Wire rod for fine steel wire cord, steel wire, cord, and manufacturing method therefor
By optimizing the chemical composition and production process, the problem of uneven hardness distribution in the cross-section of wire rods used for fine steel wire cords was solved, thereby improving hardness uniformity and stranding performance.
Patent Information
- Application Number
- PCT/CN2023/099163
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2023-06-08
- Publication Date
- 2024-12-05
AI Technical Summary
Existing technologies have failed to effectively solve the problem of uneven cross-sectional hardness distribution in wire rods used for fine steel wire cords, which affects the stranding performance of the steel wires.
By optimizing the chemical composition and production process, the hardness distribution of the wire rod and steel wire cross-section is controlled, thereby improving their uniformity and meeting users' requirements for strand performance.
It achieves uniformity of hardness in the cross-section of wire rod and steel wire, meets the processing performance requirements of fine steel wire cord, and improves the stranding performance.
Smart Images

Figure CN2023099163_05122024_PF_FP_ABST
Abstract
Description
Wire rod for fine steel cord, steel wire, cord and manufacturing method thereof Technical Field
[0001] The present invention belongs to the technical field of wire rod production methods, and in particular relates to a wire rod for fine steel cord, a steel wire, a cord and a manufacturing method thereof. Background Art
[0002] Cord steel wire rod is used in the production of tire steel cord. Wire rod undergoes various processes, including drawing and plying, during user use, leading to stringent requirements for its processing performance. The wire rod's microstructure hardness distribution is a key indicator of its processing performance. Wire rod microstructure hardness is a comprehensive reflection of its chemical composition and microstructure. Changes in microstructure hardness within the cross-section of the wire rod directly reflect its ability to deform uniformly within the cross-section. A more uniform hardness distribution across the cross-section of the wire rod promotes uniform hardness across the wire, thereby improving the plying performance of the wire and facilitating the manufacture of fine steel cord with complex and demanding structures.
[0003] Patent CN201910638740.0 discloses an ultrafine ultra-high strength steel wire, a wire rod for ultrafine ultra-high strength steel wire, and a production method thereof. The chemical composition of the wire rod for ultrafine ultra-high strength steel wire includes, by mass percentage, C 0.90% to 0.96%, Si 0.12% to 0.30%, Mn 0.30% to 0.65%, Cr 0.10% to 0.30%, Al ≤ 0.004%, Ti ≤ 0.001%, Cu ≤ 0.01%, Ni ≤ 0.01%, S ≤ 0.01%, P ≤ 0.01%, O ≤ 0.0006%, N ≤ 0.0006%, and the rest are Fe and unavoidable impurity elements, wherein the inclusion size is ≤ 4 μm, and the average density of brittle inclusions is ≤ 2 pieces / mm 2 . The wire rod for ultrafine and ultra-high strength steel wire can be used as the base material for the production of ultrafine and ultra-high strength steel wire with a diameter of 50 to 60 μm and a tensile strength of ≥4500 MPa, and in the process of drawing and preparing ultrafine and ultra-high strength steel wire, an unbroken wire mileage of ≥300 km can be achieved. The production method includes vacuum induction melting, remelting, forging and steel rolling. This patent focuses on ultrafine and ultra-high strength steel wire, wire rod for ultrafine and ultra-high strength steel wire and its production method. The above-mentioned wire rod is used in the production of ultrafine steel wire, and the stranding performance of the steel wire is not mentioned, nor is the cross-sectional hardness distribution of the wire rod and the steel wire.
[0004] In order to meet the user's requirements for the processing performance of wire rods for precision steel cord, especially the requirements for the stranding performance of steel wire made from wire rods, it is urgent to develop high-quality wire rods for precision steel cord so that the hardness distribution of its cross section is uniform, and the cross-sectional hardness distribution of steel wire prepared by wire rods is also uniform, laying the foundation for improving the stranding performance of steel wire.
[0005] Summary of the Invention
[0006] The purpose of the present invention is to provide a wire rod, steel wire, cord and a manufacturing method for fine steel cord. Through the chemical composition and production process design, the hardness distribution of the cross section of the wire rod and steel wire is uniform, meeting the user's requirements for the plying performance of the wire rod processing fine steel cord process.
[0007] In order to achieve the above object, the technical solution of the present invention is as follows:
[0008] A first aspect of the present invention provides a wire rod for fine steel cord, wherein the chemical composition of the wire rod comprises, by mass percentage:
[0009] C: 0.79% ~ 0.84%, Si: 0.15% ~ 0.30%, Mn: 0.45% ~ 0.55%, P ≤ 0.015%, S: 0.0030% ~ 0.010%, total oxygen: 0.0008% ~ 0.0022%, Als: 0.0002% ~ 0.0012%, Mg: 0.0002% ~ 0.0012%, Nb: 0.0003% ~ 0.0009%, Mo: 0.0003% ~ 0.0012%, and the balance is Fe and unavoidable impurities.
[0010] In the above technical solution, further, the ferrite Si content in the pearlite structure of the wire rod is 0.15% to 0.45%.
[0011] The selection principles and content design reasons of the chemical components of the present invention are as follows:
[0012] Carbon (C) is the primary element controlling steel wire strength. A steel wire with too low a carbon content will not meet user strength requirements, while one with too high a carbon content will exceed user requirements. Furthermore, a high carbon content increases the wire breakage rate during the drawing process, leading to increased scrap rates. Therefore, the carbon content in this invention is controlled between 0.79% and 0.84%.
[0013] Si: Silicon is the primary deoxidizing element in high-carbon steel. Low silicon content results in insufficient deoxidation of the molten steel. Excessive silicon content in the steel leads to the formation of coarse silicate inclusions, which reduces the drawability of the steel wire. Silicon dissolves into ferrite, increasing its hardness, reducing the hardness difference between ferrite and cementite, and improving the uniformity of the steel wire's microstructure. Therefore, the silicon content in this invention is controlled to 0.15% to 0.30%.
[0014] Mn: Manganese is an element that increases wire strength, ensuring the steel meets the user's tensile strength requirements. It also lowers the eutectoid transformation temperature of steel, refines the pearlite structure of the steel wire, and improves the deep processing capability of the steel wire. Therefore, the manganese content in this invention is controlled to 0.45% to 0.55%.
[0015] P: Phosphorus is prone to form banded segregation in the wire rod, which reduces the mechanical processing capability of the steel wire. Therefore, in the present invention, the silicon-phosphorus content is controlled to be ≤0.015%.
[0016] S: A high sulfur content in steel reduces the cold working properties of steel wire. Because MnS inclusions have excellent deformability, an appropriate amount of sulfur in the steel can reduce the damage caused by non-deformable inclusions and prevent the formation of microcracks caused by inclusions. Therefore, the sulfur content in the present invention is controlled to 0.0030% to 0.010%.
[0017] Total Oxygen: When the oxygen content is high, the inclusions in the steel are large and numerous, which can easily lead to microcracks during machining of the steel wire and cause the wire to split. When the oxygen content is low, the inclusions in the steel wire have poor deformation ability, which can easily cause microcracks to form between the inclusions and the steel wire matrix, hindering the improvement of the steel wire's machinability. Therefore, in the present invention, the total oxygen content of the steel wire is controlled within a range of 0.0008% to 0.0022%.
[0018] Als: When the acid-soluble aluminum content is high, Al2O3 inclusions in the steel become larger, which can easily cause cracking in the wire during processing. When the acid-soluble aluminum content in the wire rod is too low, the melting point of the inclusions in the steel is high, and the deformation capacity of the inclusions is reduced. This increases local stress in the wire during processing, making microcracks more likely to form in the wire, leading to cracking and breakage. Therefore, the acid-soluble aluminum content in the present invention is controlled to 0.0002% to 0.0012%.
[0019] Mg: Magnesium controls the oxygen content in steel and also controls the type of inclusions. High magnesium content leads to the formation of magnesia-alumina spinel inclusions, which reduce the processability of the steel wire. An appropriate magnesium content in steel improves the deformation properties of inclusions, expanding the range of inclusions with higher deformability, which helps improve the deformability of the steel wire. Therefore, the magnesium content in this invention is controlled to 0.0002% to 0.0012%.
[0020] Nb: Niobium inhibits grain growth during heating, thereby improving the uniformity of the steel wire's microstructure. However, excessive niobium content in the steel can significantly harden the wire rod during deformation, reducing its deep-processing capability. Therefore, the present invention limits niobium content to 0.0003% to 0.0009%.
[0021] Molybdenum (Mo): Molybdenum is a strong carbide-forming element. Its dispersed distribution of molybdenum carbides refines the steel wire grains and improves the uniformity of hardness distribution across the wire's cross section. However, excessive Mo content in steel reduces the machinability of the wire rod. Therefore, the Mo content in this patented material is controlled within a range of 0.0003% to 0.0012%.
[0022] A second aspect of the present invention provides a method for manufacturing the above-mentioned wire rod for fine steel cord, the method comprising the following steps:
[0023] (1) Continuous casting: The smelted molten steel is continuously cast, and the cross-sectional size of the continuous casting billet is (250-300) mm*(350-400) mm, the grain size of the continuous casting billet surface is 260-520 μm, the grain size of the continuous casting billet core is 800-1100 μm, the carbon segregation index at the 1 / 2 thickness position on the center line of the continuous casting billet cross section is controlled within the range of 0.95-1.07, the carbon segregation index at the 1 / 4 thickness position on the center line of the continuous casting billet cross section is controlled within the range of 0.96-1.06, and the carbon segregation index at the surface position on the center line of the continuous casting billet cross section is controlled within the range of 0.94-1.0;
[0024] (2) Heating and rolling: The continuous casting billet is hot charged, with a total furnace time of 3.8 to 4.5 hours, a soaking zone temperature of 1230 to 1280°C, and a soaking zone holding time of 40 to 60 minutes. After heating, the continuous casting billet is continuously rolled into a square billet, with a finishing rolling temperature of 940 to 1050°C and a billet cross-sectional size of (140 to 180) mm*(140 to 180) mm.
[0025] (3) Wire rod rolling: The total time of the billet in the furnace is 150-170 min, the temperature of the soaking section is 1130-1170 ° C, and the holding time of the soaking section is 30-50 min. Through the high-temperature diffusion of the billet, the segregation of elements such as carbon and manganese is reduced, and the grain size of the billet is controlled. After the billet is heated, it undergoes rough rolling, intermediate rolling, pre-finishing rolling, finishing rolling and double-module rolling before wire rod extrusion. The wire rod rolling specification is 5.0-6.0 mm.
[0026] (4) Wire rod cooling: After spinning, the wire rod is cooled on an air-cooled roller. The cementite precipitation temperature of the wire rod is controlled to be 740-770°C, and the pearlite phase transformation supercooling of the wire rod is controlled to be 100-150°C. When the phase transformation time on the air-cooled line is 4-6s, the pearlite content of the wire rod is ≥50%, and when the phase transformation time is 14-16s, the pearlite content is ≥95%. The wire rod after final cooling is mainly composed of sorbite, which is convenient for users to draw steel wire.
[0027] In the above technical solution, further, in step (1), the molten steel is molten iron and scrap steel, wherein the scrap steel accounts for 5% to 10% of the mass of the molten steel.
[0028] In the above technical solution, further, in step (1), the molten steel is refined in an LF furnace after being smelted in a converter, the LF furnace refining time is 30 to 50 minutes, the refining temperature is 1450 to 1550°C, and argon stirring is performed during the molten steel refining process, and the argon flow rate is 200 to 500NL / min.
[0029] In the above technical solution, further, in step (3), the pre-finishing rolling temperature of the rolled piece is 950-1000°C, and the temperature compensation deformation rate factor of the last pass of the pre-finishing rolling of the rolled piece is (1.1-2.6)*10 13 s -1 The temperature of the finished rolling is 880-960℃, and the temperature compensation deformation rate factor of the last pass of the finished rolling is (1.6-3.2)*10 14 s -1 The temperature of the double module is 890~940℃, and the temperature compensation deformation rate factor of the last pass of the double module is (4.5~9.9)*10 14 s -1 .
[0030] In the above technical solution, further, in step (3), the wire rod spinning temperature is 910-940°C. The higher spinning temperature of the wire rod increases the cooling rate of the wire rod on the air-cooled roller, laying the foundation for controlling the final structure of the wire rod.
[0031] A third aspect of the present invention provides a fine steel wire, which is manufactured using the above-mentioned wire rod.
[0032] A fourth aspect of the present invention provides a method for manufacturing the above-mentioned fine steel wire, comprising the following steps:
[0033] a. Mechanical descaling: The wire rod is mechanically descaled, and the residual rate of iron oxide scale on the wire rod surface is ≤0.07%;
[0034] b. Wire rod drawing: The wire rod is drawn through multiple passes to form an intermediate wire with a diameter of 0.8 to 1.2 mm;
[0035] c. Intermediate wire heat treatment: After the intermediate wire is heated to 880-915°C, it is cooled to 555-575°C and undergoes phase change;
[0036] d. Steel wire drawing: The intermediate wire after heat treatment is drawn into a steel wire with a diameter of 0.15 to 0.20 mm.
[0037] A fifth aspect of the present invention provides a fine cord, which is manufactured using the above-mentioned steel wire.
[0038] The beneficial effects of the present invention are:
[0039] The present invention achieves uniform hardness distribution across the cross-section of wire rods and steel wires through chemical composition and production process design, meeting users' requirements for the plying performance of wire rod processing into fine steel cords. The hardness difference at different parts of the cross-section of a wire rod with a diameter of 5.5 mm is controlled within 35 HV, and the hardness difference at the cross-section of a steel wire with a diameter of 0.175 mm is controlled within 10 HV, meeting users' quality requirements for the production of steel wires and steel cords. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 is a schematic diagram of a wire rod cross-section hardness test;
[0041] Figure 2 is a schematic diagram of the steel wire cross-section hardness test. DETAILED DESCRIPTION
[0042] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.
[0043] The chemical compositions of the wire rods of Examples 1-6 of the present invention are shown in Table 1.
[0044] Table 1 Chemical composition of wire rod
[0045] The method for manufacturing the fine steel cord wire rod comprises the following steps:
[0046] (1) Smelting: The molten steel is composed of molten iron and scrap steel, of which scrap steel accounts for 5% to 10% of the mass of the molten steel. The molten steel is smelted in a converter and then subjected to LF refining. The LF furnace refining time is 30 to 50 minutes, and the refining temperature is 1450 to 1550°C. Argon stirring is performed during the molten steel refining process, and the argon flow rate is 200 to 500 NL / min.
[0047] Table 2 Smelting process parameters
[0048] (2) Continuous casting: The smelted molten steel is continuously cast, and the cross-sectional size of the continuous casting billet is (250-300) mm*(350-400) mm, the grain size of the continuous casting billet surface is 260-520 μm, the grain size of the continuous casting billet core is 800-1100 μm, the carbon segregation index at the 1 / 2 thickness position on the center line of the continuous casting billet cross section is controlled within the range of 0.95-1.07, the carbon segregation index at the 1 / 4 thickness position on the center line of the continuous casting billet cross section is controlled within the range of 0.96-1.06, and the carbon segregation index at the surface position on the center line of the continuous casting billet cross section is controlled within the range of 0.94-1.0;
[0049] Table 3 Continuous casting process parameters
[0050] (3) Heating and rolling: The continuous casting billet is hot charged, with a total furnace time of 3.8 to 4.5 hours, a soaking zone temperature of 1230 to 1280°C, and a soaking zone holding time of 40 to 60 minutes. After heating, the continuous casting billet is continuously rolled into a square billet, with a finishing rolling temperature of 940 to 1050°C and a billet cross-sectional size of (140 to 180) mm*(140 to 180) mm.
[0051] Table 4 Heating and rolling process parameters
[0052] (4) Wire rod rolling: The total time of the billet in the furnace is 150-170 min, the temperature of the soaking section is 1130-1170 °C, and the holding time of the soaking section is 30-50 min. Through the high-temperature diffusion of the billet, the segregation of elements such as carbon and manganese is reduced, and the grain size of the billet is controlled. After the billet is heated, it undergoes rough rolling, intermediate rolling, pre-finishing rolling, finishing rolling and double-module rolling. The pre-finishing rolling temperature of the rolled piece is 950-1000 °C, and the temperature compensation deformation rate factor of the last pass of the pre-finishing rolling of the rolled piece is (1.1-2.6)*10 13 s -1 The temperature of the finished rolling is 880-960℃, and the temperature compensation deformation rate factor of the last pass of the finished rolling is (1.6-3.2)*10 14 s -1 The temperature of the double module is 890~940℃, and the temperature compensation deformation rate factor of the last pass of the double module is (4.5~9.9)*10 14 s -1 , followed by wire rod extrusion, the wire rod extrusion temperature is 910 ~ 940 ℃, through the high wire rod extrusion temperature, the wire rod cooling speed on the air cooling roller is increased, laying the foundation for controlling the final structure of the wire rod, the wire rod rolling specification is 5.0 ~ 6.0mm;
[0053] Table 5 Wire rod rolling process parameters
[0054] Table 6 Wire rod spinning process parameters
[0055] (5) Wire rod cooling: After spinning, the wire rod is cooled on an air-cooled roller. The cementite precipitation temperature of the wire rod is controlled to be 740-770°C, and the pearlite phase transformation supercooling of the wire rod is controlled to be 100-150°C. When the phase transformation time on the air-cooled line is 4-6s, the pearlite content of the wire rod is ≥50%, and when the phase transformation time is 14-16s, the pearlite content is ≥95%. The wire rod after final cooling is mainly composed of sorbite, which is convenient for users to draw steel wire.
[0056] Table 7 Wire rod cooling process parameters
[0057] The method for manufacturing steel wire using the coiled wire comprises the following steps:
[0058] a. Mechanical descaling: The wire rod is mechanically descaled, and the residual rate of iron oxide scale on the wire rod surface is ≤0.07%;
[0059] b. Wire rod drawing: The wire rod is drawn through multiple passes to form an intermediate wire with a diameter of 0.8 to 1.2 mm;
[0060] c. Intermediate wire heat treatment: After the intermediate wire is heated to 880-915°C, it is cooled to 555-575°C and undergoes phase change;
[0061] d. Steel wire drawing: The intermediate wire after heat treatment is drawn into a steel wire with a diameter of 0.15 to 0.20 mm.
[0062] Table 8 Steel wire manufacturing process parameters
[0063] The wire rods and steel wires of Examples 1-6 above were subjected to hardness tests;
[0064] Wire rod hardness test method: Divide the radius of the wire rod cross section into 5 equal parts, test the hardness values at 6 points from the surface to the core, and then analyze the hardness difference of the cross section. See Figure 1 for a schematic diagram.
[0065] Steel wire hardness test method: Divide the radius of the steel wire cross section into two equal parts, test the hardness values at three points from the surface to the core, and then analyze the hardness difference of the cross section. See Figure 2 for a schematic diagram.
[0066] The test results are shown in Table 9.
[0067] Table 9 Difference in cross-sectional hardness between wire rod (HV1) and steel wire (HV0.2)
[0068] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. The scope of protection of the present invention shall be determined by the scope defined in the claims. Other variations or modifications may be made based on the above description. Obvious variations or modifications derived therefrom shall remain within the scope of protection of the present invention.
Claims
1. A wire rod for fine steel cord, characterized in that: The chemical composition of the wire rod includes by mass percentage: C: 0.79% ~ 0.84%, Si: 0.15% ~ 0.30%, Mn: 0.45% ~ 0.55%, P ≤ 0.015%, S: 0.0030% ~ 0.010%, total oxygen: 0.0008% ~ 0.0022%, Als: 0.0002% ~ 0.0012%, Mg: 0.0002% ~ 0.0012%, Nb: 0.0003% ~ 0.0009%, Mo: 0.0003% ~ 0.0012%, the balance is Fe and unavoidable impurities.
2. The wire rod for fine steel cord according to claim 1, characterized in that: The ferrite Si content in the wire rod pearlite structure is 0.15% to 0.45%.
3. A method for manufacturing the wire rod for fine steel cord according to any one of claims 1 to 2, the method comprising the following steps: (1) Continuous casting: The smelted molten steel is continuously cast, the cross-sectional size of the continuous casting billet is (250-300) mm*(350-400) mm, the grain size of the continuous casting billet surface is 260-520 μm, the grain size of the continuous casting billet core is 800-1100 μm, the carbon segregation index at the 1 / 2 thickness position on the midline of the cross-sectional length of the continuous casting billet is controlled within the range of 0.95-1.07, the carbon segregation index at the 1 / 4 thickness position on the midline of the cross-sectional length of the continuous casting billet is controlled within the range of 0.96-1.06, and the carbon segregation index at the surface position on the midline of the cross-sectional length of the continuous casting billet is controlled within the range of 0.94-1.0; (2) Heating and rolling: The continuous casting billet is hot charged, the total furnace time is 3.8-4.5h, the soaking section temperature is 1230-1280℃, the soaking section holding time is 40-60min, the continuous casting billet is heated and continuously rolled into a square billet, the final rolling temperature is 940-1050℃, and the cross-sectional size of the square billet is (140-180)mm*(140-180)mm; (3) Wire rod rolling: The total furnace time of the square billet is 150-170 min, the temperature of the soaking section is 1130-1170 ° C, and the soaking section holding time is 30-50 min. After the square billet is heated, it undergoes rough rolling, intermediate rolling, pre-finishing rolling, finishing rolling and double module rolling before wire rod extrusion. The wire rod rolling specification is 5.0-6.0 mm; (4) Wire rod cooling: After spinning, the wire rod is cooled on an air-cooled roller. The cementite precipitation temperature of the wire rod is controlled to be 740-770°C, and the pearlite phase transformation undercooling degree of the wire rod is controlled to be 100-150°C. When the phase transformation time on the air-cooled line is 4-6s, the pearlite content of the wire rod is ≥50%; when the phase transformation time is 14-16s, the pearlite content is ≥95%.
4. The manufacturing method according to claim 3, characterized in that: In step (1), the molten steel is molten iron and scrap steel, wherein the scrap steel accounts for 5% to 10% of the mass of the molten steel.
5. The manufacturing method according to claim 3, characterized in that: In step (1), after the molten steel is smelted in a converter, it is refined in an LF furnace, the LF furnace refining time is 30 to 50 minutes, the refining temperature is 1450 to 1550° C., and argon stirring is performed during the molten steel refining process, and the argon flow rate is 200 to 500 NL / min.
6. The manufacturing method according to claim 3, characterized in that: In step (3), the pre-finishing rolling temperature of the rolled piece is 950-1000°C, and the temperature compensation deformation rate factor of the last pass of the pre-finishing rolling of the rolled piece is (1.1-2.6)*10 13 s -1 ; The temperature of the finished rolling is 880~960℃, and the temperature compensation deformation rate factor of the last pass of the finished rolling is (1.6~3.2)*10 14 s -1 ; The temperature of entering the double module is 890~940℃, and the temperature compensation deformation rate factor of the last pass of the double module of the rolled piece is (4.5~9.9)*10 14 s -1 .
7. The manufacturing method according to claim 3, characterized in that: In step (3), the wire rod spinning temperature is 910-940°C.
8. A fine steel wire, characterized in that: The steel wire is manufactured using the wire rod described in any one of claims 1-2.
9. A method for manufacturing the fine steel wire according to claim 8, characterized in that: The steps include: a. Mechanical descaling: The wire rod is mechanically descaled, and the residual iron oxide scale rate on the wire rod surface is ≤0.07%; b. Wire rod drawing: The wire rod is drawn through multiple passes to form an intermediate wire with a diameter of 0.8 to 1.2 mm; c. Heat treatment of intermediate wire: After the intermediate wire is heated to 880-915°C, it undergoes phase change at 555-575°C after cooling; d. Wire drawing: The intermediate wire after heat treatment is drawn into a steel wire with a diameter of 0.15-0.20 mm.
10. A fine cord, characterized in that: The cord is made of the steel wire according to claim 8.
Citation Information
Patent Citations
Production methods of ultra-fine and ultra-high strength steel wire, wire rod and wire rod
CN110230008B
Steel wire rod for 80 grade core thread external winding wire and manufacturing method of steel wire rod
CN105483557A
High-carbon steel wire rod low in network cementite precipitation and used for fine wire drawing and production method of high-carbon steel wire rod
CN108396221A
Low-cost cord steel wire rod and production method thereof
CN110453153A
Wire rod for ultrahigh-strength steel wire cord, steel wire, cord and manufacturing method
CN115161558A
Cited By
Production method for inhibiting martensite transformation in 80-grade tire cord steel wire rod
CN119307802A