Coating composition for separator membrane, composite separator membrane, battery cell, battery, and electrical appliance
By using a combination coating of porous phenolic resin microspheres and binder on the lithium battery isolation film, the problem of insufficient heat resistance of the isolation film is solved, the safety and energy density of the battery are improved, and good thermal stability is achieved and ion transport performance.
Patent Information
- Application Number
- PCT/CN2023/124153
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2023-10-12
- Publication Date
- 2024-12-05
AI Technical Summary
The existing lithium battery isolation film has poor heat resistance, resulting in a reduced battery safety, and the traditional heat-resistant coating will affect the breathability of the isolation film and the energy density of the battery.
Using a combination of porous phenolic resin microspheres and binder as the coating, the coating is prepared on the surface of the base film to improve the heat resistance and breathability of the isolation film, reduce the heat shrinkage rate of the base film, and enhance the safety of the battery. and capacity retention rate.
It significantly improves the thermal safety performance and energy density of the battery, ensuring the stability and ion transport performance of the battery under high temperature conditions.
Smart Images

Figure CN2023124153_05122024_PF_FP_ABST
Abstract
Description
Coating composition for separator, composite separator, battery cell, battery and electrical equipment
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310610594.7, filed on May 29, 2023, entitled “Coating composition for isolation membrane, composite isolation membrane, battery cell, battery and electrical equipment,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the technical field of lithium batteries, and in particular to a coating composition for an isolation membrane, a composite isolation membrane, a battery cell, a battery, and an electrical device. Background Art
[0004] Battery cells are widely used due to their reliable performance, pollution-free operation, and zero memory effect. For example, with increasing attention paid to environmental protection and the growing popularity of new energy vehicles, the demand for power battery cells is expected to experience explosive growth.
[0005] As battery applications become increasingly widespread, the requirements for battery safety are becoming increasingly stringent. However, the heat resistance of the separator in the battery cell is poor, resulting in poor safety. Therefore, the heat resistance of the separator needs to be improved.
[0006] Summary of the Invention
[0007] The present application provides a coating composition for an isolation membrane, a composite isolation membrane, a battery cell, a battery, and an electrical device, which can improve the heat resistance of the isolation membrane.
[0008] In a first aspect, the present application provides a coating composition for an isolation membrane, comprising: porous phenolic resin microspheres and a binder, wherein the mass ratio of the binder to the porous phenolic resin microspheres is 1:1 to 1:20.
[0009] According to the present application, a coating composition can be used to prepare a coating on the surface of a base film to obtain a composite separator. The coating composition mainly uses porous phenolic resin microspheres as a skeleton, has good heat resistance, and can effectively reduce the thermal shrinkage of the base film. Therefore, when used in batteries, it can prevent short circuits caused by contact between the positive and negative electrodes due to shrinkage of the separator under high temperature conditions, thereby improving the safety of the battery cells. In addition, its unique porous structure has no significant effect on the permeability of the base film compared to general coatings. The resulting composite separator has good ionic conductivity, which allows the battery cells to have a high capacity retention rate while maintaining good safety.
[0010] In some embodiments, the binder includes at least one of polyacrylic acid, polyacrylate, polyvinylidene fluoride, styrene-butadiene rubber, and sodium carboxymethyl cellulose. These binders can be used to stably bond the porous phenolic resin microspheres to the surface of the base film, thereby improving the stability of the composite separator and further enhancing its heat resistance.
[0011] In some embodiments, the porous phenolic resin microspheres meet at least one of the following conditions: 1) the Dv50 particle size of the porous phenolic resin microspheres is 0.1 μm to 5 μm; 2) the average pore size of the porous phenolic resin microspheres is 10 nm to 50 nm; 3) the specific surface area of the porous phenolic resin microspheres is 15 m 2 / g to 280m 2 / g; 4) the total pore volume of the porous phenolic resin microspheres is 0.700 cm 3 / g to 1.680cm 3 The composite separator obtained in this case has better heat resistance or air permeability, which is more conducive to improving the safety and capacity retention rate of the battery monomer using the composite separator.
[0012] In some embodiments, the porous phenolic resin microspheres meet at least one of the following conditions: 1) the Dv50 particle size of the porous phenolic resin microspheres is 0.12 μm to 2 μm; 2) the average pore size of the porous phenolic resin microspheres is 15 nm to 40 nm; 3) the specific surface area of the porous phenolic resin microspheres is 60 m 2 / g to 265m 2 / g; 4) the total pore volume of the porous phenolic resin microspheres is 0.910cm 3 / g to 1.560cm 3 The composite separator obtained in this case has better heat resistance or air permeability, which is more conducive to improving the safety and capacity retention rate of the battery monomer using the composite separator.
[0013] In some embodiments, the porous phenolic resin microspheres are obtained by reacting a phenolic compound and an aldehyde compound in a solvent in the presence of a catalytic amount of a phenolic polycondensation catalyst and a pore-forming amount of a porogen. Different types of porous phenolic resin microspheres can be obtained by selecting different phenolic compounds and aldehyde compounds. Furthermore, the reaction conditions can be controlled to obtain porous phenolic resin microspheres with different particle sizes, pore sizes, specific surface areas, or total pore volumes. This provides a high degree of designability, thereby enabling suitable porous phenolic resin microspheres to be obtained as needed.
[0014] In some embodiments, the molar ratio of the phenolic hydroxyl group in the phenolic compound to the aldehyde group in the aldehyde compound is 1:1.1 to 1:1.6. In this case, the porous phenolic resin microspheres obtained have a better dispersion, which is conducive to obtaining porous phenolic resin microspheres with stable properties, ensuring that the coating formed by the coating composition has more stable performance.
[0015] In some embodiments, the phenolic compound includes at least one of phenol, hydroquinone, resorcinol, catechol, cresol, and cardanol; the aldehyde compound includes formaldehyde and / or paraformaldehyde; the phenol-formaldehyde polycondensation reaction catalyst is an alkaline substance including at least one of sodium hydroxide, ammonia, triethylamine, barium hydroxide, and aniline; and the porogen includes at least one of toluene, ethylene glycol, diethyl phthalate, dioctyl phthalate, and octadecyl alcohol. The raw materials for preparing porous phenolic resin microspheres are inexpensive, readily available, and a wide variety of materials can be selected according to actual needs, making them suitable for industrial production.
[0016] In a second aspect, the present application provides a composite isolation film, comprising: a base film, and a coating formed from the coating composition according to any embodiment of the first aspect and disposed on at least one surface of the base film.
[0017] According to the present application, the composite isolation membrane includes a coating formed by the coating composition described in any embodiment of the first aspect. Therefore, it can be understood that the composite isolation membrane has the beneficial effects of the first aspect.
[0018] In some embodiments, the coating has an area density of 0.1 g / m 2 Up to 5g / m 2 At this time, the composite separator has better heat resistance and air permeability, which can make the battery cell have better safety and capacity retention rate.
[0019] In some embodiments, the composite separator satisfies the following condition: 1.25 ≤ D / d ≤ 62.5, where D is the Dv50 particle size of the porous phenolic resin microspheres and d is the average pore size of the base membrane. This allows the coating thickness to be reduced while maintaining the heat resistance and air permeability of the composite separator, thereby increasing the energy density of the battery cell.
[0020] In some embodiments, the composite separator satisfies the following relationship: 1.5≤D / d≤25. In this case, the thickness of the coating layer can be further reduced while ensuring the heat resistance and air permeability of the composite separator, thereby further improving the energy density of the battery cell.
[0021] In a third aspect, the present application provides a battery cell comprising the composite isolation membrane described in any embodiment of the second aspect.
[0022] According to the present application, the battery cell includes the composite isolation membrane described in any embodiment of the second aspect, so it can be understood that the battery cell has the beneficial effects of the second aspect.
[0023] In a fourth aspect, the present application provides a battery comprising the battery cell described in any embodiment of the third aspect.
[0024] In a fifth aspect, the present application provides an electrical device comprising at least one of the battery cells described in any embodiment of the third aspect or the batteries described in any embodiment of the fourth aspect.
[0025] The present application provides a coating composition that can be used to prepare a coating on the surface of a base film to obtain a composite isolation membrane. The composite isolation membrane has good heat resistance and air permeability, thereby obtaining a battery cell with good safety and high capacity retention. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] FIG1 is a scanning electron microscope image of the surface morphology of porous phenolic resin microspheres according to one embodiment of the present application.
[0027] FIG2 is a scanning electron microscope image of the mechanical cross-sectional morphology of porous phenolic resin microspheres according to one embodiment of the present application.
[0028] FIG3 is a schematic diagram of a battery cell according to an embodiment of the present application.
[0029] FIG. 4 is an exploded view of the battery cell shown in FIG. 3 according to an embodiment of the present application.
[0030] FIG5 is a schematic diagram of a battery module according to an embodiment of the present application.
[0031] FIG6 is a schematic diagram of a battery according to an embodiment of the present application.
[0032] FIG. 7 is an exploded view of the battery shown in FIG. 6 according to an embodiment of the present application.
[0033] FIG8 is a schematic diagram of an electrical device using a battery cell as a power source according to an embodiment of the present application.
[0034] Explanation of reference numerals: 1 battery; 2 upper housing; 3 lower housing; 4 battery module; 5 battery cell; 51 housing; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION
[0035] Below, with appropriate reference to the accompanying drawings, embodiments of the present application, including a coating composition for a separator, a battery cell, a battery, and an electrical device, are described in detail. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially identical structures may be omitted. This is to avoid unnecessary length in the following description and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0036] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0037] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0038] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0039] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0040] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0041] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0042] In order to conveniently describe the beneficial effects of the embodiments of the present application, in the context of the present application specification, unless otherwise specified, the composite isolation film refers to a coating formed by using the coating composition in the embodiments of the present application on a base film.
[0043] As mentioned in the background technology section above, while the application range of batteries is becoming increasingly broad, the requirements for battery safety are becoming increasingly stringent. A battery cell generally includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is located between the positive and negative electrode sheets and serves to conduct ions while isolating electrons.
[0044] However, current separators generally use polyolefin films, such as polyethylene films and polypropylene films. The problem is that polyolefin films have poor heat resistance. Polyethylene films and polypropylene separators will shrink severely when heated at temperatures of 130°C and 150°C, respectively, which may cause direct contact between the positive and negative electrodes, resulting in a short circuit. In severe cases, thermal runaway may occur, posing a safety hazard.
[0045] To address the aforementioned issues, a ceramic coating is often prepared on a polyolefin film in related technologies to reduce the thermal shrinkage of the separator, thereby preventing short circuits caused by direct contact between the positive and negative electrodes, thereby improving the safety of the battery cells. However, the problem is that the separator also serves as an ion conductor in the battery cells. While preparing a heat-resistant coating on the polyolefin film can reduce the thermal shrinkage of the separator to a certain extent, it also significantly affects the air permeability of the polyolefin film, resulting in a reduction in the ion pathways on the separator, causing poor ion transport performance, and thus increased polarization of the battery cells, reduced electrical performance, and decreased capacity retention. Furthermore, current heat-resistant coatings primarily use traditional ceramic materials such as boehmite, alumina, and silica, which, due to their high density, also reduce the energy density of the battery cells.
[0046] In view of the above technical problems, the embodiments of the present application propose a coating composition for an isolation membrane from the perspective of improving coating performance. The coating composition can be used to prepare a heat-resistant coating on a base membrane. The coating composition contains porous phenolic resin microspheres, which have good heat resistance and can reduce the thermal shrinkage of the isolation membrane. In addition, due to its porous structure, it does not significantly affect the air permeability of the isolation membrane, that is, it does not affect the ion transport performance of the isolation membrane. Therefore, while improving battery safety, it also has a high capacity retention rate. It is also worth noting that the density of the porous phenolic resin microspheres is lower than that of the ceramic materials in the related art, and therefore will not significantly affect the energy density of the battery cell.
[0047] Coating composition for release film
[0048] In a first aspect, an embodiment of the present application proposes a coating composition for an isolation membrane, comprising: porous phenolic resin microspheres and a binder, wherein the mass ratio of the binder to the porous phenolic resin microspheres is 1:1 to 1:20.
[0049] According to the present application, the coating composition includes porous phenolic resin microspheres and a binder. After the coating composition is used to form a coating on a base film to obtain a composite isolation membrane, the porous phenolic resin microspheres serve as the skeleton of the coating. Phenolic resin is a large class of synthetic resins produced by addition and polycondensation reactions of phenolic compounds and aldehyde compounds. Like general polymer compounds, phenolic resins possess the basic properties of polymer compounds, such as high molecular weight, diverse molecular structures, curing properties, and cracking and carbonization properties. In addition, due to the cross-linked network structure of phenolic resin and the large number of rigid benzene rings contained therein, the porous phenolic resin microspheres have excellent heat resistance, ablation resistance, flame retardancy, and strength, and can maintain their structural integrity and dimensional stability even at very high temperatures. When the composite isolation membrane is heated, the base membrane shrinks, driving the porous phenolic resin microspheres to quickly contact and squeeze each other. Since the porous phenolic resin microspheres have high heat resistance and strength, they are not easy to deform during the extrusion process, thereby applying a force opposite to the shrinkage direction to the base membrane, which can significantly reduce the thermal shrinkage rate of the base membrane and improve its heat resistance. Therefore, in the battery cell using the composite isolation membrane, the composite isolation membrane has good deformation resistance at higher temperatures, thereby reducing the probability of short circuit caused by direct contact between the positive and negative pole pieces in the battery cell, and thus the thermal safety performance of the battery cell is significantly improved.
[0050] In addition, FIG1 shows a scanning electron microscope image of the surface morphology of the porous phenolic resin microspheres obtained in one embodiment of the present application, and FIG2 shows a scanning electron microscope image of the mechanical cross-sectional morphology of the porous phenolic resin microspheres obtained in one embodiment of the present application. It can be seen that the porous phenolic resin microspheres have a continuous porous structure, so preparing the above-mentioned coating on the base membrane does not significantly affect its air permeability. It can be understood that the function of the separator in the battery cell is also to provide a transmission channel for ions. The better the air permeability of the separator, the more channels it can provide for ion conduction, that is, the better the ion transmission performance. Generally, when a coating is prepared on a base membrane, it may block some of the pores on the base membrane, resulting in a deterioration in ion transmission performance. However, in the embodiment of the present application, due to the porous structure of the porous phenolic resin microspheres, even if they block the original pores on the separator, ions can pass through the pores in the microspheres. Therefore, the composite separator obtained using the above-mentioned coating composition does not significantly reduce its air permeability compared to the base membrane.
[0051] At the same time, the porous structure of the porous phenolic resin microspheres, with their smaller pores, allows for the adsorption of electrolyte through capillary action, filling the pores of the porous phenolic resin microspheres with electrolyte. This increases the contact area between the separator and the electrolyte, thereby helping to improve the electrolyte's wetting and retention of the separator, providing ample ion channels. Compared to conventional heat-resistant coatings in the prior art, this significantly improves the ion transport performance of the composite separator. Therefore, battery cells using this composite separator exhibit less polarization during charge and discharge, resulting in higher capacity retention.
[0052] It is also worth mentioning that the porous phenolic resin microspheres have a lower density than ordinary phenolic resin microspheres due to their porous structure, thereby reducing the weight of the composite separator and thus increasing the energy density of the battery cell.
[0053] The binder in the coating composition is mainly used for stable bonding between the porous phenolic resin microspheres and the base film and between the porous phenolic resin microspheres. It can be understood that according to the description of the porous phenolic resin microspheres reducing the thermal shrinkage of the base film, that is, the porous phenolic resin microspheres exert a force on the base film in the opposite direction of the shrinkage, so the stable bonding between the porous phenolic resin microspheres and the base film has a great influence on the porous phenolic resin microspheres to play their role. If the binder is not added, it is difficult to reduce the thermal shrinkage of the base film only by the friction between the microspheres and the base film. By adding the binder, the microspheres and the base film are bonded by the binder, and the bonding force is much higher than the friction between the microspheres and the base film, thereby enabling the coating to better reduce the thermal shrinkage of the base film. In addition, the strong bonding force can also ensure that the coating on the surface of the composite separator is not easy to fall off, has better stability, and thus improves the safety of the battery cell.
[0054] In the embodiment of the present application, the mass ratio of the binder and the porous phenolic resin microspheres is further limited to 1:1 to 1:20. It can be understood that if the binder content is too high, since the heat resistance and strength of general binders are worse than those of phenolic resins, the force applied by the coating to the base film in the opposite direction of shrinkage will be reduced, thereby failing to effectively reduce the thermal shrinkage rate of the base film. In addition, too high a binder content will increase the difficulty of coating and increase production costs; if the binder content is too low, it will not be able to effectively play the role of the binder mentioned above, that is, the adhesion between the microspheres and the base film is poor, and the force applied by the coating to the base film in the opposite direction of shrinkage is reduced. At the same time, the coating is unstable and prone to powdering, affecting the heat resistance and stability of the composite isolation membrane. Therefore, it is necessary to control the mass ratio of the binding agent and the porous phenolic resin microspheres within the scope of 1:1 to 1:20. For example, the mass ratio of the binding agent and the porous phenolic resin microspheres can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, or within the scope of the above arbitrary numerical values. Preferably, the mass ratio of the binding agent and the porous phenolic resin microspheres can be 1:8 to 1:15.
[0055] In some embodiments, the binder includes at least one of polyacrylic acid, polyacrylate, polyvinylidene fluoride, styrene-butadiene rubber, and sodium carboxymethyl cellulose.
[0056] In the above embodiments, several specific binders are listed. Those skilled in the art may select one or more of these binders based on their specific needs. These binders have good adhesion properties, allowing the porous phenolic resin microspheres to be stably bonded to the surface of the base film, thereby improving the stability of the composite separator. Furthermore, these binders have good heat resistance, maintaining strong adhesion even at higher temperatures, thereby further improving the heat resistance of the composite separator.
[0057] It should be noted that the binder includes but is not limited to the substances listed above, and those skilled in the art can select any binder known in the prior art according to actual needs.
[0058] In some embodiments, the porous phenolic resin microspheres meet at least one of the following conditions: 1) the Dv50 particle size of the porous phenolic resin microspheres is 0.1 μm to 5 μm; 2) the average pore size of the porous phenolic resin microspheres is 10 nm to 50 nm; 3) the specific surface area of the porous phenolic resin microspheres is 15 m 2 / g to 280m 2 / g; 4) the total pore volume of the porous phenolic resin microspheres is 0.700 cm 3 / g to 1.680cm 3The composite separator obtained in this case has better heat resistance or air permeability, which is more conducive to improving the safety and capacity retention rate of the battery monomer using the composite separator.
[0059] In the above embodiment, the parameters related to the porous phenolic resin microspheres are further limited, so that the heat resistance or air permeability of the obtained composite separator can be improved, which is more conducive to improving the safety and capacity retention rate of the battery cell using the composite separator.
[0060] Among them, 1) the Dv50 particle size of the porous phenolic resin microspheres can be 0.1μm to 5μm. It is understood that, generally, the smaller the particle size of the porous phenolic resin microspheres, the greater the number of microspheres per unit area of the base film. Therefore, the microspheres exert a greater force on the base film opposite to the direction of contraction, and the resulting composite separator has better heat resistance. In addition, when the particle size is smaller, while ensuring the heat resistance of the composite separator, the coating is lighter and thinner, which is beneficial for increasing the energy density of the battery cell. Therefore, it is generally advisable to minimize the Dv50 particle size of the porous phenolic resin microspheres to obtain a composite separator with better heat resistance. However, if the Dv50 particle size of the porous phenolic resin microspheres is too small, the effect on the air permeability of the composite isolation membrane will increase. It is understandable that the smaller the particle size, the greater the packing density of the coating, the smaller the porosity of the coating, and even some of the porous phenolic resin microspheres will enter the pores of the base membrane, causing pore blockage. Although its porous structure can still provide a channel for ion conduction, it will still reduce the air permeability of the base membrane to a certain extent. In addition, the porous phenolic resin microspheres located inside the pores of the base membrane cannot effectively exert a force on the base membrane that is opposite to the direction of contraction, but will instead lead to a decrease in the heat resistance of the composite isolation membrane.
[0061] In summary, due to the good heat resistance and porous structure of the porous phenolic resin microspheres in the embodiments of the present application, the Dv50 particle size of the porous phenolic resin microspheres can be smaller than the ceramic material used in the heat-resistant coating in the prior art, thereby improving the energy density of the battery cell while ensuring the heat resistance and air permeability of the composite separator. Therefore, the Dv50 particle size of the porous phenolic resin microspheres can be controlled within 0.1μm to 5μm. For example, the Dv50 particle size of the porous phenolic resin microspheres can be 0.1μm, 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, 1.5μm, 2.0μm, 2.5μm, 3.0μm, 3.5μm, 4.0μm, 4.5μm, 5.0μm, or within the range of any of the above values. More preferably, the Dv50 particle size of the porous phenolic resin microspheres is controlled within a range of 0.12 μm to 2 μm.
[0062] It should be noted that the Dv50 particle size of the porous phenolic resin microspheres herein has a meaning generally known in the art. Dv50 refers to the particle size distribution based on volume at which 50% of the particles have a particle size smaller than this value. Dv50 can be measured using methods and instruments known in the art. For example, it can be measured using a laser particle size analyzer (e.g., Malvern Mastersizer 2000E, UK) in accordance with GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method.
[0063] 2) In the above embodiment, the average pore size of the porous phenolic resin microspheres is further limited. Generally speaking, the smaller the average pore size of the porous phenolic resin microspheres, the more obvious their capillary action, the better the wettability and liquid retention of the composite separator to the electrolytic salt, and the more conducive to improving the ion transmission performance of the composite separator; and under the premise of a certain total pore volume, the smaller the average pore size, the better the heat resistance and rigidity of the porous phenolic resin microspheres, which is conducive to improving the heat resistance of the composite separator. However, if the average pore size is too small, it is not conducive to increasing the total pore volume of the porous phenolic resin microspheres, and it will also increase the production cost of the porous phenolic resin microspheres. Therefore, the average pore size of the porous phenolic resin microspheres can be controlled to be between 10nm and 50nm. At this time, the resulting composite separator has good heat resistance and ion transmission performance, which can improve the safety and capacity retention of the battery cell. For example, the average pore size of the porous phenolic resin microspheres can be 10nm, 12nm, 14nm, 16nm, 20nm, 22nm, 24nm, 26nm, 28nm, 30nm, 32nm, 34nm, 36nm, 38nm, 40nm, 42nm, 44nm, 46nm, 48nm, 50nm, or within the scope of the above arbitrary numerical values. Further preferably, the average pore size of the porous phenolic resin microspheres can be controlled in 15nm to 40nm.
[0064] It should be noted that the average pore size of the porous phenolic resin microspheres in this application can be measured according to GB / T 21650.2-2008, Determination of pore size distribution and porosity of solid materials by mercury intrusion and gas adsorption method - Part 2: Analysis of mesopores and macropores by gas adsorption method.
[0065] 3) In the above embodiment, the specific surface area of the porous phenolic resin microspheres is further limited. It is understandable that the specific surface area of the porous phenolic resin microspheres is related to their particle size, pore size and total pore volume. Generally speaking, when other conditions are constant, the smaller the particle size, the smaller the pore size and the larger the total pore volume, the larger the specific surface area of the porous phenolic resin microspheres. The inventors have found through a large number of experiments that when the specific surface area of the porous phenolic resin microspheres is 15m 2 / g to 280m 2When the surface area of the porous phenolic resin microspheres is within the range of 15 m / g, the obtained composite separator has better heat resistance and ion transmission performance, better safety of the battery cell and higher capacity retention rate. 2 / g,30m 2 / g,45m 2 / g,60m 2 / g,80m 2 / g,100m 2 / g,110m 2 / g,120m 2 / g,130m 2 / g,140m 2 / g,150m 2 / g,160m 2 / g,170m 2 / g,180m 2 / g,190m 2 / g,200m 2 / g,210m 2 / g,220m 2 / g,230m 2 / g,240m 2 / g,250m 2 / g,260m 2 / g,270m 2 / g,280m 2 / g, or within the range of any of the above values. Further preferably, the specific surface area of the porous phenolic resin microspheres can be controlled within 60m 2 / g to 265m 2 / g inside.
[0066] It should be noted that the specific surface area of the porous phenolic resin microspheres in this application is measured by the following method: using a specific surface area analyzer, model TRISTAR II 3020, according to GB / T 19587-2004, the gas adsorption BET method for determining the specific surface area of solid substances: 1. Pretreatment: Place an appropriate amount of sample in a dedicated sample tube, heat and vacuum degas for 2 hours, and weigh the total weight after cooling to room temperature. Subtract the mass of the sample tube to obtain the sample mass. 2. Testing: Place the sample tube in the workstation and, at a constant low temperature, measure the amount of gas adsorbed on the solid surface at different adsorption pressures. Based on the BET multilayer adsorption theory and its formula, the sample monolayer adsorption amount is obtained, thereby calculating the specific surface area per unit mass of the solid sample. 3. Adsorption gas: nitrogen, adsorption pressure points 0.05 / 0.10 / 0.15 / 0.20 / 0.25 / 0.30, test atmosphere: high-purity liquid nitrogen atmosphere.
[0067] 4) In the above embodiment, the total pore volume of the porous phenolic resin microspheres is further limited. The larger the total pore volume of the porous phenolic resin microspheres, that is, the higher the porosity, the more ion channels are obtained in the composite isolation membrane, thereby better ion transmission performance and higher capacity retention rate of the battery cell. However, when the total pore volume of the porous phenolic resin microspheres is too large, the heat resistance and strength of the porous phenolic resin microspheres will be reduced, which may lead to a decrease in the heat resistance of the composite isolation membrane and a decrease in the safety of the battery cell. Therefore, the total pore volume of the porous phenolic resin microspheres can be controlled at 0.700 cm 3 / g to 1.680cm 3 / g range, the composite separator can better balance its heat resistance and ion transmission performance, and the battery cell has good safety and high capacity retention. For example, the total pore volume of porous phenolic resin microspheres can be 0.7cm 3 / g,0.75cm 3 / g,0.8cm 3 / g,0.85cm 3 / g,0.9cm 3 / g,0.95cm 3 / g,1.0cm 3 / g,1.05cm 3 / g,1.1cm 3 / g,1.15cm 3 / g,1.2cm 3 / g,1.25cm 3 / g,1.3cm 3 / g, 1.35cm 3 / g,1.4cm 3 / g, 1.45cm 3 / g,1.5cm 3 / g,1.55cm 3 / g,1.6cm 3 / g, 1.68cm 3 / g, or within the range of any of the above values. Further preferably, the total pore volume of the porous phenolic resin microspheres can be controlled to be 0.91 cm 3 / g to 1.56cm 3 / g range.
[0068] It should be noted that the total pore volume of the porous phenolic resin microspheres in this application is measured by the following method: using a specific surface area analyzer, model TRISTAR II 3020, reference: GB / T 21650.2-2008, the total pore volume can be directly measured.
[0069] In some embodiments, the porous phenolic resin microspheres are obtained by reacting a phenolic compound and an aldehyde compound in a solvent in the presence of a catalytic amount of a phenolic polycondensation catalyst and a pore-forming amount of a porogen.
[0070] In the above embodiment, different types of porous phenolic resin microspheres can be obtained by selecting different phenolic compounds and aldehyde compounds. In addition, the reaction conditions can be controlled to obtain porous phenolic resin microspheres with different particle sizes, pore sizes, specific surface areas or total pore volumes. This has a high degree of designability, thereby obtaining suitable porous phenolic resin microspheres according to actual needs.
[0071] For example, different phenolic compounds and aldehyde compounds can be used to obtain porous phenolic resin microspheres with different heat resistance or strength; by controlling the reaction conditions, such as the ratio of phenolic compounds to aldehyde compounds, the intensity of stirring during the reaction, and other conditions, porous phenolic resin microspheres with different particle sizes can be obtained; by controlling the addition amount, type or reaction conditions of the porogen, the average pore size of the porous phenolic resin microspheres can be controlled; and at the same time, the specific surface area and total pore volume of the porous phenolic resin microspheres can be further regulated.
[0072] It should also be noted that porous phenolic resin microspheres with different performance parameters can also be purchased directly through commercial channels.
[0073] In some embodiments, the molar ratio of the phenolic hydroxyl group in the phenolic compound to the aldehyde group in the aldehyde compound is 1:1.1 to 1:1.6.
[0074] In the above-mentioned embodiment, by can controlling the molar ratio of the phenolic hydroxyl group in phenolic compound and the aldehyde group in aldehyde compound, increase initial cross-linking polymerization reaction point in reaction system, thereby be more conducive to controlling the particle size distribution of porous phenolic resin microsphere, be that particle diameter is relatively more concentrated, namely the dispersion degree of the porous phenolic resin microsphere obtained at this moment is better, be conducive to obtaining the porous phenolic resin microsphere of stable properties, ensure that the coating performance that coating composition forms is more stable.For example, the molar ratio of the phenolic hydroxyl group in phenolic compound and the aldehyde group in aldehyde compound can be 1:1.1,1:1.15,1:1.2,1:1.25,1:3,1:1.35,1:1.4,1:1.45,1:1.5,1:1.55,1:1.6, or in the scope that above-mentioned arbitrary numerical value is formed.Further preferably, the molar ratio of the phenolic hydroxyl group in phenolic compound and the aldehyde group in aldehyde compound can be 1:1.1 to 1:1.4.
[0075] In some embodiments, the phenolic compound includes at least one of phenol, hydroquinone, resorcinol, catechol, cresol, and cardanol; the aldehyde compound includes formaldehyde and / or paraformaldehyde; the phenol-formaldehyde polycondensation reaction catalyst is an alkaline substance, including at least one of sodium hydroxide, ammonia water, triethylamine, barium hydroxide, and aniline; the porogen includes at least one of toluene, ethylene glycol, diethyl phthalate, dioctyl phthalate, and octadecyl alcohol.
[0076] In the above embodiment, the raw materials that can be used to prepare porous phenolic resin microspheres are specifically listed. The raw materials for preparing porous phenolic resin microspheres are cheap and easy to obtain, and there are many types. They can be selected according to actual needs and are suitable for industrial production.
[0077] It should also be noted that the phenolic compounds, aldehyde compounds, phenol-formaldehyde polycondensation reaction catalysts and porogens mentioned above are not limited to the ones listed above. Those skilled in the art can select other types of phenolic compounds, aldehyde compounds, phenol-formaldehyde polycondensation reaction catalysts and porogens in the prior art according to actual needs.
[0078] As some examples, porous phenolic resin microspheres can be prepared by the following method:
[0079] A phenolic compound, an aldehyde compound, a phenol-formaldehyde polycondensation reaction catalyst, and a porogen are added to a solvent to obtain a reaction system, and the reaction is carried out under heating and stirring for 3 to 8 hours, and then the pH of the reaction system is adjusted to 2 to 6, and the heating reaction is continued for 0.5 to 2 hours, and the mixture is cooled to room temperature with stirring;
[0080] The reaction system is filtered, washed, and dried to obtain porous phenolic resin microspheres.
[0081] It is understood that the above method is exemplary, and the porous phenolic resin microspheres can be prepared according to other methods known in the prior art.
[0082] As some examples, the total mass percentage of phenolic compounds and aldehyde compounds in the reaction system is 21% to 26%; the mass percentage of phenol-formaldehyde polycondensation reaction catalyst in the reaction system is 0.1% to 1%; the mass percentage of porogen in the reaction system is 5% to 10%; the remainder is solvent, which can be water.
[0083] As some examples, the heating temperature during heating and stirring is 70° C. to 100° C.
[0084] In some embodiments, the coating composition further includes a dispersant, which may include water, dimethylformamide (DMF), diethylformamide, dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), methanol, ethanol, 1-propanol, 2-propanol (isopropanol), 1-butanol (n-butanol), 2-methyl-1-propanol (isobutanol), 2-butanol (sec-butanol), 1-methyl-2-propanol (tert-butanol), pentanol, hexanol, heptanol or octanol; diols, Such as at least one of ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,5-pentanediol, hexylene glycol, glycerol, trimethylolpropane, pentaerythritol, sorbitol, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, tetraethylene glycol monobutyl ether, acetone, methyl ethyl ketone, methyl propyl ketone, cyclopentanone, ethyl acetate, γ-butyrolactone and ε-propiolactone.
[0085] In some embodiments, the solids content of the coating composition may be from 10% to 50%.
[0086] In some embodiments, the coating composition may further include other additives, such as defoaming agents, wetting agents, emulsifiers, anti-precipitation agents, etc. Those skilled in the art may select and add these additives as needed.
[0087] Preparation method of coating composition for isolation film
[0088] The present application also provides a method for preparing a coating composition for an isolation membrane, comprising the following steps: dispersing porous phenolic resin microspheres and a binder in a dispersant to obtain a coating composition for an isolation membrane.
[0089] The specific types and addition amounts of the porous phenolic resin microspheres, binder and dispersant can be selected according to any embodiment of the first aspect.
[0090] Composite isolation membrane
[0091] In a second aspect, the present application provides a composite isolation film, comprising: a base film, and a coating formed from the coating composition according to any embodiment of the first aspect and disposed on at least one surface of the base film.
[0092] According to the present application, the composite isolation membrane includes a coating formed by the coating composition of any embodiment of the first aspect, so it can be understood that the composite isolation membrane has the beneficial effects of the first aspect.
[0093] In any embodiment of the present application, the type of base film is not limited. A separator known in the art can be selected as the base film according to actual needs. For example, a single-layer polyolefin separator or a multi-layer polyolefin separator can be used as the base film. The single-layer polyolefin separator can include at least one of a polyethylene separator and a polypropylene separator. The multi-layer polyolefin separator can include at least one of a polypropylene-polyethylene-polypropylene separator and a polypropylene-polyethylene separator.
[0094] In some embodiments, the coating has an areal density of 0.1 g / m 2 Up to 5g / m 2 .
[0095] In the above embodiment, since the porous phenolic resin microspheres in the coating have good heat resistance and strength, and their density is relatively low, compared to general ceramic coatings, the above coating can still make the composite isolation membrane have good heat resistance under the condition of lower surface density. In addition, the smaller surface density can make the composite isolation membrane more breathable, so that the battery cell has good safety while having a higher capacity retention rate. At the same time, it can effectively improve the energy density of the battery cell. However, if the surface density of the coating is too low, the heat resistance of the composite isolation membrane cannot be guaranteed. Therefore, the surface density of the coating can be controlled at 0.1g / m 2 Up to 5g / m 2 In the range of, for example, the surface density of the coating can be 0.1g / m 2 , 0.2g / m 2 , 0.3g / m 2 , 0.4g / m 2 , 0.5g / m 2 , 0.6g / m 2 , 0.7g / m 2 , 0.8g / m 2 , 0.9g / m 2 , 1g / m 2 , 1.2g / m 2 , 1.4g / m 2 , 1.6g / m 2 , 1.8g / m 2 , 2g / m 2 , 2.2g / m 2 , 2.4g / m 2 , 2.6g / m 2 , 2.8g / m 2 , 3g / m 2 , 3.5g / m 2 , 4g / m 2 , 4.5g / m 2 , 5g / m 2, or within the range of any of the above values. Further preferably, the surface density of the coating can be 1g / m 2 Up to 4g / m 2 .
[0096] In some embodiments, the composite isolation membrane satisfies: 1.25≤D / d≤62.5, wherein D is the Dv50 particle size of the porous phenolic resin microspheres, and d is the average pore size of the base membrane.
[0097] In the above embodiment, the relationship between the Dv50 particle size of the porous phenolic resin microspheres and the average pore size of the base membrane is specifically defined. Through extensive experiments, the inventors have discovered that the resulting composite separator membrane exhibits excellent heat resistance and air permeability. Compared to conventional ceramic coatings, the D / d value can be even smaller. This indicates that, due to their excellent heat resistance and porous structure, the porous phenolic resin microspheres can still meet the heat resistance and air permeability requirements of the composite separator membrane even when the porous phenolic resin microspheres in the coating are relatively small. This allows for the use of a thin coating process, reducing the overall weight and thickness of the composite separator membrane, thereby increasing the energy density of the battery cell. The value of D / d can be 1.25, 1.5, 2, 2.5, 3, 3.5, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 22, 24, 26, 28, 30, 35, 40, 45, 50, 55, 60, 62.5, or any range thereof. Further preferably, the composite isolation membrane satisfies: 1.5≤D / d≤25.
[0098] battery cells
[0099] In a third aspect, the present application provides a battery cell comprising the composite isolation membrane of any embodiment of the second aspect.
[0100] According to the present application, the battery cell includes the composite isolation membrane of any embodiment of the second aspect, so it can be understood that the battery cell has the beneficial effects of the second aspect.
[0101] Typically, a battery cell consists of a positive electrode, a negative electrode, and an electrolyte. During the battery's charge and discharge processes, active ions are embedded in and extracted from the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes.
[0102] [Positive electrode]
[0103] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes the positive electrode active material of the first aspect of the present application.
[0104] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0105] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0106] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0107] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0108] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0109] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0110] [Negative electrode]
[0111] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0112] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0113] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0114] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0115] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0116] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0117] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0118] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0119] [Electrolytes]
[0120] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0121] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0122] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0123] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0124] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0125] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the composite separator can be formed into an electrode assembly through a winding process or a lamination process.
[0126] In some embodiments, the battery cell may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0127] In some embodiments, the outer packaging of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the battery cell may be a soft shell, such as a pouch-type soft shell. The soft shell may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0128] The present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square, or any other shape. For example, FIG3 shows a battery cell 5 with a square structure as an example.
[0129] In some embodiments, referring to Figure 4, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0130] Battery
[0131] In a fourth aspect, the present application provides a battery comprising a battery cell according to any embodiment of the third aspect.
[0132] According to the present application, battery cells can be assembled into a battery. One embodiment of the present application further provides a battery, comprising: a box and the above-mentioned battery cells; the battery cells are accommodated in the box.
[0133] The battery may include one or more battery cells, and those skilled in the art may select the specific number based on the application and capacity of the battery.
[0134] Furthermore, in the above-mentioned battery, multiple battery cells are assembled to form a battery module. Figure 5 shows an example battery module 4. Referring to Figure 5 , within the battery module 4, multiple battery cells 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple battery cells 5 may be secured using fasteners.
[0135] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.
[0136] Figures 6 and 7 illustrate an example battery 1. Referring to Figures 6 and 7 , the battery 1 may include a battery box and multiple battery modules 4 disposed within the box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0137] The battery may be a secondary battery or a lithium battery.
[0138] Electrical devices
[0139] In a fifth aspect, the present application provides an electrical device comprising at least one of the battery cells of any embodiment of the third aspect or the battery of any embodiment of the fourth aspect.
[0140] The present application also provides an electrical device, which includes a battery cell or battery provided in the present application. The battery cell or battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0141] As the electrical device, the battery cell or battery mentioned above can be selected according to its usage requirements.
[0142] FIG8 shows an example of an electric device, which may be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.
[0143] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be lightweight and thin, and may use a battery cell as a power source.
[0144] Example
[0145] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0146] Preparation of porous phenolic resin microspheres: Add a phenolic compound, an aldehyde compound, a catalyst, a porogen, and water in a certain proportion to a three-necked flask equipped with a mechanical stirrer and a reflux condenser. Stir and heat to 90°C. After stirring and dispersing for 4 hours, adjust the pH of the system to 2-3, continue heating the reaction for 1 hour, stop heating, and cool to room temperature with stirring.
[0147] The reactants are filtered, washed with water until neutral, and dried to obtain phenolic resin porous microspheres.
[0148] According to existing methods, phenolic resin porous microspheres with different particle sizes, average pore sizes, specific surface areas and total pore volumes can be obtained by controlling the types and addition amounts of phenolic compounds, aldehyde compounds, catalysts, and porogens in the above reaction system, or the reaction conditions.
[0149] Example 1-1
[0150] (1) Preparation of composite isolation membrane
[0151] A commercially available PE polymer microporous film with a thickness of 7 μm and an average pore size of 80 nm (from Zhuo Gao Electronic Technology Co., Ltd.) was used as the substrate. A total of 150 g of polyacrylic acid binder and porous phenolic resin microspheres were added to 850 g of deionized water in a mass ratio of 1:10 and stirred to obtain a slurry. The slurry was coated on the substrate and dried in an oven. The coating density of the binder and porous phenolic resin microspheres on the substrate was 2 g / m 2 , then rolled up to obtain a composite isolation film.
[0152] The preparation parameters of the porous phenolic resin microspheres and their Dv50 particle size, average pore size, specific surface area, and total pore volume are shown in Table 1.
[0153] (2) Preparation of positive electrode sheet
[0154] Polyvinylidene fluoride (PVDF), lithium iron phosphate (LFP), conductive carbon black, and N-methylpyrrolidone (NMP) were mixed in a mass ratio of 1.2:58.38:0.42:40 and stirred thoroughly to prepare a positive electrode slurry. 2 The loading amount is evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed and cut to obtain the positive electrode sheet.
[0155] (3) Preparation of negative electrode sheet
[0156] Artificial graphite, conductive agent acetylene black, binder styrene butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na) were added into deionized water in a mass ratio of 96.2:1.0:1.6:1.2, and stirred thoroughly to prepare a negative electrode slurry (solid content of 63%). 2 The loading amount is coated on the negative electrode current collector copper foil, and then dried, cold pressed and cut to obtain the negative electrode sheet.
[0157] (4) Preparation of electrolyte
[0158] At 25°C, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain a mixed solvent, and then LiPF6 is dissolved in the above mixed solvent to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0159] (5) Preparation of secondary batteries
[0160] The above-mentioned positive electrode sheets, composite separators, and negative electrode sheets are stacked and wound in sequence, and cold-pressed (during which the separators and the electrodes are bonded) to obtain a battery cell; the battery cell is placed in an outer package, and the above-prepared electrolyte is added. After packaging, standing, formation, aging and other processes, a secondary battery is obtained.
[0161] Examples 1-2 to 1-36 are substantially the same as Example 1-1, and some of the different parameters are detailed in Table 1.
[0162] Comparative Example 1-1
[0163] The method is substantially the same as Example 1-1, except that a commercially available PE polymer microporous film with a thickness of 7 μm and an average pore size of 80 nm is directly used as the separator of the secondary battery.
[0164] Comparative Example 1-2
[0165] It is substantially the same as Example 1-1, except that the composite separator is different. Alumina with a Dv50 of 1 μm is used instead of porous phenolic resin microspheres to prepare the composite separator as the separator of the secondary battery.
[0166] Examples 2-1 to 2-10, Comparative Example 2-1, and Comparative Example 2-2 are substantially the same as Example 1-7, and some of the different parameters are detailed in Table 2.
[0167] Test section
[0168] 1. Thermal shrinkage test of diaphragm
[0169] Sample preparation: The prepared diaphragm was punched into samples with a width of 50 mm and a length of 100 mm using a punching machine. Five parallel samples were placed on A4 paper, and then the A4 paper containing the samples was placed on corrugated paper with a thickness of 1 mm to 5 mm.
[0170] Sample test: Set the temperature of the blast oven to 150°C. After the temperature reaches the set temperature and stabilizes for 30 minutes, place the A4 paper placed on the corrugated paper into the blast oven, start timing, and after the set time (1 hour in this application) is reached, measure the length and width of the diaphragm, and mark the values as a and b respectively.
[0171] Calculation of thermal shrinkage: longitudinal (MD) thermal shrinkage = [(100-a) / 100] × 100%, transverse (TD) thermal shrinkage = [(50-b) / 50] × 100%, and the average value of 5 parallel samples is taken as the test result.
[0172] 2. Air permeability measurement method
[0173] Cut the membrane into 5cm squares and use a gas permeability tester to test the permeability of 100ml of gas through 6.45cm under a pressure of 1.21kPa. 2 The time required for the membrane to separate is used to obtain its permeability value, which is expressed in s / 100 mL.
[0174] 3. Secondary battery capacity retention test
[0175] At 25°C, charge the battery at a constant current of 1 / 3C to 4.2V. Then, charge the battery at a constant voltage of 4.2V to a current of 0.05C. Let the battery rest for 5 minutes, then discharge the battery at a constant current of 1 / 3C to 2.8V. The resulting capacity is recorded as the initial capacity, C0. Repeat these steps and simultaneously record the discharge capacity, C1000, of the secondary battery after the 1000th cycle. The capacity retention rate after 1000 cycles, P1000, is calculated as: C1000 / C0 × 100%.
[0176] The test results are shown in Table 1 and Table 2
[0177] Table 1 shows that the composite separators obtained in each example exhibit lower thermal shrinkage and significantly improved secondary battery capacity retention, compared to the comparative examples. Comparative Example 1-1, in which a polyethylene film is used directly as the secondary battery separator, exhibits poor heat resistance and, therefore, a higher thermal shrinkage, resulting in poor secondary battery safety. Furthermore, while the absence of a surface coating provides good air permeability, heat generation during the secondary battery's cycling inevitably results in the separator's inability to maintain a stable structure, leading to a lower capacity retention rate. In Comparative Example 1-2, alumina with a Dv50 particle size of 1 μm is used instead of porous phenolic resin microspheres to prepare a composite isolation membrane. Its thermal shrinkage rate is lower than that of Comparative Example 1-1, but the reduction effect is not obvious. The possible reason is that alumina has poor film-forming properties. Although it has good heat resistance itself, it does not significantly improve the heat resistance of the isolation membrane. In addition, since it does not have a porous structure, its air permeability is significantly reduced compared with the embodiment and Comparative Example 1-1, resulting in a reduction in ion transmission pathways, increased polarization, and a low capacity retention rate of the secondary battery.
[0178] Comparing Examples 1-1 to 1-20, it can be seen that the parameters of the porous phenolic resin microspheres have a certain influence on the heat resistance and air permeability of the composite separator, thereby affecting the safety and capacity retention rate of the secondary battery. When the porous phenolic resin microspheres meet the Dv50 particle size of 0.1 μm to 5 μm, the average pore size of 10 nm to 50 nm, and the specific surface area of 15 m 2 / g to 280m 2 / g, and the total pore volume is any one of 0.700cm3 / g to 1.680cm3 / g, the obtained composite separator has good heat resistance and air permeability, and the secondary battery has good safety and high capacity retention. Preferably, the porous phenolic resin microspheres meet the Dv50 particle size of 0.12μm to 2μm, the average pore size of 15nm to 40nm, and the specific surface area of 60m 2 / g to m 2 / g, total pore volume of 0.910cm 3 / g to 1.560cm 3 When the content of MgSO4 is less than 1.04, the heat resistance or air permeability of the obtained composite separator is better, and the secondary battery has better safety and higher capacity retention rate.
[0179] Comparing Examples 1-21 to 1-28 with Example 1-7, it can be seen that the coating surface density has a certain influence on the heat resistance and air permeability of the composite separator, thereby affecting the safety and capacity retention of the secondary battery. 2 Up to 5g / cm 2 When the coating surface density is 1 g / cm 2 Up to 4g / cm 2 When the composite separator is prepared, the heat resistance and air permeability of the obtained composite separator are better, and the secondary battery has better safety and higher capacity retention rate.
[0180] Comparing Examples 1-29 to 1-32 with Example 1-7, it can be seen that the molar ratio of phenolic hydroxyl groups to aldehyde groups in the raw materials for preparing porous phenolic resin microspheres has a certain influence on the heat resistance and air permeability of the composite isolation membrane, thereby affecting the safety and capacity retention rate of the secondary battery. When the molar ratio of phenolic hydroxyl groups to aldehyde groups is 1:1.1 to 1:1.6, the heat resistance and air permeability of the obtained composite isolation membrane are better, and the secondary battery has better safety and higher capacity retention rate. Preferably, when the molar ratio of phenolic hydroxyl groups to aldehyde groups is 1:1.1 to 1:1.4, the heat resistance and air permeability of the obtained composite isolation membrane are better, and the secondary battery has better safety and higher capacity retention rate.
[0181] By comparing Examples 1-33 to 1-36 and 1-7, it can be seen that the phenolic compounds and aldehyde compounds in the raw materials for preparing porous phenolic resin microspheres have a certain influence on the heat resistance and air permeability of the composite isolation membrane, and all have good heat resistance and air permeability, and the safety and capacity retention rate of the secondary battery are good.
[0182] The possible reasons for the above results have been explained in the above content of the invention and will not be repeated here.
[0183]
[0184] According to Table 2, it can be seen from the comparison of each embodiment with each comparative example that the composite isolation membrane obtained in each embodiment has a smaller thermal shrinkage and air permeability value, and the capacity retention rate of the secondary battery is better. Among them, in Comparative Example 2-1, due to the excessively high content of the binder, the porosity of the coating is small, and the heat resistance of the binder is poor, resulting in a large thermal shrinkage and air permeability value, poor heat resistance and air permeability of the composite isolation membrane, and a low capacity retention rate of the secondary battery. In Comparative Example 2-2, the content of the binder is too little, which may cause the porous phenolic resin microspheres to be unable to stably bond to the surface of the base membrane, and thus cannot effectively reduce the thermal shrinkage rate of the base membrane. At the same time, too many microspheres will also affect the air permeability of the composite isolation membrane. In addition, the stability of the composite isolation membrane is poor, resulting in a low capacity retention rate of the secondary battery.
[0185] Comparing Example 2-1, Example 2-2 and Example 1-7, it can be seen that the type of commonly used adhesive has a certain influence on the heat resistance and air permeability of the composite isolation membrane. All of them have good heat resistance and air permeability, and the safety and capacity retention rate of the secondary battery are good.
[0186] Comparing Example 2-1, Example 2-3 to Example 2-9, it can be seen that the mass ratio of the binder and the porous phenolic resin microspheres has a certain influence on the heat resistance and air permeability of the composite isolation membrane, which in turn affects the safety and capacity retention rate of the secondary battery. When the mass ratio of the binder and the porous phenolic resin microspheres is 1:1 to 1:20, the heat resistance and air permeability of the obtained composite isolation membrane are good, and the secondary battery has good safety and a higher capacity retention rate. Preferably, when the mass ratio of the binder and the porous phenolic resin microspheres is 1:8 to 1:15, the heat resistance and air permeability of the obtained composite isolation membrane are better, and the secondary battery has better safety and a higher capacity retention rate.
[0187] The possible reasons for the above results have been explained in the above content of the invention and will not be repeated here.
[0188] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A coating composition for an isolation film, comprising: Porous phenolic resin microspheres and binders, Wherein, the mass ratio of the binder to the porous phenolic resin microspheres is 1:1 to 1:
20.
2. The coating composition according to claim 1, characterized in that The binder includes at least one of polyacrylic acid, polyacrylate, polyvinylidene fluoride, styrene-butadiene rubber and sodium carboxymethyl cellulose.
3. The coating composition according to claim 1 or 2, wherein The porous phenolic resin microspheres meet at least one of the following conditions: 1) The Dv50 particle size of the porous phenolic resin microspheres is 0.1 μm to 5 μm; 2) The average pore size of the porous phenolic resin microspheres is 10 nm to 50 nm; 3) The specific surface area of the porous phenolic resin microspheres is 15 m 2 / g to 280m 2 / g; 4) The total pore volume of the porous phenolic resin microspheres is 0.700 cm 3 / g to 1.680cm 3 / g.
4. The coating composition according to any one of claims 1 to 3, wherein The porous phenolic resin microspheres meet at least one of the following conditions: 1) The Dv50 particle size of the porous phenolic resin microspheres is 0.12 μm to 2 μm; 2) The average pore size of the porous phenolic resin microspheres is 15 nm to 40 nm; 3) The specific surface area of the porous phenolic resin microspheres is 60 m 2 / g to 265m 2 / g; 4) The total pore volume of the porous phenolic resin microspheres is 0.910 cm 3 / g to 1.560cm 3 / g.
5. The coating composition according to any one of claims 1 to 4, wherein The porous phenolic resin microspheres are obtained by reacting phenolic compounds and aldehyde compounds in a solvent in the presence of a catalytic amount of a phenolic polycondensation catalyst and a pore-forming amount of a pore-forming agent.
6. The coating composition according to claim 5, wherein The molar ratio of the phenolic hydroxyl group in the phenolic compound to the aldehyde group in the aldehyde compound is 1:1.1 to 1:1.
6.
7. The coating composition according to claim 5 or 6, wherein The phenolic compound includes at least one of phenol, hydroquinone, resorcinol, catechol, cresol and cardanol; The aldehyde compound includes formaldehyde and / or paraformaldehyde; The phenol-formaldehyde polycondensation reaction catalyst is an alkaline substance, including at least one of sodium hydroxide, ammonia water, triethylamine, barium hydroxide, and aniline; The porogen includes at least one of toluene, ethylene glycol, diethyl phthalate, dioctyl phthalate, and octadecyl alcohol.
8. A composite isolation membrane comprising: basement membrane, and A coating layer formed from the coating composition according to any one of claims 1 to 7 provided on at least one surface of the base film.
9. The composite isolation membrane according to claim 8, wherein: The surface density of the coating is 0.1 g / m 2 Up to 5g / m 2 .
10. The composite isolation membrane according to claim 8 or 9, wherein: The composite isolation film satisfies: 1.25≤D / d≤62.5, Wherein, D is the Dv50 particle size of the porous phenolic resin microspheres, d is the average pore size of the base membrane.
11. The composite isolation membrane according to any one of claims 8 to 10, wherein: The composite isolation film satisfies: 1.5≤D / d≤25. 12 . A battery cell comprising the composite separator according to claim 8 .
13. A battery comprising the battery cell according to claim 12.
14. An electrical device comprising at least one of the battery cell according to claim 12 or the battery according to claim 13.
Citation Information
Patent Citations
Separator for secondary cell, and secondary cell
CN105518905A
Isolation membrane and lithium ion secondary battery
CN106328865A
Preparation method for phenolic resin microsphere coated diaphragm
CN109309184A
Coated diaphragm and preparation method thereof
CN114361706A
Coating composition, separator, secondary battery, battery module, battery pack, and electric device
CN115820064A