reaction by confining high-temperature, high-density plasma within a reactor. As part of this research, they have investigated non-magnetic austenitic steels suitable for use as structural materials for nuclear fusion devices and as materials for components such as blankets and divertors that are placed within the device.

[0011] <Definition of Terms> First, the definitions of terms used in this application will be explained.

[0012] A "nuclear fusion device" is a device that utilizes nuclear fusion reactions to generate energy and extract it outside.

[0013] A "magnetic confinement fusion device" is a fusion device that uses magnetic field lines to confine plasma for generating a fusion reaction. There are various types of magnetic confinement devices, such as "tokamak type" and "helical type," depending on the shape of the magnetic field lines. In this application, the term "magnetic confinement" is used as a general term for any device that confines plasma using magnetic field lines.

[0014] "Nonmagnetic" refers to a state in which a material does not have the properties of a magnetic material, and a state in which it can be considered to be substantially non-magnetic. A state in which it can be considered to be substantially non-magnetic refers to a case in which the magnetic properties are sufficiently small in the usage environment that the influence is negligible. For example, in the case of a material used in a magnetic confinement fusion device, this refers to a case in which the influence of the material's magnetism on the magnetic field lines that confine the plasma is negligible. Furthermore, if the non-magnetic state is expressed in terms of "relative magnetic permeability," a material can be said to be non-magnetic if its relative magnetic permeability is in the range of 1.00 to 1.02.

[0015] The relative magnetic permeability of steel can be measured, for example, by a method using a vibrating sample magnetometer.

[0016] <Magnetic Confinement Fusion Device> Fig. 1 is a cutaway perspective view showing an example of the configuration of a magnetic confinement fusion device according to one embodiment. The fusion device 1 shown in Fig. 1 is a magnetic confinement fusion device, more specifically, a helical fusion device.

[0017] 1 shows an X direction, a Y direction, and a Z direction. The X direction, the Y direction, and the Z direction intersect with each other. In the example shown in FIG. 1, the X direction, the Y direction, and the Z direction are perpendicular to each other.

[0018] The nuclear fusion device 1 has a vacuum vessel 10, a blanket 20, a divertor 30, a magnet (superconducting magnet) 40, and a cryostat 50. The blanket 20, the divertor 30, the magnet 40, and the cryostat 50 are each disposed within the vacuum vessel 10. The divertor 30 is disposed inside the blanket 20.

[0019] The vacuum vessel 10 is a container for accommodating components for continuously generating a nuclear fusion reaction. Nuclear fusion reactions use hydrogen isotopes, such as deuterium and tritium, as raw materials. Therefore, the inside of the vacuum vessel 10 is kept in an ultra-high vacuum state (for example, 10 -5 The vacuum vessel 10 must be maintained at a pressure of about 1000 Pa or less. The vacuum vessel 10 is made of, for example, stainless steel.

[0020] As a modification, the vacuum vessel 10 may be made of non-magnetic austenitic steel, which will be described later. However, the vacuum vessel 10 is located at a position away from the fusion plasma 21, and the blanket 20 is interposed between the vacuum vessel 10 and the fusion plasma 21. Therefore, the oxidation resistance or neutron radiation resistance required for the vacuum vessel 10 is relatively low compared to the oxidation resistance or neutron radiation resistance required for the blanket 20.

[0021] The blanket 20 is a component that constitutes a flow path for the liquid metal 2. The fusion plasma 21 forms a ring (torus shape) in the X-Y plane including the X and Y directions in Fig. 1. The blankets 20 are arranged so as to sandwich the fusion plasma 21 in the X or Y direction. In other words, when the fusion device 1 is in operation, the fusion plasma 21 is sandwiched between the blankets 20 in the X or Y direction.

[0022] 1, the liquid metal 2 flowing inside the blanket 20 is irradiated with neutrons generated by the fusion plasma 21. In other words, the blanket 20 has the function of receiving and shielding the neutrons generated by the fusion plasma 21.

[0023] The liquid metal 2 serves as a coolant that transfers heat generated by neutron irradiation to the outside. In other words, the blanket 20 has the function of transferring thermal energy generated by neutron irradiation to the outside (for example, a power generation facility such as a turbine generator) via the coolant (liquid metal 2).

[0024] Furthermore, when irradiated with neutrons, the liquid metal 2 serves as a fuel source that generates tritium, which is fuel for the nuclear fusion reaction. Tritium is produced by a spallation reaction caused by neutron irradiation of lithium contained in the liquid metal 2. In other words, the blanket 20 functions as a raw material supply path for generating fuel for the nuclear fusion reaction.

[0025] From the viewpoint of efficiently converting neutrons generated in the fusion plasma 21 into thermal energy, it is preferable that the blanket 20 is close to the fusion plasma 21. For this reason, the material constituting the blanket 20 is preferably non-magnetic austenitic steel, which will be described later.

[0026] The divertor 30 is a component (heat receiving device) provided on the blanket 20 at a portion that comes into contact with the divertor plasma 31. A portion of the fusion plasma 21 is connected to a portion of the surface of the blanket 20 by magnetic field lines. This is called divertor plasma. Charged particles in the plasma move along the magnetic field lines. The divertor 30 utilizes this property of charged particles to prevent impurities from entering the fusion plasma 21 as charged particles.

[0027] The divertor 30 is disposed between the blanket 20 and the fusion plasma 21. Therefore, the distance between the divertor 30 and the fusion plasma 21 is short. Therefore, the material constituting the divertor 30 is preferably non-magnetic austenitic steel, which will be described later.

[0028] The magnet 40 is a component for generating magnetic field lines to maintain the fusion plasma 21 in a pre-designed shape. The magnet 40 is a superconducting electromagnet formed by laminating superconducting wires (not shown) made of a superconducting material. The shape of the magnet 40 can be modified in various ways depending on the shape of the fusion plasma 21.

[0029] The cryostat 50 is a container that houses the magnet 40. The cryostat 50 also serves as a thermal shield for maintaining the magnet 40 in a superconducting state.

[0030] Of the multiple components (blanket 20, divertor 30, magnet 40, and cryostat 50) of the nuclear fusion device 1 shown in FIG. 1, the blanket 20 and the divertor 30 preferably contain non-magnetic austenitic steel, which will be described later.

[0031] However, there are various modifications of the components containing the non-magnetic austenitic steel described below in the nuclear fusion device 1. For example, there are cases where only one of the blanket 20 and the divertor 30 contains the non-magnetic austenitic steel described below. Alternatively, there are cases where components other than the blanket 20 and the divertor 30 contain the non-magnetic austenitic steel described below.

[0032] <Non-magnetic Austenitic Steel> Hereinafter, the austenitic steel according to the present embodiment will be described.

[0033] The austenitic steel according to the present embodiment is an alloy containing iron (Fe), Mn (manganese), Al (aluminum), and Si (silicon) as essential components.

[0034] Mn, together with Al (described later), is an essential component for achieving single-phase stabilization (hereinafter simply referred to as "stabilization") of austenitic steel (FCC phase) at high temperatures. The contents of Mn and Al must be in a predetermined relationship to stabilize austenitic steel, and these elements have a positive correlation in terms of their contents. That is, increasing Mn requires increasing Al, and decreasing Mn requires decreasing Al.

[0035] Mn is an element used in place of Ni (nickel), which has conventionally been added to stabilize austenitic steel. Furthermore, in this embodiment, by increasing the Mn content and keeping the contents of other components within predetermined ranges, the resulting austenitic steel can be made into a non-magnetic alloy.

[0036] Making austenitic steel nonmagnetic is extremely important when using it as a material for the fusion device 1. In particular, in a magnetic confinement fusion device, as described above, magnetic field lines formed by the magnet 40 are used to confine plasma. Therefore, when a magnetic material is placed near the fusion plasma 21 and the divertor plasma 31, the magnetic material may affect the shape of the magnetic field lines for confining the plasma, causing problems. The austenitic steel according to this embodiment suppresses the occurrence of such problems and enables stable operation of the fusion device.

[0037] Furthermore, when non-magnetic austenitic steel is used as the material for the fusion device 1, it is preferable that the steel have high properties as follows: Components (especially the blanket 20 and the divertor 30) located near the fusion plasma 21 are placed in a high-temperature environment, so it is preferable that they have high oxidation resistance (corrosion resistance). As will be described in detail later, the non-magnetic austenitic steel according to this embodiment has high oxidation resistance.

[0038] Components (especially the blanket 20 and the divertor 30) located near the fusion plasma 21 are irradiated with many neutrons, so it is preferable that they have high resistance to neutron irradiation.

[0039] Furthermore, a common requirement for all parts is that they preferably have sufficient mechanical strength to prevent damage to the parts.

[0040] The Mn content is, for example, preferably 28% by mass or more and 31% by mass or less, and more preferably 29% by mass or more and 30.5% by mass or less. If the Mn content is less than 28% by mass, the Al content must also be relatively reduced, which may result in the austenitic steel not being able to achieve sufficient oxidation resistance (corrosion resistance). On the other hand, if the Mn content exceeds 31% by mass, the balance with other components may be affected, resulting in a decrease in the stability of the austenitic steel (particularly, the formation of a β-Mn phase at high temperatures). Furthermore, austenitic steels containing a high Mn content of 28% by mass or more, as described above, exhibit higher mechanical strength than chromium-nickel stainless steels containing Ni and Cr as elements for stabilizing austenite.

[0041] Al is an essential component that improves the oxidation resistance (corrosion resistance) of austenitic steel and stabilizes the austenitic steel. As described above, the Al content has a positive correlation with Mn in terms of maintaining the stability of the austenitic steel.

[0042] When austenitic steel is used under high temperature conditions such as in the nuclear fusion device 1, Al forms aluminum oxide (Al 2 O 3 The oxidation resistance can be improved by forming an oxide film containing magnesium oxide, iron oxide, etc. According to the investigations of the present inventors, scale such as magnesium oxide or iron oxide is formed on the outermost surface layer of the surface layer of non-magnetic austenitic steel, and a dense oxide film containing aluminum oxide is formed along the interface between this scale and the base material. It is believed that the formation of this dense oxide film containing aluminum oxide suppresses the penetration of oxygen into the base material and the migration of elements constituting the base material to the surface. In this embodiment, the coexistence of Si, which will be described later, is believed to form a denser film, thereby improving the oxidation resistance (corrosion resistance).

[0043] The Al content is preferably 5% by mass or more and 7% by mass or less, and more preferably 5.5% by mass or more and 6.5% by mass or less. If the Al content is less than 5% by mass, the austenitic steel may not have sufficient oxidation resistance (corrosion resistance). On the other hand, if the Al content exceeds 7% by mass, the balance with other components may be affected, resulting in a decrease in the stability of the austenitic steel (especially, an increase in the Mn content may cause the formation of a β-Mn phase at high temperatures). Furthermore, as will be described later in Example 3, austenitic steel containing Al in the range of 5% by mass or more and 7% by mass or less, particularly preferably 5.5% by mass or more and 6.5% by mass or less, exhibits high mechanical strength.

[0044] Silicon is an essential component that improves the oxidation resistance (corrosion resistance) of austenitic steel and stabilizes it. As described above, when used under high-temperature conditions such as in nuclear fusion devices, silicon is thought to act as a component that forms a denser oxide film containing aluminum oxide and improves the corrosion resistance of austenitic steel.

[0045] The Si content is, for example, preferably 0.5 mass% or more and 2 mass% or less, and more preferably 0.8 mass% or more and 1.5 mass% or less. If the Si content is less than 0.5 mass%, the austenitic steel may not have sufficient oxidation resistance (corrosion resistance). On the other hand, if the Si content exceeds 2 mass%, the strength characteristics may deteriorate. Furthermore, austenitic steel containing Si as an essential component in the range of 0.5 mass% or more and 2 mass% or less, preferably 0.8 mass% or more and 1.5 mass% or less, exhibits high mechanical strength. C (carbon) is an optional component that increases the strength of austenitic steel. C may or may not be contained.

[0046] When C is contained, the content is preferably 0.3 mass% or less. If the C content exceeds 0.3 mass%, the austenite-forming components decrease, the BCC phase (ferrite phase) is more likely to occur, the stability of the austenitic steel decreases, and there is a risk of the austenitic steel becoming magnetic.

[0047] However, when the C content is small, i.e., 0.3 mass% or less, C functions as a component for stabilizing the austenitic steel. In this embodiment, since the austenitic steel is stabilized by including a large amount of Mn, the austenitic steel can be stabilized by including 0.3 mass% or less of C.

[0048] Y 2 O 3 Yttrium oxide (YO) is an optional component that improves the strength characteristics of austenitic steel. 2 O 3 By blending Y, it is possible to improve oxidation resistance (corrosion resistance) and neutron irradiation resistance. Here, neutron irradiation resistance refers to the property of generating highly radioactive materials after neutron irradiation in a nuclear fusion device. 2 O 3 By blending, it is possible to reduce the neutron irradiation resistance by acting as a sink for irradiation defects.

[0049] As described above, C acts as a component that increases the strength of austenitic steel. In this embodiment, however, the C content is set low in consideration of the stability of austenitic steel at high temperatures. Therefore, in this embodiment, from the viewpoint of improving the strength characteristics of austenitic steel, Y is used. 2 O 3 It is preferable to blend Y. 2 O 3 When blended, the content thereof is, for example, preferably 0.1% by mass or more and 1.5% by mass or less, and more preferably 0.15% by mass or more and 1% by mass or less.

[0050] Ni is an optional component that stabilizes the single-phase austenitic steel. As described above, since Mn is contained in large amounts in this embodiment as an essential component, Ni may be contained in small amounts, but from the viewpoint of the stability of the austenitic steel, it is not necessary to contain Ni. Furthermore, from the viewpoint of suppressing the magnetism of the austenitic steel, it is preferable that Ni is not contained substantially. Here, "substantially not contained" means that the Ni content is 1000 ppm or less.

[0051] Cr is an optional component that improves the oxidation resistance (corrosion resistance) of austenitic steel. However, if the Cr content is high, there is a risk of the formation of a σ phase, which may adversely affect the oxidation resistance (corrosion resistance), mechanical properties, and sometimes magnetic properties. In this embodiment, it is preferable that Cr is substantially free of Cr. Here, "substantially free of Cr" means that the Cr content is 0.5 mass% or less.

[0052] Austenitic steel with the above composition is composed of a single FCC phase, making it non-magnetic. Making it a non-magnetic material enables stable operation of nuclear fusion devices, as described above. The definition of "non-magnetic" here is as previously mentioned.

[0053] The austenitic steel according to the present embodiment having the above composition has very good oxidation resistance (corrosion resistance) at high temperatures and is a non-magnetic material. 2 O 3 By blending these elements, it is possible to improve the strength characteristics and make the material resistant to neutron irradiation. This austenitic steel is extremely suitable as a material for forming components of nuclear fusion devices.

[0054] In particular, the austenitic steel of this embodiment is characterized by its high Mn content and the essential elements of Al and Si, which effectively improves oxidation resistance (corrosion resistance) at high temperatures. This is thought to be because the aluminum oxide film formed at high temperatures is denser than that of conventionally known alloys. As shown in Example 1 below, although a temporary mass increase occurs at the beginning of the oxidation treatment, the subsequent mass increase is significantly suppressed. In other words, the dense oxide film formed in the austenitic steel of this embodiment is thought to effectively suppress the penetration of external oxidation and the migration of Fe and Mn from the inside of the austenitic steel to the surface side once the oxide film is formed.

[0055] As described above, the austenitic steel of this embodiment has a high Mn content and contains Al and Si as essential components, thereby achieving high mechanical strength. 2 O 3 Even in the case of austenitic steels that do not contain Cr, high mechanical strength can be obtained.

[0056] The austenitic steel according to the present embodiment can be produced by any method for manufacturing this type of alloy, without any particular limitations. That is, the above-described raw material metals are mixed to the above-described contents, heated to a high temperature to melt, and then forged or cast to produce austenitic steel. Further processing, such as rolling or heat treatment, can be carried out to obtain a desired shape and configuration, thereby producing an austenitic steel part. Each processing step can be carried out under conditions that are normally employed.

[0057] This austenitic steel can also be obtained by powder metallurgy, in which the above-mentioned raw metal powders are placed in a mold and compressed under pressure, and then heated to a high temperature to sinter, or the raw metal powders are mechanically mixed in a ball mill (mechanical alloying) and then sintered to produce austenitic steel.

[0058] Y as raw material 2 O 3 When using the above, it is preferable to produce austenitic steel as a dispersion-strengthened alloy by powder metallurgy such as mechanical alloying. The obtained austenitic steel can be further heated and formed and processed into various desired shapes by hot forging.

[0059] The fusion device 1 described with reference to Figure 1 is a helical-type fusion device. In the case of a helical-type fusion device 1, the fusion plasma 21 has a complex shape compared to a tokamak-type fusion device. Therefore, the blanket 20 and divertor 30 of the fusion device 1 also have complex shapes. Additive manufacturing (AM) technology, which three-dimensionally layers raw materials, is an effective method for manufacturing parts with such complex shapes.

[0060] When a manufacturing method using powder metallurgy is adopted, a molding method using AM (Additive Manufacturing) technology is particularly effective because powder can be used as a raw material.

[0061] The austenitic steel of this embodiment will be described in more detail below with reference to examples, comparative examples, and study examples, but the present invention is not limited to these examples.

[0062] Example 1: Raw powders were prepared in a glove box under an argon atmosphere. The raw powders were then ball-milled using a planetary ball mill at 300 rpm for 48 hours with a ball-to-powder ratio of 10:1. The as-milled powders were consolidated by spark plasma sintering (SPS) at 1050°C and a constant axial pressure of 50 MPa. Finally, the as-sintered cylinders were hot-rolled at 1050°C with a forging ratio of 3:1, annealed at 1050°C for 2 hours, and subsequently quenched in water to produce a sintered alloy containing, in mass%, Fe-30Mn-6Al-0.3C-1Si-1Y. 2 O 3 The austenitic steel having the composition was obtained.

[0063] Comparative Example 1: A sintered body containing, in mass %, Fe-30Mn-6Al-0.3C-1Cr-1Y was prepared in the same manner as in Example 1. 2 O 3 The austenitic steel having the composition was obtained.

[0064] [Oxidation Resistance Test] For the austenitic steels obtained in Example 1 and Comparative Example 1, as-rolled samples were cut by wire electric discharge machining, polished with a 1 μm diamond spray, and finally measured to a size of 9 mm × 9 mm × 0.5 mm. A hole with a diameter of 1.5 mm was drilled, and Al 2 O 3 The sample was hooked using a rod, and an oxidation test was performed using a muffle furnace in an air atmosphere at 600°C. The mass increase due to oxidation after several exposure times (1, 4, 9, 16, 25, 49, 100, and 225 hours) was measured with a precision electronic balance (product name: MC 5, manufactured by Sartorius) at a resolution of 1 μg.

[0065] The results are shown in Figure 2. Figure 2 is a diagram showing the mass gain curves of Example 1 and Comparative Example 1. In Comparative Example 1, the evaluation of the mass gain was sufficiently large, so the oxidation test was terminated after 100 hours. As shown in this figure, in Comparative Example 1, oxidation progressed over time, resulting in a significant increase in mass, whereas in Example 1, although there was a temporary mass gain in the early stages, there was no significant mass gain thereafter.

[0066] In the results shown in Figure 2, when the horizontal axis is plotted as the square root of time, they form a straight line, which shows that the mass increase is proportional to the square root of time. This indicates that the movement of oxygen is rate-limited by diffusion, and that the growth rate of the oxide film is inversely proportional to the thickness of the oxide film. Generally, the proportionality coefficient in this case is called the oxidation rate, and its unit is mg. 2 cm -4 h -1 is.

[0067] When calculated using the above method, the oxidation rate of the austenitic steel of Example 1 shown in FIG. 2 is 5.80×10 -6 mg 2 cm -4 h -1 On the other hand, the value of 6.97 × 10 in Comparative Example 1 shown in FIG. ―2 mg 2 cm -4 h -1 It was.

[0068] Cross-sectional EPMA observations of the samples of Example 1 and Comparative Example 1 were performed using an electron probe microanalyzer (JEOL JXA-8530F). The results confirmed that, in Comparative Example 1, a thick oxide film formed over time, whereas in Example 1, the oxide scale was very thin and showed little change over time. FIG. 3 shows an image of the sample of Example 1 observed with a scanning transmission electron microscope (STEM). FIG. 4 shows an image of the sample of Example 1 observed with an energy dispersive X-ray analyzer (EDS). As shown in FIG. 3 , austenitic steel (non-magnetic austenitic steel) 60 has a scale layer 63 composed of an oxide film 61 primarily composed of magnesium oxide and an oxide film 62 primarily composed of iron oxide. The austenitic steel 60 also has an oxide film 65 that extends continuously along the interface between the base material 64 and the scale layer 63. Furthermore, as shown in FIG. 4, a large amount of Al is detected at the position corresponding to the oxide film 65 in FIG. 3, and therefore, this oxide film 65 can be considered to be a dense film of aluminum oxide.

[0069] 3 and 4, it was confirmed that the austenitic steel 60 has an oxide film 65 containing aluminum oxide on the surface. It is strongly assumed that the improvement in oxidation resistance is due to this dense aluminum oxide film.

[0070] From the above, it was found that the austenitic steel of this embodiment has excellent oxidation resistance at high temperatures.

[0071] Example 2 After vacuum melting raw material metal, the raw material metal was hot forged into a columnar shape to obtain a forged material 70 shown in FIG. 5. FIG. 5 is an explanatory diagram showing the austenitic steel forged material produced as Example 2. The forged material 70 shown in FIG. 5 is an austenitic steel having a composition of Fe-30Mn-5Al-1Si. The forged material 70 shown in FIG. 5 is obtained by dividing a cylindrical plate into four equal parts along two straight lines that pass through the center of the circle and are perpendicular to each other. The forged material 70 has a circumferential portion 71 that includes the outer edge of the circle, and a central portion 72 that is located inside the circumferential portion 71 and includes the center of the circle.

[0072] [Effect of Thermal Aging] After electrical discharge machining of the forged material 70 shown in FIG. 5 , the specimens were punched into cylindrical shapes and subjected to thermal aging evaluation at 700°C for 10, 100, and 1000 hours. The results of the X-ray diffraction analysis of each specimen are shown in FIG. 6 . Furthermore, the results of the X-ray diffraction analysis of the forged material 70 specimens before thermal aging evaluation (i.e., the evaluation results for a holding time of 0 hours) are shown in FIG. 7 . As shown in FIGS. 6 and 7 , there was no change in the diffraction peaks on the metal surface of each specimen after varying the holding time. These results demonstrate that austenite remains stable even when held at high temperatures (e.g., 700°C) for long periods of time (e.g., 1000 hours).

[0073] Furthermore, the results of analyzing the surface of a test specimen obtained by stamping out the forged material 70 (see FIG. 5) into a columnar shape using an electron probe microanalyzer (EMPA) are shown in FIG. 8. As shown in FIG. 8, it can be seen that aluminum is uniformly dispersed on the surface of the test specimen. From this, it is considered that, similar to Example 1, a dense coating containing aluminum oxide is formed on the surface layer of the forged material 70 according to Example 2 after being held in a high-temperature environment. In other words, it is presumed that the austenitic steel according to Example 2 exhibits high oxidation resistance due to the formation of a dense oxide coating containing aluminum oxide on the surface layer, similar to the austenitic steel according to Example 1.

[0074] [Evaluation of mechanical properties in a micro-area] The forged material 70 (see FIG. 5) obtained in Example 2 was used to evaluate the mechanical properties in a micro-area. More specifically, a diamond indenter or the like was pressed against the surface of the forged material, and the indentation load-displacement curve was plotted. The results are shown in FIGS. 9 and 10. FIG. 9 shows the results of evaluating nanoindentation hardness, and FIG. 10 shows the results of evaluating elastic modulus.

[0075] (Comparative Example 2) Here, as a comparative example for evaluating the mechanical strength of the austenitic steel according to Example 2, a single crystal of austenitic steel (equivalent to chromium-nickel stainless steel, SUS316) having a composition of Fe-15Cr-20Ni was prepared, and a diamond indenter or the like was pressed against the surface of the single crystal according to Comparative Example 2, and an indentation load-displacement curve was plotted, as in Example 2. Figures 9 and 10 show the results of Comparative Example 2 together with the results of Example 2. The austenitic steel according to Comparative Example 2 shown in Figures 9 and 10 is used as a standard indicator of the mechanical strength of austenitic steel.

[0076] As shown in Figures 9 and 10, Example 2 has a larger nanoindentation hardness and a lower modulus of elasticity than Comparative Example 2. In other words, it can be seen that the austenitic steel of Example 2 has relatively higher mechanical strength than the austenitic steel of Comparative Example 2. Note that Comparative Example 2 is a single crystal, and has a different crystal structure from the austenitic steel of Example 2, which is not a single crystal. Furthermore, the composition of Comparative Example 2 differs from that of Example 2 in the metals contained other than Fe. Therefore, a pure comparison is difficult. However, Comparative Example 2, like Example 2, has a low content of C, Y 2 O 3 Therefore, it is thought that a high Mn content (rather than Cr and Ni) and the inclusion of Al and Si as essential components contribute to mechanical strength. From the above results, it is believed that austenitic steels with a high Mn content and containing Al and Si as essential components will have a low C, Y content. 2 O 3 It is estimated that even without containing the above, a higher mechanical strength than that of Comparative Example 2 can be obtained.

[0077] [Evaluation by X-ray Diffraction Device] Next, the circumferential portion 71 and the central portion 72 of the forged material 70 shown in FIG. 5 were each divided into three regions, and evaluation was performed using an X-ray diffractometer for each of the regions 70F, 70E, 70D, 70C, 70B, and 70A. The evaluation results are shown in FIG. 11. As shown in FIG. 11, peak P1 was observed in region 70F, which is the outermost surface of the circumferential portion 71. No peak corresponding to peak P1 was observed in other regions. Peak P1 is an aluminum nitride (AlN) peak. That is, in the case of Example 2, it was confirmed that aluminum nitride was present on the outermost surface of the circumferential portion 71, and that aluminum nitride was not distributed in regions other than the outermost surface.

[0078] Because aluminum nitride can cause embrittlement, when processing the austenitic steel according to this embodiment (i.e., austenitic steel with a high Mn content and containing Al and Si as essential components), it is preferable to avoid (remove) the outermost peripheral surface containing aluminum nitride. This allows for the production of a component with high toughness. As already explained, aluminum is distributed throughout the entire forged material 70 (see FIG. 5 ). Therefore, even if the outermost peripheral surface is removed, an oxide film primarily composed of aluminum oxide will form on the surface of the forged material 70 if the forged material is maintained in a high-temperature environment. Therefore, it is believed that the oxidation resistance (corrosion resistance) already explained will be maintained even if the surface of the forged material is removed.

[0079] Next, the results of a tensile strength test will be described as another index of the mechanical strength of the austenitic steel. Note that the following describes Example 3 and Comparative Example 3.

[0080] Example 3: Fe-30Mn-6Al-1Si-1.5Y was prepared by the same method as in Example 1. 2 O 3 The austenitic steel having the composition was obtained.

[0081] Comparative Example 3: Fe-30Mn-5Al-1Si-1.5Y was prepared in the same manner as in Example 1. 2 O 3 The austenitic steel having the composition was obtained.

[0082] [Mass Analysis] The results of mass analysis of the austenitic steels according to Example 3 and Comparative Example 3 are shown in Table 1. As shown in Table 1, Example 3 and Comparative Example 3 are similar except for the difference in the mass percentage of aluminum and the corresponding difference in the mass percentage of the balance Fe. The austenitic steel according to Comparative Example 3 has a mass percentage of Al of less than 5 mass%. That is, the austenitic steel according to Comparative Example 3 will be described as a comparative example because the mass percentage of aluminum, which is an essential component, is less than the lower limit already described.

[0083] Furthermore, in Table 1, carbon (C) was not intentionally added to the austenitic steels of Example 3 and Comparative Example 3. The carbon (C) content shown in Table 1 is the mass percentage of carbon unintentionally mixed in due to contamination during the manufacturing process. The carbon mass percentage listed in Table 1 is sufficiently small compared to the silicon (Si) mass percentage and yttrium (Y) mass percentage, so the influence of the carbon component contributing to mechanical strength is considered to be substantially negligible. Therefore, even if the carbon mass percentage shown in Table 1 were zero, the influence on the results of the tensile strength test described below would be considered to be negligible. In other words, Example 3 and Comparative Example 3 can be considered examples (and comparative examples) in which carbon (C) is not included.

[0084]

[0085] [Tensile Strength Test] SS-J3 (parallel portion thickness 0.50 mm, parallel portion length 5.0 mm, parallel portion width 1.2 mm) micro tensile strength test pieces were taken from the austenitic steels according to Example 3 and Comparative Example 3. Then, these test pieces were placed in a testing machine and subjected to a temperature of 25°C and a strain rate of 6.67 × 10 -4 The pure plastic strain was evaluated as / s, and the results are shown in Figure 12.

[0086] In addition, the 0.2% yield strength (σ 0.2%The ultimate tensile strengths (σ UTS ) were 1435 MPa and 1268 MPa, respectively. u ) were 9.0% and 10%, respectively.

[0087] 12 and the results of the 0.2% proof stress and ultimate tensile strength described above, it was found that when the mass proportions of Mn and Si contained in austenitic steel are fixed, increasing the mass proportion of aluminum can improve the mechanical strength of the austenitic steel. In particular, the ultimate tensile strength of Example 3 is about 13% higher than that of Comparative Example 3.

[0088] As already explained, from the viewpoint of improving the oxidation resistance (corrosion resistance) of austenitic steel, it is preferable that the mass percentage of aluminum is 5 mass% or more. However, from the results shown in FIG. 9, it is clear that from the viewpoint of improving the mechanical strength, the mass percentage of aluminum is preferably 5 mass% or more, and particularly preferably 5.5 mass% or more.

[0089] In Example 3, the mass percentage of Mn is approximately 29.8-30.1 mass%, so if the mass percentage of aluminum becomes excessive while the mass percentage of Mn is fixed, the stability of austenite may be impaired. However, by further increasing the mass percentage of Mn within a range not exceeding 31 mass%, it is believed possible to increase the mass percentage of aluminum up to 7 mass%.

[0090] The present invention is not limited to the above-described embodiments and examples, and various modifications are possible without departing from the spirit and scope of the present invention. For example, in Fig. 1, a helical-type fusion device is described as an example of a magnetic confinement fusion device, but the non-magnetic austenitic steel according to the above-described embodiments can be applied to magnetic confinement fusion devices such as tokamak-type and spheromak-type devices.

[0091] 1, the fusion device 1 has been described as having a blanket 20 and a divertor 30. As a modification of the fusion device 1, it can be applied to a fusion device that does not have a divertor 30. In this case, the blanket 20 also functions as the divertor 30.

[0092] Furthermore, for example, various modified examples have been described above, but a part of an embodiment can be applied in combination with other embodiments.

[0093] The present invention can be used, for example, in a magnetic confinement nuclear fusion device.

[0094] REFERENCE SIGNS LIST 1 Nuclear fusion device 10 Vacuum vessel 20 Blanket 21 Nuclear fusion plasma 30 Divertor 31 Divertor plasma 40 Magnet 50 Cryostat 60 Austenitic steel (non-magnetic austenitic steel) 61 Oxide film 62 Oxide film 63 Scale layer 64 Base material 65 Oxide film 70 Forged material 70A, 70B, 70C, 70D, 70E, 70F Region 71 Circumferential portion 72 Center portion

Claims

1. Mn is 28% by mass or more and 31% by mass or less, Al is 5% by mass or more and 7% by mass or less, Si is 0.5% by mass or more and 2% by mass or less, C is 0% by mass or more and 0.3% by mass or less, Y is 2 O 3 The non-magnetic austenitic steel contains 0 mass % or more and 1.5 mass % or less of Fe, with the balance being Fe and unavoidable impurities.

2. The non-magnetic austenitic steel according to claim 1, wherein the magnetic permeability of said non-magnetic austenitic steel is 1.02 or less.

3. The non-magnetic austenitic steel according to claim 1, having a surface layer containing aluminum oxide.

4. A first component including a non-magnetic austenitic steel, wherein the non-magnetic austenitic steel contains Mn of 28 mass% or more and 31 mass% or less, Al of 5 mass% or more and 7 mass% or less, Si of 0.5 mass% or more and 2 mass% or less, C of 0 mass% or more and 0.3 mass% or less, Y 2 O 3 A magnetic confinement type nuclear fusion device containing 0 mass % or more and 1.5 mass % or less of Fe, with the remainder being Fe and unavoidable impurities.

5. A magnetic confinement type nuclear fusion device according to claim 4, wherein the magnetic permeability of the non-magnetic austenitic steel is 1.02 or less.

6. A magnetic confinement type nuclear fusion device according to claim 4, having a coating containing aluminum oxide on the surface.

7. A magnetic confinement fusion device according to claim 4, wherein the first component is a blanket.

8. A magnetic confinement fusion device according to claim 4, wherein the first component is a divertor.

Citation Information

Patent Citations

  • Molding method of packaging container and molding device of the same

    JP2021028231A

  • On-vehicle display device, method for controlling on-vehicle display device, and computer program

    JP2021133804A

  • Non-magnetic steel high in volume electric resistivity

    JP1984028561A

  • Intergranular corrosion resistant fe-cr-mn series alloy and its use

    JP1991138334A

  • Austenitic high manganese steel with excellent formability, strength and weldability, and method for producing the same

    JP1994505535A