Negative electrode for secondary batteries, secondary battery, and method for producing negative electrode for secondary batteries

The integration of a carbon material and Si-based material in the negative electrode composite layer, with controlled pore size distribution, addresses the issue of reduced electrolyte permeability in Si-based batteries, enhancing battery performance and cycle characteristics by facilitating better electrolyte access.

WO2024242077A1PCT designated stage expired Publication Date: 2024-11-28PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018556
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-20
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Si-based materials for secondary batteries experience significant volume expansion and contraction during charging and discharging, leading to reduced electrolyte permeability and impaired charge/discharge cycle characteristics due to low electrolyte penetration in the negative electrode composite material layer.

Method used

A negative electrode with a carbon material and Si-based material composite layer, optimized by controlling pore size distribution through specific surface area and heat treatment, enhancing electrolyte permeability by creating a pore structure that allows easier penetration.

Benefits of technology

The optimized pore structure improves electrolyte permeability, maintaining battery performance and extending charge/discharge cycle characteristics by ensuring effective electrolyte access within the negative electrode composite material layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000023_0000
    Figure 00000023_0000
  • Figure 00000024_0000
    Figure 00000024_0000
Patent Text Reader

Abstract

Provided is a negative electrode for secondary batteries that has satisfactory electrolyte solution permeability. The negative electrode for secondary batteries comprises a negative electrode current collector and a negative electrode mixture layer disposed on the negative electrode current collector. The negative electrode for secondary batteries is characterized in that the negative electrode mixture layer includes a carbon material and a Si-based material, a pore size distribution of the negative electrode mixture layer as measured by mercury intrusion porosimetry has a peak R1 with a maximum value VR1 in a pore size range of 1-3 μm and a peak R2 with a maximum value VR2 in a pore size range of 30-100 μm, and the ratio (VR2 / VR1) of the maximum value VR2 of the peak R2 to the maximum value VR1 of the peak R1 is 0.5-100.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode for secondary battery, secondary battery, and method for manufacturing negative electrode for secondary battery

[0001] The present disclosure relates to a negative electrode for a secondary battery, a secondary battery, and a method for manufacturing a negative electrode for a secondary battery.

[0002] Currently, Si-based materials are attracting attention as a material that can increase the capacity of batteries. Si-based materials are capable of electrochemically absorbing and desorbing lithium ions, and can be charged and discharged at a much higher capacity than carbon materials such as graphite.

[0003] For example, Patent Document 1 discloses a negative electrode active material for a lithium ion secondary battery, which contains a Si-based material represented by SiOx (0<x<2) and a carbon material, and is characterized in that the negative electrode active material for a lithium ion secondary battery has voids inside.

[0004] Furthermore, for example, Patent Document 2 discloses a negative electrode that uses sintered composite particles having a specific pore volume, which are obtained by sintering graphite particles and carbonaceous particles to alloy particles that contain silicon as a constituent element and are capable of absorbing and releasing lithium.

[0005] JP 2013-219059 A JP 2001-210323 A

[0006] While Si-based materials can increase the capacity of secondary batteries, they also undergo large volumetric expansion and contraction during charging and discharging. Therefore, in a negative electrode composite layer containing a Si-based material, the expansion and contraction of the Si-based material increases the amount of electrolyte moving into and out of the negative electrode composite layer. Therefore, if the permeability of the electrolyte into the negative electrode composite layer is low, the amount of electrolyte in the negative electrode composite layer decreases during charging and discharging of the battery, which may result in a deterioration in battery characteristics such as charge-discharge cycle characteristics.

[0007] Therefore, an object of the present disclosure is to provide a negative electrode for a secondary battery that has good electrolyte permeability, a secondary battery including the negative electrode for a secondary battery, and a method for producing the negative electrode for a secondary battery.

[0008] A negative electrode for a secondary battery according to one aspect of the present disclosure includes a negative electrode current collector and a negative electrode composite layer disposed on the negative electrode current collector, the negative electrode composite layer including a carbon material and a Si-based material, and a pore size distribution of the negative electrode composite layer measured by mercury intrusion porosimetry has a maximum value V in the range of pore sizes of 1 μm or more and 3 μm or less. R1 and a maximum value V in the range of pore diameters of 30 μm or more and 100 μm or less. R2 and a peak R2 having a maximum value V R1 The maximum value V of the peak R2 R2 The ratio (V R2 / V R1 ) is 0.5 or more and 100 or less.

[0009] A secondary battery according to one aspect of the present disclosure is characterized by including the negative electrode for secondary batteries described above.

[0010] The method for producing a negative electrode for a secondary battery according to one embodiment of the present disclosure is a method for producing a negative electrode for a secondary battery having a specific surface area of ​​3 m 2 The negative electrode slurry includes a graphite material having a density of 0.1 / g or less, a Si-based material, and vaporized particles that vaporize at a temperature of 100°C or higher and 200°C or lower, and is applied to a negative electrode current collector to form a coating film, followed by rolling the coating film; and a second step of, after the first step, heat-treating the coating film at a temperature of 100°C or higher and 200°C or lower to form a negative electrode composite layer.

[0011] According to the present disclosure, it is possible to provide a negative electrode for a secondary battery that has good electrolyte permeability, a secondary battery including the negative electrode for a secondary battery, and a method for producing the negative electrode for a secondary battery.

[0012] 1 is a cross-sectional view of a secondary battery according to an embodiment of the present invention; 2 is a cross-sectional view of a negative electrode according to an embodiment of the present invention;

[0013] Hereinafter, an example of an embodiment will be described with reference to the drawings. Note that the secondary battery of the present disclosure is not limited to the embodiment described below. Also, the drawings referred to in the description of the embodiment are schematic.

[0014] FIG. 1 is a cross-sectional view of a secondary battery according to an embodiment. The secondary battery 10 shown in FIG. 1 includes a wound electrode assembly 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, an electrolyte, insulating plates 18 and 19 disposed above and below the electrode assembly 14, and a battery case 15 for accommodating the above components. The battery case 15 includes a cylindrical case body 16 with a bottom and a sealing member 17 that closes the opening of the case body 16. Note that, instead of the wound electrode assembly 14, other electrode bodies may be used, such as a laminated electrode body formed by alternately stacking positive and negative electrodes with separators interposed therebetween. Examples of the battery case 15 include cylindrical, rectangular, coin-shaped, or button-shaped metal cases, and resin cases formed by laminating resin sheets (so-called laminated cases).

[0015] The electrolyte may be an aqueous electrolyte, but is preferably a nonaqueous electrolyte containing a nonaqueous solvent and an electrolyte salt dissolved in the nonaqueous solvent. Examples of nonaqueous solvents include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. Examples of nonaqueous solvents include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and mixed solvents of these. The nonaqueous solvent may contain a halogen-substituted compound (e.g., fluoroethylene carbonate) in which at least a portion of the hydrogen atoms of these solvents are substituted with halogen atoms such as fluorine. Examples of electrolyte salts include LiPF 6 Lithium salts such as

[0016] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has, for example, a protruding portion 22, which is a portion of the side surface that protrudes inward and supports the sealing body 17. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.

[0017] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked in this order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disk or ring shape, and all components except for the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. If the internal pressure of the secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 may deform and rupture, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure further increases, the upper valve body 26 may rupture, and gas may be discharged from the opening of the cap 27.

[0018] In the secondary battery 10 shown in Fig. 1, a positive electrode lead 20 attached to the positive electrode 11 passes through a through-hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom side of the case body 16. The positive electrode lead 20 is connected by welding or the like to the underside of a filter 23, which is the bottom plate of the sealing body 17, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected by welding or the like to the inner bottom surface of the case body 16, and the case body 16 serves as the negative electrode terminal.

[0019] The positive electrode 11, the negative electrode 12, and the separator 13 will be described in detail below.

[0020] [Positive Electrode] The positive electrode 11 has a positive electrode current collector and a positive electrode composite layer disposed on the positive electrode current collector. The positive electrode composite layer may be disposed on one side of the positive electrode current collector or on both sides of the positive electrode current collector. The positive electrode current collector may be a foil of a metal, such as aluminum, that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface layer. The positive electrode composite layer is composed of, for example, a positive electrode active material, a binder, a conductive material, and the like. The positive electrode 11 can be produced, for example, by applying a positive electrode slurry containing a positive electrode active material, a binder, a conductive material, and the like to the surface of the positive electrode current collector, drying the coating, and then rolling it to form a positive electrode composite layer on both sides of the positive electrode current collector.

[0021] Examples of conductive materials contained in the positive electrode mixture layer include carbon materials such as carbon black, acetylene black, ketjen black, graphite, carbon nanotubes, etc. Examples of binders contained in the positive electrode mixture layer include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, styrene-butadiene rubber (SBR), cellulose derivatives such as carboxymethyl cellulose (CMC) or a salt thereof, and polyethylene oxide (PEO).

[0022] As the positive electrode active material, for example, a lithium transition metal composite oxide or the like is used. Examples of metal elements contained in the lithium transition metal composite oxide include Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, and W. Among them, it is preferable to contain at least one of Ni, Co, and Mn. An example of a suitable lithium transition metal composite oxide is represented by the general formula LiMO 2 (M is Ni and X, X is a metal element other than Ni, and the proportion of Ni is 50 mol % to 95 mol % based on the total number of moles of the metal elements excluding Li). Examples of X in the above formula include Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, W, etc.

[0023] [Negative Electrode] FIG. 2 is a cross-sectional view of an example of a negative electrode according to an embodiment. The negative electrode 12 includes a negative electrode current collector 40 and a negative electrode composite layer 42 disposed on the negative electrode current collector 40. While FIG. 2 illustrates a configuration in which the negative electrode composite layer 42 is disposed on one side of the negative electrode current collector 40, the negative electrode composite layer 42 may be disposed on both sides of the negative electrode current collector 40. The negative electrode current collector 40 may be a foil of a metal, such as copper, that is stable within the potential range of the negative electrode 12, or a film having such a metal disposed on its surface. The negative electrode composite layer 42 includes a negative electrode active material and may also include a binder, a conductive material, and the like. The negative electrode active material includes a carbon material and a Si-based material. In addition to the carbon material and the Si-based material, the negative electrode active material may also include a material capable of reversibly absorbing and releasing lithium ions. Examples of the binder and conductive material include those similar to those used for the positive electrode 11.

[0024] The pore size distribution of the negative electrode mixture layer 42 measured by mercury porosimetry showed a maximum value V R1 and a maximum value V in the range of pore diameters of 30 μm or more and 100 μm or less. R2 and the maximum value V of the peak R1. R1 The maximum value of peak R2 V R2 The ratio (V R2 / V R1 ) is 0.5 or more and 100 or less, preferably 0.5 or more and 100 or less, more preferably 0.5 or more and 1.0 or less. R1 The maximum value of peak R2 V R2 The ratio (V R2 / V R1 ) satisfies the above range, the permeability of the electrolyte solution into the negative electrode mixture layer 42 is enhanced. That is, the negative electrode 12 has good permeability of the electrolyte solution. The reason why the permeability of the electrolyte solution into the negative electrode mixture layer 42 is enhanced is not clear, but V R2 / V R1 It is presumed that within negative electrode mixture layer 42 where the thickness satisfies the above range, pores with relatively large diameters through which the electrolyte solution can easily permeate are present over a wide area, and as a result, the permeability of the electrolyte solution is thought to be enhanced.

[0025] The pore size distribution of the negative electrode mixture layer 42 measured by mercury porosimetry further shows that the pore size has a maximum value V in the range of 0.1 μm or more and 0.6 μm or less. R3 and the maximum value V of the peak R1. R1 The maximum value V of the peak R3 R3 The ratio (V R3 / V R1 ) is preferably 0.9 or more and 1.5 or less. R1 The maximum value V of the peak R3 R3 The ratio (V R3 / V R1 ) satisfies the above range, for example, the permeability of the electrolyte solution into negative electrode mixture layer 42 can be further improved.

[0026] In mercury intrusion porosimetry, mercury is forced into the pores of a solid sample by pressurizing the mercury, and the diameter and volume of the pores are calculated from the pressure applied to the mercury and the amount of mercury forced into the pores. When mercury to which pressure P is applied can penetrate into a pore of diameter D, the diameter D of the pore can be determined from the pressure P, the contact angle θ of the mercury, and the surface tension σ of the mercury according to the following formula. The pore volume is also calculated from the amount of mercury forced into the pore. In this disclosure, the pore diameter refers to the diameter of the pore. -4σ cos θ = PD

[0027] The pore size distribution measured by mercury intrusion porosimetry is expressed as the log differential pore volume (cm 3 / g) against the average pore diameter (μm) in each measurement section (pore distribution curve), where the horizontal axis represents the pore diameter (μm) and the vertical axis represents the log differential pore volume (cm 3 In the present disclosure, the maximum value of the peak in the pore size distribution means the value of the log differential pore volume at the apex of the peak.

[0028] The pore size distribution is measured by mercury porosimetry on the negative electrode composite layer before initial charging. For example, a measurement sample obtained by punching a negative electrode into a predetermined shape before initial charging can be used to measure the pore size distribution of the negative electrode composite layer of the measurement sample by mercury porosimetry. Note that the measurement sample only needs to have at least the negative electrode composite layer on its surface, and may also have other components such as a negative electrode current collector.

[0029] Measurement of pore size distribution by mercury intrusion porosimetry can be performed using an apparatus such as the Autopore IV9500 series manufactured by Micromeltix. During measurement, a measurement sample is sealed in a sample container under an inert atmosphere, and mercury is injected into the sample container to apply pressure to the mercury. The pressure applied to the mercury is adjusted appropriately depending on the pore size that the measurement sample may have, and is not particularly limited. For example, it is preferable to perform measurement by changing the pressure from 0.5 psi (3.4 kPa) to 60,000 psi (413,400 kPa) in order to be able to measure pore sizes over a wide range.

[0030] In this embodiment, in terms of further enhancing the permeability of the electrolyte solution into the negative electrode mixture layer 42, when the negative electrode mixture layer 42 shown in FIG. 2 is divided into two equal halves in the thickness direction into a lower half region 42a on the negative electrode current collector 40 side and an upper half region 42b on the surface side, the abundance ratio of pores corresponding to peak R2 in the upper half region 42b is preferably greater than the abundance ratio of pores corresponding to peak R2 in the lower half region 42a. As a result, the upper half region 42b on the surface side of the negative electrode mixture layer 42 has a greater number of pores with relatively large diameters through which the electrolyte solution can easily permeate, which facilitates the permeation of the electrolyte solution from the surface of the negative electrode mixture layer 42. As a result, the permeation of the electrolyte solution into the lower half region 42a is less likely to be hindered, which is thought to enhance the permeability of the electrolyte solution into the entire negative electrode mixture layer 42. Dividing negative electrode mixture layer 42 into two equal parts in the thickness direction means dividing negative electrode mixture layer 42 in half at midpoint Z of the thickness of negative electrode mixture layer 42 when the stacking direction of negative electrode current collector 40 and negative electrode mixture layer 42 is the thickness direction of negative electrode mixture layer 42. Then, negative electrode mixture layer 42 is divided into two equal parts in the thickness direction, with the negative electrode mixture layer 42 located closer to negative electrode current collector 40 being defined as lower half region 42a, and the negative electrode mixture layer 42 located farther from negative electrode current collector 40 being defined as upper half region 42b. The abundance ratio of pores corresponding to peak R2 is measured as follows.

[0031] When measuring the pore size distribution by mercury intrusion porosimetry, an electrode sample in which the upper half of the negative electrode composite layer 42 has been scraped off, leaving only the lower half, is measured, and an electrode sample that has not been subjected to the scraping process is also measured, and the ratio of the area of ​​peak R2 to the total area of ​​all pore peaks in the pore distribution curve is compared, whereby the magnitude of the abundance ratio of peak R2 in the upper half and the lower half of the negative electrode composite layer can be easily determined.

[0032] Examples of the Si-based material contained in the negative electrode active material include Si, Si alloys, and Si compounds. The Si-based material may also be, for example, composite particles containing an ion-conducting phase and a silicon phase (silicon particles in one respect) dispersed within the ion-conducting phase. The ion-conducting phase is a phase that conducts ions, and examples thereof include a silicate phase, a carbon phase, and a silicon oxide phase.

[0033] The carbon phase may be composed of, for example, amorphous carbon. Examples of amorphous carbon constituting the carbon layer include hard carbon, soft carbon, and other amorphous carbon. Amorphous carbon has an average interplanar spacing d of (002) planes measured by X-ray diffraction. 002 The carbon material has a particle size of more than 0.34 nm.

[0034] The main component of the silicon oxide phase (for example, 95% by mass or more and 100% by mass or less) may be silicon dioxide. The composition of the composite particles containing the silicon oxide phase and the silicon phase dispersed therein is generally SiO x It can be expressed as: SiO x is a material in which silicon particles are amorphous SiO 2 The oxygen content ratio x to silicon is preferably, for example, 0.5≦x<2.0, and more preferably 0.8≦x≦1.5.

[0035] The silicate phase may satisfy the following conditions (1) and / or (2): (1) The silicate phase contains at least one element selected from the group consisting of alkali metal elements and Group 2 elements (Group 2 elements of the long periodic table). (2) The silicate phase contains element L. The element L is at least one element selected from the group consisting of B, Al, Zr, Nb, Ta, V, lanthanoids, Y, Ti, P, Bi, Zn, Sn, Pb, Sb, Co, Er, F, and W. Lanthanoids is a collective term for 15 elements ranging from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71.

[0036] Regarding the above condition (1), examples of alkali metal elements include lithium (Li), potassium (K), and sodium (Na). Examples of Group 2 elements include magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba). The inclusion of an alkali metal element and / or a Group 2 element may reduce the irreversible capacity of the silicate phase. A silicate phase containing lithium (hereinafter, sometimes referred to as a "lithium silicate phase") is preferable in terms of, for example, a small irreversible capacity and a high initial charge / discharge efficiency.

[0037] The lithium silicate phase may be an oxide phase containing Li, Si, and O, and may contain other elements. The atomic ratio of O to Si in the lithium silicate phase, O / Si, is, for example, greater than 2 and less than 4. Preferably, O / Si is greater than 2 and less than 3. The atomic ratio of Li to Si in the lithium silicate phase, Li / Si, is, for example, greater than 0 and less than 4.

[0038] The lithium silicate phase has the formula: Li 2z SiO (2+z) The lithium silicate phase may contain or be composed of a lithium silicate phase represented by (0<z<2). Preferably, z satisfies the relationship 0<z<1, and z=1 / 2 (i.e., Li 2 Si 2 O 5 ) is more preferred.

[0039] The Si-based material may also include composite particles containing an ion-conducting phase and a silicon phase dispersed within the ion-conducting phase, and a coating layer covering at least a portion of the surface of the composite particles.

[0040] The coating layer present on the surface of the composite particle may include, for example, a conductive layer. Forming a conductive layer on the surface of the composite particle may increase the conductivity of the Si-based material. A conductive material containing carbon is preferred as the conductive material constituting the conductive layer. Examples of conductive materials containing carbon include conductive carbon materials. Examples of conductive carbon materials include carbon black, graphite, and amorphous carbon (amorphous carbon) with low crystallinity. Amorphous carbon is preferred because it has a strong buffering effect on the silicon phase, which changes in volume during charging and discharging. The amorphous carbon may be either easily graphitized carbon (soft carbon) or difficult-to-graphitize carbon (hard carbon). Examples of carbon black include acetylene black and ketjen black. The thickness of the conductive layer may be, for example, in the range of 1 to 200 nm. The thickness of the conductive layer can be measured by observing the cross section of the Si-containing material using a SEM or TEM (transmission electron microscope).

[0041] The content of the Si-based material is preferably 30% by mass or more relative to the total amount of the negative electrode active material, from the viewpoint of increasing the capacity of the secondary battery, etc. Furthermore, from the viewpoint of increasing the capacity of the secondary battery and suppressing swelling of the negative electrode, the content of the Si-based material is preferably 30% by mass or more and 60% by mass or less, and more preferably 35% by mass or more and 55% by mass or less, relative to the total amount of the negative electrode active material.

[0042] The average particle size of the Si-based material is preferably 3 μm or more and 15 μm or less, more preferably 4 μm or more and 12 μm or less, and even more preferably 6 μm or more and 10 μm or less, in terms of suppressing deterioration of charge-discharge cycle characteristics, etc. The average particle size is the volume average particle size D50 at which the volume integrated value becomes 50% in the particle size distribution obtained by the laser diffraction scattering method.

[0043] The carbon material contained in the negative electrode active material may be a conventionally known carbon material used as a negative electrode active material for secondary batteries, and examples thereof include graphite materials such as natural graphite such as flake graphite, lump graphite, and amorphous graphite, and artificial graphite such as lump artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB).

[0044] The carbon material has a specific surface area of ​​3 m 2 It is preferable that the graphite material has a specific surface area of ​​3 m / g or less. 2 When a graphite material having a specific surface area of ​​0.5 m / g or less is contained in negative electrode mixture layer 42, for example, pores corresponding to peak R2 are more likely to be formed in negative electrode mixture layer 42, and the permeability of the electrolyte solution into negative electrode mixture layer 42 is further enhanced. In addition, from the viewpoint of reactivity as an electrode, the specific surface area of ​​the graphite material is 0.5 m / g or less. 2 The specific surface area of ​​the graphite material is preferably 0.5 m / g or more. 2 / g or more, 2.0m 2 The specific surface area of ​​the graphite material is measured by the BET method using a conventionally known specific surface area measuring device (for example, Macsorb (registered trademark) HM model-1201 manufactured by Mountech Co., Ltd.).

[0045] The average particle size of the graphite material is preferably 5 μm or more and 30 μm or less, more preferably 10 μm or more and 25 μm or less, and even more preferably 12 μm or more and 20 μm or less, for example, in terms of suppressing swelling of the negative electrode, etc. The average particle size is the volume average particle size D50 as described above.

[0046] The content of the carbon material is, for example, preferably 40% by mass or more and 70% by mass or less, and more preferably 45% by mass or more and 65% by mass or less, relative to the total amount of the negative electrode active material.

[0047] An example of a method for manufacturing the negative electrode 12 will be described. The negative electrode 12 includes a first step of applying a negative electrode slurry containing a negative electrode active material including a carbon material and a Si-based material, vaporized particles that vaporize at a temperature of 100° C. or higher and 200° C. or lower, and a binder or the like that is added as needed, to a negative electrode current collector 40 to form a coating film, and then rolling the coating film; and a second step of heat-treating the coating film at a temperature of 100° C. or higher and 200° C. or lower to form a negative electrode composite layer 42 after the first step.

[0048] By heat treating the coating film, the vaporized particles are vaporized and released from the coating film, so that not only small pores corresponding to the peaks R1 and R3 but also relatively large pores corresponding to the peak R2 are formed in the coating film. 2 It is preferable to use graphite particles having a specific surface area of ​​3 m / g or less. 2 / g or less is a hard material, so that even if the coating film is rolled, the graphite particles are not easily crushed and the pores in the coating film are easily maintained. According to the above-described manufacturing method, it is easy to obtain negative electrode mixture layer 42 having the above-described pore size distribution.

[0049] The heat treatment time may be set to a time sufficient for vaporizing the vapor particles in the coating film, for example, 5 hours or more.

[0050] The vaporized particles include at least one of a material that sublimes at a temperature of 100° C. or higher and 200° C. or lower, a material that decomposes at a temperature of 100° C. or higher and 200° C. or lower, and a material that melts and then vaporizes at a temperature of 100° C. or higher and 200° C. or lower. Specific examples of the material include dicarboxylic acids such as fumaric acid, malonic acid, and malic acid, metal oxalates, camphor, and naphthalene. The volume average particle size of the vaporized particles is preferably 2 μm or higher and 10 μm or lower, for example, because relatively large pores corresponding to the peak R2 are likely to be formed.

[0051] To obtain the negative electrode slurry, raw materials such as the negative electrode active material and vaporized particles can be mixed using, for example, a cutter mill, a pin mill, a bead mill, a microparticle composite device (a device in which shear force is generated between a rotor having a special shape that rotates at high speed inside a tank and an impact plate), a granulator, or a kneader such as a twin-screw extrusion kneader or a planetary mixer.

[0052] The negative electrode slurry can be applied using, for example, a slit die coater, a reverse roll coater, a lip coater, a blade coater, a knife coater, a gravure coater, or a dip coater.

[0053] When the negative electrode slurry is applied to the negative electrode current collector 40 to obtain a coating film, it is preferable to heat-dry the coating film. The heat-drying temperature may be a temperature at which the vaporized particles do not vaporize, or may be a temperature at which the vaporized particles partially vaporize.

[0054] The coating film may be rolled, for example, by a roll press machine at a predetermined line pressure several times until the coating film reaches a predetermined thickness.

[0055] The maximum value V of the peak R1 in the pore size distribution of the negative electrode mixture layer 42 R1 The maximum value of peak R2 V R2 The ratio (V R2 / V R1 ), the maximum value V of peak R1 R1 The maximum value V of the peak R3 R3 The ratio (V R1 / V R3 ) can be controlled by adjusting, for example, the specific surface area of ​​the graphite particles, the volume average particle size of the vaporized particles, the viscosity of the negative electrode slurry by adding a solvent or the like, the heat treatment time and temperature, the linear pressure during coating film rolling, etc.

[0056] In the first step, for example, anode slurry A containing a carbon material and vaporized particles, and anode slurry B containing a carbon material and vaporized particles having a lower concentration than anode slurry A (which may not contain vaporized particles) may be prepared, and two-layer coating of the anode slurries A and B may be performed on the anode current collector 40. In the two-layer coating, anode slurry B is coated on the anode current collector 40 to form a coating film of anode slurry B, and then anode slurry A is coated on the coating film to form a coating film of anode slurry A. In addition, among the carbon materials contained in anode slurries A and B, at least the carbon material contained in anode slurry A has a specific surface area of ​​3 m 2 / g or less. By applying such a two-layer coating, it becomes easy to make the abundance ratio of pores corresponding to peak R2 in upper half region 42b of negative electrode composite layer 42 greater than the abundance ratio of pores corresponding to peak R2 in lower half region 42a.

[0057] [Separator] The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have either a single-layer structure or a laminated structure. A heat-resistant layer or the like may be formed on the surface of the separator.

[0058] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0059] <Example> [Fabrication of negative electrode] Specific surface area: 1.2 m 2 / g of graphite material and SiO were mixed at a mass ratio of 90:10. This mixture was used as the negative electrode active material. Then, the mass ratio of the negative electrode active material: carboxymethyl cellulose (CMC): styrene-butadiene copolymer rubber (SBR): carbon nanotubes: fumaric acid (average particle size 6 μm) was mixed so that the mass ratio was 100:1:1:1:12.5, and then mixed with optional water to prepare a negative electrode slurry. This negative electrode slurry was applied to both sides of a negative electrode current collector made of copper foil, and after drying the coating, the coating was rolled with a rolling roller. Thereafter, the coating was heat-treated at 200°C for 5 hours, thereby producing a negative electrode in which a negative electrode composite layer was formed on both sides of the negative electrode current collector.

[0060] In the obtained negative electrode, the pore size distribution of the negative electrode mixture layer was measured by mercury porosimetry, and the maximum value (V R1 : 0.087 cm 3 / g), and the maximum value (V R2 : 0.069 cm 3 / g), and the maximum value (V R3 Peak R3 with a % V content of 0.084 was observed. R2 / V R1 is 0.786, V R3 / V R1 was 0.961.

[0061] Comparative Example 1 A negative electrode was fabricated in the same manner as in Example 1, except that fumaric acid was not used. In the negative electrode of Comparative Example 1, the pore size distribution of the negative electrode mixture layer was measured by mercury porosimetry. As a result, the maximum value (V R1 : 0.098 cm 3 / g), and the maximum value (V R2 : 0.047 cm 3 / g), and the maximum value (V R3 Peak R3 with a % V content of 0.094 was observed. R2 / V R1 is 0.484, V R3 / V R1 was 0.959.

[0062] Comparative Example 2 A negative electrode was prepared in the same manner as in Example 2, except that fumaric acid was not used and the linear pressure during rolling of the coating film by a rolling roller was 10% lower than in Example 1. In the negative electrode of Comparative Example 2, the pore size distribution of the negative electrode composite layer was measured by mercury porosimetry. As a result, the maximum value (V R1 : 0.099 cm 3 / g), and the maximum value (V R2 : 0.034 cm 3 / g), and the maximum value (V R3 Peak R3 with a molecular weight of 0.130 was observed. R2 / V R1 is 0.339, V R3 / V R1 was 1.305.

[0063] Comparative Example 3: No fumaric acid was used, and the specific surface area was 0.9 m 2 A negative electrode was fabricated in the same manner as in the Examples, except that a graphite material having a pore diameter of 1.17 μm was used. R1 : 0.171 cm 3 / g), and the maximum value (V R2 : 0.026 cm 3 / g), and the maximum value (V R3 Peak R3 with a molecular weight of 0.177 was observed. R2 / V R1 is 0.154, V R3 / V R1 was 1.035.

[0064] <Comparative Example 4> Specific surface area 4.0 m 2 A negative electrode was fabricated in the same manner as in the Examples, except that a graphite material having a pore diameter of 1.05 μm was used. R1 : 0.356 cm 3 / g), and the maximum value (V R2 : 0.043 cm3 / g), and the maximum value (V R3 Peak R3 with a σ of 0.065 was observed. R2 / V R1 is 0.120, V R3 / V R1 was 0.182.

[0065] [Evaluation of Electrolyte Penetration] LiPF 5 was dissolved in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a mass ratio of 1:3. 6 An electrolyte solution was prepared by dissolving the above electrolyte solution at a concentration of 1 mol / L. 10 μL of the electrolyte solution was dropped onto the negative electrode composite layer of the negative electrodes of the Examples and Comparative Examples, and the time from the dropping of the electrolyte solution until the electrolyte solution could no longer be confirmed on the surface of the negative electrode composite layer was measured as the liquid absorption time. The results are shown in Table 1. In Table 1, the liquid absorption time of Comparative Example 1 is set as the reference (1.00), and the liquid absorption times of Examples and Comparative Examples 2 to 4 are shown as relative values.

[0066]

[0067] As shown in Table 1, the Example had a shorter liquid absorption time than Comparative Examples 1 to 4. That is, in the negative electrode composite layer containing a carbon material and a Si-based material, the pore size distribution measured by mercury intrusion porosimetry showed a maximum value V in the range of pore sizes of 1 μm or more and 3 μm or less. R1 and a maximum value V in the range of pore diameters of 30 μm or more and 100 μm or less. R2 and a peak R2 having a maximum value V R1 The maximum value V of the peak R2 R2 The ratio (V R2 / V R1 ) is 0.5 or more, a negative electrode with good electrolyte permeability can be obtained.

[0068] [Note] (1) A negative electrode composite layer is provided on the negative electrode current collector, and the negative electrode composite layer contains a carbon material and a Si-based material, and the pore size distribution of the negative electrode composite layer measured by mercury intrusion porosimetry has a maximum value V in the range of pore sizes of 1 μm or more and 3 μm or less. R1and a maximum value V in the range of pore diameters of 30 μm or more and 100 μm or less. R2 and a peak R2 having a maximum value V R1 The maximum value V of the peak R2 R2 The ratio (V R2 / V R1 (2) The maximum value V of the peak R1 is 0.5 or more and 100 or less. R1 The maximum value V of the peak R2 R2 The ratio (V R2 / V R1 (3) The negative electrode for a secondary battery according to (1), wherein the maximum value V of the peak R1 is 0.5 or more and 2.0 or less. R1 The maximum value V of the peak R2 R2 The ratio (V R2 / V R1 (4) The negative electrode for a secondary battery according to (2), wherein the pore size distribution of the negative electrode mixture layer has a maximum value V in the range of pore sizes of 0.1 μm to 0.6 μm. R3 and a peak R3 having a maximum value V R1 The maximum value V of the peak R3 R3 The ratio (V R3 / V R1 (5) The secondary battery negative electrode according to any one of (1) to (4) above, wherein the Si-based material contains composite particles having an ion-conducting phase and a silicon phase dispersed in the ion-conducting phase. (6) The carbon material has a specific surface area of ​​3 m 2 / g or less. (7) The negative electrode for a secondary battery according to any one of (1) to (5) above, comprising a graphite material having an average particle size of 5 μm or more and 30 μm or less. (8) The negative electrode for a secondary battery according to any one of (1) to (7) above, wherein the average particle size of the Si-based material is 3 μm or more and 15 μm or less. (9) The negative electrode for a secondary battery according to any one of (1) to (8) above, wherein, when the negative electrode mixture layer is equally divided in half in the thickness direction into a lower half region on the negative electrode current collector side and an upper half region on the surface side, the abundance ratio of pores corresponding to peak R2 in the upper half region is greater than the abundance ratio of pores corresponding to peak R2 in the lower half region. (10) A secondary battery comprising the negative electrode for a secondary battery according to any one of (1) to (9) above. (11) A secondary battery comprising a negative electrode for a secondary battery according to any one of (1) to (9) above. 2 (12) A method for manufacturing a negative electrode for a secondary battery, comprising: a first step of applying a negative electrode slurry, the negative electrode slurry including a graphite material having a viscosity of 100 to 200°C / g or less, a Si-based material, and vaporized particles that vaporize at a temperature of 100 to 200°C, to a negative electrode current collector to form a coating film, and then rolling the coating film; and a second step of, after the first step, heat-treating the coating film at a temperature of 100 to 200°C to form a negative electrode composite layer. (13) The method for manufacturing a negative electrode for a secondary battery according to (12) above, wherein the vaporized particles include at least one of a material that sublimes, a material that decomposes, and a material that dissolves and then vaporizes at a temperature of 100 to 200°C.

[0069] REFERENCE SIGNS LIST 10 secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 battery case, 16 case body, 17 sealing body, 18 insulating plate, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 protruding portion, 23 filter, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 40 negative electrode current collector, 42 negative electrode composite layer, 42a lower half region, 42b upper half region.

Claims

1. A negative electrode current collector and a negative electrode mixture layer provided on the negative electrode current collector, the negative electrode mixture layer containing a carbon material and a Si-based material, the pore size distribution of the negative electrode mixture layer measured by mercury intrusion porosimetry has a maximum value V in the range of pore size 1 μm or more and 3 μm or less. R1 A peak R1 having a maximum value V R2 and a maximum value V R1 The maximum value V of the peak R2 R2 The ratio (V R2 / V R1 ) is 0.5 or more and 100 or less.

2. The maximum value V of the peak R1 R1 The maximum value V of the peak R2 R2 The ratio (V R2 / V R1 2. The negative electrode for a secondary battery according to claim 1, wherein the ratio of the saturation potential to the surface potential is 0.5 or more and 2.0 or less.

3. The maximum value V of the peak R1 R1 The maximum value V of the peak R2 R2 The ratio (V R2 / V R1 3. The negative electrode for a secondary battery according to claim 2, wherein the ratio of the saturation potential to the surface potential is 0.5 or more and 1.0 or less.

4. The pore size distribution of the negative electrode mixture layer has a maximum value V R3 and a maximum value V R1 The maximum value V of the peak R3 R3 The ratio (V R3 / V R1 4. The negative electrode for secondary batteries according to claim 1, wherein the ratio of the saturation potential to the surface potential of the secondary battery is 0.9 or more and 1.5 or less.

5. The negative electrode for a secondary battery according to any one of claims 1 to 3, wherein the Si-based material includes composite particles having an ion-conducting phase and a silicon phase dispersed within the ion-conducting phase.

6. The carbon material has a specific surface area of ​​3 m 2 The negative electrode for secondary batteries according to any one of claims 1 to 3, comprising a graphite material having a surface roughness of 0.1 to 0.5 μm / g or less.

7. The negative electrode for a secondary battery according to claim 6, wherein the graphite material has an average particle size of 5 μm or more and 30 μm or less.

8. The negative electrode for a secondary battery according to any one of claims 1 to 3, wherein the average particle size of the Si-based material is 3 μm or more and 15 μm or less.

9. The negative electrode for a secondary battery according to any one of claims 1 to 3, wherein when the negative electrode mixture layer is divided in half in the thickness direction into a lower half region on the negative electrode current collector side and an upper half region on the surface side, the abundance ratio of pores corresponding to peak R2 in the upper half region is greater than the abundance ratio of pores corresponding to peak R2 in the lower half region.

10. A secondary battery comprising the negative electrode for secondary batteries according to any one of claims 1 to 3.

11. Specific surface area is 3 m 2 1. A method for producing a negative electrode for a secondary battery, comprising: a first step of applying a negative electrode slurry, the negative electrode slurry including a graphite material having a surface roughness of 100° C. or less and a Si-based material, and vaporized particles that vaporize at a temperature of 100° C. or more and 200° C. or less, to a negative electrode current collector to form a coating film, and then rolling the coating film; and a second step of, after the first step, heat-treating the coating film at a temperature of 100° C. or more and 200° C. or less to form a negative electrode composite layer.

12. The method for producing a negative electrode for a secondary battery described in claim 11, wherein the vaporized particles include at least one of a material that sublimes, a material that decomposes, and a material that dissolves and then evaporates at a temperature of 100°C or higher and 200°C or lower.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery

    JP2001210323A

  • Negative electrode active material for lithium ion secondary battery, negative electrode mixture for lithium ion secondary battery, negative electrode for lithium ion secondary battery, and lithium ion secondary battery

    JP2013219059A

  • Secondary battery negative electrode, secondary battery, and method for manufacturing secondary battery negative electrode

    WO2022230661A1

  • Negative electrode for secondary battery, and secondary battery

    WO2023032558A1