Low-friction, long-service-life superlattice composite coating, preparation method therefor and use thereof

By forming a superlattice composite coating with low friction and long life on the surface of the space mechanism, the problem of insufficient hardness and wear resistance of the molybdenum disulfide-based coating in a high vacuum environment is solved, and high hardness and low friction performance are achieved, satisfying the High reliability requirements for long-lived space institutions.

WO2024244380A1PCT designated stage expired Publication Date: 2024-12-05NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI

Patent Information

Application Number
PCT/CN2023/137948
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2023-12-11
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing molybdenum disulfide-based solid lubricating coatings have problems such as low hardness, poor load-bearing capacity and easy oxidation failure in high vacuum environments, which cannot meet the high reliability needs of long-life space mechanisms.

Method used

The titanium transition layer, TiNx bearing layer, TiNx/MoS2 gradient transition layer, MoS2/Me gradient transition layer and MoS2/Me superlattice layer are deposited successively on the substrate surface by unbalanced magnetron sputtering technology, forming a super-low friction and long life Lattice composite coating, the hardness and friction performance of the coating are improved by the design of TiNx/MoS2 gradient transition layer and MoS2/Me superlattice layer.

Benefits of technology

The coating is achieved with high hardness (greater than 7GPa), high binding force and low friction coefficient (the friction coefficient of vacuum environment is as low as 0.005-0.02), which significantly improves the service life and efficiency of the space mechanism.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023137948_05122024_PF_FP_ABST
    Figure CN2023137948_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present application discloses a low-friction, long-service-life superlattice composite coating, a preparation method therefor and a use thereof. The superlattice composite coating comprises: a titanium transition layer, a TiNx bearing layer, a TiNx / MoS2 gradient transition layer, a MoS2 / Me gradient transition layer, and a MoS2 / Me superlattice layer sequentially formed on the surface of a substrate. In the direction gradually away from the substrate, the MoS2 content in the TiNx / MoS2 gradient transition layer shows an increasing trend, and the MoS2 content in the MoS2 / Me gradient transition layer shows a decreasing trend. The superlattice composite coating of the present application has excellent mechanical and tribological properties, has a vacuum friction coefficient of less than 0.02 and a friction life of more than 4×106 revolutions, and can thus meet the requirements of ultra-low friction and ultra-long service life of aerospace vehicles. Additionally, the preparation method for the composite coating provided in the present application is simple, stable, and effective, and has significant practical value and economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

A low-friction, long-life superlattice composite coating and its preparation method and use

[0001] This application is based on and claims priority from the Chinese patent application with application number 202310611417.0 filed on May 29, 2023, and entitled “A low-friction, long-life superlattice composite coating, its preparation method and use”. Technical Field

[0002] The present application belongs to the technical field of solid lubricating coatings on the surface of space mechanisms, and specifically relates to a low-friction, long-life superlattice composite coating, and a preparation method and use thereof. Background Art

[0003] Metal friction pairs in space vehicles face severe cold welding and high-friction wear issues under high-vacuum conditions. Solid lubricant coatings are critical materials for preventing cold welding, providing lubrication, and extending their service life. Studies have shown that a significant proportion of spacecraft moving component failures are related to space lubrication. Premature failure of space lubricant coatings can have extremely serious consequences for space vehicles, even leading to complete system failure. Therefore, to ensure that space vehicles can function effectively and achieve high reliability and an extremely long service life, high-performance space solid lubrication is an essential technology. Currently, molybdenum disulfide (MoS2) coatings are widely used, thanks to their interlayer bonding via weak van der Waals bonds, allowing for easy sliding between layers and exhibiting excellent lubrication properties. However, with the development of long-life low-Earth orbit spacecraft and deep space probes, the current MoS2-based solid lubricant coatings will no longer be able to guarantee high reliability and an extremely long service life for space vehicles.

[0004] To date, various types of molybdenum disulfide coatings have been developed at home and abroad through different preparation technologies, and the process technology and methods have a great impact on their performance. Unbalanced magnetron sputtering is a green low-temperature deposition technology that can accurately control the coating composition, structure and thickness through process parameters. By designing the magnetic field distribution and transition layer matching, high-density and high-adhesion molybdenum disulfide coatings can be obtained. It has become the main preparation technology for solid lubricant coatings for friction pairs of key space mechanisms. However, traditional sputtered molybdenum disulfide coatings are usually (001) crystal plane orientation or amorphous structure, with low coating hardness and poor load-bearing capacity. In addition, its columnar structure is easily corroded by water and oxygen in humid air during transportation and storage, causing the coating's lubrication performance to deteriorate and oxidize to fail. Therefore, how to obtain a new type of molybdenum disulfide-based lubricating coating with high hardness, high load-bearing capacity, ultra-low friction and ultra-long life is an important problem that needs to be solved urgently for the new generation of long-life space mechanisms.

[0005] Summary of the Invention

[0006] The main purpose of this application is to provide a low-friction, long-life superlattice composite coating and its preparation method and use, so as to overcome the shortcomings of the existing technology.

[0007] To achieve the aforementioned invention objectives, the technical solutions adopted in this application include:

[0008] The embodiment of the present application provides a low-friction and long-life superlattice composite coating, which comprises: a titanium transition layer, a TiN transition layer, and a x Carrier layer, TiN x / MoS2 gradient transition layer, MoS2 / Me gradient transition layer and MoS2 / Me superlattice layer;

[0009] Wherein, x is 0.5 to 1, Me includes any one or a combination of two or more of Ti, Zr, V, Nb, Cr, Mo, Zn, and Cd; and, in a direction gradually away from the substrate, the TiN x The content of MoS2 in the MoS2 / MoS2 gradient transition layer tends to increase, and the content of MoS2 in the MoS2 / Me gradient transition layer tends to decrease; the MoS2 / Me superlattice layer includes alternately stacked MoS2 layers and Me layers; the MoS2 layers in the MoS2 / Me superlattice layer grow in an orientation parallel to the MoS2 (002) plane.

[0010] The present invention also provides a method for preparing the aforementioned low-friction and long-life superlattice composite coating, which comprises: depositing a titanium transition layer, a TiN transition layer, and a TiN transition layer on the substrate surface in sequence by using an unbalanced magnetron sputtering technique. x Carrier layer, TiN x / MoS2 gradient transition layer, MoS2 / Me gradient transition layer and MoS2 / Me superlattice layer to obtain the low-friction and long-life superlattice composite coating.

[0011] The embodiments of the present application also provide the use of the low-friction, long-life superlattice composite coating in the field of surface protection of space mechanisms.

[0012] Compared with the prior art, the present invention has the following advantages:

[0013] (1) This application adopts the unbalanced magnetron sputtering technology of Ar and N2 reactive sputtering to prepare TiN by the reaction of Ti and nitrogen plasma. x Carrier layer and TiN x / MoS2 gradient transition layer, the coating provides excellent mechanical properties of strong bonding (greater than 15N) and high hardness (greater than 7GPa), suitable for surface protection of components in high-impact environments; and can significantly improve the wear resistance of the coating, which is beneficial to extending the service life of space mechanisms;

[0014] (2) This application adopts the non-balanced magnetron sputtering technology of multi-target alternating deposition, and prepares the MoS2 / Me superlattice coating by alternating deposition of amorphous metal phase and molybdenum disulfide. The provided coating has the characteristics of preferred orientation of the (0002) crystal plane of molybdenum disulfide, which can greatly reduce the friction coefficient and wear rate of the coating. The friction coefficient in vacuum environment is as low as 0.005-0.02, and the friction life exceeds 4×10 6 The rotation is conducive to improving the efficiency, reliability and service life of space agencies. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments recorded in this application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0016] Figure 1 is a TiN prepared in Example 3 of the present application. x -SEM image of the cross section of MoS2 / Zn-3 coating;

[0017] Figure 2 is a TiN prepared in Example 3 of the present application. x -Hardness and elastic modulus test graph of MoS2 / Zn-3 coating;

[0018] FIG3 is a TiN prepared in Example 3 of the present application. x - Adhesion morphology and force curve of MoS2 / Zn-3 coating;

[0019] FIG4 is a TiN prepared in Example 3 of the present application x -Friction curve of MoS2 / Zn-3 coating in vacuum environment;

[0020] Figure 5 is a TiN prepared in Example 3 of the present application x -Friction life curve of MoS2 / Zn-3 coating in vacuum environment.

[0021] FIG6 is a transmission electron microscope image of the MoS2 layer in the MoS2 / Me superlattice layer prepared in a typical embodiment of the present application grown in an orientation parallel to the MoS2 (002) plane. DETAILED DESCRIPTION

[0022] In view of the defects of the existing technology, the inventors of this case have proposed the technical solution of this application after long-term research and extensive practice. The bonding mode, bonding form and other physical properties of the coating and the substrate are crucial to the bonding strength, mechanical properties and tribological properties of the coating, especially the wear resistance of the coating. x Carrier layer, TiNx The MoS2 / Me lubricating coating is applied between the substrate and the MoS2 / Me lubricating coating, significantly impacting its adhesion, load-bearing capacity, and mechanical properties. The interface introduced by the superlattice structure promotes the growth of MoS2 (002) planes in a parallel orientation, further improving the coating's structural density and enhancing its mechanical and tribological properties.

[0023] The technical solutions of this application are described clearly and completely below. Obviously, the embodiments described are only a portion of the embodiments of this application, not all of them. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of this application without creative effort are also within the scope of protection of this application.

[0024] Specifically, as one aspect of the technical solution of the present application, a low-friction and long-life superlattice composite coating is provided, which comprises: a titanium transition layer, a TiN transition layer, and a TiN transition layer formed on the surface of a substrate in sequence. x Carrier layer, TiN x / MoS2 gradient transition layer, MoS2 / Me gradient transition layer and MoS2 / Me superlattice layer;

[0025] Wherein, x is 0.5 to 1, Me includes any one or a combination of two or more of Ti, Zr, V, Nb, Cr, Mo, Zn, and Cd; and, in a direction gradually away from the substrate, the TiN x The content of MoS2 in the MoS2 / MoS2 gradient transition layer tends to increase, and the content of MoS2 in the MoS2 / Me gradient transition layer tends to decrease; the MoS2 / Me superlattice layer includes alternately stacked MoS2 layers and Me layers; the MoS2 layers in the MoS2 / Me superlattice layer grow in an orientation parallel to the MoS2 (002) plane.

[0026] In the traditional sputtering process of MoS2, high-energy plasma during PVD sputtering causes defects in the deposited MoS2, causing MoS2 to preferentially grow in the (100) plane direction, where the interplanar spacing of the (100) plane is 0.31nm. However, the present application adopts a method of alternating deposition of MoS2 layers and Me layers. Based on the interaction between MoS2 and the metal interface, the MoS2 layer grows in an orientation parallel to the MoS2 (002) plane. Specifically, the transmission electron microscope image of the MoS2 layer in the MoS2 / Me superlattice layer prepared in the present application growing in an orientation parallel to the MoS2 (002) plane can be seen in Figure 6. It can be seen from Figure 6 that the interplanar spacing of molybdenum disulfide is 0.62nm, indicating that the MoS2 layer grows in an orientation parallel to the MoS2 (002) plane.

[0027] In some preferred embodiments, the hardness of the superlattice composite coating is above 7 GPa.

[0028] In some preferred embodiments, the bonding force between the superlattice composite coating and the substrate is above 15N, and the material of the substrate includes, but is not limited to, 316L stainless steel, TC4 titanium alloy, or single crystal silicon wafer.

[0029] In some preferred embodiments, the friction coefficient of the superlattice composite coating in a vacuum environment is less than 0.02, and the wear life is less than 4×10 6 Turn above.

[0030] Furthermore, the friction coefficient of the superlattice composite coating in a vacuum environment is 0.005 to 0.02.

[0031] In some preferred embodiments, the superlattice composite coating has a thickness of 2.0 to 3.0 μm.

[0032] In some preferred embodiments, the thickness of the titanium transition layer is 50 to 150 nm.

[0033] In some preferred embodiments, the TiN x The thickness of the supporting layer is 150 to 300 nm.

[0034] In some preferred embodiments, the TiN x The thickness of the MoS2 gradient transition layer is 50 to 150 nm.

[0035] In some preferred embodiments, the thickness of the MoS2 / Me gradient transition layer is 100 to 300 nm.

[0036] In some preferred embodiments, the thickness of the MoS2 / Me superlattice layer is 1.5 to 2.5 μm.

[0037] In some preferred embodiments, the modulation ratio of MoS2 to Me in the MoS2 / Me superlattice layer is t MoS2 ∶t Me It is 5:1-2:1.

[0038] In some preferred embodiments, the modulation period of the MoS2 / Me superlattice layer is Λ=4-20 nm.

[0039] In some preferred embodiments, the metal atom content in the MoS2 / Me superlattice layer is 5 to 15 at%.

[0040] In some preferred embodiments, the MoS2 / Me superlattice layer comprises a plurality of alternatingly stacked periodic layers, and each alternatingly stacked periodic layer comprises a MoS2 layer and a Me layer.

[0041] Another aspect of the embodiment of the present application further provides a method for preparing the aforementioned low-friction, long-life superlattice composite coating, which comprises: depositing a titanium transition layer, a TiN transition layer, and a TiN transition layer on the substrate surface in sequence by using an unbalanced magnetron sputtering technique; x Carrier layer, TiN x / MoS2 gradient transition layer, MoS2 / Me gradient transition layer and MoS2 / Me superlattice layer to obtain a superlattice composite coating with low friction and long life.

[0042] In some preferred embodiments, the preparation method includes: using unbalanced magnetron sputtering technology, using a titanium target as a cathode target material, using an inert gas as a working gas, applying a sputtering current to the titanium target, and applying a negative bias to the substrate, thereby depositing a titanium transition layer on the surface of the substrate, wherein the sputtering current is 3.0~5.0A, the substrate bias is -100~-150V, the working gas flow rate is 20~30sccm, the substrate temperature is 50~150℃, the reaction chamber pressure is 0.1~2.0Pa, and the deposition time is 300~900s.

[0043] Furthermore, the inert gas is argon, but is not limited thereto.

[0044] In some preferred embodiments, the preparation method specifically includes: using unbalanced magnetron sputtering technology, using a titanium target as a cathode target, using an inert gas and N2 as a working gas, applying a sputtering current to the titanium target, and applying a negative bias voltage to the substrate, thereby depositing TiN on the surface of the titanium transition layer. x The carrier layer is characterized in that the sputtering current is 3.0 to 5.0 A, the substrate bias is -100 to -150 V, the flow rate of the inert gas is 20 to 30 sccm, the flow rate of N2 is 5 to 15 sccm, the substrate temperature is 50 to 150° C., the reaction chamber pressure is 0.1 to 2.0 Pa, and the deposition time is 2400 to 4800 s.

[0045] Furthermore, the inert gas is argon, but is not limited thereto.

[0046] In some preferred embodiments, the preparation method specifically includes: using unbalanced magnetron sputtering technology, using titanium target and molybdenum disulfide target as cathode target materials, using inert gas and N2 as working gas, applying sputtering current to the titanium target and molybdenum disulfide target, applying negative bias to the substrate, thereby x TiN is deposited on the surface of the supporting layer x / MoS2 gradient transition layer, wherein the sputtering current applied to the titanium target gradually decreases from 3.0~5.0A to 0, the sputtering current applied to the molybdenum disulfide target gradually increases from 0 to 1.2~2.0A, the substrate bias is -30~-70V, the flow rate of the inert gas is 10~20sccm, the flow rate of N2 is 5~15sccm, the substrate temperature is 50~150℃, the reaction chamber pressure is 0.1~2.0Pa, and the deposition time is 300~900s.

[0047] Furthermore, the inert gas is argon, but is not limited thereto.

[0048] In some preferred embodiments, the preparation method specifically includes: using unbalanced magnetron sputtering technology, using a metal Me target and a molybdenum disulfide target as cathode targets, using an inert gas as a working gas, applying a sputtering current to the metal Me target and the molybdenum disulfide target, and applying a negative bias voltage to the substrate, thereby x / MoS2 gradient transition layer is deposited on the surface to obtain MoS2 / Me gradient transition layer, wherein the sputtering current applied to the metal Me target gradually increases from 0 to 0.6~1.4A, the sputtering current applied to the molybdenum disulfide target is 1.2~2.0A, the substrate bias is -30~-70V, the flow rate of inert gas is 10~20sccm, the substrate temperature is 50~150℃, the reaction chamber pressure is 0.1~2.0Pa, and the deposition time is 300~900s; the material of the metal Me target is selected from any one of Ti, Zr, V, Nb, Cr, Mo, Zn, and Cd.

[0049] Furthermore, the inert gas is argon, but is not limited thereto.

[0050] In some preferred embodiments, the preparation method specifically includes: using unbalanced magnetron sputtering technology, using a molybdenum disulfide target and a metal Me target as cathode targets, using an inert gas as a working gas, applying a negative bias to the substrate, applying a sputtering current to the molybdenum disulfide target and the metal Me target, alternately depositing MoS2 layers and Me layers, thereby depositing a MoS2 / Me superlattice layer on the surface of the MoS2 / Me gradient transition layer, thereby obtaining a superlattice composite coating, wherein the sputtering current applied to the molybdenum disulfide target is 1.2~2.0A, the sputtering current applied to the metal Me target is 0.6~1.4A, the substrate bias is -30~-70V, the working gas flow rate is 10~20sccm, the substrate temperature is 50~150℃, the reaction chamber pressure is 0.1~2.0Pa, and the deposition time is 6000~8000s; the deposition time for each cycle of alternating deposition of MoS2 layers and Me layers is 10~90s.

[0051] Furthermore, the inert gas is argon, but is not limited thereto.

[0052] In some preferred embodiments, the preparation method further comprises: evacuating the reaction chamber to a vacuum degree of 3.0×10 -5 torr, the cleaned substrate is first subjected to plasma etching.

[0053] Furthermore, the plasma etching process includes: applying a bias voltage of -400 to -500 V to the substrate, the substrate temperature is 50 to 150° C., and the etching time is 1200 to 2400 s.

[0054] In some preferred embodiments, the material of the substrate includes 316L stainless steel, TC4 titanium alloy or single crystal silicon wafer, but is not limited thereto.

[0055] In some preferred embodiments, the substrate comprises a spatial mechanism.

[0056] In some more specific embodiments, the method for preparing the low-friction and long-life superlattice composite coating comprises:

[0057] The method adopts an unbalanced magnetron sputtering technology, uses a titanium target as a cathode target material, uses Ar as a working gas, applies a sputtering current to the titanium target, and applies a negative bias voltage to the substrate, thereby depositing a titanium transition layer on the substrate surface, wherein the sputtering current is 3.0 to 5.0 A, the substrate bias voltage is -100 to -150 V, the working gas flow rate is 20 to 30 sccm, the substrate temperature is 50 to 150 ° C, the reaction chamber pressure is 0.1 to 2.0 Pa, and the deposition time is 300 to 900 s; the method adopts an unbalanced magnetron sputtering technology, uses a titanium target as a cathode target material, uses Ar and N2 as working gases, applies a sputtering current to the titanium target, and applies a negative bias voltage to the substrate, thereby depositing TiN on the substrate surface. x The carrier layer is characterized in that the sputtering current is 3.0 to 5.0 A, the substrate bias is -100 to -150 V, the working gas Ar flow rate is 20 to 30 sccm, the N2 flow rate is 5 to 15 sccm, the substrate temperature is 50 to 150 ° C, the reaction chamber pressure is 0.1 to 2.0 Pa, and the deposition time is 2400 to 4800 s; an unbalanced magnetron sputtering technology is adopted, with a titanium target and a molybdenum disulfide target as cathode target materials, Ar and N2 as working gases, a sputtering current is applied to the titanium target and the molybdenum disulfide target, and a negative bias is applied to the substrate, so that the TiN x TiN is deposited on the surface of the supporting layer x / MoS2 gradient transition layer, wherein the sputtering current applied to the titanium target gradually decreases from 3.0 to 5.0 A to 0, the sputtering current applied to the molybdenum disulfide target gradually increases from 0 to 1.2 to 2.0 A, the substrate bias is -30 to -70 V, the working gas Ar flow rate is 10 to 20 sccm, the N2 flow rate gradually decreases from 5 to 15 sccm to 0, the substrate temperature is 50 to 150 ° C, the reaction chamber pressure is 0.1 to 2.0 Pa, and the deposition time is 300 to 900 s; an unbalanced magnetron sputtering technology is adopted, with a molybdenum disulfide target and a metal target as cathode target materials, an inert gas Ar as the working gas, a negative bias is applied to the substrate, and a sputtering current is applied to the molybdenum disulfide target and the metal target, thereby x A MoS2 / Me gradient transition layer is deposited on a MoS2 / MoS2 gradient transition layer, wherein the sputtering current applied to the MoS2 target is 1.2-2.0 A, the sputtering current applied to the metal target gradually increases from 0 to 0.6-1.4 A, the substrate bias is -30--70 V, the working gas Ar flow rate is 10-20 sccm, the substrate temperature is 50-150°C, the reaction chamber pressure is 0.1-2.0 Pa, and the deposition time is 300-900 s; an unbalanced magnetron sputtering technique is adopted, with a MoS2 target and a metal target as cathode target materials, and an inert gas Ar as the working gas. A negative bias is applied to the substrate, a sputtering current is applied to the molybdenum disulfide target and the metal target, and the sputtering time of each target is precisely controlled by a program, thereby depositing a MoS2 / Me superlattice layer on the gradient transition layer, wherein the sputtering current applied to the molybdenum disulfide target is 1.2 to 2.0 A, the sputtering current applied to the metal target is 0.6 to 1.4 A, the substrate bias is -30 to -70 V, the working gas Ar flow rate is 10 to 20 sccm, the substrate temperature is 50 to 150 ° C, the reaction chamber pressure is 0.1 to 2.0 Pa, and the deposition time is 6000 to 8000 s; the TiN x -MoS2 / Me superlattice composite coating (the aforementioned "superlattice composite coating") includes a titanium transition layer, a TiN transition layer, and a plurality of other layers sequentially stacked in the thickness direction. x Carrier layer, TiN x / MoS2 gradient transition layer, MoS2 / Me gradient transition layer and MoS2 / Me superlattice layer.

[0058] Another aspect of the embodiments of the present application further provides the use of the aforementioned low-friction, long-life superlattice composite coating in the field of surface protection of space mechanisms.

[0059] The inventors of this case also conducted the following performance tests on the superlattice composite coating prepared above:

[0060] The coating thickness was tested using a scanning electron microscope, and the test results showed that the coating was 2.0 to 3.0 μm.

[0061] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindentation system. The diamond indenter was used to indent to a depth of 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. x -The nanohardness of MoS2 / Me superlattice composite coatings is greater than 7GPa.

[0062] Adhesion testing was performed using an automatic scratch tester. Three scratch tests were performed at different locations according to the machine's operating procedures. The experimental conditions were a loading rate of 5 to 10 N / min, a scratch length of 5 mm, and a loading force of 20 N. The test results showed that the superlattice composite coating exhibited a bonding strength greater than 15 N.

[0063] Friction and wear testing was performed using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. Laser confocal microscopy was used to measure the wear cross-section. The wear volume was multiplied by the travel step length, and the wear rate was calculated by dividing the wear volume by the load and travel. The friction coefficient and wear rate results are shown in Table 2.

[0064] Friction life testing was conducted using a CSM tribometer in a vacuum environment to analyze tribological properties. Using a 9Cr18 steel ball as the counterweight, the test was conducted at a rotational speed of 1000 rpm, an 8mm track radius, and a normal load of 5N. The test results showed that the friction coefficient remained less than 0.02 throughout the entire friction test, and the friction life was expected to reach 4.6 million revolutions.

[0065] In summary, through the above technical solutions, the superlattice composite coating provided by this application has good mechanical properties such as hardness and bonding strength, has good friction and wear performance in a vacuum environment, and can meet the requirements of lubrication stability and long service life of space mechanisms.

[0066] The technical solution of the present application is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the scope of protection of the present application is not limited to the following embodiments.

[0067] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0068] Example 1

[0069] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. Unbalanced magnetron sputtering technology is used to prepare TiN on the substrate surface. x -MoS2 / Zn-1 superlattice composite coating, mainly including the following steps:

[0070] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0071] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, the substrate temperature is 50 ~ 150 ° C. x -MoS2 / Zn-1 superlattice composite coating, the cavity is filled with high-purity argon gas, Ti target (purity of 99.99at.%), MoS2 target (purity of 99.9at.%) and Zn target (purity of 99.9at.%) are arranged and controlled, and unbalanced magnetron sputtering technology is used. The specific steps are as follows:

[0072] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0073] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 150 nm was deposited on the substrate surface.

[0074] The titanium target sputtering current is 5.0A, the substrate bias voltage is -80V, the working gas is Ar and N2, among which the Ar gas flow rate is 30sccm, the N2 flow rate is 10sccm, the deposition substrate temperature is 120℃, the pressure is 1Pa, the deposition time is 2400s, and TiN is deposited on the surface of the titanium transition layer. x Bearing layer, thickness is about 150nm;

[0075] Gradually reduce the titanium target sputtering current to 0A, and gradually increase the molybdenum disulfide target sputtering current to 1.6A. The working gases are Ar and N2, where the Ar gas flow rate is 16sccm, the N2 flow rate is 10sccm, the substrate bias is -50V, the deposition substrate temperature is 80℃, the pressure is 1.0Pa, and the deposition time is 600s. x TiN is deposited on the surface of the bearing layer x / MoS2 gradient transition layer thickness is about 100nm;

[0076] The sputtering current of the MoS2 target was kept at 1.6A, while the sputtering current of the Zn target was gradually increased to 0.6A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 80℃, the pressure was 1.0Pa, the deposition time was 600s, and the TiN x A MoS2 / Zn gradient transition layer is deposited on the surface of the MoS2 / MoS2 gradient transition layer, with a thickness of about 200 nm;

[0077] The sputtering current of the molybdenum disulfide target is kept at 1.6A, the sputtering current of Zn is kept at 0.6A, and MoS2 and Zn are deposited alternately. The target deposition time per cycle is 90s, and the total deposition time is 7000s. A MoS2 / Zn superlattice layer with a thickness of about 2μm is deposited on the surface of the MoS2 / Zn gradient transition layer.

[0078] Prepared TiN x The specific composition parameters of the -MoS2 / Zn-1 superlattice composite coating sample are shown in Table 1.

[0079] After the above deposition process, TiN x -MoS2 / Zn-1 superlattice composite coating was tested as follows:

[0080] The coating thickness was measured using scanning electron microscopy.

[0081] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0082] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0083] Example 2

[0084] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. Unbalanced magnetron sputtering technology is used to prepare TiN on the substrate surface. x -MoS2 / Zn-2 supercrystalline composite lattice coating, mainly including the following steps:

[0085] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0086] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, the substrate temperature is 50 ~ 150 ° C. x -MoS2 / Zn-2 supercrystalline composite lattice coating, the cavity is filled with high-purity argon gas, and a Ti target (purity of 99.99at.%), a MoS2 target (purity of 99.9at.%) and a Zn target (purity of 99.9at.%) are used in the control setting. The unbalanced magnetron sputtering technology is used. The specific steps are as follows:

[0087] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0088] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 150 nm was deposited on the substrate surface.

[0089] The titanium target sputtering current is 5.0A, the substrate bias voltage is -80V, the working gas is Ar and N2, among which the Ar gas flow rate is 30sccm, the N2 flow rate is 10sccm, the deposition substrate temperature is 120℃, the pressure is 1Pa, the deposition time is 4800s, and TiN is deposited on the surface of the titanium transition layer. x The bearing layer has a thickness of about 300 nm;

[0090] Gradually reduce the titanium target sputtering current to 0A, and gradually increase the molybdenum disulfide target sputtering current to 1.6A. The working gases are Ar and N2, where the Ar gas flow rate is 16sccm, the N2 flow rate is 10sccm, the substrate bias is -50V, the deposition substrate temperature is 80℃, the pressure is 1.0Pa, and the deposition time is 600s. x TiN is deposited on the surface of the bearing layer x / MoS2 gradient transition layer thickness is about 100nm;

[0091] The sputtering current of the MoS2 target was kept at 1.6A, while the sputtering current of the Zn target was gradually increased to 0.6A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 80℃, the pressure was 1.0Pa, the deposition time was 600s, and the TiN x A MoS2 / Zn gradient transition layer is deposited on the surface of the MoS2 / MoS2 gradient transition layer, with a thickness of about 200 nm;

[0092] The sputtering current of the molybdenum disulfide target is kept at 1.6A, the sputtering current of Zn is kept at 0.6A, and MoS2 and Zn are deposited alternately. The target deposition time per cycle is 90s, and the total deposition time is 7000s. A MoS2 / Me superlattice layer with a thickness of about 2μm is deposited on the surface of the MoS2 / Zn gradient transition layer.

[0093] Prepared TiN x The specific composition parameters of the -MoS2 / Zn-2 superlattice composite coating sample are shown in Table 1.

[0094] After the above deposition process, TiN x -MoS2 / Zn-2 superlattice composite coating was tested as follows:

[0095] The coating thickness was measured using scanning electron microscopy.

[0096] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0097] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0098] Example 3

[0099] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. Unbalanced magnetron sputtering technology is used to prepare TiN on the substrate surface. x -MoS2 / Zn-3 superlattice composite coating, mainly including the following steps:

[0100] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0101] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, the substrate temperature is 50 ~ 150 ° C. x-MoS2 / Zn-3 superlattice composite coating, the cavity is filled with high-purity argon gas, Ti target (purity of 99.99at.%), MoS2 target (purity of 99.9at.%) and Zn target (purity of 99.9at.%) are arranged and controlled, using unbalanced magnetron sputtering technology. The specific steps are as follows:

[0102] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0103] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 150 nm was deposited on the substrate surface.

[0104] The titanium target sputtering current is 5.0A, the substrate bias voltage is -80V, the working gas is Ar and N2, among which the Ar gas flow rate is 30sccm, the N2 flow rate is 10sccm, the deposition substrate temperature is 120℃, the pressure is 1Pa, the deposition time is 3600s, and TiN is deposited on the surface of the titanium transition layer. x Bearing layer, thickness is about 220nm;

[0105] Gradually reduce the titanium target sputtering current to 0A, and gradually increase the molybdenum disulfide target sputtering current to 1.6A. The working gases are Ar and N2, where the Ar gas flow rate is 16sccm, the N2 flow rate is 10sccm, the substrate bias is -50V, the deposition substrate temperature is 80℃, the pressure is 1.0Pa, and the deposition time is 600s. x TiN is deposited on the surface of the bearing layer x / MoS2 gradient transition layer thickness is about 100nm;

[0106] The sputtering current of the MoS2 target was kept at 1.6A, while the sputtering current of the Zn target was gradually increased to 0.6A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 80℃, the pressure was 1.0Pa, the deposition time was 600s, and the TiN x A MoS2 / Zn gradient transition layer is deposited on the surface of the MoS2 / MoS2 gradient transition layer, with a thickness of about 200 nm;

[0107] The sputtering current of the molybdenum disulfide target is kept at 1.6A, the sputtering current of Zn is kept at 0.6A, and MoS2 and Zn are deposited alternately. The target deposition time per cycle is 90s, and the total deposition time is 7000s. A MoS2 / Me superlattice layer with a thickness of about 2μm is deposited on the surface of the MoS2 / Zn gradient transition layer.

[0108] Prepared TiN xThe specific composition parameters of the -MoS2 / Zn-3 superlattice composite coating sample are shown in Table 1.

[0109] After the above deposition process, TiN x -MoS2 / Zn-3 superlattice composite coating was tested as follows:

[0110] The coating thickness was measured using scanning electron microscopy.

[0111] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0112] Adhesion test, using an automatic scratch tester to test the coating adhesion, according to the automatic scratch tester operating procedures, three scratch tests were performed at different positions, the experimental conditions were loading speed: 5 ~ 10N / min, scratch length: 5mm, loading force: 20N. The test results show that the prepared TiN x -The bonding strength of MoS2 / Zn-3 superlattice composite coating can reach 18N.

[0113] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0114] The friction life test was conducted using a CSM friction tester in a vacuum environment to analyze the tribological properties. A 9Cr18 steel ball was used as the counterpart, with a rotational speed of 1000 rpm, an orbit radius of 8 mm, and a normal load of 5 N. The test results showed that the friction coefficient was less than 0.02 throughout the entire friction test, and the friction life could reach 4×10 6 Ten thousand turns.

[0115] The TiN prepared in this embodiment x -The cross-sectional SEM image of the MoS2 / Zn-3 coating is shown in Figure 1. x -MoS2 / Zn-3 coating hardness and elastic modulus test diagram is shown in Figure 2; the prepared TiN x -MoS2 / Zn-3 coating bonding morphology and force curve are shown in Figure 3; the prepared TiN x -The friction curve of MoS2 / Zn-3 coating in vacuum environment is shown in Figure 4; x -The friction life curve of MoS2 / Zn-3 coating in vacuum environment is shown in Figure 5.

[0116] Example 4

[0117] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. Unbalanced magnetron sputtering technology is used to prepare TiN on the substrate surface. x -MoS2 / Ti superlattice composite coating, mainly including the following steps:

[0118] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0119] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, the substrate temperature is 50 ~ 150 ° C. x -MoS2 / Ti superlattice composite coating, the cavity is filled with high-purity argon gas, and a Ti target (purity of 99.99at.%), a MoS2 target (purity of 99.9at.%), and a Ti target (purity of 99.9at.%) are arranged and controlled using unbalanced magnetron sputtering technology. The specific steps are as follows:

[0120] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0121] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 150 nm was deposited on the substrate surface.

[0122] The titanium target sputtering current is 5.0A, the substrate bias voltage is -80V, the working gas is Ar and N2, among which the Ar gas flow rate is 30sccm, the N2 flow rate is 10sccm, the deposition substrate temperature is 120℃, the pressure is 1Pa, the deposition time is 3600s, and TiN is deposited on the surface of the titanium transition layer. x Bearing layer, thickness is about 220nm;

[0123] Gradually reduce the titanium target sputtering current to 0A, and gradually increase the molybdenum disulfide target sputtering current to 1.6A. The working gases are Ar and N2, where the Ar gas flow rate is 16sccm, the N2 flow rate is 10sccm, the substrate bias is -50V, the deposition substrate temperature is 80℃, the pressure is 1.0Pa, and the deposition time is 600s. x TiN is deposited on the surface of the bearing layer x / MoS2 gradient transition layer thickness is about 100nm;

[0124] The sputtering current of the molybdenum disulfide target was kept at 1.6A, and the sputtering current of the Ti target was gradually increased to 1.2A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 80℃, the pressure was 1.0Pa, the deposition time was 600s, and the TiN x A MoS2 / Ti gradient transition layer is deposited on the surface of the MoS2 / MoS2 gradient transition layer, with a thickness of about 200 nm;

[0125] The sputtering current of the molybdenum disulfide target is kept at 1.6A, the sputtering current of Ti is kept at 1.2A, and MoS2 and Ti are deposited alternately. The target deposition time per cycle is 90s, and the total deposition time is 7000s. A MoS2 / Ti superlattice layer with a thickness of about 2μm is deposited on the surface of the MoS2 / Ti gradient transition layer.

[0126] Prepared TiN x The specific composition parameters of the -MoS2 / Ti superlattice composite coating sample are shown in Table 1.

[0127] After the above deposition process, TiN x -MoS2 / Ti superlattice composite coating was tested as follows:

[0128] The coating thickness was measured using scanning electron microscopy.

[0129] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the coating thickness. The average value of six points was taken. The test results are shown in Table 2.

[0130] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0131] Example 5

[0132] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. Unbalanced magnetron sputtering technology is used to prepare TiN on the substrate surface. x -MoS2 / Cr superlattice composite coating, mainly including the following steps:

[0133] After drying with nitrogen, the sample was placed in anhydrous ethanol solution and ultrasonically cleaned for 10 minutes, and then dried with nitrogen.

[0134] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, the substrate temperature is 50 ~ 150 ° C. x -MoS2 / Cr superlattice composite coating, the cavity is filled with high-purity argon gas, Ti target (purity of 99.99at.%), MoS2 target (purity of 99.9at.%) and Cr target (purity of 99.9at.%) are arranged and controlled, using unbalanced magnetron sputtering technology. The specific steps are as follows:

[0135] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0136] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 150 nm was deposited on the substrate surface.

[0137] The titanium target sputtering current is 5.0A, the substrate bias voltage is -80V, the working gas is Ar and N2, among which the Ar gas flow rate is 30sccm, the N2 flow rate is 10sccm, the deposition substrate temperature is 120℃, the pressure is 1Pa, the deposition time is 3600s, and TiN is deposited on the surface of the titanium transition layer. x Bearing layer, thickness is about 220nm;

[0138] Gradually reduce the titanium target sputtering current to 0A, and gradually increase the molybdenum disulfide target sputtering current to 1.6A. The working gases are Ar and N2, where the Ar gas flow rate is 16sccm, the N2 flow rate is 10sccm, the substrate bias is -50V, the deposition substrate temperature is 80℃, the pressure is 1.0Pa, and the deposition time is 600s. x TiN is deposited on the surface of the bearing layer x / MoS2 gradient transition layer thickness is about 100nm;

[0139] The sputtering current of the MoS2 target was kept at 1.6A, and the sputtering current of the Cr target was gradually increased to 1.0A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 80℃, the pressure was 1.0Pa, the deposition time was 600s, and the TiN x A MoS2 / Cr gradient transition layer is deposited on the surface of the MoS2 / MoS2 gradient transition layer, with a thickness of about 200 nm;

[0140] The sputtering current of the molybdenum disulfide target is kept at 1.6A, the sputtering current of Cr is kept at 0.6A, MoS2 and Cr are deposited alternately, the target deposition time per cycle is 90s, the total deposition time is 7000s, and a MoS2 / Cr superlattice layer with a thickness of about 2μm is deposited on the surface of the MoS2 / Cr gradient transition layer.

[0141] Prepared TiN x The specific composition parameters of the -MoS2 / Cr supercrystalline composite lattice coating sample are shown in Table 1.

[0142] After the above deposition process, TiN x -MoS2 / Cr superlattice composite coating was tested as follows:

[0143] The coating thickness was measured using scanning electron microscopy.

[0144] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0145] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0146] Comparative Example 1

[0147] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. The unbalanced magnetron sputtering technology is used to prepare the molybdenum disulfide coating on the substrate surface, which mainly includes the following steps:

[0148] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0149] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, with the substrate temperature at 50-150°C. MoS2 coating was deposited by filling the chamber with high-purity argon gas, using a Ti target (purity of 99.99 at.%) and a MoS2 target (purity of 99.9 at.%), using unbalanced magnetron sputtering technology. The specific steps are as follows:

[0150] For plasma etching, a bias voltage of -400 V was applied to the substrate, the program running time was 1200 s, and the substrate temperature was 120 °C.

[0151] The titanium target sputtering current was 5A, the substrate bias voltage was -100V, the working gas was Ar, the gas flow rate was 15sccm, the deposition substrate temperature was 120°C, the pressure was 0.8Pa, and the deposition time was 1000s. A titanium transition layer with a thickness of about 200nm was deposited on the substrate surface.

[0152] The titanium target sputtering current was gradually reduced to 0 A, while the molybdenum disulfide target sputtering current was gradually increased to 1.6 A. The working gas was Ar, the gas flow rate was 18 sccm, the substrate bias was -50 V, the deposition substrate temperature was 80 ° C, the pressure was 0.8 Pa, and the deposition time was 1000 s. A titanium / molybdenum disulfide gradient transition layer with a thickness of about 250 nm was deposited on the surface of the titanium transition layer.

[0153] The sputtering current of the molybdenum disulfide target was kept at 1.6 A, and the other conditions remained unchanged. The deposition time was 8000 s until the total thickness of the molybdenum disulfide coating reached 2.5 μm.

[0154] The specific composition parameters of the prepared MoS2 coating samples are shown in Table 1.

[0155] The MoS2 coating obtained after the above deposition process was tested as follows:

[0156] The coating thickness was measured using scanning electron microscopy.

[0157] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0158] Adhesion testing was performed using an automatic scratch tester. Three scratch tests were performed at different locations according to the machine's operating procedures. The experimental conditions were a loading rate of 5 to 10 N / min, a scratch length of 5 mm, and a loading force of 20 N. The test results are shown in Table 2.

[0159] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0160] Comparative Example 2

[0161] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. The MoS2-Zn-1 composite coating is prepared on the substrate surface using unbalanced magnetron sputtering technology, which mainly includes the following steps:

[0162] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0163] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, and then sputter clean the target for 1200s, with the substrate temperature at 50-150°C. MoS2-Zn composite coatings were deposited by filling the chamber with high-purity argon gas, using a Ti target (purity of 99.99 at.%), a MoS2 target (purity of 99.9 at.%), and a Zn target (purity of 99.9 at.%), using unbalanced magnetron sputtering technology. The specific steps are as follows:

[0164] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0165] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 300 nm was deposited on the substrate surface.

[0166] The titanium target sputtering current was gradually reduced to 0 A, while the molybdenum disulfide target sputtering current was gradually increased to 1.6 A and the Zn target sputtering current was increased to 0.6 A. The working gas was Ar, the gas flow rate was 16 sccm, the substrate bias was -50 V, the deposition substrate temperature was 80 ° C, the pressure was 1.0 Pa, and the deposition time was 1200 s. A Ti / MoS2 / Zn gradient transition layer with a thickness of about 300 nm was deposited on the surface of the titanium transition layer.

[0167] The sputtering current of the molybdenum disulfide target was kept at 1.6 A, the sputtering current of Zn was kept at 0.6 A, and MoS2 and Zn were co-deposited for a total deposition time of 7000 s until the thickness of the MoS2-Zn coating reached 2.5 μm.

[0168] The specific composition parameters of the prepared MoS2-Zn-1 coating sample are shown in Table 1.

[0169] The MoS2-Zn-1 coating obtained after the above deposition process was subjected to the following tests:

[0170] The coating thickness was measured using scanning electron microscopy.

[0171] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0172] Adhesion testing was performed using an automatic scratch tester. Three scratch tests were performed at different locations according to the machine's operating procedures. The experimental conditions were a loading speed of 5 to 10 N / min, a scratch length of 5 mm, and a loading force of 20 N. The test results are shown in Table 2.

[0173] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, and a reciprocating sliding method was employed. The test frequency was 5 Hz, the track length was 5 mm, the travel distance was 720 m, and the normal load was 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0174] Comparative Example 3

[0175] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. The MoS2-Zn-2 composite coating is prepared on the substrate surface using unbalanced magnetron sputtering technology, which mainly includes the following steps:

[0176] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0177] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, with the substrate temperature at 50-150°C. MoS2-Zn-2 composite coatings were deposited in a chamber filled with high-purity argon. Ti targets (99.99 at.%), MoS2 targets (99.9 at.%), and Zn targets (99.9 at.%) were used for the control setup. Unbalanced magnetron sputtering technology was used. The specific steps are as follows:

[0178] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0179] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 150 nm was deposited on the substrate surface.

[0180] Reduce the titanium target sputtering current to 0A, and gradually increase the molybdenum disulfide target sputtering current to 1.6A. The working gas is Ar, the Ar gas flow rate is 16sccm, the substrate bias is -50V, the deposition substrate temperature is 80℃, the pressure is 1.0Pa, the deposition time is 600s, and the MoS2 transition layer thickness is about 100nm.

[0181] The sputtering current of the molybdenum disulfide target was maintained at 1.6 A, while the sputtering current of the Zn target was gradually increased to 0.6 A. The working gas was Ar, the gas flow rate was 16 sccm, the substrate bias was -50 V, the deposition substrate temperature was 80 ° C, the pressure was 1.0 Pa, and the deposition time was 600 s. A MoS2 / Zn gradient transition layer with a thickness of about 200 nm was deposited on the surface of the MoS2 gradient transition layer.

[0182] The sputtering current of the molybdenum disulfide target is kept at 1.6A, the sputtering current of Zn is kept at 0.6A, MoS2 and Zn are deposited alternately, the target deposition time per cycle is 90s, the total deposition time is 7000s, and a MoS2 / Me superlattice layer with a thickness of about 2μm is deposited on the surface of the gradient transition layer.

[0183] The specific composition parameters of the prepared MoS2-Zn-2 composite coating sample are shown in Table 1.

[0184] The MoS2-Zn-2 composite coating obtained after the above deposition treatment was subjected to the following tests:

[0185] The coating thickness was measured using scanning electron microscopy.

[0186] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0187] Adhesion testing was performed using an automatic scratch tester. Three scratch tests were performed at different locations according to the machine's operating procedures. The experimental conditions were a loading speed of 5 to 10 N / min, a scratch length of 5 mm, and a loading force of 20 N. The test results are shown in Table 2.

[0188] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, and a reciprocating sliding method was employed. The frequency was 5 Hz, the track length was 5 mm, the travel distance was 720 m, and the normal load was 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0189] Comparative Example 4

[0190] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. The MoS2-Zn-3 composite coating is prepared on the substrate surface using unbalanced magnetron sputtering technology, which mainly includes the following steps:

[0191] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0192] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, with the substrate temperature at 50-150°C. MoS2-Zn-3 composite coatings were deposited in a chamber filled with high-purity argon. Ti targets (99.99 at.%), MoS2 targets (99.9 at.%), and Zn targets (99.9 at.%) were used in the control setup. Unbalanced magnetron sputtering technology was used. The specific steps are as follows:

[0193] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0194] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 150 nm was deposited on the substrate surface.

[0195] The titanium target sputtering current is 5.0A, the substrate bias voltage is -80V, the working gas is Ar and N2, among which the Ar gas flow rate is 30sccm, the N2 flow rate is 10sccm, the deposition substrate temperature is 120℃, the pressure is 1Pa, the deposition time is 3600s, and TiN is deposited on the surface of the titanium transition layer. x Bearing layer, thickness is about 220nm;

[0196] Reduce the titanium target sputtering current to 0A, and gradually increase the molybdenum disulfide target sputtering current to 1.6A. The working gases are Ar and N2, where the Ar gas flow rate is 16sccm, the N2 flow rate is 10sccm, the substrate bias is -50V, the deposition substrate temperature is 80℃, the pressure is 1.0Pa, and the deposition time is 600s. x The thickness of the MoS2 transition layer deposited on the surface of the bearing layer is about 100nm;

[0197] The sputtering current of the molybdenum disulfide target was maintained at 1.6A, while the sputtering current of the Zn target was gradually increased to 0.6A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 80°C, the pressure was 1.0Pa, and the deposition time was 600s. A MoS2 / Zn gradient transition layer with a thickness of about 200nm was deposited on the surface of the MoS2 transition layer.

[0198] The sputtering current of the molybdenum disulfide target is kept at 1.6A, the sputtering current of Zn is kept at 0.6A, MoS2 and Zn are deposited alternately, the target deposition time per cycle is 90s, the total deposition time is 7000s, and a MoS2 / Me superlattice layer with a thickness of about 2μm is deposited on the surface of the gradient transition layer.

[0199] The specific composition parameters of the prepared MoS2-Zn-3 composite coating sample are shown in Table 1.

[0200] The MoS2-Zn-3 composite coating obtained after the above deposition treatment was subjected to the following tests:

[0201] The coating thickness was measured using scanning electron microscopy.

[0202] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0203] Adhesion testing was performed using an automatic scratch tester. Three scratch tests were performed at different locations according to the machine's operating procedures. The experimental conditions were a loading speed of 5 to 10 N / min, a scratch length of 5 mm, and a loading force of 20 N. The test results are shown in Table 2.

[0204] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0205] Comparative Example 5

[0206] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. The MoS2-Zn-4 composite coating is prepared on the substrate surface using unbalanced magnetron sputtering technology, which mainly includes the following steps:

[0207] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0208] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, with the substrate temperature at 50-150°C. MoS2-Zn-4 composite coatings were deposited in a chamber filled with high-purity argon. Ti targets (99.99 at.%), MoS2 targets (99.9 at.%), and Zn targets (99.9 at.%) were used in the control setup. Unbalanced magnetron sputtering technology was used. The specific steps are as follows:

[0209] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0210] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 150 nm was deposited on the substrate surface.

[0211] The titanium target sputtering current is 5.0A, the substrate bias voltage is -80V, the working gas is Ar and N2, among which the Ar gas flow rate is 30sccm, the N2 flow rate is 10sccm, the deposition substrate temperature is 120℃, the pressure is 1Pa, the deposition time is 3600s, and TiN is deposited on the substrate surface. x Bearing layer, thickness is about 220nm;

[0212] Gradually reduce the titanium target sputtering current to 0A, and gradually increase the molybdenum disulfide target sputtering current to 1.6A. The working gases are Ar and N2, where the Ar gas flow rate is 16sccm, the N2 flow rate is 10sccm, the substrate bias is -50V, the deposition substrate temperature is 80℃, the pressure is 1.0Pa, and the deposition time is 600s. x TiN is deposited on the surface of the bearing layer x / MoS2 gradient transition layer thickness is about 100nm;

[0213] The sputtering current of the molybdenum disulfide target was maintained at 1.6A, while the Zn sputtering current was increased to 0.6A. MoS2 and Zn were deposited alternately. The target deposition time per cycle was 90s, and the total deposition time was 7000s. A MoS2 / Me superlattice layer with a thickness of about 2μm was deposited on the surface of the gradient transition layer.

[0214] The specific composition parameters of the prepared MoS2-Zn-4 composite coating sample are shown in Table 1.

[0215] The MoS2-Zn-4 composite coating obtained after the above deposition treatment was subjected to the following tests:

[0216] The coating thickness was measured using scanning electron microscopy.

[0217] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0218] Adhesion testing was performed using an automatic scratch tester. Three scratch tests were performed at different locations according to the machine's operating procedures. The experimental conditions were a loading speed of 5 to 10 N / min, a scratch length of 5 mm, and a loading force of 20 N. The test results are shown in Table 2.

[0219] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0220] Comparative Example 6

[0221] In this embodiment, the substrate material is 316L, TC4 or single crystal silicon wafer. The MoS2-Zn-5 composite coating is prepared on the substrate surface using unbalanced magnetron sputtering technology, which mainly includes the following steps:

[0222] The surface of the substrate was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 10 minutes, dried with nitrogen, and then placed in an anhydrous ethanol solution for ultrasonic cleaning for 10 minutes, and dried with nitrogen.

[0223] The cleaned substrate was placed in an unbalanced magnetron sputtering chamber and evacuated to a vacuum degree of less than 1×10 -3 Pa, then sputter clean the target for 1200s, with the substrate temperature at 50-150°C. MoS2-Zn-5 composite coatings were deposited in a chamber filled with high-purity argon. Ti targets (99.99 at.%), MoS2 targets (99.9 at.%), and Zn targets (99.9 at.%) were used in the control setup. Unbalanced magnetron sputtering technology was used. The specific steps are as follows:

[0224] For plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 1800 s, and the substrate temperature was 150 °C.

[0225] The titanium target sputtering current was 5.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 30 sccm, the deposition substrate temperature was 120°C, the pressure was 1 Pa, and the deposition time was 900 s. A titanium transition layer with a thickness of about 150 nm was deposited on the substrate surface.

[0226] The titanium target sputtering current is 5.0A, the substrate bias voltage is -80V, the working gas is Ar and N2, among which the Ar gas flow rate is 30sccm, the N2 flow rate is 10sccm, the deposition substrate temperature is 120℃, the pressure is 1Pa, the deposition time is 3600s, and TiN is deposited on the substrate surface. x Bearing layer, thickness is about 220nm;

[0227] Gradually reduce the titanium target sputtering current to 0A, and gradually increase the molybdenum disulfide target sputtering current to 1.6A. The working gases are Ar and N2, where the Ar gas flow rate is 16sccm, the N2 flow rate is 10sccm, the substrate bias is -50V, the deposition substrate temperature is 80℃, the pressure is 1.0Pa, and the deposition time is 600s. x TiN is deposited on the surface of the bearing layer x / MoS2 gradient transition layer thickness is about 100nm;

[0228] The sputtering current of the MoS2 target was kept at 1.6A, while the sputtering current of the Zn target was gradually increased to 0.6A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 80℃, the pressure was 1.0Pa, the deposition time was 600s, and the TiN x A MoS2 / Zn gradient transition layer is deposited on the surface of the MoS2 / MoS2 gradient transition layer, with a thickness of about 200 nm;

[0229] The specific composition parameters of the prepared MoS2-Zn-5 composite coating sample are shown in Table 1.

[0230] The MoS2-Zn-5 composite coating obtained after the above deposition treatment was subjected to the following tests:

[0231] The coating thickness was measured using scanning electron microscopy.

[0232] The hardness and elastic modulus of the coating were measured using an MTS NanoIndenter G200 nanoindenter system. The diamond indenter was used and the indentation depth was 200 nm, which was 1 / 10 of the film thickness. The average value of six points was taken. The test results are shown in Table 2.

[0233] Adhesion testing was performed using an automatic scratch tester. Three scratch tests were performed at different locations according to the machine's operating procedures. The experimental conditions were a loading speed of 5 to 10 N / min, a scratch length of 5 mm, and a loading force of 20 N. The test results are shown in Table 2.

[0234] Friction and wear tests were conducted using a CSM tribometer under vacuum conditions. A 9Cr18 steel ball was used as the counterweight, with a reciprocating sliding motion at a frequency of 5 Hz, a track length of 5 mm, a travel distance of 720 m, and a normal load of 5 N. The friction coefficient and wear rate results are shown in Table 2.

[0235] The elemental composition contents of seven coatings in Comparative Examples 1-6 and Examples 1-5 prepared by different metal targets and deposition times are shown in Table 1 and named as follows: MoS2, MoS2-Zn-1, MoS2-Zn-2, MoS2-Zn-3, MoS2-Zn-4, MoS2-Zn-5, TiN x -MoS2 / Zn-1、TiN x -MoS2 / Zn-2、TiN x -MoS2 / Zn-3、TiN x -MoS2 / Ti、TiN x -MoS2 / Cr.

[0236] Table 1: Composition parameters of seven coating samples in Examples and Comparative Examples

[0237] It can be seen from Table 1 that the metal content of the deposited coating is 5.0-15%, and the main component is molybdenum disulfide, which meets the requirements of lubricating functional coating.

[0238] The nanoindentation equipment was used to press six points with a depth of 200 nm on the surface of the seven coating samples in the examples and comparative examples, and the hardness and elastic modulus were measured. The results are shown in Table 2 below. As can be seen from Table 2, the five examples of TiN x -The hardness of MoS2 / Me coating is not less than 7GPa.

[0239] Table 2: Hardness, elastic modulus, bonding strength, vacuum friction coefficient and wear rate (×10 -7 mm 3 / Nm) table

[0240] TiN in Example 3 x -MoS2 / Zn-3 has the best mechanical and tribological properties.

[0241] In summary, the TiN x -MoS2 / Me has good mechanical properties such as hardness (not less than 7GPa), a friction coefficient of 0.007 in a vacuum environment, and a friction life of more than four million revolutions, which can meet the requirements of lubrication stability and long service life of space mechanisms.

[0242] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments using other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0243] It should be understood that the technical solution of the present application is not limited to the above-mentioned specific implementation cases. Any technical variations made according to the technical solution of the present application without departing from the scope of protection of the purpose of the present application and the claims shall fall within the scope of protection of the present application.

Claims

1. A method for preparing a low-friction and long-life superlattice composite coating, characterized in that: include: The unbalanced magnetron sputtering technology is adopted, a titanium target is used as a cathode target material, an inert gas is used as a working gas, a sputtering current is applied to the titanium target, and a negative bias voltage is applied to the substrate, so as to deposit a titanium transition layer on the substrate surface, wherein the sputtering current is 3.0 to 5.0 A, the substrate bias voltage is -100 to -150 V, the working gas flow rate is 20 to 30 sccm, the substrate temperature is 50 to 150° C., the reaction chamber pressure is 0.1 to 2.0 Pa, and the deposition time is 300 to 900 s. Unbalanced magnetron sputtering technology is used, with titanium target as cathode target, inert gas and N2 as working gas, sputtering current is applied to the titanium target, and negative bias is applied to the substrate, so that TiN is deposited on the surface of the titanium transition layer. x The carrier layer, wherein the sputtering current is 3.0 to 5.0 A, the substrate bias voltage is -100 to -150 V, the flow rate of the inert gas is 20 to 30 sccm, the flow rate of N2 is 5 to 15 sccm, the substrate temperature is 50 to 150° C., the reaction chamber pressure is 0.1 to 2.0 Pa, and the deposition time is 2400 to 4800 s; The unbalanced magnetron sputtering technology is adopted, with titanium target and molybdenum disulfide target as cathode target, inert gas and N2 as working gas, sputtering current is applied to the titanium target and molybdenum disulfide target, and negative bias is applied to the substrate, so that the TiN x TiN is deposited on the surface of the supporting layer x / MoS2 gradient transition layer, wherein the sputtering current applied to the titanium target is gradually reduced from 3.0 to 5.0 A to 0, the sputtering current applied to the molybdenum disulfide target is gradually increased from 0 to 1.2 to 2.0 A, the substrate bias is -30 to -70 V, the flow rate of the inert gas is 10 to 20 sccm, the flow rate of N2 is 5 to 15 sccm, the substrate temperature is 50 to 150 ° C, the reaction chamber pressure is 0.1 to 2.0 Pa, and the deposition time is 300 to 900 s; The unbalanced magnetron sputtering technology is adopted, with metal Me target and molybdenum disulfide target as cathode target materials, inert gas as working gas, sputtering current is applied to the metal Me target and molybdenum disulfide target, and negative bias is applied to the substrate, so that the TiN x / MoS2 gradient transition layer is deposited on the surface to obtain MoS2 / Me gradient transition layer, wherein the sputtering current applied to the metal Me target is gradually increased from 0 to 0.6-1.4A, the sputtering current applied to the molybdenum disulfide target is 1.2-2.0A, the substrate bias is -30--70V, the flow rate of the inert gas is 10-20sccm, the substrate temperature is 50-150°C, the reaction chamber pressure is 0.1-2.0Pa, and the deposition time is 300-900s; And, using unbalanced magnetron sputtering technology, using a molybdenum disulfide target and a metal Me target as cathode target materials, using an inert gas as a working gas, applying a negative bias voltage to the substrate, applying a sputtering current to the molybdenum disulfide target and the metal Me target, alternately depositing MoS2 layers and Me layers, thereby depositing a MoS2 / Me superlattice layer on the surface of the MoS2 / Me gradient transition layer, thereby obtaining a superlattice composite coating, wherein the sputtering current applied to the molybdenum disulfide target is 1.2 to 2.0 A, the sputtering current applied to the metal Me target is 0.6 to 1.4 A, the substrate bias is -30 to -70 V, the working gas flow rate is 10 to 20 sccm, the substrate temperature is 50 to 150° C., the reaction chamber pressure is 0.1 to 2.0 Pa, and the deposition time is 6000 to 8000 s; the deposition time of each cycle of alternating deposition of MoS2 layers and Me layers is 10 to 90 s; The low-friction and long-life superlattice composite coating comprises: a titanium transition layer, a TiN x Carrier layer, TiN x / MoS2 gradient transition layer, MoS2 / Me gradient transition layer and MoS2 / Me superlattice layer; wherein x is 0.5 to 1, Me is selected from any one or a combination of two or more of Ti, Zr, V, Nb, Cr, Mo, and Cd; and, in a direction gradually away from the substrate, the TiN x The content of MoS2 in the MoS2 / MoS2 gradient transition layer is increasing, and the content of MoS2 in the MoS2 / Me gradient transition layer is decreasing; the MoS2 / Me superlattice layer comprises a plurality of alternating superimposed periodic layers, and each alternating superimposed periodic layer comprises a MoS2 layer and a Me layer; the MoS2 layer in the MoS2 / Me superlattice layer grows in a parallel orientation to the MoS2 (002) plane; the friction coefficient of the superlattice composite coating in a vacuum environment is less than 0.02, and the wear life is 4×10 6 Turn above.

2. The preparation method according to claim 1, characterized in that Also includes: The reaction chamber was evacuated to a vacuum degree of 3.0×10 -5 torr or less, and firstly subjecting the cleaned substrate to plasma etching.

3. The preparation method according to claim 1, characterized in that: The matrix is ​​selected from a spatial structure.

4. A low-friction and long-life superlattice composite coating prepared by the preparation method according to any one of claims 1 to 3.

5. The superlattice composite coating according to claim 4, characterized in that: The hardness of the superlattice composite coating is above 7 GPa.

6. The superlattice composite coating according to claim 4, characterized in that: The bonding force between the superlattice composite coating and the substrate is above 15N, and the material of the substrate is selected from 316L stainless steel, TC4 titanium alloy or single crystal silicon wafer.

7. The superlattice composite coating according to claim 4, characterized in that: The thickness of the titanium transition layer is 50-150 nm.

8. The superlattice composite coating according to claim 4, characterized in that: The TiN x The thickness of the bearing layer is 150-300 nm; the TiN x The thickness of the MoS2 / Me gradient transition layer is 50-150nm; the thickness of the MoS2 / Me gradient transition layer is 100-300nm; the thickness of the MoS2 / Me superlattice layer is 1.5-2.5μm; the thickness of the superlattice composite coating is 2.0-3.0μm.

9. The superlattice composite coating according to claim 4, characterized in that: The modulation ratio of MoS2 to Me in the MoS2 / Me superlattice layer is t MoS2 :t Me It is 5:1-2:

1.

10. The superlattice composite coating according to claim 4, characterized in that: The modulation period of the MoS2 / Me superlattice layer is Λ=4-20nm.

11. The superlattice composite coating according to claim 4, characterized in that: The metal atom content in the MoS2 / Me superlattice layer is 5 to 15 at%.

12. Use of the low-friction and long-life superlattice composite coating according to any one of claims 4 to 11 in the field of surface protection of space mechanisms.

Citation Information

Patent Citations

  • High-temperature wear-resistant self-lubricating coating for fingertip sealing and preparation method thereof

    CN115287592A

  • Superlattice composite coating with low friction and long service life as well as preparation method and application thereof

    CN116497457A

  • Multi-layer coating having excellent adhesion and sliding properties and production method thereof

    US20060234081A1

Cited By

  • Disulfide composite film and preparation method and application thereof

    CN120041785A