Preparation method for high-performance rutile-type titanium dioxide by means of sulfuric acid method
Through multi-layer coating technology and organic treatment, the dispersion and weatherability of rutile titanium dioxide of sulfuric acid method are improved, and the problem of insufficient performance in coatings is solved by the sulfuric acid method, and the improvement of gloss, brightness and comprehensive performance is achieved.
Patent Information
- Application Number
- PCT/CN2023/120622
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-27
- Filing Date
- 2023-09-22
- Publication Date
- 2024-12-05
AI Technical Summary
The rutile titanium dioxide prepared by the sulfuric acid method is insufficient in the coating, making it difficult to meet the high requirements for comprehensive performance of green and environmentally friendly coatings.
Using multiple layers of envelope technology with different density, through the gradual addition of silicon, zirconium and aluminum envelope agents and controlling the pH value, dense silicon oxide, zirconium oxide and alumina layers are formed, combined with organic envelope treatment to improve the titanium dioxide. Dispersibility and weather resistance.
It significantly improves the dispersion and weather resistance of titanium dioxide, enhances gloss and brightness, expands product application performance, and is suitable for high-performance coatings.
Smart Images

Figure PCTCN2023120622-FTAPPB-I100001 
Figure PCTCN2023120622-FTAPPB-I100002
Abstract
Description
A method for preparing high-performance sulfuric acid-processed rutile titanium dioxide Technical Field
[0001] The present application relates to the technical field of titanium dioxide preparation, and more specifically, to a method for preparing high-performance sulfuric acid-processed rutile titanium dioxide. Background Art
[0002] Titanium dioxide, also known as titanium dioxide, is a pigment with excellent optical properties, stable chemical properties, a high refractive index, and good hiding power. It is widely used in coatings, plastics, papermaking, inks, and other fields. The coatings industry is the largest consumer of titanium dioxide pigments. With technological breakthroughs and the application of green and environmentally friendly coatings, this market is driving further and more stable growth, thus placing higher demands on the comprehensive performance of titanium dioxide.
[0003] The main production methods of titanium dioxide in China are sulfuric acid method and chlorination method. Among them, the output of titanium dioxide produced by sulfuric acid method can account for 90% of the total. Although the proportion is high, its comprehensive performance is still somewhat lower than that of titanium dioxide produced by chloride method. In order to improve the performance of titanium dioxide produced by sulfuric acid method, a common method is to coat and modify the surface of titanium dioxide.
[0004] The specific steps of coating modification are: beating the primary titanium dioxide, inorganic coating, organic coating, filtering and washing, drying, and pulverizing. Common coating agents used in inorganic coating modification include aluminum, silicon, and zirconium salts. Titanium dioxide is mainly categorized by coating type into silicon-aluminum double-layer coating and zirconium-aluminum double-layer coating.
[0005] The above two titanium dioxides have excellent performance in terms of brightness, hue, and relative hiding power, but their dispersibility and weather resistance in coatings are insufficient. Therefore, it is of great significance to prepare a titanium dioxide with better dispersibility and weather resistance.
[0006] Summary of the Invention
[0007] In order to improve the weather resistance and dispersibility of sulfuric acid process rutile titanium dioxide, the present application provides a method for preparing high-performance sulfuric acid process rutile titanium dioxide.
[0008] The present application provides a method for preparing high-performance rutile titanium dioxide produced by the sulfate process, which adopts the following technical solution: a method for preparing high-performance rutile titanium dioxide produced by the sulfate process, comprising subjecting a primary product of rutile titanium dioxide produced by the sulfate process to pulping, inorganic coating, filtering and washing, drying, air flow pulverization, and organic coating;
[0009] The inorganic coating comprises the following steps:
[0010] S1. Add a silicon coating agent to the slurry obtained by beating, wherein the amount of the silicon coating agent added is 1.0-1.4% of the weight of the TiO2 in terms of SiO2, and add an inorganic acid to adjust the pH to 6.2-7.2, and mature to form a silicon oxide layer;
[0011] S2, adding a zirconium coating agent, the amount of which is 0.35-0.5% of the weight of TiO2 as ZrO2, adding an inorganic base to adjust the pH to 8.2-9.0, and aging to form a zirconium oxide layer;
[0012] S3, adding aluminum coating agent A, the amount of which is 1.2-1.4% of the weight of TiO2 calculated as Al2O3, adding sulfate to adjust the pH to 8.0-8.5, and aging to form a first aluminum oxide layer;
[0013] S4. Add aluminum coating agent B, the amount of which is 0.9-1.2% of the weight of TiO2 in terms of Al2O3, add inorganic acid to adjust the pH to 6.8-7.1, and mature to form a second aluminum oxide layer.
[0014] By adopting the above technical solution, during the coating process, the amount of coating agent is controlled to provide a basis for forming films with different sparseness and density; the pH is controlled to control the hydrolysis rate of the coating agent, thereby forming micelles of different sizes; under the cooperation of the above two conditions, a dense silicon oxide layer, a dense zirconium oxide layer, a dense first aluminum oxide layer and a sparse second aluminum oxide layer are formed.
[0015] The dense silicon oxide layer improves titanium dioxide's weather resistance, the dense zirconium oxide layer enhances both weather resistance and gloss, and the dense first aluminum oxide layer further enhances both weather resistance and brightness. The outermost layer, a sparse second aluminum oxide layer, not only improves titanium dioxide's dispersion but also facilitates subsequent washing and filtration of the slurry. Titanium dioxide coated with four layers of varying densities exhibits enhanced weather resistance and dispersibility, along with excellent gloss and brightness, making it ideal for use in coatings.
[0016] Optionally, the specific steps in S1 are: heating the pulped slurry to 75-85° C., adding a silicon coating agent, slowly adding an inorganic acid within 150-200 minutes to adjust the pH to 6.2-7.2, and aging for 60-80 minutes to obtain the product.
[0017] By adopting the above technical solution, the slurry temperature is controlled to improve the coating effect, and the local H + concentration, slowing down the formation rate of silicic acid, avoiding the nucleation coating caused by the natural nucleation of silicic acid, improving the effect of the formed dense film, and improving the weather resistance of titanium dioxide.
[0018] Optionally, the silicon coating agent is a sodium silicate aqueous solution with a concentration of 150-220 g / L calculated as SiO2.
[0019] Optionally, the specific steps in S2 are: cooling the slurry obtained after aging in S2 to 55-65° C., slowly adding a zirconium coating agent within 90-120 minutes, and simultaneously adding an inorganic base to adjust the pH to 8.2-9.0, and aging for 50-80 minutes to obtain the product.
[0020] By adopting the above technical solution and controlling the reaction conditions within the above range, the coating effect is improved, and the zirconium coating agent and inorganic base are added in parallel to form a dense zirconium oxide layer, thereby improving the weather resistance and glossiness of titanium dioxide.
[0021] Optionally, the zirconium coating agent is an aqueous solution of zirconium sulfate, with a concentration of 150-200 g / L calculated as ZrO2.
[0022] Optionally, the specific steps of S3 are: maintaining the temperature of the slurry after aging in S2, adding aluminum coating agent A within 50-70 minutes, and adding sulfate solution to adjust the pH to 8.0-8.5, and aging for 20-40 minutes.
[0023] Optionally, the aluminum coating agent A is a sodium metaaluminate aqueous solution or a potassium aluminate solution, and its concentration is 160-200 g / L in terms of Al2O3.
[0024] Optionally, the sulfate solution is an aqueous solution of aluminum sulfate, and its concentration is 80-120 g / L in terms of Al2O3.
[0025] Optionally, the specific steps of S4 are: maintaining the temperature of the slurry after aging in S3, adding aluminum coating agent B within 30-40 minutes, and adding inorganic acid to adjust the pH to 6.8-7.1, and aging for 80-100 minutes.
[0026] By adopting the above technical solution, the following conditions before and after the reaction of the aluminum coating agent A are preferably controlled: 1) slurry temperature; 2) the method of adding the aluminum coating agent A and the inorganic acid in parallel within the above time range; 3) aging time; so as to polymerize and form a looser aluminum oxide film, thereby improving the dispersibility of titanium dioxide.
[0027] Optionally, the aluminum coating agent B is a sodium metaaluminate aqueous solution or a potassium aluminate solution, and its concentration is 160-200 g / L in terms of Al2O3.
[0028] In summary, this application has the following beneficial effects:
[0029] 1. This application coats rutile titanium dioxide with multiple layers of films made of different materials and densities, so that the titanium dioxide fully takes into account comprehensive performance indicators such as hue, hiding power, gloss, dispersion and weather resistance, and expands the product's application performance and scope for better application in coatings;
[0030] 2. In this application, the following conditions are preferred before and after each reaction: 1) slurry temperature; 2) method of adding coating agent; 3) aging time; so as to form different sparse and dense film layers through polymerization to enhance the performance of titanium dioxide. DETAILED DESCRIPTION
[0031] The present application is further described in detail below with reference to the embodiments.
[0032] Example
[0033] Example 1
[0034] A method for preparing high-performance rutile titanium dioxide using the sulfuric acid method, comprising the following steps:
[0035] 1) Beating: grind the sulfuric acid process rutile titanium dioxide primary product, pass it through a 325 mesh sieve, mix 10 kg of the sieved titanium dioxide primary product with desalted water (salt content of 3 mg / L) and beat it to prepare a slurry with a concentration of 25 wt%, add a sodium hydroxide aqueous solution (concentration of 15 wt%) to adjust the pH to 10, and then add a sodium silicate aqueous solution (concentration of 160 g / L in terms of SiO2) and disperse it for 30 minutes. The amount of sodium silicate added is 0.35% of the amount of TiO2 in terms of SiO2; wet grinding and dispersion, cyclone classification to remove particles with a particle size of more than 10 μm, use a particle size analyzer to detect the particle size range, and select the primary product to be coated with a particle size of 0.26-0.30 μm as the slurry;
[0036] [It should be noted that the pH adjusted by adding sodium hydroxide aqueous solution can be selected within the range of 9.1-11. The above selection does not have a significant impact on the test results. In the examples of this application, only pH 10 is used as an example for brief description.]
[0037] 2) Inorganic coating, the specific steps are as follows:
[0038] S1. After setting the coating tank temperature to 75°C and the agitator speed to 46 r / min, add the slurry and the silicon coating agent (sodium silicate aqueous solution, the concentration is 150 g / L in terms of SiO2), the amount of sodium silicate aqueous solution added is 1.0% of the weight of TiO2 in terms of SiO2, slowly add inorganic acid (10 wt% sulfuric acid solution) over 180 min to adjust the pH to 6.8, and mature for 70 min to form a dense silicon oxide film;
[0039] [In other embodiments, the inorganic acid solution is selected from sulfuric acid, hydrochloric acid, and phosphoric acid.]
[0040] S2. Cool the slurry after aging in step S1 to 60° C., adjust the stirrer speed to 75 r / min, and slowly add a zirconium coating agent (aqueous solution of zirconium sulfate, with a concentration of 150 g / L calculated as ZrO2) over 105 minutes. The amount of the aqueous solution of zirconium sulfate added is 0.35% of the weight of the TiO2 calculated as ZrO2. Simultaneously, add an inorganic base (aqueous solution of sodium hydroxide with a concentration of 20 wt%) to adjust the slurry pH to 8.2. Aqueous solution is aging for 65 minutes to form a dense zirconium oxide film.
[0041] [In other embodiments, the solute in the inorganic alkaline solution can be selected from sodium hydroxide, potassium hydroxide, and sodium carbonate.]
[0042] S3. Maintaining the temperature of the slurry after aging in S2, slowly add aluminum coating agent A (sodium metaaluminate aqueous solution, with a concentration of 160 g / L calculated as Al2O3) over 60 minutes, with the amount of sodium metaaluminate aqueous solution added accounting for 1.2% of the weight of TiO2 calculated as Al2O3. Simultaneously, add sulfate solution (aluminum sulfate aqueous solution, with a concentration of 80 g / L calculated as Al2O3) and adjust the slurry pH to 8.0. Agitation is carried out for 30 minutes to form a dense first aluminum oxide film.
[0043] S4. Maintaining the temperature of the slurry after aging in S3, an aluminum coating agent B (aqueous solution of sodium metaaluminate, with a concentration of 160 g / L calculated as Al2O3) is added within 35 minutes. The amount of aluminum coating agent B added is 0.9% of the weight of TiO2 calculated as Al2O3. Simultaneously, an inorganic acid (a sulfuric acid solution with a concentration of 15 wt%) is added to adjust the slurry pH to 6.8. The slurry is aged for 90 minutes to form a sparse second aluminum oxide film.
[0044] 3) The slurry after aging in step S4 is filtered and washed with desalted water until the filter cake resistivity reaches 200 Ω·m, dehydrated, dried, and then pulverized using a jet mill to control the particle size to 0.15-0.3 μm;
[0045] 4) Organic coating treatment: adding an organic coating agent (trimethylolpropane, trimethylolethane), the amount of the organic coating agent added is 0.25% of the weight of TiO2, wherein the weight ratio of trimethylolpropane to trimethylolethane is 1:1;
[0046] 5) Discharge the material and cool it to 25°C to obtain high-performance sulfuric acid process rutile titanium dioxide.
[0047] [It should be noted that, after washing the filter cake with desalted water in step 3), the resistivity of the filter cake can be selected within the range of 180-230 Ω·m. The above selection does not significantly affect the test results. In the embodiment of this application, only 200 Ω·m is briefly introduced as an example;
[0048] In step 4), the organic coating agent can be selected from isopropanolamine, triethanolamine, polyols, and silicones. This selection does not significantly affect the test results. In this embodiment, trimethylolpropane (polyol) and trimethylolethane (polyol) are briefly described as examples. Similarly, the amount of the organic coating agent added can be selected within the range of 0.25%-0.4% by weight of the TiO2. In this embodiment, only 0.25% is used as an example for brief description. The weight ratio of trimethylolpropane to trimethylolethane can be adjusted as needed. In this embodiment, only 1:1 is used as an example for brief description.
[0049] Example 2
[0050] A method for preparing high-performance rutile titanium dioxide using the sulfuric acid method is different from Example 1 in that the specific steps of the inorganic coating are as follows:
[0051] S1. After setting the coating tank temperature to 75°C and the agitator speed to 46 r / min, add the slurry and the silicon coating agent (sodium silicate aqueous solution, the concentration is 180 g / L in terms of SiO2), the amount of sodium silicate aqueous solution added is 1.2% of the weight of TiO2 in terms of SiO2, slowly add inorganic acid (10 wt% sulfuric acid solution) over 180 min to adjust the pH to 6.8, and mature for 70 min to form a dense silicon oxide film;
[0052] S2. Cool the slurry after aging in step S1 to 60° C., adjust the stirrer speed to 75 r / min, and slowly add a zirconium coating agent (aqueous solution of zirconium sulfate, with a concentration of 170 g / L calculated as ZrO2) over 105 minutes. The amount of the aqueous solution of zirconium sulfate added is 0.45% of the weight of TiO2 calculated as ZrO2. Simultaneously, add an inorganic base (aqueous solution of sodium hydroxide with a concentration of 20 wt%) to adjust the pH of the slurry to 8.6. The mixture is aged for 65 minutes to form a dense zirconium oxide film.
[0053] S3. Maintaining the temperature of the slurry after aging in S2, slowly add aluminum coating agent A (sodium metaaluminate aqueous solution, with a concentration of 180 g / L calculated as Al2O3) over 60 minutes, with the amount of sodium metaaluminate aqueous solution added accounting for 1.3% of the weight of TiO2 calculated as Al2O3. Simultaneously, add sulfate solution (aluminum sulfate aqueous solution, with a concentration of 100 g / L calculated as Al2O3) and adjust the slurry pH to 8.3. Agitation is carried out for 30 minutes to form a dense first aluminum oxide film.
[0054] S4. Maintain the temperature of the slurry after aging in S3, add aluminum coating agent B (sodium aluminate aqueous solution, concentration is 180g / L in terms of Al2O3) within 35 minutes, the amount of aluminum coating agent B added is 1.05% of the weight of TiO2 in terms of Al2O3, and at the same time add inorganic acid (sulfuric acid solution with a concentration of 15wt%) to adjust the slurry pH to 7.0, and mature for 90 minutes to form a sparse second aluminum oxide film.
[0055] Example 3
[0056] A method for preparing high-performance rutile titanium dioxide using the sulfuric acid method is different from Example 1 in that the specific steps of the inorganic coating are as follows:
[0057] S1. After setting the coating tank temperature to 75°C and the agitator speed to 46 r / min, add the slurry and the silicon coating agent (sodium silicate aqueous solution, the concentration is 220 g / L in terms of SiO2), the amount of sodium silicate aqueous solution added is 1.4% of the weight of TiO2 in terms of SiO2, slowly add inorganic acid (10 wt% sulfuric acid solution) over 180 min to adjust the pH to 7.2, and mature for 70 min to form a dense silicon oxide film;
[0058] S2. Cool the slurry after aging in step S1 to 60° C., adjust the stirrer speed to 75 r / min, and slowly add a zirconium coating agent (aqueous zirconium sulfate solution with a concentration of 200 g / L calculated as ZrO2) over 105 minutes. The amount of the aqueous zirconium sulfate solution added is 0.5% of the weight of the TiO2 calculated as ZrO2. Simultaneously, add an inorganic base (aqueous sodium hydroxide solution with a concentration of 20 wt %) to adjust the slurry pH to 9.0. The mixture is aged for 65 minutes to form a dense zirconium oxide film.
[0059] S3. Maintaining the temperature of the slurry after aging in S2, slowly add aluminum coating agent A (sodium metaaluminate aqueous solution, with a concentration of 200 g / L calculated as Al2O3) over 60 minutes, with the amount of sodium metaaluminate aqueous solution added accounting for 1.4% of the weight of TiO2 calculated as Al2O3. Simultaneously, add sulfate solution (aluminum sulfate aqueous solution, with a concentration of 120 g / L calculated as Al2O3) and adjust the slurry pH to 8.5. Agitation is carried out for 30 minutes to form a dense first aluminum oxide film.
[0060] S4. Maintain the temperature of the slurry after aging in S3, add aluminum coating agent B (sodium aluminate aqueous solution, with a concentration of 200 g / L in terms of Al2O3) within 35 minutes, and the amount of aluminum coating agent B added is 1.2% of the weight of TiO2 in terms of Al2O3. At the same time, add inorganic acid (sulfuric acid solution with a concentration of 15wt%) to adjust the slurry pH to 7.1, and age for 90 minutes to form a sparse second aluminum oxide film.
[0061] Comparative Example 1
[0062] A method for preparing rutile titanium dioxide using a sulfuric acid method, which differs from Example 1 in that the specific steps of the inorganic coating are as follows:
[0063] S1. After setting the coating tank temperature to 70°C and the stirrer speed to 46 r / min, add slurry and sodium silicate aqueous solution, the concentration of which is 120 g / L in terms of SiO2 and the amount added is 1.0% by weight of TiO2 in terms of SiO2, slowly add 10 wt% sulfuric acid solution over 100 min to adjust the pH to 6.2, and mature for 50 min to form a silicon oxide film;
[0064] S2. Maintain the temperature of the slurry after aging in S1, slowly add an aqueous solution of sodium aluminate (concentration of 140 g / L in terms of Al2O3, and an amount of 2.1% of the weight of TiO2 in terms of Al2O3) within 65 minutes, and simultaneously add an aqueous solution of aluminum sulfate (concentration of 60 g / L in terms of Al2O3), adjust the pH of the slurry to 6.8, and age for 75 minutes to form an alumina film.
[0065] Comparative Example 2
[0066] A method for preparing rutile titanium dioxide using a sulfuric acid method, which differs from Example 1 in that the specific steps of the inorganic coating are as follows:
[0067] S1. After setting the coating tank temperature to 70°C and the stirrer speed to 46 r / min, a zirconium coating agent (aqueous zirconium sulfate solution with a concentration of 130 g / L as ZrO2) was slowly added over 80 min. The amount of the aqueous zirconium sulfate solution added was 0.35% of the weight of the TiO2 as ZrO2. An inorganic base (aqueous sodium hydroxide solution with a concentration of 20 wt %) was simultaneously added to adjust the slurry pH to 8.2. The mixture was aged for 40 min to form a dense zirconium oxide film.
[0068] S2. Maintaining the temperature of the slurry after aging in S1, slowly add aluminum coating agent A (sodium metaaluminate aqueous solution, with a concentration of 140 g / L calculated as Al2O3) over 40 minutes, with the amount of sodium metaaluminate aqueous solution added accounting for 1.2% of the weight of TiO2 calculated as Al2O3. Simultaneously, add sulfate solution (aluminum sulfate aqueous solution, with a concentration of 60 g / L calculated as Al2O3) and adjust the slurry pH to 8.0. Agitation is carried out for 15 minutes to form a dense first aluminum oxide film.
[0069] S3. Maintain the temperature of the slurry after aging in S2, add aluminum coating agent B (sodium aluminate aqueous solution, concentration is 140g / L in terms of Al2O3) within 25 minutes, the amount of aluminum coating agent B added is 0.9% of the weight of TiO2 in terms of Al2O3, and at the same time add inorganic acid (sulfuric acid solution with a concentration of 15wt%) to adjust the slurry pH to 6.8, and age for 60 minutes to form a sparse second aluminum oxide film.
[0070] Comparative Example 3
[0071] A sulfuric acid method rutile titanium dioxide, branded by Anhui Anada Titanium Co., Ltd., model ATR312 (Note: This product has been coated with silicon and aluminum and organically treated).
[0072] Comparative Example 4
[0073] A sulfuric acid-processed rutile titanium dioxide, branded by Panzhihua Iron and Steel Group Titanium Co., Ltd., model R298 (Note: this product has been coated with zirconium and aluminum and organically treated).
[0074] Performance testing
[0075] Test products: 1) sulfuric acid method rutile titanium dioxide prepared in the examples and comparative examples; 2) sample A; 3) sample B; Preparation of sample A and sample B: The sulfuric acid method rutile titanium dioxide prepared in the examples and comparative examples, two equal portions of each titanium dioxide, each 10 kg, were added to 90 kg of water-based acrylic paint (from Changzhou Kuncai Chemical Co., Ltd., model KC10-08) and 90 kg of oil-based alkyd paint (from Zhengzhou Qingteng Paint Co., Ltd., model CS-01), respectively, to prepare sample A and sample B, and the following performance tests were performed. The test results are recorded in the table below.
[0076] Detection method
[0077] 1. Brightness, hue, and relative hiding power: Samples A and B were coated on tinplate (0.23 μm thick), dried at 180°C for 15 min, and then tested using a spectrophotometer.
[0078] 2. Dispersibility: Stir sample A at 2500 r / min for 1 min and shake sample B at 23°C for 30 min, then use a scraper fineness meter to test. The smaller the count, the better the dispersibility.
[0079] 3. Weather resistance: Add 1g titanium dioxide to 10mL concentrated sulfuric acid, stir until mixed, place in a constant temperature oil bath at 175℃ for 1h, add crushed ice, add distilled water to 100mL, stir until mixed, filter to remove the filter residue, add 2mL hydrogen peroxide to 10mL of the filtrate, add distilled water to 100mL, shake well, let stand at 25℃ for 5min, and detect the absorbance value. A small value indicates high weather resistance.
[0080] Table Performance Test Results
[0081] As can be seen from the table, the sulfuric acid process rutile titanium dioxide prepared in this application has better brightness, b value, relative hiding power, dispersibility and weather resistance than the existing titanium dioxide; this shows that by coating four layers of film with different densities and different properties, the performance of the sulfuric acid process rutile titanium dioxide prepared is better and can be better used in coatings.
[0082] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed, but as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A method for preparing high-performance sulfuric acid-processed rutile titanium dioxide, It is characterized in that The method includes pulping, inorganic coating, filtering and washing, drying, air flow pulverizing and organic coating treatment of the initial product of rutile titanium dioxide produced by the sulfuric acid process; Wherein, the inorganic coating comprises the following steps: S1. Add silicon coating agent to the pulp obtained by beating, and the amount added is SiO 2 TiO 2 1.0-1.4% by weight, adding inorganic acid to adjust the pH to 6.2-7.2, aging to form a silicon oxide layer; S2, add zirconium coating agent, the amount of which is ZrO 2 TiO 2 0.35-0.5% by weight, adding inorganic base to adjust the pH to 8.2-9.0, aging to form a zirconium oxide layer; S3, add aluminum coating agent A, the amount of which is Al 2 O 3 TiO 2 1.2-1.4% by weight, adding sulfate to adjust the pH to 8.0-8.5, aging to form a first aluminum oxide layer; S4, add aluminum coating agent B, the amount of which is Al 2 O 3 TiO 2 0.9-1.2% by weight, adding inorganic acid to adjust the pH to 6.8-7.1, aging, to form a second aluminum oxide layer.
2. The method for preparing high-performance sulfuric acid-processed rutile titanium dioxide according to claim 1, It is characterized in that The specific steps in S1 are: heating the pulped slurry to 75-85° C., adding a silicon coating agent, slowly adding an inorganic acid within 150-200 min to adjust the pH to 6.2-7.2, and aging for 60-80 min to obtain the product.
3. The method for preparing high-performance sulfuric acid-processed rutile titanium dioxide according to claim 2, Features: The silicon coating agent is a sodium silicate aqueous solution with a concentration of SiO 2 Calculated as 150-220g / L.
4. The method for preparing high-performance sulfuric acid-processed rutile titanium dioxide according to claim 1, It is characterized in that The specific steps in S2 are: cooling the slurry obtained after aging in S2 to 55-65° C., slowly adding a zirconium coating agent within 90-120 min, and adding an inorganic base to adjust the pH to 8.2-9.0, and aging for 50-80 min to obtain the product.
5. The method for preparing high-performance sulfuric acid-processed rutile titanium dioxide according to claim 4, Features: The zirconium coating agent is a zirconium sulfate aqueous solution with a concentration of ZrO 2 It is calculated as 150-200g / L.
6. The method for preparing high-performance sulfuric acid-processed rutile titanium dioxide according to claim 1, It is characterized in that The specific steps of S3 are: maintaining the temperature of the slurry after aging in S2, adding aluminum coating agent A within 50-70 minutes, and adding sulfate solution to adjust the pH to 8.0-8.5, and aging for 20-40 minutes to obtain the product.
7. The method for preparing high-performance sulfuric acid-processed rutile titanium dioxide according to claim 6, Features: The aluminum coating agent A is a sodium aluminate aqueous solution or a potassium aluminate solution, and its concentration is Al 2 O 3 It is calculated to be 160-200g / L.
8. The method for preparing high-performance sulfuric acid-processed rutile titanium dioxide according to claim 6, Features: The sulfate solution is an aqueous solution of aluminum sulfate, and its concentration is Al 2 O 3 80-120g / L.
9. The method for preparing high-performance sulfuric acid-processed rutile titanium dioxide according to claim 1, It is characterized in that The specific steps of S4 are: maintaining the temperature of the slurry after aging in S3, adding aluminum coating agent B within 30-40 minutes, and adding inorganic acid to adjust the pH to 6.8-7.1, and aging for 80-100 minutes to obtain the product.
10. The method for preparing high-performance sulfuric acid-processed rutile titanium dioxide according to claim 9, Features: The aluminum coating agent B is a sodium aluminate aqueous solution or a potassium aluminate solution, and its concentration is Al 2 O 3 It is calculated to be 160-200g / L.
Citation Information
Patent Citations
Preparation method of titanium dioxide pigment special for coating with high weather resistance
CN109266049A
Preparation method of chlorination-process titanium dioxide silicon-zirconium-aluminium ternary coating
CN109321002A
Preparation method of special titanium dioxide for outdoor building coating
CN114149698A
Preparation method of high-performance rutile type titanium dioxide by sulfuric acid method
CN116715981A
Rutile-type titanium dioxide particle and its production
JP1997202620A