Negative pressure formation method for lithium manganese iron phosphate battery and battery applying method
Through the negative pressure transformation method and three-stage constant current charging, the problems of gas production and brown spots during the transformation of lithium manganese iron phosphate battery are solved, the circulation and storage performance of the battery are improved, and more efficient electrochemical performance is achieved.
Patent Information
- Application Number
- PCT/CN2023/101024
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2023-06-19
- Publication Date
- 2024-12-05
AI Technical Summary
Lithium manganese iron phosphate batteries are prone to serious gas production and brown spot problems during the chemical formation process. The existing lithium iron phosphate process is not completely applicable, resulting in poor battery performance.
The negative pressure generation method is adopted, and the state of charge and charging current is controlled through three-stage constant current charging and vacuum extraction, and the charging current is gradually increased to adjust the stability and density of the SEI film, reducing gas production and brown spot phenomena.
It effectively reduces gas production and brown spot problems during the formation of lithium manganese iron phosphate batteries, improves the circulation and storage performance of the batteries, and improves the electrochemical performance and production efficiency.
Smart Images

Figure CN2023101024_05122024_PF_FP_ABST
Abstract
Description
A negative pressure formation method for lithium manganese iron phosphate battery and battery using the same
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 31, 2023, with application number 2023106499718. The entire contents of the above application are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of lithium battery manufacturing, and in particular to a negative pressure formation method for a lithium manganese iron phosphate battery and a battery using the same. Background Art
[0003] As the energy density of lithium iron phosphate (LFP) batteries gradually surpasses the limits of the system, LFP (LIM) is gradually entering the attention of major manufacturers due to its higher voltage platform (3.6V). A high voltage platform can increase the energy density of the corresponding battery. In certain cases, the energy density of LFP batteries is more than 15% higher than that of LFP batteries, basically reaching the level of NCM523. At the same time, the safety performance of LFP batteries is far superior to that of ternary batteries, leading to increasing research on LFP batteries.
[0004] During the battery cell manufacturing process, the formation step is a particularly crucial step in the post-processing phase. Formation is the initial charging process for the battery cell and the first stage of formation of the SEI film at the negative electrode interface. The structure of the SEI directly impacts the battery cell's DCR, cycling, and storage performance. Lithium manganese iron phosphate (LMFP) batteries are most commonly used in commercial vehicles and energy storage, placing extremely high demands on cycling and storage.
[0005] However, there is currently little research on the formation process for lithium iron phosphate (LFP) batteries. Because LFP and LFP both belong to the phosphate system, most manufacturers currently simply adopt the LFP system's formation scheme with simple modifications. Due to LFP's higher platform voltage and dual-platform voltage, the LFP system's formation process is not fully applicable to the LFP system. Furthermore, due to the system's unique characteristics, LFP battery formation can result in severe gassing and brown spots at the interface between the two cells.
[0006] Summary of the Invention
[0007] In order to improve the problem of severe gas production and brown spots in lithium manganese iron phosphate batteries during formation, the present application provides a negative pressure formation method for lithium manganese iron phosphate batteries and a battery using the same.
[0008] In the first aspect, the embodiment of the present application provides a negative pressure formation method for a lithium manganese iron phosphate battery, the method comprising the following steps: vacuuming, standing, and charging a semi-finished battery cell to obtain a formed battery cell; the charging process is a three-stage constant current charging process, wherein, during the three-stage constant current charging process, the charging current I and the state of charge S must satisfy the following relationship: in the first stage of constant current charging, I1≤0.1C, state of charge 5%≤S1≤15%; in the second stage of constant current charging, 0.05C≤I2≤0.15C, state of charge 15%≤S2≤25%; in the third stage of constant current charging, 0.15C≤I3≤0.25C, state of charge 35%≤S3≤45%. The negative pressure formation method provided by the present application utilizes negative pressure (vacuuming) to promptly discharge the gas generated by the semi-finished battery cell during the formation process; and by controlling the state of charge (SOC) and charging current of the semi-finished battery cell during the formation process, the problem of brown spots in the lithium manganese iron phosphate battery is improved.
[0009] In one embodiment, during the three-stage constant current charging process, the current I1 < I2 < I3. During the three-stage constant current charging process, gradually increasing the charging current is beneficial to adjusting the balance between the stability and density of the SEI film. This is because when the formation current is large, the electron transmission speed of the external circuit is fast. In order to balance the electrochemical reaction, the lithium ion diffusion speed inside the battery is fast, and the speed of forming the SEI film is fast, but at the same time, the stability of the SEI film formed during the formation is poor. On the other hand, when the formation current is too low, the lithium ion diffusion speed inside the battery is slow, and the SEI film formed is relatively stable, but the ion permeability of the SEI film is reduced. Therefore, increasing or decreasing the charging current has both advantages and disadvantages to the formation method. When charging the semi-finished battery cell using a step-by-step constant current charging method, it helps to timely adjust the balance between the stability and density of the SEI film during the formation process.
[0010] In one embodiment, the vacuum treatment is to vacuum the semi-finished battery cell to -90 to -80 KPa.
[0011] In one embodiment, the electrolyte of the semi-finished battery cell includes a solute, a solvent, and an additive, wherein the additive includes vinylene carbonate (VC).
[0012] In one embodiment, the additive of the electrolyte of the semi-finished battery cell further includes fluoroethylene carbonate (FEC).
[0013] In one embodiment, the solute of the electrolyte of the semi-finished battery cell includes lithium hexafluorophosphate (LiPF6).
[0014] In one embodiment, the solvent of the electrolyte of the semi-finished battery cell includes at least one of ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethylene glycol dimethyl ether (DME), and propylene carbonate (PC).
[0015] In one embodiment, the filling coefficient of the semi-finished battery cell is 3.0-4.0, where the filling coefficient refers to the ratio of the electrolyte filling volume to the rated capacity.
[0016] In one embodiment, a negative pressure formation method for a lithium manganese iron phosphate battery includes the following steps: S1. At a formation temperature of 35 to 55° C., the semi-finished battery cell is vacuumed to -90 to -80 KPa, left to stand for 3 to 10 minutes, and then a first constant current charge is performed, wherein the charging current I1 is ≤ 0.1C, and charging is stopped when the state of charge S1 reaches 5 to 15%; S2. A second constant current charge is performed, wherein the charging current I2 is 0.05 to 0.15C, and charging is stopped when the state of charge S2 reaches 15 to 25%; S3. A third constant current charge is performed, wherein the charging current I3 is 0.05 to 0.15C, and charging is stopped when the state of charge reaches S335 to 45%, thereby obtaining a formed battery cell.
[0017] In one embodiment, in S1 , S2 , and S3 , a constant vacuum level is maintained.
[0018] In one embodiment, in steps S1, S2, and S3, after each charging stop, the semi-finished battery cells are allowed to rest for 3 to 10 minutes. Resting the cells after each charging stop allows the electrolyte to fully penetrate the interior of the battery, ensuring internal battery stability and allowing the electrochemical reactions within the battery to reach equilibrium. This also improves monitoring accuracy during the formation process.
[0019] In one embodiment, the semi-finished battery cell is a prismatic battery cell or a soft-pack battery cell.
[0020] In a second aspect, an embodiment of the present application provides a lithium iron manganese phosphate battery, wherein the positive electrode active coating of the lithium iron manganese phosphate battery includes a lithium iron manganese phosphate material, and the lithium iron manganese phosphate battery is subjected to a negative pressure formation treatment using any of the methods described above.
[0021] In one embodiment, the coating density of the positive electrode active coating of the lithium manganese iron phosphate battery is 200-250 g / m 2 .
[0022] In one embodiment, the negative electrode active coating of the lithium manganese iron phosphate battery includes at least one of graphite and silicon-carbon composite materials.
[0023] In one embodiment, the coating area density of the negative electrode active coating of the lithium manganese iron phosphate battery is 100-125 g / m2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0024] FIG1 is a lithium manganese iron phosphate battery cell prepared by the negative pressure formation method provided by treatment group 1A of Example 1;
[0025] FIG2 shows a lithium manganese iron phosphate battery cell prepared by the negative pressure formation method provided in the comparative group 3E of Example 5. DETAILED DESCRIPTION
[0026] Example 1
[0027] 1. Preparation of semi-finished battery cells
[0028] Step 1. Prepare a slurry of negative electrode material graphite, conductive agent acetylene black, binder CMC, and SBR in a mass ratio of 94:1:2:3 and apply it to the copper foil current collector, followed by vacuum drying to obtain a negative electrode sheet;
[0029] Step 2. LiMn cathode material 0.6 Fe 0.4 PO4, conductive agent acetylene black, and binder PVDF are prepared into a slurry in a mass ratio of 94:3:3 and coated on an aluminum foil current collector, which is then vacuum-dried to obtain a positive electrode sheet.
[0030] Step 3. Prepare the electrolyte: The electrolyte used is a mixture of EC, DMC, and EMC dissolved in 1 mol / L LiPF6, with a mass ratio of EC:DMC:EMC = 1:1:1. In addition, the electrolyte also contains 0.5% VC and 1% FEC.
[0031] Step 4. Assemble the positive electrode sheet, negative electrode sheet, Celgard2400 separator and electrolyte into semi-finished soft-pack batteries.
[0032] 2. Form the prepared soft pack battery
[0033] S1. Evacuate the semi-finished cell to -85 kPa at a formation temperature of 45°C and maintain a constant vacuum and temperature throughout the formation process. Allow the cell to rest for 5 minutes. Then, perform the first constant-current charge at a charging current I1 of 0.05C. Stop charging when the state of charge (S1) reaches 10%, and allow the cell to rest for 5 minutes.
[0034] S2. Perform the second constant current charge, where the charging current I2 is 0.1C. When the state of charge S2 reaches 20%, charging is stopped and the device is left standing for 5 minutes.
[0035] S3. Perform the third constant current charging, wherein the charging current I3 is 0.2C. When the state of charge S3 reaches 40%, the charging is stopped and the battery is left to stand for 5 minutes to obtain the formed battery cell.
[0036] The treatment groups 1A to 4A and the comparative groups 1A to 3A of Example 1 used the current of the three-stage constant current charge in the negative pressure formation method of the lithium manganese iron phosphate battery as a variable. The variables of the treatment groups 1A to 4A and the comparative groups 1A to 3A of Example 1 are shown in Table 1. Except for the above differences, the preparation of the semi-finished soft-pack battery cells and the negative pressure formation method operating steps of the treatment groups 1A to 4A and the comparative groups 1A to 3A of Example 1 were strictly consistent.
[0037] Table 1. Variables of cells formed in treatment groups 1A to 4A and comparison groups 1A to 3A
[0038] Test Example 1
[0039] 1. Test subjects
[0040] The battery cells of each treatment group and control group after formation in Example 1.
[0041] 2. Test Method
[0042] (1) HPPC test: The formed cell is subjected to a 2C discharge current for 10 seconds at 25°C. After standing for 40 seconds, a 1C charge current is applied to the battery for 10 seconds. The DC internal resistance (DCIR) of the cell is calculated.
[0043] (2) Cycle test: At 25°C, the lithium-ion battery is charged at a constant current of 1C to a voltage of 4.2V, and then charged at a constant voltage of 4.2V to a current of 0.05C. The above is considered one charge-discharge cycle. The battery cell is subjected to 1000 charge-discharge cycles at 25°C under the above conditions. The capacity retention rate is calculated according to formula ①.
[0044] (3) Storage stability test: At room temperature, the lithium-ion battery was charged at a constant current of 1C to a voltage of 4.2V, then charged at a constant voltage of 4.2V to a current of 0.05C. The initial capacity retention rate of the battery cell was measured. The battery cell was then stored in a 55°C constant temperature box for 30 days, after which the final capacity retention rate of the battery cell was measured. The storage capacity recovery rate was calculated according to formula ②.
[0045] (4) Battery cell status: To determine the normal standard of the battery cell, there are no obvious black spots on the surface of the electrode, and the color of the interface is uniform.
[0046] (5) Liquid loss rate: Use electronic weighing method to test the electrolyte loss rate (i.e. the percentage of electrolyte loss to the mass of injected electrolyte) by measuring the difference between the weight of the battery cell before formation and the weight of the battery cell after formation.
[0047] (6) Formation time: Use a timer to measure the formation time.
[0048] 3. Test results and analysis
[0049] The test results of this test example are shown in Table 2, wherein this test example mainly explores the effect of the change in current on the battery cell during the three-stage constant current charging during the formation method. First, in the comparison group 1A, due to the small formation current, the formation time is long, the production efficiency is significantly reduced, and in addition, the diffusion rate of lithium ions inside the battery is relatively slow, the ion permeability of the SEI film is reduced, resulting in an increase in the charging polarization internal resistance of the battery cell. In the comparison group 2A, the formation current is too large. Although the formation time is short, due to the fast electron transmission speed of the external circuit, in order to balance the electrochemical reaction, the diffusion rate of lithium ions inside the battery is fast, and the stability of the SEI film formed during formation is poor, which causes the SEI film of the battery cell used in long-term circulation to fall off, thereby continuously forming a new SEI film, increasing the irreversible capacity loss of the battery cell, and accelerating the capacity decay of the battery cell, resulting in a poor capacity retention rate of the battery cell after formation and a large internal resistance.
[0050] Secondly, during the three-stage constant current charging process, treatment groups 1A to 3A gradually increased the charging current. Furthermore, as the current increased within the same step, the electrical performance of the corresponding formed cells showed a trend of first increasing and then decreasing. This is because increasing or decreasing the formation current affects the formation of the SEI film. Therefore, this test example confirms that the formation current affects the balance between the stability and density of the SEI film in the battery cell. Among treatment groups 1A to 3A, the electrical performance of the cells formed in treatment group 1A was the best, as shown in Figure 1. In treatment group 4A, the cells were not formed using a gradually increasing charging current method. Test results show that the electrochemical performance of the cells formed in treatment group 4A declined compared to those formed in treatment group 1A.
[0051] Table 2. Test results of this test case
[0052] Example 2
[0053] In this embodiment, treatment group 1B was set up according to treatment group 1A of Example 1. Furthermore, treatment groups 1B-3B and comparative groups 1B-2B of Example 2 used the charge state of the three-stage constant current charging in the negative pressure formation method for lithium manganese iron phosphate batteries as a variable. The variables for treatment groups 1B-3B and comparative groups 1B-2B are shown in Table 3. Furthermore, the preparation of semi-finished soft-pack batteries and the negative pressure formation method procedures for treatment groups 1B-3B and comparative groups 1B-2B of Example 2 were strictly consistent with those of treatment group 1A of Example 1.
[0054] Table 3. Variables of cells formed in treatment groups 1B to 3B and comparison groups 1B to 2B
[0055] Test Example 2
[0056] 1. Test subjects
[0057] The cells of each treatment group and the control group after formation in Example 2.
[0058] 2. Test Method
[0059] Refer to the test method in Test Example 1.
[0060] 3. Test results and analysis
[0061] The test results for this example are shown in Table 4. This test primarily explored the impact of changes in SOC on the battery cells during three-stage constant-current charging during the formation process. For lithium manganese iron phosphate batteries, the SOC setting not only affects the formation time but also influences whether the cells will develop brown spots. For treatment groups 1B-3B, as the SOC increases during the same step, the electrical performance of the corresponding formed cells shows a trend of first increasing and then decreasing.
[0062] In comparison group 1B, when the SOC state of each of the three-stage constant-current charging is too low, the formation time is long and the internal resistance increases significantly; in comparison group 2B, when the SOC state of each of the three-stage constant-current charging is too high, although the formation time is short, black spots appear on the surface of the battery cell and the storage performance is significantly reduced.
[0063] Table 4. Test results of this test case
[0064] Example 3
[0065] In this embodiment, treatment group 1C was set up according to treatment group 1A of Example 1. Furthermore, the vacuum degree of the three-stage constant current charging in the negative pressure formation method for lithium manganese iron phosphate batteries in treatment groups 1C to 5C and comparative group 1C of Example 3 was used as a variable. The variables for treatment groups 1C to 5C and comparative group 1C are shown in Table 5. Furthermore, the preparation of semi-finished soft-pack batteries and the negative pressure formation method in treatment groups 1C to 5C of Example 3 and comparative group 1C were strictly consistent with those in treatment group 1A of Example 1.
[0066] Table 5. Variables of cells formed in treatment groups 1C to 5C and control group 1C
[0067] Test Example 3
[0068] 1. Test subjects
[0069] The cells of each treatment group and control group after formation in Example 3.
[0070] 2. Test Method
[0071] Refer to the test method in Test Example 1.
[0072] 3. Test results and analysis
[0073] The test results of this test example are shown in Table 6. This test example primarily explored the effects of varying vacuum levels on battery cells during three-stage constant-current charging during the formation method. As can be seen in control group 1C, the lithium iron phosphate (LFP) cells formed under normal pressure exhibited severe flatulence, significantly impacting their storage stability and electrochemical performance. In treatment groups 1C to 5C, the effects of varying negative pressures on the performance of the cells were explored. For the cells formed under treatment groups 1C to 5C, the electrochemical performance and storage stability of the cells initially increased and then decreased with decreasing vacuum levels. The test results indicate that the LFP cells formed under vacuum levels of -90 to -80 kPa exhibited superior electrochemical performance and storage stability. The LFP cells formed in treatment group 1C exhibited the best performance.
[0074] Table 6. Test results of this test case
[0075] Example 4
[0076] In this embodiment, treatment group 1D was set up based on treatment group 1A of Example 1. Furthermore, treatment groups 1D to 5D of Example 4 used the formation temperature in the negative pressure formation method for lithium manganese iron phosphate batteries as a variable. The variables for treatment groups 1D to 5D are shown in Table 7. Furthermore, treatment groups 1D to 5D of Example 4 prepared semi-finished soft-pack batteries with reference to treatment group 1A of Example 1, and the negative pressure formation method operating steps remained strictly consistent.
[0077] Table 7. Variables of cells formed in treatment groups 1D to 5D
[0078] Test Example 4
[0079] 1. Test subjects
[0080] The cells of each treatment group and control group after formation in Example 4.
[0081] 2. Test Method
[0082] Refer to the test method in Test Example 1.
[0083] 3. Test results and analysis
[0084] The test results of this test example are shown in Table 8. This test example primarily explored the impact of changes in the formation temperature during the negative pressure formation method on the lithium manganese iron phosphate battery cells. In treatment groups 1D to 5D, as the formation temperature increased, the electrochemical performance and storage stability of the lithium manganese iron phosphate cells showed a trend of first increasing and then decreasing. The test results show that when the formation temperature was 35 to 55°C, the lithium manganese iron phosphate cells obtained had better electrochemical performance and storage stability. The lithium manganese iron phosphate cells obtained in treatment group 1D had the best performance.
[0085] Table 8. Test results of this test case
[0086] Example 5
[0087] Treatment group 1E
[0088] This treatment group is set up as treatment group 1E according to the preparation method of semi-finished soft-pack batteries and negative pressure formation provided by treatment group 1A in Example 1.
[0089] Treatment group 2E
[0090] This treatment group uses the negative pressure formation method provided by treatment group 1E of Example 5 to form the prepared battery cells. The difference between this treatment group and treatment group 1E of Example 5 is that this treatment group only performs vacuum treatment before the first constant current charging. In addition to the above differences, the operating steps of preparing semi-finished soft-pack battery cells and negative pressure formation method of this treatment group are strictly consistent with those of treatment group 1E of Example 5.
[0091] Treatment group 3E
[0092] This treatment group uses the negative pressure formation method provided by treatment group 1E of Example 5 to form the prepared battery cells. The difference between this treatment group and treatment group 1E of Example 5 is that this treatment group does not undergo static treatment after three-stage constant current charging. In addition to the above differences, the operating steps of preparing semi-finished soft-pack battery cells and negative pressure formation method of this treatment group are strictly consistent with those of treatment group 1E of Example 5.
[0093] Control group 1E
[0094] This comparative group used the negative pressure formation method provided by treatment group 1E of Example 5 to form the prepared battery cells. The difference between this comparative group and treatment group 1E of Example 5 is that this comparative group only used a one-step constant current charging to a state of charge of 40%. Apart from the above differences, the operating steps for preparing the semi-finished soft-pack battery cells and the negative pressure formation method of this comparative group were strictly consistent with those of treatment group 1E of Example 5. Specifically, the steps of the soft-pack battery formation method of this comparative group are as follows:
[0095] At a formation temperature of 45°C, the semi-finished battery cell was evacuated to -85KPa and a constant vacuum and temperature were maintained during the subsequent formation process. The cell was allowed to stand for 5 minutes and then subjected to constant current charging. The charging current I was 0.1C. Charging was stopped when the state of charge S reached 40%. The cell was allowed to stand for 5 minutes to obtain a formed battery cell.
[0096] Control group 2E
[0097] This comparative group used the negative pressure formation method provided by treatment group 1E of Example 5 to form the prepared battery cells. The difference between this comparative group and treatment group 1E of Example 5 is that this comparative group used four-stage constant current charging to a state of charge (SOC) of 40%. Apart from the above differences, the operating steps for preparing the semi-finished soft-pack battery cells and the negative pressure formation method of this comparative group were strictly consistent with those of treatment group 1E of Example 5. Specifically, the steps of the soft-pack battery formation method of this comparative group were as follows:
[0098] S1-S2 were strictly consistent with treatment group 1E of Example 5;
[0099] S3. Perform the third constant current charge, where the charging current I3 is 0.2C. When the state of charge S3 reaches 30%, charging is stopped and allowed to stand for 5 minutes.
[0100] S4. Perform the fourth constant current charging, wherein the charging current I3 is 0.3C. When the state of charge S4 reaches 40%, the charging is stopped and the battery is left to stand for 5 minutes to obtain the formed battery cell.
[0101] Control group 3E
[0102] This comparative group used the negative pressure formation method provided by treatment group 1E of Example 5 to form the prepared battery cells. The difference between this comparative group and treatment group 1E of Example 5 is that this comparative group used a three-step constant current charging and one-step constant voltage method to form the battery cells. Apart from the above differences, the operating steps for preparing the semi-finished soft-pack battery cells and the negative pressure formation method of this comparative group were strictly consistent with those of treatment group 1E of Example 5. Specifically, the steps of the soft-pack battery formation method of this comparative group are as follows:
[0103] S1-S2 were strictly consistent with treatment group 1E of Example 5;
[0104] S3. Perform the third constant current charge, where the charging current I3 is 0.2C. When the voltage reaches 4.2V, charge at a constant voltage until the current reaches 0.05C and then stop charging. Let it stand for 5 minutes, at which point the state of charge S3 reaches 100%.
[0105] Test Example 5
[0106] 1. Test subjects
[0107] The battery cells of each treatment group and the control group after formation in Example 5.
[0108] 2. Test Method
[0109] Refer to the test method in Test Example 1.
[0110] 3. Test results and analysis
[0111] The test results of this test example are shown in Table 9, in which this test example mainly explores the impact of the negative pressure formation method of the lithium manganese iron phosphate battery on the battery cell. In the comparison group 1E, the lithium manganese iron phosphate battery cell was not formed using segmented constant current charging. From the test results and the observation of the state of the battery cell after formation, it can be seen that when the battery cell SOC state is 40% by one step of constant current charging, brown spots will appear on the battery cell, the stability of the SEI film formed is low, and the electrochemical performance will be greatly reduced. In the comparison group 2E, four-stage constant current charging is used, the steps are more cumbersome, and the production efficiency is reduced. In the comparison group 3E, as shown in Figure 2, in the last step of charging, the battery cell is charged using a constant current and constant voltage method, which causes brown spots to appear on the surface of the battery cell and a decrease in the electrochemical performance of the obtained lithium iron phosphate battery cell.
[0112] Compared to treatment group 1E, the storage stability of the lithium iron phosphate cells produced using the formation method provided by treatment group 2E decreased. This may be because the negative pressure can promptly discharge the gases generated during the formation process. Although treatment group 2E also uses negative pressure for formation, the lack of constant negative pressure leads to a decrease in storage stability. The electrochemical performance of the lithium iron phosphate cells produced using the formation method provided by treatment group 3E decreased. This may be due to the lack of timely rest after charging, which reduces the internal stability of the cells.
[0113] Table 9. Test results of this test case
Claims
1. A negative pressure formation method for a lithium manganese iron phosphate battery, the method comprising the following steps: vacuumizing, standing, and charging a semi-finished battery cell to obtain a formed battery cell; The charging process is a three-stage constant current charging, wherein: In the three-stage constant current charging process, the charging current I and the state of charge S need to satisfy the following relationship: The first stage is constant current charging, I1≤0.1C, state of charge 5%≤S1≤15%; The second stage is constant current charging, 0.05C≤I2≤0.15C, state of charge 15%≤S2≤25%; The third stage is constant current charging, 0.15C≤I3≤0.25C, state of charge 35%≤S3≤45%.
2. The method of claim 1, wherein: In the three-stage constant current charging process, the current I1<I2<I3.
3. The method of claim 1, wherein: The vacuum treatment is to vacuum the semi-finished battery cell to -90 to -80 KPa.
4. The method of claim 1, wherein: The electrolyte of the semi-finished battery cell includes a solute, a solvent, and an additive, wherein the additive includes vinylene carbonate.
5. The method of claim 4, wherein: The liquid injection coefficient of the semi-finished battery cell is 3.0-4.
0.
6. The method according to any one of claims 1 to 5, wherein: The method comprises the following steps: S1. At a formation temperature of 35 to 55°C, the semi-finished battery cell is evacuated to -90 to -80Kpa, left to stand for 3 to 10 minutes, and then the first constant current charging is performed, the charging current I1≤0.1C, and the charging is stopped when the state of charge S1 reaches 5 to 15%; S2. Perform the second constant current charging, wherein the charging current I2 is 0.05-0.15C, and charging is stopped when the state of charge S2 reaches 15-25%; S3. Perform the third constant current charging, wherein the charging current I3 is 0.05-0.15C, and stop charging when the state of charge S3 reaches 35-45% to obtain a formed battery cell.
7. The method of claim 6, wherein: In S1, S2 and S3, a constant vacuum degree is maintained.
8. The method of claim 7, wherein: In the steps S1, S2 and S3, each time charging is stopped, the semi-finished battery cell needs to be left to stand for 3 to 10 minutes.
9. The method of claim 6, wherein: The semi-finished battery cell is a square battery cell or a soft-pack battery cell.
10. A lithium iron manganese phosphate battery, wherein the positive electrode active coating of the lithium iron manganese phosphate battery comprises a lithium iron manganese phosphate material, and the lithium iron manganese phosphate battery is subjected to negative pressure formation treatment using the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Lithium ion battery formation method
CN107768723A
Lithium ion battery formation process and lithium ion battery obtained by same
CN111883866A
Formation method of square aluminum shell battery
CN113725508A
Lithium iron phosphate battery and formation method thereof
CN115966790A
Lithium ion secondary battery and charging method therefor
US20150380777A1