Phosphate composite positive electrode active material and preparation method therefor, positive electrode sheet, battery cell, battery and electric device
By exfoliating graphene oxide into graphene oxide and reacting it with metal salts to form a phosphate cathode active material precursor, combined with lithium and carbon source treatment, the problem of poor electronic conductivity of phosphate cathode active materials was solved, achieving low-cost and high-efficiency battery performance improvement.
Patent Information
- Application Number
- PCT/CN2023/138578
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2023-12-13
- Publication Date
- 2024-12-05
AI Technical Summary
Existing phosphate cathode active materials have poor electronic conductivity, while graphene coating is costly and has poor interfacial bonding, which affects the battery's capacity utilization and electrochemical performance.
Using graphite oxide as raw material, it is exfoliated into graphene oxide by high-speed shearing, and reacted with metal salt and precipitant to form a phosphate cathode active material precursor. Combined with lithium source, phosphorus source and carbon source, it is spray-dried, granulated and sintered to form a phosphate composite cathode active material coated with amorphous carbon.
It reduces raw material and energy costs, improves electronic and ionic conductivity, promotes efficient electron transport, and enhances battery capacity and electrochemical performance.
Smart Images

Figure CN2023138578_05122024_PF_FP_ABST
Abstract
Description
Phosphate composite positive electrode active material and preparation method thereof, positive electrode sheet, battery cell, battery and electrical device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310637376.2 filed on May 31, 2023, entitled “Phosphate composite positive electrode active material and preparation method thereof, positive electrode sheet, battery cell, battery and electrical device”, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to a phosphate composite positive electrode active material and a preparation method thereof, a positive electrode sheet, a battery cell, a battery and an electrical device. Background Art
[0004] In recent years, batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. The positive electrode active material is one of the key factors affecting the electrochemical performance of the battery. Phosphate positive electrode active materials have become one of the most popular positive electrode active materials due to their advantages such as abundant raw material sources. However, the electronic conductivity of phosphate positive electrode active materials is poor. At present, the electronic conductivity of phosphate positive electrode active materials is mainly improved by coating phosphate positive electrode active materials with graphene. However, the raw material cost of graphene is high, and the interfacial bonding force between graphene and phosphate positive electrode active material particles is poor, making it difficult to achieve complete coating, thereby affecting the capacity of the battery and the electrochemical performance of the battery. The above statements are only used to provide background technical information related to this application and do not necessarily constitute prior art.
[0005] Summary of the Invention
[0006] The present application provides a phosphate composite positive electrode active material and a preparation method thereof, a positive electrode plate, a battery cell, a battery and an electrical device, which can reduce the raw material cost, energy consumption cost and time cost of the phosphate composite positive electrode active material, and can also improve the capacity and electrochemical performance of the phosphate composite positive electrode active material.
[0007] In a first aspect, the present application provides a method for preparing a phosphate composite positive electrode active material, comprising the following steps: providing a first mixed solution comprising graphite oxide and a metal salt for preparing a phosphate positive electrode active material, wherein the solvent in the first mixed solution comprises water; subjecting the first mixed solution to a first exfoliation reaction at a first shear rate of 6000 r / min or higher, so that the graphite oxide is exfoliated into graphene oxide, thereby obtaining a second mixed solution; maintaining the first shear rate, adding a precipitant or an aqueous solution of the precipitant to the second mixed solution for a second precipitation reaction, thereby obtaining a third mixed solution, wherein the precipitant comprises one or more of oxalic acid and a water-soluble oxalate. ; The third mixed liquid is washed and dried to obtain a mixture of a phosphate positive electrode active material precursor and graphene oxide; the phosphate positive electrode active material precursor and graphene oxide mixture are ground with a lithium source, a phosphorus source, a carbon source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source in the presence of a first solvent to obtain a slurry, which is then spray-dried, granulated, and sintered to obtain a phosphate composite positive electrode active material, wherein the phosphate composite positive electrode active material includes a phosphate positive electrode active material, amorphous carbon coating the phosphate positive electrode active material, and reduced graphene oxide coating the amorphous carbon.
[0008] The method for preparing the phosphate composite cathode active material provided herein uses low-cost graphite oxide as a raw material, thereby reducing raw material costs, energy consumption, and time costs during production. The method for preparing the phosphate composite cathode active material provided herein also has the advantages of simple process and high production efficiency, making it easy to industrialize and mass-produce.
[0009] The preparation method of the phosphate composite positive electrode active material provided in this application can obtain a phosphate composite positive electrode active material with a single crystal phase, high purity, small particle size, narrow particle size distribution, uniform element distribution, and high batch consistency. In addition, the obtained phosphate composite positive electrode active material can form a continuous conductive network. Therefore, the phosphate composite positive electrode active material obtained by the preparation method provided in this application has high electronic conductivity and high ionic conductivity, which is conducive to promoting the efficient transmission of electrons and shortening the transmission path of ions, thereby helping to improve the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0010] In any embodiment, the first stripping reaction is performed in a high-speed dispersing homogenizer.
[0011] In any embodiment, the first shearing speed is 6000-15000 r / min, and can be optionally 6000-10000 r / min.
[0012] In any embodiment, the time of the first stripping reaction is 30-150 minutes, and optionally 60-120 minutes.
[0013] In any embodiment, the number of layers of the graphene oxide is 1-6, and can be optionally 3-5.
[0014] Adjusting the first shear rate and the duration of the first exfoliation reaction can adjust the number of graphene oxide layers. The higher the first shear rate and the longer the first exfoliation reaction, the fewer graphene oxide layers are obtained by exfoliating the graphite oxide. Therefore, the preparation methods provided in the embodiments of the present application can also regulate the number of graphene oxide layers.
[0015] In any embodiment, the mass ratio of the graphite oxide to the metal salt used to prepare the phosphate positive electrode active material is 0.03:1-0.08:1.
[0016] In any embodiment, the concentration of the metal salt for preparing the phosphate positive electrode active material in the first mixed solution is 0.5-2 mol / L.
[0017] In any embodiment, the metal salt used to prepare the phosphate positive active material includes a water-soluble divalent metal salt. Optionally, the water-soluble divalent metal salt includes one or more of sulfate, nitrate, hydrochloride and acetate.
[0018] In any embodiment, the divalent metal element includes Mn element and / or Fe element and optionally M element, and the M element represents the doping element of the Mn position and / or Fe position of the phosphate composite positive electrode active material, optionally including one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr.
[0019] In any embodiment, the second precipitation reaction time is 10-60 minutes.
[0020] In any embodiment, the molar ratio of the precipitant to the metal salt used to prepare the phosphate positive electrode active material is 1:1-3:1. By adjusting the amount of the precipitant, it is helpful to improve the conversion efficiency of the metal ions and reduce the difference in precipitation rates of different metal ions in the reaction system, thereby facilitating the uniform co-precipitation of the metal ions, and further facilitating the ratio of each metal element in the prepared phosphate composite positive electrode active material to the ratio of each metal element in the raw material to have a high consistency. By adjusting the amount of the precipitant, it is also helpful to make the co-precipitation reaction more complete, thereby reducing the metal ion content in the reaction waste liquid, reducing the difficulty of the waste liquid treatment process and reducing environmental pollution; in addition, it is also helpful to improve the purity of the obtained phosphate positive electrode active material precursor and reduce the impurity content.
[0021] In any embodiment, the precipitant includes one or more of oxalic acid, sodium oxalate, potassium oxalate, and ammonium oxalate.
[0022] In any embodiment, the concentration of the aqueous solution of the precipitant is 0.5-2 mol / L.
[0023] In any embodiment, the step of providing a first mixed solution containing graphite oxide and a metal salt for preparing a phosphate positive electrode active material includes the following steps: under a protective gas atmosphere, adding graphite oxide to water, and then adding the metal salt for preparing a phosphate positive electrode active material, and dispersing them evenly to obtain the first mixed solution.
[0024] In any embodiment, the shielding gas includes nitrogen, an inert gas, or a combination thereof.
[0025] In any embodiment, the first solvent includes one or more of an alcohol solvent and water, and may optionally include one or more of ethanol and water.
[0026] In any embodiment, the grinding process comprises a high-energy ball milling process or a sand milling process.
[0027] In any embodiment, the grinding process is performed at a rotation speed of 1000-2500 r / min.
[0028] In any embodiment, the grinding treatment time is 1-5 hours.
[0029] In any embodiment, the sintering process includes a pre-sintering process and a high-temperature sintering process;
[0030] In any embodiment, the temperature of the pre-sintering process is 350-550°C, and optionally 400-500°C.
[0031] In any embodiment, the pre-sintering treatment time is 2-12 hours, and optionally 3-10 hours.
[0032] In any embodiment, the temperature of the high-temperature sintering treatment is 600-800°C, and optionally 650-750°C.
[0033] In any embodiment, the high-temperature sintering treatment time is 5-24 hours, and can be optionally 8-12 hours.
[0034] In any embodiment, the pre-sintering process is performed under a protective gas atmosphere.
[0035] In any embodiment, the high-temperature sintering process is performed under a protective gas atmosphere.
[0036] In any embodiment, the phosphate positive electrode active material precursor and graphene oxide mixture are ground with a lithium source, a phosphorus source, a carbon source, an optional Li-site doping element source, an optional P-site doping element source, and an optional O-site doping element source in the presence of a first solvent to obtain a slurry, and then spray-dried, granulated, and sintered to obtain a phosphate composite positive electrode active material. The steps include: grinding the phosphate positive electrode active material precursor and graphene oxide mixture with a lithium source, a phosphorus source, an optional Li-site doping element source, an optional P-site doping element source, and an optional O-site doping element source in the presence of a first solvent for a first time to obtain a first slurry; spray-drying and granulating the first slurry to obtain a powder, and then pre-sintering to obtain a pre-sintered powder; grinding the pre-sintered powder with the carbon source in the presence of a first solvent for a second time to obtain a second slurry; spray-drying and granulating the second slurry to obtain a powder, and then high-temperature sintering and optionally crushing to obtain the phosphate composite positive electrode active material.
[0037] This allows the obtained phosphate composite positive electrode active material to form a continuous conductive network, which is beneficial to improving the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0038] In any embodiment, the rotation speed of the first grinding process is 1500-2500 r / min.
[0039] In any embodiment, the first grinding process is performed for 1-5 hours.
[0040] In any embodiment, the rotation speed of the second grinding process is 1000-2500 r / min.
[0041] In any embodiment, the second grinding process is performed for 1-3 hours.
[0042] In any embodiment, the Li-site doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W.
[0043] In any embodiment, the P-site doping element includes one or more elements selected from the group consisting of B, S, Si, and N.
[0044] In any embodiment, the O-site doping element includes one or more elements selected from the group consisting of S, F, Cl, and Br.
[0045] In any embodiment, the lithium source includes one or more of lithium hydroxide, lithium carbonate, lithium dihydrogen phosphate, lithium hydrogen phosphate, lithium nitrate, and lithium acetate.
[0046] In any embodiment, the phosphorus source includes one or more of phosphoric acid, ammonium monohydrogen phosphate, and ammonium dihydrogen phosphate.
[0047] In any embodiment, the carbon source comprises one or more of sucrose, glucose, polyvinyl alcohol, polyethylene glycol, phenolic resin, citric acid and cyclodextrin.
[0048] In any embodiment, the Li-site doping element source includes one or more of sulfate, nitrate, hydrochloride and acetate of the Li-site doping element.
[0049] In any embodiment, the P-site doping element source includes one or more of sulfates, borates, nitrates, and silicates of the P-site doping element.
[0050] In any embodiment, the O-site doping element source includes one or more of a simple substance and an ammonium salt of the O-site doping element.
[0051] The second aspect of the present application provides a phosphate composite positive electrode active material prepared by the method of the first aspect of the present application, wherein the phosphate composite positive electrode active material includes a phosphate positive electrode active material, amorphous carbon coating the phosphate positive electrode active material, and reduced graphene oxide coating the amorphous carbon.
[0052] The phosphate composite positive electrode active material provided in the present application has the characteristics of single crystal phase, high purity, regular morphology, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency. In addition, the phosphate composite positive electrode active material also has a continuous conductive network and a shortened ion transmission path, which is conducive to promoting the efficient transmission of electrons and ions, and thus is conducive to improving the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0053] In any embodiment, the volume distribution particle size Dv50 of the phosphate composite positive electrode active material satisfies 0.5 μm≤Dv50≤3 μm.
[0054] In any embodiment, the volume distribution particle sizes Dv90 and Dv50 of the phosphate composite positive active material satisfy 1<Dv90 / Dv50≤1.5.
[0055] In any embodiment, the powder resistivity of the phosphate composite positive electrode active material is 1-100 Ω·cm.
[0056] In any embodiment, the molecular formula of the phosphate positive electrode active material is Li a N b Fe x Mn y M 1-x-y P 1-m Q mO 4- n R n , M represents a doping element for the Mn position and / or Fe position, optionally including one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr; N represents a doping element for the Li position, optionally including one or more elements of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents a doping element for the P position, optionally including one or more elements of B, S, Si and N; R represents an O-position doping element, optionally including one or more elements of S, F, Cl and Br; 0.9≤a≤1.1; 0≤b≤0.1; 0≤x≤1; 0≤y≤1; 0≤1-xy<1; 0≤m≤0.1; 0≤n≤0.1.
[0057] In any embodiment, 0.001≤x≤0.999, 0.001≤y≤0.999, and 0≤1-xy≤0.10.
[0058] In any embodiment, 0.199≤x≤0.500, 0.499≤y≤0.800, and 0<1-xy≤0.10.
[0059] The third aspect of the present application provides a positive electrode plate, including a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, the positive electrode film layer including a phosphate composite positive electrode active material prepared by the method of the first aspect of the present application or the phosphate composite positive electrode active material of the second aspect of the present application.
[0060] A fourth aspect of the present application provides a battery cell, comprising the positive electrode sheet according to the third aspect of the present application.
[0061] A fifth aspect of the present application provides a battery, comprising the battery cell of the fourth aspect of the present application.
[0062] A sixth aspect of the present application provides an electrical device comprising the battery of the fifth aspect of the present application.
[0063] The electric device of the present application includes the battery provided by the present application, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.
[0065] FIG1 is a schematic structural diagram of a battery cell provided in some embodiments of the present application.
[0066] FIG2 is an exploded schematic diagram of a battery cell provided in some embodiments of the present application.
[0067] FIG3 is a schematic structural diagram of a battery module provided in some embodiments of the present application.
[0068] FIG4 is a schematic structural diagram of a battery pack provided in some embodiments of the present application.
[0069] FIG5 is an exploded schematic diagram of the battery pack shown in FIG4 .
[0070] FIG6 is a schematic diagram of an electrical device provided in some embodiments of the present application.
[0071] Figure 7(a) shows the Mn prepared in Example 1 0.6 Fe 0.4 Scanning electron microscope (SEM) image of the mixture of C2O4·2H2O and graphene oxide, FIG7(b) shows the Mn prepared in Comparative Example 1. 0.6 Fe 0.4 Scanning electron microscope (SEM) image of C2O4·2H2O.
[0072] FIG8( a ) shows a scanning electron microscope (SEM) image of the phosphate composite positive electrode active material prepared in Example 1, and FIG8( b ) shows a scanning electron microscope (SEM) image of the phosphate composite positive electrode active material prepared in Comparative Example 1.
[0073] FIG9 is a capacity-voltage curve of button cells prepared from the phosphate composite positive electrode active materials of Example 1 and Comparative Example 1.
[0074] FIG10 is a rate curve of button cells prepared from the phosphate composite positive active materials of Example 1 and Comparative Example 1.
[0075] In the accompanying drawings, which are not necessarily drawn to scale, the reference numerals are as follows: 1. battery pack; 2. upper housing; 3. lower housing; 4. battery module; 5. battery cell; 51. housing; 52. electrode assembly; 53. cover plate. DETAILED DESCRIPTION
[0076] Hereinafter, the embodiments of the phosphate composite positive electrode active material and its preparation method, positive electrode sheet, battery cell, battery and electrical device of the present application will be specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0077] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0078] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.
[0079] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.
[0080] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0081] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0082] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0083] Unless otherwise specified, in this application, the terms "first", "second", "third", etc. are used to distinguish different objects rather than to describe a specific order or a primary-secondary relationship.
[0084] In this application, the terms "plurality" and "multiple" refer to two or more.
[0085] Unless otherwise specified, the terms used in this application have the common meanings that are commonly understood by those skilled in the art.
[0086] Unless otherwise stated, the numerical values of the various parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application. Unless otherwise stated, the test temperature of each parameter is 25°C.
[0087] Poor electronic conductivity is a major factor limiting the large-scale application of phosphate cathode active materials. Currently, the main method is to directly mix phosphate cathode active materials with commercially available graphene, and then prepare coated phosphate composite cathode active materials through complex hydrothermal or high-temperature solid-phase methods to improve the electronic conductivity of the core of the phosphate cathode active material. However, the high price of commercially available graphene leads to high raw material costs for phosphate composite cathode active materials, which is not conducive to their widespread application. At the same time, the interfacial bonding strength between graphene and the core of the phosphate cathode active material is also poor, making it difficult to achieve complete coating and form a continuous conductive network. As a result, the electronic conductivity of the phosphate composite cathode active material cannot achieve the expected effect, which in turn affects the battery's capacity and electrochemical performance.
[0088] In addition, graphene-coated phosphate composite positive electrode active materials are mainly prepared by high-temperature solid-phase methods, such as physical grinding and mixing of lithium source, manganese source, iron source, doping element source and graphene by high-energy ball milling. Due to the particle size of each raw material, it is difficult to mix manganese and iron elements at the atomic level, and the doping elements are not easy to enter the interior of the phosphate crystals, which affects the electrochemical performance of the prepared phosphate composite positive electrode active material. At the same time, the content of each metal element in the prepared phosphate composite positive electrode active material is also greatly deviated from the metal ratio in the raw materials, resulting in poor batch consistency of the product.
[0089] In view of this, the inventors improved the preparation process of phosphate composite positive electrode active materials.
[0090] The present application provides a method for preparing a phosphate composite positive electrode active material, comprising the following steps: providing a first mixed solution comprising graphite oxide and a metal salt for preparing a phosphate positive electrode active material, wherein the solvent in the first mixed solution comprises water; subjecting the first mixed solution to a first exfoliation reaction at a first shear rate of 6000 r / min or higher, so as to exfoliate the graphite oxide into graphene oxide, thereby obtaining a second mixed solution; maintaining the first shear rate, adding a precipitant or an aqueous solution of the precipitant to the second mixed solution, thereby performing a second precipitation reaction, thereby obtaining a third mixed solution, wherein the precipitant comprises one or more of oxalic acid and a water-soluble oxalate; The third mixed liquid is washed and dried to obtain a mixture of a phosphate positive electrode active material precursor and graphene oxide; the mixture of the phosphate positive electrode active material precursor and the graphene oxide is ground with a lithium source, a phosphorus source, a carbon source, an optional Li-site doping element source, an optional P-site doping element source, and an optional O-site doping element source in the presence of a first solvent to obtain a slurry, which is then spray-dried, granulated, and sintered to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material, amorphous carbon coated with the phosphate positive electrode active material, and reduced graphene oxide coated with the amorphous carbon.
[0091] The first peeling reaction is carried out in a high-speed dispersing homogenizer.
[0092] The high-speed disperser homogenizer has a unique stator and rotor structure, which can generate super strong shear force and can also circulate materials to complete online dispersing, emulsifying, homogenizing and mixing processes.
[0093] When preparing phosphate composite positive electrode active materials, the high-speed rotation of a high-speed dispersing homogenizer can be used to draw the first mixed liquid into its working chamber. Its strong centrifugal force is then used to radially throw the material into the narrow and precise gap between the rotor and stator. At this time, the material is fully dispersed and crushed under the effects of strong liquid phase shear, liquid layer friction, and tearing collision. It is then ejected at high speed through the stator slots and then changes its flow direction under the resistance of the material itself and the container wall. At the same time, under the action of the upper and lower axial suction forces generated in the rotor area, two strong turbulent flows are formed. In this way, after multiple cycles, graphite oxide (usually in block form) can be exfoliated into graphene oxide, and the metal ions in the first mixed liquid can also be tightly adsorbed on the graphene oxide. Conventional agitators, on the other hand, can only play a simple dispersing role even at high stirring speeds and cannot exfoliate graphite oxide into graphene oxide.
[0094] The surface of the graphene oxide peeled off from graphite oxide has oxygen-containing functional groups (such as hydroxyl, carboxyl, etc.), which can produce electrostatic adsorption with metal ions with positive charge, so that metal salts can be closely adsorbed on the graphene oxide surface. After adding the precipitant, the nucleus can grow and attach in situ on the graphene oxide surface, and under the strong dispersion and crushing effect of the high-speed dispersion homogenizer, the phosphate positive active material precursor wrapped by graphene oxide can also be formed. In addition, under the high-speed shearing effect of the high-speed dispersion homogenizer, the initial concentration of the reaction system can be instantly increased after adding the precipitant, and the metal salt and the precipitant are directly subjected to coprecipitation reaction, which is conducive to faster nucleation rather than particle growth, and then is conducive to preparing a phosphate positive active material precursor with a small particle size; In addition, it is also conducive to each metal element to be uniformly coprecipitated, and then the phosphate positive active material precursor obtained can also be made to have a regular morphology, a narrow particle size distribution, a uniform element distribution and a high batch consistency.
[0095] When the obtained phosphate positive electrode active material precursor and graphene oxide mixture is further ground with a lithium source, a phosphorus source, a carbon source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source in the presence of a first solvent, the carbon source can be filled between the phosphate positive electrode active material particles, forming an in-situ grown amorphous carbon coating layer on the surface of the phosphate positive electrode active material. The amorphous carbon coating layer can enhance the interfacial interaction between the graphene coating layer and the phosphate positive electrode active material, and can also form a continuous conductive network with the outer graphene coating layer. The continuous conductive network can interconnect the phosphate positive electrode active material particles in the positive electrode film layer and can reduce the aggregation of the phosphate positive electrode active material particles, so that the prepared phosphate composite positive electrode active material has high electronic conductivity, which is beneficial to the efficient transmission of electrons and is also beneficial to improving the cycle performance and rate performance of the battery.
[0096] The phosphate positive electrode active material precursor obtained by the preparation method provided in the embodiment of the present application has the advantages of regular morphology, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency. When it is used as a raw material to continue to prepare a phosphate composite positive electrode active material, the grinding time (such as high-energy ball milling or sand milling) can be reduced, thereby reducing the energy consumption cost and time cost in production; it is also easy to achieve uniform mixing of multiple elements (such as Mn element, Fe element, doping element, etc.), and the ratio of each metal element in the prepared phosphate composite positive electrode active material is highly consistent with the ratio of each metal element in the raw material, thereby also making the prepared phosphate composite positive electrode active material have high batch consistency and good electrochemical performance.
[0097] Therefore, the method for preparing the phosphate composite positive active material provided in the embodiments of the present application uses low-cost graphite oxide as a raw material, thereby reducing the raw material cost during production, and also reducing energy consumption and time costs. The method for preparing the phosphate composite positive active material provided in the embodiments of the present application also has the advantages of simple process and high production efficiency, and is therefore easy to industrialize and mass-produce.
[0098] The preparation method of the phosphate composite positive electrode active material provided in the embodiments of the present application can obtain a phosphate composite positive electrode active material with a single crystal phase, high purity, small particle size, narrow particle size distribution, uniform element distribution, and high batch consistency. In addition, the obtained phosphate composite positive electrode active material can form a continuous conductive network. Therefore, the phosphate composite positive electrode active material obtained by the preparation method provided in the embodiments of the present application has high electronic conductivity and high ionic conductivity, which is conducive to promoting the efficient transmission of electrons and shortening the transmission path of ions, thereby helping to improve the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0099] The first shearing speed can be 6000 r / min, 7000 r / min, 8000 r / min, 9000 r / min, 10000 r / min, 11000 r / min, 12000 r / min, 13000 r / min, 14000 r / min, 15000 r / min, or any range thereof. Alternatively, in some embodiments, the first shearing speed is 6000-15000 r / min, optionally 6000-10000 r / min.
[0100] In some embodiments, the first stripping reaction time may be 30-150 minutes, and optionally 60-120 minutes.
[0101] In some embodiments, the number of graphene oxide layers may be 1-6, optionally 3-5.
[0102] Adjusting the first shear rate and the duration of the first exfoliation reaction can adjust the number of graphene oxide layers. The higher the first shear rate and the longer the first exfoliation reaction, the fewer graphene oxide layers are obtained by exfoliating the graphite oxide. Therefore, the preparation methods provided in the embodiments of the present application can also regulate the number of graphene oxide layers.
[0103] In some embodiments, the mass ratio of graphite oxide to the metal salt used to prepare the phosphate positive active material may be 0.03:1-0.08:1.
[0104] In some embodiments, the concentration of the metal salt used to prepare the phosphate positive electrode active material in the first mixed solution may be 0.5-2 mol / L. The concentration of the metal salt refers to the total concentration of all metal salts used to prepare the phosphate positive electrode active material in the first mixed solution. For example, if the metal salt includes ferrous sulfate and manganese sulfate, the concentration of the metal salt refers to the total concentration of ferrous sulfate and manganese sulfate.
[0105] In some embodiments, the metal salt used to prepare the phosphate positive active material includes a water-soluble divalent metal salt. Alternatively, the water-soluble divalent metal salt may include one or more of a sulfate, a nitrate, a hydrochloride, and an acetate of a divalent metal.
[0106] In some embodiments, the divalent metal element may include an Mn element and / or an Fe element and an optional M element, where the M element represents a doping element at the Mn position and / or Fe position of the phosphate composite positive electrode active material, and optionally includes one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr.
[0107] The phosphate cathode active material precursor refers to the product of a precipitation reaction between a metal salt used to prepare the phosphate cathode active material and a precipitant. In some embodiments, the phosphate cathode active material precursor may include manganese iron oxalate, etc.
[0108] In some embodiments, the step of providing a first mixed solution containing graphite oxide and a metal salt for preparing a phosphate positive electrode active material includes the following steps: under a protective gas atmosphere, adding graphite oxide to water, and then adding the metal salt for preparing a phosphate positive electrode active material, and dispersing them evenly to obtain a first mixed solution.
[0109] In some embodiments, the shielding gas may include nitrogen, an inert gas, or a combination thereof.
[0110] In some embodiments, the second precipitation reaction time can be 10-60 minutes.
[0111] In some embodiments, the molar ratio of the precipitant to the metal salt used to prepare the phosphate positive electrode active material can be 1:1-3:1. By adjusting the amount of the precipitant, it is helpful to improve the conversion efficiency of the metal ions and reduce the difference in precipitation rates of different metal ions in the reaction system, thereby facilitating the uniform co-precipitation of the metal ions, and thus facilitating the ratio of each metal element in the prepared phosphate composite positive electrode active material to the ratio of each metal element in the raw material to have a high degree of consistency. By adjusting the amount of the precipitant, it is also helpful to make the co-precipitation reaction more complete, thereby reducing the metal ion content in the reaction waste liquid, reducing the difficulty of the waste liquid treatment process and reducing environmental pollution; in addition, it is also helpful to improve the purity of the obtained phosphate positive electrode active material precursor and reduce the content of impurities.
[0112] In some embodiments, the precipitant may include one or more of oxalic acid, sodium oxalate, potassium oxalate, and ammonium oxalate.
[0113] The precipitant can be added to the second mixed solution in the form of an aqueous solution of the precipitant. In some embodiments, the concentration of the aqueous solution of the precipitant can be 0.5-2 mol / L.
[0114] In some embodiments, when washing the third mixed liquid, the washing liquid may include ethanol, water, or a mixture of the two, and the number of washing times may be one or more, which is not limited in the embodiments of the present application.
[0115] The washed material can be dried using a known drying process. In some embodiments, a vacuum drying process can be used. Optionally, the drying temperature can be below 100°C.
[0116] The grinding process can adopt a suitable grinding method known in the art. In some embodiments, the grinding process can include high-energy ball milling or sand milling, which is not limited in the present embodiment.
[0117] In some embodiments, the grinding process may be performed at a rotation speed of 1000-2500 rpm.
[0118] In some embodiments, the grinding process may last for 1-5 hours.
[0119] In some embodiments, the sintering process may include a pre-sintering process and a high-temperature sintering process.
[0120] In some embodiments, the temperature of the pre-sintering process may be 350°C-550°C, optionally 400°C-500°C.
[0121] In some embodiments, the pre-sintering treatment time may be 2-12 hours, optionally 3-10 hours.
[0122] In some embodiments, the pre-sintering process may be performed under a protective gas atmosphere.
[0123] In some embodiments, the temperature of the high-temperature sintering process may be 600°C-800°C, optionally 650°C-750°C.
[0124] In some embodiments, the high temperature sintering treatment time may be 5-24 hours, optionally 8-12 hours.
[0125] In some embodiments, the high temperature sintering process may be performed under a protective gas atmosphere.
[0126] In some embodiments, the pre-sintering process and the high temperature sintering process may be performed in a tube furnace.
[0127] In some embodiments, the shielding gas may include nitrogen, an inert gas, or a combination thereof.
[0128] In some embodiments, the step of grinding a mixture of a phosphate positive electrode active material precursor and graphene oxide with a lithium source, a phosphorus source, a carbon source, an optional Li-site doping element source, an optional P-site doping element source, and an optional O-site doping element source in the presence of a first solvent to obtain a slurry, and then spray drying, granulating, and sintering to obtain a phosphate composite positive electrode active material comprises the following steps: grinding the mixture of a phosphate positive electrode active material precursor and graphene oxide with a lithium source, a phosphorus source, an optional Li-site doping element source, an optional P-site doping element source, and an optional O-site doping element source in the presence of a first solvent for a first time to obtain a first slurry; spray drying and granulating the first slurry to obtain a powder, and then pre-sintering to obtain a pre-sintered powder; grinding the pre-sintered powder with a carbon source in the presence of the first solvent for a second time to obtain a second slurry; spray drying and granulating the second slurry to obtain a powder, and then high-temperature sintering and optionally crushing to obtain the phosphate composite positive electrode active material. Optionally, the crushing can be air flow crushing.
[0129] This allows the obtained phosphate composite positive electrode active material to form a continuous conductive network, which is beneficial to improving the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0130] In some embodiments, the rotation speed of the first grinding process can be 1500-2500 r / min.
[0131] In some embodiments, the first grinding process may last for 1-5 hours.
[0132] In some embodiments, the rotation speed of the second grinding process can be 1000-2500 r / min.
[0133] In some embodiments, the second grinding process may last for 1-3 hours.
[0134] In some embodiments, the first solvent may include one or more of an alcohol solvent and water, and may optionally include one or more of ethanol and water.
[0135] In some embodiments, the lithium source can be a lithium-containing compound known in the art that can be used to prepare phosphate positive active materials. For example, the lithium source can include one or more of lithium hydroxide, lithium carbonate, lithium dihydrogen phosphate, lithium hydrogen phosphate, lithium nitrate and lithium acetate.
[0136] In some embodiments, the phosphorus source may be a phosphorus-containing compound known in the art for preparing phosphate positive active materials. For example, the phosphorus source may include one or more of phosphoric acid, ammonium monohydrogen phosphate, and ammonium dihydrogen phosphate.
[0137] In some embodiments, the carbon source may include one or more of an organic carbon source and an inorganic carbon source. For example, the carbon source may include one or more of sucrose, glucose, polyvinyl alcohol, polyethylene glycol, phenolic resin, citric acid, and cyclodextrin.
[0138] In some embodiments, the Li-site doping element may include one or more elements of Zn, Al, Na, K, Mg, Nb, Mo, and W.
[0139] In some embodiments, the Li-site doping element source may include one or more of sulfate, nitrate, hydrochloride, and acetate of the Li-site doping element.
[0140] In some embodiments, the P-site doping element may include one or more elements of B, S, Si, and N.
[0141] In some embodiments, the P-site doping element source may include one or more of sulfates, borates, nitrates, and silicates of the P-site doping element.
[0142] In some embodiments, the O-site doping element may include one or more elements of S, F, Cl, and Br.
[0143] In some embodiments, the O-site doping element source may include one or more of a simple substance and an ammonium salt of the O-site doping element.
[0144] In the preparation method of the phosphate composite cathode active material provided herein, the amount of each raw material added can conform to the stoichiometric ratio of the target phosphate composite cathode active material. In some embodiments, the amount of the lithium source added can be slightly excessive, for example, 100%-110% of the theoretical mass of the lithium source, where the theoretical mass of the lithium source refers to the mass of the lithium source calculated based on the stoichiometric ratio of the phosphate composite cathode active material.
[0145] In the preparation method of the phosphate composite positive electrode active material provided in this application, unless otherwise specified, all raw materials and instruments used can be directly purchased. Each raw material may contain or not contain crystalline water.
[0146] The present invention also provides a phosphate composite cathode active material obtained by the above-mentioned preparation method. The phosphate composite cathode active material includes a phosphate cathode active material, amorphous carbon coating the phosphate cathode active material, and reduced graphene oxide coating the amorphous carbon.
[0147] The phosphate composite positive electrode active material provided in the embodiments of the present application has the characteristics of a single crystal phase, high purity, regular morphology, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency. In addition, the phosphate composite positive electrode active material also has a continuous conductive network and a shortened ion transport path, which is conducive to promoting the efficient transmission of electrons and ions, and thus is conducive to improving the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0148] In some embodiments, the volume distribution particle size Dv50 of the phosphate composite positive active material satisfies 0.5 μm≤Dv50≤3 μm.
[0149] In some embodiments, the volume distribution particle sizes Dv90 and Dv50 of the phosphate composite positive active material satisfy 1<Dv90 / Dv50≤1.5.
[0150] In some embodiments, the powder resistivity of the phosphate composite positive active material may be 1-100 Ω·cm.
[0151] In some embodiments, the phosphate positive electrode active material has the formula Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R n , M represents a doping element for the Mn position and / or Fe position, optionally including one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr; N represents a doping element for the Li position, optionally including one or more elements of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents a doping element for the P position, optionally including one or more elements of B, S, Si and N; R represents an O-position doping element, optionally including one or more elements of S, F, Cl and Br; 0.9≤a≤1.1; 0≤b≤0.1; 0≤x≤1; 0≤y≤1; 0≤1-xy<1; 0≤m≤0.1; 0≤n≤0.1.
[0152] In some embodiments, 0.001≤x≤0.999, 0.001≤y≤0.999, 0≤1-xy≤0.10. Alternatively, 0.199≤x≤0.500, 0.499≤y≤0.800, 0<1-xy≤0.10.
[0153] The embodiment of the present application also provides a positive electrode plate.
[0154] The positive electrode sheet includes a positive electrode current collector and a positive electrode film disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces that face each other in the thickness direction of the positive electrode current collector, and the positive electrode film is disposed on either or both of the two opposing surfaces of the positive electrode current collector.
[0155] The positive electrode film layer includes the above-mentioned phosphate composite positive electrode active material or the phosphate composite positive electrode active material obtained by the above-mentioned preparation method. Of course, the positive electrode film layer may also include other positive electrode active materials, for example, it may also include lithium transition metal oxides and the like. Examples of lithium transition metal oxides may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. The modified compound may be a doping modification and / or surface coating modification of the positive electrode active material.
[0156] In some embodiments, the positive electrode film layer may further optionally include a positive electrode conductive agent. The present application does not particularly limit the type of the positive electrode conductive agent. As examples, the positive electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0157] In some embodiments, the positive electrode film layer may further optionally include a positive electrode binder. This application does not particularly limit the type of positive electrode binder. As an example, the positive electrode binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.
[0158] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0159] The positive electrode film layer is typically formed by coating a positive electrode slurry onto a positive electrode current collector, drying it, and cold pressing it. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional positive electrode conductive agent, an optional positive electrode binder, and any other components in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP).
[0160] An embodiment of the present application also provides a battery.
[0161] The battery mentioned in the embodiments of the present application may be a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in the present application may include a battery cell, a battery module, or a battery pack.
[0162] A battery cell is the smallest unit of a battery, independently capable of charging and discharging. A battery cell can be cylindrical, rectangular, or have other shapes, though this is not a limitation in the present invention. Figure 1 shows a battery cell 5 with a rectangular structure as an example.
[0163] When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed series via a busbar. In some embodiments, the battery may be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module. In some embodiments, the battery may be a battery pack, which includes a housing and battery cells, with the battery cells or battery modules housed in the housing. In some embodiments, the housing may serve as part of the vehicle's chassis structure. For example, a portion of the housing may form at least a portion of the vehicle's floor, or a portion of the housing may form at least a portion of the vehicle's crossbeam or longitudinal beam.
[0164] In some embodiments, the battery may be an energy storage device, including an energy storage container, an energy storage cabinet, and the like.
[0165] The battery cells mentioned in the embodiments of the present application include lithium-ion primary battery cells, lithium-ion secondary battery cells, lithium metal battery cells, negative electrode-free lithium metal battery cells, etc., which are not limited in the embodiments of the present application.
[0166] The battery cell includes an electrode assembly, which may be a wound structure or a laminated structure, and the present invention is not limited thereto.
[0167] The battery cell also includes an outer packaging, which can be used to encapsulate the electrode assembly and electrolyte. The outer packaging can be a hard shell, such as a hard plastic shell, aluminum shell, steel shell, etc. The outer packaging can also be a soft package, such as a bag-type soft package. The soft package can be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0168] In some embodiments, as shown in Figure 2, the outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a bottom plate and side plates connected to the bottom plate, which together form a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 is used to cover the opening, thereby sealing the receiving cavity. The electrode assembly 52 is enclosed in the receiving cavity. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and can be adjusted according to needs.
[0169] In some embodiments, battery cells can be assembled into a battery module. The number of battery cells contained in a battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module. Figure 3 is a schematic diagram of a battery module 4 as an example. As shown in Figure 3, in the battery module 4, multiple battery cells 5 can be arranged in sequence along the length of the battery module 4. Of course, they can also be arranged in any other manner. The multiple battery cells 5 can further be fixed by fasteners.
[0170] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.
[0171] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0172] Figures 4 and 5 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a housing and multiple battery modules 4 disposed within the housing. The housing comprises an upper housing 2 and a lower housing 3. The upper housing 2 covers the lower housing 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the housing.
[0173] The battery cell includes the above-mentioned positive electrode sheet and negative electrode sheet. The structure and composition of the negative electrode sheet can be selected according to the type of battery cell, and the embodiment of the present application is not limited to this.
[0174] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and comprising a negative electrode active material. For example, the negative electrode current collector may have two opposing surfaces in its thickness direction, and the negative electrode film layer may be disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0175] The negative electrode active material may be a material known in the art. As an example, the negative electrode active material may include, but is not limited to, one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composites, silicon-nitrogen composites, and silicon alloy materials. Tin-based materials may include one or more of elemental tin, tin oxide, and tin alloy materials. The present application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials may also be used.
[0176] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent. The present application does not particularly limit the type of the negative electrode conductive agent. For example, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0177] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of the negative electrode binder. As examples, the negative electrode binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, aqueous acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).
[0178] In some embodiments, the negative electrode film layer may further optionally include other additives, such as thickeners, such as sodium carboxymethyl cellulose (CMC), PTC thermistor materials, and the like.
[0179] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0180] The negative electrode film layer is typically formed by coating the negative electrode slurry onto the negative electrode current collector, drying it, and cold pressing it. The negative electrode slurry is typically formed by dispersing the negative electrode active material, optional negative electrode conductive agent, optional negative electrode binder, and other optional additives in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.
[0181] The negative electrode sheet does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode sheet may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) disposed on the surface of the negative electrode current collector and sandwiched between the negative electrode current collector and the negative electrode film layer. In some embodiments, the negative electrode sheet may further include a protective layer covering the surface of the negative electrode film layer.
[0182] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a metal layer disposed on at least one surface of the negative electrode current collector. The metal layer may include one or more of lithium element and lithium alloy.
[0183] A lithium alloy may be an alloy of metallic lithium and other metallic elements or non-metallic elements. For example, the other metallic elements in the lithium alloy may include one or more of tin, zinc, aluminum, magnesium, silver, gold, gallium, indium, and platinum, and the non-metallic elements in the lithium alloy may include one or more of boron, carbon, and silicon.
[0184] In some embodiments, the negative electrode sheet may further include a negative electrode current collector but not a metal layer, thereby forming a negative electrode metal-free battery cell.
[0185] In some embodiments, the negative electrode plate may also be directly made of a sheet (or foil) of lithium or a lithium alloy.
[0186] [Electrolytes]
[0187] The electrolyte conducts active ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte, and the electrolyte can be selected based on needs. For example, the electrolyte can include one or more of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte solution).
[0188] In some embodiments, the electrolyte is an electrolyte solution including an electrolyte salt and a solvent.
[0189] As an example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium bisoxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0190] The type of solvent is not specifically limited and can be selected according to actual needs. In some embodiments, as an example, the solvent can include ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE) One or more.
[0191] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature power performance.
[0192] [Isolation film]
[0193] Battery cells using liquid electrolytes, as well as some using solid electrolytes, also include a separator. This separator is positioned between the positive and negative electrodes, primarily preventing short circuits between the positive and negative electrodes while allowing active ions to pass through. This application does not specifically limit the type of separator; any known porous separator with good chemical and mechanical stability may be used.
[0194] In some embodiments, the material of the isolation membrane can include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different.
[0195] The preparation method of battery cells is well known. In some embodiments, the positive electrode sheet, separator, negative electrode sheet and electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, separator, and negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process, and the electrode assembly is placed in an outer package, dried and injected with the above-mentioned electrolyte, and then subjected to vacuum packaging, standing, formation, shaping and other processes to obtain a battery cell. Multiple battery cells can also be further connected in series, in parallel or in a mixed connection to form a battery module. Multiple battery modules can also be connected in series, in parallel or in a mixed connection to form a battery pack. In some embodiments, multiple battery cells can also directly form a battery pack.
[0196] Electrical devices
[0197] The present application also provides an electrical device, which includes the battery of the present application. The battery can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.
[0198] The electrical device can select a specific type of battery, such as a battery cell, a battery module, or a battery pack, according to its usage requirements.
[0199] Figure 6 is a schematic diagram of an exemplary electrical device. This device is a pure electric vehicle, hybrid electric vehicle, or plug-in hybrid electric vehicle. To meet the device's high power and high energy density requirements, a battery pack or battery module can be used as a power source.
[0200] As another example, an electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a battery cell as a power source.
[0201] Example
[0202] The following examples describe the present disclosure in more detail and are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise indicated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and used directly without further processing, and all instruments used in the examples are commercially available.
[0203] Example 1
[0204] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by the addition of ferrous sulfate and manganese sulfate, with a Mn:Fe molar ratio of 6:4, to form a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0205] The first mixed solution was sheared and stripped using a high-speed homogenizer, with a rotation speed (shear rate) of 8000r / min and a stripping reaction time of 120min to prepare a second mixed solution, in which graphite oxide was stripped into graphene oxide. Maintaining the speed at 8000r / min, an oxalic acid aqueous solution as a precipitant was added to the second mixed solution to form an instantaneous supersaturated suspension, with a molar ratio of oxalic acid as the precipitant to the metal salt of 1:2, and a precipitation reaction time of 20min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation. The slurry was then placed in a vacuum oven at 80°C for drying to obtain Mn 0.6 Fe 0.4 A mixture of C2O4·2H2O and graphene oxide, in which graphene oxide encapsulates Mn 0.6 Fe 0.4 C2O4·2H2O.
[0206] Mn 0.6 Fe 0.4 A mixture of C2O4·2H2O and graphene oxide, Li2CO3 and NH4H2PO4 in a molar ratio of Li:Mn:Fe:P=1.02:0.6:0.4:1 was weighed, and then an appropriate amount of deionized water was added as a solvent and sand-milled at a speed of 2500 r / min for 2 hours to obtain a slurry. The obtained slurry was transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature was set to 210°C. The obtained powder was placed in a tube furnace at 400°C and a nitrogen atmosphere for 5 hours, and naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder was placed in a sand mill, an appropriate amount of deionized water was added as a solvent, and 6wt% sucrose (based on the total weight of the pre-sintered powder) was weighed and placed in a sand mill, and sand-milled at a speed of 2500 r / min for 2 hours to obtain a slurry. The obtained slurry was transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature was set to 210°C. The obtained powder was placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and then pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, coated phosphate positive electrode active material LiMn 0.6 Fe 0.4 Amorphous carbon of PO4 and reduced graphene oxide coated with amorphous carbon.
[0207] Example 2
[0208] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by the addition of ferrous sulfate and manganese sulfate, with a Mn:Fe molar ratio of 6:4, to form a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0209] The first mixed solution was sheared and stripped using a high-speed homogenizer, with a rotation speed (shear rate) of 10,000 r / min and a stripping reaction time of 60 min to prepare a second mixed solution, in which graphite oxide was stripped into graphene oxide. Maintaining the speed at 10,000 r / min, an oxalic acid aqueous solution as a precipitant was added to the second mixed solution to form an instantaneous supersaturated suspension, with a molar ratio of oxalic acid as the precipitant to the metal salt of 1:2, and a precipitation reaction time of 20 min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation. The slurry was then placed in a vacuum oven at 80°C for drying to obtain Mn 0.6 Fe 0.4 A mixture of C2O4·2H2O and graphene oxide, in which graphene oxide encapsulates Mn 0.6 Fe 0.4 C2O4·2H2O.
[0210] Mn 0.6 Fe 0.4 A mixture of C2O4·2H2O and graphene oxide, Li2CO3 and NH4H2PO4 in a molar ratio of Li:Mn:Fe:P=1.02:0.6:0.4:1 was weighed, and then an appropriate amount of deionized water was added as a solvent and sand-milled at a speed of 2500 r / min for 2 hours to obtain a slurry. The obtained slurry was transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature was set to 210°C. The obtained powder was placed in a tube furnace at 400°C and a nitrogen atmosphere for 5 hours, and naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder was placed in a sand mill, an appropriate amount of deionized water was added as a solvent, and 6wt% sucrose (based on the total weight of the pre-sintered powder) was weighed and placed in a sand mill, and sand-milled at a speed of 2500 r / min for 2 hours to obtain a slurry. The obtained slurry was transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature was set to 210°C. The obtained powder was placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and then pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, coated phosphate positive electrode active material LiMn 0.6 Fe 0.4Amorphous carbon of PO4 and reduced graphene oxide coated with amorphous carbon.
[0211] Example 3
[0212] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by the addition of ferrous sulfate and manganese sulfate, with a Mn:Fe molar ratio of 7:3, to form a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0213] The first mixed solution was sheared and stripped using a high-speed homogenizer, with a rotation speed (shear rate) of 6000r / min and a stripping reaction time of 120min to prepare a second mixed solution, in which graphite oxide was stripped into graphene oxide. Maintaining the speed at 6000r / min, an aqueous solution of ammonium oxalate as a precipitant was added to the second mixed solution to form an instantaneous supersaturated suspension, with a molar ratio of ammonium oxalate to metal salt of 1:2, and a precipitation reaction time of 20min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation. The slurry was then placed in a vacuum oven at 80°C for drying to obtain Mn 0.7 Fe 0.3 A mixture of C2O4·2H2O and graphene oxide, in which graphene oxide encapsulates Mn 0.7 Fe 0.3 C2O4·2H2O.
[0214] Mn 0.7 Fe 0.3 A mixture of C2O4·2H2O and graphene oxide, Li2CO3, and NH4H2PO4 in a molar ratio of Li:Mn:Fe:P = 1.02:0.7:0.3:1 was weighed, and then an appropriate amount of deionized water was added as a solvent. The mixture was sand-milled at 2500 r / min for 2 hours to obtain a slurry. The resulting slurry was transferred to a spray dryer for spray drying and granulation to obtain a powder, with the drying temperature set at 210°C. The resulting powder was sintered in a tube furnace at 400°C under a nitrogen atmosphere for 5 hours and naturally cooled to room temperature to obtain a pre-sintered powder. The pre-sintered powder was placed in a sand mill, an appropriate amount of deionized water was added as a solvent, and 6 wt% PVA (based on the total weight of the pre-sintered powder) was weighed and placed in a sand mill. The mixture was sand-milled at 2500 r / min for 2 hours to obtain a slurry. The resulting slurry was transferred to a spray dryer for spray drying and granulation to obtain a powder, with the drying temperature set at 210°C. The obtained powder was placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and then pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.7Fe 0.3 PO4, coated phosphate positive electrode active material LiMn 0.7 Fe 0.3 Amorphous carbon of PO4 and reduced graphene oxide coated with amorphous carbon.
[0215] Example 4
[0216] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by the addition of ferrous sulfate and manganese sulfate, with a Mn:Fe molar ratio of 6:4, to form a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0217] The first mixed solution was sheared and stripped using a high-speed homogenizer, with a rotation speed (shear rate) of 8000r / min and a stripping reaction time of 120min to prepare a second mixed solution, in which graphite oxide was stripped into graphene oxide. Maintaining the speed at 8000r / min, an aqueous solution of ammonium oxalate as a precipitant was added to the second mixed solution to form an instantaneous supersaturated suspension, with a molar ratio of ammonium oxalate to metal salt of 1:2, and a precipitation reaction time of 20min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation. The slurry was then placed in a vacuum oven at 80°C for drying to obtain Mn 0.6 Fe 0.4 A mixture of C2O4·2H2O and graphene oxide, in which graphene oxide encapsulates Mn 0.6 Fe 0.4 C2O4·2H2O.
[0218] Mn 0.6 Fe 0.4A mixture of C2O4·2H2O and graphene oxide, Li2CO3, and NH4H2PO4 in a molar ratio of Li:Mn:Fe:P = 1.02:0.6:0.4:1 was weighed, and then an appropriate amount of deionized water was added as a solvent. The mixture was sand-milled at a speed of 2500 r / min for 2 hours to obtain a slurry. The obtained slurry was transferred to a spray dryer for spray drying and granulation to obtain a powder, and the drying temperature was set to 210°C. The obtained powder was placed in a tube furnace and sintered at 400°C under a nitrogen atmosphere for 5 hours, and then naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder was placed in a sand mill, an appropriate amount of deionized water was added as a solvent, and 3wt% PVA and 3% glucose (based on the total weight of the pre-sintered powder) were weighed and placed in a sand mill. The mixture was sand-milled at a speed of 2500 r / min for 2 hours to obtain a slurry. The obtained slurry was transferred to a spray dryer for spray drying and granulation to obtain a powder, and the drying temperature was set to 210°C. The obtained powder was placed in a tube furnace and sintered at 720°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and then pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, coated phosphate positive electrode active material LiMn 0.6 Fe 0.4 Amorphous carbon of PO4 and reduced graphene oxide coated with amorphous carbon.
[0219] Comparative Example 1
[0220] Under nitrogen gas protection, ferrous sulfate and manganese sulfate were added to an appropriate amount of deionized water at a Mn:Fe molar ratio of 6:4 to prepare a 1 mol / L mixed metal salt solution, and then dispersed and dissolved using a stirrer at a rotation speed of 600 r / min to prepare a mixed solution.
[0221] Under the condition of stirring speed of 600r / min, the precipitant oxalic acid aqueous solution was added to the mixed solution to form an instantaneous supersaturated suspension. The molar ratio of the precipitant oxalic acid to the metal salt was 1:2. The precipitation reaction time was 20min, until the reaction was complete. The obtained mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation. The slurry was then placed in a vacuum oven at 80℃ for drying to obtain Mn 0.6 Fe 0.4 C2O4·2H2O.
[0222] Mn 0.6 Fe 0.4C2O4·2H2O, Li2CO3 and NH4H2PO4 are weighed in a molar ratio of Li:Mn:Fe:P=1.02:0.6:0.4:1, and then an appropriate amount of deionized water is added as a solvent. The mixture is sand-milled at a speed of 2500 r / min for 2 hours to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 400°C in a nitrogen atmosphere for 5 hours, and naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder is placed in a sand mill, an appropriate amount of deionized water is added as a solvent, and 11wt% sucrose (based on the total weight of the pre-sintered powder) is weighed and placed in a sand mill. The mixture is sand-milled at a speed of 2500 r / min for 2 hours to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder was placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and then pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, coated phosphate positive electrode active material LiMn 0.6 Fe 0.4 Amorphous carbon of PO4.
[0223] Comparative Example 2
[0224] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by the addition of ferrous sulfate and manganese sulfate, with a Mn:Fe molar ratio of 6:4, to form a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0225] The first mixed solution was sheared and stripped using a high-speed homogenizer, with a rotation speed (shear rate) of 8000r / min and a stripping reaction time of 120min to prepare a second mixed solution, in which graphite oxide was stripped into graphene oxide. Maintaining the speed at 8000r / min, an oxalic acid aqueous solution as a precipitant was added to the second mixed solution to form an instantaneous supersaturated suspension, with a molar ratio of oxalic acid as the precipitant to the metal salt of 1:2, and a precipitation reaction time of 20min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation. The slurry was then placed in a vacuum oven at 80°C for drying to obtain Mn 0.6 Fe 0.4 A mixture of C2O4·2H2O and graphene oxide, in which graphene oxide encapsulates Mn 0.6 Fe 0.4 C2O4·2H2O.
[0226] Mn 0.6 Fe 0.4 A mixture of C2O4·2H2O and graphene oxide, Li2CO3, and NH4H2PO4 was weighed in a molar ratio of Li:Mn:Fe:P = 1.02:0.6:0.4:1. An appropriate amount of deionized water was added as a solvent, and the mixture was sand-milled at 2500 r / min for 2 hours to obtain a slurry. The resulting slurry was transferred to a spray dryer for spray drying and granulation to obtain a powder, with the drying temperature set at 210°C. The resulting powder was sintered in a tube furnace at 400°C under a nitrogen atmosphere for 5 hours, and then naturally cooled to room temperature to obtain a pre-sintered powder. The pre-sintered powder was placed in a sand mill, an appropriate amount of deionized water was added as a solvent, and sand-milled at 2500 r / min for 2 hours to obtain a slurry. The resulting slurry was transferred to a spray dryer for spray drying and granulation to obtain a powder, with the drying temperature set at 210°C. The obtained powder was placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and then pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, coated phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4-reduced graphene oxide.
[0227] Test section
[0228] (1) Powder resistivity test
[0229] Use a powder resistivity tester, such as the PRCD1100 from Yuanneng Technology, to test the powder resistivity of phosphate composite cathode active materials. Place a certain amount of phosphate composite cathode active material powder in a dedicated mold. Then, place the mold on a compaction density instrument and set the pressure to 4 MPa. After applying pressure, read the corresponding powder resistivity.
[0230] (2) Volume distribution particle size Dv50 test
[0231] Use a laser particle size analyzer, such as the Malvern Master Size 3000, to measure the volume distribution particle size of the phosphate composite cathode active material. Dv50 refers to the particle size at which the cumulative volume distribution percentage of the material reaches 50%. The test is based on GB / T 19077-2016.
[0232] (3) Metal element content test
[0233] The contents of manganese and iron in the phosphate composite positive electrode active material are measured by ICP-OES using an inductively coupled plasma optical emission spectrometer, such as Plasma 3000, and their molar ratios are calculated.
[0234] (4) Test of average number of graphene layers
[0235] The number of graphene layers is determined using an atomic force microscope, such as a Multimode 8. The thickness of a single layer of graphene is typically between 0.4 nm and 0.7 nm. By observing the graphene morphology using an atomic force microscope, the number of graphene layers can be estimated based on the height curve.
[0236] (5) Preparation and testing of button batteries
[0237] The phosphate composite positive active material prepared in the above embodiments and comparative examples, polyvinylidene fluoride (PVDF), and conductive carbon were added to a certain amount of N-methylpyrrolidone (NMP) in a weight ratio of 90:5:5, stirred in a drying room to form a slurry, and the slurry was coated on aluminum foil, dried, and cold pressed to form a positive electrode sheet. A lithium sheet was used as the negative electrode and assembled with the above-prepared positive electrode sheet in a button box to form a button battery. The concentration of the electrolyte was 1 mol / L, the lithium salt was LiPF6, and the solvent was a mixed system of ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC) in a volume ratio of 1:1:1.
[0238] At 25°C, the prepared button cell was charged at a constant current of 0.1C to 4.3V. It was then charged at a constant voltage at 4.3V to a current of ≤0.05C and allowed to rest for 2 minutes. The charge capacity at this point was recorded as C0. The button cell was then discharged at a constant current of 0.1C to 2.0V. The discharge capacity at this point was the initial discharge capacity, recorded as D0. The specific discharge capacity of the button cell (mAh / g) is D0 / m, where m represents the mass of the phosphate composite positive electrode active material.
[0239] At 25°C, each button cell prepared above was charged at a constant current of 1C to 4.3V. Then, constant voltage charging was performed at 4.3V to a current ≤ 0.05C. The cells were allowed to rest for 2 minutes, and the charge capacity at this point was recorded as the first cycle charge capacity. The button cells were then discharged at a constant current of 1C to 2.0V, and the discharge capacity at this point was recorded as the first cycle discharge capacity. The button cells were subjected to cyclic charge and discharge tests according to the above method, and the discharge capacity after each cycle was recorded. The capacity retention rate of the button cell after 200 cycles = discharge capacity after 200 cycles / discharge capacity after the first cycle.
[0240] At 25°C, the button batteries prepared above were charged to 4.3V at constant currents of 0.1C, 0.5C, 1C, 2C, 5C and 10C, respectively, and then charged at constant voltage at 4.3V to a current ≤0.05C and allowed to stand for 2 min; the button batteries were then discharged to 2.0V at constant currents of 0.1C, 0.5C, 1C, 2C, 5C and 10C, respectively, and the discharge capacities of the button batteries at different charge and discharge rates (0.1C, 0.5C, 1C, 2C, 5C and 10C) were recorded.
[0241] The above test results are shown in Table 1.
[0242] Table 1
[0243] Figure 7(a) shows the Mn prepared in Example 1 0.6 Fe 0.4 Scanning electron microscope (SEM) image of the mixture of C2O4·2H2O and graphene oxide, FIG7(b) shows the Mn prepared in Comparative Example 1. 0.6 Fe 0.4 Scanning electron microscope (SEM) image of C2O4·2H2O. As can be seen from Figure 7, the phosphate cathode active material precursor obtained by the preparation method provided in the embodiment of the present application has the characteristics of regular morphology, small particle size, narrow particle size distribution, and can also be well wrapped by graphene oxide.
[0244] Figure 8(a) shows a scanning electron microscope (SEM) image of the phosphate composite positive electrode active material prepared in Example 1, and Figure 8(b) shows a scanning electron microscope (SEM) image of the phosphate composite positive electrode active material prepared in Comparative Example 1. As can be seen from Figure 8, the phosphate composite positive electrode active material obtained using the preparation method provided in the examples of the present application can form a continuous conductive network.
[0245] Figure 9 is a capacity-voltage curve of a button cell prepared from the phosphate composite positive electrode active materials of Example 1 and Comparative Example 1. Figure 10 is a rate curve of a button cell prepared from the phosphate composite positive electrode active materials of Example 1 and Comparative Example 1. Based on the test results of Figures 9 and 10 and Table 1, it can be seen that the preparation method provided by the embodiments of the present application can not only reduce the cost of raw materials, but also make the obtained phosphate composite positive electrode active material have the characteristics of regular morphology, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency, and can also form a continuous conductive network and shorten the ion transmission path, which is conducive to promoting the efficient transmission of electrons and ions, thereby making the battery have high discharge specific capacity, good rate performance and good cycle stability.
[0246] In Comparative Example 2, no carbon source was added when preparing the phosphate composite positive electrode active material. At this time, a continuous conductive network could not be constructed in the phosphate composite positive electrode active material, resulting in the prepared phosphate composite positive electrode active material having high powder resistivity and poor electron transport capacity, which in turn affected the rate performance of the battery. In addition, it also affected the cycle stability of the battery.
[0247] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing a phosphate composite positive electrode active material, comprising the following steps: Providing a first mixed solution comprising graphite oxide and a metal salt for preparing a phosphate positive electrode active material, wherein the solvent in the first mixed solution comprises water; The first mixed solution is subjected to a first exfoliation reaction at a first shear rate of more than 6000 r / min, so that the graphite oxide is exfoliated into graphene oxide, thereby obtaining a second mixed solution; Maintaining the first shear rate, adding a precipitant or an aqueous solution of the precipitant to the second mixed solution to perform a second precipitation reaction to obtain a third mixed solution, wherein the precipitant includes one or more of oxalic acid and a water-soluble oxalate; Washing and drying the third mixed solution to obtain a mixture of a phosphate positive electrode active material precursor and graphene oxide; The phosphate positive electrode active material precursor and graphene oxide mixture are ground with a lithium source, a phosphorus source, a carbon source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source in the presence of a first solvent to obtain a slurry, and then spray-dried, granulated, and sintered to obtain a phosphate composite positive electrode active material. in, The phosphate composite positive electrode active material comprises a phosphate positive electrode active material, amorphous carbon coating the phosphate positive electrode active material, and reduced graphene oxide coating the amorphous carbon.
2. The method according to claim 1, in, The first stripping reaction is carried out in a high-speed dispersing homogenizer; and / or, The first shearing speed is 6000-15000 r / min, and can be 6000-10000 r / min; and / or, The first stripping reaction time is 30-150 minutes, and can be 60-120 minutes; and / or, The number of layers of the graphene oxide is 1-6, and can be 3-5.
3. The method according to claim 1 or 2, in, The mass ratio of the graphite oxide to the metal salt used to prepare the phosphate positive electrode active material is 0.03:1-0.08:1; and / or, The concentration of the metal salt used to prepare the phosphate positive electrode active material in the first mixed solution is 0.5-2 mol / L; and / or, The metal salt used to prepare the phosphate positive electrode active material includes a water-soluble divalent metal salt. Optionally, the water-soluble divalent metal salt includes one or more of sulfate, nitrate, hydrochloride and acetate.
4. The method according to claim 3, in, The divalent metal element includes Mn element and / or Fe element and optionally M element, wherein M element represents the doping element of Mn position and / or Fe position of the phosphate composite positive electrode active material, and optionally includes one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr.
5. The method according to any one of claims 1 to 4, in, The second precipitation reaction time is 10-60 min; and / or, The molar ratio of the precipitant to the metal salt used to prepare the phosphate positive electrode active material is 1:1-3:1; and / or, The precipitant comprises one or more of oxalic acid, sodium oxalate, potassium oxalate and ammonium oxalate; and / or, The concentration of the aqueous solution of the precipitant is 0.5-2 mol / L.
6. The method according to any one of claims 1 to 5, in, The step of providing a first mixed solution containing graphite oxide and a metal salt for preparing a phosphate positive electrode active material comprises the following steps: Under a protective gas atmosphere, adding graphite oxide to water, then adding a metal salt for preparing a phosphate positive electrode active material, and dispersing the mixture evenly to obtain the first mixed solution; Optionally, the protective gas includes nitrogen, an inert gas or a combination thereof.
7. The method according to any one of claims 1 to 6, in, The first solvent includes one or more of an alcohol solvent and water, and may be one or more of ethanol and water; and / or, The grinding process includes high-energy ball milling or sand milling; and / or, The grinding process has a rotation speed of 1000-2500 r / min; and / or, The grinding time is 1-5h.
8. The method according to any one of claims 1 to 7, in, The sintering process includes a pre-sintering process and a high-temperature sintering process; Optionally, the pre-sintering temperature is 350-550° C., optionally 400-500° C.; and / or, Optionally, the pre-sintering treatment time is 2-12 hours, optionally 3-10 hours; and / or, Optionally, the temperature of the high temperature sintering treatment is 600-800° C., optionally 650-750° C.; and / or, Optionally, the high temperature sintering treatment time is 5-24 hours, optionally 8-12 hours; and / or, Optionally, the pre-sintering process is performed under a protective gas atmosphere; and / or, Optionally, the high-temperature sintering treatment is performed under a protective gas atmosphere.
9. The method according to claim 8, in, The steps of grinding the mixture of the phosphate positive electrode active material precursor and graphene oxide with a lithium source, a phosphorus source, a carbon source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source in the presence of a first solvent to obtain a slurry, and then spray drying, granulating, and sintering to obtain a phosphate composite positive electrode active material include the following steps: The phosphate positive electrode active material precursor and the graphene oxide mixture are subjected to a first grinding treatment with a lithium source, a phosphorus source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source in the presence of a first solvent to obtain a first slurry; The first slurry is spray-dried and granulated to obtain powder, and then pre-sintered to obtain pre-sintered powder; Grinding the pre-sintered powder and the carbon source for a second time in the presence of a first solvent to obtain a second slurry; The second slurry is spray-dried and granulated to obtain powder, which is then subjected to high-temperature sintering treatment and optionally crushing treatment to obtain the phosphate composite positive electrode active material.
10. The method according to claim 9, in, The rotation speed of the first grinding process is 1500-2500r / min; and / or, The first grinding treatment lasts for 1-5 hours; and / or, The rotation speed of the second grinding process is 1000-2500r / min; and / or, The second grinding process lasts for 1-3 hours.
11. The method according to any one of claims 1 to 10, in, The Li-site doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W; and / or, The P-site doping element includes one or more elements selected from B, S, Si and N; and / or, The O-site doping element includes one or more elements selected from the group consisting of S, F, Cl and Br.
12. The method according to any one of claims 1 to 11, in, The lithium source includes one or more of lithium hydroxide, lithium carbonate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, lithium nitrate and lithium acetate; and / or, The phosphorus source includes one or more of phosphoric acid, ammonium monohydrogen phosphate and ammonium dihydrogen phosphate; and / or, The carbon source comprises one or more of sucrose, glucose, polyvinyl alcohol, polyethylene glycol, phenolic resin, citric acid and cyclodextrin; and / or, The Li-doping element source includes one or more of sulfate, nitrate, hydrochloride and acetate of the Li-doping element; and / or, The P-site doping element source includes one or more of sulfates, borates, nitrates and silicates of the P-site doping element; and / or, The O-site doping element source includes one or more of a simple substance and an ammonium salt of the O-site doping element.
13. A phosphate composite positive electrode active material prepared by the method according to any one of claims 1 to 12, wherein the phosphate composite positive electrode active material comprises a phosphate positive electrode active material, amorphous carbon coating the phosphate positive electrode active material, and reduced graphene oxide coating the amorphous carbon.
14. The phosphate composite positive electrode active material according to claim 13, in, The volume distribution particle size Dv50 of the phosphate composite positive electrode active material satisfies 0.5 μm≤Dv50≤3 μm; and / or, The volume distribution particle sizes Dv90 and Dv50 of the phosphate composite positive electrode active material satisfy 1<Dv90 / Dv50≤1.5; and / or, The powder resistivity of the phosphate composite positive electrode active material is 1-100Ω·cm.
15. The phosphate composite positive electrode active material according to claim 13 or 14, in, The molecular formula of the phosphate positive electrode active material is Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R n , M represents a doping element at the Mn position and / or the Fe position, and may optionally include one or more elements selected from the group consisting of Ni, Co, Mg, Zn, Ca, Ti, V and Cr; N represents a Li-site doping element, optionally including one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents a P-site doping element, which may optionally include one or more elements selected from B, S, Si and N; R represents an O-position doping element, which may optionally include one or more elements selected from S, F, Cl and Br; 0.9≤a≤1.1; 0≤b≤0.1; 0≤x≤1; 0≤y≤1; 0≤1-xy<1; 0≤m≤0.1; 0≤n≤0.
1.
16. The phosphate composite positive electrode active material according to claim 15, in, 0.001≤x≤0.999, 0.001≤y≤0.999, 0≤1-xy≤0.10; Optionally, 0.199≤x≤0.500, 0.499≤y≤0.800, 0<1-xy≤0.
10.
17. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, in, The positive electrode film layer comprises a phosphate composite positive electrode active material prepared by the method according to any one of claims 1 to 12 or a phosphate composite positive electrode active material according to any one of claims 13 to 16.
18. A battery cell comprising the positive electrode sheet according to claim 17.
19. A battery comprising the battery cell according to claim 18.
20. An electrical device comprising the battery according to claim 19.
Citation Information
Patent Citations
Preparation method of graphene modified LiMnxFe1-xPO4 / C composite material
CN104993133A
Graphene composite catalyst for fuel cell and preparation method of graphene composite catalyst
CN106654305A
A mechanochemical polymerization method for preparing graphene / metal oxide composite electrode materials
CN109216044A
Lithium iron phosphate nanorod / graphene composite material as well as preparation method and application thereof
CN109904409A
Carbon-coated graphene / metal oxide composite material and preparation method thereof
CN113690429A
Cited By
Secondary battery and preparation method thereof, battery pack, energy storage system and electric equipment
CN119920887A
Preparation method of anion-cation co-doped high-entropy sodium ion battery positive electrode material
CN121506854A