Heterostructure and preparation method therefor
By forming a warped defect layer and a control layer in a heterogeneous integration technology, the problem of low bond strength caused by ion implantation is solved, and higher bond strength and diffusion ability are achieved.
Patent Information
- Application Number
- PCT/CN2023/131844
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2023-11-15
- Publication Date
- 2024-12-05
AI Technical Summary
In heterogeneous integration technology, ion implantation causes wafer warping, resulting in difficult diffusion of bonding waves and low bonding strength.
By forming a warped defect layer and a control layer on a single crystal functional material substrate and a heterogeneous substrate substrate, the bonding gap is reduced, the diffusion ability of the bonding wave is enhanced, and the first and second ion implantation and dielectric deposition are adopted. The process forms a warp control layer and adjusts the warp state differences to meet preset conditions.
The bonding strength of the heterostructure and the diffusion ability of the bonding wave are enhanced, the area and strength of the bonding area are improved, and the problems of bonding difficulty and cost are solved.
Smart Images

Figure CN2023131844_05122024_PF_FP_ABST
Abstract
Description
A heterogeneous structure and preparation method thereof Technical Field
[0001] The present invention relates to the technical field of heterogeneous integration, and in particular to a heterogeneous structure and a preparation method thereof. Background Art
[0002] In the field of heterogeneous integration, heterogeneous integration of multiple materials on semiconductor materials with a single function to form heterojunctions or heterointerfaces with multiple functions can yield high-performance devices with higher power, higher frequency or higher speed. This is an important development direction of heterogeneous integration technology at this stage and will open up a new path for the future development of microelectronics technology.
[0003] Ion-cutting heterogeneous integration technology based on ion implantation can peel high-quality single-crystal thin films from any single-crystal wafer through ion implantation and combine them with a heterogeneous substrate wafer through bonding. However, since ion implantation can cause wafer warping, a large gap will exist between the ion-implanted wafer and the substrate wafer during the bonding process, making it difficult for the bonding wave to diffuse and resulting in low bonding strength.
[0004] Summary of the Invention
[0005] The present application provides a method for preparing a heterostructure, by causing both the heterogeneous substrate substrate and the single crystal functional material substrate to warp, so as to reduce the bonding gap between the heterogeneous substrate substrate and the single crystal functional material substrate, thereby enhancing the diffusion ability of the bonding wave and thus enhancing the bonding strength.
[0006] In one aspect, the present application provides a method for preparing a heterostructure, comprising:
[0007] Provide single crystal functional material substrates and heterogeneous substrates;
[0008] Performing a first ion implantation on the single crystal functional material substrate to form a first defect layer, wherein the single crystal functional material substrate having the first defect layer is in a warped state;
[0009] Performing a warpage control process on the foreign substrate to form a warpage control layer, wherein the foreign substrate on which the warpage control layer is formed is in a warped state;
[0010] Bonding a single crystal functional material substrate forming the first defect layer and a heterogeneous substrate forming the warpage control layer to obtain a heterogeneous bonded body;
[0011] The heterogeneous bonded body is peeled off to obtain a target heterostructure.
[0012] Furthermore, a difference in warping state between the foreign substrate forming the warp regulating layer and the single crystal functional material substrate forming the first defect layer satisfies a preset difference condition.
[0013] Furthermore, the performing warpage control treatment on the foreign substrate to form a warpage control layer includes:
[0014] Acquiring warping state data of the single crystal functional material substrate forming the first defect layer;
[0015] performing a warpage control process on the foreign substrate, and monitoring warpage state data of the foreign substrate during the warpage control process;
[0016] Taking the warping state data of the single crystal functional material substrate forming the first defect layer as the warping state target, adjust the warping processing condition parameters of the heterogeneous substrate until the warping state difference between the heterogeneous substrate and the single crystal functional material substrate forming the first defect layer meets the preset difference condition, thereby forming the warping control layer.
[0017] Furthermore, the foreign substrate includes a first surface and a second surface arranged opposite to each other, the first surface being used for bonding with a single crystal functional material substrate forming the first defect layer; and the warpage control layer is prepared by:
[0018] A second ion implantation is performed on the second surface of the foreign substrate to form a second defect layer serving as the warpage regulating layer.
[0019] Furthermore, the foreign substrate includes a first surface and a second surface arranged opposite to each other, the first surface being used for bonding with a single crystal functional material substrate forming the first defect layer; and the warpage control layer is prepared by:
[0020] performing a dielectric deposition process on the first surface of the foreign substrate to form a stress regulating dielectric layer serving as the warpage regulating layer;
[0021] The medium deposited by the medium deposition process can generate thermal mismatch with the foreign substrate.
[0022] Furthermore, the thermal expansion coefficient of the medium deposited by the medium deposition process is different from the thermal expansion coefficient of the foreign substrate.
[0023] Furthermore, the implanted ions in the first ion implantation include at least one of hydrogen ions and rare gas ions.
[0024] Furthermore, the implanted ions of the second ion implantation include one or more of hydrogen ions, rare gas ions, nitrogen ions, phosphorus ions, oxygen ions and boron ions.
[0025] Furthermore, the single crystal functional material substrate is a silicon substrate, an indium phosphide substrate, a gallium arsenide substrate, a gallium nitride substrate, a silicon carbide substrate, a gallium oxide substrate or a diamond substrate.
[0026] Furthermore, the foreign substrate is a silicon carbide substrate, a diamond substrate, a barium sulfide substrate or a silicon substrate.
[0027] Furthermore, during the first ion implantation process, the preparation method satisfies at least one of the following characteristics:
[0028] The energy range of the first ion implanted is 50keV-10mev;
[0029] The dose of the first ion implantation is 1×10 16 / cm 2 -1×10 18 / cm 2 ;
[0030] The temperature for implanting the first ions is -20°C to 200°C.
[0031] Furthermore, during the second ion implantation process, the preparation method satisfies at least one of the following characteristics:
[0032] The energy range of the second ion implanted is 50keV-10mev;
[0033] The dose of the second ion implantation is 1×10 13 / cm 2 -1×10 18 / cm 2 ;
[0034] The temperature for implanting the second ions is -20°C to 200°C.
[0035] Furthermore, the medium deposited by the medium deposition process is one or more of aluminum oxide medium, silicon dioxide medium, aluminum nitride medium, silicon nitride medium or hafnium dioxide medium.
[0036] Furthermore, during the dielectric deposition process, the preparation method satisfies at least one of the following characteristics:
[0037] The dielectric deposition temperature is 200℃-500℃;
[0038] The dielectric deposition thickness is 2nm-500nm.
[0039] Furthermore, the target heterostructure has a functional material thin film layer, and the thickness of the functional material thin film layer is 30nm-20000nm.
[0040] Furthermore, the warping state difference refers to the warping difference between the foreign substrate forming the warping control layer and the single crystal functional material substrate forming the first defect layer;
[0041] The preset difference condition is satisfied when the warpage difference is less than or equal to a preset value, and the preset value is 45 μm-50 μm.
[0042] On the other hand, the present application provides a heterostructure, which is prepared using the heterostructure preparation method described above.
[0043] The present application provides a method for preparing a heterogeneous structure, which has the following beneficial effects:
[0044] The heterostructure preparation method of the present application includes providing a single crystal functional material substrate and a heterogeneous substrate substrate; performing a first ion implantation on the single crystal functional material substrate to form a first defect layer, the single crystal functional material substrate forming the first defect layer is in a warped state; performing a warping control treatment on the heterogeneous substrate substrate to form a warping control layer, the heterogeneous substrate substrate forming the warping control layer is in a warped state; bonding the single crystal functional material substrate forming the first defect layer and the heterogeneous substrate substrate forming the warping control layer to obtain a heterogeneous bonded body; peeling the heterogeneous bonded body to obtain a target heterostructure. The heterostructure preparation method of the present application forms a first defect layer in the single crystal functional material substrate and a warping control layer in the heterogeneous substrate substrate, so that both the heterogeneous substrate substrate and the single crystal functional material substrate are warped. In this way, the bonding gap between the heterogeneous substrate substrate and the single crystal functional material substrate can be reduced, thereby enhancing the diffusion ability of the bonding wave and thereby enhancing the bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the technical solutions and advantages of the embodiments of the present application or the prior art, the following is a brief introduction to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0046] FIG1 is a schematic diagram of a process for preparing a heterostructure according to an embodiment of the present application;
[0047] FIG2 is a schematic diagram of a process for forming a warpage control layer according to an embodiment of the present application;
[0048] FIG3 is a schematic diagram of a specific process of a method for preparing a heterostructure provided in an embodiment of the present application;
[0049] FIG4 is a schematic diagram of a specific process of another method for preparing a heterostructure provided in an embodiment of the present application;
[0050] FIG5 is a schematic structural diagram of a single crystal functional material substrate provided in an embodiment of the present application;
[0051] FIG6 is a schematic structural diagram of a heterogeneous substrate provided in an embodiment of the present application;
[0052] FIG7 is a schematic structural diagram of a single crystal functional material substrate with a first defect layer formed thereon, provided in an embodiment of the present application;
[0053] FIG8 is a schematic structural diagram of a heterogeneous substrate substrate on which a second defect layer is formed, provided in an embodiment of the present application;
[0054] FIG9 is a schematic structural diagram of a heterogeneous bonded body provided in an embodiment of the present application;
[0055] FIG10 is a schematic structural diagram of a target heterostructure provided in an embodiment of the present application;
[0056] FIG11 is a schematic structural diagram of a heterogeneous substrate on which a stress regulating dielectric layer is formed, provided in an embodiment of the present application;
[0057] FIG12 is a schematic structural diagram of another heterogeneous bonded body provided in an embodiment of the present application;
[0058] FIG13 is a schematic structural diagram of another target heterostructure provided in an embodiment of the present application.
[0059] The following is a supplementary explanation of the accompanying drawings: 1-single crystal functional material substrate; 2-heterogeneous substrate substrate; 21-first surface; 22-second surface; 10-single crystal functional material substrate layer; 101-functional material thin film layer; 20-heterogeneous substrate substrate layer; 201-heterogeneous substrate layer; 30-first defect layer; 40-second defect layer; 50-stress regulation dielectric layer. DETAILED DESCRIPTION
[0060] The following will be combined with the accompanying drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0061] For the following defined terms, these definitions shall apply unless a different definition is given in the claims or elsewhere in this specification. All numerical values, whether or not explicitly indicated, are defined herein as being modified by the term "about". The term "about" generally refers to a numerical range that one of ordinary skill in the art would consider equivalent to the stated value to produce substantially the same properties, functions, results, etc. A numerical range indicated by a lower value and an upper value is defined to include all numerical values included in the numerical range and all subranges included in the numerical range.
[0062] It should be noted that the terms "first," "second," and the like in the specification and claims of this application and the accompanying drawings are used to distinguish similar objects and are not necessarily used to describe a particular order or precedence. It should be understood that the terms used in this manner are interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including," "having," and any variations thereof are intended to cover non-exclusive inclusions.
[0063] The following describes the heterostructure preparation method provided in the embodiments of the present application. Please refer to Figures 1-4, which are flow charts of the heterostructure preparation method. This specification provides the method operation steps as described in the embodiments or flow charts, but more or fewer operation steps may be included based on conventional or non-creative labor. The order of steps listed in the embodiments is only one way of executing the order of many steps and does not represent the only execution order. When the preparation method is actually executed, it can be executed in the order of the methods shown in the embodiments or the accompanying drawings or in parallel. The heterostructure preparation method provided in the embodiments of the present application includes:
[0064] S101. Provide a single crystal functional material substrate 1 and a heterogeneous substrate substrate 2.
[0065] In some embodiments, referring to FIG5 , the single crystal functional material substrate 1 may be a silicon substrate, an indium phosphide substrate, a gallium arsenide substrate, a gallium nitride substrate, a silicon carbide substrate, a gallium oxide substrate or a diamond substrate; illustratively, the single crystal functional material substrate 1 may be a 2-12 inch wafer.
[0066] In some embodiments, referring to FIG. 6 , the foreign substrate 2 may be a silicon carbide substrate, a diamond substrate, a barium sulfide substrate, or a silicon substrate; illustratively, the foreign substrate 2 may be a 2-12 inch wafer.
[0067] It should be noted that the single crystal functional material substrate 1 and the heterogeneous substrate 2 are made of different materials.
[0068] S102. Referring to FIG. 7 , a first ion implantation is performed on the single-crystal functional material substrate 1 to form a first defect layer 30. The single-crystal functional material substrate 1 having the first defect layer 30 is in a warped state.
[0069] In some embodiments, the single crystal functional material substrate 1 has a bonding surface for bonding to a foreign substrate 2; first ions are injected into the bonding surface of the single crystal functional material substrate 1 to form a first defect layer 30, see Figure 7, the direction of the arrow in Figure 7 is the direction of the first ion injection.
[0070] Specifically, due to the implantation of the first ions, the single-crystal functional material substrate 1 may be warped, and the single-crystal functional material substrate 1 forming the first defect layer 30 is in a warped state.
[0071] In some embodiments, the implanted ions of the first ion implantation include at least one of hydrogen ions and rare gas ions; in this way, the effect of the first ion implantation and the stripping effect of the first defect layer 30 during the annealing process can be ensured.
[0072] In some embodiments, the parameters of the first ion implantation include: the energy of the first ion beam for forming the first defect layer 30 may be 50kev-10000kev, the dose of the first ion implantation may be 1×10 16 / cm 2 -1×10 18 / cm 2 The temperature for injecting the first ions is -20°C-200°C; in this way, the effect of the first ion implantation and the stripping effect of the first defect layer 30 during the annealing process can be guaranteed.
[0073] The upper limit of the first ion beam energy may be 10000kev, 9800kev, 9700kev, etc., and the lower limit of the first ion beam energy may be 50kev, 60kev, 70kev, etc. It is understood that the first ion beam energy may be any value within the above range, which is not enumerated here.
[0074] The upper limit of the temperature for injecting the first ions may be 200° C., 190° C., 180° C., etc., and the lower limit of the temperature for injecting the first ions may be -20° C., -15° C., -10° C., etc. It is understood that the temperature for injecting the first ions may be any value within the above range, which is not enumerated here.
[0075] The greater the relative atomic mass of the first ions to be implanted, the greater the ion beam energy required for the implantation.
[0076] Specifically, by controlling the energy and dosage of the first ion beam during the first ion implantation process, the first defect layer 30 can be stripped during the annealing process.
[0077] S103 . Referring to FIG. 8 and FIG. 11 , a warpage control process is performed on the foreign substrate 2 to form a warpage control layer. The foreign substrate 2 with the warpage control layer is in a warped state.
[0078] In the embodiment of the present application, S103 includes:
[0079] S201 . Obtain warping state data of the single crystal functional material substrate 1 on which the first defect layer 30 is formed.
[0080] In some embodiments, warping state data of the single crystal functional material substrate 1 forming the first defect layer 30 is detected based on a warping detection device; wherein the warping state data includes a warping degree.
[0081] S202 . Perform a warpage control process on the foreign substrate 2 , and monitor the warpage state data of the foreign substrate 2 during the warpage control process.
[0082] In some embodiments, during the warpage control process of the foreign substrate 2 , the warpage state data of the foreign substrate 2 may be continuously acquired based on a preset time interval.
[0083] Among them, the method for obtaining the warping state data of the heterogeneous substrate substrate 2 can be the same as the method for obtaining the warping state data of the single crystal functional material substrate 1 that forms the first defect layer 30, that is, based on the warping detection equipment, the current warping state data of the heterogeneous substrate substrate 2 is detected.
[0084] The current warping state data includes the current warping degree.
[0085] S203. Taking the warping state data of the single crystal functional material substrate 1 forming the first defect layer 30 as the warping state target, adjust the warping processing condition parameters of the heterogeneous substrate 2 until the warping state difference between the heterogeneous substrate 2 and the single crystal functional material substrate 1 forming the first defect layer 30 meets the preset difference condition, thereby forming a warping control layer.
[0086] In this way, by using the warping state data of the single crystal functional material substrate 1 as the warping state target, monitoring and regulating the warping state of the heterogeneous substrate 2 can improve the efficiency of warping regulation of the heterogeneous substrate 2, thereby improving the preparation efficiency of the heterogeneous structure.
[0087] In some embodiments, by adjusting the warping processing condition parameters of the foreign substrate 2 , the warping of the foreign substrate 2 can be controlled, that is, the warping state data of the foreign substrate 2 can be changed.
[0088] In some embodiments, the warping state difference refers to the warping difference between the heterogeneous substrate 2 forming the warping control layer and the single crystal functional material substrate 1 forming the first defect layer 30; the preset difference condition is met when the warping difference is less than or equal to a preset value.
[0089] The preset value may be 45 μm-50 μm.
[0090] In some specific embodiments, during the warping control process of the heterogeneous substrate 2, the warping of the single crystal functional material substrate 1 forming the first defect layer 30 is taken as the warping state target, and the warping processing condition parameters of the heterogeneous substrate 2 are adjusted to change the warping of the heterogeneous substrate 2 so that the difference between the warping of the heterogeneous substrate 2 and the warping of the single crystal functional material substrate 1 forming the first defect layer 30 is less than or equal to a preset value; in this way, not only can the bonding area be increased, the diffusion ability of the bonding wave be enhanced, and the bonding strength be increased, but also the bonding difficulty and cost can be reduced to a certain extent.
[0091] In some embodiments, the warpage difference can indicate the situation of the bonding gap between the heterogeneous substrate substrate 2 forming the warpage regulation layer and the single crystal functional material substrate 1 forming the first defect layer 30; specifically, the larger the absolute value of the warpage difference, the larger the bonding gap between the heterogeneous substrate substrate 2 forming the warpage regulation layer and the single crystal functional material substrate 1 forming the first defect layer 30, and correspondingly, the smaller the absolute value of the warpage difference, the smaller the bonding gap between the heterogeneous substrate substrate 2 forming the warpage regulation layer and the single crystal functional material substrate 1 forming the first defect layer 30.
[0092] In the embodiment of the present application, please refer to Figures 6 and 8. The heterogeneous substrate base plate 2 includes a first surface 21 and a second surface 22 arranged opposite to each other, and the first surface 21 is used to bond with the single crystal functional material substrate 1 that forms the first defect layer 30; the warping control layer includes being prepared by the following method: performing a second ion implantation on the second surface 22 of the heterogeneous substrate base plate 2 to form a second defect layer 40 serving as the warping control layer.
[0093] In some embodiments, see FIG8 , second ions are implanted into the second surface 22 of the foreign substrate 2 to form a second defect layer 40 that can serve as a warpage regulating layer; see FIG8 , the arrow direction in FIG8 is the direction of the second ion implantation.
[0094] Specifically, due to the implantation of the second ions, the foreign substrate 2 may be warped, and the foreign substrate 2 forming the second defect layer 40 is in a warped state.
[0095] In some embodiments, the implanted ions of the second ion implantation include one or more of hydrogen ions, rare gas ions, nitrogen ions, phosphorus ions, oxygen ions and boron ions; in this way, the effect of the first ion implantation and the stripping effect of the first defect layer 30 during the annealing process can be guaranteed.
[0096] In some embodiments, the condition parameters of the second ion implantation include: the energy of the second ion beam for forming the second defect layer 40 may be 50kev-10000kev, the dose of the second ion implantation may be 1×10 13 / cm 2 -1×10 18 / cm 2 The temperature for injecting the second ions is -20°C-200°C; in this way, the effect of the first ion implantation and the stripping effect of the first defective layer 30 during the annealing process can be guaranteed.
[0097] The upper limit of the second ion beam energy may be 10000kev, 9800kev, 9700kev, etc., and the lower limit of the second ion beam energy may be 50kev, 60kev, 70kev, etc. It is understood that the second ion beam energy may be any value within the above range, which is not enumerated here.
[0098] The upper limit of the temperature for injecting the second ions may be 200° C., 190° C., 180° C., etc., and the lower limit of the temperature for injecting the second ions may be -20° C., -15° C., -10° C., etc. It is understood that the temperature for injecting the second ions may be any value within the above range, which is not enumerated here.
[0099] The greater the relative atomic mass of the implanted second ions, the greater the ion beam energy required for the implantation.
[0100] Specifically, by controlling the energy and dosage of the second ion beam during the second ion implantation process, the second defect layer 40 can be stripped during the annealing process.
[0101] In some embodiments, when the second defect layer 40 serves as a warping control layer, the warping processing condition parameters may include one or more of the second ion beam energy, the dose of the second ions injected, and the temperature of the second ions injected; that is, in the process of performing warping control processing on the heterogeneous substrate 2, the warping of the single crystal functional material substrate 1 that forms the first defect layer 30 is taken as the warping state target, and the warping of the heterogeneous substrate 2 is changed by adjusting at least one of the second ion beam energy, the dose of the second ions injected, and the temperature of the second ions injected, so that the difference between the warping of the heterogeneous substrate 2 and the warping of the single crystal functional material substrate 1 that forms the first defect layer 30 is less than or equal to a preset value; in this way, through the warping control of the second defect layer 40, the difference in the warping between the heterogeneous substrate 2 and the single crystal functional material substrate 1 is less than or equal to the preset value, which can reduce the bonding gap between the heterogeneous substrate 2 and the single crystal functional material substrate 1, thereby enhancing the diffusion ability of the bonding wave and increasing the bonding strength.
[0102] For example, compared with the warping of the single crystal functional material substrate 1 that forms the first defect layer 30, when the warping of the heterogeneous substrate 2 is smaller and the warping difference is greater than a preset value, the implantation dose of the second ion can be adjusted to increase the warping of the heterogeneous substrate 2 until the warping difference is less than or equal to the preset value.
[0103] In some other embodiments, referring to FIG. 11 , the warpage control layer is prepared by: performing a dielectric deposition process on the first surface 21 of the heterogeneous substrate 2 to form a stress control dielectric layer 50 serving as the warpage control layer; wherein the dielectric deposited by the dielectric deposition process can produce a thermal mismatch with the heterogeneous substrate 2.
[0104] In some embodiments, referring to FIG. 11 , a dielectric is deposited onto the first surface 21 of the foreign substrate 2 to form a stress regulating dielectric layer 50 that can serve as a warpage regulating layer.
[0105] Specifically, due to dielectric deposition, the foreign substrate 2 may be warped, and the foreign substrate 2 forming the stress regulating dielectric layer 50 is in a warped state.
[0106] In some embodiments, the medium deposited by the medium deposition process is one or more of aluminum oxide medium, silicon dioxide medium, aluminum nitride medium, silicon nitride medium or hafnium dioxide medium; in this way, the warpage control effect on the heterogeneous substrate 2 can be ensured.
[0107] In some embodiments, the condition parameters of the dielectric deposition process include: a dielectric deposition temperature of 200° C.-500° C., and a dielectric deposition thickness of 2 nm-500 nm; in this way, the warpage control effect on the heterogeneous substrate 2 can be ensured.
[0108] The upper limit of the dielectric deposition temperature may be 500° C., 480° C., 460° C., etc., and the lower limit of the dielectric deposition temperature may be 200° C., 230° C., 260° C., etc. It is understood that the dielectric deposition temperature may be any value within the above range, which is not enumerated here.
[0109] The upper limit of the dielectric deposition thickness may be 500 nm, 480 nm, 460 nm, etc., and the lower limit of the dielectric deposition thickness may be 2 nm, 5 nm, 8 nm, etc. It is understood that the dielectric deposition thickness may be any value within the above range, which is not enumerated here.
[0110] In some embodiments, when the stress-regulating dielectric layer 50 serves as the warpage regulating layer, the warpage processing condition parameters may include at least one of the dielectric deposition temperature and the dielectric deposition thickness; that is, in the process of performing warpage regulation processing on the heterogeneous substrate 2, the warpage of the single-crystal functional material substrate 1 forming the first defect layer 30 is taken as the warpage state target, and the warpage of the heterogeneous substrate 2 is changed by adjusting at least one of the dielectric deposition temperature and the dielectric deposition thickness, so that the difference between the warpage of the heterogeneous substrate 2 and the warpage of the single-crystal functional material substrate 1 forming the first defect layer 30 is less than or equal to a preset value; in this way, through the warpage regulation of the stress-regulating dielectric layer 50, the difference between the warpage of the heterogeneous substrate 2 and the single-crystal functional material substrate 1 is less than or equal to the preset value, which can reduce the bonding gap between the heterogeneous substrate 2 and the single-crystal functional material substrate 1, thereby enhancing the diffusion ability of the bonding wave and increasing the bonding strength.
[0111] For example, compared with the warping of the single crystal functional material substrate 1 that forms the first defect layer 30, when the warping of the heterogeneous substrate 2 is smaller and the warping difference is greater than a preset value, the dielectric deposition thickness can be adjusted to increase the warping of the heterogeneous substrate 2 until the warping difference is less than or equal to the preset value.
[0112] Furthermore, the thermal expansion coefficient of the medium deposited by the medium deposition process is different from the thermal expansion coefficient of the foreign substrate 2 .
[0113] In some embodiments, since the thermal expansion coefficient of the medium deposited by the medium deposition process is different from the thermal expansion coefficient of the heterogeneous substrate 2, during the high-temperature medium deposition process, the medium deposited by the medium deposition process is thermally mismatched with the heterogeneous substrate 2, that is, the medium deposited by the medium deposition process and the heterogeneous substrate 2 produce different degrees of expansion. In this way, the heterogeneous substrate 2 can be warped, and the heterogeneous substrate 2 forming the stress regulation medium layer 50 is in a warped state.
[0114] S104. Referring to FIG. 9 and FIG. 12 , the single crystal functional material substrate 1 forming the first defect layer 30 and the heterogeneous substrate 2 forming the warpage control layer are bonded to obtain a heterogeneous bonded body.
[0115] In some embodiments, when the difference in warping state between the heterogeneous substrate substrate 2 forming the warping regulation layer and the single crystal functional material substrate 1 forming the first defect layer 30 meets a preset difference condition, the single crystal functional material substrate 1 forming the first defect layer 30 and the heterogeneous substrate substrate 2 forming the warping regulation layer are bonded to obtain a heterogeneous bonded body.
[0116] In some embodiments, please refer to Figure 9, a single crystal functional material substrate 1 that forms the first defect layer 30 and a heterogeneous substrate substrate 2 that forms the second defect layer 40 are bonded to obtain a heterogeneous bonded body including a single crystal functional material substrate layer 10 that forms the first defect layer 30 and a heterogeneous substrate substrate layer 20 that forms the second defect layer 40.
[0117] In some other embodiments, please refer to Figure 12, a single crystal functional material substrate 1 that forms the first defect layer 30 and a heterogeneous substrate substrate 2 that forms the stress regulation medium layer 50 are bonded to obtain a heterogeneous bonded body including a single crystal functional material substrate layer 10 that forms the first defect layer 30 and a heterogeneous substrate substrate layer 20 that forms the stress regulation medium layer 50.
[0118] In some embodiments, the bonding method of the single crystal functional material substrate 1 forming the first defect layer 30 and the heterogeneous substrate substrate 2 forming the warp regulation layer includes but is not limited to hydrophilic bonding, room temperature vacuum activation bonding and anodic bonding; the activation gas can be one or more of argon, nitrogen and oxygen, the activation time can be 10s-540s, and the activation power can be 50W-1000W.
[0119] Among them, the upper limit of the activation time can be 540s, 520s, 480s, etc., and the lower limit of the activation time can be 10s, 15s, 20s, etc. It is understandable that the activation time can be any point value within the above range, which is not enumerated here.
[0120] Among them, the upper limit power of the activation power can be 1000W, 960W, 920W, etc., and the lower limit power of the activation power can be 50W, 55W, 60W, etc. It is understandable that the activation power can be any point value within the above range, which is not enumerated here.
[0121] S105. Please refer to Figures 10 and 13, the heterogeneous bonded body is peeled off to obtain the target heterostructure.
[0122] In some embodiments, please refer to Figure 9, when the second defect layer 40 serves as the warping regulation layer, the heterogeneous bonded body is annealed and peeled, so that the single crystal functional material substrate layer 10 is peeled along the first defect layer 30 to form a functional material thin film layer 101 having a first preset thickness, and the heterogeneous substrate substrate layer 20 is peeled along the second defect layer 40 to form a heterogeneous substrate layer 201 having a second preset thickness, thereby obtaining a target heterostructure including a functional material thin film layer 101 and a heterogeneous substrate layer 201, please refer to Figure 10.
[0123] In the embodiment of the present application, the first preset thickness of the functional material thin film layer 101 is 30 nm-20000 nm. This can increase the applicable scope of the target heterostructure and broaden the use scenarios of the target heterostructure.
[0124] The upper limit of the first preset thickness of the functional material thin film layer 101 may be 20,000 nm, 19,500 nm, 19,000 nm, etc., and the lower limit of the first preset thickness of the functional material thin film layer 101 may be 30 nm, 35 nm, 40 nm, etc. It is understood that the first preset thickness of the functional material thin film layer 101 may be any value within the above range, which is not enumerated here.
[0125] The annealing conditions for annealing and peeling the heterogeneous bonded body may be at least one of nitrogen and hydrogen, and the annealing temperature may be 50° C.-400° C.
[0126] The upper limit of the annealing temperature may be 400° C., 380° C., 360° C., etc., and the lower limit of the annealing temperature may be 50° C., 70° C., 90° C., etc. It is understood that the annealing temperature may be any point within the above range, which is not enumerated here.
[0127] Specifically, the depth of the first defect layer 30 directly affects the thickness of the functional material thin film layer 101. The smaller the distance between the first defect layer 30 and the bonding surface of the single crystal functional material substrate 1, the smaller the thickness of the prepared functional material thin film layer 101.
[0128] Accordingly, the depth of the second defect layer 40 directly affects the thickness of the foreign substrate layer 201 . The smaller the distance between the second defect layer 40 and the second surface 22 of the foreign substrate 2 , the thicker the prepared foreign substrate layer 201 .
[0129] Specifically, during the annealing and peeling process of the hetero-bonded body in FIG. 9 , the annealing treatment can release the stress and warping of the hetero-bonded body, so that a flat target hetero-structure can be obtained, as shown in FIG. 10 .
[0130] It is understandable that in an application scenario where a flat target heterostructure is required, the second defect layer 40 can be selected as the warpage regulating layer.
[0131] In some other embodiments, please refer to Figure 12. When the stress regulation dielectric layer 50 serves as the warp regulation layer, the heterogeneous bonded body is annealed and peeled so that the single crystal functional material substrate layer 10 is peeled along the first defect layer 30 to form a functional material thin film layer 101 having a first preset thickness, thereby obtaining a target heterostructure including the functional material thin film layer 101, the stress regulation dielectric layer 50 and the heterogeneous substrate substrate layer 20, see Figure 13.
[0132] The annealing conditions for annealing and peeling the heterogeneous bonded body may be at least one of nitrogen and hydrogen, and the annealing temperature may be 50° C.-400° C.
[0133] The upper limit of the annealing temperature may be 400° C., 380° C., 360° C., etc., and the lower limit of the annealing temperature may be 50° C., 70° C., 90° C., etc. It is understood that the annealing temperature may be any point within the above range, which is not enumerated here.
[0134] Specifically, during the annealing and peeling process of the heterojunction body in FIG12 , due to the presence of the stress regulating dielectric layer 50 , the annealing treatment cannot release the stress and warping of the heterojunction body to make the target heterojunction structure flat. In this way, a warped target heterojunction structure can be obtained, as shown in FIG13 .
[0135] It is understandable that in an application scenario where a target heterostructure needs to be warped, the stress-regulating dielectric layer 50 can be selected as the warping-regulating layer.
[0136] The heterostructure preparation method provided in the embodiments of the present application has the following beneficial effects:
[0137] 1. By forming a first defect layer in a single-crystal functional material substrate and a second defect layer in a heterogeneous substrate, the difference in warping state between the heterogeneous substrate forming the second defect layer and the single-crystal functional material substrate forming the first defect layer meets a preset difference condition. In this way, the bonding gap between the heterogeneous substrate and the single-crystal functional material substrate can be reduced, thereby enhancing the diffusion ability of the bonding wave, increasing the area of the bonding region, and thereby enhancing the bonding strength, thereby obtaining a flat target heterostructure.
[0138] 2. By forming a first defect layer in a single-crystal functional material substrate and forming a stress-regulating dielectric layer in a heterogeneous substrate, the difference in warping state between the heterogeneous substrate forming the stress-regulating dielectric layer and the single-crystal functional material substrate forming the first defect layer meets a preset difference condition. In this way, the bonding gap between the heterogeneous substrate and the single-crystal functional material substrate can be reduced, thereby enhancing the diffusion ability of the bonding wave, increasing the area of the bonding region, and thereby enhancing the bonding strength, thereby obtaining a warped target heterostructure.
[0139] 3 and 5-10 , the following describes specific embodiments of the present application in combination with the above-mentioned heterostructure preparation method. Examples 1-9 use the following method to prepare the target heterostructure:
[0140] S11. Provide a single crystal functional material substrate 1 and a heterogeneous substrate substrate 2.
[0141] S12. Perform a first ion implantation on the single crystal functional material substrate 1 to form a first defect layer 30. The single crystal functional material substrate 1 with the first defect layer 30 is in a warped state.
[0142] The implanted ions of the first ion implantation may be hydrogen ions, the first ion beam energy for forming the first defect layer 30 may be E1, the dose of the first ion implantation may be A1, and the temperature for implanting the first ions may be T1.
[0143] S13 . Obtain warping state data of the single-crystal functional material substrate 1 on which the first defect layer 30 is formed.
[0144] Wherein, based on the warpage detection equipment, the warpage state data of the single crystal functional material substrate 1 forming the first defect layer 30 is detected; the warpage state data includes the warpage degree.
[0145] S14 . Perform a second ion implantation on the foreign substrate 2 to control the warping of the foreign substrate 2 , and monitor the warping state data of the foreign substrate 2 during the warping control process.
[0146] Among them, second ions are implanted into the second surface 22 of the foreign substrate 2; the implanted ions of the second ion implantation may be nitrogen ions, the second ion beam energy for forming the second defect layer 40 may be E2, the dose of the implanted second ions may be A2, and the temperature for implanting the second ions may be T2.
[0147] Wherein, based on the warpage detection equipment, the current warpage state data of the foreign substrate base plate 2 is detected; the warpage state data includes the warpage degree.
[0148] S15. Taking the warping state data of the single crystal functional material substrate 1 forming the first defect layer 30 as the warping state target, adjust at least one of the second ion beam energy, the dose of the second ions injected, and the temperature of the second ions injected, until the warping state difference between the heterogeneous substrate 2 and the single crystal functional material substrate 1 forming the first defect layer 30 meets the preset difference condition, thereby forming the second defect layer 40.
[0149] Among them, the warping state difference refers to the warping difference between the heterogeneous substrate 2 forming the second defect layer 40 and the single crystal functional material substrate 1 forming the first defect layer 30; the preset difference condition is met when the warping difference is less than or equal to the preset value.
[0150] The preset value may be 45 μm-50 μm.
[0151] S16. Bond the single crystal functional material substrate 1 forming the first defect layer 30 and the heterogeneous substrate 2 forming the second defect layer 40 to obtain a heterogeneous bonded body.
[0152] The heterogeneous bonded body includes a single crystal functional material substrate layer 10 forming a first defect layer 30 and a heterogeneous substrate substrate layer 20 forming a second defect layer 40 .
[0153] The bonding method may be hydrophilic bonding, the activation time may be t, and the activation power may be P.
[0154] S17. Peel off the heterogeneous bonded body to obtain the target heterostructure.
[0155] During the annealing and peeling process, the single crystal functional material substrate layer 10 is peeled off along the first defect layer 30 to form a functional material thin film layer 101 with a first preset thickness, and the heterogeneous substrate substrate layer 20 is peeled off along the second defect layer 40 to form a heterogeneous substrate layer 201 with a second preset thickness, thereby obtaining a flat target heterostructure including the functional material thin film layer 101 and the heterogeneous substrate layer 201.
[0156] The thickness of the functional material thin film layer 101 is δ1.
[0157] The annealing condition for the annealing stripping may be nitrogen, and the annealing temperature may be T3.
[0158] The relevant parameters of Examples 1-9 are detailed in Table 1.
[0159] Table 1
[0160] Referring to Figures 4-7 and 11-13, other specific embodiments of the present application are described below in combination with the above-mentioned heterostructure preparation method. Examples 10-18 use the following method to prepare the target heterostructure:
[0161] S21. Provide a single crystal functional material substrate 1 and a heterogeneous substrate substrate 2.
[0162] S22. Perform a first ion implantation on the single crystal functional material substrate 1 to form a first defect layer 30. The single crystal functional material substrate 1 with the first defect layer 30 is in a warped state.
[0163] The implanted ions of the first ion implantation may be helium ions, the first ion beam energy for forming the first defect layer 30 may be E1, the dose of the first ion implantation may be A1, and the temperature for implanting the first ions may be T1.
[0164] S23 . Obtain warping state data of the single-crystal functional material substrate 1 on which the first defect layer 30 is formed.
[0165] Wherein, based on the warpage detection equipment, the warpage state data of the single crystal functional material substrate 1 forming the first defect layer 30 is detected; the warpage state data includes the warpage degree.
[0166] S24. Perform dielectric deposition processing on the foreign substrate 2 to control the warping of the foreign substrate 2, and monitor the warping state data of the foreign substrate 2 during the warping control processing.
[0167] The medium is deposited on the first surface 21 of the foreign substrate 2; the medium deposition temperature is T4, and the medium deposition thickness is δ2.
[0168] Wherein, based on the warpage detection equipment, the current warpage state data of the foreign substrate base plate 2 is detected; the warpage state data includes the warpage degree.
[0169] S25. Taking the warping state data of the single crystal functional material substrate 1 forming the first defect layer 30 as the warping state target, adjust at least one of the dielectric deposition temperature and the dielectric deposition thickness until the warping state difference between the heterogeneous substrate 2 and the single crystal functional material substrate 1 forming the first defect layer 30 meets the preset difference condition, thereby forming a stress-regulating dielectric layer 50.
[0170] Among them, the warping state difference refers to the warping difference between the heterogeneous substrate 2 forming the stress regulation medium layer 50 and the single crystal functional material substrate 1 forming the first defect layer 30; the preset difference condition is met when the warping difference is less than or equal to the preset value.
[0171] The preset value may be 45 μm-50 μm.
[0172] S26. Bond the single crystal functional material substrate 1 forming the first defect layer 30 and the heterogeneous substrate 2 forming the stress regulation dielectric layer 50 to obtain a heterogeneous bonded body.
[0173] The heterogeneous bonded body includes a single crystal functional material substrate layer 10 forming a first defect layer 30 and a heterogeneous substrate substrate layer 20 forming a stress regulating dielectric layer 50 .
[0174] The bonding method may be anodic bonding, the activation time may be t, and the activation power may be P.
[0175] S27. Peel off the heterogeneous bonded body to obtain the target heterostructure.
[0176] During the annealing and peeling process, the single crystal functional material substrate layer 10 is peeled off along the first defect layer 30 to form a functional material thin film layer 101 with a first preset thickness, thereby obtaining a warped target heterostructure including the functional material thin film layer 101, the stress regulation medium layer 50 and the heterogeneous substrate layer 20.
[0177] The thickness of the functional material thin film layer 101 is δ1.
[0178] The annealing conditions for the annealing stripping may be a mixed gas of nitrogen and hydrogen, and the annealing temperature may be T3.
[0179] The relevant parameters of Examples 10-18 are detailed in Table 2.
[0180] Table 2
[0181] Compared with Examples 1-18, the preparation method of the comparative example does not include warping control treatment of the heterogeneous substrate. The preparation method of the comparative example is as follows: providing a single crystal functional material substrate and a heterogeneous substrate; performing a first ion implantation on the single crystal functional material substrate to form a first defect layer, and the single crystal functional material substrate forming the first defect layer is in a warped state; bonding the single crystal functional material substrate forming the first defect layer and the heterogeneous substrate to obtain a heterogeneous bonded body; peeling the heterogeneous bonded body to obtain the target heterostructure. The single crystal functional material substrate in the comparative example is in a warped state, while the heterogeneous substrate is in a flat state. As a result, the bonding gap between the single crystal functional material substrate in a warped state and the heterogeneous substrate in a flat state is large, and the bonding strength is low.
[0182] The above description fully discloses the specific embodiments of the present invention. It should be noted that any modifications made by those skilled in the art to the specific embodiments of the present invention do not depart from the scope of the claims. Accordingly, the scope of the claims of the present invention is not limited solely to the foregoing specific embodiments.
Claims
1. A method for preparing a heterostructure, characterized in that: The method comprises: Providing a single crystal functional material substrate (1) and a heterogeneous substrate substrate (2); Performing a first ion implantation on the single crystal functional material substrate (1) to form a first defect layer (30), wherein the single crystal functional material substrate (1) on which the first defect layer (30) is formed is in a warped state; Performing a warping control process on the foreign substrate base plate (2) to form a warping control layer, wherein the foreign substrate base plate (2) forming the warping control layer is in a warped state; Bonding a single crystal functional material substrate (1) forming the first defect layer (30) and a heterogeneous substrate substrate (2) forming the warpage regulating layer to obtain a heterogeneous bonded body; The heterogeneous bonded body is peeled off to obtain a target heterogeneous structure.
2. The method for preparing a heterostructure according to claim 1, characterized in that: The difference in warping state between the foreign substrate (2) forming the warping regulating layer and the single crystal functional material substrate (1) forming the first defect layer (30) satisfies a preset difference condition.
3. The method for preparing a heterostructure according to claim 1, characterized in that: The step of performing a warpage control process on the foreign substrate (2) to form a warpage control layer comprises: Acquiring warping state data of the single crystal functional material substrate (1) forming the first defect layer (30); Performing a warping control process on the foreign substrate base plate (2), and during the warping control process, monitoring the warping state data of the foreign substrate base plate (2); Taking the warping state data of the single crystal functional material substrate (1) forming the first defect layer (30) as the warping state target, the warping processing condition parameters of the heterogeneous substrate substrate (2) are adjusted until the warping state difference between the heterogeneous substrate substrate (2) and the single crystal functional material substrate (1) forming the first defect layer (30) meets the preset difference condition, thereby forming the warping control layer.
4. The method for preparing a heterostructure according to claims 1-3, characterized in that: The foreign substrate base plate (2) comprises a first surface (21) and a second surface (22) arranged opposite to each other, wherein the first surface (21) is used for bonding with a single crystal functional material substrate (1) forming the first defect layer (30); The warpage regulating layer is prepared by the following method: A second ion implantation is performed on the second surface (22) of the foreign substrate base (2) to form a second defect layer (40) serving as the warpage regulating layer.
5. The method for preparing a heterostructure according to claims 1-3, characterized in that: The foreign substrate base plate (2) comprises a first surface (21) and a second surface (22) arranged opposite to each other, wherein the first surface (21) is used for bonding with a single crystal functional material substrate (1) forming the first defect layer (30); The warpage regulating layer is prepared by the following method: Performing a dielectric deposition process on the first surface (21) of the foreign substrate base plate (2) to form a stress regulating dielectric layer (50) serving as the warpage regulating layer; The medium deposited by the medium deposition process can produce thermal mismatch with the foreign substrate base plate (2).
6. The method for preparing a heterostructure according to claim 5, characterized in that: The thermal expansion coefficient of the medium deposited by the medium deposition process is different from the thermal expansion coefficient of the foreign substrate base plate (2).
7. The method for preparing a heterostructure according to any one of claims 1 to 3, characterized in that: The implanted ions of the first ion implantation include at least one of hydrogen ions and rare gas ions.
8. The method for preparing a heterostructure according to claim 4, characterized in that: The implanted ions of the second ion implantation include one or more of hydrogen ions, rare gas ions, nitrogen ions, phosphorus ions, oxygen ions and boron ions.
9. The method for preparing a heterostructure according to any one of claims 1 to 3, characterized in that: The single crystal functional material substrate (1) is a silicon substrate, an indium phosphide substrate, a gallium arsenide substrate, a gallium nitride substrate, a silicon carbide substrate, a gallium oxide substrate or a diamond substrate.
10. The method for preparing a heterostructure according to any one of claims 1 to 3, characterized in that: The foreign substrate (2) is a silicon carbide substrate, a diamond substrate, a barium sulfide substrate or a silicon substrate.
11. The method for preparing a heterostructure according to any one of claims 1 to 3, characterized in that: In the first ion implantation process, the preparation method satisfies at least one of the following characteristics: The energy range of the first ion implanted is 50kev-10mev; The dose of the first ion implantation is 1×10 16 / cm 2 -1×10 18 / cm 2 ; The temperature for implanting the first ions is -20°C to 200°C.
12. The method for preparing a heterostructure according to claim 4, characterized in that: In the second ion implantation process, the preparation method satisfies at least one of the following characteristics: The energy range of the second ion implantation is 50kev-10mev; The dose of the second ion implantation is 1×10 13 / cm 2 -1×10 18 / cm 2 ; The temperature for implanting the second ions is -20°C to 200°C.
13. The method for preparing a heterostructure according to claim 5 or 6, characterized in that: The medium deposited by the medium deposition process is one or more of aluminum oxide medium, silicon dioxide medium, aluminum nitride medium, silicon nitride medium or hafnium dioxide medium.
14. The method for preparing a heterostructure according to claim 5 or 6, characterized in that: In the dielectric deposition process, the preparation method satisfies at least one of the following characteristics: The dielectric deposition temperature is 200℃-500℃; The dielectric deposition thickness is 2nm-500nm.
15. The method for preparing a heterostructure according to any one of claims 1 to 3, characterized in that: The target heterostructure has a functional material thin film layer (101), and the thickness of the functional material thin film layer (101) is 30nm-20000nm.
16. The method for preparing a heterostructure according to claim 2 or 3, characterized in that: The warping state difference refers to the difference in warping between the foreign substrate substrate (2) forming the warping control layer and the single crystal functional material substrate (1) forming the first defect layer (30); The preset difference condition is that the warpage difference is less than or equal to a preset value, and the preset value is 45 μm-50 μm.
17. A heterostructure, characterized in that The heterostructure is prepared by the method for preparing the heterostructure according to any one of claims 1 to 16.
Citation Information
Patent Citations
Flexible single crystal thin film preparation method based on stress compensation and flexible single crystal thin film
CN109166792A
Preparation method of silicon-based heterogeneous integrated silicon carbide thin film structure
CN109686656A
Single crystal thin film composite substrate and manufacturing method thereof
CN110828298A
Method for bonding substrate wafer and single crystal piezoelectric wafer and composite single crystal piezoelectric wafer substrate
CN111477543A
Composite heterogeneous integrated semiconductor structure, semiconductor device and preparation method
CN112530855A