Double-sided adhesive sheet, laminate, and display device

The double-sided adhesive sheet with a controlled gel fraction and high light transmittance composition addresses the issue of copper mesh visibility in touch panels at high temperatures, ensuring transparent and durable display devices.

WO2024242016A1PCT designated stage expired Publication Date: 2024-11-28OJI HLDG CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018113
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional adhesive sheets used with copper mesh-based transparent conductive films in touch panels become visible and reduce transparency when exposed to high temperatures, due to changes in the blackened film's hue, affecting the visibility and design of display devices.

Method used

A double-sided adhesive sheet with a specific composition and photocuring process, using a (meth)acrylic copolymer, monofunctional and bifunctional acrylic acid ester monomers, and a photopolymerization initiator, which maintains a controlled gel fraction ratio and high light transmittance, suppressing the visualization of the copper mesh even at elevated temperatures.

Benefits of technology

The adhesive sheet effectively maintains the transparency and design integrity of display devices by preventing the visualization of the copper mesh, even under high temperature conditions, ensuring excellent visibility and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018113_28112024_PF_FP_ABST
    Figure JP2024018113_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing an adhesive sheet with which the visualization of a copper mesh can be prevented even when the adhesive sheet is bonded to a copper mesh-based transparent electroconductive film. The present invention relates to a double-sided adhesive sheet obtained by photocuring an adhesive composition containing: a (meth)acrylic copolymer (A); a monofunctional (meth)acrylic acid ester monomer (B1) having a C10-20 linear, branched, or cyclic alkyl group; a bifunctional (meth)acrylic acid ester monomer (B2) having a reactive functional group bonded by a linking group derived from a C4-12 linear diol; and a photopolymerization initiator (C), excluding hydrogen abstraction-type polymerization initiators, wherein the gel fraction G1 and the gel fraction G2 of the double-sided adhesive sheet measured by a prescribed measurement method have a relationship of 5 ≤ G2 - G1 ≤ 20.
Need to check novelty before this filing date? Find Prior Art

Description

Double-sided adhesive sheet, laminate and display device

[0001] The present invention relates to a double-sided pressure-sensitive adhesive sheet, a laminate, and a display device.

[0002] In recent years, display devices such as liquid crystal displays (LCDs) and input devices such as touch panels have been widely used in various fields. Touch panels are of various types, including resistive and capacitive types, with capacitive types being the most commonly used. In the manufacture of display devices equipped with these touch panels, transparent adhesive sheets are used to bond optical components, for example, to bond a display device and an input device.

[0003] Traditionally, metal oxides such as ITO (indium tin oxide) have been widely used for transparent conductive films in touch panels. Although ITO is a transparent and conductive material, its conductivity is known to be inferior to that of metals such as copper. For example, using ITO for the transparent conductive film of a large-screen touch panel sensor has been problematic, as it can sometimes result in a loss of detection accuracy. For this reason, the use of a metal mesh such as copper for the transparent conductive film of a touch panel has been considered.

[0004] However, because metal meshes such as copper have a metallic luster, they reflect external light, making the copper mesh (copper wiring) visible, reducing the transparency of the transparent conductive film and the visibility and design of the touch panel. For this reason, studies have been conducted to suppress reflection by overlaying a black oxide film on the copper mesh. For example, Patent Document 1 discloses a conductive laminate for a touch panel, comprising: a light-transmitting substrate; a light-transmitting underlayer; a first copper oxynitride layer located on the underlayer's surface opposite to the surface that contacts the substrate; a copper layer located on the first copper oxynitride layer's surface opposite to the surface that contacts the underlayer; and a second copper oxynitride layer located on the copper layer's surface opposite to the surface that contacts the first copper oxynitride layer. Patent Document 2 also discloses a method for manufacturing a touch panel sensor, which includes the steps of: preparing a double-sided film material by bonding a first single-sided film material having a metal layer and a blackened metal layer in this order on one main surface of the film substrate and a second single-sided film material having a blackened metal layer and a metal layer in this order on one main surface of the film substrate together using an adhesive or bonding agent; simultaneously etching the metal layers of the double-sided film material using a photolithography method with double-sided exposure to form a metal wiring pattern; and bonding a cover glass to the blackened metal layer side using an adhesive or bonding agent and then bonding the film substrate to the metal layer side.

[0005] International Publication No. 2016 / 136117 Japanese Patent Application Laid-Open No. 2015-125563

[0006] However, the inventors' investigations revealed that when a conventional adhesive sheet is attached to a transparent conductive film having a copper mesh overlaid with a blackened film and the film is placed in a high-temperature environment, for example, the hue of the blackened film changes and the copper mesh becomes visible.

[0007] Therefore, in order to solve these problems of the conventional technology, the inventors conducted research with the aim of providing an adhesive sheet that can suppress the visualization of copper mesh even when the adhesive sheet is attached to a copper mesh-based transparent conductive film.

[0008] Specific embodiments of the present invention are described below. [1] A double-sided PSA sheet obtained by photocuring a PSA composition comprising: a (meth)acrylic copolymer (A), a monofunctional (meth)acrylic acid ester monomer (B1) having a linear, branched, or cyclic alkyl group having 10 to 20 carbon atoms, a bifunctional (meth)acrylic acid ester monomer (B2) having reactive functional groups linked by a linking group derived from a linear diol having 4 to 12 carbon atoms, and a photopolymerization initiator (C) excluding hydrogen abstraction polymerization initiators, wherein the gel fractions G1 and G2 of the double-sided PSA sheet measured by the following measurement method satisfy the relationship 5≦G2−G1≦20: (Gel fraction G1) The gel fraction of the double-sided PSA sheet is measured using a plain-woven stainless steel wire mesh with a void ratio (porosity) of 41.6% and a wire diameter of 0.06 mm; (Gel fraction G2) The gel fraction of the double-sided PSA sheet is measured using a twill-woven stainless steel mesh with a void ratio (void fraction) of 27.8% and a wire diameter of 0.04 mm. [2] The double-sided PSA sheet according to [1], wherein the PSA composition further contains an organotin compound (D). [3] The double-sided PSA sheet according to [1] or [2], wherein the (meth)acrylic copolymer contains (a1) units derived from an acrylate having a linear or branched alkyl group with 1 to 10 carbon atoms, (a2) units derived from a methacrylate having a linear or branched alkyl group with 1 to 10 carbon atoms, and (a3) ​​units derived from a hydroxyl group-containing (meth)acrylate. [4] The double-sided PSA sheet according to any one of [1] to [3], wherein the content of the monofunctional (meth)acrylic acid ester monomer (B1) is 0.1 to 10 parts by mass and the content of the bifunctional (meth)acrylic acid ester monomer (B2) is 0.05 to 5 parts by mass per 100 parts by mass of the (meth)acrylic copolymer (A). [5] The double-sided pressure-sensitive adhesive sheet according to any one of [2] to [4], wherein the content of the organotin compound (D) is 0.001 to 0.5 parts by mass relative to 100 parts by mass of the methacrylic copolymer (A). [6] The double-sided pressure-sensitive adhesive sheet according to any one of [1] to [5], wherein the total light transmittance is 80% or more. [7] A laminate comprising the double-sided pressure-sensitive adhesive sheet according to any one of [1] to [6], and a copper mesh-based transparent conductive film.[8] A display device comprising the double-sided pressure-sensitive adhesive sheet according to any one of [1] to [6] and a copper mesh-based transparent conductive film.

[0009] According to the present invention, even when a pressure-sensitive adhesive sheet is attached to a copper mesh-based transparent conductive film, the copper mesh can be prevented from becoming visible, thereby enabling the manufacture of a display device with excellent visibility and design.

[0010] Fig. 1 is a schematic diagram showing an example of the cross section of the configuration of the double-sided PSA sheet of the present invention, and Fig. 2 is a photograph illustrating a method for sealing the PSA layer in a stainless steel wire mesh when measuring the gel fraction of the double-sided PSA sheet.

[0011] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits. In addition, in this specification, "(meth)acrylate" means acrylate or methacrylate.

[0012] (Double-Sided Pressure-Sensitive Adhesive Sheet) The present invention relates to a double-sided pressure-sensitive adhesive sheet obtained by photocuring a pressure-sensitive adhesive composition comprising: a (meth)acrylic copolymer (A); a monofunctional (meth)acrylic acid ester monomer (B1) having a linear, branched, or cyclic alkyl group having 10 to 20 carbon atoms; a bifunctional (meth)acrylic acid ester monomer (B2) having reactive functional groups linked by a linking group derived from a linear diol having 4 to 12 carbon atoms; and a photopolymerization initiator (C) excluding hydrogen abstraction polymerization initiators. The gel fractions G1 and G2 of the double-sided pressure-sensitive adhesive sheet measured using the following measurement method satisfy the relationship 5≦G2−G1≦20. (Gel Fraction G1) The gel fraction of the double-sided pressure-sensitive adhesive sheet is measured using a plain-woven stainless steel wire mesh with a void ratio (porosity) of 41.6% and a wire diameter of 0.06 mm. (Gel fraction G2) The gel fraction of the double-sided PSA sheet is measured using a twill stainless steel wire mesh with a space fraction (void fraction) of 27.8% and a wire diameter of 0.04 mm. Note that in this specification, the space fraction (void fraction) and wire diameter of the stainless steel wire mesh used to measure each gel fraction are values ​​in the manufacturer's catalog or disclosed by the manufacturer.

[0013] The gel fraction G1 of the double-sided PSA sheet is preferably 0 to 60%, and more preferably 2 to 55%. By keeping the gel fraction G1 within this range, oxygen permeability can be ensured to a degree that does not discolor the blackened layer of the copper mesh. As a result, visualization of the copper mesh can be suppressed.

[0014] The gel fraction G1 of the double-sided PSA sheet was measured by the following method. First, the release sheets on both sides were peeled off, and the PSA layer was accurately weighed using a balance capable of measuring to four decimal places in grams. The weight W of the PSA layer sample was determined by rounding the weight to the nearest four decimal places. A The weighed pressure-sensitive adhesive layer sample W was placed at the center of a 6 cm x 6 cm sheet of 150 mesh stainless steel wire mesh (plain weave, wire diameter 0.06 mm, void ratio 41.6%). A[g] is placed on the stainless steel mesh, the mesh is folded in half, and then the open ends (three sides) are folded twice each to close the sample adhesive layer, sealing the sample in the bag-shaped stainless steel mesh. The weight of the stainless steel mesh alone is accurately measured in advance using a balance capable of measuring in grams to four decimal places. The weight W of the stainless steel mesh is calculated by rounding the value to the fourth decimal place. M [g]. Next, the bag-shaped stainless steel wire mesh with the sealed adhesive layer sample is immersed in ethyl acetate at a temperature of 40°C for 24 hours, and then the bag-shaped stainless steel wire mesh with the sealed sample is removed from the ethyl acetate. At this time, components of the adhesive layer may seep out through the mesh of the sealed bag-shaped stainless steel wire mesh and adhere to the surface of the bag-shaped stainless steel wire mesh. Such substances that seep out from the bag-shaped stainless steel wire mesh and adhere to the outside, even if they are in a gel form, are removed using a rag or the like. The surface of the bag-shaped stainless steel wire mesh with only the residue of the adhesive layer sample sealed in this way is further washed with fresh ethyl acetate. The bag-shaped stainless steel wire mesh whose surface has been washed with ethyl acetate is heated in an explosion-proof oven at a temperature of 100°C for 8 hours to completely evaporate the volatile components such as ethyl acetate used for immersion and washing, and then the weight of the bag-shaped stainless steel wire mesh with only the residue of the adhesive layer sample sealed after drying is accurately measured using a balance capable of weighing in grams to four decimal places. The weight measured was rounded off to the fourth decimal place to obtain the weight W of the bag-shaped stainless steel mesh after drying, in which only the residue of the adhesive layer sample was sealed. G The weight (W A [g]), weight of the stainless steel mesh only (W M [g]) and the weight of the stainless steel mesh with only the residue of the adhesive layer sample sealed in (W G The gel fraction G1 is calculated from the weight of the sample (W [g]) using the following formula: Gel fraction G1 = (W G -W M ) / W A ×100...formula

[0015] The double-sided PSA sheet preferably has a gel fraction G2 of 10 to 70%, and more preferably 15 to 65%. By keeping the gel fraction G2 within this range, good adhesive properties such as adhesive strength and durability can be achieved.

[0016] The gel fraction G2 of the double-sided PSA sheet was measured by the following method. First, the release sheets on both sides were peeled off, and the PSA layer was accurately weighed using a balance capable of measuring to four decimal places in grams. The weight W of the PSA layer sample was determined by rounding the weight to the nearest four decimal places. A The weighed pressure-sensitive adhesive layer sample W was placed at the center of a 6 cm x 6 cm sheet of 300 mesh stainless steel wire mesh (twill weave, wire diameter 0.04 mm, void ratio 27.8%). A [g] is placed on the stainless steel mesh, the mesh is folded in half, and then the open ends (three sides) are folded twice each to close the sample adhesive layer, sealing the sample in the bag-shaped stainless steel mesh. The weight of the stainless steel mesh alone is accurately measured in advance using a balance capable of measuring in grams to four decimal places. The weight W of the stainless steel mesh is calculated by rounding the value to the fourth decimal place. M[g]. Next, the bag-shaped stainless steel wire mesh with the sealed adhesive layer sample is immersed in ethyl acetate at a temperature of 40°C for 24 hours, and then the bag-shaped stainless steel wire mesh with the sealed sample is removed from the ethyl acetate. At this time, components of the adhesive layer may seep out through the mesh of the sealed bag-shaped stainless steel wire mesh and adhere to the surface of the bag-shaped stainless steel wire mesh. Such substances that seep out from the bag-shaped stainless steel wire mesh and adhere to the outside, even if they are in a gel form, are removed using a rag or the like. The surface of the bag-shaped stainless steel wire mesh with only the residue of the adhesive layer sample sealed in this way is further washed with fresh ethyl acetate. The bag-shaped stainless steel wire mesh whose surface has been washed with ethyl acetate is heated in an explosion-proof oven at a temperature of 100°C for 8 hours to completely evaporate the volatile components such as ethyl acetate used for immersion and washing, and then the weight of the bag-shaped stainless steel wire mesh with only the residue of the adhesive layer sample sealed after drying is accurately measured using a balance capable of weighing in grams to four decimal places. The weight measured was rounded off to the fourth decimal place to obtain the weight W of the bag-shaped stainless steel mesh after drying, in which only the residue of the adhesive layer sample was sealed. G The weight (W A [g]), weight of the stainless steel mesh only (W M [g]) and the weight of the stainless steel mesh with only the residue of the adhesive layer sample sealed in (W G The gel fraction G2 is calculated from the weight of the sample (W [g]) using the following formula: Gel fraction G2 = (W G -W M ) / W A ×100...formula

[0017] In this embodiment, the value of gel fraction G2 - gel fraction G1 (G2 - G1) is preferably 5 or more, more preferably 6 or more, even more preferably 7 or more, even more preferably 8 or more, even more preferably 9 or more, and particularly preferably 10 or more. Furthermore, the value of G2 - G1 is preferably 20 or less. By controlling the value of G2 - G1 within the above range, discoloration of the blackened film laminated on the copper mesh can be suppressed, and visualization of the copper mesh can be suppressed. In this embodiment, the base polymer is not crosslinked (crosslinking using a crosslinking agent is not performed), and a crosslinked structure is formed using only the active energy ray-curable component, forming an IPN structure in which the base polymer becomes entangled. As a result, it is presumed that it is possible to control the value of gel fraction G2 - gel fraction G1 (G2 - G1) within the above range.

[0018] In this embodiment, by setting the G2-G1 value of the double-sided pressure-sensitive adhesive sheet within the above range, the oxygen permeability (P A As a result, for example, the amount of oxygen present in the vicinity of the blackened film of the copper mesh can be made to be equal to or greater than a certain level. In this case, it is presumed that extraction and reduction of oxygen in the blackened film can be suppressed, and discoloration can be suppressed.

[0019] The double-sided pressure-sensitive adhesive sheet of this embodiment is preferably composed only of a pressure-sensitive adhesive layer, but may also have a support. In this case, examples of the support include plastic films such as polystyrene, styrene-acrylic copolymer, acrylic resin, polyethylene terephthalate, polycarbonate, polyether ether ketone, and triacetyl cellulose; and optical films such as anti-reflection films and electromagnetic wave shielding films. When the double-sided pressure-sensitive adhesive sheet has a support, the gel fraction refers to the gel fraction of the pressure-sensitive adhesive layer. When the double-sided pressure-sensitive adhesive sheet is a pressure-sensitive adhesive sheet, it may be a sheet composed of multiple pressure-sensitive adhesive layers, but is preferably a pressure-sensitive adhesive sheet composed of a single pressure-sensitive adhesive layer.

[0020] Although the application of the double-sided pressure-sensitive adhesive sheet of this embodiment is not particularly limited, it is preferably used for bonding copper mesh-based transparent conductive films, as this can suppress the visualization of the copper mesh. Furthermore, it is preferable that the copper mesh has a blackened film. The blackened film is a film formed by a blackening treatment, in which an anti-reflective black coating is formed on the copper mesh. Examples of blackened films include films containing copper oxide (CuO) and copper oxynitride (CuNO). The blackened film is not particularly limited as long as it can suppress the reflectance of the copper mesh, and known blackened films can be used, such as films containing black pigments. In the blackening treatment, a copper oxide film or copper oxynitride film can be formed on the copper mesh by sputtering or other known methods. Furthermore, the blackening treatment may involve electrodeposition coating of a black pigment.

[0021] In particular, the blackened film is preferably a copper oxide film or a copper oxynitride film. In this case, the double-sided pressure-sensitive adhesive sheet of this embodiment is preferably for bonding a copper mesh-based transparent conductive film with a copper oxide film or a copper mesh-based transparent conductive film with a copper oxynitride film.

[0022] The double-sided pressure-sensitive adhesive sheet of this embodiment can also be used as a component of a general display device or optical device.

[0023] The thickness of the double-sided pressure-sensitive adhesive sheet of this embodiment can be appropriately set depending on the application and is not particularly limited. Typically, the thickness of the double-sided pressure-sensitive adhesive sheet is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 30 μm or more, and particularly preferably 40 μm or more. Furthermore, the thickness of the double-sided pressure-sensitive adhesive sheet is preferably 1000 μm or less, more preferably 800 μm or less, even more preferably 600 μm or less, even more preferably 500 μm or less, and particularly preferably 400 μm or less. By setting the thickness of the double-sided pressure-sensitive adhesive sheet within the above range, it becomes easier to control the gel fraction (G2-G1 value) of the double-sided pressure-sensitive adhesive sheet. Furthermore, by setting the thickness of the double-sided pressure-sensitive adhesive sheet within the above range, it is possible to ensure sufficient conformability to uneven surfaces and further enhance durability.

[0024] The total light transmittance of the double-sided PSA sheet is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. The total light transmittance of the double-sided PSA sheet may be 100%. By setting the total light transmittance of the double-sided PSA sheet within the above range, transparency can be increased, making it suitable for use in optical applications such as display devices. The total light transmittance is a value measured in accordance with JIS K 7361-1:1997 in an environment of 23°C and 50% relative humidity.

[0025] The haze of the double-sided pressure-sensitive adhesive sheet is preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less. The lower limit of the haze value of the double-sided pressure-sensitive adhesive sheet is not particularly limited and may be 0%. By setting the haze of the double-sided pressure-sensitive adhesive sheet within the above range, transparency can be increased, making it suitable for optical applications such as display devices. The haze is a value measured in accordance with JIS K 7136:2000 in an environment of 23°C and relative humidity of 50%.

[0026] The adhesive strength of the double-sided pressure-sensitive adhesive sheet to glass is preferably 2 N / 10 mm or more, more preferably 5 N / 10 mm or more. Furthermore, the adhesive strength of the double-sided pressure-sensitive adhesive sheet to glass is preferably 25 N / 10 mm or less, more preferably 20 N / 10 mm or less. By setting the adhesive strength of the double-sided pressure-sensitive adhesive sheet to glass above the above range, unintended peeling does not occur, while by setting it below the above range, it can be easily peeled off in the event of incorrect application or when dismantling the panel for recycling. The adhesive strength of the double-sided pressure-sensitive adhesive sheet described above is the value of the adhesive strength to glass measured in accordance with the adhesive strength measurement method specified in JIS Z 0237, using a 100 μm thick polyethylene terephthalate (PET) film backed on one side of the double-sided pressure-sensitive adhesive sheet and soda glass as the adherend.

[0027] (Adhesive Composition) The double-sided adhesive sheet of the present embodiment is formed from an adhesive composition containing: a (meth)acrylic copolymer (A); a monofunctional (meth)acrylic acid ester monomer (B1) having a linear, branched or cyclic alkyl group having 10 to 20 carbon atoms; a bifunctional (meth)acrylic acid ester monomer (B2) having reactive functional groups linked by a linking group derived from a linear diol having 4 to 12 carbon atoms; and a photopolymerization initiator (C) excluding hydrogen abstraction polymerization initiators.

[0028] ((Meth)acrylic Copolymer (A)) The (meth)acrylic copolymer (A) preferably has a transparency that does not reduce the visibility of a display device, and preferably has a unit derived from (meth)acrylate. In this specification, the term "unit" refers to a repeating unit (monomer unit) that constitutes a polymer.

[0029] The (meth)acrylic copolymer (A) preferably contains (a1) units derived from an acrylate having a linear or branched alkyl group having 1 to 10 carbon atoms, (a2) units derived from a methacrylate having a linear or branched alkyl group having 1 to 10 carbon atoms, and (a3) ​​units derived from a hydroxyl group-containing (meth)acrylate. Furthermore, the content of (a1) units derived from an acrylate having a linear or branched alkyl group having 1 to 10 carbon atoms, relative to the total mass of the (meth)acrylic copolymer, is preferably 15 to 79.5 mass%, the content of (a2) units derived from a methacrylate having a linear or branched alkyl group having 1 to 10 carbon atoms is preferably 20 to 79.5 mass%, and the content of (a3) ​​units derived from a hydroxyl group-containing (meth)acrylate is preferably 0.5 to 15 mass%. In this embodiment, the use of a (meth)acrylic copolymer having specific structural units makes it easier to control the gel fraction (G2-G1 value) of the double-sided PSA sheet. This makes it difficult for the blackened film on the copper mesh of the transparent conductive film to be reduced, and discoloration can be effectively suppressed. Furthermore, in this embodiment, by using a (meth)acrylic copolymer having a specific structural unit, the cohesive force of the pressure-sensitive adhesive can be increased, and a pressure-sensitive adhesive sheet with excellent adhesive properties and durability can be obtained.

[0030] -(a1) Units Derived from an Acrylate Having a Linear or Branched Alkyl Group Having 1 to 10 Carbon atoms- (a1) Examples of acrylates having a linear or branched alkyl group having 1 to 10 carbon atoms include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, sec-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, pentyl acrylate, hexyl acrylate, octyl acrylate, isooctyl acrylate, isononyl acrylate, isodecyl acrylate, and 2-ethylhexyl acrylate. These may be used alone or in combination of two or more. Among these, the (meth)acrylic copolymer preferably has units derived from an acrylate having a branched alkyl group having 1 to 10 carbon atoms, and more preferably has units derived from an acrylate having a branched alkyl group having 4 to 10 carbon atoms. The unit derived from such an acrylate having a branched alkyl group preferably includes a unit derived from 2-ethylhexyl acrylate (2EHA). In addition, in this embodiment, the (meth)acrylic copolymer also preferably includes a unit derived from an acrylate having a branched alkyl group with 1 to 10 carbon atoms and a unit derived from an acrylate having a linear alkyl group with 1 to 10 carbon atoms, and more preferably includes a unit derived from an acrylate having a branched alkyl group with 4 to 10 carbon atoms and a unit derived from an acrylate having a linear alkyl group with 1 to 5 carbon atoms.

[0031] The content of (a1) units derived from an acrylate having a linear or branched alkyl group having 1 to 10 carbon atoms is preferably 15% by mass or more, and more preferably 20% by mass or more, relative to the total mass of the (meth)acrylic copolymer. Furthermore, the content of (a1) units derived from an acrylate having a linear or branched alkyl group having 1 to 10 carbon atoms is preferably 79.5% by mass, and more preferably 70% by mass or less, relative to the total mass of the (meth)acrylic copolymer. By ensuring that the content of (a1) units derived from an acrylate having a linear or branched alkyl group having 1 to 10 carbon atoms falls within the above range, it becomes easier to obtain a pressure-sensitive adhesive sheet that can exhibit excellent adhesive strength, appropriately control the gel fraction (value of G2-G1), and suppress visualization of the copper mesh.

[0032] (a2) Units Derived from Methacrylate Having a Linear or Branched Alkyl Group Having 1 to 10 Carbon atoms (a2) Examples of methacrylates having a linear or branched alkyl group having 1 to 10 carbon atoms include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, sec-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, hexyl methacrylate, octyl methacrylate, isooctyl methacrylate, isononyl methacrylate, isodecyl methacrylate, and 2-ethylhexyl methacrylate. These may be used alone or in combination of two or more. Among these, the (meth)acrylic copolymer preferably has units derived from a methacrylate having a branched alkyl group having 1 to 10 carbon atoms, and more preferably has units derived from a methacrylate having a branched alkyl group having 4 to 10 carbon atoms. The unit derived from such a methacrylate having a branched alkyl group preferably includes a unit derived from 2-ethylhexyl methacrylate (2EHMA). In addition, in this embodiment, the (meth)acrylic copolymer also preferably includes a unit derived from a methacrylate having a branched alkyl group with 1 to 10 carbon atoms and a unit derived from a methacrylate having a linear alkyl group with 1 to 10 carbon atoms, and more preferably includes a unit derived from a methacrylate having a branched alkyl group with 4 to 10 carbon atoms and a unit derived from a methacrylate having a linear alkyl group with 1 to 5 carbon atoms.

[0033] It is preferable that the alkyl groups in (a1) the acrylate having a linear or branched alkyl group with 1 to 10 carbon atoms and (a2) the methacrylate having a linear or branched alkyl group with 1 to 10 carbon atoms are the same type.

[0034] The content of (a2) units derived from methacrylate having a linear or branched alkyl group having 1 to 10 carbon atoms is preferably 20% by mass or more, and more preferably 25% by mass or more, relative to the total mass of the (meth)acrylic copolymer. Furthermore, the content of (a2) units derived from methacrylate having a linear or branched alkyl group having 1 to 10 carbon atoms is preferably 79.5% by mass or more, and more preferably 75% by mass or less, relative to the total mass of the (meth)acrylic copolymer. By ensuring that the content of (a2) units derived from methacrylate having a linear or branched alkyl group having 1 to 10 carbon atoms falls within the above range, it becomes easier to obtain a pressure-sensitive adhesive sheet that can exhibit excellent adhesive strength, appropriately control the gel fraction (value of G2-G1), and suppress visualization of the copper mesh.

[0035] -(a3) Units Derived from Hydroxyl Group-Containing (Meth)acrylate- Examples of the (a3) ​​hydroxyl group-containing (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and polyalkylene glycol mono(meth)acrylate. These may be used alone or in combination of two or more. Of these, at least one selected from 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate is preferably used.

[0036] The content of units derived from the (a3) ​​hydroxyl group-containing (meth)acrylate is preferably 0.5% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, relative to the total mass of the (meth)acrylic copolymer. Furthermore, the content of units derived from the (a3) ​​hydroxyl group-containing (meth)acrylate is preferably 15% by mass or less, more preferably 13% by mass or less, relative to the total mass of the (meth)acrylic copolymer. By keeping the content of units derived from the (a3) ​​hydroxyl group-containing (meth)acrylate within the above range, excellent adhesive strength can be exhibited, and the gel fraction (G2-G1 value) of the PSA sheet can be easily controlled.

[0037] -Other Monomer Units- The (meth)acrylic copolymer may contain other monomer units in addition to those described above. Examples of other monomers include (meth)acrylic acid ester units having a cyclic group, such as cyclohexyl (meth)acrylate and benzyl (meth)acrylate, as well as (meth)acrylonitrile, vinyl acetate, styrene, vinyl chloride, vinylpyrrolidone, and vinylpyridine. The content of other monomer units in the (meth)acrylic copolymer is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less.

[0038] -Physical Properties of (Meth)acrylic Copolymer- The weight-average molecular weight of the (meth)acrylic copolymer is preferably 100,000 or more, more preferably 200,000 or more. Furthermore, the weight-average molecular weight of the (meth)acrylic copolymer is preferably 3,000,000 or less, more preferably 2,000,000 or less. By setting the weight-average molecular weight within the above range, it becomes easier to appropriately control the gel fraction (G2-G1 value) of the PSA sheet, and sufficient conformability to uneven surfaces can be ensured. The weight-average molecular weight of the (meth)acrylic copolymer is the weight-average molecular weight of the (meth)acrylic copolymer contained in the PSA composition. The weight-average molecular weight is a value measured by gel permeation chromatography (GPC) and calculated using polystyrene as a standard.

[0039] (Monofunctional (meth)acrylic acid ester monomer (B1)) The monofunctional (meth)acrylic acid ester monomer (B1) is a monomer having one reactive double bond in the molecule and having a linear, branched, or cyclic alkyl group having 10 to 20 carbon atoms. Examples of the monofunctional (meth)acrylic acid ester monomer (B1) having a linear, branched, or cyclic alkyl group having 10 to 20 carbon atoms include isobornyl (meth)acrylate, isostearyl (meth)acrylate, stearyl acrylate (meth)acrylate, lauryl (meth)acrylate, isodecyl (meth)acrylate, cetyl (meth)acrylate, isomyristyl (meth)acrylate, undeca(meth)acrylate, tridecyl (meth)acrylate, and dicyclopentanyl (meth)acrylate. Among them, the monofunctional (meth)acrylic acid ester monomer (B1) is preferably at least one selected from the group consisting of isobornyl (meth)acrylate, isostearyl (meth)acrylate, and lauryl (meth)acrylate. Commercially available examples of the monofunctional (meth)acrylic acid ester monomer (B1) include IBXA manufactured by Osaka Organic Chemical Industry Ltd., ISTA manufactured by Osaka Organic Chemical Industry Ltd., and LA manufactured by Osaka Organic Chemical Industry Ltd.

[0040] In this embodiment, by using a monomer having a carbon number within a predetermined range as the monofunctional (meth)acrylic acid ester monomer (B1), the crosslink density of the polymer in the double-sided PSA sheet can be controlled, and a loose network structure can be formed. This allows the value of the gel fraction G2 - gel fraction G1 (G2 - G1) of the double-sided PSA sheet to be within a predetermined range, thereby increasing the oxygen permeability of the double-sided PSA sheet and suppressing discoloration of the blackened film of the copper mesh.

[0041] In the pressure-sensitive adhesive composition, the content of the monofunctional (meth)acrylic acid ester monomer (B1) relative to 100 parts by mass of the (meth)acrylic copolymer (A) is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more. Furthermore, the content of the monofunctional (meth)acrylic acid ester monomer (B1) is preferably 10 parts by mass or less. By ensuring that the content of the monofunctional (meth)acrylic acid ester monomer (B1) falls within the above range, the value of the gel fraction G2 - gel fraction G1 (G2 - G1) of the double-sided pressure-sensitive adhesive sheet can be set within a predetermined range, thereby increasing the oxygen permeability of the double-sided pressure-sensitive adhesive sheet and suppressing discoloration of the blackened film of the copper mesh.

[0042] (Bifunctional (meth)acrylic acid ester monomer (B2)) The bifunctional (meth)acrylic acid ester monomer (B2) has two reactive functional groups. The two reactive functional groups are linked by a linking group derived from a linear diol having 4 to 12 carbon atoms. The two reactive functional groups are more preferably linked by a linking group derived from a linear diol having 6 to 12 carbon atoms, and even more preferably linked by a linking group derived from a linear diol having 6 to 10 carbon atoms.

[0043] The bifunctional (meth)acrylic acid ester monomer (B2) is preferably one represented by the following structural formula:

[0044] In the above formula, R 1 and R 2 are each independently a hydrogen atom or a methyl group, and preferably a hydrogen atom. R is a linear alkylene group having 4 to 12 carbon atoms, and R is preferably an alkylene group having 6 to 12 carbon atoms, and more preferably an alkylene group having 6 to 10 carbon atoms.

[0045] Examples of bifunctional (meth)acrylic acid ester monomers (B2) in which reactive functional groups are linked by a linking group derived from a linear diol having 4 to 12 carbon atoms include 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, and 1,10-decanediol diacrylate. Among these, the bifunctional (meth)acrylic acid ester monomer (B2) is preferably at least one selected from the group consisting of 1,6-hexanediol diacrylate and 1,10-decanediol diacrylate. Commercially available examples of bifunctional (meth)acrylic acid ester monomers (B2) include A-HD-N, A-NOD-N, and A-DOD-N manufactured by Shin-Nakamura Chemical Co., Ltd.

[0046] In this embodiment, by using a bifunctional (meth)acrylic acid ester monomer (B2) in which reactive functional groups are linked by a linking group derived from a linear diol having 4 to 12 carbon atoms, it becomes easier to appropriately control the gel fraction (value of G2-G1) of the double-sided PSA sheet measured by the above-mentioned measurement method, and as a result, visualization of the copper mesh can be effectively suppressed when the PSA sheet is attached to a copper mesh-based transparent conductive film. This is thought to be because the flexibility of the (meth)acrylic copolymer (A), which is the base polymer, can be increased by linking the two reactive functional groups via a linear diol having 4 to 12 carbon atoms, which has high structural flexibility.

[0047] In this embodiment, by using the bifunctional (meth)acrylic acid ester monomer (B2) as described above, the crosslink density of the polymer in the PSA sheet can be controlled, and a loose network structure can be formed. This allows the value of the gel fraction G2 - gel fraction G1 (G2 - G1) of the double-sided PSA sheet to be within a predetermined range, thereby increasing the oxygen permeability of the double-sided PSA sheet and suppressing discoloration of the blackened film of the copper mesh.

[0048] In the pressure-sensitive adhesive composition, the content of the bifunctional (meth)acrylic acid ester monomer (B2) relative to 100 parts by mass of the (meth)acrylic copolymer (A) is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.2 parts by mass or more. Furthermore, the content of the bifunctional (meth)acrylic acid ester monomer (B2) is preferably 5 parts by mass or less. By ensuring that the content of the bifunctional (meth)acrylic acid ester monomer (B2) falls within the above range, the value of the gel fraction G2 - gel fraction G1 (G2 - G1) of the double-sided pressure-sensitive adhesive sheet can be kept within a predetermined range, thereby increasing the oxygen permeability of the double-sided pressure-sensitive adhesive sheet and suppressing discoloration of the blackened film of the copper mesh.

[0049] (Photopolymerization initiator (C)) The photopolymerization initiator (C) initiates polymerization of a polyfunctional monomer by irradiation with active energy rays. Here, "active energy rays" refers to electromagnetic waves or charged particle rays that have an energy quantum, and examples thereof include ultraviolet rays, electron beams, visible light, X-rays, and ion beams. Among these, ultraviolet rays or electron beams are preferred from the viewpoint of versatility, and ultraviolet rays are particularly preferred.

[0050] The photopolymerization initiator (C) used in this embodiment is a photopolymerization initiator other than a hydrogen abstraction polymerization initiator. By using a photopolymerization initiator other than a hydrogen abstraction polymerization initiator, discoloration of the blackened layer can be more effectively suppressed.

[0051] Examples of the photopolymerization initiator (C) include hydroxyalkylphenone-based photopolymerization initiators such as 1-hydroxycyclohexyl phenyl ketone; acetophenone-based photopolymerization initiators such as 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 1-[4-(2-hydroxyethoxyl)-phenyl]-2-hydroxy-methylpropanone, and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methyl-1-propanone; acylphosphine oxide-based photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and 2,4,6-trimethylbenzoyl)phenylphosphine oxide; and oil-soluble polymerization initiators such as oxime ester-based photopolymerization initiators and cationic photopolymerization initiators. Among these, the photopolymerization initiator is preferably at least one selected from the group consisting of hydroxyalkylphenone-based photopolymerization initiators and acylphosphine oxide-based photopolymerization initiators.

[0052] Commercially available photopolymerization initiators (C) include Omnirad 819 and Omnirad 184 manufactured by IGM Resins B.V.

[0053] The content of the photopolymerization initiator (C) in the pressure-sensitive adhesive composition is preferably 0.01 parts by mass or more, and more preferably 0.05 parts by mass or more, per 100 parts by mass of the (meth)acrylic copolymer. Furthermore, the content of the photopolymerization initiator (C) in the pressure-sensitive adhesive composition is preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, per 100 parts by mass of the (meth)acrylic copolymer. By keeping the content of the photopolymerization initiator within the above range, the hardness of the double-sided pressure-sensitive adhesive sheet can be increased, and the durability, processability, and adhesion of the double-sided pressure-sensitive adhesive sheet can be improved.

[0054] (Organotin Compound (D)) The PSA composition may contain an organotin compound (D). Examples of the organotin compound (D) include dimethyltin dichloride, dimethyltin dilaurate, dimethyltin di(2-ethylhexanoate), dimethyltin diacetate, dibutyltin dilaurate, dihexyltin diacetate, dioctyltin dilaurate, dibutyltin diacetylacetonate, dibutyltin diacetate, dibutyltin dioctoate, dioctyltin diacetylacetonate, dioctyltin diketanoate, dioctylstannoxane, dioctyltin dicarboxylate, dioctyltin oxide, dimethyltin bis(isooctylthioglycolate) salt, dioctyltin bis(isooctylthioglycolate) salt, tin octoate, and tin decanoate. Among these, it is preferable to use at least one selected from dioctyltin dilaurate and dioctyltin oxide as the organotin compound, and it is more preferable to use dioctyltin dilaurate.

[0055] In this embodiment, the content of the organotin compound (D) contained in the pressure-sensitive adhesive composition is preferably 0.5 parts by mass or less, more preferably 0.4 parts by mass or less, even more preferably 0.3 parts by mass or less, even more preferably 0.2 parts by mass or less, and particularly preferably 0.1 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic copolymer. The content of the organotin compound (D) contained in the pressure-sensitive adhesive composition is preferably 0.001 parts by mass or more relative to 100 parts by mass of the (meth)acrylic copolymer. By setting the content of the organotin compound (D) contained in the pressure-sensitive adhesive composition within the above range, the blackened film on the copper mesh of the transparent conductive film is less likely to be reduced, discoloration can be effectively suppressed, and visualization of the copper mesh can be suppressed.

[0056] (Solvent) The pressure-sensitive adhesive composition may further contain a solvent, which is used to improve the coatability of the pressure-sensitive adhesive composition.

[0057] Examples of such solvents include hydrocarbons such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; halogenated hydrocarbons such as dichloromethane, trichloroethane, trichloroethylene, tetrachloroethylene, and dichloropropane; alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, isobutyl alcohol, and diacetone alcohol; ethers such as diethyl ether, diisopropyl ether, dioxane, and tetrahydrofuran; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, isophorone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, amyl acetate, and ethyl butyrate; and polyols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate, and derivatives thereof.

[0058] The solvent may be used alone or in combination of two or more. The content of the solvent in the pressure-sensitive adhesive composition is not particularly limited, but may be 25 parts by mass or more and 500 parts by mass or less, and 30 parts by mass or more and 400 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic copolymer. Furthermore, the content of the solvent may be 10% by mass or more and 90% by mass or less, and 20% by mass or more and 80% by mass or less, relative to the total mass of the pressure-sensitive adhesive composition.

[0059] (Optional Components) In this embodiment, the pressure-sensitive adhesive composition may contain optional components such as those listed below, depending on the application and required properties. However, it is preferable that the pressure-sensitive adhesive composition does not substantially contain a crosslinking agent. Specifically, the content of the crosslinking agent in the pressure-sensitive adhesive composition is preferably 0.1 mass % or less. When the content of the crosslinking agent in the pressure-sensitive adhesive composition is within the above range, it can be said that the pressure-sensitive adhesive composition does not substantially contain a crosslinking agent.

[0060] Examples of optional components include silane coupling agents, plasticizers, antioxidants, metal corrosion inhibitors, tackifiers, polymerization initiators, polymerizable monomers, ultraviolet absorbers, etc. In this case, the content of the optional components is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, even more preferably 1 part by mass or less, still more preferably 0.5 parts by mass or less, and particularly preferably 0.1 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic copolymer.

[0061] As the silane coupling agent, for example, a reactive functional group-containing silane coupling agent can be used. Examples include mercapto-based silane coupling agents, (meth)acrylic silane coupling agents, isocyanate-based silane coupling agents, epoxy-based silane coupling agents, and amino-based silane coupling agents. Examples of mercapto-based silane coupling agents include mercaptoalkoxysilane compounds (e.g., mercapto group-substituted alkoxy oligomers), but as described below, attention must be paid to the content. Other reactive functional group-containing silane coupling agents include those described in

[0094] to

[0096] of JP 2020-114914 A.

[0062] Examples of plasticizers include non-functional acrylic polymers. Examples of antioxidants include phenol-based antioxidants, amine-based antioxidants, lactone-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants. Examples of metal corrosion inhibitors include benzotriazole-based resins. Examples of tackifiers include rosin-based resins, terpene-based resins, terpene-phenol-based resins, coumarone-indene-based resins, styrene-based resins, xylene-based resins, phenol-based resins, petroleum resins, and methacrylic resins. Examples of ultraviolet absorbers include benzotriazole-based compounds and benzophenone-based compounds.

[0063] The pressure-sensitive adhesive composition of the present embodiment is also preferably one that does not contain any of the optional components described above, and contains, as solid components, only the (meth)acrylic copolymer (A), a monofunctional (meth)acrylic acid ester monomer (B1) having a linear, branched, or cyclic alkyl group having 10 to 20 carbon atoms, a bifunctional (meth)acrylic acid ester monomer (B2) having a reactive functional group linked by a linking group derived from a linear diol having 4 to 12 carbon atoms, and a photopolymerization initiator (C) excluding hydrogen abstraction polymerization initiators. The pressure-sensitive adhesive composition of the present embodiment is also preferably one that contains, as solid components, only the (meth)acrylic copolymer (A), a monofunctional (meth)acrylic acid ester monomer (B1) having a linear, branched, or cyclic alkyl group having 10 to 20 carbon atoms, a bifunctional (meth)acrylic acid ester monomer (B2) having a reactive functional group linked by a linking group derived from a linear diol having 4 to 12 carbon atoms, a photopolymerization initiator (C) excluding hydrogen abstraction polymerization initiators, and an organotin compound (D).

[0064] (Double-sided PSA sheet with release sheet) A release sheet is preferably attached to at least one surface of the double-sided PSA sheet of this embodiment. This embodiment also relates to a double-sided PSA sheet with a release sheet. The release sheet is peeled off from the double-sided PSA sheet when the double-sided PSA sheet is used.

[0065] Fig. 1 is a cross-sectional view showing an example of the configuration of a double-sided pressure-sensitive adhesive sheet with a release sheet. The double-sided pressure-sensitive adhesive sheet 1 shown in Fig. 1 has release sheets 12 (12a, 12b) on both sides of a pressure-sensitive adhesive layer 11. The double-sided pressure-sensitive adhesive sheet in Fig. 1 is a non-carrier type single-layer pressure-sensitive adhesive sheet, and is a double-sided pressure-sensitive adhesive sheet.

[0066] Examples of the release sheet include a release laminate sheet having a release sheet substrate and a release agent layer provided on one side of the release sheet substrate, or a polyolefin film such as a polyethylene film or a polypropylene film as a low-polarity substrate. Paper or a polymer film is used as the release sheet substrate in the release laminate sheet. Examples of the release agent constituting the release agent layer include general-purpose addition-type or condensation-type silicone-based release agents and long-chain alkyl group-containing compounds. In particular, addition-type silicone-based release agents with high reactivity are preferably used. Specific examples of silicone-based release agents include BY24-4527 and SD-7220 manufactured by Toray Dow Corning Silicone Co., Ltd., and KS-3600, KS-774, and X62-2600 manufactured by Shin-Etsu Chemical Co., Ltd. Furthermore, the silicone-based release agent may contain SiO 2 Units and (CH 3 ) 3 SiO 1/2 Unit or CH 2 =CH(CH 3 ) SiO 1/2 It is preferable to contain a silicone resin, which is an organosilicon compound having a unit. Specific examples of silicone resins include BY24-843, SD-7292, and SHR-1404 manufactured by Toray Dow Corning Silicone Co., Ltd., and KS-3800 and X92-183 manufactured by Shin-Etsu Chemical Co., Ltd.

[0067] In order to facilitate peeling, it is preferable that the release sheets 12a and 12b have different releasability in the release sheet 12. In other words, if the releasability from one side is different from the releasability from the other side, it becomes easy to peel off only the release sheet 12 with the higher releasability first. In this case, the releasability of the release sheets 12a and 12b may be adjusted depending on the lamination method and lamination order.

[0068] (Method for manufacturing double-sided pressure-sensitive adhesive sheet) The manufacturing process of the double-sided pressure-sensitive adhesive sheet of this embodiment preferably includes a step of applying a pressure-sensitive adhesive composition onto a release sheet to form a coating film. Hereinafter, the step of applying a pressure-sensitive adhesive composition onto a release sheet to form a coating film will be described as a representative example.

[0069] The PSA composition for forming the PSA sheet can be applied using a known coating device, such as a blade coater, air knife coater, roll coater, bar coater, gravure coater, microgravure coater, rod blade coater, lip coater, die coater, curtain coater, etc. The coating film can be heated using a known heating device, such as a heating furnace or an infrared lamp.

[0070] This embodiment includes a step of photocuring the coating film. That is, the double-sided pressure-sensitive adhesive sheet of this embodiment is a photocurable double-sided pressure-sensitive adhesive sheet. Examples of light used for light irradiation include ultraviolet light and visible light. Of these, ultraviolet light with a wavelength of 250 to 400 nm is preferably used. The ultraviolet irradiation conditions are an irradiance of 0.1 mW / cm when measured using an ultraviolet illuminance meter with spectral sensitivity centered on a wavelength of 365 nm. 2 The light intensity is 500 mJ / cm 2 The above is desirable. By adopting such ultraviolet irradiation conditions, a pressure-sensitive adhesive sheet with a high gel fraction and excellent durability can be obtained. As the light source, a chemical lamp, an ultraviolet fluorescent lamp such as a black lamp, a high-pressure mercury lamp, a low-pressure mercury lamp, an ultra-high-pressure mercury lamp, a mercury-xenon lamp, a metal halide lamp, an LED lamp, a carbon arc, a xenon arc, etc. can be used.

[0071] In the process of photo-curing the coating film, the cumulative amount of ultraviolet light irradiated is 500 mJ / cm 2 It is preferable that the concentration is 1000 mJ / cm or more. 2 More preferably, 1500 mJ / cm or more. 2 It is more preferable that the cumulative amount of ultraviolet light irradiated is 20,000 mJ / cm or more. 2 It is preferable that:

[0072] The double-sided pressure-sensitive adhesive sheet of this embodiment is completely cured by a photo-curing process. The cumulative amount of ultraviolet light required for complete curing varies depending on the components contained in the pressure-sensitive adhesive composition. For example, the cumulative amount of ultraviolet light irradiated is 3000 mJ / cm. 2That is, the double-sided pressure-sensitive adhesive sheet of this embodiment is a pressure-sensitive adhesive composition comprising a (meth)acrylic copolymer (A), a monofunctional (meth)acrylic acid ester monomer (B1) having a linear, branched or cyclic alkyl group having 10 to 20 carbon atoms, a bifunctional (meth)acrylic acid ester monomer (B2) having reactive functional groups linked by a linking group derived from a linear diol having 4 to 12 carbon atoms, and a photopolymerization initiator (C) excluding hydrogen abstraction polymerization initiators, which is exposed to an integrated light dose of 3000 mJ / cm. 2 This double-sided pressure-sensitive adhesive sheet is photocured by irradiating it with ultraviolet light so that the adhesive becomes

[0073] Before the step of photocuring the coating film, a step of drying the coating film may be provided as necessary. The temperature in the drying step is preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher. The temperature in the drying step is preferably 150°C or lower. The treatment time in the drying step is preferably 10 seconds or longer, more preferably 1 minute or longer. The treatment time in the drying step is preferably 1 hour or shorter.

[0074] (Method of Using the Pressure-Sensitive Adhesive Sheet) In a method of using the double-sided pressure-sensitive adhesive sheet of this embodiment, one release sheet of the double-sided pressure-sensitive adhesive sheet with a release sheet is peeled off and the sheet is brought into contact with a copper mesh-based transparent conductive film for bonding, and then the other release sheet is peeled off and the sheet is brought into contact with another adherend. If the pressure-sensitive adhesive sheet is a semi-cured pressure-sensitive adhesive sheet that contains a polymerization initiator and is post-curable, the pressure-sensitive adhesive layer may be completely cured by irradiating it with active energy rays in this state.

[0075] (Laminate / Display Device) This embodiment may relate to a laminate including the above-described double-sided pressure-sensitive adhesive sheet and a copper mesh-based transparent conductive film. For example, in the laminate of this embodiment, it is preferable that a copper mesh-based transparent conductive film is laminated on one side of the double-sided pressure-sensitive adhesive sheet, and another adherend is laminated on the other side of the double-sided pressure-sensitive adhesive sheet. It is preferable that the double-sided pressure-sensitive adhesive sheet is directly attached to the side of the copper mesh-based transparent conductive film on which the copper mesh is formed.

[0076] This embodiment may also relate to a display device including the above-described double-sided pressure-sensitive adhesive sheet and a copper mesh-based transparent conductive film. For example, in the display device of this embodiment, it is preferable that a copper mesh-based transparent conductive film is laminated on one side of the double-sided pressure-sensitive adhesive sheet, and another adherend is laminated on the other side of the double-sided pressure-sensitive adhesive sheet. It is preferable that the double-sided pressure-sensitive adhesive sheet is directly attached to the side of the copper mesh-based transparent conductive film on which the copper mesh is formed.

[0077] Other adherends include, for example, optical components constituting display devices, and examples of optical components include various components in optical products such as touch panels and image display devices. Examples of components for touch panels include hard coat films, fingerprint-resistant films, and cover films. Examples of components for image display devices include anti-reflection films, alignment films, polarizing films, retardation films, and brightness enhancement films used in liquid crystal display devices. Examples of materials used for these components include glass, polycarbonate, polyethylene terephthalate, polymethyl methacrylate, polyethylene naphthalate, cycloolefin polymers, triacetyl cellulose, polyimide, and cellulose acylate.

[0078] [Method for Manufacturing Laminate] The method for manufacturing a laminate of this embodiment preferably includes a step of applying pressure while the double-sided pressure-sensitive adhesive sheet of this embodiment is in contact with the surface of the copper mesh-based transparent conductive film that contacts the copper mesh. In this case, degassing may be performed by applying pressure, or a degassing step may be performed before or after the pressurizing step. The pressurizing step may also be performed while heating is being performed, or a heating step may be performed before or after the pressurizing step. For example, the double-sided pressure-sensitive adhesive sheet may be brought into contact with the copper mesh-based transparent conductive film, and then pressurized, heated, and degassed in this state using an autoclave or the like, or pressurized and vacuum degassed in this state to improve adhesion.

[0079] The features of the present invention will be explained in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, treatment contents, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the specific examples shown below.

[0080] [Synthesis Example] <Synthesis of (meth)acrylic copolymer A-1> 2-ethylhexyl acrylate (2EHA) as an acrylate having a branched alkyl group with 1 to 10 carbon atoms, 2-ethylhexyl methacrylate (2EHMA) as a methacrylate having a branched alkyl group with 1 to 10 carbon atoms, and 2-hydroxyethyl methacrylate (2HEMA) as a hydroxyl group-containing (meth)acrylate were blended in a mass ratio of 2EHA:2EHMA:2HEMA = 20:70:10, and polymerized in ethyl acetate as a polymerization solvent in the presence of AIBN (azobisisobutyronitrile) by heating to 60°C. As a result, a solution (a-1) containing a crosslinkable (meth)acrylic copolymer (A-1) having a solids concentration of 50 mass% and a weight average molecular weight of 480,000 was obtained.

[0081] <Synthesis of (meth)acrylic copolymer A-2> Methyl acrylate (MA) and 2-ethylhexyl acrylate (2EHA) as acrylates having a linear or branched alkyl group containing 1 to 10 carbon atoms, 2-ethylhexyl methacrylate (2EHMA) as a methacrylate having a branched alkyl group containing 1 to 10 carbon atoms, and 2-hydroxyethyl acrylate (2HEA) as a hydroxyl group-containing (meth)acrylate were blended in a mass ratio of MA:2EHA:2EHMA:2HEA = 30:35:25:10, and polymerized in ethyl acetate as a polymerization solvent in the presence of AIBN (azobisisobutyronitrile) by heating to 60°C. This yielded a solution (a-2) containing a crosslinkable (meth)acrylic copolymer (A-2) having a solids concentration of 50% by mass and a weight average molecular weight of 800,000.

[0082] <Synthesis of (meth)acrylic copolymer A-3> 2-ethylhexyl acrylate (2EHA) as an acrylate having a branched alkyl group having 1 to 10 carbon atoms, methyl methacrylate (MMA) and 2-ethylhexyl methacrylate (2EHMA) as methacrylates having a linear and branched alkyl group having 1 to 10 carbon atoms, and 2-hydroxyethyl acrylate (2HEA) as a hydroxyl group-containing (meth)acrylate were blended in a mass ratio of 2EHA:MMA:2EHMA:2HEA = 20:10:60:10, and polymerized in ethyl acetate as a polymerization solvent in the presence of AIBN (azobisisobutyronitrile) by heating to 60°C. This yielded a solution (a-3) containing a crosslinkable (meth)acrylic copolymer (A-3) having a solids concentration of 50% by mass and a weight average molecular weight of 400,000.

[0083] <Synthesis of (meth)acrylic copolymer A-4> Butyl acrylate (BA) as an acrylate having a linear alkyl group having 1 to 10 carbon atoms and 2-hydroxyethyl acrylate (2HEA) as a hydroxyl group-containing (meth)acrylate were blended in a mass ratio of BA:2HEA = 70:30, and polymerized in ethyl acetate as a polymerization solvent in the presence of AIBN (azobisisobutyronitrile) by heating to 60°C. This yielded a solution (a-4) containing a crosslinkable (meth)acrylic copolymer (A-4) with a solids concentration of 50 mass% and a weight average molecular weight of 500,000.

[0084] <Weight-average molecular weight> The weight-average molecular weight of the (meth)acrylic copolymer was measured by gel permeation chromatography (GPC) using the following method. The GPC measurement conditions were as follows: Solvent: tetrahydrofuran Column: Shodex KF801, KF803L, KF800L, KF800D (four columns manufactured by Showa Denko K.K. were connected and used) Column temperature: 40°C Sample concentration: 0.5% by mass Detector: RI-2031plus (manufactured by JASCO) Pump: RI-2080plus (manufactured by JASCO) Flow rate (flow rate): 0.8 ml / min Injection volume: 10 μl Calibration curve: A calibration curve using 10 samples of standard polystyrene Shodex standard polystyrene (manufactured by Showa Denko K.K.) with Mw = 1,320 to 2,500,000 was used.

[0085] Example 1 Preparation of Pressure-Sensitive Adhesive Composition To 100 parts by mass of the (meth)acrylic copolymer (A-1) contained in solution (a-1), 5 parts by mass of isobornyl acrylate (IBXA) as a monofunctional (meth)acrylic acid ester monomer (B1) having a cyclic alkyl group having 10 carbon atoms, 1 part by mass of 1,6-hexanediol diacrylate (A-HD-N) as a bifunctional (meth)acrylic acid ester monomer (B2) in which a reactive functional group is linked by a linking group derived from a linear diol having 6 carbon atoms, and 0.5 parts by mass of Omnirad 819 (manufactured by IGM Resins B.V.) as a photopolymerization initiator were added, and the resulting mixture was added to ethyl acetate so that the concentration of the raw materials was 40% by mass, followed by stirring, to prepare a pressure-sensitive adhesive composition.

[0086] <Preparation of double-sided PSA sheet> The PSA composition prepared as described above was applied uniformly with an applicator to the surface of a 50 μm thick polyethylene terephthalate film (first release sheet, Oji F-Tex Co., Ltd., 50RL-07(2)) equipped with a release agent layer treated with a silicone-based release agent, so as to form a coating film with a coating thickness of 100 μm after drying. This coating film was dried at 80°C for 3 minutes in an air-circulating constant-temperature oven, thereby forming a PSA layer (double-sided PSA sheet of Example 1) on the surface of the first release sheet.

[0087] <Preparation of double-sided pressure-sensitive adhesive sheet with release sheet> Next, a 38 μm thick second release sheet (Oji F-Tex Co., Ltd., 38RL-07(L)) with a release strength different from that of the first release sheet was laminated to the surface of the pressure-sensitive adhesive layer, and the laminate was aged for 14 days at 23°C and a relative humidity of 50%. This resulted in a double-sided pressure-sensitive adhesive sheet with a release sheet, having a first release sheet / double-sided pressure-sensitive adhesive sheet / second release sheet configuration in which the pressure-sensitive adhesive layer (pressure-sensitive adhesive sheet) was sandwiched between a pair of release sheets with different release strengths. Next, a high-pressure mercury lamp was used from the second release sheet side of this pressure-sensitive adhesive sheet with a release sheet, and an integrated light intensity of 3000 mJ / cm was applied. 2 Thus, a photocured double-sided pressure-sensitive adhesive sheet with a release sheet was obtained.

[0088] Example 2 A photocured double-sided PSA sheet with a release sheet was obtained using the same procedure as in Example 1, except that the solution (a-1) of (meth)acrylic copolymer (A-1) was changed to the solution (a-2) of (meth)acrylic copolymer (A-2), and the isobornyl acrylate (IBXA) was changed to isostearyl acrylate (ISTA), a monofunctional (meth)acrylic acid ester monomer having a branched alkyl group with 18 carbon atoms.

[0089] Example 3 The solution (a-1) of the (meth)acrylic copolymer (A-1) was changed to the solution (a-3) of the (meth)acrylic copolymer (A-3), isobornyl acrylate (IBXA) was changed to lauryl acrylate (LA), which is a monofunctional (meth)acrylic acid ester monomer having a linear alkyl group with 12 carbon atoms, and further, 1,6-hexanediol diacrylate (A-HD-N) was changed to 1,10-decanediol diacrylate (A-DOD-N), which is a bifunctional (meth)acrylic acid ester monomer in which reactive functional groups are linked by a linking group derived from a linear diol with 10 carbon atoms, and 0.5 parts by mass of Omnirad 819 (manufactured by IGM Resins B.V.) as a photopolymerization initiator was changed to Omnirad 184 (manufactured by IGM Resins B.V.). A photocured double-sided PSA sheet with a release sheet was obtained in the same manner as in Example 1, except that the amount of the acrylic resin used was changed to 1.0 part by mass of the acrylic resin (manufactured by B.V.).

[0090] Example 4 A photocured double-sided PSA sheet with a release sheet was obtained using the same procedure as in Example 1, except that isobornyl acrylate (IBXA) was changed to isostearyl acrylate (ISTA), a monofunctional (meth)acrylic acid ester monomer having a branched alkyl chain with 18 carbon atoms, 1,6-hexanediol diacrylate (A-HD-N) was changed to 1,10-decanediol diacrylate (A-DOD-N), a bifunctional (meth)acrylic acid ester monomer in which the functional group is linked by a linear diol having 10 carbon atoms, and 0.5 parts by mass of Omnirad 819 (manufactured by IGM Resins B.V.) was changed to 1.0 part by mass of Omnirad 184 (manufactured by IGM Resins B.V.) as the photopolymerization initiator.

[0091] Comparative Example 1 A photocured double-sided PSA sheet with a release sheet was obtained using the same procedure as in Example 1, except that isobornyl acrylate (IBXA) was changed to methyl acrylate (MA), a monofunctional (meth)acrylic acid ester monomer having an alkyl group with one carbon atom.

[0092] Comparative Example 2 A photocured double-sided PSA sheet with a release sheet was obtained using the same procedure as in Example 1, except that the solution (a-1) of base polymer (A-1) was changed to the solution (a-4) of base polymer (A-4), and 1,6-hexanediol diacrylate (A-HD-N) was changed to a trifunctional acrylic acid ester monomer, trimethylolpropane triacrylate (A-TMPT).

[0093] Comparative Example 3 A double-sided PSA sheet with a release sheet was obtained using the same procedure as in Example 1, except that 0.5 parts by mass of an isocyanate-based compound (D-110N, manufactured by Mitsui Chemicals, Inc.) serving as a crosslinking agent was added instead of adding the monofunctional (meth)acrylic acid ester monomer, the bifunctional (meth)acrylic acid ester monomer, and the photoinitiator.

[0094] Example 11 Preparation of Pressure-Sensitive Adhesive Composition To 100 parts by mass of the (meth)acrylic copolymer (A-1) contained in solution (a-1), 5 parts by mass of isobornyl acrylate (IBXA) as a monofunctional (meth)acrylic acid ester monomer (B1) having a cyclic alkyl group having 10 carbon atoms, 1 part by mass of 1,6-hexanediol diacrylate (A-HD-N) as a bifunctional (meth)acrylic acid ester monomer (B2) in which a reactive functional group is linked by a linking group derived from a linear diol having 6 carbon atoms, 0.5 parts by mass of Omnirad 819 (manufactured by IGM Resins B.V.) as a photopolymerization initiator, and 0.02 parts by mass of dioctyltin dilaurate as an organotin compound were added, and the resulting mixture was added to ethyl acetate so that the concentration of the raw materials was 40% by mass, followed by stirring, to prepare a pressure-sensitive adhesive composition.

[0095] <Preparation of double-sided PSA sheet> The PSA composition prepared as described above was applied uniformly with an applicator to the surface of a 50 μm thick polyethylene terephthalate film (first release sheet, Oji F-Tex Co., Ltd., 50RL-07(2)) equipped with a release agent layer treated with a silicone-based release agent, so as to form a coating film with a coating thickness of 100 μm after drying. This coating film was dried at 80°C for 3 minutes in an air-circulating constant-temperature oven, thereby forming a PSA layer (double-sided PSA sheet of Example 11) on the surface of the first release sheet.

[0096] <Preparation of double-sided pressure-sensitive adhesive sheet with release sheet> Next, a 38 μm thick second release sheet (Oji F-Tex Co., Ltd., 38RL-07(L)) with a release strength different from that of the first release sheet was laminated to the surface of the pressure-sensitive adhesive layer, and the laminate was aged for 14 days at 23°C and a relative humidity of 50%. This resulted in a double-sided pressure-sensitive adhesive sheet with a release sheet, having a first release sheet / double-sided pressure-sensitive adhesive sheet / second release sheet configuration in which the pressure-sensitive adhesive layer (pressure-sensitive adhesive sheet) was sandwiched between a pair of release sheets with different release strengths. Next, a high-pressure mercury lamp was used from the second release sheet side of this pressure-sensitive adhesive sheet with a release sheet, and an integrated light intensity of 3000 mJ / cm was applied. 2 Thus, a photocured double-sided pressure-sensitive adhesive sheet with a release sheet was obtained.

[0097] Example 12 A photocured double-sided PSA sheet with a release sheet was obtained in the same manner as in Example 11, except that the solution (a-1) of (meth)acrylic copolymer (A-1) was changed to the solution (a-2) of (meth)acrylic copolymer (A-2), the isobornyl acrylate (IBXA) was changed to isostearyl acrylate (ISTA), which is a monofunctional (meth)acrylic acid ester monomer having a branched alkyl group having 18 carbon atoms, and the dioctyltin dilaurate was changed to dioctyltin oxide.

[0098] Example 13 The solution (a-1) of the (meth)acrylic copolymer (A-1) was changed to the solution (a-3) of the (meth)acrylic copolymer (A-3), isobornyl acrylate (IBXA) was changed to lauryl acrylate (LA), which is a monofunctional (meth)acrylic acid ester monomer having a linear alkyl group with 12 carbon atoms, and further, 1,6-hexanediol diacrylate (A-HD-N) was changed to 1,10-decanediol diacrylate (A-DOD-N), which is a bifunctional (meth)acrylic acid ester monomer in which reactive functional groups are linked by a linking group derived from a linear diol with 10 carbon atoms, and 0.5 parts by mass of Omnirad 819 (manufactured by IGM Resins B.V.) as a photopolymerization initiator was changed to Omnirad 184 (manufactured by IGM Resins B.V.). A photocured double-sided PSA sheet with a release sheet was obtained in the same manner as in Example 11, except that the amount of the adhesive (manufactured by B.V.) was changed to 1.0 part by mass.

[0099] Example 14 A photocured double-sided PSA sheet with a release sheet was obtained in the same manner as in Example 11, except that isobornyl acrylate (IBXA) was changed to isostearyl acrylate (ISTA), a monofunctional (meth)acrylic acid ester monomer having a branched alkyl chain with 18 carbon atoms, 1,6-hexanediol diacrylate (A-HD-N) was changed to 1,10-decanediol diacrylate (A-DOD-N), a bifunctional (meth)acrylic acid ester monomer in which the functional group is linked by a linear diol having 10 carbon atoms, and 0.5 parts by mass of Omnirad 819 (manufactured by IGM Resins B.V.) was changed to 1.0 part by mass of Omnirad 184 (manufactured by IGM Resins B.V.) as the photopolymerization initiator.

[0100] Comparative Example 11 A photocured double-sided PSA sheet with a release sheet was obtained using the same procedure as in Example 11, except that isobornyl acrylate (IBXA) was changed to methyl acrylate (MA), a monofunctional (meth)acrylic acid ester monomer having an alkyl group with one carbon atom.

[0101] Comparative Example 12 A photocured double-sided PSA sheet with a release sheet was obtained using the same procedure as in Example 11, except that the solution (a-1) of base polymer (A-1) was changed to the solution (a-4) of base polymer (A-4), and 1,6-hexanediol diacrylate (A-HD-N) was changed to a trifunctional acrylic acid ester monomer, trimethylolpropane triacrylate (A-TMPT).

[0102] Comparative Example 13 A double-sided PSA sheet with a release sheet was obtained using the same procedure as in Example 11, except that 0.5 parts by mass of an isocyanate-based compound (D-110N, manufactured by Mitsui Chemicals, Inc.) serving as a crosslinking agent was added instead of adding the monofunctional (meth)acrylic acid ester monomer, the bifunctional (meth)acrylic acid ester monomer, and the photoinitiator.

[0103] (Evaluation and Measurement) <Measurement of Gel Fraction G1> The gel fraction G1 of the double-sided PSA sheets with release sheets prepared in the Examples and Comparative Examples was measured by the following method. The first and second release sheets were peeled off, and the PSA layer (double-sided PSA sheet) alone was accurately weighed to three decimal places using a balance capable of weighing in grams to four decimal places (a PSA layer sample of approximately 0.1 g was weighed, and the measured value was rounded to the fourth decimal place to represent the W value). A The weighed pressure-sensitive adhesive layer sample W was placed at the center of a 150-mesh stainless steel wire mesh sheet (plain weave, wire diameter 0.06 mm, porosity 41.6%) measuring 6 cm x 6 cm. AAfter placing a weight [g] on the stainless steel mesh, the mesh was folded in half, and then the open ends (three sides) were folded twice each (Fig. 2), sealing the pressure-sensitive adhesive layer sample inside the bag-shaped stainless steel mesh. The weight of the 6 cm x 6 cm stainless steel mesh alone was accurately measured in advance to three decimal places, similar to the pressure-sensitive adhesive layer sample (the weight W of the stainless steel mesh measured to four decimal places and rounded to the fourth decimal place). M [g]). Next, the bag-shaped stainless steel mesh with the sealed adhesive layer sample was immersed in 100 ml of ethyl acetate at a temperature of 40°C for 24 hours, and then the bag-shaped stainless steel mesh with the sealed sample was taken out of the ethyl acetate. At this time, any adhesive components that had leaked out through the mesh of the sealed bag-shaped stainless steel mesh to the surface were removed using a waste cloth or the like, and the surface of the bag-shaped stainless steel mesh with only the residue of the adhesive layer sample sealed in was washed with fresh ethyl acetate. Next, the bag-shaped stainless steel mesh whose surface had been washed with ethyl acetate was heated in an explosion-proof oven at a temperature of 100°C for 8 hours to evaporate the ethyl acetate, and then the weight after drying was accurately measured to three decimal places (the weight of the bag-shaped stainless steel mesh with only the residue of the adhesive layer sample sealed in after drying, measured to four decimal places, and the value after rounding off to the fourth decimal place was used as the weight W G The weight W of the pressure-sensitive adhesive layer sample thus measured was A [g], weight of stainless steel mesh only W M [g], the weight W of the stainless steel mesh in which only the residue of the adhesive layer sample is sealed G The gel fraction G1 was calculated from [g] using the following formula: Gel fraction G1 = (W G -W M ) / W A ×100...formula

[0104] <Measurement of Gel Fraction G2> The gel fraction G2 of the double-sided PSA sheets with release sheet produced in the Examples and Comparative Examples was determined using the same method as for measuring gel fraction G1, except that the 150-mesh stainless steel wire mesh was replaced with a 300-mesh stainless steel wire mesh (twill weave, wire diameter 0.04 mm, void ratio 27.8%), using the following formula: Gel fraction G2=(W G -W M ) / WA ×100...formula

[0105] <Suitability of copper mesh-based transparent conductive film> (Preparation of conductive film for evaluation) According to the method described in Example 3 of Japanese Patent No. 6607918, a transparent conductive film was prepared by providing a copper conductive layer on both sides of a 100 μm polyethylene terephthalate substrate. Subsequently, a lattice-shaped wiring pattern with a pitch of 200 μm and a line width of 15 μm was formed on the conductive portions on both sides of this conductive film using a photolithography technique, thereby preparing a copper mesh-based transparent conductive film for evaluation. Then, according to the method described in Example 3 of Japanese Patent No. 6607918, a blackened film was formed on the copper mesh.

[0106] (Preparation of Evaluation Samples) The release sheet on the light release side of the double-sided PSA sheets with release sheets prepared in the Examples and Comparative Examples was peeled off, and the sheet was adhered to one side of a glass slide (S9112, manufactured by Matsunami Glass Co., Ltd.) using a hand roller. Next, the release sheet on the heavy release side of the glass-backed PSA sheet was peeled off, and the sheet was adhered to the copper mesh-based transparent conductive film for evaluation prepared above. Next, the double-sided PSA sheets prepared in the Examples and Comparative Examples were adhered to the surface of the copper mesh-based transparent conductive film of the laminate having a "glass / adhesive layer / copper mesh-based transparent conductive film" configuration. Next, the release sheet on the heavy release side was peeled off, and a glass slide (S9112, manufactured by Matsunami Glass Co., Ltd.) was adhered using a vacuum laminating device (JE2020B-MVH model, manufactured by Joyo Engineering Co., Ltd.) to prepare a "glass / adhesive layer / copper mesh-based transparent conductive film / adhesive layer / glass" laminate. Next, this laminate was autoclaved for 30 minutes at 50°C and 0.5 MPa. Thereafter, the film was left to stand for 24 hours under conditions of 23° C. and a relative humidity of 50%, to prepare a sample for evaluating the suitability of the copper mesh-based transparent conductive film.

[0107] (Evaluation of copper mesh-based transparent conductive film suitability) The copper mesh-based transparent conductive film suitability evaluation samples prepared above were treated in an oven at 95°C for 250 hours. Thereafter, the appearance of the evaluation samples was visually observed, and the wiring portion was observed under an optical microscope. The copper mesh-based transparent conductive film suitability was evaluated based on the following evaluation criteria. None of the samples exhibited any lifting, peeling, or bubble formation. A: The copper mesh portion was not visible to the naked eye. There was no color change in the wiring portion even under microscope observation. B: The copper mesh portion was not visible to the naked eye, but a clear hue change was observed in the wiring portion under microscope observation, but the color change was uniform overall. C: The copper mesh portion was not visible to the naked eye, but a clear hue change was observed in the wiring portion under microscope observation, and the hue was different between the edge and center of the sample. D: The edge of the sample appeared slightly cloudy to the naked eye, and a clear hue change was observed in the wiring portion under microscope observation, and the hue was also different between the edge and center of the sample. E: The copper mesh portion was visible to the naked eye, and microscopic observation revealed that the wiring portion had clearly changed in hue and had developed a glossy appearance.

[0108] <Total Light Transmittance and Haze Value> The release sheet on the light release side of the double-sided pressure-sensitive adhesive sheet with release sheet (double-sided pressure-sensitive adhesive sheet thickness: 100 μm) prepared in the Examples and Comparative Examples was peeled off, and the sheet was attached to one side of a glass slide (S9112, manufactured by Matsunami Glass Co., Ltd.) using a hand roller. This laminate was then autoclaved for 30 minutes at 50°C and 0.5 MPa. The release sheet on the heavy release side was then peeled off to prepare an evaluation sample with a "glass / pressure-sensitive adhesive layer" configuration. The total light transmittance of the obtained sample was measured in accordance with JIS K 7361-1. The haze value of the obtained sample was also measured in accordance with JIS K 7136. These measurements were performed three times, and the average value was used for each measurement. An integrating sphere light transmittance measuring device (NDH-5000, manufactured by Nippon Denshoku Industries Co., Ltd.) was used for the measurements. As a result, the double-sided pressure-sensitive adhesive sheets produced in the examples and comparative examples all had a total light transmittance of 90% to 100% in an environment of 23°C and 50% relative humidity, and a haze value of less than 1% in an environment of 23°C and 50% relative humidity.

[0109]

[0110]

[0111] When the double-sided pressure-sensitive adhesive sheet obtained in the examples was attached to a copper mesh-based transparent conductive film and treated under high-temperature conditions, the change in hue of the wiring portion was suppressed and the visibility of the copper mesh portion was suppressed.

[0112] 1 double-sided adhesive sheet with release sheet 11 double-sided adhesive sheet (adhesive layer) 12a, 12b release sheet

Claims

1. A double-sided pressure-sensitive adhesive sheet obtained by photocuring a pressure-sensitive adhesive composition comprising: (A) (meth)acrylic copolymer; (B1) a monofunctional (meth)acrylic acid ester monomer having a linear, branched or cyclic alkyl group having 10 to 20 carbon atoms; (B2) a bifunctional (meth)acrylic acid ester monomer having a reactive functional group linked via a linking group derived from a linear diol having 4 to 12 carbon atoms; and (C) a photopolymerization initiator excluding a hydrogen abstraction type polymerization initiator, wherein the gel fraction G1 and gel fraction G2 of the double-sided pressure-sensitive adhesive sheet measured by the following measurement method satisfy the relationship 5≦G2-G1≦20; (Gel fraction G1) The gel fraction of the double-sided pressure-sensitive adhesive sheet is measured using a plain-woven stainless steel wire mesh having a space ratio (void ratio) of 41.6% and a wire diameter of 0.06 mm; (Gel fraction G2) The gel fraction of the double-sided pressure-sensitive adhesive sheet is measured using a twill-woven stainless steel wire mesh having a space ratio (void ratio) of 27.8% and a wire diameter of 0.04 mm.

2. The double-sided pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive composition further contains an organotin compound (D).

3. The double-sided pressure-sensitive adhesive sheet according to claim 1, wherein the (meth)acrylic copolymer contains (a1) units derived from an acrylate having a linear or branched alkyl group having 1 to 10 carbon atoms, (a2) units derived from a methacrylate having a linear or branched alkyl group having 1 to 10 carbon atoms, and (a3) ​​units derived from a hydroxyl group-containing (meth)acrylate.

4. The double-sided pressure-sensitive adhesive sheet according to claim 1, wherein the content of the monofunctional (meth)acrylic acid ester monomer (B1) is 0.1 to 10 parts by mass, and the content of the bifunctional (meth)acrylic acid ester monomer (B2) is 0.05 to 5 parts by mass, relative to 100 parts by mass of the (meth)acrylic copolymer (A).

5. The double-sided pressure-sensitive adhesive sheet according to claim 1, wherein the content of the organotin compound (D) is 0.001 to 0.5 parts by mass per 100 parts by mass of the (meth)acrylic copolymer (A).

6. The double-sided pressure-sensitive adhesive sheet according to claim 1, having a total light transmittance of 80% or more.

7. A laminate comprising the double-sided pressure-sensitive adhesive sheet according to any one of claims 1 to 6 and a copper mesh-based transparent conductive film.

8. A display device comprising the double-sided pressure-sensitive adhesive sheet according to any one of claims 1 to 6 and a copper mesh-based transparent conductive film.

Citation Information

Patent Citations

  • Curable pressure-sensitive adhesive composition, pressure-sensitive adhesive, and pressure-sensitive adhesive sheet

    JP2014133812A

  • Composite member, adhesive and adhesive sheet

    JP2017196830A

  • Ultraviolet-curable adhesive composition

    JP2019052213A

  • Double-sided adhesive sheet, laminate and display device

    JP7285367B1

  • Adhesive composition, adhesive agent, and adhesive sheet

    WO2015145767A1