Optical pressure-sensitive adhesive sheet

The optical adhesive sheet with tailored properties addresses the issue of strain stress changes in foldable display panels, improving bendability and adhesion by maintaining a low stress change rate and ensuring strong adhesion during deformation.

WO2024242086A1PCT designated stage expired Publication Date: 2024-11-28NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018593
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-21
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional optical adhesive sheets for foldable display panels exhibit large changes in strain stress during bending, which affects the panel's foldability and bendability, leading to increased force requirements as the bending angle increases.

Method used

An optical adhesive sheet with specific properties, including an elongation of 1000% or more and strain stress ratios of (S1-S2)/(L1-L2) ≤ 0.028, S1 ≤ 40 N/cm², and S2 ≤ 20 N/cm², designed to minimize strain stress changes during bending, ensuring good bendability and cohesive force.

Benefits of technology

The adhesive sheet effectively suppresses strain stress changes, enhancing the foldability and bendability of foldable display panels by maintaining a low stress change rate and ensuring strong adhesion, even under deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018593_28112024_PF_FP_ABST
    Figure JP2024018593_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The pressure-sensitive adhesive sheet (10) is an optical pressure-sensitive adhesive sheet, and the elongation L1 (%) and the strain stress S1 (N / cm 2) at break point in a tensile test under conditions of 25°C and a tensile speed of 300 mm / min, and the strain stress S2 (N / cm 2) at an elongation L2 (%) of half of the elongation L1 satisfy (S1 - S2) / (L1 - L2) ≤ 0.028.
Need to check novelty before this filing date? Find Prior Art

Description

Optical adhesive sheet

[0001] The present invention relates to an optical pressure-sensitive adhesive sheet.

[0002] A display panel has a laminated structure including elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. In the manufacturing process of such a display panel, for example, an optically transparent adhesive sheet (optical adhesive sheet) is used to bond the elements included in the laminated structure.

[0003] Meanwhile, development of repeatedly foldable display panels for smartphones and tablet devices is progressing. Specifically, foldable display panels can be repeatedly deformed between a bent shape and a flat, non-bent shape. In such foldable display panels, each element in the laminated structure is made to be repeatedly foldable, and a thin optical adhesive sheet is used to bond such elements. Optical adhesive sheets for foldable display panels are described, for example, in Patent Document 1 below.

[0004] Japanese Patent Application Laid-Open No. 2018-111754

[0005] When a foldable display panel is bent, the bent portion of the optical adhesive sheet in the panel is substantially elongated, and strain stress is generated locally at the bent portion. During the bending process, as the bending amount (bending angle) increases, the strain stress also increases, and the force required to further bend increases. The magnitude of the change in strain stress at the bent portion of the optical adhesive sheet during this bending process affects the foldability of the panel. In conventional optical adhesive sheets, the change in strain stress during the bending process is relatively large.

[0006] The present invention provides an optical adhesive sheet suitable for achieving good foldability in a foldable display panel.

[0007] The present invention [1] is an optical pressure-sensitive adhesive sheet, and the elongation L1 (%) and strain stress S1 (N / cm) at the breaking point of the optical pressure-sensitive adhesive sheet in a tensile test under conditions of 25°C and a tensile speed of 300 mm / min are measured. 2 ) and the strain stress S2 (N / cm) at an elongation L2 (%) that is half the elongation L1. 2 ) and includes an optical adhesive sheet that satisfies (S1-S2) / (L1-L2)≦0.028.

[0008] The present invention [2] includes the optical pressure-sensitive adhesive sheet according to the above [1], which has an elongation of 1000% or more at the breaking point in the tensile test.

[0009] The present invention [3] is characterized in that the strain stress S1 is 40 N / cm 2 The optical pressure-sensitive adhesive sheet according to the above [1] or [2] is as follows:

[0010] The present invention [4] is a method for determining the strain stress S1 (N / cm) relative to the elongation L1 (%). 2 The optical pressure-sensitive adhesive sheet according to any one of [1] to [3] above, wherein the ratio of [amount of adhesion] to [best fit] is 0.020 or less.

[0011] As described above, the optical pressure-sensitive adhesive sheet of the present invention has an elongation L1 (%) and a strain stress S1 (N / cm) at the breaking point in a tensile test (25°C, tensile speed 300 mm / min). 2 ) and the strain stress S2 (N / cm 2 ) and satisfy (S1-S2) / (L1-L2)≦0.028. Such an optical adhesive sheet is suitable for suppressing changes in strain stress during the folding process, and is therefore suitable for achieving good folding properties in foldable display panels.

[0012] 2A is a cross-sectional schematic diagram of one embodiment of the optical pressure-sensitive adhesive sheet of the present invention. It also shows an example of a method for using the optical pressure-sensitive adhesive sheet of the present invention. 2A shows a step of bonding the optical pressure-sensitive adhesive sheet to a first adherend, 2B shows a step of joining the first adherend and the second adherend via the optical pressure-sensitive adhesive sheet, and 2C shows an aging step. It also shows stress-strain curves obtained in a tensile test of the pressure-sensitive adhesive sheets of Examples 1 to 7 and Comparative Examples 1 and 2. It also shows a stress-strain curve obtained in a tensile test of the pressure-sensitive adhesive sheet of Example 1.

[0013] As shown in Fig. 1 , a pressure-sensitive adhesive sheet 10 as one embodiment of the optical pressure-sensitive adhesive sheet of the present invention has a sheet shape of a predetermined thickness and extends in a direction (plane direction) perpendicular to the thickness direction H. The pressure-sensitive adhesive sheet 10 has an adhesive surface 11 on one side in the thickness direction H and an adhesive surface 12 on the other side in the thickness direction H. Fig. 1 exemplarily shows a state in which release liners L1, L2 are bonded to the adhesive surfaces 11, 12 of the pressure-sensitive adhesive sheet 10. The release liner L1 is disposed on the adhesive surface 11. The release liner L2 is disposed on the adhesive surface 12. The release liners L1, L2 are each peeled off at a predetermined timing when the pressure-sensitive adhesive sheet 10 is used.

[0014] The adhesive sheet 10 is an optically transparent adhesive sheet that is disposed at a light passage location in a flexible device. Examples of flexible devices include flexible display panels. Examples of flexible display panels include foldable display panels and rollable display panels. Flexible display panels have a laminated structure that includes elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. The adhesive sheet 10 is used, for example, to bond elements included in the laminated structure during the manufacturing process of the flexible display panel.

[0015] The adhesive sheet 10 was subjected to a tensile test at 25°C at a tensile speed of 300 mm / min, and the elongation L1 (%) and strain stress S1 (N / cm 2 ) and the strain stress S2 (N / cm) at elongation L2 (%), which is half (0.5 times) the elongation L1. 2 ) satisfies (S1-S2) / (L1-L2)≦0.028. Specific methods for conducting tensile tests are as described below in the examples. The value of (S1-S2) / (L1-L2) represents the rate of change in strain stress (stress change rate R) from elongation L2 to elongation L1 of the PSA sheet. A small stress change rate R means that the change in strain stress is small when the PSA sheet is deformed relatively greatly.

[0016] The stress change rate R [= (S1-S2) / (L1-L2)] of the pressure-sensitive adhesive sheet 10 being 0.028 or less is suitable for suppressing changes in strain stress at the folded portion of the pressure-sensitive adhesive sheet 10 during the bending process of an adherend to which the pressure-sensitive adhesive sheet 10 is attached. Therefore, the pressure-sensitive adhesive sheet 10 is suitable for achieving good foldability in a foldable display panel. From the viewpoint of suppressing changes in strain stress during the above-mentioned bending process, the stress change rate R is preferably 0.025 or less, more preferably 0.021 or less, and even more preferably 0.018 or less. The stress change rate R is, for example, 0.001 or more, 0.005 or more, or 0.010 or more.

[0017] The elongation L1 at the break point of the pressure-sensitive adhesive sheet 10 in the above-mentioned tensile test (25°C, tensile speed 300 mm / min) is preferably 1000% or more, more preferably 1300% or more, and even more preferably 1700% or more, from the viewpoint of ensuring the strength of the pressure-sensitive adhesive sheet 10. The elongation L1 is, for example, 5000% or less, 3000% or less, 2700% or less, or 2500% or less. Methods for adjusting the elongation L1 of the pressure-sensitive adhesive sheet 10 include, for example, selecting the type of base polymer in the pressure-sensitive adhesive sheet 10, adjusting the molecular weight and amount of the base polymer, and selecting the type of crosslinking agent and adjusting the amount of the crosslinking agent.

[0018] The strain stress S1 is preferably 40 N / cm from the viewpoint of suppressing the strain stress during the bending process. 2 Less than or equal to 35 N / cm, more preferably 2 Below 30 N / cm, more preferably 2 The strain stress S1 is preferably 5 N / cm from the viewpoint of ensuring the cohesive force of the adhesive sheet 10. 2 More preferably, 10 N / cm 2 More preferably, 12 N / cm 2 The distortion stress S1 of the pressure-sensitive adhesive sheet 10 can be adjusted, for example, by selecting the type of base polymer in the pressure-sensitive adhesive sheet 10, adjusting the molecular weight and the amount of base polymer blended, and by selecting the type of crosslinking agent and adjusting the amount of crosslinking agent blended (the same applies to the method for adjusting the distortion stress S2).

[0019] Strain stress S1 (N / cm) relative to elongation L1 (%) 2 From the viewpoint of suppressing the change in strain stress during the bending process, the ratio (S1 / L1) of the strain stress (S1 / L1) is preferably 0.020 or less, more preferably 0.018 or less, and even more preferably 0.016 or less. The ratio (S1 / L1) is, for example, 0.001 or more, 0.002 or more, or 0.005 or more.

[0020] The strain stress S2 is preferably 20 N / cm from the viewpoint of suppressing the strain stress during the bending process. 2 Less than or equal to 15 N / cm, more preferably 2 or less, more preferably 12 N / cm 2 The strain stress S2 is preferably 3 N / cm from the viewpoint of ensuring the cohesive force of the pressure-sensitive adhesive sheet 10. 2 More preferably, 5N / cm 2 More preferably, 7N / cm 2 More preferably, 8N / cm 2 That's all.

[0021] The shear storage modulus G1 of the PSA sheet 10 at -30°C is preferably 120 kPa or less, more preferably 100 kPa or less, even more preferably 80 kPa or less, and even more preferably 70 kPa or less, from the viewpoint of stress relaxation at the deformed portion when the PSA sheet 10 is deformed (such as bent or curved). The shear storage modulus G1 is preferably 45 kPa or more, more preferably 50 kPa or more, and even more preferably 55 kPa or more, from the viewpoint of ensuring good adhesiveness and handleability of the PSA sheet 10. The shear storage modulus G1 of the PSA sheet 10 is determined by dynamic viscoelasticity measurement, which will be described later in the examples (the same applies to the shear storage moduli G2 to G4 described later). Methods for adjusting the shear storage modulus G1 of the PSA sheet 10 include, for example, selecting the type of base polymer in the PSA sheet 10, adjusting the molecular weight and amount of base polymer, and selecting the type of crosslinking agent and adjusting the amount of crosslinking agent (the same applies to the shear storage moduli G2 to G4 described later).

[0022] The shear storage modulus G2 of the PSA sheet 10 at −20° C. is preferably 60 kPa or less, more preferably 50 kPa or less, and even more preferably 45 kPa or less, from the viewpoint of the above-mentioned stress relaxation in the PSA sheet 10. From the viewpoint of ensuring good adhesiveness and handleability in the PSA sheet 10, the shear storage modulus G2 is preferably more than 40 kPa, and more preferably 45 kPa or more.

[0023] The ratio (G1 / G2) of the shear storage modulus G1 (-30°C) to the shear storage modulus G2 (-20°C) is preferably 1.8 or less, more preferably 1.7 or less, and even more preferably 1.6 or less, from the viewpoint of ensuring a stable stress relaxation function of the PSA sheet 10 in the low temperature range. The ratio (G1 / G2) is, for example, 0.9 or more, 1.0 or more, or 1.1 or more.

[0024] The shear storage modulus G3 of the PSA sheet 10 at 25°C is preferably 50 kPa or less, more preferably 40 kPa or less, even more preferably 30 kPa or less, and even more preferably 23 kPa or less, from the viewpoint of the above-mentioned stress relaxation in the PSA sheet 10. From the viewpoint of ensuring good adhesiveness and handleability in the PSA sheet 10, the shear storage modulus G3 is preferably more than 18 kPa, more preferably 19 kPa or more, and even more preferably 20 kPa or more.

[0025] The shear storage modulus G4 of the pressure-sensitive adhesive sheet 10 at 60°C is preferably 50 kPa or less, more preferably 40 kPa or less, even more preferably 30 kPa or less, and even more preferably 23 kPa or less, from the viewpoint of the above-mentioned stress relaxation in the pressure-sensitive adhesive sheet 10. From the viewpoint of ensuring good adhesiveness, cohesive strength, and handleability in the pressure-sensitive adhesive sheet 10, the shear storage modulus G4 is preferably 13 kPa or more, more preferably 15 kPa or more, and even more preferably 17 kPa or more.

[0026] The thickness of the pressure-sensitive adhesive sheet 10 is preferably 45 μm or more, more preferably 48 μm or more, and even more preferably 50 μm or more, from the viewpoint of ensuring a good stress relaxation function in the pressure-sensitive adhesive sheet 10. The thickness of the pressure-sensitive adhesive sheet 10 is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 70 μm or less, from the viewpoint of thinning the flexible device.

[0027] The moisture permeability of the pressure-sensitive adhesive sheet 10 measured under conditions of 40°C and a relative humidity of 92% is preferably 400 g / m from the viewpoint of suppressing swelling of the pressure-sensitive adhesive sheet 10 in a humid environment. 2 24h or less, preferably 395g / m 2 24 hours or less, more preferably 390 g / m 2 24 hours or less, more preferably 380 g / m 2 - 24 hours or less. The moisture permeability of the PSA sheet 10 refers to the moisture permeability when the PSA sheet 10 has a thickness of 50 μm. A PSA sheet 10 with low moisture permeability is suitable for suppressing partial swelling at the edges of the PSA sheet 10 when the PSA sheet 10 is used to bond adherends (swelling occurs due to moisture penetration into the edges). Suppressing partial swelling at the edges of the PSA sheet 10 is suitable for suppressing peeling of the edges from the adherend. Methods for adjusting the moisture permeability of the PSA sheet 10 include, for example, selecting the type of base polymer in the PSA sheet 10, adjusting the molecular weight, and adjusting the amount of the base polymer. Selecting the type of base polymer includes selecting the type and amount of the side chain of the base polymer. Selecting the type of side chain of the base polymer includes adjusting the length of the alkyl moiety in the side chain and selecting the type and amount of functional group contained in the side chain. Methods for adjusting the moisture permeability of the PSA sheet 10 also include selecting the type and amount of additives other than the base polymer. The method for measuring the moisture permeability of the pressure-sensitive adhesive sheet 10 is as described below in the examples.

[0028] The dielectric constant D1 of the PSA sheet 10 at 100 kHz (the dielectric constant before humidification, described below) is preferably 4.0 or less, more preferably 3.8 or less, and even more preferably 3.6 or less, from the viewpoint of achieving good sensing sensitivity in the touch sensor provided in the display panel. The dielectric constant D1 is, for example, 3.0 or more, 3.3 or more, or 3.5 or more. Methods for adjusting the dielectric constant D1 include, for example, selecting the type of base polymer in the PSA sheet 10, adjusting the molecular weight, and adjusting the amount of the base polymer. Selecting the type of base polymer includes selecting the type and adjusting the amount of the side chain of the base polymer. Selecting the type of side chain of the base polymer includes adjusting the length of the alkyl moiety in the side chain and selecting the type and adjusting the amount of the functional group contained in the side chain. Methods for adjusting the dielectric constant D1 also include selecting the type and adjusting the amount of additives other than the base polymer (the same applies to the dielectric constant D2, described below). Specific methods for measuring the dielectric constant are as described below in the examples.

[0029] The dielectric constant D2 of the PSA sheet 10 after 24 hours in an environment of 40°C and 92% relative humidity (after humidification) is preferably 4.0 or less, preferably 3.8 or less, and more preferably 3.6 or less, from the viewpoint of realizing good sensing sensitivity in a humidified environment in a touch sensor provided in a display panel. The dielectric constant D2 is, for example, 2.8 or more, 3.0 or more, or 3.2 or more.

[0030] From the viewpoint of obtaining stable dielectric properties in the adhesive sheet 10, the ratio of the relative dielectric constant D2 to the relative dielectric constant D1 (D2 / D1) is preferably 0.80 or more, more preferably 0.85 or more, and is preferably 1.1 or less, more preferably 1.05 or less.

[0031] The adhesive strength F1 of the PSA sheet 10 in a peel test (first peel test) under conditions of 25°C, a peel angle of 180°, and a tensile speed of 60 mm / min is preferably 2.0 N / 10 mm or more, more preferably 2.2 N / 10 mm or more, from the viewpoint of suppressing peeling of the PSA sheet 10 from the adherend in the room temperature range. The adhesive strength F1 refers to the adhesive strength to a polyimide (PI) film at 25°C. The specific method for measuring the adhesive strength F1 is as described below in the Examples. Methods for adjusting the adhesive strength F1 include, for example, selecting the type of base polymer in the PSA sheet 10, adjusting the molecular weight, and adjusting the blending amount. Selecting the type of base polymer includes adjusting the composition of the monomers forming the base polymer. Methods for adjusting the adhesive strength F1 also include selecting the type of components other than the base polymer in the PSA sheet 10 and adjusting the blending amount of these components. Examples of such components include crosslinkers, silane coupling agents, and oligomers. The above-described adhesive strength adjustment method also applies to the adhesive strength F2 described below.

[0032] The adhesive strength F2 of the PSA sheet 10 in a peel test (second peel test) under conditions of 65°C, a peel angle of 180°, and a tensile speed of 60 mm / min is preferably 1.3 N / 10 mm or more, preferably 1.5 N / 10 mm or more, and more preferably 1.7 N / 10 mm or more, from the viewpoint of suppressing peeling of the PSA sheet 10 from the adherend in the high temperature range. The adhesive strength F2 means the adhesive strength to a PI film at 65°C. The specific method for measuring the adhesive strength F2 is as described below in the examples.

[0033] The pressure-sensitive adhesive sheet 10 is a sheet-shaped pressure-sensitive adhesive formed from a pressure-sensitive adhesive composition. The pressure-sensitive adhesive sheet 10 (pressure-sensitive adhesive composition) contains at least a base polymer.

[0034] The base polymer is an adhesive component that imparts adhesiveness to the pressure-sensitive adhesive sheet 10. Examples of base polymers include acrylic polymers, silicone polymers, polyester polymers, polyurethane polymers, polyamide polymers, polyvinyl ether polymers, vinyl acetate / vinyl chloride copolymers, modified polyolefin polymers, epoxy polymers, fluoropolymers, and rubber polymers. The base polymers may be used alone or in combination of two or more. From the viewpoint of ensuring good transparency and adhesiveness in the pressure-sensitive adhesive sheet 10, acrylic polymers are preferred as the base polymer.

[0035] An acrylic polymer is a copolymer of monomer components containing 50% by mass or more of (meth)acrylic acid ester. "(Meth)acrylic" means acrylic and / or methacrylic.

[0036] As the (meth)acrylic acid ester, preferably, a (meth)acrylic acid alkyl ester is used, and more preferably, a (meth)acrylic acid alkyl ester in which the number of carbon atoms in the alkyl group is 1 to 20. The (meth)acrylic acid alkyl ester may have a linear or branched alkyl group, or may have an alicyclic alkyl group.

[0037] Examples of (meth)acrylic acid alkyl esters having a linear or branched alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, n-hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, and isooctyl (meth)acrylate. , nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (i.e., lauryl (meth)acrylate), isotridecyl (meth)acrylate, tetradecyl (meth)acrylate, isotetradecyl (meth)acrylate, pentadecyl (meth)acrylate, cetyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, and nonadecyl (meth)acrylate.

[0038] Examples of (meth)acrylic acid alkyl esters having an alicyclic alkyl group include (meth)acrylic acid cycloalkyl esters, (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring, and (meth)acrylic acid esters having a tricyclic or higher aliphatic hydrocarbon ring. Examples of (meth)acrylic acid cycloalkyl esters include cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate. Examples of (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring include isobornyl (meth)acrylate. Examples of (meth)acrylic acid esters having three or more aliphatic hydrocarbon rings include dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate.

[0039] As the (meth)acrylic acid alkyl ester, from the viewpoint of achieving a balance between the flexibility and adhesive strength required of an adhesive sheet for flexible device applications and the low moisture permeability of the adhesive sheet in the adhesive sheet 10, preferably at least one selected from (meth)acrylic acid alkyl esters having an alkyl group containing 6 to 14 carbon atoms is used, more preferably at least one selected from (meth)acrylic acid alkyl esters having an alkyl group containing 8 to 12 carbon atoms is used, and even more preferably at least two selected from (meth)acrylic acid alkyl esters having an alkyl group containing 8 to 12 carbon atoms are used. Preferred (meth)acrylic acid alkyl esters having an alkyl group containing 6 to 14 carbon atoms are 2-ethylhexyl acrylate (2EHA), n-octyl acrylate (NOAA), isononyl acrylate (INAA), and lauryl acrylate (LA).

[0040] The proportion of the (meth)acrylic acid alkyl ester in the monomer components is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 97% by mass or more, from the viewpoint of appropriately exhibiting flexibility, adhesive strength, and low moisture permeability in the PSA sheet 10. This proportion is, for example, 99.9% by mass or less, 99.5% by mass or less, or 99% by mass or less. When a first (meth)acrylic acid alkyl ester selected from (meth)acrylic acid alkyl esters having an alkyl group of 8 to 12 carbon atoms is used in combination with a second (meth)acrylic acid alkyl ester selected from (meth)acrylic acid alkyl esters having an alkyl group of 8 to 12 carbon atoms, the proportion of the first (meth)acrylic acid alkyl ester in the monomer components is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, and preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% ​​by mass or less. The proportion of the second (meth)acrylic acid alkyl ester in the monomer components is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 65% ​​by mass or less.

[0041] The monomer component may include a copolymerizable monomer copolymerizable with the (meth)acrylic acid alkyl ester. Examples of the copolymerizable monomer include a monomer having a polar group. Examples of the polar group-containing monomer include a hydroxy group-containing monomer, a monomer having a nitrogen atom-containing ring, and a carboxy group-containing monomer. The polar group-containing monomer is useful for modifying the acrylic polymer, such as by introducing crosslinking points into the acrylic polymer and ensuring the cohesive strength of the acrylic polymer. The monomer component preferably includes a hydroxy group-containing monomer, but does not include a monomer having a nitrogen atom-containing ring or a carboxy group-containing monomer.

[0042] Examples of hydroxy group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. As the hydroxy group-containing monomer, at least one selected from the group consisting of 2-hydroxyethyl acrylate (2HEA) and 4-hydroxybutyl acrylate (4HBA) is preferably used.

[0043] The proportion of the hydroxy group-containing monomer in the monomer components is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, from the viewpoint of introducing a crosslinked structure into the acrylic polymer and ensuring cohesive strength in the pressure-sensitive adhesive sheet 10. From the viewpoint of adjusting the polarity of the acrylic polymer (which is related to the compatibility of the acrylic polymer with various additive components in the pressure-sensitive adhesive sheet 10), this proportion is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.

[0044] Examples of monomers having a nitrogen atom-containing ring include N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, and N-vinylisothiazole.

[0045] When a monomer having a nitrogen atom-containing ring is used, the proportion of the monomer having a nitrogen atom-containing ring in the monomer components is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and even more preferably 0.5% by mass or more, from the viewpoints of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10 and ensuring the adhesive strength to the adherend of the pressure-sensitive adhesive sheet 10. This proportion is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, from the viewpoints of adjusting the glass transition temperature of the acrylic polymer and adjusting the polarity of the acrylic polymer (which is related to the compatibility of the acrylic polymer with various additive components in the pressure-sensitive adhesive sheet 10).

[0046] Examples of carboxy group-containing monomers include acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.

[0047] When a carboxy group-containing monomer is used, the proportion of the carboxy group-containing monomer in the monomer components is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 0.8% by mass or more, from the viewpoints of introducing a crosslinked structure into the acrylic polymer, ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10, and ensuring the adhesive strength to the adherend in the pressure-sensitive adhesive sheet 10. This proportion is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, from the viewpoints of adjusting the glass transition temperature of the acrylic polymer and avoiding the risk of corrosion of the adherend by acid.

[0048] The proportion of the polar group-containing monomer in the monomer component (when multiple polar group-containing monomers are included, the proportion of the total amount of the multiple polar group-containing monomers) is preferably 7% by mass or less, more preferably 5% by mass or less, even more preferably 3.5% by mass or less, and particularly preferably 3% by mass or less, from the viewpoint of lowering the glass transition temperature of the base polymer and ensuring the flexibility of the PSA sheet 10. This proportion is, for example, 0.1% by mass or more, 0.5% by mass or more, or 0.8% by mass or more.

[0049] The monomer component may contain other copolymerizable monomers. Examples of the other copolymerizable monomers include acid anhydride monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, alkoxy group-containing monomers, and aromatic vinyl compounds. These other copolymerizable monomers may be used alone or in combination of two or more.

[0050] The monomer components forming the base polymer preferably include a (meth)acrylic acid alkyl ester and a polar group-containing monomer, and more preferably include a (meth)acrylic acid alkyl ester having an alkyl group with 8 to 12 carbon atoms and a hydroxy group-containing monomer. In this case, the proportion of the hydroxy group-containing monomer in the total amount of the (meth)acrylic acid alkyl ester and the hydroxy group-containing monomer is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.8 mass% or more, from the viewpoints of introducing a crosslinked structure into the acrylic polymer and ensuring cohesive strength in the PSA sheet 10. From the viewpoints of lowering the glass transition temperature of the base polymer and ensuring the flexibility of the PSA sheet 10, this proportion is preferably 5 mass% or less, more preferably 3.5 mass% or less, even more preferably 3 mass% or less, even more preferably 2 mass% or less, and even more preferably 1.5 mass% or less. When the monomer components forming the base polymer include a (meth)acrylic acid alkyl ester having an alkyl group with 8 to 12 carbon atoms and a hydroxy group-containing monomer, it preferably does not include a monomer having a nitrogen atom-containing ring or a carboxy group-containing monomer.

[0051] The base polymer preferably has a crosslinked structure. Examples of methods for introducing a crosslinked structure into a base polymer include the following first and second methods. In the first method, a base polymer having a functional group reactive with the crosslinking agent and a crosslinking agent are blended into a pressure-sensitive adhesive composition, and the base polymer and the crosslinking agent are reacted in a pressure-sensitive adhesive sheet. In the second method, a polyfunctional compound is included as a crosslinking agent in the monomer components forming the base polymer, and a base polymer having a branched structure (crosslinked structure) introduced into the polymer chain is formed by polymerization of the monomer components. These methods may be used in combination.

[0052] Examples of the crosslinking agent used in the first method include compounds that react with functional groups (such as hydroxyl groups and carboxyl groups) contained in the base polymer. Examples of such crosslinking agents include isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, and carbodiimide crosslinking agents. The crosslinking agents used in the first method may be used alone or in combination of two or more. As the crosslinking agent in the first method, an isocyanate crosslinking agent is preferably used because it has high reactivity with the hydroxyl groups and carboxyl groups in the base polymer and facilitates the introduction of a crosslinked structure.

[0053] Examples of isocyanate crosslinking agents include tolylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, tetramethylxylylene diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, and polymethylene polyphenylisocyanate. Also included as isocyanate crosslinking agents are derivatives of these isocyanates. Examples of the isocyanate derivatives include isocyanurate-modified products and polyol-modified products. Commercially available isocyanate crosslinking agents include, for example, Coronate L (a trimethylolpropane adduct of tolylene diisocyanate, manufactured by Tosoh Corporation), Coronate HL (a trimethylolpropane adduct of hexamethylene diisocyanate, manufactured by Tosoh Corporation), Coronate HX (an isocyanurate of hexamethylene diisocyanate, manufactured by Tosoh Corporation), Takenate D110N (a trimethylolpropane adduct of xylylene diisocyanate, manufactured by Mitsui Chemicals), and Takenate 600 (1,3-bis(isocyanatomethyl)cyclohexane, manufactured by Mitsui Chemicals).

[0054] Peroxide crosslinking agents include dibenzoyl peroxide, di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, and t-butylperoxypivalate.

[0055] Epoxy crosslinkers include bisphenol A, epichlorohydrin-type epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol glycidyl ether, trimethylolpropane triglycidyl ether, diglycidylaniline, diamine glycidylamine, N,N,N',N'-tetraglycidyl-m-xylylenediamine, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.

[0056] The amount of crosslinking agent in the first method is, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, and more preferably 0.1 parts by mass or more, per 100 parts by mass of base polymer, from the viewpoint of ensuring the cohesive strength of the PSA sheet 10. From the viewpoint of ensuring good tackiness in the PSA sheet 10, the amount of crosslinking agent in ...

[0057] In the second method, the monomer components (including a polyfunctional compound and a monofunctional monomer for introducing a crosslinked structure) may be polymerized in one step or in multiple steps. In the multi-step polymerization method, first, a monofunctional monomer for forming a base polymer is polymerized (preliminary polymerization), thereby preparing a prepolymer composition containing a partial polymer (a mixture of a low-polymerization polymer and unreacted monofunctional monomer). Next, a polyfunctional compound as a crosslinking agent is added to the prepolymer composition, and then a polymerization reaction is allowed to proceed in a reaction system containing the partial polymer and the polyfunctional compound (main polymerization).

[0058] Examples of polyfunctional compounds include polyfunctional monomers and polyfunctional oligomers containing two or more ethylenically unsaturated double bonds in one molecule, and polyfunctional monomers include polyfunctional (meth)acrylates.

[0059] Examples of the polyfunctional (meth)acrylate include difunctional (meth)acrylate, trifunctional (meth)acrylate, and tetrafunctional or higher polyfunctional (meth)acrylate.

[0060] Examples of bifunctional (meth)acrylates include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, glycerin di(meth)acrylate, ethoxylated bisphenol A diacrylate (BPAEODE), and neopentyl glycol di(meth)acrylate.

[0061] Examples of trifunctional (meth)acrylates include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tris(acryloyloxyethyl)isocyanurate.

[0062] Examples of tetrafunctional or higher polyfunctional (meth)acrylates include ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, alkyl-modified dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0063] Examples of polyfunctional oligomers include urethane (meth)acrylate oligomers, polyester (meth)acrylate oligomers, polyether (meth)acrylate oligomers, polyol (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, polyethylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate.

[0064] The polyfunctional compound as the crosslinking agent in the second method may be used alone or in combination of two or more. As the polyfunctional compound, a polyfunctional monomer is preferably used, and more preferably at least one selected from the group consisting of dipentaerythritol hexaacrylate (DPHA), 1,6-hexanediol diacrylate (HDDA), and trimethylolpropane triacrylate (TMPTA) is used.

[0065] The amount of the polyfunctional compound as a crosslinking agent in the monomer components is preferably 0.02 parts by mass or more, more preferably 0.04 parts by mass or more, and even more preferably 0.06 parts by mass or more per 100 parts by mass of the monofunctional monomer, from the viewpoint of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10. The amount of the polyfunctional compound is preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less per 100 parts by mass of the monofunctional monomer, from the viewpoint of ensuring good tackiness in the pressure-sensitive adhesive sheet 10.

[0066] The acrylic polymer (base polymer) can be formed by polymerizing the above-mentioned monomer components. Examples of polymerization methods include solution polymerization, emulsion polymerization, and solvent-free photopolymerization (e.g., ultraviolet polymerization). Examples of solvents used in solution polymerization include ethyl acetate and toluene. A chain transfer agent may be used in the polymerization. Examples of polymerization initiators include thermal polymerization initiators and photopolymerization initiators. The polymerization initiators may be used alone or in combination. The amount of the polymerization initiator used is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.07 parts by mass or more, per 100 parts by mass of the monomer components. It is also preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less.

[0067] Examples of thermal polymerization initiators include azo polymerization initiators and peroxide polymerization initiators. Examples of azo polymerization initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionate)dimethyl, 4,4'-azobis-4-cyanovaleric acid, azobisisovaleronitrile, and 2,2'-azobis(2-amidinopropane)dihydrochloride. Examples of peroxide polymerization initiators include dibenzoyl peroxide, t-butyl permaleate, and lauroyl peroxide.

[0068] Examples of the photopolymerization initiator include a radical photopolymerization initiator, a cationic photopolymerization initiator, and an anionic photopolymerization initiator.

[0069] Examples of the radical photopolymerization initiator include an acylphosphine oxide photopolymerization initiator, a benzoin ether photopolymerization initiator, and an acetophenone photopolymerization initiator.

[0070] Examples of acylphosphine oxide photopolymerization initiators include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-di-n-butoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. Examples of benzoin ether photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one. Examples of acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone.

[0071] The weight average molecular weight of the base polymer is preferably 100,000 or more, more preferably 300,000 or more, and even more preferably 500,000 or more, from the viewpoint of ensuring cohesive strength in the pressure-sensitive adhesive sheet 10. The weight average molecular weight of the base polymer is measured by gel permeation chromatography (GPC) and calculated in polystyrene equivalent terms.

[0072] The glass transition temperature (Tg) of the base polymer is preferably 0° C. or lower, more preferably −10° C. or lower, and even more preferably −20° C. or lower. The glass transition temperature is, for example, −80° C. or higher.

[0073] The glass transition temperature (Tg) of the base polymer can be determined using the theoretical glass transition temperature calculated based on the Fox equation below. The Fox equation is a relationship between the glass transition temperature Tg of a polymer and the glass transition temperature Tgi of a homopolymer of the monomers constituting the polymer. In the Fox equation below, Tg represents the glass transition temperature (°C) of the polymer, Wi represents the weight fraction of monomer i constituting the polymer, and Tgi represents the glass transition temperature (°C) of the homopolymer formed from monomer i. Literature values ​​can be used for the glass transition temperature of the homopolymer. For example, the "Polymer Handbook" (4th edition, John Wiley & Sons, Inc., 1999) lists the glass transition temperatures of various homopolymers. Meanwhile, the glass transition temperature of a homopolymer of a monomer can also be determined using the method specifically described in JP 2007-51271 A.

[0074] Fox's formula: 1 / (273+Tg)=Σ[Wi / (273+Tgi)]

[0075] The PSA composition may contain a silane coupling agent. The content of the silane coupling agent in the PSA composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, relative to 100 parts by mass of the base polymer. The content is preferably 5 parts by mass or less, more preferably 3 parts by mass or less.

[0076] The PSA composition may contain other components as needed. Examples of the other components include solvents, tackifiers, plasticizers, softeners, antioxidants, fillers, colorants, UV absorbers, surfactants, and antistatic agents. Examples of the solvent include polymerization solvents used as needed during polymerization of the acrylic polymer, and solvents added to the polymerization reaction solution after polymerization. Examples of the solvent include ethyl acetate and toluene.

[0077] The PSA sheet 10 can be produced, for example, by applying the above-described PSA composition to a release liner L1 (first release liner) to form a coating film, and then drying the coating film. The PSA sheet 10 may also be produced by applying the above-described PSA composition to a release liner L1 (first release liner) to form a coating film, laminating a release liner L2 (second release liner) on top of the coating film, and then drying the coating film between the release liners.

[0078] The release liner L1 may be, for example, a flexible plastic film. Examples of such plastic films include polyester films such as polyethylene terephthalate films, polyethylene films, and polypropylene films. The thickness of the release liner L1 is, for example, 3 μm or more and, for example, 200 μm or less. The surface of the release liner L1 is preferably release-treated.

[0079] Examples of methods for applying the PSA composition include roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating. The drying temperature for the coating film is, for example, 50°C to 200°C. The drying time is, for example, 5 seconds to 20 minutes.

[0080] The release liner L2 is preferably a flexible plastic film whose surface has been treated for release properties. The plastic films described above for the release liner L1 can be used as the release liner L2.

[0081] In this manner, a pressure-sensitive adhesive sheet 10 can be manufactured in which the pressure-sensitive adhesive surfaces 11, 12 are covered and protected by the release liners L1, L2.

[0082] The haze of the pressure-sensitive adhesive sheet 10 is preferably 3% or less, more preferably 2% or less, and more preferably 1% or less. The haze of the pressure-sensitive adhesive sheet 10 can be measured using a haze meter in accordance with JIS K7136 (2000). Examples of haze meters include the "NDH2000" manufactured by Nippon Denshoku Industries Co., Ltd. and the "HM-150" manufactured by Murakami Color Research Laboratory Co., Ltd.

[0083] The total light transmittance of the pressure-sensitive adhesive sheet 10 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. The total light transmittance of the pressure-sensitive adhesive sheet 10 is, for example, 100% or less. The total light transmittance of the pressure-sensitive adhesive sheet 10 can be measured in accordance with JIS K 7375 (2008).

[0084] 2A to 2C show an example of how the adhesive sheet 10 is used.

[0085] In this method, first, as shown in Figure 2A, the adhesive sheet 10 is attached to one surface in the thickness direction H of a first member 21 (adherend). The first member 21 is, for example, one element in the laminated structure of a flexible display panel. Examples of such elements include a pixel panel, a polarizing film, a touch panel, and a cover film (the same applies to the second member 22 described below). This process provides the adhesive sheet 10, which will be used for bonding to other members, on the first member 21.

[0086] 2B , one surface of the first member 21 in the thickness direction H is bonded to the other surface of the second member 22 in the thickness direction H via the adhesive sheet 10 on the first member 21. The second member 22 is, for example, another element in the laminated structure of the flexible display panel.

[0087] Next, as shown in Figure 2C, the adhesive sheet 10 between the first member 21 and the second member 22 is aged. Aging increases the bonding strength between the adhesive sheet 10 and the members 21 and 22. The aging temperature is, for example, 20°C to 160°C. The aging time is, for example, 1 minute to 21 days. When aging is performed by autoclave treatment (heat and pressure treatment), the temperature is, for example, 30°C to 80°C, the pressure is, for example, 0.1 to 0.8 MPa, and the treatment time is, for example, 15 minutes or more.

[0088] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to these examples. The specific numerical values ​​of the blending amounts (contents), physical property values, parameters, etc. described below can be substituted with the upper limits (numerical values ​​defined as "equal to or less than") or lower limits (numerical values ​​defined as "equal to or more than") of the corresponding blending amounts (contents), physical property values, parameters, etc. described in the above-mentioned "Description of the Invention."

[0089] Example 1 Preparation of Prepolymer Composition In a flask, 0.05 parts by mass of 2,2-dimethoxy-1,2-diphenylethan-1-one (trade name "Omnirad 651", manufactured by IGM Resins) as a first photopolymerization initiator and 0.05 parts by mass of 1-hydroxycyclohexyl phenyl ketone (trade name "Omnirad 184", manufactured by IGM Resins) as a second photopolymerization initiator were added to a monomer mixture containing 60 parts by mass of 2-ethylhexyl acrylate (2EHA), 39 parts by mass of lauryl acrylate (LA), and 1 part by mass of 4-hydroxybutyl acrylate (4HBA). The mixture was then irradiated with ultraviolet light in a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a first prepolymer composition (containing monomer components that had not undergone a polymerization reaction) with a polymerization rate of approximately 10%.

[0090] <Preparation of Pressure-Sensitive Adhesive Composition> 100 parts by mass of the first prepolymer composition, 0.06 parts by mass of dipentaerythritol hexaacrylate (DPHA) as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed together to obtain a first pressure-sensitive adhesive composition.

[0091] <Formation of Pressure-Sensitive Adhesive Layer> A first pressure-sensitive adhesive composition was applied to the release-treated surface of a first release liner (trade name "Diafoil MRF#75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) having a release-treated surface on one side to form a coating film. Next, the release-treated surface of a second release liner (trade name "Diafoil MRE#75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) having a release-treated surface on one side was laminated onto the coating film on the first release liner. Next, the coating film between the release liners was irradiated with ultraviolet light to photocure the coating film and form a pressure-sensitive adhesive layer (thickness 50 μm). For ultraviolet irradiation, a black light was used as the irradiation light source, and the irradiation intensity was 5 mW / cm. 2 It was decided.

[0092] In this manner, a pressure-sensitive adhesive sheet (50 μm thick) with a double-sided release liner of Example 1 was prepared (the composition of the pressure-sensitive adhesive sheet is shown in Tables 1 and 2 in parts by mass).

[0093] [Example 2] A PSA sheet of Example 2 with a double-sided release liner was produced in the same manner as the PSA sheet of Example 1, except that in preparing the prepolymer composition, the blending amount of 2EHA was set to 51 parts by mass and the blending amount of LA was set to 48 parts by mass.

[0094] [Example 3] A PSA sheet of Example 3 with a double-sided release liner was produced in the same manner as the PSA sheet of Example 1, except that in preparing the prepolymer composition, the blending amount of 2EHA was set to 58 parts by mass and the blending amount of 4HBA was set to 3 parts by mass.

[0095] Example 4 First, 0.05 parts by mass of a first photopolymerization initiator (Omnirad 651) and 0.05 parts by mass of a second photopolymerization initiator (Omnirad 184) were added to a monomer mixture containing 29 parts by mass of n-octyl acrylate (NOAA), 70 parts by mass of 2EHA, and 1 part by mass of 4HBA in a flask. The mixture was then irradiated with ultraviolet light in a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a second prepolymer composition with a polymerization rate of approximately 10%.

[0096] Next, 100 parts by mass of the second prepolymer composition, 0.06 parts by mass of DPHA as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (KBM-403) were mixed together to obtain a second PSA composition.

[0097] Next, an adhesive layer (thickness 50 μm) was formed between the first and second release liners in the same manner as in Example 1, except that the second adhesive composition was used instead of the first adhesive composition.

[0098] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) of Example 4 with double-sided release liners was prepared.

[0099] Example 5 First, 0.05 parts by mass of a first photopolymerization initiator (Omnirad 651) and 0.05 parts by mass of a second photopolymerization initiator (Omnirad 184) were added to a monomer mixture containing 70 parts by mass of isononyl acrylate (INAA), 29 parts by mass of LA, and 1 part by mass of 4HBA in a flask. The mixture was then irradiated with ultraviolet light in a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a third prepolymer composition with a polymerization rate of approximately 10%.

[0100] Next, 100 parts by mass of the third prepolymer composition, 0.06 parts by mass of DPHA as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (KBM-403) were mixed together to obtain a third pressure-sensitive adhesive composition.

[0101] Next, an adhesive layer (thickness 50 μm) was formed between the first and second release liners in the same manner as in Example 1, except that the third adhesive composition was used instead of the first adhesive composition.

[0102] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) of Example 5 with double-sided release liners was prepared.

[0103] [Example 6] A PSA sheet of Example 6 with a double-sided release liner was produced in the same manner as the PSA sheet of Example 4, except that in preparing the prepolymer composition, the blending amount of 2EHA was set to 50 parts by mass and the blending amount of NOAA was set to 49 parts by mass.

[0104] [Example 7] A PSA sheet of Example 7 with a double-sided release liner was produced in the same manner as the PSA sheet of Example 5, except that in preparing the prepolymer composition, the amount of INAA blended was 50 parts by mass and the amount of LA blended was 49 parts by mass.

[0105] Comparative Example 1 A PSA sheet with a double-sided release liner of Comparative Example 1 was produced in the same manner as the PSA sheet of Example 1, except for the following: In preparing the prepolymer composition, the blended amounts of 2EHA were 56 parts by mass, LA were 34 parts by mass, 4HBA were 7 parts by mass, and 2 parts by mass of N-vinyl-2-pyrrolidone (NVP) were blended. In preparing the PSA composition, 1 part by mass of the following acrylic oligomer was further blended.

[0106] <Oligomer Preparation> First, in a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, a mixture containing 60 parts by weight of dicyclopentanyl methacrylate (DCPMA), 40 parts by weight of methyl methacrylate (MMA), 3.5 parts by weight of α-thioglycerol as a chain transfer agent, and 100 parts by weight of toluene as a solvent was stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator was added to the mixture to prepare a reaction solution. This was reacted under a nitrogen atmosphere at 70°C for 1 hour and then at 80°C for 2 hours (polymerization reaction). Next, the reaction solution was heated to 130°C to volatilize and remove the toluene, chain transfer agent, and unreacted monomer. This resulted in an acrylic oligomer (solid) as a hydrophobic oligomer without polar groups. The weight-average molecular weight of this acrylic oligomer was 5100.

[0107] [Comparative Example 2] A PSA sheet with a double-sided release liner of Comparative Example 2 was produced in the same manner as the PSA sheet of Example 1, except for the following: In preparing the prepolymer composition, the blended amounts of 2EHA were 44 parts by mass, LA was 34 parts by mass, 4HBA was 6 parts by mass, and NVP was 7 parts by mass. In preparing the PSA composition, 1 part by mass of the above-mentioned acrylic oligomer was further blended.

[0108] <Moisture Permeability> The moisture permeability was examined for each of the pressure-sensitive adhesive sheets of Examples 1 to 7 and Comparative Examples 1 and 2. Specifically, the results are as follows.

[0109] First, the PSA sheet with double-sided release liners was left to stand for 3 days in an atmosphere at a temperature of 23°C and a relative humidity of 55%. This adjusted the condition of the PSA sheet. Next, one of the release liners was peeled from the PSA sheet, and the exposed surface was then covered with a 25 μm-thick triacetyl cellulose (TAC) film (moisture permeability: 1070 g / m). 2 The other release liner was then peeled off from the pressure-sensitive adhesive sheet on the TCA film, yielding a sample film for measuring moisture permeability.

[0110] Next, the moisture permeability in the thickness direction of the PSA sheet was measured in accordance with the moisture permeability test (cup method) of JIS Z0208. Specifically, first, a predetermined amount of calcium chloride weighed in advance was placed in a test cup (an aluminum cup with a circular opening of 30 mm diameter, a cup used in the cup method of JIS Z0208), and the opening of the cup was blocked with a sample film. The area of ​​the sample film blocking the opening of the cup corresponds to the area of ​​a circle with a diameter of 30 mm. Next, the cup with the sample film was placed in a constant temperature and humidity chamber at a temperature of 40°C and a relative humidity of 90%, and left for 24 hours. Next, the calcium chloride removed from the cup was weighed. The increased mass (g) of calcium chloride was calculated by multiplying the area (m 2 The value was divided by the moisture permeability (g / m) of the PSA sheet. 2The moisture permeability (24h) is shown in Tables 1 and 2. The moisture permeability thus obtained is that of the pressure-sensitive adhesive sheet with TAC film, but since the moisture permeability of the TAC film is much greater than that of the pressure-sensitive adhesive sheet, the moisture permeability of the sample film was considered to be that of the pressure-sensitive adhesive sheet.

[0111] <Relative Dielectric Constant> The relative dielectric constant was examined for each of the pressure-sensitive adhesive sheets of Examples 1 to 7 and Comparative Examples 1 and 2. Specifically, it is as follows.

[0112] First, a measurement sample was prepared by sandwiching the adhesive sheet between copper foil and an electrode. Next, the dielectric constant of the measurement sample was measured at a frequency of 100 kHz under the following conditions in accordance with JIS K6911 using an Agilent Technologies Precision Impedance Analyzer 4294A (first dielectric constant measurement). The measurement results are shown in Tables 1 and 2 as the dielectric constant D1 of the adhesive sheet at 100 kHz.

[0113] [Conditions for measuring relative permittivity] Electrode configuration: aluminum plate with a diameter of 12.1 mm and a thickness of 0.5 mm Counter electrode: 3 oz copper plate Measurement environment: temperature 25°C, relative humidity 50%

[0114] Furthermore, the PSA sheet was subjected to a humidification treatment, and then the dielectric constant of the PSA sheet was measured (second dielectric constant measurement). In the humidification treatment, the PSA sheet was stored for 24 hours in an environment of 40°C and a relative humidity of 92%. The method for measuring the second dielectric constant was the same as the first dielectric constant measurement method described above. The measurement results are shown in Tables 1 and 2 as the dielectric constant D2 at 100 kHz after humidification of the PSA sheet. The ratio of the dielectric constant D2 to the above-mentioned dielectric constant D1 (D2 / D1) is also shown in Tables 1 and 2.

[0115] <Shear Storage Elastic Modulus> The dynamic viscoelasticity of each of the pressure-sensitive adhesive sheets of Examples 1 to 7 and Comparative Examples 1 and 2 was measured.

[0116] For each PSA sheet, the required number of measurement samples were prepared. Specifically, first, multiple PSA sheet pieces cut from the PSA sheet were laminated together to prepare a sample sheet approximately 1.5 mm thick. Next, this sheet was punched out to obtain cylindrical pellets (7.9 mm in diameter) as measurement samples.

[0117] The measurement sample was then fixed to a 7.9 mm diameter parallel plate jig using a dynamic viscoelasticity measuring device (product name "Discovery Hybrid Reometer-2 (DHR-2)", manufactured by TA Instruments), and dynamic viscoelasticity measurements were performed. In this measurement, the measurement mode was shear mode, the measurement temperature range was -50°C to 150°C, the heating rate was 5°C / min, and the frequency was 1 Hz. From the measurement results, the shear storage modulus at predetermined temperatures (-30°C, -20°C, 25°C, and 60°C) was read. The shear storage modulus G1 (kPa) at -30°C, the shear storage modulus G2 (kPa) at -20°C, the shear storage modulus G3 (kPa) at 25°C, and the shear storage modulus G4 (kPa) at 60°C are shown in Tables 1 and 2. The ratio of shear storage modulus G1 to shear storage modulus G2 (G1 / G2) is also shown in Tables 1 and 2.

[0118] <180° Peel Test> The adhesive strength of each of the pressure-sensitive adhesive sheets of Examples 1 to 7 and Comparative Examples 1 and 2 to an adherend was examined by a 180° peel test.

[0119] Specifically, the required number of measurement samples were first prepared for each PSA sheet. To prepare the measurement samples, the first release liner was first peeled from the PSA sheet, and the resulting exposed surface was bonded to a plasma-treated polyethylene terephthalate (PET) film (product name "Lumirror S10", 50 μm thick, manufactured by Toray Industries, Inc.) to obtain a laminate. The plasma treatment was performed using a plasma irradiation device (product name "AP-TO5", manufactured by Sekisui Kogyo Co., Ltd.) at a voltage of 160 V, a frequency of 10 kHz, and a treatment speed of 5000 mm / min. Next, test pieces (10 mm wide x 100 mm long) were cut out from the laminate (PET film / PSA sheet / second release liner). Next, the second release liner was peeled off from the adhesive sheet of this test piece, and the exposed surface was bonded to a polyimide (PI) film (product name "GV200", thickness 80 μm, manufactured by Kolon Co., Ltd.) whose surface had been plasma-treated. Next, the PI film with the adhesive sheet (test piece) was subjected to a heating and pressure treatment at a temperature of 50°C and a pressure of 0.5 MPa for 15 minutes. This caused the test piece to be pressure-bonded to the PI film. In this way, a measurement sample was prepared.

[0120] Next, the test sample was left to stand at room temperature for 30 minutes, and then a 180° peel test was performed to peel the test piece from the PI film on the test sample, and the force required for peeling (peel strength) was measured (first peel test). A tensile tester (product name "Autograph AG-50NX plus" manufactured by Shimadzu Corporation) was used for this measurement. The measurement temperature was 25°C, the relative humidity was 55%, the test piece was peeled from the PI film at a 180° angle, the test piece was pulled at a speed of 60 mm / min, and the peel length was 50 mm. The average measured peel strength is shown in Tables 1 and 2 as adhesive strength F1 (N / 10 mm).

[0121] On the other hand, a peel test (second peel test) was carried out under the same conditions as the first peel test, except that the measurement temperature was changed to 65° C. The measurement results are shown in Tables 1 and 2 as adhesive strength F2 (N / 10 mm).

[0122] <Tensile Test> The pressure-sensitive adhesive sheets of Examples 1 to 7 and Comparative Examples 1 and 2 were subjected to the following tensile test.

[0123] Specifically, a measurement sample was first prepared for each PSA sheet. In preparing the measurement samples, a double-sided release liner PSA sheet piece (30 mm wide x 100 mm long) was first cut out from the double-sided release liner PSA sheet. Next, one release liner was peeled off from the sheet piece, and the PSA sheet piece was then rolled lengthwise onto the other release liner, taking care to avoid trapping air bubbles, to form a cylindrical shape (cylinder height 30 mm). In this way, a cylindrical PSA sheet piece was obtained as a measurement sample.

[0124] Next, a tensile test was performed on the measurement sample using a Tensilon tensile tester (product name "Autograph AG-50NX plus" manufactured by Shimadzu Corporation) under an environment of 25°C and 50% relative humidity, and the tensile stress generated during the tensile process was measured. This resulted in a stress-strain curve (load-elongation curve). In this tensile test, the initial chuck distance was 10 mm, and the measurement sample (cylindrical adhesive sheet piece) was pulled in the height direction of the cylindrical shape at a pulling speed of 300 mm / min.

[0125] The measurement results for the pressure-sensitive adhesive sheets of Examples 1 to 7 and Comparative Examples 1 and 2 are shown in the graph of Figure 3. The measurement results for the pressure-sensitive adhesive sheet of Example 1 are shown in the graph of Figure 4. In each of the graphs of Figures 3 and 4, the horizontal axis represents the elongation (%) of the measurement sample, and the vertical axis represents the strain stress (N / cm) of the measurement sample. 2 3, curves E1 to E7 are the stress-strain curves of the pressure-sensitive adhesive sheets of Examples 1 to 7, and curves C1 and C2 are the stress-strain curves of the pressure-sensitive adhesive sheets of Comparative Examples 1 and 2. In FIG. 4, curve E1 is the stress-strain curve of the pressure-sensitive adhesive sheet of Example 1, and point P 1 and point P 2 is shown. Point P 1 is the elongation L1 (%) and strain stress S1 (N / cm) at the time when the measurement sample breaks (break point). 2 ) represents the point P 2 is the strain stress S2 (N / cm) at an elongation L2 (%) that is half (0.5 times) the elongation L1 2 ) and the measurement results of the tensile test for each PSA sheet are the elongation L1 (%) at the breaking point and the strain stress S1 (N / cm2 ), elongation L2 (%) at half the elongation L1, and strain stress S2 (N / cm 2 ) are shown in Tables 1 and 2. The values ​​of (S1-S2) / (L1-L2) and S1 / L1 are also shown in Tables 1 and 2. The value of (S1-S2) / (L1-L2) represents the rate of change in strain stress (stress change rate R) from elongation L2 to elongation L1. For example, in the stress-strain curve shown in Figure 4, point P 1 and point P 2 The slope of the line segment (shown by the dashed line) connecting these corresponds to the value of the stress change rate R [= (S1-S2) / (L1-L2)]. A small stress change rate R means that the change in strain stress when the PSA sheet is deformed relatively greatly is small.

[0126] The pressure-sensitive adhesive sheet of Comparative Example 1 had a relatively large stress change rate R of 0.050. The pressure-sensitive adhesive sheet of Comparative Example 2 had a relatively large stress change rate R of 0.037. In contrast, the pressure-sensitive adhesive sheets of Examples 1 to 7 had a small stress change rate R of 0.028 or less. That is, the pressure-sensitive adhesive sheets of Examples 1 to 7 experienced a small change in strain stress when the pressure-sensitive adhesive sheet was deformed relatively greatly.

[0127]

[0128]

[0129] The above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and should not be interpreted as limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.

[0130] The optical pressure-sensitive adhesive sheet of the present invention is suitably used, for example, in the production of display panels.

[0131] 10 Adhesive sheet (optical adhesive sheet) 11, 12 Adhesive surface H Thickness direction L1, L2 Release liner 21 First member 22 Second member

Claims

1. An optical adhesive sheet, comprising: an optical adhesive sheet having an elongation L1 (%) and a strain stress S1 (N / cm) at a breaking point in a tensile test at 25° C. and a tensile speed of 300 mm / min. 2 ) and the strain stress S2 (N / cm 2 ) and (S1-S2) / (L1-L2)≦0.

028.

2. The optical adhesive sheet according to claim 1, which has a breaking point at an elongation of 1000% or more in the tensile test.

3. The strain stress S1 is 40 N / cm 2 The optical adhesive sheet according to claim 1 , wherein:

4. The strain stress S1 (N / cm 2 4. The optical adhesive sheet according to claim 1, wherein the ratio of the above is 0.020 or less.

Citation Information

Patent Citations

  • Tacky adhesive and tacky adhesive sheet

    JP2012214544A

  • Adhesive composition, adhesive agent and adhesive sheet

    JP2015042746A

  • Adhesive for repeated flexing devices, adhesive sheet, repeated flexing laminated member, and repeated flexing device

    JP2022087156A

  • Foldable optical adhesive sheet

    JP2023055632A