Coated positive electrode material and preparation method therefor, coating processing system for positive electrode material, and secondary battery
Through nano spray treatment and calcination technology, the problems of unevenness and continuity of the coating layer of the positive electrode material are solved, the electrochemical stability and preparation efficiency are improved, and the efficient and low-cost preparation of the coated positive electrode material is achieved.
Patent Information
- Application Number
- PCT/CN2023/114665
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2023-08-24
- Publication Date
- 2024-12-05
AI Technical Summary
In the existing method of coating the cathode material, there are problems of unevenness and discontinuity of the coating layer, which affects the electrochemical performance of the battery.
Using nano spray treatment technology, the coating material and the positive electrode material body are spray mixed in a rolling state through a three-dimensional mixer, and calcined in the pyrolysis equipment to form a nano-clad layer to ensure uniform distribution and continuity of the coating elements. .
The uniformity and continuity of the coating layer are improved, the electrochemical stability is enhanced, and the material bonding and wall adhesion problems in wet coating are avoided, achieving low-cost and efficient preparation.
Smart Images

Figure PCTCN2023114665-FTAPPB-I100001 
Figure 00000017_0000 
Figure 00000017_0001
Abstract
Description
Coated positive electrode material and preparation method thereof, coating processing system for positive electrode material and secondary battery
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 29, 2023, with application number 2023106115402 and invention name “Coated positive electrode material and preparation method thereof, coating processing system of positive electrode material and secondary battery”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of electrochemical technology, and in particular to a coated positive electrode material and a preparation method thereof, a coating processing system for the positive electrode material, and a secondary battery. Background Art
[0003] With the development of new energy vehicles, the research and development of high-capacity, long-life, low-cost, safe and environmentally friendly cathode materials is particularly urgent. Currently, commercial lithium battery cathode materials mainly include layered lithium cobalt oxide, ternary materials, spinel lithium manganese oxide, and olivine lithium iron phosphate. Different types of cathode materials have different advantages and disadvantages, and usually need to be modified and improved through methods such as doping and coating to adapt to actual usage requirements. Among them, the main function of coating is to act as a protective layer to isolate the direct contact between the electrolyte and the active electrode material, reduce the occurrence of side reactions, such as reducing transition metal precipitation, forming a thinner SEI film, and reducing the precipitation of oxygen atoms, thereby improving electrochemical stability.
[0004] However, in the current conventional coating treatment, the main method used is a rough coating (dry or wet method) synthesis method to modify the positive electrode active material. Although this method is simple and low-cost, the coating layer usually has problems of unevenness and discontinuity, resulting in part of the active material surface still being exposed to the electrolyte, thereby affecting the electrochemical performance of the battery.
[0005] Summary of the Invention
[0006] Based on this, the present application provides a coated positive electrode material and a preparation method thereof, a coating processing system for the positive electrode material, and a secondary battery to improve the uniformity and continuity of the coating layer.
[0007] The first aspect of the present application provides a coated positive electrode material, comprising: a positive electrode material body and a nano-coating layer coated on the surface of the positive electrode material body, the nano-coating layer containing a coating element, the theoretical content of the coating element in the coated positive electrode material is m wt%, and the average value of the actual content of the coating element measured at multiple different positions of the coated positive electrode material is m'wt%, wherein Δm=︱m-m'︱, and 0<Δm≤0.02%.
[0008] In some embodiments of the present application, the coated positive electrode material satisfies at least one of the following conditions:
[0009] (1) The coating element includes one or more of Ti, Mg, Al, Zr, Y, Mo, Nb and B;
[0010] (2) The positive electrode material includes lithium nickel cobalt manganese oxide Li w Ni 1-x-y Co x Mn y O2, 0.95≤w≤1.05, 0≤x≤1, 0≤y≤1;
[0011] (3) The average particle size of the coated positive electrode material is 2 μm to 20 μm;
[0012] (4) The average thickness of the nano-coating layer is 5 nm to 30 nm.
[0013] The second aspect of the present application provides a method for preparing a coated positive electrode material, comprising:
[0014] spraying a suspension containing a coating material to form nano-spray droplets of the coating material, and causing the nano-spray droplets to contact a rolling cathode material body and adhere to the surface of the cathode material body to obtain a crude coating product; and
[0015] The rough coating product is calcined to form a nano coating layer on the surface of the cathode material body, thereby obtaining a coated cathode material.
[0016] In some embodiments of the present application, the three-dimensional mixer satisfies at least one of the following conditions:
[0017] (1) The rolling speed is 4 rpm to 10 rpm.
[0018] (2) The mass ratio of the coating element in the coating material to the positive electrode material body is 600ppm to 3000ppm.
[0019] In some embodiments of the present application, the spray treatment satisfies at least one of the following conditions:
[0020] (1) The temperature of the spray treatment is 35°C to 65°C;
[0021] (2) The spray pressure of the spray treatment is 0.15MPa to 0.30MPa;
[0022] (3) The spray treatment is a multi-point uniform-speed spray treatment. Optionally, the spray rate of the spray treatment is 0.1 kg / min to 0.3 kg / min.
[0023] In some embodiments of the present application, the calcination process satisfies at least one of the following conditions:
[0024] (1) The calcination temperature is 250°C to 750°C;
[0025] (2) The calcination treatment time is 8h to 16h;
[0026] (3) The calcination treatment is carried out under a protective atmosphere. Optionally, the protective atmosphere includes one or more of nitrogen, argon, helium and neon.
[0027] In some embodiments of the present application, the steps of preparing the suspension containing the coating substance include:
[0028] The coating material is mixed with an organic solvent to obtain the suspension containing the coating material. Optionally, the mass ratio of the coating element in the coating material to the organic solvent is (6-12):100.
[0029] In some embodiments of the present application, the preparation method satisfies at least one of the following conditions:
[0030] (1) The coating material includes one or more oxygen-containing compounds of Ti, Mg, Al, Zr, Y, Mo, Nb and B;
[0031] (2) The organic solvent includes one or more of alcohol and amide organic solvents. Optionally, the organic solvent includes one or more of ethanol, methanol and N,N-dimethylformamide.
[0032] The third aspect of the present application provides a coating processing system for a cathode material, comprising:
[0033] A three-dimensional mixer for spraying and mixing the coating material and the cathode material body so that the coating material adheres to the surface of the cathode material body;
[0034] The pyrolysis equipment is connected to the three-dimensional mixer and is used to calcine the product after the spray mixing process to form a nano coating layer on the surface of the positive electrode material body.
[0035] In some embodiments of the present application, the coating processing system satisfies at least one of the following conditions:
[0036] (1) The three-dimensional mixer is provided with a spray channel along the central axis, and at least one spray outlet is provided on the tube wall of the spray channel;
[0037] (2) The pyrolysis equipment includes a pyrolysis furnace or a pyrolysis kiln.
[0038] The fourth aspect of the present application provides a secondary battery, comprising the coated positive electrode material described in the first aspect of the present application or the coated positive electrode material prepared by the preparation method described in the second aspect of the present application.
[0039] The fifth aspect of the present application provides an electrical device comprising the secondary battery described in the fourth aspect of the present application.
[0040] The electric device of the present application includes the secondary battery provided by the present application, and thus has at least the same advantages as the secondary battery.
[0041] The coated positive electrode material provided in the present application has a theoretical content value m wt% of the coating element contained in its nano-coating layer, and a difference Δm between the average value m'wt% of the actual content measured at multiple different positions is within the above range, which can achieve a uniform distribution of the coating element in the coated positive electrode material, so that the nano-coating layer has relatively high uniformity and continuity.
[0042] In addition, compared with conventional rough coating (dry or wet method), the preparation method provided by the present application can form nano-sized coating material spray droplets by spraying the suspension containing the coating material; at the same time, the positive electrode material body in the rolling state is also rotating at a uniform speed and continuously, so that the spray droplets can be evenly scattered and attached to the surface of the positive electrode material body, thereby greatly improving the uniformity and consistency of the coating material coated on the surface of the positive electrode material body. In addition, the positive electrode material body in the rolling state can also be rolled and mixed with the coating material, thereby effectively avoiding the problem of material adhesion and wall adhesion during the wet coating process. The preparation method provided by the present application has a simple process, a short reaction time, a continuous reaction, a large processing capacity, and a uniform distribution of coating elements, and can produce a coated positive electrode material at a lower cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] FIG1 is a comparison diagram of the laser particle size distribution of the coated lithium nickel cobalt manganese oxide of Example 1 and Comparative Example 1;
[0044] FIG2 is a schematic diagram of the overall equipment for preparing coated lithium nickel cobalt manganese oxide in the present application;
[0045] FIG3 is a SEM comparison of the coated lithium nickel cobalt manganese oxide of Example 1(a) and Comparative Example 1(b). DETAILED DESCRIPTION
[0046] To facilitate understanding of the present application, a more comprehensive description of the present application will be provided below with reference to the accompanying drawings. The accompanying drawings illustrate preferred embodiments of the present application. However, the present application may be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and comprehensive understanding of the disclosure of the present application.
[0047] For simplicity, this application only explicitly discloses certain numerical ranges. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, although not explicitly stated, each point or individual value between the endpoints of a range is included in the range. Thus, each point or individual value may serve as its own lower limit or upper limit and be combined with any other point or individual value, or with other lower limits or upper limits, to form an unspecified range.
[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. It should be noted that, unless otherwise stated, the term "and / or" used herein includes any and all combinations of one or more related listed items, and "above" and "below" are inclusive of the number, and the meaning of "a variety" in "one or more" is more than two.
[0049] The above disclosure of the present application is not intended to describe every disclosed embodiment or every implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided through a series of examples, which can be used in various combinations. In each example, the enumeration is intended only as a representative group and should not be construed as exhaustive.
[0050] The first aspect of the present application provides a coated positive electrode material, comprising a positive electrode material body and a nano-coating layer coated on the surface of the positive electrode material body, wherein the nano-coating layer contains a coating element, the theoretical content of the coating element in the coated positive electrode material is m wt%, and the average value of the actual content of the coating element measured at multiple different positions of the coated positive electrode material is m'wt%, wherein Δm=︱m-m'︱, and 0<︱Δm︱≤0.02%.
[0051] It should be noted that the theoretical content value m wt% of the coating element in the coated positive electrode material can be determined by the feeding amount; and the average value m'wt% of the actual content of the coating element measured at multiple different positions of the coated positive electrode material can be obtained by sampling and testing multiple different positions of the coated positive electrode material, measuring the actual content value of the coating element in the coated positive electrode material at each position by elemental microanalysis (such as EDS spectrometer), and taking the average value of each actual content value to obtain m'wt%.
[0052] It can be understood that the above-mentioned multiple different position points include at least three different position points.
[0053] The coated positive electrode material provided in the present application has a theoretical content value m wt% of the coating element contained in its nano-coating layer, and the absolute value Δm of the difference between the average value m'wt% of the actual content value is within the above range, which can achieve a uniform distribution of the coating element in the coated positive electrode material, so that the nano-coating layer has relatively high uniformity and continuity.
[0054] In some embodiments, the coating element includes one or more of Ti, Mg, Al, Zr, Y, Mo, Nb, and B.
[0055] In some embodiments, the cathode material comprises lithium nickel cobalt manganese oxide Li w Ni 1-x-y Co x Mn y O2, 0.95≤w≤1.05, 0≤x≤1, 0≤y≤1. It can be understood that the positive electrode material body also includes lithium nickel cobalt aluminum oxide, lithium cobalt oxide, lithium-rich manganese-based positive electrode materials, etc.
[0056] In some embodiments, the average particle size of the coated positive electrode material is 2 μm to 20 μm. For example, the average particle size can be 2 μm, 5 μm, 8 μm, 11 μm, 14 μm, 17 μm, 20 μm, or within a range consisting of any of the above values;
[0057] The average particle size of the coated positive electrode material is well known in the art and can be measured using instruments and methods known in the art. For example, it can be conveniently measured using a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd., UK, with reference to GB / T 19077-2016 Particle Size Distribution - Laser Diffraction Method.
[0058] In some embodiments, the average thickness of the nanocoating layer is 5 nm to 30 nm. For example, the average thickness of the nanocoating layer can be 5 nm, 10 nm, 15 nm, 20 nm, and 30 nm.
[0059] The average thickness of the nanocoating is determined by obtaining an equivalent thickness, directly observing the nanocoating by TEM imaging, and confirming that the order of magnitude of the equivalent thickness obtained previously is an appropriate value, wherein the equivalent thickness is obtained after taking into account the composition of the nanocoating obtained by composition analysis (TEM-EDX: transmission electron microscopy-energy dispersive X-ray spectroscopy) and the amount of elements obtained by inductively coupled plasma mass spectrometry (ICP-MS).
[0060] The second aspect of the present application provides a method for preparing a coated positive electrode material, which can be used to prepare the coated positive electrode material described in the first aspect of the present application, and may include the following steps:
[0061] S10, spraying a suspension containing a coating material to form nano-spray droplets of the coating material, causing the nano-spray droplets to contact a rolling cathode material body and adhere to the surface of the cathode material body, thereby obtaining a crude coating product;
[0062] S20, calcining the crude coating product to form a nano-coating layer on the surface of the positive electrode material body to obtain a coated positive electrode material.
[0063] Compared with conventional rough coating (dry or wet method), the preparation method provided by the present application can form nano-sized spray droplets of the coating material by spraying the suspension containing the coating material; at the same time, the positive electrode material body in the rolling state is also rotating at a uniform speed and continuously, so that the spray droplets can be evenly scattered and attached to the surface of the positive electrode material body, thereby greatly improving the uniformity and consistency of the coating material coated on the surface of the positive electrode material body. In addition, the positive electrode material body in the rolling state can also be rolled and mixed with the coating material, thereby effectively avoiding the problem of material adhesion and wall adhesion during the wet coating process. The preparation method provided by the present application has a simple process, short reaction time, continuous reaction, large processing capacity, and uniform distribution of coating elements, and can produce coated positive electrode materials at a lower cost.
[0064] The third aspect of the present application provides a coating processing system for positive electrode materials, in which the coated positive electrode material described in the first aspect of the present application can be prepared using the preparation method described in the second aspect of the present application.
[0065] In some embodiments, as shown in Figure 2, the coating treatment system includes: a three-dimensional mixer 1, which is used to spray mix the coating material and the positive electrode material body so that the coating material is attached to the surface of the positive electrode material body; a pyrolysis device 2, which is connected to the three-dimensional mixer 1 and is used to calcine the product after the spray mixing treatment to form a nano-coating layer on the surface of the positive electrode material body.
[0066] In some embodiments, the spraying treatment is performed in a three-dimensional mixer 1 , and the calcination treatment is performed in a pyrolysis device 2 .
[0067] Since the three-dimensional mixer 1 is connected to the pyrolysis equipment 2 used for calcination treatment, the crude coating product can be transferred to the pyrolysis equipment 2 after obtaining the crude coating product. That is, in the process of transferring from the mixing process to the pyrolysis process, the crude coating product does not need to come into contact with the external environment, thereby enabling the coating reaction to be carried out continuously. This can reduce the problems of pollution, loss, performance variation, etc. that may be caused by contact with the external environment when the material is transferred between discontinuous processes in the conventional rough coating method.
[0068] In some embodiments, as shown in FIG2 , the three-dimensional mixer 1 and the pyrolysis device 2 in the present application are connected and arranged, and the three-dimensional mixer 1 can roll or rotate along the central axis, and a spray channel is provided along the central axis. After the positive electrode material body is added to the three-dimensional mixer, it will rotate as the three-dimensional mixer 1 rolls; after a suspension containing the coating material is introduced into the three-dimensional mixer 1 along the spray channel, the suspension is sprayed under high pressure to form nano-spray droplets of the coating material; the nano-spray droplets then adhere to the surface of the continuously rotating positive electrode material body, and as the positive electrode material body rotates, the nano-spray droplets can be evenly scattered on its surface, thereby achieving uniform and continuous coating of its surface. Afterwards, the positive electrode material body with the nano-spray droplets evenly attached to its surface is transferred to the pyrolysis device for calcination. After calcination, a continuous and uniform coating layer is formed on the surface of the positive electrode material body, obtaining the final coated positive electrode material product. Since the three-dimensional mixer 1 is connected to the pyrolysis equipment 2, the above-mentioned overall mixing, coating and calcination processes can be carried out continuously, which can effectively reduce or avoid the problems of contamination, loss, performance variation, etc. that may be caused by contact with the external environment when the material is transferred between discontinuous processes in the conventional rough coating method.
[0069] In some embodiments, the three-dimensional mixer described in the present application can be a conventional three-dimensional mixer, which is provided with a spray channel for spray treatment along the central axis, and a plurality of spray outlets are provided on the tube wall of the high-pressure spray channel, thereby realizing multi-point uniform speed spray treatment with the spray channel as the spray point.
[0070] In some embodiments, the pyrolysis device 2 includes a pyrolysis furnace or a pyrolysis kiln.
[0071] It can be understood that the pyrolysis furnace or pyrolysis kiln described in the present application can be a conventional pyrolysis furnace or pyrolysis kiln, which is connected to the aforementioned three-dimensional mixer 1 and can achieve continuous coating treatment of the lithium positive electrode material body.
[0072] In some embodiments, the rolling speed is 4 rpm to 10 rpm. For example, the rolling speed can be 4 rpm, 5 rpm, 6 rpm, 7 rpm, 8 rpm, 9 rpm, 10 rpm, or any range thereof. The rolling speed of the three-dimensional mixer is within a suitable range, which facilitates more uniform adhesion of the nano-spray droplets of the coating material to the surface of the positive electrode material body.
[0073] In some embodiments, the mass ratio of the coating element in the coating material to the cathode material is 600 ppm to 3000 ppm. For example, the mass ratio of the coating element in the coating material to the cathode material can be 1000 ppm, 1500 ppm, 2000 ppm, 2500 ppm, or any range thereof.
[0074] It can be understood that, for example, when the coating material is Al(OH)3, it refers to the mass ratio of the coating element Al to the positive electrode material body.
[0075] It is understood that the mass ratio of the coating element in the coating material to the positive electrode material body, expressed in ppm, means that 1 mg of the coating element is contained in 1 kg of the positive electrode material body. For example, when the coating material is Al(OH)3, it means that 1 mg of the coating element Al is contained in 1 kg of the positive electrode material body.
[0076] In some embodiments, the spraying treatment is a multi-point uniform speed spraying treatment.
[0077] In some embodiments, the temperature of the spray treatment is 35° C. to 65° C. For example, the temperature of the three-dimensional mixer can be 40° C., 45° C., 50° C., 55° C., 60° C., 65° C., or any range thereof.
[0078] In some embodiments, the spray pressure of the spray treatment is 0.15 MPa to 0.30 MPa. For example, the spray pressure of the spray treatment can be 0.18 MPa, 0.21 MPa, 0.24 MPa, 0.27 MPa, or any range thereof.
[0079] Controlling the spray pressure within an appropriate range is conducive to the formation of nano-scale spray droplets from the spray material. Among them, the nano-spray droplets are more evenly combined with the material particles. After low-temperature calcination, the coating elements can be more evenly and tightly integrated with the material particles, which is more conducive to ion conduction during the charge and discharge process and improves the electrical performance of the material.
[0080] In some embodiments, the spraying rate of the spraying treatment is 0.1 kg / min to 0.3 kg / min. For example, the spraying rate can be 0.1 kg / min, 0.2 kg / min, 0.3 kg / min, or any range thereof. A spraying rate within a suitable range facilitates more uniform dispersion of the nano-spray droplets of the coating material on the surface of the cathode material body.
[0081] In some embodiments, the calcination temperature is 250° C. to 750° C. For example, the calcination temperature can be 300° C., 350° C., 400° C., 450° C., 500° C., 550° C., 600° C., 650° C., 700° C., or any range thereof.
[0082] In some embodiments, the calcination treatment time is 8 hours to 16 hours. For example, the calcination treatment time can be 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, or any range thereof.
[0083] In some embodiments, the calcination process is performed under a protective atmosphere.
[0084] In some embodiments, the protective atmosphere includes, but is not limited to, one or more of nitrogen, argon, helium, and neon.
[0085] In some embodiments of the present application, the preparation method may further include the following step S30 of preparing the suspension containing the coating substance:
[0086] S30, mixing the coating material with an organic solvent to obtain the suspension containing the coating material.
[0087] In some embodiments, the mass ratio of the coating element in the coating material to the organic solvent is (6-12): 100. For example, the mass ratio of the coating element in the coating material to the organic solvent can be 7:100, 8:100, 9:100, 10:100, 11:100, or any range thereof.
[0088] In the present application, the type of coating material is not particularly limited, and conventional coating materials in the art can be used. For example, the coating material includes one or more oxygen-containing compounds of elements such as Ti, Mg, Al, Zr, Y, Mo, Nb, and B.
[0089] It can be understood that the oxygen-containing compounds of elements such as Ti, Mg, Al, Zr, Y, Mo, Nb and B refer to compounds containing any of the above elements and oxygen at the same time.
[0090] Optionally, the coating material can be one or more acidic oxides of elements such as Ti, Mg, Al, Zr, Y, Mo, Nb and B, or one or more basic oxides of elements such as Ti, Mg, Al, Zr, Y, Mo, Nb and B.
[0091] In the present application, the type of the organic solvent is not particularly limited, and conventional organic solvents in the art can be used. For example, the organic solvent includes one or more of alcohols and amides. Alternatively, the organic solvent includes one or more of ethanol, methanol, and N,N-dimethylformamide.
[0092] In some embodiments, after obtaining the coated positive electrode material in step S30, the preparation method may further include the following step S40:
[0093] S40, the step of sieving the coated positive electrode material to obtain a finished product.
[0094] The fourth aspect of the present application provides a secondary battery, comprising the coated positive electrode material described in the first aspect of the present application or the coated positive electrode material prepared by the preparation method described in the second aspect of the present application.
[0095] In some embodiments, the secondary battery may include a lithium-ion secondary battery.
[0096] In some embodiments, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery's charge and discharge processes, active ions are intercalated and released between the positive and negative electrode sheets. The electrolyte conducts ions between the positive and negative electrode sheets. The separator, positioned between the positive and negative electrode sheets, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.
[0097] The fifth aspect of the present application provides an electric device, comprising the secondary battery described in the fourth aspect of the present application, wherein the secondary battery can be used as a power source in the electric device.
[0098] In some embodiments, the type of electrical device is not particularly limited and can be any electronic device known in the art. For example, the electronic device can include, but is not limited to, a laptop computer, a pen-type computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, an automobile, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, a power tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.
[0099] Example
[0100] The following are specific examples, which describe the present disclosure in more detail. These examples are intended for illustrative purposes only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are also commercially available.
[0101] Example 1
[0102] Dissolve 380g of Al(OH)3 powder in 1.6kg of ethanol and stir at room temperature for 30 minutes to form a suspension. Place 100kg of lithium nickel cobalt manganese oxide in a 200L three-dimensional mixer, rotate at a constant speed of 6rpm / min, maintain the mixer temperature at 45°C, and spray the Al(OH)3 suspension at multiple points at a constant speed with the central axis of the three-dimensional mixer as the spray point at a pressure of 0.2MPa and a speed of 0.16kg / min. After spraying, transfer the material to a pyrolysis equipment, set the temperature to 450°C, keep it warm for 14 hours, cool it, and pass it through a 400-mesh sieve to obtain the finished product.
[0103] Example 2
[0104] Dissolve 540g of TiOSO4 powder in 2kg of methanol and stir at room temperature for 20 minutes to form a suspension. Place 100kg of lithium nickel cobalt manganese oxide in a 200L three-dimensional mixer, rotate at a constant speed of 8rpm / min, and maintain the mixer temperature at 50°C. Spray the TiOSO4 suspension at multiple points at a constant speed, using the central axis of the three-dimensional mixer as the spray point, at a pressure of 0.25MPa and a speed of 0.2kg / min. After spraying, transfer the material to a pyrolysis device, set the temperature to 650°C, maintain the temperature for 16 hours, and then cool and pass it through a 400-mesh sieve to obtain the finished product.
[0105] Comparative Example 1
[0106] Comparative Example 1 is a conventional dry coating, which specifically includes: placing 760g Al(OH)3 powder and 200kg lithium nickel cobalt manganese oxide in a 500L high-speed mixer and mixing at 380rpm / min for 20 minutes. After mixing, the materials pass through the discharge bin and the bowl loading machine and enter the roller kiln. The constant temperature zone is kept at 450℃ for 14h, and after cooling, they are sieved through a 400-mesh sieve to obtain the finished product.
[0107] Comparative Example 2
[0108] Comparative Example 2 is a conventional dry coating method, which specifically includes: placing 1080g of TiOSO4 powder and 200kg of lithium nickel cobalt manganese oxide in a 500L high-speed mixer and mixing at 380rpm / min for 20 minutes. After mixing, the materials pass through the discharge bin and the bowl loading machine and enter the roller kiln. The constant temperature zone is kept at 650℃ for 16 hours, and after cooling, they are sieved through a 400-mesh sieve to obtain the finished product.
[0109] The coated lithium nickel cobalt manganese oxides prepared in Examples 1-2 and Comparative Examples 1-2 were subjected to relevant performance tests, and the test results are shown in Table 1 below. In addition, the coated lithium nickel cobalt manganese oxide was made into electrode samples and tested using a scanning electron microscope (SEM) and an energy dispersive spectrometer (EDS). The instruments used a focused electron beam to excite the sample surface to generate secondary electrons, backscattered electrons, and characteristic X-rays, and other secondary information. This secondary information was collected and detected for analysis of the sample surface micromorphology and micro-region composition.
[0110] Table 1
[0111] It can be seen from Table 1 above that the average value of the actual content of the multi-point detection of the coating element in the embodiment is closer to the theoretical value, indicating that compared with the traditional dry coating method, the coated lithium nickel cobalt manganese oxide prepared by the method of the present application has a more firmly bonded coating element to the material particles and is less likely to fall off during the subsequent processing steps; at the same time, it can be seen from Table 1, Figures 1 and 3 above that when the sample particle sizes in Example 1 and Comparative Example 1 are basically the same, the difference between the multi-point test data in Example 1 is smaller, indicating that its coating is more uniform.
[0112] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0113] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that a person skilled in the art could make various modifications and improvements without departing from the spirit of the present application, all of which fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.
Claims
1. A coated positive electrode material, characterized in that: include: Positive electrode material body; and A nano coating layer is coated on the surface of the positive electrode material body, wherein the nano coating layer contains a coating element, wherein the theoretical content of the coating element in the coated positive electrode material is m wt%, and the average value of the actual content of the coating element measured at multiple different positions of the coated positive electrode material is m'wt%, wherein Δm=︱m-m'︱, and 0<Δm≤0.02%.
2. The coated positive electrode material according to claim 1, characterized in that: Satisfy at least one of the following conditions: (1) The coating element includes one or more of Ti, Mg, Al, Zr, Y, Mo, Nb and B; (2) The positive electrode material body includes lithium nickel cobalt manganese oxide Li w Ni 1-x-y Co x Mn y O2, 0.95≤w≤1.05, 0≤x≤1, 0≤y≤1; (3) The average particle size of the coated positive electrode material is 2 μm to 20 μm; (4) The average thickness of the nano-coating layer is 5 nm to 30 nm.
3. A method for preparing a coated positive electrode material according to claim 1 or 2, characterized in that: include: A suspension containing a coating material is sprayed to form nano-spray droplets of the coating material, and the nano-spray droplets are brought into contact with a rolling cathode material body and attached to a surface of the cathode material body to obtain a crude coating product; and The rough coating product is calcined to form a nano coating layer on the surface of the positive electrode material body to obtain a coated positive electrode material.
4. The preparation method according to claim 3, characterized in that: The preparation method satisfies at least one of the following conditions: (1) The rolling speed is 4 rpm to 10 rpm; (2) The mass ratio of the coating element in the coating material to the positive electrode material body is 600ppm to 3000ppm.
5. The preparation method according to claim 3 or 4, characterized in that: The spray treatment satisfies at least one of the following conditions: (1) The temperature of the spray treatment is 35°C to 65°C; (2) The spray pressure of the spray treatment is 0.15MPa to 0.30MPa; (3) The spray treatment is a multi-point uniform speed spray treatment, Optionally, the spraying rate of the spraying treatment is 0.1 kg / min to 0.3 kg / min.
6. The preparation method according to claim 3 or 4, characterized in that: The calcination treatment satisfies at least one of the following conditions: (1) The calcination temperature is 250°C to 750°C; (2) The calcination time is 8 hours to 16 hours; (3) The calcination treatment is carried out under a protective atmosphere. Optionally, the protective atmosphere includes one or more of nitrogen, argon, helium and neon.
7. The preparation method according to claim 3 or 4, characterized in that: The preparation steps of the suspension containing the coated substance include: The coating material is mixed with an organic solvent to obtain a suspension containing the coating material, Optionally, the mass ratio of the coating element in the coating material to the organic solvent is (6-12):
100.
8. The preparation method according to claim 7, characterized in that: Satisfy at least one of the following conditions: (1) The coating material includes one or more oxygen-containing compounds of Ti, Mg, Al, Zr, Y, Mo, Nb and B; (2) The organic solvent includes one or more of alcohol and amide organic solvents. Optionally, the organic solvent includes one or more of ethanol, methanol and N,N-dimethylformamide.
9. A coating processing system for positive electrode materials, characterized in that: include: A three-dimensional mixer, used for spraying and mixing the coating material and the cathode material body, so that the coating material is attached to the surface of the cathode material body; The pyrolysis equipment is connected to the three-dimensional mixer and is used to calcine the product after the spray mixing treatment to form a nano coating layer on the surface of the positive electrode material body.
10. The coating processing system according to claim 9, characterized in that: Satisfy at least one of the following conditions: (1) The three-dimensional mixer is provided with a spray channel along the central axis, and at least one spray outlet is provided on the tube wall of the spray channel; (2) The pyrolysis equipment includes a pyrolysis furnace or a pyrolysis kiln.
11. A secondary battery, characterized in that: It includes the coated positive electrode material according to claim 1 or 2, or the coated positive electrode material prepared by the preparation method according to any one of claims 3 to 8, or the coated positive electrode material prepared by the coating processing system according to claim 9 or 10.
Citation Information
Patent Citations
Coated positive electrode material and preparation method thereof, coating treatment system of positive electrode material and secondary battery
CN116487565A
Positive active material, positive electrode, lithium battery including the same, and method of manufacturing thereof
US20150228973A1
Positive active material, positive electrode, and lithium battery including the same and method of manufacture thereof
US20150243970A1
Positive electrode active material
US20210288307A1
Material mixing process for preparing high-nickel positive electrode material and use thereof
WO2022206065A1