Composite current collector, negative electrode sheet, secondary battery, electric device and preparation method
By reasonably matching the characteristics of the support layer and the conductive layer in the composite fluid and improving their ductility coefficient, the problem of poor processability of the composite fluid is solved, high energy density and mechanical strength in the secondary battery are achieved, and the battery is improved Cycle performance and safety.
Patent Information
- Application Number
- PCT/CN2023/133631
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2023-11-23
- Publication Date
- 2024-12-05
AI Technical Summary
The processability of existing composite fluids is poor, which affects its application and promotion in secondary batteries, especially when energy density and safety requirements in the fields of lithium-ion batteries are increased.
By designing a composite fluid that includes an organic support layer and a conductive layer, the elastic modulus is finely adjusted by reasonably matching the thickness, tensile breaking strength, yield strength and elastic modulus of the support layer and conductive layer, and the distribution coefficient α is used to finely adjust the elastic modulus Distribution ensures that the ductile coefficient of the composite fluid collector reaches 150 Pa·m or above, thereby improving its performance in pole sheet processing and battery cycle.
It significantly improves the processability of the composite fluid collection, reduces the problems of pole pieces and cell cracking, improves the cycle performance and safety and reliability of the battery, and has excellent energy density and mechanical strength.
Smart Images

Figure CN2023133631_05122024_PF_FP_ABST
Abstract
Description
Composite current collector, negative electrode sheet, secondary battery, power device and preparation method
[0001] Related applications
[0002] This application claims priority to the Chinese patent application filed on May 29, 2023, with application number CN202310617611X and entitled “Composite current collector, negative electrode sheet, secondary battery, electrical device and preparation method”, the entire text of which is hereby incorporated by reference. Technical Field
[0003] The present application relates to the technical field of secondary batteries, and in particular to a composite current collector, a negative electrode sheet, a secondary battery, an electrical device, and a preparation method. Background Art
[0004] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.
[0005] With the gradual promotion of secondary battery technologies such as lithium-ion batteries in consumer electronics, electric vehicles, and energy storage power stations, the demand for secondary battery energy density is becoming increasingly higher. Composite current collectors, which incorporate a polymer-based support layer on a metal current collector, offer lower density at the same thickness and offer significant advantages in safety and cost. However, the poor processability of composite current collectors has seriously hampered their further application.
[0006] Therefore, it is necessary to further develop new products of composite current collectors.
[0007] Summary of the Invention
[0008] According to various embodiments and examples of the present application, the present application provides a composite current collector, a negative electrode sheet, a secondary battery, an electrical device, and a preparation method. The composite current collector can have significantly improved processability while maintaining good energy density.
[0009] In a first aspect, the present application provides a composite current collector comprising a support layer and a conductive layer disposed on at least one side of the support layer, wherein the support layer is an organic support layer;
[0010] The thickness of the support layer is recorded as d1, the tensile strength is recorded as T1, the yield strength is recorded as Q1, and the elastic modulus is recorded as G1;
[0011] The total thickness of the conductive layer is recorded as d2, the tensile strength at break is recorded as T2, and the elastic modulus is recorded as G2;
[0012] The composite current collector satisfies the following condition: (d1×T1-(d2×T2)×(1-α)-d1×Q1×α)≥150 Pa·m, where α=G1 / (G1+G2).
[0013] For a composite current collector including an organic support layer and a conductive layer, by reasonably matching the thickness d1, tensile fracture strength T1, yield strength Q1 and elastic modulus G1 of the support layer and the thickness d2, tensile fracture strength T2 and elastic modulus G2 of the conductive layer, and also using the distribution coefficient α = G1 / (G1+G2) to finely adjust the distribution of the elastic modulus between the support layer and the conductive layer, (d1×T1-(d2×T2)×(1-α)-d1×Q1×α) can be defined as the ductility coefficient of the composite current collector. The ductility coefficient can be expressed as follows: under stress, when the composite current collector enters the yield deformation stage after elastic deformation, the residual force that the unit width of the support layer can withstand. The "residual force" can roughly correspond to the residual force that the composite current collector can withstand when it breaks after deducting the force that it can withstand at the elastic limit; the greater this residual force, based on the stress-strain relationship, the greater the elongation of the composite current collector during the later plastic deformation. When the ductility coefficient of the composite current collector is ≥150, the elongation at break of the composite current collector is higher, and the processability for mass production is better, which is beneficial to reducing the fracture of the composite current collector during the electrode processing and improving the processing efficiency. It can also reduce or avoid the increase in local interface side reactions caused by wrinkling of the electrode during the charge and discharge process, thereby improving the battery cycle performance; and at the cell level, it is beneficial to reduce the cracking problem that may be caused by the gradual increase in the electrode expansion force in the later stage of the battery cell cycle, which is beneficial to improving the cycle performance and safety and reliability of the battery cell.
[0014] In some embodiments, the thickness d1 of the support layer is 2 μm-13 μm;
[0015] Optionally, the thickness d1 of the support layer is 2.4 μm-8 μm;
[0016] Further optionally, the thickness d1 of the support layer is 2.8 μm-6 μm.
[0017] The thicker the composite current collector, the lower the cell energy density. However, if the composite current collector is too thin, it can withstand less force and has a low elongation, which is detrimental to processability. Adjusting the thickness of the support layer can indirectly adjust the thickness of the composite current collector, allowing it to better balance optimal energy density and superior processability.
[0018] In some embodiments, the tensile strength at break of the support layer T1 is ≥ 200 MPa;
[0019] Optionally, the tensile fracture strength T1 of the support layer is ≥300 MPa.
[0020] The higher the tensile strength of the support layer, the greater the force it can withstand, the better the mechanical strength of the composite current collector is, and the better the processability of the composite current collector is.
[0021] In some embodiments, the yield strength Q1 of the support layer is ≥80 MPa;
[0022] Optionally, the yield strength Q1 of the support layer is ≥100 MPa.
[0023] The higher the yield strength of the support layer, the better its ability to resist slight plastic deformation, and the more conducive it is to the processing of the composite current collector.
[0024] In some embodiments, the composite current collector satisfies any one or more of the following characteristics:
[0025] The total thickness d2 of the conductive layer is 0.6 μm-2.4 μm; optionally, the total thickness d2 of the conductive layer is 1 μm-2.4 μm; further optionally, the total thickness d2 of the conductive layer is 1.4 μm-2.0 μm;
[0026] The single-side thickness d2 of the conductive layer s 0.3 μm-1.2 μm; Optionally, the thickness d2 of the conductive layer on one side s 0.5 μm-1.2 μm; further optionally, the thickness d2 of the conductive layer on one side s 0.7μm-1.0μm;
[0027] The thickness D of the composite current collector a 3 μm-15 μm; Optionally, the thickness D of the composite current collector a 3 μm-10 μm; further optionally, the thickness D of the composite current collector a 4.4μm-6μm.
[0028] By adjusting the thickness of the conductive layer or directly controlling the thickness of the composite current collector so that the thickness of the composite current collector is within a certain range, the composite current collector can better have both better energy density and superior processability.
[0029] In some embodiments, the tensile strength T2 of the conductive layer is ≥ 250 MPa;
[0030] Optionally, the tensile strength T2 of the conductive layer is ≥300 MPa.
[0031] The higher the tensile strength of the conductive layer, the more favorable it is for the processability of the composite current collector.
[0032] In some embodiments, the composite current collector satisfies any one or more of the following characteristics:
[0033] The elastic modulus G1 of the support layer is ≥2 GPa; optionally, the elastic modulus G1 of the support layer is ≥3 GPa;
[0034] The elastic modulus G2 of the conductive layer is 40 GPa-70 GPa; optionally, the elastic modulus G2 of the conductive layer is 45 GPa-55 GPa;
[0035] The α is 0.045-0.30; optionally, the α is 0.05-0.15; further optionally, the α is 0.055-0.12.
[0036] By regulating the distribution of the elastic modulus between the support layer and the conductive layer, for example, by adjusting the value of α=G1 / (G1+G2), the magnitude of the force exerted on the support layer and the conductive layer in the composite current collector under stress can be reasonably adjusted, thereby better improving the overall bearing capacity of the composite current collector, and further improving the processability of the composite current collector. Among them, when the current collector material composed of the support layer and the conductive layer is subjected to stress, during the elastic deformation stage, due to the different elastic moduli (stiffness) of the two material layers, the actual forces exerted on the support layer and the conductive layer are not consistent. The material with a large elastic modulus is often subjected to a greater force. Therefore, by adjusting the distribution coefficient, the respective force proportions of the support layer and the conductive layer in the composite current collector can be regulated.
[0037] In some embodiments, (d1×T1-(d2×T2)×(1-α)-d1×Q1×α)≥200 Pa·m;
[0038] Optionally, (d1×T1-(d2×T2)×(1-α)-d1×Q1×α)≥250 Pa·m.
[0039] The greater the ductility coefficient of the composite current collector, the higher the elongation at break of the composite current collector, the better the mass production processability will be, and it will be more conducive to reducing the fracture of the composite current collector during the electrode processing process and improving the processing quality rate; at the battery cell level, it will also be more conducive to reducing the cracking problem that may be caused by the gradual increase in the electrode expansion force in the later stage of the battery cell cycle, and will be more conducive to improving the cycle performance and safety and reliability of the battery cell.
[0040] In some embodiments, the support layer is made of a polymer-based material or a polymer-based composite material;
[0041] Optionally, the polymer component in the supporting layer includes polyimide, polyamide, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyethylene, polypropylene, polypropylene, acrylonitrile-butadiene-styrene copolymer, polyvinyl alcohol, polystyrene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, sodium polystyrene sulfonate, polyacetylene, silicone rubber, polyformaldehyde, polyphenylene ether, polyphenylene sulfide, polyethylene glycol, polysulfur nitride polymer materials, polyphenylene, polypyrrole, polyaniline, polythiophene, polypyridine, cellulose, starch, protein, epoxy resin, phenolic resin, and one or more of the derivatives of the above materials, the cross-linked products of the above materials and the copolymers of the above materials.
[0042] When polymer materials are selected as the main material of the support layer, polymers have a lighter density and better ductility than conductive metals, which can reduce the surface density of the composite current collector, thereby helping to improve the energy density of the battery cell. It can also improve the overall ductility of the composite current collector, which is beneficial to improving the processing efficiency of the electrode sheet.
[0043] The main material of the support layer may or may not contain other materials besides polymers, and may also form a composite material with other materials. When it is a polymer-based composite material, it can be appropriately selected based on performance requirements and in accordance with processing requirements to improve the processability of the composite current collector, battery core performance, or a combination thereof, such as improving one or more of the composite current collector's properties such as volume resistivity, elongation at break, and Young's modulus.
[0044] In some embodiments, the polymer component in the support layer includes polyimide, and the polyimide includes one or both of homophenyl polyimide and biphenyl polyimide;
[0045] Optionally, the polymer component in the support layer includes biphenyl polyimide;
[0046] Further optionally, the support layer comprises biphenyl polyimide in an amount of ≥50% by mass;
[0047] Further optionally, the support layer comprises biphenyl polyimide in an amount of ≥80% by mass;
[0048] Further optionally, the support layer is made of biphenyl polyimide.
[0049] Polyimide is an organic carbonyl polymer containing an imide ring in its main chain. It has excellent mechanical properties and heat resistance, high mechanical strength, and good high-temperature resistance. Using polyimide in the support layer can leverage its tensile strength, yield strength, and elastic modulus to better synergize with the tensile strength and elastic modulus of the conductive layer, thereby better adjusting the ductility coefficient of the composite current collector. This is more beneficial for achieving the dual requirements of good energy density and excellent processability of the composite current collector.
[0050] Both phenylene-type polyimide and biphenyl-type polyimide possess the aforementioned common advantages of polyimide. Furthermore, compared to phenylene-type polyimide as the main material for the support layer, the composite current collector prepared using biphenyl-type polyimide as the main material for the support layer can significantly improve one or more of the following properties: mechanical properties (such as tensile strength, elastic modulus, elongation at break), performance (such as coating efficiency, cold pressing elongation, cold pressing fracture frequency), and battery cell performance (such as cycle capacity retention).
[0051] In some embodiments, the conductive layer includes a metal material. Optionally, the metal material includes one or more of copper and a copper alloy.
[0052] When the conductive layer comprises a metal material, it is advantageous to provide better conductivity. Furthermore, when the metal material comprises one or more of copper and copper alloys, it is easier to control the ductility coefficient of the composite current collector within an appropriate range. Furthermore, it is also easier to control parameters such as the tensile strength and elastic modulus of the conductive layer within a more suitable range, thereby better balancing the energy density of the battery cell and the processability of the composite current collector.
[0053] In a second aspect, the present application provides a negative electrode plate, which includes the composite current collector described in the first aspect of the present application.
[0054] In a third aspect, the present application provides a secondary battery comprising at least one of the composite current collector described in the first aspect of the present application and the negative electrode sheet described in the second aspect of the present application.
[0055] When the negative electrode plate includes the composite current collector described in the first aspect of the present application, it can have both good energy density and high mechanical strength, and can reduce or avoid the increase in local interfacial side reactions caused by wrinkling of the plate during charging and discharging, thereby improving the battery cycle performance; further, for secondary batteries containing the aforementioned composite current collector or the aforementioned negative electrode plate, it is also beneficial to reduce the cracking problem that may be caused by the gradual increase in the expansion force of the plate in the later stage of the battery cell cycle, which is beneficial to improving the cycle performance and safety and reliability of the battery cell.
[0056] In a fourth aspect, the present application provides an electrical device comprising at least one of the composite current collector described in the first aspect of the present application, the negative electrode sheet described in the second aspect of the present application, and the secondary battery described in the third aspect of the present application.
[0057] In a fifth aspect, the present application provides a method for preparing the composite current collector described in the first aspect of the present application, which comprises the following steps: forming the conductive layer on at least one side of the support layer to prepare the composite current collector.
[0058] A supporting layer with a specific thickness d1, a specific tensile fracture strength T1, a specific yield strength Q1 and a specific elastic modulus G1 is used to further form a conductive layer with a specific thickness d2, a specific tensile fracture strength T2 and a specific elastic modulus G2. The prepared composite current collector has a high ductility coefficient, a high elongation at break, and better processability in mass production, which is beneficial to reducing the fracture of the composite current collector during the electrode processing process and improving the processing quality rate. It can also reduce or avoid the increase in local interfacial side reactions caused by wrinkling of the electrode during the charging and discharging process, thereby improving the battery cycle performance; and at the cell level, it is beneficial to reduce the cracking problem that may be caused by the gradual increase in the expansion force of the electrode in the later stage of the cell cycle, which is beneficial to improving the cycle performance and safety and reliability of the battery cell.
[0059] In a sixth aspect, the present application provides a method for preparing a negative electrode sheet, which comprises the following steps: coating a negative electrode slurry on at least one side surface of the composite current collector described in the first aspect of the present application, drying, and cold pressing to prepare the negative electrode sheet.
[0060] When the composite current collector provided in the first aspect of the present application is used to prepare the negative electrode plate, the prepared negative electrode plate can have both good energy density and high mechanical strength, which can reduce or avoid the increase in local interfacial side reactions caused by wrinkling of the plate during the charging and discharging process, thereby improving the battery cycle performance; further preparation of a secondary battery containing the aforementioned composite current collector or the aforementioned negative electrode plate is also beneficial to reducing the cracking problem that may be caused by the gradual increase in the expansion force of the plate in the later stage of the battery cell cycle, which is beneficial to improving the cycle performance and safety and reliability of the battery cell.
[0061] The details of one or more embodiments of the present application are set forth in the accompanying drawings and the description below. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] In order to better describe and illustrate the embodiments, examples, or examples of the applications disclosed herein, reference may be made to one or more of the accompanying drawings. The additional details or examples used to describe the accompanying drawings should not be considered as limiting the scope of the disclosed applications, the embodiments, examples, or examples currently described, and the best modes currently understood for these applications. Moreover, the same reference numerals are used throughout the drawings to represent the same parts. In the drawings:
[0063] FIG1 is a schematic structural diagram of a composite current collector in one embodiment of the present application, wherein the conductive layers are located on both sides of the support layer;
[0064] FIG2 is a schematic structural diagram of a composite current collector in one embodiment of the present application, wherein the conductive layer is located on a single side of the support layer;
[0065] FIG3 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0066] FIG4 is an exploded view of the secondary battery of one embodiment of the present application shown in FIG3 ;
[0067] FIG5 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of the present application.
[0068] Description of reference numerals:
[0069] 5, secondary battery; 51, shell; 52, electrode assembly; 53, cover plate; 6, power-consuming device; 100, composite current collector; 110, support layer; 120, conductive layer. DETAILED DESCRIPTION
[0070] Below, some embodiments of the composite current collector, negative electrode sheet, secondary battery, electrical device and preparation method of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0071] Numerical value " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and selected lower limit and upper limit define the boundary of special range. The scope that this mode limits can be to include end value or not include end value, and any end value can be included or not included independently, and can be arbitrarily combined, and promptly any lower limit can form a scope with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if minimum range value 1 and 2 are listed, and if maximum range value 3,4 and 5 are also listed, then the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, numerical range " ab " represents the abbreviation of any real number combination between a and b, and wherein a and b are all real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is merely an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to listing the parameter as, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, and so on. For example, when a parameter is expressed as an integer selected from "2-10", this is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.
[0072] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0073] Those skilled in the art will appreciate that, in the method for each embodiment or embodiment, the writing order of each step does not mean a strict execution order and constitutes any limitation to the implementation process, and the detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of the application can be performed in sequence, or can be performed randomly, or can preferably be performed in sequence. For example, method M includes steps (a) and (b), indicating that method M may include steps (a) and (b) performed in sequence, or may include steps (b) and (a) performed in sequence. For example, method M may also include step (c), indicating that step (c) can be added to method M in any order, for example, method M may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0074] In this application, in open technical features or technical solutions described with words such as "contain," "include," and "include," unless otherwise specified, additional members other than the listed members are not excluded, and it can be regarded as providing both closed features or solutions consisting of the listed members and open features or solutions including additional members in addition to the listed members. For example, A includes a1, a2, and a3. Unless otherwise specified, it may also include other members or not. It can be regarded as providing both the feature or solution of "A consists of a1, a2, and a3" or "A is selected from a1, a2, and a3", and the feature or solution of "A includes not only a1, a2, and a3, but also other members."
[0075] In this application, unless otherwise specified, A (such as B) means that B is a non-limiting example of A, and it can be understood that A is not limited to B.
[0076] In this application, when "multiple," "multiple," "multiple," or "several" is used, unless otherwise specified, it means a quantity greater than or equal to two. For example, "one or more" means one or greater than or equal to two. It is understood that when "any number" of items is used, it refers to any suitable combination of multiple items, that is, any combination of "any number" of items in a manner that does not conflict with each other and can implement this application.
[0077] The terms "combination thereof", "any combination thereof", "any combination thereof" and the like used in this application include all suitable combinations of any two or more of the listed items.
[0078] In this application, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc. shall be based on the technical solution that can implement this application.
[0079] Herein, the terms "preferred," "better," and "excellent" are used solely to describe preferred implementations or examples and should not be construed as limiting the scope of protection of this application. If multiple "preferred" terms appear in a technical solution, each "preferred" term is considered independent unless otherwise specified and there are no contradictions or mutual constraints.
[0080] In this application, the terms "optionally," "optional," and "optional" are optional, meaning they can be either "yes" or "no." If a technical solution contains multiple "optional" clauses, unless otherwise specified and without inconsistencies or mutual constraints, each "optional" clause is independent of the other. Unless otherwise specified, the terms "optionally include," "optionally include," and "optionally include" in this application, for example, "optionally include," mean "may include or not include."
[0081] In this application, "further", "further", "particularly", "for example", "such as", "example", "for example", etc. are used for descriptive purposes to indicate differences in content, but should not be understood as limiting the scope of protection of this application.
[0082] In this application, the terms "first," "second," "third," and "fourth," etc., in "the first aspect," "the second aspect," "the third aspect," and "the fourth aspect," etc., are used for descriptive purposes only and should not be understood as indicating or implying relative importance or quantity, nor as implicitly indicating the importance or quantity of the technical features indicated. Furthermore, "first," "second," "third," and "fourth," etc., are only used for non-exhaustive enumeration and description purposes and should be understood not to constitute closed-ended limitations on quantity.
[0083] In this application, when describing a data range, if the unit is followed only by the right endpoint, it means that the units of the left and right endpoints are the same. For example, "3~5h" or "3-5h" both indicate that the units of the left endpoint "3" and the right endpoint "5" are both hours, and both have the same meaning as "3h~5h". The units of other parameters such as temperature and size are also understood in the same way.
[0084] The weight of the relevant components mentioned in the embodiments or examples of the present application can not only refer to the content of each component, but also represent the proportional relationship of the weight between the components. Therefore, as long as the content of the relevant components in accordance with the embodiments or examples of the present application is proportionally enlarged or reduced, it is within the scope disclosed in the present application. Further, the weight or mass in the embodiments or examples of the present application can be mass units known in the chemical industry such as micrograms (μg), milligrams (mg), grams (g), kilograms (kg). In the present application, the numerical values expressed in percentages such as weight share, weight percentage, mass share, mass percentage, weight percentage content or mass percentage content, if not otherwise specified, the corresponding "%" corresponds to "wt%" or "weight %".
[0085] In this application, if there is no other indication, the unit of parameter is ℃, which means "degrees Celsius", the unit of time is h, which means "hour", min, which means "minute", the unit of length is mm, which means "millimeter", μm, which means "micrometer", nm, which means "nanometer", km, which means "kilometer", m, which means "meter", and the unit of wave number is cm. -1 The unit of viscosity is mPa·S, which stands for "milliPascal·second". The unit of surface density is mg / cm 2 Indicates "milligrams per square centimeter", volume density unit g / cm 3All represent "grams per cubic centimeter", the molar concentration unit mol / L represents "mole per liter", mmol / L represents "millimoles per liter", the amount of substance unit mol represents "mole", the voltage unit V represents "volt", the battery capacity unit Ah represents "ampere-hour", the modulus or pressure unit MPa represents "megapascal", GPa represents "giapascal", Pa represents "Pascal", and the energy density unit Wh / Kg represents "watt-hour per kilogram". 1GPa=1000MPa, 1MPa=1×10 6 Pa.
[0086] In this application, "greater than or equal to" and "greater than or equal to" can both be expressed as "≥", "less than or equal to" and "less than or equal to" can both be expressed as "≤", "greater than" can be equivalently expressed as ">", and "less than" can be equivalently expressed as "<". In this application, unless otherwise specified, "greater than or equal to" and "≥" can be regarded as providing two solutions of "greater than" and "equal to". In this application, unless otherwise specified, "less than or equal to" and "≤" can be regarded as providing two solutions of "less than" and "equal to".
[0087] In this application, exemplary descriptions such as "in some embodiments (or examples)" and "in one embodiment (or example)" may include but are not limited to the following meanings: these solutions can be combined with other solutions in a suitable manner to form new technical solutions.
[0088] With the gradual promotion of secondary battery technologies such as lithium-ion batteries in consumer electronics, electric vehicles, and energy storage power stations, the requirements for the energy density of secondary batteries are becoming increasingly higher. In terms of current collectors, the thickness of traditional copper foil negative electrode current collectors can be reduced to a relatively thin thickness (such as 4.5μm). However, in the process of preparing battery cells, there are common problems such as wrinkling during winding and unwinding, cracking during cold pressing, and broken belts. The improvement of processability has basically reached the limit. In order to further improve the energy density, a composite current collector with a "metal-polymer-metal" sandwich structure has a lighter density at the same thickness and has special advantages in safety and cost. Therefore, it has become a research hotspot in the current industry. However, the processability of the composite current collector is relatively poor, which seriously affects the further promotion and application of the composite current collector: during the production and processing, since the polymer layer has lower stiffness and temperature resistance than metal, the composite current collector may also have poor processability problems such as warping of the pole ear during coating and drying, and excessive cold pressing extension; in addition, based on the current composite current collector manufacturing process, defects such as pinholes are prone to appear on the surface of the composite current collector, which can easily lead to problems such as coating leakage, scraping off the belt and cracking of the cold pressed pole piece during use. Moreover, these problems are likely to be further aggravated when the thickness of the current collector is further reduced.
[0089] In a first aspect, the present application provides a composite current collector comprising a support layer and a conductive layer disposed on at least one side of the support layer, wherein the support layer is an organic support layer;
[0090] The thickness of the support layer is recorded as d1, the tensile fracture strength is recorded as T1, the yield strength is recorded as Q1, and the elastic modulus is recorded as G1;
[0091] The total thickness of the conductive layer is recorded as d2, the tensile strength at break is recorded as T2, and the elastic modulus is recorded as G2;
[0092] The composite current collector satisfies the following condition: (d1×T1-(d2×T2)×(1-α)-d1×Q1×α)≥150 Pa·m, where α=G1 / (G1+G2).
[0093] In this application, unless otherwise specified, "support layer" refers to the structural layer in the composite current collector that supports the conductive layer. Unless otherwise specified, the support layer is primarily made of organic materials, which offer a lower density than conductive metals, thereby meeting the energy density requirements of the battery cell.
[0094] Unless otherwise specified, the primary material of the "organic support layer" used in this application is an organic material, further primarily including a polymer material. Polymers can provide a certain degree of mechanical strength. Functional additives suitable for the composite current collector may also be added to the organic support layer as needed.
[0095] Unless otherwise specified, the terms "primarily composed of" or "primarily includes" as used herein mean that the weight percentage of the listed material is at least 50%, further 60%, further 70%, further 80%, further 90%, or any of the following weight percentages, or greater than or equal to any of the following weight percentages, or a range consisting of any two of the following weight percentages: 50%, 60%, 70%, 80%, 90%, 95%, 96%, 97%, 98%, 99%, 100%, etc. Non-limiting examples of the range consisting of any two of the foregoing weight percentages include 50%-100%, 60%-100%, 70%-100%, 80%-100%, 90%-100%, etc. For example, "the main material of A is B" or "A primarily includes B" means that the weight percentage of B in A can meet any of the aforementioned appropriate conditions to preferably obtain a better ductility coefficient.
[0096] In this application, (d1×T1-(d2×T2)×(1-α)-d1×Q1×α) is defined as the ductility coefficient of the composite current collector. The ductility coefficient can be expressed as follows: under stress, when the composite current collector enters the yield deformation stage after elastic deformation, the residual force that the unit width of the support layer can withstand. This "residual force" can roughly correspond to the residual after deducting the elastic limit from the force that the composite current collector can withstand when it breaks; the greater the residual force, based on the stress-strain relationship, the greater the elongation of the composite current collector during the later plastic deformation. The unit of the ductility coefficient is MPa·μm or Pa·m, and can also be converted to N / m. Physically, it can be considered as the force per unit width. Micrometers (μm) can be used as the unit of thickness, and MPa can be used as the unit of tensile fracture strength T1, T2 and yield strength Q1 to calculate the value of the ductility coefficient.
[0097] In this application, G1 / (G1+G2) is defined as the distribution coefficient α of the composite current collector, which is equal to the ratio of the elastic modulus of the support layer to the sum of the elastic modulus of the support layer and the elastic modulus of the conductive layer. It can reflect the distribution ratio of the elastic modulus of the composite current collector between the support layer and the conductive layer, and represents the proportion of the elastic modulus of the support layer in the elastic modulus of the composite system composed of the support layer and the conductive layer. The distribution coefficient α is a dimensionless value. When the composite current collector material composed of the support layer and the conductive layer is subjected to force, in the elastic deformation stage, due to the different elastic moduli (stiffness) of the two material layers, the actual forces exerted on the support layer and the conductive layer are not consistent. Materials with large elastic modulus tend to be subjected to greater forces. Thus, by adjusting the distribution coefficient, the respective force proportions of the support layer and the conductive layer in the composite current collector can be regulated.
[0098] For a composite current collector including an organic support layer and a conductive layer, by reasonably matching the thickness d1, tensile fracture strength T1, yield strength Q1 and elastic modulus G1 of the support layer and the thickness d2, tensile fracture strength T2 and elastic modulus G2 of the conductive layer, and also using the distribution coefficient α to finely adjust the distribution of the elastic modulus between the support layer and the conductive layer, the ductility coefficient of the composite current collector is regulated (d1×T1-(d2×T2)×(1-α)-d1×Q1×α); when the ductility coefficient of the composite current collector is greater than or equal to 150, the elongation at break of the composite current collector is higher, and the mass production processability is better, which is beneficial to reducing the fracture of the composite current collector during the electrode processing process and improving the processing quality rate. It can also reduce or avoid the increase in local interfacial side reactions caused by wrinkling of the electrode during the charge and discharge process, thereby improving the battery cycle performance; and at the cell level, it is beneficial to reduce the cracking problem that may be caused by the gradual increase in the electrode expansion force in the later stage of the cell cycle, which is beneficial to improving the cycle performance and safety and reliability of the cell.
[0099] If the elongation coefficient is less than 150Pa·m, the elongation of the composite current collector is low, which can easily lead to low yield during the electrode processing and poor cycle performance of the battery cell. The thickness d1, tensile fracture strength T1, yield strength Q1, elastic modulus G1 of the support layer, as well as the total thickness d2, tensile fracture strength T2 and elastic modulus G2 of the conductive layer work together to affect the elongation coefficient of the composite current collector. As some aspects of the synergy, for example, too thick may affect the energy density, and too thin thickness may not only lead to low processing yield, but also easily lead to poor electrode interface during the cycle of the battery cell, large cycle expansion, and thus affect the cycle performance; in addition, the elastic modulus and tensile fracture strength also have an impact on the cycle performance of the battery cell.
[0100] In this application, unless otherwise specified, the test temperature of the thickness d1, tensile strength at break T1, yield strength Q1, elastic modulus G1 of the support layer, and the total thickness d2, tensile strength at break T2, and elastic modulus G2 of the conductive layer are all 15°C to 35°C, for example, 20°C to 30°C, and further such as 25°C.
[0101] In this application, unless otherwise specified, for the determination of tensile fracture strength T1 and T2, yield strength Q1, elastic modulus G1 and G2, a sample of the following dimensions, made of the same material as the object to be tested (the conductive layer or support layer of the composite current collector), is selected for tensile testing: the sample width is 15 mm and the length is 150 mm. It can be understood that the tensile test applies a tensile force along the length direction of the sample, which corresponds to the length direction of the coil of the current collector and can be recorded as the MD direction. Unless otherwise specified, for the tensile fracture strength T1 and T2, the tensile test is performed using the following parameters: a stretching distance of 50 mm and a stretching rate of 50 mm / min. Unless otherwise specified, the elastic modulus G1 and G2 are obtained by analyzing the tensile test results at an elongation of 1%; elastic modulus = tensile strength in the elastic deformation stage / corresponding elongation = tensile strength in the elastic deformation stage / 1%; wherein, the elongation refers to the percentage of the increase in length (ΔL) along the stretched direction of the sample under the action of the tensile force relative to the initial length (L0) when not stretched, and is numerically equal to ΔL / L0×100%. It should be noted that for the tests of parameters such as tensile strength, yield strength, and elastic modulus, if the thickness of the conductive layer is relatively thin (e.g., ≤2μm) and it is difficult to conduct a tensile test directly, or it is difficult to prepare and test samples of the same thickness, the composition of the conductive layer can be detected first, and then samples of the same material with a measurable thickness (e.g., 10μm to 100μm) can be prepared for the corresponding tensile test.
[0102] In the present application, for composite current collector samples taken from secondary batteries or electrode plates, for testing parameters such as tensile fracture strength, yield strength, and elastic modulus, the support layer can be peeled off from the composite current collector sample for tensile testing; for the conductive layer, the composition of the conductive layer can be first detected, and then a sample of the same material with a measurable thickness (such as 10μm to 100μm) can be prepared for corresponding tensile testing.
[0103] The composite current collector provided in the present application satisfies the following conditions: (d1×T1-(d2×T2)×(1-α)-d1×Q1×α)≥150Pa·m, wherein α=G1 / (G1+G2). Furthermore, the test samples of T1, Q1, G1, T2 and G2 all meet the following conditions: width is 15mm, length is 150mm; further, the test parameters under the stretching mode include: stretching distance is 50mm, stretching rate is 50mm / min. Further, the test temperature of d1, T1, Q1, G1, d2, T2 and G2 is 15℃~35℃, for example, 20℃~30℃, further such as 25℃.
[0104] In some embodiments, at 15° C. to 35° C., the composite current collector satisfies the following condition: (d1×T1-(d2×T2)×(1-α)-d1×Q1×α)≥150 Pa·m, where α=G1 / (G1+G2).
[0105] In this application, unless otherwise specified, the tensile strength T1, yield strength Q1 and elastic modulus G1 of the support layer, as well as the tensile strength T2 and elastic modulus G2 of the conductive layer can be obtained by testing and analysis using a tensile testing machine (as a non-limiting example, such as INSTRON3365 tensile testing machine).
[0106] As a non-limiting example, the sample width (which may be recorded as w0) is 15 mm, the sample length is 150 mm, the stretching distance (which may be recorded as s0) is 50 mm, and the stretching rate is 50 mm / min. Each parameter can be calculated by the following formula:
[0107] Yield strength = yield point tensile force / sample cross-sectional area; where sample cross-sectional area = w0 × sample thickness;
[0108] Tensile strength at break = tensile force at break / cross-sectional area of sample; where cross-sectional area of sample = w0 × sample thickness;
[0109] Elastic modulus = tensile strength corresponding to elongation δ / δ; where elongation δ is 1%; Elongation at break = (length of sample stretched to break - s0) / s0 × 100%;
[0110] Elastic modulus = tensile strength in the elastic deformation stage / corresponding elongation. For the convenience of calculation, the tensile strength corresponding to 1% elongation (elastic deformation stage) / 1% is used for calculation;
[0111] In addition, for conductive layer samples with a thin thickness (such as ≤2μm), the composition of the conductive layer can be tested first, and then samples of the same material with a measurable thickness (such as 10μm to 100μm) can be prepared for corresponding tensile testing.
[0112] The conductive layer may be located on one side of the supporting layer or on both sides of the supporting layer.
[0113] FIG1 is a schematic structural diagram of a composite current collector 100 in one embodiment of the present application, which includes a support layer 110 and conductive layers 120 located on both sides of the support layer.
[0114] FIG2 is a schematic structural diagram of a composite current collector 100 in another embodiment of the present application, which includes a support layer 110 and a conductive layer 120 located on one side of the support layer.
[0115] In some embodiments, the thickness d1 of the support layer is 2 μm-13 μm; alternatively, the thickness d1 of the support layer is 2.4 μm-8 μm; further alternatively, the thickness d1 of the support layer is 2.8 μm-6 μm. The thickness of the support layer may also be any of the following thicknesses or a range consisting of any two of the following thicknesses: 2 μm, 2.4 μm, 2.8 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, etc. The thickness d1 of the support layer may also be selected from any of the following ranges: 2.8 μm-13 μm, 2.8 μm-8 μm, etc.
[0116] The thicker the composite current collector, the lower the energy density of the battery cell. If the composite current collector is too thin, it will result in a lower force it can withstand and a lower elongation, which is not conducive to processability. By adjusting the thickness of the support layer, the thickness of the composite current collector can be indirectly adjusted, so that the composite current collector can better combine better energy density and superior processability. If the support layer is too thin, it is easy to increase the difficulty of processing the composite current collector and reduce the production efficiency, which is not conducive to mass application. If the support layer is too thick, it is easy to lead to a decrease in advantages in terms of increased energy density and improved battery cell production efficiency, and it will also lead to higher costs and lower cost performance.
[0117] In some embodiments, the tensile strength at break of the support layer, T1, is ≥ 200 MPa. Furthermore, the tensile strength at break of the support layer, T1, can be ≥ 300 MPa. The tensile strength at break of the support layer, T1, can also be any of the following strengths, or can be greater than or equal to any of the following strengths, or can be selected from a range consisting of any two of the following strengths: 200 MPa, 240 MPa, 250 MPa, 300 MPa, 350 MPa, 365 MPa, 400 MPa, 450 MPa, 500 MPa, 540 MPa, 550 MPa, 600 MPa, etc. The tensile strength at break T1 of the support layer may be selected from any of the following ranges: 200 MPa to 600 MPa, 240 MPa to 600 MPa, 250 MPa to 600 MPa, 300 MPa to 600 MPa, 200 MPa to 550 MPa, 240 MPa to 550 MPa, 250 MPa to 550 MPa, 300 MPa to 550 MPa, etc.
[0118] The higher the tensile strength of the support layer, the greater the force it can withstand, the better the mechanical strength of the composite current collector is, and the better the processability of the composite current collector is.
[0119] In some embodiments, the yield strength Q1 of the support layer is ≥80 MPa. Optionally, the yield strength Q1 of the support layer is ≥100 MPa. The yield strength Q1 of the support layer may also be any of the following strengths, or may be greater than or equal to any of the following strengths, or may be selected from a range consisting of any two of the following strengths: 80 MPa, 90 MPa, 100 MPa, 120 MPa, 150 MPa, 160 MPa, 180 MPa, 200 MPa, 210 MPa, 220 MPa, 225 MPa, 240 MPa, 250 MPa, etc. The yield strength Q1 of the support layer can be selected from any of the following ranges: 80MPa~250MPa, 90MPa~250MPa, 100MPa~250MPa, 150MPa~250MPa, 80MPa~225MPa, 90MPa~225MPa, 100MPa~225MPa, 150MPa~225MPa, etc.
[0120] The higher the yield strength of the support layer, the better its ability to resist slight plastic deformation, and the more conducive it is to the processing of the composite current collector.
[0121] In some embodiments, the total thickness d2 of the conductive layer is 0.6 μm-2.4 μm. The total thickness d2 of the conductive layer can also be any of the following thicknesses or a range consisting of any two of the following thicknesses: 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.8 μm, 2 μm (e.g., 2.0 μm), 2.2 μm, 2.4 μm, etc. The total thickness d2 of the conductive layer can also be selected from any of the following ranges: 1.5 μm-2 μm, 1.6 μm-2 μm, 1 μm-2.4 μm, 1.4 μm-2.4 μm, 1.4 μm-2.0 μm, etc.
[0122] In this application, when the conductive layer is located on a single side of the support layer, the total thickness d2 of the conductive layer is numerically equal to the thickness of the single side; when the conductive layer is located on both sides of the support layer, the total thickness d2 of the conductive layer is numerically equal to the sum of the thicknesses of both sides. When the conductive layer is located on both sides of the support layer, the thicknesses of the two sides can be the same or different. When the materials of the two conductive layers are different, the total thickness, average tensile strength at break, and average elastic modulus can be analyzed based on the test results of the two conductive layers, and used as d2, T2, and G2, respectively, to calculate the ductility coefficient of the composite current collector.
[0123] In some embodiments, the thickness d2 of the conductive layer on one side is s The thickness of the conductive layer on one side is d2. s The thickness of the conductive layer may be any one of the following thicknesses or a range of any two of the following thicknesses: 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, etc. The thickness of the conductive layer on one side d2 s It can also be selected from any of the following ranges: 0.5 μm-1 μm, 0.8 μm-1.2 μm, 0.5 μm-1.2 μm, 0.7 μm-1.0 μm, etc.
[0124] In some embodiments, the thickness D of the composite current collector a The thickness of the composite current collector is 3μm-15μm. a The thickness may also be any of the following or a range selected from any two of the following thicknesses: 3 μm, 3.4 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.4 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, 15 μm, etc. The thickness D of the composite current collector is 3 μm, 3.4 μm, 3.5 μm, 4 μm, 5 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.4 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, 15 μm, etc. aIt can also be selected from any of the following ranges: 4μm-15μm, 4μm-14μm, 4μm-10μm, 5μm-15μm, 5μm-14μm, 5μm-10μm, 6μm-15μm, 6μm-14μm, 6μm-10μm, 6μm-8μm, 3μm-10μm, 4.4μm-6μm, etc.
[0125] In some embodiments, the composite current collector satisfies any one or more of the following characteristics:
[0126] The total thickness d2 of the conductive layer is 0.6 μm-2.4 μm; optionally, the total thickness d2 of the conductive layer is 1 μm-2.4 μm; further optionally, the total thickness d2 of the conductive layer is 1.4 μm-2.0 μm;
[0127] Single-side thickness d2 of the conductive layer s 0.3 μm-1.2 μm; optionally, the single-side thickness d2 of the conductive layer s 0.5 μm-1.2 μm; further optionally, the single-side thickness d2 of the conductive layer s 0.7μm-1.0μm;
[0128] Thickness D of composite current collector a 3μm-15μm; Optionally, the thickness D of the composite current collector a 3 μm-10 μm; further optionally, the thickness D of the composite current collector a 4.4μm-6μm;
[0129] Among them, the total thickness of the conductive layer d2, the thickness of the conductive layer on one side d2 s , the thickness of the composite current collector D a Any one of the parameters may also have the appropriate features of any of the aforementioned embodiments, and the three parameters may also be selected from a suitable combination of the aforementioned features in a suitable manner.
[0130] By adjusting the thickness of the conductive layer or directly controlling the thickness of the composite current collector so that the thickness of the composite current collector is within a certain range, the composite current collector can better have both better energy density and superior processability.
[0131] If the composite current collector is too thick, the degree of improvement in the weight energy density and volume energy density of the battery cell may be reduced. If the composite current collector is too thin, it may become incompatible with the current battery cell preparation process, which may lead to a decrease in quality rate and be unfavorable for industrial application.
[0132] If the conductive layer is too thin, the conductive current capacity of the composite current collector may be weakened, which is not conducive to the rate performance of the battery cell; if the conductive layer is too thick, the unit area volume of the composite current collector may increase, thereby reducing the advantage of the composite current collector in improving the energy density of the battery cell.
[0133] In some embodiments, the tensile strength at break of the conductive layer, T2, is ≥ 250 MPa; alternatively, the tensile strength at break of the conductive layer, T2, is ≥ 300 MPa. The tensile strength at break of the conductive layer, T2, can also be any of the following strengths, or can be greater than or equal to any of the following strengths, or can be selected from a range consisting of any two of the following strengths: 250 MPa, 260 MPa, 270 MPa, 280 MPa, 300 MPa, 320 MPa, 325 MPa, 340 MPa, 350 MPa, etc. The tensile strength at break of the conductive layer, T2, can be selected from any of the following ranges: 250 MPa to 350 MPa, 260 MPa to 350 MPa, 300 MPa to 350 MPa, etc.
[0134] The higher the tensile strength of the conductive layer, the more favorable it is for the processability of the composite current collector.
[0135] In some embodiments, the elastic modulus G1 of the support layer is ≥ 2 GPa; optionally, the elastic modulus G1 of the support layer is ≥ 3 GPa. The elastic modulus G1 of the support layer may also be any of the following moduli, or may be greater than or equal to any of the following moduli, or may be selected from a range consisting of any two of the following moduli: 2 GPa, 2.5 GPa, 3 GPa, 3.5 GPa, 4 GPa, 4.2 GPa, 4.5 GPa, 4.6 GPa, 4.8 GPa, 5 GPa, 5.5 GPa, 6 GPa, 6.5 GPa, 7 GPa, 7.5 GPa, 8 GPa, 10 GPa, etc. The elastic modulus G1 of the support layer may also be selected from any of the following ranges: 2 GPa to 10 GPa, 3 GPa to 10 GPa, 4 GPa to 10 GPa, 2 GPa to 8 GPa, 3 GPa to 8 GPa, 4 GPa to 8 GPa, etc.
[0136] In some embodiments, the elastic modulus G2 of the conductive layer is 40 GPa-70 GPa; alternatively, the elastic modulus G2 of the conductive layer is 45 GPa-55 GPa. The elastic modulus G2 of the conductive layer can also be any of the following moduli or a range consisting of any two of the following moduli: 40 GPa, 43 GPa, 45 GPa, 50 GPa, 55 GPa, 58 GPa, 60 GPa, 65 GPa, 70 GPa, etc. The elastic modulus G2 of the conductive layer can also be selected from any of the following ranges: 40 GPa-60 GPa, 43 GPa-60 GPa, 45 GPa-60 GPa, 43 GPa-58 GPa, etc.
[0137] In some embodiments, the partition coefficient α is 0.045-0.30; alternatively, the partition coefficient α is 0.05-0.15; further alternatively, the partition coefficient α is 0.055-0.12. The distribution coefficient α can also be any of the following values or an interval consisting of any two of the following values: 0.045, 0.050, 0.060, 0.080, 0.090, 0.095, 0.098, 0.100, 0.103, 0.105, 0.106, 0.108, 0.110, 0.115, 0.116, 0.118, 0.120, 0.125, 0.130, 0.140, 0.145, 0.150, 0.155, 0.160, 0.165, 0.170, 0.180, 0.185, 0.190, 0.195, 0.200, 0.21, 0.22, 0.24, 0.25, 0.26, 0.28, 0.30, etc. The distribution coefficient α can also be selected from any of the following ranges: 0.05-0.3, 0.05-0.20, 0.05-0.15, 0.055-0.25, 0.055-0.20, 0.055-0.15, 0.1-0.15, 0.1-0.14 (including 0.10-0.14), etc.
[0138] In some embodiments, the composite current collector satisfies any one or more of the following characteristics:
[0139] The elastic modulus G1 of the support layer is ≥ 2 GPa; optionally, the elastic modulus G1 of the support layer is ≥ 3 GPa;
[0140] The elastic modulus G2 of the conductive layer is 40 GPa-70 GPa; optionally, the elastic modulus G2 of the conductive layer is 45 GPa-55 GPa;
[0141] α is 0.045-0.30; optionally, α is 0.05-0.15; further optionally, α is 0.055-0.12.
[0142] By regulating the distribution of the elastic modulus between the support layer and the conductive layer, for example, by adjusting the value of α=G1 / (G1+G2), the force exerted on the support layer and the conductive layer in the composite current collector under stress can be reasonably adjusted, thereby better improving the overall bearing capacity of the composite current collector and further improving the processability of the composite current collector.
[0143] In some embodiments, the elongation coefficient (d1×T1-(d2×T2)×(1-α)-d1×Q1×α) is ≥150Pa·m. The elongation coefficient may also be any of the following values, or may be greater than or equal to any of the following values, or may be selected from an interval consisting of any two of the following values: 150Pa·m, 180Pa·m, 200Pa·m, 250Pa·m, 300Pa·m, 350Pa·m, 400Pa·m, 450Pa·m, 500Pa·m, 550Pa·m, 600Pa·m, 650Pa·m, 700Pa·m, 750Pa·m, 800Pa·m, 840Pa·m, 850Pa·m, 900Pa·m, 1000Pa·m, 10 18Pa·m, 1020Pa·m, 1025Pa·m, 1050Pa·m, 1100Pa·m, 1200Pa·m, 1300Pa·m, 1400Pa·m, 1450Pa·m, 1500Pa·m, 1520Pa·m, 1550Pa ·m, 1590Pa·m, 1600Pa·m, 1650Pa·m, 1700Pa·m, 1800Pa·m, 2000Pa·m, 2200Pa·m, 2250Pa·m, 2300Pa·m, 2400Pa·m, 2500Pa·m, etc. The elongation coefficient can also be selected from any of the following ranges: ≥250Pa·m, ≥500Pa·m, ≥600Pa·m, ≥800Pa·m, ≥1000Pa·m, 150Pa·m-2500Pa·m, 180Pa·m-2500Pa·m, 250Pa·m-2500Pa·m, 500Pa·m-2500Pa·m, 600Pa·m-2500Pa·m, etc.
[0144] The greater the ductility coefficient of the composite current collector, the higher the elongation at break of the composite current collector, the better the mass production processability will be, and it will be more conducive to reducing the fracture of the composite current collector during the electrode processing process and improving the processing quality rate; at the battery cell level, it will also be more conducive to reducing the cracking problem that may be caused by the gradual increase in the electrode expansion force in the later stage of the battery cell cycle, and will be more conducive to improving the cycle performance and safety and reliability of the battery cell.
[0145] In this application, the "processing quality rate" of a current collector is defined as the ratio of the number of qualified electrode sheets produced during the cell manufacturing process to the total current collector production input. It can also be defined as the ratio of the length of qualified electrode sheets produced during the cell manufacturing process to the total length of the current collector produced. For each cell process, it can also be expressed as the coating quality rate. Furthermore, parameters such as the frequency of cold press cracking can also reflect the processing quality rate. A higher processing quality rate indicates better processability of the current collector.
[0146] In this application, the "coating quality rate" of a current collector refers to the ratio of the length of qualified electrode sheets produced during the cell coating process to the length of the current collector input. The coating production quality rate can be calculated by recording the number of meters of qualified coated electrode sheets produced during the coating process for every 100,000 meters of current collector. The "coating quality rate" of a current collector reflects the processability of the current collector during the cell coating process. A higher coating quality rate indicates better processability of the current collector.
[0147] In this application, the "cold press fracture frequency" of the current collector refers to the number of times a unit length of the current collector fractures and fails during the cold pressing process of the battery cell, and the unit can be "times / km" or "km / time". The cold press cracking frequency of the current collector can be evaluated by recording the number of cracks in the cold pressing process of 100,000 meters of current collector coated pole pieces. The "cold press fracture frequency" of the current collector reflects the processability of the current collector in the cold pressing process of the battery cell. When the unit is "km / time", the higher the value of the cold press fracture frequency, the less likely it is to crack, reflecting that the processability of the current collector is better. When the unit is "times / km", the lower the value of the cold press fracture frequency, the less likely it is to crack, reflecting that the processability of the current collector is better. Wherein, 1km=1000m.
[0148] In some embodiments, the material of the support layer is a polymer-based material or a polymer-based composite material; optionally, the polymer component in the support layer includes polyimide, polyamide, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyethylene, polypropylene, polypropylene, acrylonitrile-butadiene-styrene copolymer, polyvinyl alcohol, polystyrene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, sodium polystyrene sulfonate, polyacetylene, silicone rubber, polyformaldehyde, polyphenylene ether, polyphenylene sulfide, polyethylene glycol, polysulfur nitride polymer materials, polyphenylene, polypyrrole, polyaniline, polythiophene, polypyridine, cellulose, starch, protein, epoxy resin, phenolic resin, and one or more of the derivatives of the above materials, the cross-linked products of the above materials and the copolymers of the above materials.
[0149] In the present application, unless otherwise specified, the “polymer-based material” is substantially composed of polymers. It is understood that the inevitable impurities introduced during the processing are not excluded.
[0150] In this application, unless otherwise specified, a "polymer-based composite material" includes a polymer having a weight percentage of ≥50%, and may also include one or more additives. Non-limiting examples of additives include one or more metallic materials, inorganic non-metallic materials, etc. In the "polymer-based composite material," the weight percentage of the polymer is at least 50%, and may further be 60%, 70%, 80%, 85%, or 90%. It may also be any of the following weight percentages, or may be greater than or equal to any of the following percentages and less than or equal to 100%. Alternatively, it may be selected from a range consisting of any two of the following weight percentages: 50%, 60%, 70%, 80%, 85%, 90%, 95%, 96%, 97%, 98%, 99%, 100%, etc. Non-limiting examples of the range consisting of any two of the foregoing weight percentages include 50% to 100%, 60% to 100%, 70% to 100%, 80% to 100%, 90% to 100%, etc. The weight percentage of the polymer in the polymer-based composite material may meet any of the aforementioned appropriate conditions, preferably to obtain a preferred ductility coefficient.
[0151] The additives in the polymer-based composite material can be appropriately selected based on processing requirements and one or more of the requirements for the performance of the composite current collector, the pole piece, and the battery cell.
[0152] The metal material additive may include, but is not limited to, one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, iron, iron alloys, silver, and silver alloys.
[0153] Inorganic non-metallic materials may include, but are not limited to, one or more of carbon-based materials, aluminum oxide, silicon dioxide, silicon nitride, silicon carbide, boron nitride, silicates, and titanium oxide, and may also include, but are not limited to, one or more of glass materials, ceramic materials, and ceramic composite materials. Carbon-based materials may include, but are not limited to, one or more of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0154] In some embodiments, the additive may include a carbon-based material coated with a metal material, such as one or more of nickel-coated graphite powder and nickel-coated carbon fiber.
[0155] When polymer materials are selected as the main material of the support layer, polymers have a lighter density and better ductility than conductive metals, which can reduce the surface density of the composite current collector, thereby helping to improve the energy density of the battery cell. It can also improve the overall ductility of the composite current collector, which is beneficial to improving the processing efficiency of the electrode sheet.
[0156] The main material of the support layer may or may not contain other materials besides polymers, and may also form a composite material with other materials. When it is a polymer-based composite material, it can be appropriately selected based on performance requirements and in accordance with processing requirements to improve the processability of the composite current collector, battery core performance, or a combination thereof. For example, one or more of the composite current collector's properties such as volume resistivity, elongation at break, and Young's modulus can be improved.
[0157] In some embodiments, the polymer component in the support layer includes polyimide. Further, the polyimide may include one or both of homophenyl polyimide and biphenyl polyimide.
[0158] In some embodiments, the polymer component of the support layer may include biphenyl polyimide.
[0159] In some embodiments, the support layer comprises biphenyl polyimide with a mass percentage of ≥50%; alternatively, the support layer comprises biphenyl polyimide with a mass percentage of ≥80%; further alternatively, the support layer is made of biphenyl polyimide. The mass percentage of biphenyl polyimide in the support layer can also be any of the following percentages: 50%, 60%, 70%, 80%, 90%, 95%, 96%, 97%, 98%, 99%, 100%, etc., or can be greater than or equal to any of the aforementioned percentages and less than or equal to 100%, or can be selected from an interval consisting of any two of the aforementioned percentages, non-limiting examples of which include 50% to 100%, 60% to 100%, 70% to 100%, 80% to 100%, 90% to 100%, etc.
[0160] In some embodiments, the polymer component in the support layer is a combination of a homophenyl polyimide and a biphenyl polyimide. In some embodiments, the weight percentage of the biphenyl polyimide can be any of the following percentages: 50%, 60%, 67%, 70%, 75%, 80%, 90%, 95%, 96%, 97%, 98%, 99%, 100%, etc., or can be greater than or equal to any of the aforementioned percentages and less than or equal to 100%, or can be selected from a range consisting of any two of the aforementioned percentages, such as, for example, 50% to 100%, 60% to 100%, 70% to 100%, 80% to 100%, 90% to 100%, etc. In other embodiments, the weight ratio of the biphenyl polyimide to the homophenyl polyimide can be any of the following ratios or ratios, or can be selected from a range consisting of any two of the following ratios or ratios: 9:1, 8:2, 7:3, 6:4, etc.
[0161] Polyimide is an organic carbonyl polymer containing an imide ring in its main chain. It has excellent mechanical properties and heat resistance, high mechanical strength, and good high-temperature resistance. Using polyimide in the support layer can leverage its tensile strength, yield strength, and elastic modulus to better synergize with the tensile strength and elastic modulus of the conductive layer, thereby better adjusting the ductility coefficient of the composite current collector. This is more beneficial for achieving the dual requirements of good energy density and excellent processability of the composite current collector.
[0162] Both benzene-type polyimide and biphenyl-type polyimide have the aforementioned common advantages of polyimide, among which biphenyl-type polyimide has more excellent high-temperature resistance and mechanical properties. By introducing biphenyl-type polyimide into the composite current collector, for example as the main material (≥50 weight%), it is beneficial to improve the high-temperature tensile properties of the composite current collector, and it is beneficial to maintain good flatness during the high-temperature battery preparation process such as coating, unwinding and drying. It can also avoid defective products caused by curling, wrinkling and even breakage due to the volatilization of solvents, water, etc., and better improve the processing quality rate. As the operating speed of battery mass production equipment gradually increases, the drying temperature in the battery process also gradually increases, and the improvement of the high-temperature mechanical properties of the current collector becomes more important for the manufacturing quality rate. In addition, the improvement of the mechanical properties of the composite current collector is also conducive to reducing the shrinkage and expansion of the battery during the charging and discharging process, which is beneficial to the integrity of the positive and negative electrode interfaces of the battery, and can reduce or avoid the increase of local interface side reactions caused by wrinkling of the pole piece during the charging and discharging process, thereby helping to improve the cycle performance of the battery.
[0163] Compared with using biphenyl polyimide as the main material of the support layer, when biphenyl polyimide is used as the main material of the support layer, the prepared composite current collector can significantly improve one or more of the mechanical properties (such as tensile strength, elastic modulus, elongation at break, etc.), usage performance (such as coating quality, cold pressing elongation, cold pressing fracture frequency, etc.), and battery cell performance (such as cycle capacity retention rate, etc.).
[0164] In this application, the “cold pressing elongation” of the current collector refers to the difference between the extended length of the cell electrode after cold pressing and the initial length (L 0C The cold pressing elongation of the electrode can be evaluated by measuring the extension length of the electrode after cold pressing of a 1 meter (m) long current collector coated electrode. At this time, the cold pressing elongation = (length of the electrode after cold pressing - L 0C ) / L 0C ×100%,L 0C Take 1 meter (m). The "cold pressing elongation" of the current collector reflects the deformation of the current collector during the cold pressing process of the battery cell.
[0165] By using biphenyl polyimide as the supporting layer, the mechanical strength of the composite current collector can be significantly improved, and further it is beneficial to improve the process efficiency and performance of the battery cell; in addition, the pinhole defect rate can also be reduced.
[0166] In some embodiments, the biphenyl polyimide used in this application contains The structure is connected by two N atoms on the two imide rings. Furthermore, its infrared spectrum is at a wave number of 1618.65 cm -1 、1420.2cm -1 、1218.98cm -1 、888.9cm -1 、695.72cm -1 、673.08cm -1 There is a vibration peak in at least one of them.
[0167] In some embodiments, the conductive layer includes a metal material, and optionally, the metal material includes one or more of aluminum and an aluminum alloy. In addition to mainly containing copper, the copper alloy also contains doping elements. The types of doping elements may include one or more of metal elements and non-metallic elements, wherein the doped metal elements may include but are not limited to one or more of nickel, nickel, titanium, titanium, silver, etc., and the doped non-metallic elements may include but are not limited to one or more of nitrogen (N), oxygen (O), carbon (C), silicon (Si), boron (B), etc. The weight proportion of the doping element in the copper alloy may be ≤10%, and the weight proportion of the doping element in the copper alloy may further be any of the following percentages, or may be greater than 0 and less than or equal to any of the following percentages, or may be selected from the interval consisting of any two of the following percentages: 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.
[0168] When the conductive layer comprises a metal material, it is advantageous to provide better conductivity. Furthermore, when the metal material comprises one or more of copper and copper alloys, it is easier to control the ductility coefficient of the composite current collector within an appropriate range. Furthermore, it is also easier to control parameters such as the tensile strength and elastic modulus of the conductive layer within a more suitable range, thereby better balancing the energy density of the battery cell and the processability of the composite current collector.
[0169] In some embodiments, the support layer can be a single-layer structure or a multi-layer structure, as long as it meets the requirements of the aforementioned ductility coefficient and related parameters. When the support layer has a multi-layer structure, the material composition and distribution of each structural layer can be the same or different.
[0170] In some embodiments, the thickness D of the composite current collector aIt can be equal to d1+d2 or greater than d1+d2. a When it is greater than d1+d2, the composite current collector further includes other structural layers in addition to the aforementioned support layer and conductive layer.
[0171] The composite current collector can be used as a negative electrode current collector, either as a negative electrode current collector in a negative electrode sheet or as a component of a negative electrode current collector. For example, while meeting the characteristics of the composite current collector of the present application, other functional structural layers can be further laminated to produce a negative electrode current collector with more functions.
[0172] In the field of secondary batteries (such as lithium-ion secondary batteries), generally speaking, the negative electrode tends to choose a metal material that is inert to lithium (such as copper or its alloys) as the negative electrode current collector conductive material, while the positive electrode tends to choose a material that is resistant to oxidation (such as aluminum or its alloys) as the positive electrode current collector conductive material. Among them, aluminum and copper are exemplary metal materials with high electrical conductivity. Therefore, the mechanical properties of the conductive layer metal materials of the positive and negative electrode current collectors may differ, resulting in different ductility coefficients.
[0173] When the composite current collector of the first aspect of the present application is used as a negative electrode current collector, the advantages of the aforementioned embodiments can be brought into play.
[0174] In a second aspect, the present application provides a negative electrode plate, which includes the composite current collector according to the first aspect of the present application.
[0175] The negative electrode sheet includes a negative electrode current collector, which includes the composite current collector described in the first aspect of the present application. In other embodiments, the composite current collector described in the first aspect of the present application is used as the negative electrode current collector. In some embodiments, the composite current collector described in the first aspect of the present application is used as a portion of the negative electrode current collector.
[0176] When the negative electrode plate includes the composite current collector described in the first aspect of the present application, it can have both good energy density and high mechanical strength, and can reduce or avoid the increase in local interfacial side reactions caused by wrinkling of the negative electrode plate during the charging and discharging process, thereby improving the battery cycle performance; further, for secondary batteries containing the aforementioned composite current collector or the negative electrode plate described in the second aspect of the present application, it is also beneficial to reduce the cracking problem that may be caused by the gradual increase in the expansion force of the plate in the later stage of the battery cell cycle, which is beneficial to improving the cycle performance and safety and reliability of the battery cell.
[0177] The negative electrode sheet includes the composite current collector described in the first aspect of the present application and a negative electrode film layer arranged on at least one side of the composite current collector, at least one negative electrode film layer includes a negative electrode active material layer, and any negative electrode active material layer independently contains a negative electrode active substance.
[0178] In some embodiments, the negative electrode active material may adopt a negative electrode active material for a battery that is well known in the art. As a non-limiting example, the negative electrode active material may include one or more of the following materials or substances: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. Silicon-based materials may include one or more of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may include one or more of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials or substances, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0179] In some embodiments, the negative electrode active material includes a silicon-based material. In this case, using the composite current collector described in the first aspect of this application as the negative electrode current collector can effectively reduce the cracking problem that may occur in the later stages of the battery cell cycle due to the gradual increase in the expansion force of the electrode sheet, and significantly improve the cycle performance and safety and reliability of the battery cell.
[0180] In some embodiments, the negative electrode active material includes one or more of a carbon-based material, a silicon-based material, a tin-based material, and lithium titanate, as well as modified forms of any of the foregoing materials, wherein the modified form includes one or more of a doping modification and a coating modification. Both the doping modification method and the coating modification method can adopt or refer to existing modification methods in the art, including but not limited to the selection of element types and doping amounts. Carbon-based materials may include but are not limited to one or more of graphite materials, soft carbon, hard carbon, etc. Graphite materials may include one or more of artificial graphite and natural graphite.
[0181] As a non-limiting example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction. Further, the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0182] In some embodiments, the negative electrode film layer may further optionally include a binder. In some embodiments, the negative electrode active material layer may further optionally include a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS). Without limitation, the weight percentage of the binder in the negative electrode active material layer may be 0-10%, further 0-5%, further 1%-5%, and further optionally 1%-3%.
[0183] In some embodiments, the negative electrode film layer may further include a conductive agent. In some embodiments, the negative electrode active material layer may further include a conductive agent. The conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. Without limitation, the weight percentage of the conductive agent in the negative electrode active material layer may be 0-10%, and further optionally 0-5%.
[0184] In some embodiments, the negative electrode film layer may further optionally include other additives, such as thickeners. In some embodiments, the negative electrode active material layer may further optionally include other additives, such as thickeners. Non-limiting examples of thickeners may include sodium carboxymethyl cellulose (CMC-Na). Without limitation, the weight percentage of other additives in the negative electrode active material layer may be 0-10%, further optionally 0-5%, further optionally 0-3%, and further optionally 0-2%.
[0185] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (a non-limiting example of the solvent is deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on at least one side of the negative electrode current collector, and after drying, compacting (compacting can be performed by cold pressing) and other processes, the negative electrode sheet can be obtained. The surface of the negative electrode current collector coated with the negative electrode slurry can be on a single surface of the negative electrode current collector or on both surfaces of the negative electrode current collector. The solid content of the negative electrode slurry can be 40wt% to 60wt%. The compacted density of the negative electrode sheet can be 1.4g / cm 3 ~1.75g / cm 3 , further optional 1.5g / cm 3 ~1.7g / cm 3 .
[0186] In this application, wt% means weight percentage.
[0187] The "compacted density" used in this application has a meaning well known in the art and is one of the reference indicators of material energy density. The compacted density of the negative electrode plate refers to the ratio of the mass of the negative electrode active material layer to its volume. The compacted density of the positive electrode plate refers to the ratio of the mass of the positive electrode active material layer to its volume. In this application, unless otherwise specified, for the positive electrode plate or the negative electrode plate, the plate area before and after cold pressing does not change much, and the corresponding compacted density calculation formula is: Compacted density = coating surface density / (plate thickness after cold pressing - collector thickness). Coating surface density = slurry dry weight / plate area before cold pressing.
[0188] In a third aspect, the present application provides a secondary battery comprising at least one of the composite current collector described in the first aspect of the present application and the negative electrode sheet described in the second aspect of the present application.
[0189] For secondary batteries containing the aforementioned composite current collector or the aforementioned negative electrode plate, they can have both good energy density and high mechanical strength, and can reduce or avoid the increase in local interface side reactions caused by wrinkling of the plate during charging and discharging. Furthermore, it is also beneficial to reduce the cracking problem that may be caused by the gradual increase in the expansion force of the plate in the later stage of the battery cell cycle, which is beneficial to improving the cycle performance and safety and reliability of the battery cell.
[0190] In some embodiments, the secondary battery includes the negative electrode sheet described in the second aspect of the present application, and also includes a positive electrode sheet and a separator; wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet.
[0191] In this application, unless otherwise specified, the electrode plate can be a positive electrode plate or a negative electrode plate, and the "active material" in the electrode plate refers to a substance that can reversibly embed and release active ions. Unless otherwise specified, "negative electrode active material" refers to a substance used for the negative electrode plate that can reversibly embed and release active ions; "positive electrode active material" refers to a substance used for the positive electrode plate that can reversibly release and embed active ions. When the secondary battery is charging, the active ions are released from the positive electrode and embedded in the negative electrode through the electrolyte; when the secondary battery is discharging, the active ions are released from the negative electrode and embedded in the positive electrode. The active ions are not particularly limited and can be lithium ions, in which case it corresponds to a lithium-ion secondary battery.
[0192] In this application, “active material” and “active substance” have the same meaning and can be used interchangeably; “positive electrode active substance” and “positive electrode active material” have the same meaning and can be used interchangeably; “negative electrode active substance” and “negative electrode active material” have the same meaning and can be used interchangeably.
[0193] In this application, unless otherwise specified, "active material layer" includes the positive electrode active material layer of the positive electrode sheet and the negative electrode active material layer of the negative electrode sheet. Depending on the specific circumstances, it can refer to either the positive electrode active material layer or the negative electrode active material layer. It is understood that the positive electrode active material layer contains a positive electrode active material, and the negative electrode active material layer contains a negative electrode active material.
[0194] Negative electrode
[0195] The negative electrode sheet in the third and fourth aspects of the present application includes the negative electrode sheet provided in the second aspect of the present application.
[0196] Positive electrode
[0197] In the present application, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, at least one positive electrode film layer includes a positive electrode active material layer, and further, any positive electrode active material layer independently contains a positive electrode active substance.
[0198] Without limitation, the weight percentage of the positive electrode active material in the positive electrode active material layer may be ≥80 wt %, and further may be ≥90 wt %.
[0199] As a non-limiting example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction. Further, the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0200] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material on a polymer material substrate. Without limitation, in the positive electrode current collector, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. Without limitation, in the positive electrode current collector, non-limiting examples of the polymer material substrate include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0201] In some embodiments of the present application, the positive electrode active material includes a lithium ion material; further, the secondary battery is a lithium ion secondary battery.
[0202] In some embodiments of the present application, the secondary battery is a lithium-ion secondary battery. Lithium-ion secondary batteries utilize the intercalation and deintercalation of lithium ions in electrodes and their transport through electrolytes to achieve charge and discharge. Generally speaking, the active ions in lithium-ion secondary batteries are lithium ions, but this is not limited to this.
[0203] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries that is well known in the art. As a non-limiting example, the positive electrode active material may include one or more of the following materials or substances: lithium-containing phosphates with an olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials or substances, and other traditional materials or substances that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, non-limiting examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and their modified compounds. Non-limiting examples of lithium cobalt oxide include LiCoO2; non-limiting examples of lithium nickel oxide include LiNiO2; non-limiting examples of lithium manganese oxide include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxide include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ) etc. Non-limiting examples of lithium nickel cobalt aluminum oxide include LiNi 0.80 Co 0.15 Al 0.05 O2. Non-limiting examples of olivine-structured lithium-containing phosphates may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon. Non-limiting examples of lithium iron phosphate include LiFePO4 (also referred to as LFP); non-limiting examples of lithium manganese phosphate include LiMnPO4.
[0204] It is understandable that the battery will be accompanied by lithium (Li) deintercalation and consumption during the charge and discharge process, and the content of Li in the positive electrode plate is different when the battery is discharged to different states. In the exemplary description of the positive electrode active material in this application, unless otherwise specified, the Li content can be the initial state of the material or the non-initial state after the charge and discharge cycle. The positive electrode active material is applied to the positive electrode plate in the battery system. After the charge and discharge cycle, the Li content in the positive electrode active material contained in the positive electrode plate usually changes. Among them, the Li content can be measured using the atomic molar content, but is not limited to this. Regarding "the Li content is the initial state of the material", the initial state of the material refers to the state before the material is added to the positive electrode slurry. It is understandable that new materials or new substances obtained by appropriate modification on the basis of the listed positive electrode active materials are also within the scope of positive electrode active materials. The aforementioned appropriate modification refers to an acceptable modification method for the positive electrode active material, and a non-limiting example is coating modification.
[0205] In the exemplary descriptions of the positive electrode active material in this application, the oxygen (O) content is only a theoretical value. Lattice oxygen release will cause the atomic molar content of oxygen to change, and the actual O content will fluctuate. The O content can be measured by atomic molar content, but is not limited to this.
[0206] In some embodiments, the positive electrode film layer may further optionally include a binder. In some embodiments, the positive electrode active material layer may further optionally include a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. Typically, the weight percentage of the binder in the positive electrode active material layer may be 0 to 10 wt%, further 0 to 8 wt%, and further 1 wt% to 5 wt%, based on the total weight of the positive electrode active material layer.
[0207] In some embodiments, the positive electrode film layer may further optionally include a conductive agent. In some embodiments, the positive electrode active material layer may further optionally include a conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. Typically, the weight percentage of the conductive agent in the positive electrode active material layer may be 0 to 10 wt %, further 0 to 8 wt %, and further 0 to 5 wt %, based on the total weight of the positive electrode active material layer.
[0208] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent to form a positive electrode slurry; the positive electrode slurry is coated on at least one side of the positive electrode current collector, and after drying, compaction (compaction can be performed by cold pressing), etc., the positive electrode sheet can be obtained. The type of solvent in the positive electrode slurry can include but is not limited to any of the aforementioned embodiments. For example, the type of solvent in the positive electrode slurry can include but is not limited to N-methylpyrrolidone (NMP), and NMP can be further used as a single solvent. The surface of the positive electrode current collector coated with the positive electrode slurry can be on a single surface of the positive electrode current collector or on both surfaces of the positive electrode current collector. The solid content of the positive electrode slurry can be 40wt% to 80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000mPa·s to 25000mPa·s. The compacted density of the positive electrode sheet can be 3.0g / cm 3 ~3.6g / cm 3 , optional 3.3g / cm 3 ~3.5g / cm 3 .
[0209] electrolytes
[0210] The electrolyte conducts active ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte; it can be selected based on needs. For example, the electrolyte can be liquid, gel, or solid.
[0211] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent. In a lithium-ion secondary battery, the electrolyte salt may include an electrolyte lithium salt.
[0212] Without limitation, the concentration of the electrolyte salt in the electrolyte solution may be 0.5 mol / L to 5 mol / L.
[0213] In some embodiments, the electrolyte lithium salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0214] In some embodiments, the solvent is an organic solvent.
[0215] In some embodiments, the organic solvent in the electrolyte can include one or more of esters, carbonates and ethers. In some embodiments thereof, the organic solvent includes esters. Carbonate solvents can include one or more of carbonates and halogenated carbonates. As the non-limiting example of organic solvents, such as ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB) and any of the foregoing fluorochemicals.
[0216] In some embodiments, the solvent of the electrolyte may include ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate (BC, ), one or more of fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0217] As non-limiting examples, the ether organic solvent may include one or more of tetrahydrofuran (THF), dimethoxymethane (DMM), 1,2-dimethoxyethane (DME), 1,2-dimethoxypropane (DMP), diglyme (DG), and the like.
[0218] In some embodiments, the electrolyte may further include additives. For example, the additives may be used to improve the performance of the solid electrolyte interface (SEI) film, such as at least one of anode film-forming additives and cathode film-forming additives. The additives may also include additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve high or low temperature performance, additives that increase conductivity, etc.
[0219] In some embodiments, the additives in the electrolyte may include one or more of vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), methylene methanedisulfonate (MMDS), 1-propylene-1,3-sultone (PST), vinyl sulfite (ES), propylene sulfite (PS), vinyl sulfate (DTD), succinonitrile (SN), adiponitrile (AND), sulfonate cyclic quaternary ammonium salt, tris(trimethylsilyl) phosphate (TMSP), tris(trimethylsilyl) borate (TMSB) and anisole.
[0220] Isolation film
[0221] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0222] In some embodiments, the material of the separator may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0223] In some embodiments, the thickness of the isolation film is 6 μm to 40 μm, and optionally 12 μm to 20 μm.
[0224] Electrode assembly, electrochemical energy storage device, secondary battery, power device
[0225] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0226] In some embodiments, the electrochemical energy storage device may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0227] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0228] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft shell, such as a pouch-type soft shell. The material of the soft shell can be plastic. Further, non-limiting examples of plastic can include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0229] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG3 shows a secondary battery 5 having a square structure as an example.
[0230] In some embodiments, referring to FIG4 , the outer package may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the separator can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to actual needs.
[0231] In a fourth aspect, the present application provides an electrical device comprising at least one of the composite current collector described in the first aspect of the present application, the positive electrode sheet described in the second aspect of the present application, and the secondary battery described in the third aspect of the present application.
[0232] Secondary batteries can be used as power sources or energy storage units for electrical devices. These devices include, but are not limited to, mobile devices, electric vehicles, electric trains, ships, satellites, and energy storage systems. Examples of mobile devices include, but are not limited to, mobile phones and laptops; and examples of electric vehicles include, but are not limited to, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, and electric trucks.
[0233] As an electrical device, a secondary battery can be selected according to its usage requirements.
[0234] FIG5 shows an example of an electric device 6. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the electric device's requirements for high power and high energy density of secondary batteries, a battery pack or battery module may be used.
[0235] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0236] In a fifth aspect, the present application provides a method for preparing the composite current collector described in the first aspect of the present application, which comprises the following steps: forming a conductive layer on at least one side of a support layer to prepare a composite current collector.
[0237] A supporting layer with a specific thickness d1, a specific tensile fracture strength T1, a specific yield strength Q1 and a specific elastic modulus G1 is used to further form a conductive layer with a specific thickness d2, a specific tensile fracture strength T2 and a specific elastic modulus G2. The prepared composite current collector has a high ductility coefficient, a high elongation at break, and better processability in mass production, which is beneficial to reducing the fracture of the composite current collector during the electrode processing process and improving the processing quality rate. It can also reduce or avoid the increase in local interfacial side reactions caused by wrinkling of the electrode during the charging and discharging process, thereby improving the battery cycle performance; and at the cell level, it is beneficial to reduce the cracking problem that may be caused by the gradual increase in the expansion force of the electrode in the later stage of the cell cycle, which is beneficial to improving the cycle performance and safety and reliability of the battery cell.
[0238] Methods for forming the conductive layer on at least one side of the support layer may include, but are not limited to, one or more of physical deposition (such as vapor deposition) technology, chemical deposition technology, electroplating, spraying, casting, hot pressing, and the like.
[0239] It can be understood that the conductive layer can be formed on at least one side surface of the support layer, but is not limited thereto.
[0240] In a sixth aspect, the present application provides a method for preparing a negative electrode sheet, which can be used to prepare the negative electrode sheet described in the second aspect of the present application.
[0241] In some embodiments, a method for preparing a negative electrode sheet is provided, comprising the steps of coating a negative electrode slurry on at least one side of the composite current collector described in the first aspect of the present application, drying, and cold pressing to prepare a negative electrode sheet.
[0242] The method for preparing the negative electrode sheet provided in this aspect can also refer to the second aspect of this application.
[0243] The drying step after coating the negative electrode slurry can be performed in a conventional manner in the art, for example, by drying at 90° C. to 120° C.
[0244] The cold pressing step after drying the coating layer can be performed using conventional methods in the art. Cold pressing can produce a negative electrode sheet having a predetermined compaction density. Non-limiting examples of the compaction density of the negative electrode sheet can be found in the context of this application.
[0245] When the composite current collector provided in the first aspect of the present application is used to prepare the negative electrode plate, the prepared negative electrode plate can have both good energy density and high mechanical strength, which can reduce or avoid the increase in local interfacial side reactions caused by wrinkling of the plate during the charging and discharging process, thereby improving the battery cycle performance; further preparation of a secondary battery containing the aforementioned composite current collector or the aforementioned negative electrode plate is also beneficial to reducing the cracking problem that may be caused by the gradual increase in the expansion force of the plate in the later stage of the battery cell cycle, which is beneficial to improving the cycle performance and safety and reliability of the battery cell.
[0246] Below, some embodiments of the present application are described. The embodiment described below is exemplary, is only used to explain the present application, and cannot be construed as limiting the present application. In the embodiment, if no technology or conditions are indicated, it is carried out according to the description above, or according to the technology or conditions described in the document in this area or according to the product specification. Reagents used or instruments that are not indicated by the manufacturer are conventional products that can be obtained commercially, or can be synthesized in a conventional manner by commercially available products.
[0247] Preparation of negative electrode current collector
[0248] 1.1. Preparation of composite current collector for negative electrode
[0249] Refer to Table 1 and Table 2 to select the materials for the support layer and the conductive layer of Examples 1-20 and Comparative Examples 1-7 to prepare the negative electrode current collector; with respect to other parameters other than Table 1 and Table 2, Examples 1-20 and Comparative Examples 1-7 are basically the same and can be appropriately adjusted to meet the requirements of the preparation parameters in Table 1 and Table 2.
[0250] The preparation method of the negative electrode current collector using Example 1 as an example: a 10 μm thick PP base film roll (as a support layer) is used, and a 2 μm thick Cu layer is deposited on its front and back surfaces using vacuum vapor deposition technology (as a conductive layer, 1 μm thick on each side), to obtain a 12 μm thick aluminum composite current collector, named "12 μm CP". A vacuum evaporation equipment (Baofeng FZZ-1650) is used, and the vacuum degree is controlled at ≤1×10 -3 Pa, membrane speed 300m / min, copper wire feed rate 500mm / min, heating power 6kW-12kW, single deposition thickness of approximately 50nm, and 20 deposition passes in both directions to achieve a Cu metal layer thickness of 1μm on each side. The prepared composite current collector was used as the negative electrode current collector in Example 1.
[0251] In Example 19, the negative electrode current collector was prepared using a method basically consistent with that in Example 1, except that the conductive layer was prepared using copper alloy (model T18010).
[0252] In Example 20, the negative electrode current collector was prepared using a method basically consistent with that in Example 1, except that the conductive layer was prepared using copper alloy (model C19910).
[0253] In Comparative Example 8, no support layer was provided, and a copper foil (Cu foil) with a thickness of about 6 μm was used as the negative electrode current collector (denoted as “6 μm Cu”), as shown in Table 1.
[0254] 1.2. Parameter Control
[0255] (1) Measurement of support layer thickness and conductive layer thickness
[0256] The thickness of the base film (support layer) and the metal layer (conductive layer) in the composite current collector was measured by Ar ion polishing the cross section (JEOL IB19500CP) and then magnifying it to 10,000 times using a scanning electron microscope (JEOL IB-19500).
[0257] (2) Yield strength, tensile strength, elastic modulus and elongation at break tests
[0258] The tensile test was performed using an INSTRON 3365 tensile testing machine to measure the tensile properties of the polymer base film, metal conductive layer, and composite current collector. The sample width was 15 mm, the length was 150 mm, the stretching distance was 50 mm, and the stretching rate was 50 mm / min.
[0259] Yield strength = yield point tensile force / sample cross-sectional area; where sample cross-sectional area = 15 mm × sample thickness;
[0260] Tensile strength at break = tensile force at break / cross-sectional area of sample; where cross-sectional area of sample = 15 mm × sample thickness;
[0261] Elongation at break = (length of sample stretched to break - 50) / 50 × 100%; the unit of the length of sample stretched to break is the same as the unit of the stretched distance, mm; Elastic modulus = tensile strength corresponding to 1% elongation / 1%.
[0262] Elastic modulus = tensile strength in the elastic deformation stage / corresponding elongation. For the convenience of calculation, the tensile strength corresponding to 1% elongation (elastic deformation stage) / 1% is used for calculation.
[0263] In addition, since the conductive layer is relatively thin, the conductive layer is prepared into samples with a uniform thickness (within the range of 10 μm to 100 μm) for tensile testing.
[0264] Secondary battery assembly:
[0265] Choose NCM 811 The positive electrode material / graphite negative electrode material chemical system 60Ah battery cell was evaluated.
[0266] The current collectors of Examples 1-20 and Comparative Examples 1-8 were used in the preparation of negative electrode sheets, and the coating weight of the negative electrode slurry was 12 mg / cm 2 The negative electrode active material accounts for 96.5% of the dry weight of the negative electrode slurry, and the compaction density is 1.65g / cm 3The negative electrode slurry is composed of graphite (as the negative electrode active material), Super-P conductive agent, styrene-butadiene rubber (as a binder) and CMC (sodium carboxymethyl cellulose, as a plasticizer) mixed in a mass ratio of 96.5:1.5:1:1, and the solvent is water.
[0267] The current collector of the positive electrode sheet is an aluminum foil with a thickness of 13 μm, and the active material coating weight of the positive electrode sheet is 20 mg / cm 2 The positive electrode active material accounts for 97% of the dry weight of the positive electrode slurry, and the compaction density is 3.5g / cm 3 The composition of the positive electrode slurry is: a mixture of ternary positive electrode active material, Super-P conductive agent and PVDF (polyvinylidene fluoride) binder in a mass ratio of 97:1.5:1.5, and the solvent is NMP (N-methylpyrrolidone).
[0268] A polypropylene diaphragm with a thickness of 7 μm was used.
[0269] A solution prepared by dissolving 1 mol / L (M) of lithium hexafluorophosphate (LiPF6) in ethylene carbonate / ethyl methyl carbonate (EC / EMC) was used as the electrolyte.
[0270] Table 1. Negative electrode current collector
[0271] In Table 1, PP represents polypropylene, PET represents polyethylene terephthalate, PI-1 represents homphenyl polyimide, and PI-2 represents biphenyl polyimide.
[0272] Table 2. Negative electrode current collector
[0273] In Table 2, the extension coefficient is equal to (d1×T1-(d2×T2)×(1-α)-d1×Q1×α); the distribution coefficient α=G1 / (G1+G2).
[0274] Test methods and analysis:
[0275] 1. Processing performance characterization:
[0276] 1.1. Coating production rate, also known as coating rate or production rate
[0277] The coating production rate is calculated by recording the number of meters of qualified coated electrodes produced through the coating process for 100,000 meters of composite current collector.
[0278] 1.2. Cold pressing cracking frequency, also recorded as cold pressing fracture frequency
[0279] The frequency of cold pressing cracking of the composite current collector is evaluated by recording the number of times the electrode coated with the composite current collector of 100,000 meters is cracked during the cold pressing process; the unit is km / time, and the higher the value, the less likely it is to crack.
[0280] 1.3. Cold pressing elongation
[0281] The cold pressing elongation rate of the electrode was evaluated by measuring the extended length of a 1m long composite current collector coated electrode after cold pressing, where the cold pressing elongation rate = (length of the electrode after cold pressing - 1) / 1 × 100%, where the unit of the length of the electrode after cold pressing is meter (m). The cold pressing elongation rate of each embodiment was determined by taking the average value of 5 measurements.
[0282] 2. Battery performance characterization
[0283] 2.1. Battery cell energy density
[0284] The battery cells prepared in each embodiment and comparative example were subjected to charge and discharge tests using a battery tester (Xinwei 5V100A) to evaluate the cycle performance of the battery. The test voltage range was 4.25V-2.5V, and the charge and discharge current rate was 1C / 1C.
[0285] The energy density of the battery = the initial capacity of the battery at a current density of 1C × the voltage platform / the weight of the battery cell, where the capacity and voltage platform of the battery cell are directly read from the charge and discharge data, and the weight of the battery cell is obtained by weighing with a balance with three decimal places of accuracy.
[0286] 2.2. Battery cell cycle performance
[0287] The battery cell cycle number is the number of cycles corresponding to the cell capacity decaying to 80% of the capacity of the first cycle of the cell.
[0288] Test results and analysis:
[0289] The tensile strength and elongation at break of the negative electrode current collectors prepared in the above embodiments and comparative examples can be found in Table 3. The test results of the cell energy density and cell cycle performance of the secondary batteries prepared in the above embodiments and comparative examples can be found in Table 3.
[0290] The tensile strength and elongation at break of a current collector have the following physical meanings: The tensile strength is the ratio of the maximum stress a current collector can withstand before breaking to its cross-sectional area before stretching, while the elongation at break is the ratio of the elongation at break to its length before stretching. Higher tensile strength and elongation at break indicate better processing performance and a lower likelihood of breakage during battery cell fabrication.
[0291] The negative electrode composite current collectors prepared in Examples 1-17, 19-20 of the present application all have high tensile strength and elongation at break, good processability, and good energy density. The support layer in Example 18 is thicker than that in other examples, and the negative electrode composite current collectors prepared therefrom all have high tensile strength and elongation at break, good processability, and a certain energy density. It should be noted that compared to the low energy density of the current collector without a support layer (traditional copper foil), Example 18 still has a certain energy density advantage. The test results of the traditional copper foil positive electrode current collector can be found in Comparative Example 8.
[0292] Examples 1-20 all exhibited excellent cell cycling performance, with the number of cycles to 80% capacity decay exceeding 800. Examples 1-16 and 18-20 all achieved cycle numbers exceeding 1000 and 1150. The conductive layer thickness of Example 17 was thinner than that of the other examples, and although the number of cycles to 80% capacity decay was lower than that of Examples 1-16 and 18-20, it still showed a certain degree of improvement compared to Comparative Examples 1-7.
[0293] Examples 1-20 all have a higher coating production excellence rate, a higher cold pressing elongation rate and a higher cold pressing cracking frequency in the unit of "km / time" (that is, less prone to cracking), which shows that they all have good processability; among them, the coating production excellence rates in Examples 1-20 are all above 80%, generally higher than 85%, and most are higher than 90%, and some can achieve ≥99%; the cold pressing elongation rates in Examples 1-20 are generally ≥0.5% (further generally ≥0.6%), among which, the cold pressing elongation rates of Examples 1-17 and 19-20 are ≥0.6%; the cold pressing cracking rate of Examples 1-20 is ≥5km / time, and is not prone to cracking.
[0294] The ductility coefficients of the composite current collectors in the negative electrode sheets of Comparative Examples 1-7 are all lower than 150 Pa·m. At this time, the tensile fracture strength of the composite current collectors in the negative electrode sheets generally decreases, and the elongation at fracture is significantly reduced, resulting in poor overall mechanical properties and significantly poor processability of the composite current collectors. The coating production rate is all lower than 60%, less than 10% for Comparative Example 2, and less than 40% for Comparative Examples 1, 4, 5, and 7.
[0295] Although the supporting layer thickness d1, tensile fracture strength T1, yield strength Q1, elastic modulus G1, and the total thickness d2, tensile fracture strength T2, elastic modulus G2 of the conductive layer, and the distribution coefficient α of the composite current collector in Comparative Examples 1 and 6 are within the parameter ranges of Examples 1-20, since the ductility coefficient of the composite current collector is lower than 150 Pa·m, the overall mechanical properties of the composite current collector are significantly reduced, and the processability is significantly deteriorated, and the coating production rate and the frequency of cold pressing cracking are both low.
[0296] The support layer of Comparative Example 2 is thinner, the yield strength Q1 and tensile fracture strength T1 of the support layer of Comparative Example 3 are relatively low, the conductive layer of Comparative Example 4 is thicker, the yield strength Q1 and tensile fracture strength T1 of the support layer of Comparative Example 5 are relatively low, and the elastic modulus G2 of the conductive layer of Comparative Example 7 is relatively high, all of which lead to the ductility coefficient of the composite current collector being lower than 150 Pa·m, the overall mechanical properties of the prepared composite current collector are significantly reduced, and the processability is significantly deteriorated, and the coating production rate and cold pressing cracking frequency are both low.
[0297] Table 3.
[0298] In Table 3, the number of cycles of the battery cell is the number of cycles corresponding to the battery cell capacity decaying to 80% of the capacity of the first cycle of the battery cell.
[0299] The technical features of the above-mentioned embodiments and examples can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments and examples are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0300] It should be noted that the present application is not limited to the above-mentioned embodiments and examples. The above-mentioned embodiments and examples are only examples. Within the scope of the technical solution of the present application, embodiments that have substantially the same structure as the technical idea and exert the same effect are all included in the technical scope of the present application. The above embodiments and examples only express several embodiments of the present application, and their descriptions are relatively detailed, but they cannot be understood as limiting the scope of the patent. In addition, without departing from the scope of the subject matter of the present application, various modifications that can be thought of by those skilled in the art are applied to the embodiments, and other methods of constructing by combining some of the constituent elements in the embodiments are also included in the scope of the present application. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all fall within the scope of protection of the present application. Therefore, the scope of protection of the present application shall be based on the attached claims, and the description and drawings may be used to explain the content of the claims.
Claims
1. A composite current collector, comprising a support layer and a conductive layer disposed on at least one side of the support layer, wherein the support layer is an organic support layer; The thickness of the support layer is denoted as d1, the tensile strength is denoted as T1, the yield strength is denoted as Q1, and the elastic modulus is denoted as G1; The total thickness of the conductive layer is denoted as d2, the tensile strength at break is denoted as T2, and the elastic modulus is denoted as G2; The composite current collector satisfies the following conditions: (d1×T1-(d2×T2)×(1-α)-d1×Q1×α)≥150Pa·m, where α=G1 / (G1+G2).
2. The composite current collector according to claim 1, wherein: The thickness d1 of the support layer is 2 μm-13 μm; Optionally, the thickness d1 of the support layer is 2.4 μm-8 μm; Further optionally, the thickness d1 of the support layer is 2.8 μm-6 μm.
3. The composite current collector according to claim 1 or 2, wherein: The tensile fracture strength T1 of the support layer is ≥200MPa; Optionally, the tensile fracture strength T1 of the support layer is ≥300 MPa.
4. The composite current collector according to any one of claims 1 to 3, wherein: The yield strength Q1 of the support layer is ≥80MPa; Optionally, the yield strength Q1 of the support layer is ≥100 MPa.
5. The composite current collector according to any one of claims 1 to 4, wherein: The composite current collector satisfies any one or more of the following characteristics: The total thickness d2 of the conductive layer is 0.6 μm-2.4 μm; optionally, the total thickness d2 of the conductive layer is 1 μm-2.4 μm; further optionally, the total thickness d2 of the conductive layer is 1.4 μm-2.0 μm; The single-side thickness d2 of the conductive layer s 0.3 μm-1.2 μm; Optionally, the single-side thickness d2 of the conductive layer s 0.5 μm-1.2 μm; further optionally, the single-side thickness d2 of the conductive layer s 0.7μm-1.0μm; The thickness D of the composite current collector a 3 μm-15 μm; Optionally, the thickness D of the composite current collector a 3 μm-10 μm; further optionally, the thickness D of the composite current collector a 4.4μm-6μm.
6. The composite current collector according to any one of claims 1 to 5, wherein: The tensile strength of the conductive layer is T2≥250MPa; Optionally, the tensile fracture strength T2 of the conductive layer is ≥300 MPa.
7. The composite current collector according to any one of claims 1 to 6, wherein: The composite current collector satisfies any one or more of the following characteristics: The elastic modulus G1 of the support layer is ≥2 GPa; optionally, the elastic modulus G1 of the support layer is ≥3 GPa; The elastic modulus G2 of the conductive layer is 40 GPa-70 GPa; optionally, the elastic modulus G2 of the conductive layer is 45 GPa-55 GPa; The α is 0.045-0.30; optionally, the α is 0.05-0.15; further optionally, the α is 0.055-0.
12.
8. The composite current collector according to any one of claims 1 to 7, wherein: (d1×T1-(d2×T2)×(1-α)-d1×Q1×α)≥200Pa·m; Optionally, (d1×T1-(d2×T2)×(1-α)-d1×Q1×α)≥250Pa·m.
9. The composite current collector according to any one of claims 1 to 8, wherein: The material of the support layer is a polymer-based material or a polymer-based composite material; Optionally, the polymer component in the supporting layer includes polyimide, polyamide, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyethylene, polypropylene, polypropylene, acrylonitrile-butadiene-styrene copolymer, polyvinyl alcohol, polystyrene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, sodium polystyrene sulfonate, polyacetylene, silicone rubber, polyformaldehyde, polyphenylene ether, polyphenylene sulfide, polyethylene glycol, polysulfur nitride polymer materials, polyphenylene, polypyrrole, polyaniline, polythiophene, polypyridine, cellulose, starch, protein, epoxy resin, phenolic resin, and one or more of the derivatives of the above materials, the cross-linked products of the above materials and the copolymers of the above materials.
10. The composite current collector according to any one of claims 1 to 9, wherein: The polymer component in the support layer includes polyimide, and the polyimide includes one or both of homophenyl polyimide and biphenyl polyimide; Optionally, the polymer component in the support layer includes biphenyl polyimide; Further optionally, the support layer comprises biphenyl polyimide in an amount of ≥50% by mass; Further optionally, the support layer comprises biphenyl polyimide in an amount of ≥80% by mass; Further optionally, the material of the support layer is biphenyl polyimide.
11. The composite current collector according to any one of claims 1 to 10, wherein: The conductive layer includes a metal material. Optionally, the metal material includes one or more of copper and a copper alloy.
12. A negative electrode sheet, comprising the composite current collector according to any one of claims 1 to 11.
13. A secondary battery, wherein: The secondary battery comprises at least one of the composite current collector according to any one of claims 1 to 11 and the negative electrode sheet according to claim 12. 14 . An electrical device comprising at least one of the composite current collector according to claim 1 , the negative electrode sheet according to claim 12 , and the secondary battery according to claim 13 . 15 . The method for preparing the composite current collector according to claim 1 , comprising the following steps: forming the conductive layer on at least one side of the support layer to prepare the composite current collector.
16. A method for preparing a negative electrode sheet, comprising the following steps: coating a negative electrode slurry on at least one side of the composite current collector according to any one of claims 1 to 11, drying, and cold pressing to prepare the negative electrode sheet.
Citation Information
Patent Citations
Current collector, electrode pole sheet and electrochemical device
CN110660998A
Composite current collector, electrode plate and electrochemical device
CN110943227A
Positive current collector, positive pole piece and electrochemical device
CN111180736A
Positive current collector, positive pole piece and electrochemical device
CN112186196A
Positive current collector, positive pole piece, electrochemical device, electric vehicle and electronic product
CN112259744A
Cited By
Electrolyte, preparation method thereof and lithium ion battery
CN121642146A