Composite current collector and preparation method therefor, and electrode sheet, battery and electric device

By using the composite conductive layer of alternately stacked metal oxide layer and metal layer in the battery, the corrosion problem of fluoride ions on the conductive layer in the electrolyte is solved, the stability and performance of the battery are improved, and more efficient conductivity is achieved and corrosion resistance.

WO2024243867A1PCT designated stage expired Publication Date: 2024-12-05JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD

Patent Information

Application Number
PCT/CN2023/097489
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

During the battery charge and discharge cycle, the self-catalytic decomposition of LiPF6 in the electrolyte produces fluorine ions, which leads to corrosion of the conductive layer of the composite liquid collector, resulting in poor conductivity and attenuation of performance. Especially the thin conductive layer of the traditional composite liquid collector makes it possible to cause the conductive layer to cause the Fluorine ion corrosion is more obvious.

Method used

The composite conductive layer of a polymer film and a metal oxide layer arranged alternately stacked metal oxide layer and metal layer are prepared by physical vapor deposition. The metal oxide layer can effectively suppress fluoride ion corrosion, the metal layer provides conductivity, and improves the alternating structure. Conductive efficiency of electron flow.

Benefits of technology

It significantly improves the stability and performance of the composite fluid collection in the battery, extends the cycle life of the battery, and improves the corrosion resistance and preparation efficiency of the conductive layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023097489_05122024_PF_FP_ABST
    Figure CN2023097489_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a composite current collector and a preparation method therefor, and an electrode sheet, a battery and an electric device. The composite current collector in the present application comprises a polymer film and a composite conductive layer arranged on at least one side of the polymer film, wherein the composite conductive layer comprises a metal oxide layer and a metal layer which are alternately stacked.
Need to check novelty before this filing date? Find Prior Art

Description

Composite current collector, preparation method thereof, electrode sheet, battery and electrical device Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a composite current collector, a preparation method thereof, an electrode plate, a battery, and an electrical device. Background Art

[0002] During the battery's charge and discharge cycles, the LiPF6 in the electrolyte undergoes autocatalytic decomposition due to the humidity and elevated temperature, producing fluoride ions. These fluoride ions continuously penetrate the interior of the composite current collector, reacting with the conductive layer of the composite current collector and corroding it. This leads to defects in the conductive layer and poor conductivity, ultimately causing significant performance degradation during the battery's charge and discharge cycles. Furthermore, because the conductive layer of conventional composite current collectors is relatively thin (approximately 1 μm), the battery's performance degradation caused by fluoride ion corrosion is even more pronounced.

[0003] Summary of the Invention

[0004] According to various embodiments of the present application, a composite current collector, a preparation method thereof, an electrode plate, a battery, and an electrical device are provided. The composite current collector can effectively inhibit fluoride ions in the electrolyte from corroding the conductive layer, thereby improving its stability in the battery, thereby promoting the promotion and application of the composite current collector.

[0005] In a first aspect of the present application, a composite current collector is provided, comprising a polymer film and a composite conductive layer disposed on at least one side of the polymer film, wherein the composite conductive layer comprises metal oxide layers and metal layers alternately stacked.

[0006] In some embodiments, the outermost layer of the composite conductive layer is the metal oxide layer.

[0007] In some embodiments, the innermost layer of the composite conductive layer is the metal oxide layer.

[0008] In some embodiments, in the composite conductive layer located on one side of the polymer film, the number of metal layers is N, N≥1, and N is an integer, and the number of metal oxide layers is M, M=N or M=N+1.

[0009] In some embodiments, 2≤N≤50.

[0010] In some embodiments, the metal oxide in the metal oxide layer includes one or more of aluminum oxide, silicon oxide, titanium oxide, copper oxide, nickel oxide, chromium oxide, zinc oxide, magnesium oxide, cobalt oxide, zirconium oxide, tin oxide, and indium tin oxide.

[0011] In some embodiments, the metal layer includes one or more of aluminum, copper, gold, silver, nickel, and zinc.

[0012] In some embodiments, the thickness Hn of a single layer of the metal oxide layer and the thickness Hm of the metal layer adjacent thereto satisfy the following condition: 0<Hn≤10%Hm.

[0013] In some embodiments, the total thickness of the metal oxide layer accounts for ≤10% of the thickness of the composite conductive layer.

[0014] In some embodiments, the thickness of the composite conductive layer is 500 nm-2000 nm, and optionally 700 nm-1200 nm.

[0015] In some embodiments, the polymer in the polymer film includes one or more of polyethylene terephthalate (PET), polypropylene (PP), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polyethylene (PE), polypropylene, polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyphenylene sulfide (PPS), polyphenylene oxide (PPO), polystyrene (PS) and polyimide (PI).

[0016] In some embodiments, the polymer film has a thickness of 1 μm to 10 μm.

[0017] The second aspect of the present application provides a method for preparing the composite current collector described in the first aspect of the present application, comprising the following steps: alternately preparing the stacked metal oxide layer and the metal layer on at least one side of the polymer film.

[0018] In some embodiments, the metal oxide layer and the metal layer are each independently prepared by physical vapor deposition.

[0019] In some embodiments, the physical vapor deposition method includes one or more of an evaporation method and a magnetron sputtering method.

[0020] The third aspect of the present application provides an electrode plate, comprising the composite current collector described in the first aspect of the present application or the composite current collector prepared by the preparation method described in the second aspect of the present application.

[0021] The fourth aspect of the present application provides a battery comprising the electrode plate described in the third aspect of the present application.

[0022] In a fifth aspect of the present application, an electrical device is provided, comprising the battery described in the fourth aspect of the present application.

[0023] The details of one or more embodiments of the present application are set forth in the description below. Other features, objects, and advantages of the present application will become apparent from the description and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] FIG1 is an overall morphology diagram of the composite current collector prepared in Example 2 of the present application.

[0025] FIG2 is a local morphology diagram of the composite current collector prepared in Example 2 of the present application. DETAILED DESCRIPTION

[0026] The following will clearly and completely describe the technical solutions of this application in conjunction with specific embodiments. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art in the technical field of this application. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "one or more" as used herein includes any and all combinations of one or more related listed items. The meaning of the term "multiple" in this application is at least two, such as two, three, etc., unless otherwise clearly and specifically limited.

[0028] In this application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0029] In this application, when referring to numerical ranges, unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges subsumed therein.

[0030] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0031] One embodiment of the present application provides a composite current collector, comprising a polymer film and a composite conductive layer disposed on at least one side of the polymer film, wherein the composite conductive layer comprises metal oxide layers and metal layers alternately stacked.

[0032] The metal layer in the above-mentioned composite current collector can provide conductivity, and the metal oxide layer can effectively inhibit the corrosion of the metal layer by fluoride ions in the electrolyte, thereby improving the stability of the performance of the composite current collector during the charge and discharge cycle, and thus promoting the promotion and application of the composite current collector. In addition, the presence of the metal oxide layer can also improve the elongation at break of the composite current collector. This is because during the stretching process, the amorphous metal oxide can promote the slip between the metal layers, and the regular alternating structure of the metal oxide layer-metal layer can play a regular role in the transmission of the electron flow, promoting the rapid conduction of the electron flow along the direction parallel to the metal layer. It can be understood that the composite conductive layer can be located on one side of the polymer film in the thickness direction, or on both sides in the thickness direction. In the above-mentioned composite current collector, the innermost layer of the composite conductive layer can be a metal oxide layer or a metal layer; the outermost layer of the composite conductive layer can be a metal oxide layer or a metal layer.

[0033] In the present application, the outermost layer of the composite conductive layer refers to the surface layer of the composite conductive layer away from the polymer film, and the innermost layer of the composite conductive layer refers to the bottom layer of the composite conductive layer close to the polymer film.

[0034] In some embodiments, the outermost layer of the composite conductive layer is a metal oxide layer. In the composite current collector, the outermost metal oxide layer of the composite conductive layer (i.e., the metal oxide layer farthest from the polymer film) can further inhibit fluoride ion corrosion of the metal layer and prevent the metal layer from chemical corrosion or physical damage.

[0035] In some embodiments, the innermost layer of the composite conductive layer is a metal oxide layer. In the composite current collector, the innermost layer of the composite conductive layer is a metal oxide layer, which can improve the adhesion between the composite conductive layer and the polymer film.

[0036] In some embodiments, in the composite conductive layer on one side of the polymer film, the number of metal layers is N, N≥1, and N is an integer, and the number of metal oxide layers is M, M=N or M=N+1.

[0037] It should be noted that when the outermost layer of the composite conductive layer is a metal oxide layer, when M=N+1, the metal oxide layer is located on the surface of the polymer film. Since the metal oxide layer and the metal layer are alternately stacked, in this case, the outermost and innermost sides of the composite conductive layer in its thickness direction are both metal oxide layers. The innermost metal oxide layer of the composite conductive layer (i.e., the metal oxide layer closest to the polymer film) can enhance the adhesion between the composite conductive layer and the polymer film, and the outermost metal oxide layer of the composite conductive layer (i.e., the metal oxide layer farthest from the polymer film) can prevent the metal layer from being chemically corroded or physically damaged. For example, when the composite conductive layer is only provided on one side of the polymer film in the thickness direction, N is 2, M is 2, and the composite current collector includes a polymer film, a metal layer, a metal oxide layer, a metal layer, a metal oxide layer, or a composite current collector includes a polymer film, a metal oxide layer, a metal layer, a metal oxide layer, and a metal layer stacked in sequence; N is 2, M is 3, and the composite current collector includes a polymer film, a metal oxide layer, a metal layer, a metal oxide layer, a metal layer, and a metal oxide layer stacked in sequence.

[0038] In some embodiments, 2≤N≤50. Controlling N within the above range can further improve the corrosion resistance and preparation efficiency of the composite current collector. When N exceeds the above range, the preparation efficiency of the composite current collector is low. When N is less than the above range, the number of metal oxide layers is small, and the composite current collector is less effective in resisting fluoride ion corrosion.

[0039] In some embodiments, the metal oxide in the metal oxide layer includes one or more of aluminum oxide (Al2O3), silicon oxide (SiO2), titanium oxide (TiO2), copper oxide (CuO), nickel oxide (NiO), chromium oxide (Cr2O3), zinc oxide (ZnO), magnesium oxide (MgO), cobalt oxide (CoO), zirconium oxide (ZrO2), tin oxide (SnO2), and indium tin oxide (In2O3·SnO2). The above metal oxides have the advantages of easy availability of raw materials and good stability. In some optional embodiments, the metal oxide in the metal oxide layer includes one or more of aluminum oxide, silicon oxide, and titanium oxide.

[0040] In some embodiments, the single-layer thickness Hn of the metal oxide layer and the thickness Hm of the adjacent metal layer satisfy the following condition: 0 < Hn ≤ 10% Hm. Controlling Hn and Hm to meet these conditions can prevent the single-layer thickness Hn of the metal oxide layer from being too thick, which could affect the conductivity of the composite current collector, and can further effectively inhibit corrosion of the metal layer by fluoride ions in the electrolyte, thereby further improving the stability of the composite current collector during charge-discharge cycles and promoting the promotion and application of the composite current collector. It should be noted that the single-layer thickness Hn of each metal oxide layer can be the same or different, and the single-layer thickness Hm of each metal layer can also be the same or different.

[0041] In some embodiments, the total thickness of the metal oxide layers accounts for ≤10% of the thickness of the composite conductive layer. The total thickness of the metal oxide layers refers to the sum of the thicknesses of all metal oxide layers in the composite conductive layer. If the total thickness of the metal oxide layers accounts for a high percentage of the thickness of the composite conductive layer, the conductivity of the composite current collector may be poor.

[0042] In some embodiments, the thickness of the composite conductive layer is 500nm-2000nm. When the thickness of the composite conductive layer is too thin, the conductivity of the composite conductive layer is poor; when the thickness of the composite conductive layer is too thick, the weight of the composite conductive layer is heavy, which is not conducive to improving the energy density of the battery. When the thickness of the composite conductive layer is within the above range, the conductivity of the composite current collector and the energy density of the battery can be taken into account. Furthermore, the thickness of the composite conductive layer is 700nm-1200nm. Specifically, the thickness of the composite conductive layer includes but is not limited to: 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1400nm, 1600nm, 1800nm, 2000nm.

[0043] In some embodiments, the polymer in the polymer film includes one or more of polyethylene terephthalate (PET), polypropylene (PP), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polyethylene (PE), polypropylene, polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyphenylene sulfide (PPS), polyphenylene oxide (PPO), polystyrene (PS) and polyimide (PI).

[0044] In some embodiments, the thickness of the polymer film is 1 μm to 10 μm. Controlling the thickness of the polymer film within the above range helps reduce the difficulty and cost of preparing the polymer film and promotes the application of composite current collectors containing the polymer film in batteries. Alternatively, the polymer film can be prepared by a melt-extrusion-biaxial stretching method. It is understood that the thickness of the polymer film includes but is not limited to: 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, and 10 μm.

[0045] Another embodiment of the present application provides a method for preparing the composite current collector described above, comprising the steps of alternately forming a stack of metal oxide layers and metal layers on at least one side of a polymer film. The composite current collector prepared by the above method comprises stacked metal oxide layers and metal layers, and thus, this method has at least the same advantages as the above composite current collector.

[0046] In some embodiments, the metal oxide layer and the metal layer are independently prepared by physical vapor deposition. Physical vapor deposition can be used to simply prepare the metal oxide layer and the metal layer.

[0047] In some specific embodiments, the physical vapor deposition method includes one or more of an evaporation method and a magnetron sputtering method, thereby further simplifying the preparation of the metal oxide layer and the metal layer.

[0048] In some more specific embodiments, the metal layer is formed by evaporation. Specifically, the process conditions for preparing the aluminum metal layer include: the raw material is high-purity aluminum wire (purity ≥ 99.9%), the heating temperature is greater than the melting point of the aluminum wire, the vacuum degree of the vacuum chamber is ≤ 0.1 Pa, and the deposition time is 0.5s-40s each time. The process conditions for controlling the aluminum metal layer include the above-mentioned process parameters, which can improve the uniformity, density and integrity of the prepared aluminum metal layer, thereby improving the conductivity of the aluminum metal layer. It is understood that the vacuum degree of the vacuum chamber includes but is not limited to: 0.05Pa, 0.06Pa, 0.07Pa, 0.08Pa, 0.09Pa, 0.1Pa; the deposition time includes but is not limited to: 0.5s, 2s, 5s, 8s, 10s, 12s, 15s, 18s, 20s, 22s, 25s, 28s, 30s, 32s, 35s, 38s, 40s.

[0049] In some more specific embodiments, the metal layer is formed by magnetron sputtering. Specifically, the process conditions for preparing the aluminum metal layer include: the target material is a high-purity aluminum target material (purity ≥ 99.9%), the target power supply is a DC power supply, and the power density is 10W / cm 2 -150W / cm 2The vacuum degree of the vacuum chamber is ≤0.5Pa, the gas source is argon, the flow rate of argon is 10mL / min-500mL / min, and the deposition time each time is 1s-60s.

[0050] It should be noted that the process conditions for controlling the aluminum metal layer, including the above process parameters, can improve the uniformity, density and integrity of the prepared aluminum metal layer, thereby improving the conductivity of the aluminum metal layer. It is understood that the power density includes but is not limited to: 10W / cm 2 、30W / cm 2 , 50W / cm 2 , 70W / cm 2 , 90W / cm 2 、110W / cm 2 、130W / cm 2 、150W / cm 2 ; The vacuum degree of the vacuum chamber includes but is not limited to: 0.1Pa, 0.2Pa, 0.3Pa, 0.4Pa, 0.5Pa; the flow rate of argon gas includes but is not limited to: 10mL / min, 50mL / min, 100mL / min, 150mL / min, 200mL / min, 250mL / min, 300mL / min, 350mL / min, 400mL / min, 450mL / min, 500mL / min; the deposition time for each time includes but is not limited to: 1s, 5s, 10s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, 60s.

[0051] In some more specific embodiments, the metal oxide layer is formed by evaporation. Specifically, the process conditions for preparing the metal oxide layer include: the raw material is a high-purity metal wire (purity ≥99.9%), the heating temperature during the evaporation process is greater than the melting point of the metal wire, the gas source is oxygen, the oxygen flow rate is 10mL / min-500mL / min, the vacuum degree of the vacuum chamber is ≤0.5Pa, and the deposition time for each deposition is 0.1s-10s. The process conditions for controlling the metal oxide layer include the above-mentioned process parameters, which can improve the uniformity, density and integrity of the prepared metal oxide layer, thereby improving the corrosion resistance of the composite current collector (mainly resistance to fluoride ion corrosion). It is understood that the vacuum degree of the vacuum chamber includes but is not limited to: 0.1Pa, 0.2Pa, 0.3Pa, 0.4Pa, 0.5Pa; the deposition time for each deposition includes but is not limited to: 0.1s, 1s, 2s, 3s, 4s, 5s, 6s, 7s, 8s, 9s, 10s.

[0052] In some more specific embodiments, the metal oxide layer is formed by magnetron sputtering. Specifically, the process conditions for preparing the metal oxide layer include: the target material is a high-purity metal oxide target material (purity ≥ 99.9%), the target power supply is a DC power supply, and the power density is 10W / cm 2 -150W / cm 2 The vacuum degree of the vacuum chamber is ≤0.5Pa, the gas source is argon, the flow rate of argon is 10mL / min-500mL / min, and the deposition time each time is 0.5s-30s.

[0053] It should be noted that controlling the process conditions of the metal oxide layer including the above process parameters can improve the uniformity, density and integrity of the prepared metal oxide layer, thereby improving the corrosion resistance of the composite current collector (mainly resistance to fluoride ion corrosion). It is understood that the power density includes but is not limited to: 10W / cm 2 、30W / cm 2 , 50W / cm 2 , 70W / cm 2 , 90W / cm 2 、110W / cm 2 、130W / cm 2 、150W / cm 2 ; The vacuum degree of the vacuum chamber includes but is not limited to: 0.1Pa, 0.2Pa, 0.3Pa, 0.4Pa, 0.5Pa; the flow rate of argon gas includes but is not limited to: 10mL / min, 50mL / min, 100mL / min, 150mL / min, 200mL / min, 250mL / min, 300mL / min, 350mL / min, 400mL / min, 450mL / min, 500mL / min; the deposition time for each time includes but is not limited to: 0.5s, 5s, 10s, 15s, 20s, 25s, 30s.

[0054] Another embodiment of the present application further provides an electrode plate, comprising the above-mentioned composite current collector or the composite current collector prepared by the above-mentioned preparation method. It should be noted that the electrode plate of the present application can, for example, be formed by mixing positive electrode active material / negative electrode active material, conductive agent, binder and solvent to form a slurry, and the slurry is coated on the composite current collector of the present application using a method for preparing electrode plates well known to those skilled in the art. Depending on the active material, the electrode plate can be divided into a positive electrode plate and a negative electrode plate. The present application has no particular restrictions on the preparation method of the electrode plate, and the above-mentioned preparation method can be a preparation method well known to those skilled in the art.

[0055] Another embodiment of the present application also provides a battery, including the above-mentioned electrode plate. The above-mentioned electrode plate can be a positive electrode plate or a negative electrode plate. The above-mentioned battery may, for example, include a positive electrode plate, a negative electrode plate, an electrolyte and a diaphragm. The diaphragm is arranged between the positive electrode plate and the negative electrode plate, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through. The electrolyte plays the role of conducting ions between the positive electrode plate and the negative electrode plate. During the charge and discharge process of the battery, lithium ions are embedded and extracted back and forth between the positive electrode plate and the negative electrode plate. The above-mentioned positive electrode plate and / or negative electrode plate can adopt the electrode plate of the present application.

[0056] Another embodiment of the present application further provides an electrical device comprising the above-mentioned battery. The above-mentioned battery can be used as a power source or energy storage unit in the above-mentioned electrical device, including but not limited to electric vehicles, smart home appliances, computers, tablets, mobile phones, digital cameras, etc.

[0057] The present application is further described in detail below with reference to specific examples and comparative examples. For experimental parameters not specified in the following specific examples, reference should be made to the guidance provided in the present application documents. Reference may also be made to experimental manuals in the art or other experimental methods known in the art, or to the experimental conditions recommended by the manufacturer. It is understood that the instruments and raw materials used in the following examples are relatively specific and may not be limited thereto in other specific examples.

[0058] Example 1

[0059] Prepare the composite current collector as follows:

[0060] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:

[0061] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 20 s per deposition.

[0062] (b) Preparation of the metal oxide layer: The starting material was a high-purity metal wire (99.93%). During the evaporation process, the heating temperature was greater than the melting point of the metal wire. The gas source was oxygen at a flow rate of 100 mL / min. The vacuum level of the vacuum chamber was 0.3 Pa, and each deposition time was 0.3 s.

[0063] A multi-layer composite current collector was prepared according to the above-mentioned process conditions, wherein both sides of the PET film in the thickness direction had two aluminum metal layers and three aluminum oxide layers (metal oxide layers), and one side of the PET film in the thickness direction had a structure in which a metal oxide layer, an aluminum metal layer, a metal oxide layer, an aluminum metal layer, and a metal oxide layer were stacked in sequence, with each aluminum metal layer having a thickness of 500 nm and each metal oxide layer having a thickness of 5 nm.

[0064] Example 2

[0065] The preparation method of the composite current collector in this embodiment is the same as that in Example 1, except that: in the process condition (a) for preparing the aluminum metal layer, the deposition time is 2.1 s each time; in the prepared composite current collector, both sides of the PET film in the thickness direction have 19 aluminum metal layers and 20 aluminum oxide layers, and the thickness of each aluminum metal layer is 53 nm.

[0066] Example 3

[0067] The preparation method of the composite current collector in this embodiment is the same as that in Example 1, except that: in the process condition (a) for preparing the aluminum metal layer, the deposition time for each time is 0.8 s; in the process condition (b) for preparing the metal oxide layer, the deposition time for each time is 0.1 s; in the prepared composite current collector, both sides of the PET film in the thickness direction have 50 aluminum metal layers and 51 aluminum oxide layers, the thickness of each aluminum metal layer is 20 nm, and the thickness of each metal oxide layer is 1.9 nm.

[0068] Example 4

[0069] Prepare the composite current collector as follows:

[0070] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:

[0071] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 2.1 s per deposition.

[0072] (b) Preparation of metal oxide layer: The target material is silicon oxide target (purity is 99.95%), and the target power supply is a DC power supply with a power density of 50 W / cm 2 The vacuum degree of the vacuum chamber is 0.1 Pa, the gas source is argon, the argon flow rate is 60 mL / min, and the deposition time is 1.0 s each time;

[0073] A multi-layer composite current collector was prepared according to the above process conditions, in which both sides of the PET film in the thickness direction had 19 aluminum metal layers and 20 silicon oxide layers (metal oxide layers), the thickness of each aluminum metal layer was 53 nm, and the thickness of each metal oxide layer was 5 nm.

[0074] Example 5

[0075] Prepare the composite current collector as follows:

[0076] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:

[0077] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 2.1 s per deposition.

[0078] (b) Preparation of metal oxide layer: The target material is titanium oxide target (purity is 99.95%), and the target power supply is a DC power supply with a power density of 50 W / cm 2 The vacuum degree of the vacuum chamber is 0.1 Pa, the gas source is argon, the argon flow rate is 60 mL / min, and the deposition time is 1.2 s each time;

[0079] A multi-layer composite current collector was prepared according to the above process conditions, in which both sides of the PET film in the thickness direction had 19 aluminum metal layers and 20 titanium oxide layers (metal oxide layers), the thickness of each aluminum metal layer was 53 nm, and the thickness of each metal oxide layer was 5 nm.

[0080] Example 6

[0081] Prepare the composite current collector as follows:

[0082] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:

[0083] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 2.1 s per deposition.

[0084] (b) Preparation of metal oxide layer: The target material is copper oxide target (purity is 99.95%), and the target power supply is a DC power supply with a power density of 50 W / cm 2The vacuum degree of the vacuum chamber is 0.1 Pa, the gas source is argon, the argon flow rate is 60 mL / min, and the deposition time is 1.5 s each time;

[0085] A multi-layer composite current collector was prepared according to the above process conditions, in which both sides of the PET film in the thickness direction had 19 aluminum metal layers and 20 copper oxide layers (metal oxide layers), the thickness of each aluminum metal layer was 53 nm, and the thickness of each metal oxide layer was 5 nm.

[0086] Example 7

[0087] Prepare the composite current collector as follows:

[0088] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:

[0089] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 2.1 s per deposition.

[0090] (b) Preparation of metal oxide layer: nickel oxide target (purity 99.95%), target power supply is DC power supply, power density 50W / cm 2 The vacuum degree of the vacuum chamber is 0.1 Pa, the gas source is argon, the argon flow rate is 60 mL / min, and the deposition time is 1.3 s each time;

[0091] A multi-layer composite current collector was prepared according to the above process conditions, in which both sides of the PET film in the thickness direction had 19 aluminum metal layers and 20 copper oxide layers (metal oxide layers), the thickness of each aluminum metal layer was 53 nm, and the thickness of each metal oxide layer was 5 nm.

[0092] Example 8

[0093] The preparation method of the composite current collector in this embodiment is the same as that in Example 1, except that the PET film is replaced by a PEN film.

[0094] Example 9

[0095] The preparation method of the composite current collector in this embodiment is the same as that in Example 1, except that the PET film is replaced by a PP film.

[0096] Example 10

[0097] The preparation method of the composite current collector in this embodiment is the same as that in Example 1, except that the PET film is replaced by a PPS film.

[0098] Example 11

[0099] The preparation method of the composite current collector of this embodiment is the same as that of Example 1, except that: in the process condition (a) for preparing the aluminum metal layer, each deposition time is 10 s; and in the prepared composite current collector, the thickness of each aluminum metal layer is 250 nm.

[0100] Example 12

[0101] The preparation method of the composite current collector of this embodiment is the same as that of Example 1, except that: in the process condition (a) for preparing the aluminum metal layer, the deposition time is 40 s each time; and in the prepared composite current collector, the thickness of each aluminum metal layer is 1000 nm.

[0102] Example 13

[0103] The preparation method of the composite current collector of this embodiment is the same as that of Example 1, except that: in the process condition (a) for preparing the aluminum metal layer, the deposition time is 8 s each time; and in the prepared composite current collector, the thickness of each aluminum metal layer is 200 nm.

[0104] Example 14

[0105] The preparation method of the composite current collector of this embodiment is the same as that of Example 1, except that: in the process condition (b) for preparing the metal oxide layer, the deposition time is 1.2 s each time; and in the prepared composite current collector, the thickness of each metal oxide layer is 20 nm.

[0106] Example 15

[0107] The preparation method of the composite current collector of this embodiment is the same as that of Example 1, except that: in the process condition (b) for preparing the metal oxide layer, the deposition time is 2.0 s each time; and in the prepared composite current collector, the thickness of each metal oxide layer is 33 nm.

[0108] Example 16

[0109] The preparation method of the composite current collector of this embodiment is the same as that of Example 1, except that: in the process condition (b) for preparing the metal oxide layer, the deposition time is 2.4 s each time; and in the prepared composite current collector, the thickness of each metal oxide layer is 40 nm.

[0110] Example 17

[0111] The preparation method of the composite current collector of this embodiment is the same as that of Example 1, except that the composite current collector of this embodiment has one aluminum metal layer and two aluminum oxide layers.

[0112] Example 18

[0113] The preparation method of the composite current collector in this embodiment is the same as that in Example 1, except that: metal oxide layers and aluminum metal layers are alternately deposited on one side of the thickness direction of the biaxially oriented PET film. The composite current collector has two aluminum metal layers and three aluminum oxide layers. It is a structure in which PET film, metal oxide layer, aluminum metal layer, metal oxide layer, aluminum metal layer, and metal oxide layer are stacked in sequence. The thickness of each aluminum metal layer is 500 nm, and the thickness of each metal oxide layer is 5 nm.

[0114] Example 19

[0115] The preparation method of the composite current collector of this embodiment is the same as that of Example 1, except that:

[0116] In the prepared multilayer composite current collector, both sides of the PET film in the thickness direction have two aluminum metal layers and two aluminum oxide layers (metal oxide layers). One side of the PET film in the thickness direction is a structure in which aluminum metal layer, metal oxide layer, aluminum metal layer, and metal oxide layer are stacked in sequence. The thickness of each aluminum metal layer is 500 nm, and the thickness of each metal oxide layer is 5 nm.

[0117] Comparative Example 1

[0118] The preparation method of the composite current collector of Comparative Example 1 is the same as that of Example 1, except that: an aluminum metal layer is deposited on both sides of the thickness direction of the biaxially oriented PET film, the deposition time is 40s, and the thickness of the aluminum metal layer on one side of the PET film is 1000nm.

[0119] Performance Testing

[0120] The square resistance, tensile strength, elongation at break, thermal shrinkage and electrochemical performance of the composite current collectors prepared in each embodiment and comparative example were tested, and the test results are shown in Table 1. The specific test methods are as follows:

[0121] (1) Sheet resistance: The prepared flat composite current collector sample was placed on the sample stage and the sheet resistance of the sample was tested using a four-probe sheet resistance meter.

[0122] (2) Tensile strength and elongation at break: The tensile strength and elongation at break of the prepared composite current collector were tested with reference to GB / T 1040.3-2006.

[0123] (4) Thermal shrinkage: The thermal shrinkage of the prepared composite current collector was tested with reference to GB / T 10003-2008, and the heat treatment conditions were 150° C. for 30 min.

[0124] (5) The overall morphology and local morphology of the composite current collectors prepared in Example 2 and Comparative Example 1 were observed using a transmission electron microscope. The results are shown in Figures 1-2.

[0125] (6) Electrochemical performance test

[0126] (6.1) Assembly of lithium-ion batteries

[0127] Preparation of positive electrode sheet: The positive electrode current collector adopts the composite current collector prepared in each embodiment and comparative example, and the positive electrode active material is LiNi 0.6 Mn 0.2 Co 0.2 O2 (NCM622), the conductive agent is carbon nanotubes, the binder is polyvinylidene fluoride (PVDF), and the solvent is N-methylpyrrolidone (NMP). The above-mentioned positive electrode active material, conductive agent, binder and solvent are prepared into a positive electrode slurry with a certain fluidity according to the mass ratio of 67.2%:9.4%:1.1%:22.3% (the mass of the positive electrode slurry is 100%), coated on the positive electrode current collector, and dried to form a positive electrode sheet;

[0128] Preparation of negative electrode sheet: The negative electrode current collector uses traditional copper foil (thickness of 6 μm), the negative electrode active material uses artificial graphite, the conductive agent is carbon nanotubes, the binder is sodium carboxymethyl cellulose (CMC), and the solvent is pure water. The above negative electrode active material, conductive agent, binder and solvent are prepared in a mass ratio of 48.0%:5.0%:19.4%:27.6% to form a negative electrode slurry with a certain fluidity (the mass of the negative electrode slurry is 100%), which is coated on the negative electrode current collector and dried to form a negative electrode sheet;

[0129] The positive and negative electrode sheets were prepared into lithium-ion batteries through rolling, slicing, assembly, injection, and packaging. The separator used a polyethylene diaphragm coated with alumina ceramic (thickness 25 μm), and the electrolyte used was 1 mol·L -1 The carbonate solution of LiPF6, the carbonates are propylene carbonate, ethylene carbonate, and ethyl methyl carbonate, and the mass ratio of the three is 1:1:1.

[0130] (6.2) The assembled lithium-ion battery was cycled 600 times at a charge / discharge rate of 1 C. The battery capacity retention after the cycles was recorded. The voltage range for the cycles was 3.0 V to 4.2 V. Capacity retention after 600 cycles (%) = discharge capacity at the 600th cycle / charge capacity at the 600th cycle × 100%.

[0131] Table 1

[0132] Figure 1 shows the overall morphology of the composite current collector prepared in Example 2, and Figure 2 shows a localized morphology of the composite current collector prepared in Example 2. Furthermore, an elemental scan was performed on the composite current collector in Figure 2 , and the test results showed that aluminum oxide (metal oxide layer) and aluminum (metal layer) were alternately stacked in the composite current collector in Figure 2 .

[0133] As can be seen from Figures 1-2, the composite current collector prepared in Example 2 has a structure in which metal oxide layers and metal layers are alternately stacked, and both the metal layers and the metal oxide layers are dense structures. The metal oxide layers have a good insulating effect on the adjacent metal layers.

[0134] It can be seen from Table 1 that compared with Comparative Example 1, the tensile strength, elongation at break and cycle performance of the composite current collectors prepared in Examples 1-19 are significantly improved, indicating that the provided metal oxide layer improves the elongation at break and tensile strength of the composite current collector, while inhibiting the corrosion of the composite current collector by the electrolyte to a certain extent, thereby improving the stability of the composite current collector.

[0135] By comparing the square resistance data of Examples 1-10, Example 14, Example 15, and Comparative Example 1, it can be found that when the total thickness of the metal layer in the composite current collector is basically the same, the alternating stacking structure formed by the metal layer and the metal oxide layer in Examples 1-10, Example 14, and Example 15 will not significantly affect the conductivity of the composite current collector. Since the total thickness of the metal layer of the composite current collector of Examples 11-13 and Example 17 is quite different from the total thickness of the metal layer of Example 1, the square resistance of the composite current collector of Examples 11-13 changes greatly accordingly. Compared with Example 1, the square resistance of the composite current collector of Example 16 is higher, which is caused by the higher proportion of the thickness of the metal oxide layer therein. Compared with Example 1, the thermal shrinkage rate of the composite current collector of Example 13 is higher, which is due to the large difference in the total thickness of the metal layer in the current collector of Example 13 and the total thickness of the metal layer in the current collector of Example 1. In addition, although the square resistance or thermal shrinkage of the composite current collectors of Examples 11-13 and Example 17 changed, the capacity retention rates of the batteries of Examples 11-13 and Example 17 were still significantly higher than that of the battery of Comparative Example 1.

[0136] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0137] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, and these modifications and improvements fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.

Claims

1. A composite current collector, comprising a polymer film and a composite conductive layer arranged on at least one side of the polymer film, wherein the composite conductive layer comprises metal oxide layers and metal layers alternately stacked.

2. The composite current collector according to claim 1, wherein: The composite current collector has at least one of the following characteristics: (1a) The outermost layer of the composite conductive layer is the metal oxide layer; (1b) The innermost layer of the composite conductive layer is the metal oxide layer.

3. The composite current collector according to claim 1 or 2, wherein: In the composite conductive layer located on one side of the polymer film, the number of metal layers is N, N≥1, and N is an integer, and the number of metal oxide layers is M, M=N or M=N+1; Optionally, 2≤N≤50.

4. The composite current collector according to any one of claims 1 to 3, wherein: The metal oxide in the metal oxide layer includes one or more of aluminum oxide, silicon oxide, titanium oxide, copper oxide, nickel oxide, chromium oxide, zinc oxide, magnesium oxide, cobalt oxide, zirconium oxide, tin oxide and indium tin oxide.

5. The composite current collector according to any one of claims 1 to 4, wherein: The metal layer includes one or more of aluminum, copper, gold, silver, nickel and zinc.

6. The composite current collector according to any one of claims 1 to 5, wherein: The single layer thickness Hn of the metal oxide layer and the thickness Hm of the metal layer adjacent thereto satisfy the following condition: 0<Hn≤10%Hm.

7. The composite current collector according to any one of claims 1 to 6, wherein: The percentage of the total thickness of the metal oxide layer to the thickness of the composite conductive layer is ≤10%.

8. The composite current collector according to any one of claims 1 to 7, wherein: The thickness of the composite conductive layer is 500nm-2000nm, and can be optionally 700nm-1200nm.

9. The composite current collector according to any one of claims 1 to 8, wherein: The polymer in the polymer film includes one or more of polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene and polyimide.

10. The composite current collector according to any one of claims 1 to 9, wherein: The polymer film has a thickness of 1 μm-10 μm. 11 . The method for preparing the composite current collector according to claim 1 , comprising the following step: alternately preparing the stacked metal oxide layer and the metal layer on at least one side of the polymer film.

12. The preparation method according to claim 11, wherein The metal oxide layer and the metal layer are independently prepared by physical vapor deposition; Optionally, the physical vapor deposition method includes one or more of an evaporation method and a magnetron sputtering method.

13. An electrode plate, comprising the composite current collector according to any one of claims 1 to 10 or the composite current collector prepared by the preparation method according to any one of claims 11 to 12.

14. A battery comprising the electrode sheet according to claim 13.

15. An electrical device comprising the battery according to claim 14.

Citation Information

Patent Citations

  • Electrode pole piece and electrochemical device

    CN110676460A

  • Positive pole piece and electrochemical device

    CN112186195A

  • Positive current collector and preparation method thereof

    CN112751036A

  • Thermal shrinkage composite current collector and application thereof

    CN114497568A

  • Positive electrode plate, and electrochemical apparatus and electronic apparatus including such positive electrode plate

    US20220223836A1

Cited By

  • Functional foil current collector and preparation method thereof, pole piece and battery

    CN120565687A