Pole piece, electrode assembly, battery cell, battery, and electrical device

By setting the compaction density of the middle part of the active material layer on the electrode sheet is smaller than the edge, and using a primer to connect the current collector, the problem of easy extrusion of the electrolyte is solved, and the performance and cycle life of the battery cell are improved.

WO2024244419A1PCT designated stage expired Publication Date: 2024-12-05CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/140368
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2023-12-20
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The processing process of electrode components in battery cells of electric vehicles is complicated, resulting in limited battery performance and cycle life, especially the problem of easy extrusion of electrolyte is difficult to solve.

Method used

Design an electrode sheet with an average compaction density of the active material layer in the middle of the current collector less than the edge, increasing the porosity in the middle to accommodate more electrolyte, and connecting and fixing the current collector through the basecoat layer to improve the performance of the electrode assembly and stability.

Benefits of technology

It effectively reduces the phenomenon of easy extrusion of electrolyte, improves the performance and cycle life of the battery cell, and simplifies the processing process of electrode assembly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023140368_05122024_PF_FP_ABST
    Figure CN2023140368_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Embodiments of the present application disclose a pole piece, an electrode assembly, a battery cell, a battery, and an electrical device. The pole piece comprises: a current collector; an active material layer laid on the surface of the current collector, the average compaction density of the portion of the active material layer laid in the center portion of the current collector being less than the average compaction density of the portion of the active material layer laid on the edge portion of the current collector. The pole piece, the electrode assembly, the battery cell, the battery and the electrical device provided by the embodiments of the present application can improve electrode assembly performance.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode pieces, electrode assemblies, battery cells, batteries and electrical equipment

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310640974.5 filed on May 31, 2023, entitled “Pole piece, electrode assembly, battery cell, battery and electrical equipment,” the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the field of batteries, and more specifically, to a pole piece, an electrode assembly, a battery cell, a battery, and an electrical device. Background Art

[0004] Energy conservation and emission reduction are key to the sustainable development of the automotive industry. In this context, electric vehicles, due to their energy-saving and environmentally friendly advantages, have become a crucial component of the industry's sustainable development. Battery technology, in turn, is a crucial factor in the development of electric vehicles.

[0005] The overall battery manufacturing process is long and complex, encompassing a series of steps, including coating, sheeting, assembly, laser welding, and fluid injection. The processing of the electrode assembly within the battery cell is particularly critical, directly impacting the processing efficiency and performance of the battery cell. Therefore, improving the processing efficiency and performance of the electrode assembly is a pressing technical challenge.

[0006] Summary of the Invention

[0007] The embodiments of the present application provide a pole piece, an electrode assembly, a battery cell, a battery, and an electrical device, which can improve the performance of the electrode assembly.

[0008] In a first aspect, a pole piece is provided, comprising: a current collector; an active material layer laid on the surface of the current collector; the average compaction density of the portion of the active material layer laid on the middle of the current collector is less than the average compaction density of the portion laid on the edge of the current collector.

[0009] Therefore, in the electrode of the embodiment of the present application, the average compaction density of the portion of the active material layer located in the middle of the current collector is set to be lower than the average compaction density of the portion located at the edge of the current collector, so that the porosity of the portion of the active material layer located in the middle is greater than the porosity of the portion located at the edge. In this way, the central area can accommodate more electrolyte, which can effectively solve the problem of lithium deposition caused by the electrolyte being easily squeezed out in the central area. In other words, it can effectively reduce the lithium deposition phenomenon, thereby improving the performance and cycle life of the battery cell.

[0010] In some embodiments, the average thickness of the portion of the active material layer disposed in the middle of the current collector is greater than the average thickness of the portion disposed at the edge of the current collector. By setting the average thickness of the active material layer to be greater in the middle portion and smaller in the edge portion, it is easier to achieve the effect of having a lower average compaction density of the portion of the active material layer disposed in the middle of the current collector and a higher average compaction density of the portion disposed at the edge of the current collector, thereby facilitating processing.

[0011] In some embodiments, a first groove opening toward the active material layer is provided in the middle of the current collector, and the average thickness of the bottom wall of the first groove is less than the average thickness of the edge of the current collector. Through the first groove, the average thickness of the active material layer laid in the middle of the current collector can be greater than the average thickness of the part laid on the edge of the current collector.

[0012] In some embodiments, the electrode further comprises: a primer layer disposed at least partially between the current collector and the active material layer. The primer layer can be used to connect and secure the current collector and the active material layer, and can also be used to increase the electrical conductivity of the electrode.

[0013] In some embodiments, the middle portion of the current collector is in direct contact with the active material layer, and the primer layer is disposed between the edge of the current collector and the active material layer. Thus, regardless of whether the middle portion of the current collector is provided with the first groove, since the edge of the current collector is provided with an additional primer layer compared to the middle portion, it is convenient to set the average thickness of the middle portion of the active material layer to be greater than the average thickness of its edge portions, thereby facilitating the average compaction density of the middle portion of the active material layer to be lower than the average compaction density of its edge portions.

[0014] In some embodiments, the primer layer is disposed throughout the entire area between the current collector and the active material layer. Thus, the primer layer can more effectively connect and secure the current collector and the active material layer, and can also increase the conductivity of the electrode, thereby improving the stability and performance of the electrode.

[0015] In some embodiments, a portion of the primer layer corresponding to the middle portion of the current collector is provided with a second groove opening toward the active material layer. The middle portion of the active material layer is located within the second groove, so that the average thickness of the middle portion of the active material layer is greater than the average thickness of the edge portion thereof, thereby also achieving an average compaction density of the portion of the active material layer laid in the middle portion of the current collector less than the average compaction density of the portion of the active material layer laid at the edge of the current collector.

[0016] In some embodiments, the average thickness of the bottom wall of the second groove is less than the average thickness of the portion of the primer layer corresponding to the edge of the current collector. In this way, regardless of whether the middle portion of the current collector is provided with the first groove, and regardless of whether the average thickness of the bottom wall of the second groove exceeds the depth of the first groove, the average thickness of the middle portion of the active material layer can be greater than the average thickness of its edge portion, and further, the average compaction density of the portion of the active material layer laid in the middle portion of the current collector can be less than the average compaction density of the portion of the active material layer laid in the edge of the current collector. The structure is simple and easy to implement.

[0017] In some embodiments, the edge of the current collector includes a first part and a second part, the first part is located at one end of the current collector in the width direction of the pole piece, the second part is located at the other end of the current collector in the width direction of the pole piece, and the middle part of the current collector is located between the first part and the second part.

[0018] The middle of the current collector is set in the middle position of the width direction of the pole piece. After the pole piece is processed into an electrode assembly, whether it is a wound electrode assembly or a laminated electrode assembly, the middle of the current collector corresponds to the middle position of the electrode assembly, and the portion of the active material layer laid in the middle of the current collector also corresponds to the middle position of the electrode assembly. In particular, for a wound electrode assembly, taking the figure as an example, when the compaction density of the portion of the active material layer laid in the middle of the current collector is large, the porosity of this portion is relatively small, which can accommodate more electrolyte, and can effectively solve the problem of lithium deposition caused by the easy extrusion of electrolyte in the middle area, that is, it can effectively reduce the lithium deposition phenomenon, thereby improving the performance and cycle life of the battery cell.

[0019] In some embodiments, the edge of the current collector includes a third part and a fourth part, the third part is located at one end of the current collector in the length direction of the pole piece; the fourth part is located at the other end of the current collector in the length direction of the pole piece, and the middle part of the current collector is located between the third part and the fourth part, so as to be suitable for different types of electrode assemblies. For example, it can be applied to laminated electrode assemblies to effectively reduce the lithium plating phenomenon of laminated electrode assemblies, thereby improving the performance and cycle life of battery cells.

[0020] In some embodiments, along the width direction of the pole piece, the ratio of the average width W1 of the middle part of the current collector to the average width W2 of the pole piece is in the range of [1 / 3, 2 / 3]. If the ratio of W1 to W2 is too small, for example, less than 1 / 3, the width W1 of the middle part of the current collector will be too small, and the width W1 of the part where the active material layer is laid in the middle part of the current collector will also be too small, that is, only a small part of the area can achieve the effect of increasing the compaction density, and correspondingly, only a small part of the area can reduce the lithium plating problem, and the effect of improving the performance and cycle life of the battery cell will not be obvious. On the contrary, if the ratio of W1 to W2 is too large, for example, greater than 2 / 3, the width W1 of the middle part of the current collector will be too large, that is, the width W1 of the part where the active material layer is laid in the middle part of the current collector will also be too large. Although it can effectively solve the lithium plating problem of the pole piece, it will increase the cost of the electrode assembly and increase the difficulty of processing the electrode assembly.

[0021] In some embodiments, along the width direction of the pole piece, the ratio of the average width of the middle part of the current collector to the average width of the pole piece is in the range of [40%, 60%], so that the width of the part where the active material layer is laid in the middle part of the current collector will not be too large or too small, which can not only effectively solve the lithium plating problem of the pole piece, but also make the processing difficulty and cost of the electrode assembly not too high, thereby improving the processing efficiency of the battery cell.

[0022] In some embodiments, along the thickness direction of the electrode sheet, the difference H1-H2 between the average thickness H1 of the portion of the active material layer laid on the middle of the current collector and the average thickness H2 of the portion laid on the edge of the current collector, and the ratio of the average thickness H2 of the portion of the active material layer laid on the edge of the current collector are in the range of [1%, 3%]. If the ratio between the thickness difference H1-H2 and the average thickness H2 is too small, the value of the difference H1-H2 of the electrode sheet will be set too small, and the difference between the average compaction density of the portion of the active material layer laid on the middle of the current collector and the average compaction density of the portion of the active material layer laid on the edge of the current collector will also be too small, which may affect the performance of the electrode sheet and fail to effectively solve the lithium plating problem. On the contrary, if the ratio between the thickness difference H1-H2 and the average thickness H2 is too large, the value of the difference H1-H2 of the electrode sheet is set too large, which will increase the difficulty of processing the electrode sheet and may also affect the structural strength of the electrode sheet, thereby affecting the processing efficiency of the electrode assembly and the battery cell.

[0023] In some embodiments, along the thickness direction of the electrode sheet, the difference between the average thickness of the portion of the active material layer laid in the middle of the current collector and the average thickness of the portion laid on the edge of the current collector is H, the unit of H is μm, and the average compaction density of the portion of the active material layer laid in the middle of the current collector is Y, the unit of Y is g / cm 3, H and Y satisfy Y=KH, where the value range of K is [0.1, 0.4].

[0024] Taking into account that the average compaction density of the part of the active material layer laid in the middle of the current collector has a certain range of values, therefore, if the proportional coefficient K is too large, the thickness difference H will be too large. In this case, on the one hand, the average thickness of the part of the active material layer laid in the middle of the current collector may be too large, which will make the thickness of the pole piece too large, thereby affecting the energy density of the battery cell formed by the processing of the pole piece. On the other hand, the average thickness of the part of the active material layer laid on the edge of the current collector may be too small, which will lead to weak structural strength of the pole piece and affect the performance of the pole piece.

[0025] On the contrary, if the proportional coefficient K is too small, the thickness difference H will be too small. For example, the thickness difference H may approach zero, which will make the thickness of the part of the active material layer laid on the middle of the current collector approximately equal to the thickness of the part of the active material layer laid on the edge of the current collector. Correspondingly, the difference between the average compaction density of the part of the active material layer laid on the middle of the current collector and the average compaction density of the part of the active material layer laid on the edge of the current collector will also be too small, which may affect the performance of the electrode and fail to solve the lithium plating problem well.

[0026] In some embodiments, the average compaction density of the portion of the active material layer located in the middle of the current collector is Y, where the unit of Y is g / cm 3 The total coating mass of the material laid on the surface of the current collector facing the active material layer is M, and the unit of M is g / 1540.25mm 2 , Y and M satisfy Y=NM, where the value range of N is [1, 7].

[0027] When the total coating mass M of the material laid on the surface of the current collector facing the active material layer is constant, if the proportional coefficient N is too large, the average compaction density Y of the portion of the active material layer laid in the middle of the current collector will be too large. Correspondingly, the average compaction density of the portion of the active material layer laid on the edge of the current collector will be even greater, which will increase the difficulty and cost of processing the electrode sheet. Conversely, if the proportional coefficient N is too small, the average compaction density Y of the portion of the active material layer laid in the middle of the current collector will be too small, failing to meet the design requirements of the electrode sheet, reducing the performance of the electrode sheet, and further reducing the performance of the electrode assembly formed by the electrode sheet.

[0028] In some embodiments, the average thickness of the middle of the pole piece is substantially equal to the average thickness of the edge of the pole piece, so that both surfaces of the pole piece are relatively flat, facilitating subsequent processing into an electrode assembly, and making the spacing between different pole piece layers in the electrode assembly relatively uniform, thereby reducing the problem of lithium plating caused by large spacing differences, thereby improving the space utilization and energy density of the battery cell, and reducing lithium plating during the long charge and discharge cycle of the battery cell, thereby improving the cycle life and safety of the battery cell.

[0029] In some embodiments, the electrode sheet includes two active material layers, with the current collector located between the two active material layers. The two active material layers may be any of the active material layers described above with different compaction densities, thereby simultaneously reducing lithium deposition on both sides of the electrode sheet and further improving the performance of the electrode assembly and battery cell.

[0030] In a second aspect, an electrode assembly is provided, comprising: a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet and / or the negative electrode sheet comprises the electrode sheet in the first aspect or any one embodiment of the first aspect.

[0031] In some embodiments, the positive electrode sheet and the negative electrode sheet are wound to form the electrode assembly.

[0032] In some embodiments, the electrode assembly is cylindrical.

[0033] In a third aspect, a battery cell is provided, comprising: the electrode assembly in the second aspect or any one embodiment of the second aspect.

[0034] In a fourth aspect, a battery is provided, comprising a plurality of battery cells, wherein the battery cells comprise the battery cells in the third aspect or any one embodiment of the third aspect.

[0035] In a fifth aspect, an electrical device is provided, comprising: the battery in the fourth aspect or any one embodiment of the fourth aspect, wherein the battery is used to provide electrical energy.

[0036] In some embodiments, the electrical equipment is a vehicle, a ship, or a spacecraft. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] FIG1 is a schematic structural diagram of a vehicle according to an embodiment of the present application;

[0038] FIG2 is a schematic diagram of the exploded structure of a battery according to an embodiment of the present application;

[0039] FIG3 is a schematic diagram of the exploded structure of a battery cell according to an embodiment of the present application;

[0040] FIG4 is a schematic structural diagram of a pole piece according to an embodiment of the present application;

[0041] FIG5 is a schematic structural diagram of a pole piece according to another embodiment of the present application;

[0042] FIG6 is a schematic structural diagram of a pole piece according to another embodiment of the present application;

[0043] 7 to 17 are schematic cross-sectional views of at least a portion of the pole pieces according to different embodiments of the present application.

[0044] In the drawings, the drawings are not drawn to scale. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present application will be described below with reference to the accompanying drawings.

[0046] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0047] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first" and "second" in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order or a primary-secondary relationship.

[0048] References to "embodiments" in this application mean that a particular feature, structure, or characteristic described in connection with the embodiment may be included in at least one embodiment of the application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described in this application may be combined with other embodiments.

[0049] In the description of this application, it should be noted that, unless otherwise expressly specified or limited, the terms "mounted," "connected," "connected," and "attached" should be understood in a broad sense. For example, they may refer to fixed connections, detachable connections, or integral connections; they may refer to direct connections, indirect connections through an intermediate medium, or internal connections between two components. Those skilled in the art will understand the specific meanings of the above terms in this application based on specific circumstances.

[0050] The term "and / or" in this application simply describes an association between related objects, indicating that three possible relationships exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this application generally indicates that the related objects are in an "or" relationship.

[0051] In the embodiments of this application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components in different embodiments are omitted. It should be understood that the thickness, length, width, and other dimensions of the various components in the embodiments of this application, as well as the overall thickness, length, width, and other dimensions of the integrated device shown in the drawings are merely illustrative and should not constitute any limitation on this application.

[0052] The term "multiple" in this application refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0053] In the embodiment of the present application, the battery cell may be a secondary battery. A secondary battery refers to a battery cell that can be continuously used by activating active materials by charging after the battery cell is discharged.

[0054] The battery cells can be lithium-ion batteries, sodium-ion batteries, sodium-lithium-ion batteries, lithium metal batteries, sodium metal batteries, lithium-sulfur batteries, magnesium-ion batteries, nickel-hydrogen batteries, nickel-cadmium batteries, lead-acid batteries, etc., which are not limited in the embodiments of the present application.

[0055] In some implementations, the battery cell in the embodiment of the present application may be a metal battery. Specifically, the metal battery may include a lithium metal secondary battery, a sodium metal battery, or a magnesium metal battery, etc., which is not limited in the embodiment of the present application.

[0056] A battery cell typically includes an electrode assembly. This assembly includes a positive electrode, a negative electrode, and a separator. During the charge and discharge process of a battery cell, active ions (such as lithium ions) are inserted and removed between the positive and negative electrodes. The separator, placed between the positive and negative electrodes, prevents short circuits between the positive and negative electrodes while allowing the active ions to pass through.

[0057] In some embodiments, the positive electrode may be a positive electrode sheet, which may include a positive electrode current collector and a positive electrode active material disposed on at least one surface of the positive electrode current collector.

[0058] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material is provided on either or both of the two facing surfaces of the positive electrode current collector.

[0059] As an example, the positive electrode current collector can be a metal foil, a foamed metal or a composite current collector. For example, as the metal foil, aluminum or stainless steel with a silver surface treatment, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium can be used. The foamed metal can be nickel foam, copper foam, aluminum foam, alloy foam, or carbon foam. The composite current collector may include a polymer material base and a metal layer. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).

[0060] As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0061] In some embodiments, the negative electrode may be a negative electrode sheet, which may include a negative electrode current collector and a negative electrode active material disposed on at least one surface of the negative electrode current collector.

[0062] As an example, the negative electrode current collector has two surfaces facing each other in its thickness direction, and the negative electrode active material is provided on either or both of the two facing surfaces of the negative electrode current collector.

[0063] As an example, the negative electrode current collector may be a metal foil, a metal foam, or a composite current collector. For example, the metal foil may be silver-surface-treated aluminum or stainless steel, stainless steel, copper, aluminum, nickel, a carbon electrode, carbon, nickel, or titanium. The composite current collector may include a polymer material base layer and a metal layer. The metal foam may be nickel foam, copper foam, aluminum foam, alloy foam, or carbon foam. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, or silver alloy, etc.) on a polymer material substrate (such as a substrate made of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).

[0064] As an example, the negative electrode active material may be a negative electrode active material known in the art for use in battery cells. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate.

[0065] In some embodiments, the electrode assembly further includes a separator disposed between the positive electrode and the negative electrode.

[0066] In some embodiments, the separator is a separator. The present application has no particular limitation on the type of separator, and any known separator with a porous structure having good chemical and mechanical stability can be selected.

[0067] As an example, the main material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride, and ceramics.

[0068] In some embodiments, the separator is a solid electrolyte, which is disposed between the positive electrode and the negative electrode and serves to transport ions and isolate the positive and negative electrodes.

[0069] In some embodiments, the battery cell also includes an electrolyte, which acts as a conductor of ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte, and the electrolyte can be selected based on needs. The electrolyte can be liquid, gel, or solid.

[0070] In some embodiments, the electrode assembly is a wound structure, wherein the positive electrode sheet and the negative electrode sheet are wound into the wound structure.

[0071] In some embodiments, the electrode assembly is a laminate structure.

[0072] As an example, multiple positive electrode sheets and multiple negative electrode sheets can be provided respectively, and the multiple positive electrode sheets and the multiple negative electrode sheets can be alternately stacked.

[0073] As an example, a plurality of positive electrode sheets may be provided, and the negative electrode sheet may be folded to form a plurality of stacked folded segments, with a positive electrode sheet being sandwiched between adjacent folded segments.

[0074] As an example, both the positive electrode sheet and the negative electrode sheet are folded to form a plurality of stacked folded segments.

[0075] As an example, a plurality of separators may be provided, each of which is disposed between any adjacent positive electrode sheets or negative electrode sheets.

[0076] As an example, the separator may be provided continuously, and may be provided between any adjacent positive electrode sheets or negative electrode sheets by folding or winding.

[0077] In some embodiments, the shape of the electrode assembly can be cylindrical, flat, or polygonal.

[0078] In some embodiments, the electrode assembly is provided with tabs that can conduct current from the electrode assembly. The tabs include a positive tab and a negative tab.

[0079] In some embodiments, a battery cell may include a housing. The housing is used to encapsulate components such as the electrode assembly and electrolyte. The housing may be a steel housing, an aluminum housing, a plastic housing (e.g., polypropylene), a composite metal housing (e.g., a copper-aluminum composite housing), or an aluminum-plastic film. The housing includes a shell and a cover.

[0080] As an example, the battery cell can be a cylindrical battery cell, a prismatic battery cell, a soft-pack battery cell or a battery cell of other shapes. The prismatic battery cell includes a square-shell battery cell, a blade-shaped battery cell, and a polygonal battery. The polygonal battery is, for example, a hexagonal battery, etc. There is no special limitation in this application.

[0081] The battery mentioned in the embodiments of the present application may include one or more battery cells to provide a single physical module with higher voltage and capacity. When there are multiple battery cells, the multiple battery cells are connected in series, in parallel or in hybrid through a busbar.

[0082] In some embodiments, the battery may be a battery module. When there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module.

[0083] In some embodiments, the battery may be a battery pack, which includes a case and battery cells, wherein the battery cells or battery modules are housed in the case.

[0084] In some embodiments, the box body can be used as a part of the chassis structure of the vehicle. For example, part of the box body can become at least a part of the floor of the vehicle, or part of the box body can become at least a part of the cross beam and longitudinal beam of the vehicle.

[0085] The battery cells in the embodiments of the present application are internally provided with an electrode assembly. During the process of injecting electrolyte into the battery cells, the electrode assembly is typically infiltrated from one end face of the electrode assembly, for example, from the end face where the electrode tab of the electrode assembly is located. Therefore, during this infiltration process, the central region of the electrode pieces constituting the electrode assembly is less effectively infiltrated than the edge regions. Furthermore, during subsequent use of the battery cells, after multiple cycles of charge and discharge, the central region of the electrode pieces is more likely to swell, squeezing out the electrolyte and increasing the resistance to ion movement, which can easily cause lithium deposition in the central region of the electrode pieces, thereby affecting the performance and service life of the battery cells.

[0086] Therefore, the embodiments of the present application provide a pole piece, an electrode assembly, a battery cell, a battery and an electrical device that can solve the above-mentioned problems. The pole piece of the embodiment of the present application includes a current collector and an active material layer laid on the surface of the current collector. The average compaction density of the portion of the active material layer laid on the middle of the current collector is less than the average compaction density of the portion laid on the edge of the current collector, that is, the porosity of the portion of the active material layer located in the middle is greater than the porosity of the portion located at the edge. In this way, the central area can accommodate more electrolyte, which can effectively solve the problem of lithium deposition caused by the easy extrusion of the electrolyte in the central area, that is, it can effectively reduce the lithium deposition phenomenon, thereby improving the performance and cycle life of the battery cell.

[0087] The technical solutions described in the embodiments of this application are applicable to various electrical devices that use batteries.

[0088] Electrical equipment can be vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys, and electric tools, etc. Vehicles can be fuel vehicles, gas vehicles, or new energy vehicles. New energy vehicles can be pure electric vehicles, hybrid vehicles, or extended-range vehicles, etc. Spacecraft include airplanes, rockets, space shuttles, and spacecraft, etc. Electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Electric tools include metal cutting electric tools, grinding electric tools, assembly electric tools, and railway electric tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, etc. The embodiments of the present application do not impose any special restrictions on the above-mentioned electrical equipment.

[0089] For the convenience of description, the following embodiments are described by taking the electric device as a vehicle as an example.

[0090] For example, as shown in FIG1 , it is a structural schematic diagram of a vehicle 1 according to an embodiment of the present application. The vehicle 1 may be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle may be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A motor 40, a controller 30 and a battery 10 may be provided inside the vehicle 1. The controller 30 is used to control the battery 10 to supply power to the motor 40. For example, a battery 10 may be provided at the bottom, front or rear of the vehicle 1. The battery 10 may be used to power the vehicle 1. For example, the battery 10 may be used as an operating power source for the vehicle 1, for the circuit system of the vehicle 1, for example, for the working power requirements during the start-up, navigation and operation of the vehicle 1. In another embodiment of the present application, the battery 10 may not only be used as an operating power source for the vehicle 1, but also as a driving power source for the vehicle 1, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1.

[0091] To meet different power requirements, a battery can include multiple battery cells, which can be connected in series, parallel, or in a hybrid configuration. A hybrid configuration refers to a combination of series and parallel connections. A battery can also be referred to as a battery pack. Alternatively, multiple battery cells can be connected in series, parallel, or in a hybrid configuration to form a battery module, which can then be connected in series, parallel, or in a hybrid configuration to form a battery. In other words, multiple battery cells can be directly connected to form a battery, or they can be first connected to form battery modules, which can then be connected to form a battery.

[0092] For example, Figure 2 shows a schematic structural diagram of a battery 10 according to an embodiment of the present application. The battery 10 may include a plurality of battery cells 20. As shown in Figure 2, the battery 10 may further include a case 11, the interior of the case 11 being a hollow structure, and the plurality of battery cells 20 being accommodated in the case 11. Figure 2 shows a possible implementation of the case 11 of an embodiment of the present application. As shown in Figure 2, the case 11 may include two parts, referred to herein as a first case portion 111 and a second case portion 112, which are snapped together. The shapes of the first case portion 111 and the second case portion 112 may be determined according to the shape of the combination of the plurality of battery cells 20 inside, and at least one of the first case portion 111 and the second case portion 112 has an opening. For example, as shown in Figure 2, the first box body part 111 and the second box body part 112 can both be hollow rectangular parallelepipeds and each has only one open face. The opening of the first box body part 111 and the opening of the second box body part 112 are arranged opposite to each other, and the first box body part 111 and the second box body part 112 are interlocked to form a box body 11 with a closed chamber.

[0093] For another example, unlike that shown in Figure 2, only one of the first and second housing portions 111, 112 may be a hollow rectangular parallelepiped with an opening, while the other may be a plate-shaped structure to cover the opening. For example, in this example, the second housing portion 112 is a hollow rectangular parallelepiped with only one open face, and the first housing portion 111 is a plate-shaped structure. In this example, the first housing portion 111 covers the opening of the second housing portion 112 to form a housing 11 having a closed chamber, which can be used to accommodate multiple battery cells 20. The multiple battery cells 20 are connected in parallel, in series, or in a mixed combination and then placed within the housing 11 formed by the first and second housing portions 111, 112 being fastened together.

[0094] Optionally, the battery 10 may also include other structures, which will not be described in detail here. For example, the battery 10 may also include a busbar component, which is used to achieve electrical connection between multiple battery cells 20, such as parallel connection, series connection, or mixed connection. Specifically, the busbar component can achieve electrical connection between the battery cells 20 by connecting to the electrode terminals 214 of the battery cells 20. Furthermore, the busbar component can be fixed to the electrode terminals 214 of the battery cells 20 by welding. The electrical energy of the multiple battery cells 20 can be further led out through the box 11 via a conductive mechanism.

[0095] The number of battery cells 20 in the battery 10 can be set to any value based on different power requirements. Multiple battery cells 20 can be connected in series, parallel, or in a hybrid manner to achieve higher capacity or power. Since each battery 10 may include a large number of battery cells 20, for ease of installation, the battery cells 20 can also be grouped, with each group of battery cells 20 forming a battery module. The number of battery cells 20 included in a battery module is not limited and can be set according to requirements.

[0096] Figure 3 is a schematic diagram of a partially exploded structure of a battery cell 20 according to one embodiment of the present application. For example, the battery cell 20 shown in Figure 3 may be any of the battery cells 20 shown in Figure 2 . As shown in Figure 3 , the battery cell 20 according to this embodiment of the present application may include a housing 21. Specifically, the housing 21 may include a shell 211 having a hollow structure with at least one opening 2111; a cover plate 212 for covering the opening 2111 of the shell 211; and an electrode assembly 22 housed within the shell 21.

[0097] It should be understood that the housing 211 of the present embodiment is a component for accommodating the electrode assembly 22. The housing 211 may be a hollow structure with an opening 2111 formed at one or more ends. For example, if the housing 211 is a hollow structure with an opening 2111 formed at one end, a single cover plate 212 may be provided. For another example, as shown in FIG3 , if the housing 211 is a hollow structure with openings 2111 formed at opposite ends, two cover plates 212 may be provided, with the two cover plates 212 respectively covering the openings 2111 at both ends of the housing 211.

[0098] The housing 211 may be in various shapes, such as a cylinder, a cuboid, or other polyhedrons. For example, as shown in FIG3 , in the embodiment of the present application, the housing 211 is mainly described as a cylindrical structure.

[0099] It should be understood that the cover plate 212 in the embodiment of the present application is used to cover the opening 2111 of the housing 211 to isolate the internal environment of the battery cell 20 from the external environment. The shape of the cover plate 212 can be adapted to the shape of the housing 211. As shown in Figure 3, the housing 211 has a cylindrical structure, and the cover plate 212 is a circular plate-shaped structure adapted to the housing 211.

[0100] In the embodiment of the present application, the housing 211 can be made of a variety of materials, such as copper, iron, aluminum, steel, and aluminum alloys. The cover plate 212 can also be made of a variety of materials, such as copper, iron, aluminum, steel, and aluminum alloys. Optionally, the material of the cover plate 212 can be the same as or different from that of the housing 211.

[0101] It should be understood that the battery cell 20 also includes an electrode terminal 214. The electrode terminal 214 of the embodiment of the present application is used to electrically connect to the electrode assembly 22 inside the battery cell 20 to output the electrical energy of the battery cell 20. Specifically, the battery cell 20 may include at least two electrode terminals 214, and the at least two electrode terminals 214 may include at least one positive electrode terminal and at least one negative electrode terminal. The positive electrode terminal is used to electrically connect to the positive electrode tab of the electrode assembly 22, and the negative electrode terminal is used to electrically connect to the negative electrode tab of the electrode assembly 22. The positive electrode terminal and the positive electrode tab may be directly or indirectly connected, and the negative electrode terminal and the negative electrode tab may be directly or indirectly connected. Exemplarily, the positive electrode terminal may be electrically connected to the positive electrode tab through a connecting member, and the negative electrode terminal may be electrically connected to the negative electrode tab through a connecting member.

[0102] In some embodiments, the at least two electrode terminals 214 included in the battery cell 20 can be located on different walls, or can also be located on different walls. For example, as shown in FIG3 , in a cylindrical battery cell 20 of an embodiment of the present application, the two electrode terminals 214 can be located on two oppositely disposed cover plates 212 , such that each electrode terminal 214 is electrically connected to a corresponding one of the tabs 221 located at both ends of the electrode assembly 22 .

[0103] In the battery cell 20, the electrode assembly 22 is a component in the battery cell 20 where an electrochemical reaction occurs. Depending on actual usage requirements, the electrode assembly 22 in the shell 211 can be set to one or more. For example, as shown in FIG3 , an electrode assembly 22 is provided in the battery cell 20. The type and shape of the electrode assembly 22 can also be set according to actual usage requirements. For example, the electrode assembly 22 can be a cylinder, a rectangular parallelepiped, etc. For example, as shown in FIG3 , if the shell 211 is a cylindrical structure, the corresponding electrode assembly 22 can also be a cylindrical structure to improve the internal space utilization of the battery cell 20 and the energy density of the battery cell 20; for another example, if the shell 211 is a rectangular parallelepiped structure, the electrode assembly 22 can be a rectangular parallelepiped structure or a cylindrical structure. The embodiments of the present application are not limited to this.

[0104] It should be understood that, as shown in Figure 3, the electrode assembly 22 includes a tab 221 and an electrode body 222, wherein the tab 221 of the electrode assembly 22 may include a positive tab and a negative tab, the positive tab may be formed by stacking the portion of the positive electrode sheet that is not coated with the positive electrode active material layer, and the negative tab may be formed by stacking the portion of the negative electrode sheet that is not coated with the negative electrode active material layer; the electrode body 222 may be formed by stacking or winding the positive electrode sheet and the negative electrode sheet.

[0105] The following describes the electrode sheet used to form an electrode assembly according to an embodiment of the present application, in conjunction with the accompanying drawings. Figure 4 shows a schematic structural diagram of the electrode sheet 3 according to an embodiment of the present application, shown in an unfolded state. As shown in Figure 4 , the electrode sheet 3 includes: a current collector 31; an active material layer 32 applied to the surface of the current collector 31; the average compaction density of the portion 321 of the active material layer 32 applied to the center 311 of the current collector 31 is less than the average compaction density of the portion 322 applied to the edge 312 of the current collector 31.

[0106] In the embodiment of the present application, the electrode sheet 3 may be a positive electrode sheet, or the electrode sheet 3 may also be a negative electrode sheet. For example, for any electrode assembly 22, the positive electrode sheet included in the electrode assembly 22 may be the electrode sheet 3, and / or the negative electrode sheet may be the electrode sheet 3; and the electrode assembly 22 may be a wound electrode assembly 22 or a laminated electrode assembly 22, but the embodiment of the present application is not limited thereto.

[0107] It should be understood that the electrode sheet 3 of the embodiment of the present application may include a tab portion 301 and a main body portion 302, wherein the tab portion 301 is used to form the tab 221 of the electrode assembly 22, and the main body portion 302 is used to form the electrode main body portion 222 of the electrode assembly 22. Specifically, the tab portion 301 of the electrode sheet 3 can be formed by stacking the portion of the electrode sheet 3 that is not coated with the active material layer 32. For example, for a positive electrode sheet, the tab portion 301 can be formed by stacking the portion of the positive electrode sheet that is not coated with the positive active material layer; for a negative electrode sheet, the tab portion 301 can be formed by stacking the portion of the negative electrode sheet that is not coated with the negative active material layer. The main body portion 302 of the electrode sheet 3 is used to stack or wind to form the electrode main body portion 222 of the electrode assembly 22.

[0108] For the sake of convenience of description, the current collector 31 included in the electrode 3 of the embodiment of the present application mainly refers to the current collector 31 of the main body 302 of the electrode 3; correspondingly, the active material layer 32 of the electrode 3 mainly refers to the active material layer 32 of the main body 302 of the electrode 3, and this part of the active material layer 32 is laid on the surface of the corresponding current collector 31.

[0109] For ease of description, the embodiment of the present application defines a length direction X and a width direction Y for the pole piece 3. Specifically, the length direction X of the pole piece 3 is the extension direction of the pole piece 3, the width direction Y of the pole piece 3 is the arrangement direction of the pole ear portion 301 and the main body portion 302 of the pole piece 3, and the length direction X and the width direction Y are perpendicular to each other.

[0110] It should be understood that the active material layer 32 is laid on the surface of the current collector 31 in the embodiment of the present application means that: along the thickness direction of the electrode 3, the current collector 31 includes two surfaces arranged opposite to each other, and the active material layer 32 is laid on any one of the two surfaces. The thickness direction of the electrode 3 is perpendicular to the length direction X and the width direction Y of the electrode 3, that is, the length direction X, the width direction Y and the thickness direction of the electrode 3 are perpendicular to each other.

[0111] In the embodiment of the present application, the average compaction density of the portion 321 of the active material layer 32 of the pole piece 3, which is laid on the middle portion 311 of the current collector 31, is less than the average compaction density of the portion 322 laid on the edge 312 of the current collector 31. That is, the porosity of the portion 321 of the active material layer 32 located in the middle is greater than the porosity of the portion 322 located at the edge. In this way, the central area of ​​the pole piece 3 can accommodate more electrolyte, which can effectively solve the problem of lithium deposition caused by the electrolyte being easily squeezed out of the central area. That is, it can effectively reduce the lithium deposition phenomenon, thereby improving the performance and cycle life of the battery cell 20.

[0112] In the embodiment of the present application, the middle portion 311 of the current collector 31 is closer to the center of the current collector 31 than the edge 312 of the current collector 31, and the middle portion 311 of the current collector 31 can refer to the middle portion of the length direction X of the pole piece 3 and / or the middle portion of the width direction Y of the pole piece 3.

[0113] In some embodiments, the edge 312 of the current collector 31 includes a first portion 3121, which is located at one end of the current collector 31 in the width direction Y of the electrode sheet 3, and the middle portion 311 of the current collector 31 is located at the other end of the current collector 31 in the width direction Y of the electrode sheet 3. Specifically, taking FIG. 4 as an example, in the width direction Y of the electrode sheet 3, the edge 312 of the current collector 31 includes a first portion 3121, which can be located on either side of the middle portion 311 of the current collector 31, and the middle portion 311 of the current collector 31 is closer to the center of the main body 302 than the first portion 3121.

[0114] Furthermore, the edge 312 of the current collector 31 further includes a second portion 3122, which is located at the other end of the current collector 31 in the width direction Y of the electrode piece 3, and the middle portion 311 of the current collector 31 is located between the first portion 3121 and the second portion 3122. Specifically, as shown in FIG4 , in the width direction Y of the electrode piece 3, the middle portion 311 of the current collector 31 is located between the first portion 3121 and the second portion 3122. Therefore, the middle portion 311 of the current collector 31 is closer to the center of the main body 302 than the first portion 3121 or the second portion 3122.

[0115] The middle portion 311 of the current collector 31 is arranged in the middle position of the width direction Y of the electrode sheet 3. After the electrode sheet 3 is processed into the electrode assembly 22, whether it is a wound electrode assembly 22 or a laminated electrode assembly 22, the middle portion 311 of the current collector 31 corresponds to the middle position of the electrode assembly 22, and the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 also corresponds to the middle position of the electrode assembly 22. In particular, for the wound electrode assembly 22, taking Figure 3 as an example, when the compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 is relatively high, the porosity of this portion 321 is relatively small, which can accommodate more electrolyte, and can effectively solve the problem of easy extrusion of electrolyte in the middle area and causing lithium deposition, that is, it can effectively reduce the lithium deposition phenomenon, thereby improving the performance and cycle life of the battery cell 20.

[0116] Figures 5 and 6 respectively show other possible structural schematic diagrams of the electrode piece 3 of the embodiment of the present application, and the electrode piece 3 shown in Figures 5 and 6 is in the unfolded state. Taking Figures 5 and 6 as examples, the middle portion 311 of the current collector 31 may include not only the middle portion of the electrode piece 3 in the width direction Y, but also the middle portion of the electrode piece 3 in the length direction X.

[0117] In some embodiments, the edge 312 of the current collector 31 includes a third portion 3123, the third portion 3123 is located at one end of the current collector 31 in the length direction X of the electrode 3, and the middle portion 311 of the current collector 31 is located at the other end of the current collector 31 in the length direction X of the electrode 3. Specifically, taking Figures 5 and 6 as examples, in the length direction X of the electrode 3, the edge 312 of the current collector 31 may include a third portion 3123, the third portion 3123 may be located on either side of the middle portion 311 of the current collector 31, and the middle portion 311 of the current collector 31 is closer to the center of the main body 302 than the third portion 3123.

[0118] Furthermore, the edge 312 of the current collector 31 further includes a fourth portion 3124, which is located at the other end of the current collector 31 in the length direction X of the pole piece 3, and the middle portion 311 of the current collector 31 is located between the third portion 3123 and the fourth portion 3124. Specifically, as shown in Figures 5 and 6, in the length direction X of the pole piece 3, the middle portion 311 of the current collector 31 is located between the third portion 3123 and the fourth portion 3124. Therefore, the middle portion 311 of the current collector 31 is closer to the center of the main body 302 than the third portion 3123 or the fourth portion 3124.

[0119] In addition, considering that the length direction X of the electrode piece 3 is the extension direction of the electrode piece 3, the lengths of the electrode pieces 3 used in different types of electrode assemblies 22 are different. Therefore, as shown in Figures 5 and 6, in the length direction X of the electrode piece 3, the electrode piece 3 may include one or more third parts 3123, and correspondingly, may also include one or more fourth parts 3124, and the middle part 311 of the current collector 31 is located between a third part 3123 and a corresponding fourth part 3124.

[0120] Different types of pole pieces 3 can be applied to different types of electrode assemblies 22. For example, for the electrode assembly 22 of the wound cylindrical battery cell 20 shown in Figure 3, the pole piece 3 shown in Figure 4 or Figure 5 can generally be used, so that along the width direction Y of the pole piece 3, or along the height direction Y of the electrode assembly 22, the middle part 311 of the current collector 31 can correspond to the middle position of the electrode assembly 22, so that the pole piece 3 of the embodiment of the present application can effectively reduce the lithium plating phenomenon, thereby improving the performance and cycle life of the battery cell 20. For another example, for the electrode assembly 22 of the wound square battery cell 20, the pole piece 3 shown in Figure 4 or Figure 5 can generally be used, which can increase the porosity of the middle area in the height direction of the electrode assembly 22, thereby reducing the lithium plating phenomenon. In particular, for the wound square battery cell 20, the pole piece 3 shown in Figure 6 can also be used. For example, in the electrode assembly 22 formed after winding the electrode sheet 3, the middle portion 311 of the current collector 31 can be used to form the large surface of the electrode assembly 22, and the edge 312 of the current collector 31 can be used to form the edge portion of the electrode assembly 22. For example, the first portion 3121 and the second portion 3122 can be used to form the end portion of the electrode assembly 22, and the third portion 3123 and the fourth portion 3124 can be used to form the corner portion or the bend portion of the electrode assembly 22.

[0121] For another example, a laminated electrode assembly 22 may include multiple positive electrode sheets and multiple negative electrode sheets, with the multiple positive electrode sheets and the multiple negative electrode sheets being alternately stacked. Alternatively, multiple positive electrode sheets may be provided, with the negative electrode sheet being folded to form multiple stacked folded segments, with a positive electrode sheet sandwiched between adjacent folded segments. Alternatively, both the positive electrode sheet and the negative electrode sheet are folded to form multiple stacked folded segments. For the electrode sheet in the electrode assembly 22 that is folded to form multiple stacked folded segments, the electrode sheet may be a electrode sheet 3 as shown in any one of Figures 4 to 6 , wherein the electrode sheet 3 shown in Figure 6 may be folded at the third portion 3123 and the fourth portion 3124 . For the electrode assembly 22 provided with a plurality of electrode sheets, the plurality of electrode sheets can be obtained by processing the electrode sheet 3 shown in FIG6 . For example, the electrode sheet 3 can be cut at the third portion 3123 and the fourth portion 3124 so that the middle portion of each electrode sheet 3 obtained after cutting corresponds to the middle portion 311 of the current collector 31 in the embodiment of the present application. Through the above-mentioned arrangement, the electrode sheet 3 in the embodiment of the present application can effectively reduce the lithium plating phenomenon of the laminated electrode assembly 22, thereby improving the performance and cycle life of the battery cell 20, but the embodiment of the present application is not limited to this.

[0122] It should be understood that the size of the middle portion 311 of the current collector 31 in the embodiment of the present application can be flexibly set according to actual applications. For example, as shown in Figures 4 to 6, along the width direction Y of the electrode 3, the ratio of the average width W1 of the middle portion 311 of the current collector 31 to the average width W2 of the electrode 3 is in the range of [1 / 3, 2 / 3]. If the ratio of W1 to W2 is too small, for example, less than 1 / 3, the width W1 of the middle portion 311 of the current collector 31 will be too small, and the width W1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 will also be too small, that is, only a small part of the area can achieve the effect of increasing the compaction density, correspondingly, only a small part of the area can reduce the lithium plating problem, and the effect of improving the performance and cycle life of the battery cell 20 will not be obvious. On the contrary, if the ratio of W1 to W2 is too large, for example, greater than 2 / 3, the width W1 of the middle part 311 of the current collector 31 will be too large, that is, the width W1 of the part 321 where the active material layer 32 is laid on the middle part 311 of the current collector 31 will also be too large. Although it can effectively solve the lithium plating problem of the electrode 3, it will increase the cost of the electrode assembly 22 and increase the processing difficulty of the electrode assembly 22.

[0123] Therefore, the ratio of W1 to W2 should not be too large or too small. For example, along the width direction Y of the pole piece 3, the ratio of the average width W1 of the middle part 311 of the current collector 31 to the average width W2 of the pole piece 3 is in the range of [40%, 60%], so that the width W1 of the portion 321 of the active material layer 32 laid on the middle part 311 of the current collector 31 will not be too large or too small, which can not only effectively solve the lithium plating problem of the pole piece 3, but also make the processing difficulty and cost of the electrode assembly 22 not too high, so as to improve the processing efficiency of the battery cell 20. For another example, along the width direction Y of the pole piece 3, the ratio of the average width W1 of the middle part 311 of the current collector 31 to the average width W2 of the pole piece 3 can be set to 1 / 3, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65 or 2 / 3, and the embodiments of the present application are not limited to this.

[0124] Similarly, along the length direction X of the electrode 3, the length of the middle portion 311 of the current collector 31 can be flexibly set according to the actual application. For example, whether to provide the third portion 3123 and the length of the third portion 3123 can be determined according to the actual application; for another example, whether to provide the fourth portion 3124 and the length of the fourth portion 3124 can also be determined according to the actual application. The embodiments of the present application are not limited to this.

[0125] It should be understood that for the sake of ease of description, the embodiments of the present application are described in detail below mainly using the pole piece 3 shown in FIG4 as an example, but the relevant description is also applicable to other embodiments shown in FIG5 and FIG6 , which will not be repeated here.

[0126] It should be understood that the compaction density of the embodiment of the present application represents the density of the electrode 3 after the extrusion process, for example, it can represent the density of the electrode 3 after the cold pressing process. The average compaction density of the portion 321 of the active material layer 32 of the embodiment of the present application, which is laid on the middle portion 311 of the current collector 31, can be set according to actual application, and the value range of the average compaction density of the portion 321 can be the same or different for the positive electrode and the negative electrode.

[0127] In some embodiments, if the electrode 3 is a positive electrode, the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 may be in the range of [2.5 g / cm 3 , 3g / cm 3 ], further, the value range can be [2.7g / cm 3 , 2.8g / cm 3 ] to meet the design requirements and effectively avoid lithium plating. For example, the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 can be specifically set to 2.5 g / cm 3 , 2.6g / cm 3 , 2.7g / cm 3 , 2.8g / cm 3 , 2.9g / cm 3 or 3g / cm 3 .

[0128] Correspondingly, when the electrode 3 is a positive electrode, the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 can be in the range of [2 g / cm 3 , 2.6g / cm 3 ], further, the value range can be [2.3g / cm 3 , 2.5g / cm 3 ] to meet the design requirements. For example, the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 can be specifically set to 2g / cm 3 , 2.1g / cm 3 , 2.2g / cm 3 , 2.3g / cm 3 , 2.4g / cm 3 , 2.5g / cm 3 or 2.6g / cm 3 .

[0129] In some embodiments, if the electrode 3 is a negative electrode, the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 may be in the range of [1.2 g / cm 3 , 1.6g / cm 3 ], further, the value range can be [1.3g / cm 3 , 1.5g / cm 3 ] to meet the design requirements and effectively avoid lithium plating. For example, the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 can be specifically set to 1.2 g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 or 1.6 g / cm 3 .

[0130] Correspondingly, when the electrode 3 is a negative electrode, the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 can be in the range of [1.0 g / cm 3 , 1.7g / cm 3 ], further, the value range can be [1.3g / cm 3 , 1.6g / cm 3 ] to meet the design requirements. For example, the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 can be specifically set to 1.0 g / cm 3 , 1.1g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 or 1.7 g / cm 3 .

[0131] It should be understood that in the embodiment of the present application, the average compaction density of the portion 321 of the active material layer 32 disposed on the middle portion 311 of the current collector 31 is lower than the average compaction density of the portion 322 disposed on the edge 312 of the current collector 31. This can be achieved in a variety of ways. For example, this can be achieved by adjusting the cold pressing process; for another example, it can be achieved by setting different thicknesses in different regions.

[0132] FIG7 and FIG8 respectively illustrate partial cross-sectional schematic diagrams of the electrode piece 3 according to different embodiments of the present application. For example, FIG7 and FIG8 may be partial cross-sectional schematic diagrams of any electrode piece 3 shown in FIG4 to FIG6 , wherein the cross section is perpendicular to the longitudinal direction X of the electrode piece 3. As shown in FIG7 and FIG8 , different compaction densities can be achieved by setting different thicknesses in different regions of the active material layer 32.

[0133] Specifically, the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 is greater than the average thickness H2 of the portion 322 laid on the edge 312 of the current collector 31. Before the compaction process, that is, when the active material layer 32 is laid on the surface of the current collector 31, the coating thickness of different regions can be set to be the same or different. However, after the compaction process, by setting the average thickness H1 of the middle portion 321 of the active material layer 32 to be larger and the average thickness H2 of the edge portion 322 to be smaller, it is easy to achieve the effect of having a lower average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 and a higher average compaction density of the portion 322 laid on the edge 312 of the current collector 31, thereby facilitating processing.

[0134] It should be understood that the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 may refer to: along the thickness direction Z of the electrode 3, the average value of the thickness of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31. Similarly, the average thickness H2 of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 may refer to: along the thickness direction Z of the electrode 3, the average value of the thickness of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31. In particular, the thickness direction Z of the electrode 3 in the embodiment of the present application is perpendicular to the length direction X and the width direction Y of the electrode 3.

[0135] It should be understood that the different thicknesses of different regions of the active material layer 32 in the embodiment of the present application can be achieved in a variety of ways. For example, taking Figure 7 as an example, the surface of the active material layer 32 away from the current collector 31 can be uneven to achieve the thickness requirements of different regions. Specifically, before the compaction treatment, that is, when the active material layer 32 is laid on the surface of the current collector 31, the coating thickness of different regions can be set to be the same or different. For example, the average thickness H1 of the middle part 321 of the active material layer 32 can be set to be equal to or unequal to the average thickness H2 of the edge part 322, but after a special compaction treatment, the average thickness H1 of the middle part 321 of the active material layer 32 can be larger, while the average thickness H2 of the edge part 322 is smaller, thereby achieving the average compaction density of the portion 321 of the active material layer 32 laid on the middle part 311 of the current collector 31 is smaller, while the average compaction density of the portion 322 laid on the edge 312 of the current collector 31 is larger.

[0136] For another example, unlike FIG7 , the surface of the active material layer 32 away from the current collector 31 can also be substantially flush, and this can be achieved through different arrangements. Specifically, taking FIG8 as an example, the middle portion 311 of the current collector 31 is provided with a first groove 313 opening toward the active material layer 32, and the average thickness H21 of the bottom wall of the first groove 313 is less than the average thickness H22 of the edge 312 of the current collector 31. Specifically, the bottom wall of the first groove 313 corresponds to the middle portion 311 of the current collector 31. Through the first groove 313, different thicknesses of the active material layer 32 can be achieved. In the process of laying the active material layer 32 on the surface of the current collector 31, the surface of the active material layer 32 away from the current collector 31 can be set to be substantially flush. Due to the provision of the first groove 313, the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 is larger, while the average thickness H2 of the portion 322 laid on the edge 312 of the current collector 31 is smaller. Furthermore, during the compaction process, since the surface of the active material layer 32 away from the current collector 31 is substantially flush, no special compaction treatment is required for different regions. After the compaction process, the surface of the active material layer 32 away from the current collector 31 can still remain substantially flush, facilitating subsequent processing of the electrode sheet 3 and assembly into an electrode assembly. Furthermore, the provision of the first groove 313 also achieves a lower average compaction density for the portion 321 of the active material layer 32 located in the middle portion 311 of the current collector 31, while a higher average compaction density for the portion 322 located at the edge 312 of the current collector 31.

[0137] It should be understood that when the surface of the active material layer 32 away from the current collector 31 is basically flush, other methods can also be used to achieve that the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle 311 of the current collector 31 is greater than the average thickness H2 of the portion 322 laid on the edge 312 of the current collector 31.

[0138] It should be understood that the pole piece 3 in the embodiment of the present application further includes: a primer layer 33 disposed in at least a portion of the area between the current collector 31 and the active material layer 32. The primer layer 33 can be used to connect and secure the current collector 31 and the active material layer 32, and can also be used to increase the electrical conductivity of the pole piece 3. For example, the material of the primer layer 33 may include a binder and / or a conductive material. For another example, the primer layer 33 may include a conductive material. Taking lithium batteries as an example, commonly used conductive materials for lithium batteries may include traditional conductive agents such as conductive carbon black (SP), conductive graphite, and carbon fibers; or they may also include novel conductive agents such as carbon nanotubes, graphene, and mixed conductive pastes thereof. For another example, the primer layer 33 may include a binder. Still taking lithium batteries as an example, commonly used binders primarily include at least one of the following: polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR) emulsion, carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyacrylonitrile (PAN), and polyacrylate.

[0139] It should be understood that different thicknesses of different regions of the active material layer 32 can be achieved by different arrangements of the primer layer 33 and the current collector 31 .

[0140] In some embodiments, the primer layer 33 may be provided in a partial region between the current collector 31 and the active material layer 32 to achieve different thicknesses in different regions of the active material layer 32. For example, FIG9 and FIG10 respectively illustrate partial cross-sectional schematic diagrams of the pole piece 3 according to different embodiments of the present application. For example, FIG9 and FIG10 may be partial cross-sectional schematic diagrams of any pole piece 3 as shown in FIG4 to FIG6, wherein the cross section is perpendicular to the length direction X of the pole piece 3.

[0141] As shown in Figures 9 and 10, the middle part 311 of the current collector 31 is in direct contact with the active material layer 32, and a primer layer 33 is provided between the edge 312 of the current collector 31 and the active material layer 32, that is, there is no primer layer 33 between the middle part 311 of the current collector 31 and the corresponding middle part 321 of the active material layer 32, so that this part of the current collector 31 is in direct contact with the active material layer 32; and there is a primer layer 33 between the edge 312 of the current collector 31 and the corresponding edge part 322 of the active material layer 32, so that this part of the current collector 31 and the active material layer 32 are indirectly connected through the primer layer 33. In this way, regardless of whether the middle part 311 of the current collector 31 is provided with a first groove 313, since the edge 312 of the current collector 31 is provided with an additional primer layer 33 compared to the middle part 311, the average thickness H1 of the middle part 321 of the active material layer 32 is larger than the average thickness H2 of its edge part 322, thereby facilitating the realization of the average compaction density of the middle part 321 of the active material layer 32 being smaller than the average compaction density of the edge part 322.

[0142] For example, as shown in FIG9 , a local primer layer 33 may be further provided on the basis of the pole piece 3 shown in FIG8 , so as to achieve different thicknesses in different areas of the active material layer 32. Specifically, on the basis of providing the first groove 313 in the middle portion 311 of the current collector 31, no primer layer 33 may be provided in the middle portion 311 of the current collector 31, and a primer layer 33 may be provided on the edge 312 of the current collector 31. In this way, when the surface of the active material layer 32 away from the current collector 31 is substantially flush, the difference between the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 and the average thickness H2 of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 is equal to the sum of the depth of the first groove 313 in the middle portion 311 of the current collector 31 and the thickness of the primer layer 33 located at the edge 312 of the current collector 31. Therefore, by adjusting the depth of the first groove 313 in the middle part 311 of the current collector 31 and the thickness of the base coating 33 located at the edge 312 of the current collector 31, the difference between the average thickness H1 and the average thickness H2 can be adjusted, and then the difference between the average compaction density of the portion 321 of the active material layer 32 laid on the middle part 311 of the current collector 31 and the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 can also be adjusted.

[0143] For another example, as shown in FIG10 , different thicknesses can be achieved in different regions of the active material layer 32 by providing a primer layer 33 and not providing the primer layer 33, without providing the first groove 313 in the middle portion 311 of the current collector 31. Specifically, when the surface of the active material layer 32 away from the current collector 31 is substantially flush, the difference between the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 and the average thickness H2 of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 is equal to the thickness of the primer layer 33 located at the edge 312 of the current collector 31. Therefore, by adjusting the coating thickness of the primer layer 33, the difference between the average thickness H1 and the average thickness H2 can be directly adjusted, and then the difference between the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 and the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 can also be adjusted. The structure is simple and easy to implement.

[0144] In some embodiments, the primer layer 33 may also be provided in the entire region between the current collector 31 and the active material layer 32, and different thicknesses may also be achieved in different regions of the active material layer 32. For example, FIG11 and FIG12 respectively illustrate partial cross-sectional schematic diagrams of the pole piece 3 according to different embodiments of the present application. For example, FIG11 and FIG12 may be partial cross-sectional schematic diagrams of any pole piece 3 as shown in FIG4 to FIG6, wherein the cross section is perpendicular to the length direction X of the pole piece 3.

[0145] As shown in Figures 11 and 12, a primer layer 33 is provided throughout the area between the current collector 31 and the active material layer 32. Thus, the primer layer 33 can more effectively connect and secure the current collector 31 and the active material layer 32, and can also increase the conductivity of the electrode 3, thereby improving the stability and performance of the electrode 3.

[0146] In some embodiments, a portion 331 of the primer layer 33 corresponding to the middle portion 311 of the current collector 31 is provided with a second groove 333 opening toward the active material layer 32. Regardless of whether the middle portion 311 of the current collector 31 is provided with the first groove 313, the portion 331 of the primer layer 33 corresponding to the middle portion 311 of the current collector 31 may be provided with the second groove 333, and the middle portion 321 of the active material layer 32 is located within the second groove 333, so that the average thickness H1 of the middle portion 321 of the active material layer 32 is greater than the average thickness H2 of the edge portion 322 thereof, and further, the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 is less than the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31.

[0147] In some embodiments, the average thickness H31 of the bottom wall of the second groove 333 is less than the average thickness H32 of the portion 332 of the primer layer 33 corresponding to the edge 312 of the current collector 31. As shown in Figures 11 and 12, the bottom wall of the second groove 333 corresponds to the middle portion 311 of the current collector 31. In this way, regardless of whether the middle portion 311 of the current collector 31 is provided with the first groove 313, and regardless of whether the average thickness H31 of the bottom wall of the second groove 333 exceeds the depth of the first groove 313, the average thickness H1 of the middle portion 321 of the active material layer 32 can be greater than the average thickness H2 of its edge portion 322. Furthermore, the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 can be less than the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31. This structure is simple and easy to implement.

[0148] For example, taking Figure 11 as an example, if the middle part 311 of the current collector 31 is not provided with the first groove 313, then the surface of the bottom wall of the second groove 333 facing the current collector 31 is basically flush with the surface of the portion 332 of the base coating 33 corresponding to the edge 312 of the current collector 31 facing the current collector 31, and the average thickness H31 of the bottom wall of the second groove 333 is less than the average thickness H32 of the portion 332 of the base coating 33 corresponding to the edge 312 of the current collector 31. The structure is simple and easy to process.

[0149] For another example, taking FIG12 as an example, if the middle portion 311 of the current collector 31 is provided with a first groove 313, then the surface of the bottom wall of the second groove 333 facing the current collector 31 protrudes beyond the surface of the portion 332 of the primer layer 33 corresponding to the edge 312 of the current collector 31 facing the current collector 31. In this case, the average thickness H31 of the bottom wall of the second groove 333 may be less than, equal to, or greater than the depth of the first groove 313, and may also be less than, equal to, or greater than the average thickness H32 of the portion 332 of the primer layer 33 corresponding to the edge 312 of the current collector 31. In both cases, the average thickness H1 of the middle portion 321 of the active material layer 32 can be greater than the average thickness H2 of its edge portion 322. The embodiments of the present application are not limited to this.

[0150] In the embodiments of the present application, the above figures mainly take the example of a portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 having substantially the same thickness. Alternatively, the thickness of the portion 322 may also be set to a stepped thickness. Specifically, FIG13 shows a partial cross-sectional schematic diagram of a pole piece 3 of another embodiment of the present application. For example, FIG13 may be a possible partial cross-sectional schematic diagram of a pole piece 3 as shown in any of FIG4 to FIG6 , where the cross section is perpendicular to the length direction X of the pole piece 3.

[0151] As shown in FIG13 , the thickness of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 may be unequal at different locations. For example, the thickness of the edge portion 322 of the active material layer 32 may be gradually increased from the center portion 321 toward the direction away from the center portion 321, so that the corresponding compaction density gradually decreases, thereby reducing lithium plating and improving the performance and service life of the electrode assembly 22 and the battery cell 20. Specifically, the thickness difference can be achieved by different arrangements of the first groove 313 and / or the second groove 333. For example, a first groove 313 may be provided in the middle portion 311 of the current collector 31, while a primer layer 33 is not provided in the middle portion 311; in addition, a primer layer 33 is also not provided in the area close to the middle portion 311 of the edge 312 of the current collector 31, while a primer layer 33 is provided in the area away from the middle portion 311, so as to achieve that the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 is the largest, while the average thickness of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 is smaller, and in the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31: the average thickness H2' of the area close to the middle portion 311 is greater than the average thickness H2 of the area away from the middle portion 311.

[0152] It should be understood that the embodiments shown in Figures 7 to 13 above are described using the active material layer 32 on either side of the current collector 31 as an example. The active material layer 32 on the other side of the current collector 31 can be flexibly configured according to actual applications.

[0153] FIG14 shows a schematic cross-sectional view of a pole piece 3 according to another embodiment of the present application. For example, FIG14 may be a possible schematic cross-sectional view of any pole piece 3 as shown in FIG4 to FIG6 , and the cross section is perpendicular to the length direction X of the pole piece 3. As shown in FIG14 , one side of the current collector 31 is provided with an active material layer 32 having inconsistent compaction density according to an embodiment of the present application. For example, FIG14 takes the active material layer 32 shown in FIG8 as an example, but other embodiments as shown in FIG7 to FIG13 are applicable. However, an active material layer 32′ having consistent compaction density is provided on the other side of the current collector 31. For example, an active material layer 32′ having uniform thickness can be provided on the other side of the current collector 31 to simplify the structure and facilitate processing.

[0154] For another example, unlike the arrangement shown in FIG14 , active material layers 32 having inconsistent compaction densities according to the embodiment of the present application may be disposed on both sides of the current collector 31. Specifically, the pole piece 3 includes two active material layers 32, with the current collector 31 positioned between the two active material layers 32. The two active material layers 32 may be any of the active material layers 32 having inconsistent compaction densities described above, thereby simultaneously reducing lithium deposition on both sides of the pole piece 3 and further improving the performance of the electrode assembly 22 and the battery cell 20.

[0155] Figures 15 and 16 show two possible cross-sectional schematic diagrams of an electrode 3 including two active material layers 32 according to an embodiment of the present application. For example, Figures 15 and 16 may be possible cross-sectional schematic diagrams of any electrode 3 in Figures 4 to 6 , respectively, and the cross section is perpendicular to the length direction X of the electrode 3.

[0156] In some embodiments, active material layers 32 are provided on both sides of the current collector 31, and are provided in the same manner, so that the electrode 3 has a symmetrical structure relative to a plane perpendicular to the thickness direction Z, which facilitates processing and improves processing efficiency. For example, taking Figures 15 and 16 as examples, Figure 15 uses the current collector 31 and two active material layers 32 arranged in the manner shown in Figure 8 as an example, and Figure 16 uses the current collector 31, two primer layers 33, and two active material layers 32 arranged in the manner shown in Figure 10 as an example, but the embodiments of the present application are not limited to this.

[0157] Figure 17 shows another possible cross-sectional schematic diagram of the electrode 3 including two active material layers 32 in an embodiment of the present application. For example, Figure 17 may be a possible cross-sectional schematic diagram of any electrode 3 as shown in Figures 4 to 6 , and the cross-section is perpendicular to the length direction X of the electrode 3.

[0158] In some embodiments, active material layers 32 are respectively provided on both sides of the current collector 31, but the arrangement and / or the size of the arrangement may be different, so that the pole piece 3 is an asymmetric structure relative to the plane perpendicular to the thickness direction Z, the arrangement is more flexible, and the application is more extensive. For example, as shown in FIG17 , FIG17 takes the arrangement of the current collector 31, two layers of primer 33, and two layers of active material layer 32 as shown in FIG9 and FIG10 , respectively, as an example. For another example, the arrangement shown in any two other embodiments may also be adopted. For another example, the arrangement of the same embodiment may also be adopted, but the thickness of the corresponding areas of the two layers of active material layer 32 may be different, and the embodiments of the present application are not limited to this.

[0159] In some embodiments, the average thickness of the middle portion of the pole piece 3 is substantially equal to the average thickness of the edge of the pole piece 3. Specifically, as shown in Figures 14 to 16, the middle portion of the pole piece 3 is a region corresponding to the middle portion 311 of the current collector 31, and the edge of the pole piece 3 is a region corresponding to the edge 312 of the current collector 31. The average thickness of the middle portion of the pole piece 3 and the average thickness of the edge of the pole piece 3 are both equal to H0, so that both surfaces of the pole piece 3 are relatively flat, which is convenient for subsequent processing into the electrode assembly 22, so that the spacing between different pole piece layers in the electrode assembly 22 is relatively uniform, reducing the problem of lithium plating caused by large spacing differences, which can not only improve the space utilization and energy density of the battery cell 20, but also reduce lithium plating during the long-term charge and discharge cycle of the battery cell 20, thereby improving the cycle life and safety of the battery cell 20.

[0160] It should be understood that the thickness dimensions of different types of electrode sheets 3 in the embodiments of the present application can be flexibly set according to actual applications. For example, along the thickness direction Z of the electrode sheet 3, the ratio of the difference H1-H2 between the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 and the average thickness H2 of the portion 322 laid on the edge 312 of the current collector 31, to the average thickness H2 of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 is in the range of [1%, 3%].

[0161] If the ratio between the difference H1-H2 and the average thickness H2 is too small, the value of the difference H1-H2 of the pole piece 3 will be set too small, and the difference between the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 and the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 will also be too small, which may affect the performance of the pole piece 3 and fail to solve the lithium plating problem well. On the contrary, if the ratio between the difference H1-H2 and the average thickness H2 is too large, the value of the difference H1-H2 of the pole piece 3 is set too large, which will increase the difficulty of processing the pole piece 3, and may also affect the structural strength of the pole piece 3, thereby affecting the processing efficiency of the electrode assembly 22 and the battery cell 20.

[0162] For example, the ratio between the difference H1-H2 and the average thickness H2 can generally be set to 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8% or 3%.

[0163] In an embodiment of the present application, the difference between the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle 311 of the current collector 31 and the average thickness H2 of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 is equal to H1-H2. In different embodiments, the difference H1-H2 can be flexibly set.

[0164] For example, for the embodiment with uneven compaction density on one side as shown in FIG14 , for the active material layer 32 on the side with uneven compaction density, the value range of the difference H1 −H2 can be set according to actual application.

[0165] For example, if the electrode 3 is a positive electrode, the value range of the difference H1-H2 is generally set to [1 μm, 10 μm]. For example, the difference H1-H2 can be equal to 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm. For another example, if the electrode 3 is a negative electrode, the value range of the difference H1-H2 is generally set to [1 μm, 6 μm]. For example, the difference H1-H2 can be equal to 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, or 6 μm.

[0166] For another example, in the case where the compaction densities of the two active material layers 32 shown in Figures 15 to 17 are uneven, the range of the difference H1-H2 for each active material layer 32 can be set according to the actual application, and the difference H1-H2 of the two active material layers 32 can be equal or different. Here, any active material layer 32 is taken as an example.

[0167] For example, if the electrode 3 is a positive electrode, the value range of the difference H1-H2 is usually set to [1μm, 4μm]. For example, the difference H1-H2 can be equal to 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm or 4μm. For another example, if the electrode 3 is a negative electrode, the value range of the difference H1-H2 is usually set to [1μm, 3μm]. For example, the difference H1-H2 can be equal to 1μm, 1.5μm, 2μm, 2.5μm or 3μm. The difference H1-H2 of the active material layer 32 on one side of the electrode 3 should not be too large to meet the structural strength requirements of the electrode 3 and improve the structural stability of the electrode 3.

[0168] In some embodiments, the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 can be flexibly set according to actual applications; the average thickness H2 of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 can also be flexibly set according to actual applications. For the sake of brevity, they will not be described one by one here.

[0169] It should be understood that the average thickness H1 of the portion 321 of the active material layer 32 disposed on the middle portion 311 of the current collector 31 and the average thickness H2 of the portion 322 of the active material layer 32 disposed on the edge 312 of the current collector 31 in the embodiment of the present application may be related to various factors. For example, it may be related to the compaction density of the active material layer 32 or the mass of the material on the surface of the current collector 31.

[0170] In some embodiments, along the thickness direction Z of the electrode 3, the difference between the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 and the average thickness H2 of the portion 322 laid on the edge 312 of the current collector 31 is H, that is, the difference H is equal to H1-H2, the unit of H is μm, and the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 is Y, and the unit of Y is g / cm 3 , H and Y satisfy Y=KH, where the value range of K is [0.1, 0.4].

[0171] Taking into account that the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 has a certain range of values, therefore, if the proportional coefficient K is too large, the difference H will be too large. In this case, on the one hand, the average thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 may be too large, which will make the thickness of the pole piece 3 too large, thereby affecting the energy density of the battery cell 20 formed by the processing of the pole piece 3. On the other hand, the average thickness H2 of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 may be too small, which will cause the structural strength of the pole piece 3 to be weak, affecting the performance of the pole piece 3.

[0172] On the contrary, if the proportional coefficient K is too small, the difference H will be too small. For example, the difference H may approach zero, which will make the thickness H1 of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 and the thickness H2 of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 approximately equal. Correspondingly, the difference between the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 and the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 will also be too small, which may affect the performance of the electrode 3 and fail to solve the lithium plating problem well.

[0173] Therefore, the proportional coefficient K of the embodiment of the present application should not be too small or too low. For example, the proportional coefficient K can be specifically set to 0.1, 0.15, 0.2, 0.25, 0.3, 0.35 or 0.4 to improve the performance of the electrode 3 and effectively solve the problem of lithium deposition.

[0174] In some embodiments, the average compaction density of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 is Y, where the unit of Y is g / cm 3 The total coating mass of the material laid on the surface of the current collector 31 facing the active material layer 32 is M, and the unit of M is g / 1540.25mm 2 , Y and M satisfy Y=NM, and the value range of N is [1, 7]. Among them, the material laid on the surface of the current collector 31 facing the active material layer 32 includes the active material layer 32 and the primer layer 33 laid on one side of the current collector 31, and the mass of the primer layer 33 may be zero. That is, if there is no primer layer 33 between the current collector 31 and the active material layer 32, the total coating mass of the material laid on the surface of the current collector 31 facing the active material layer 32 includes the total mass of the active material layer 32 coated on one side of the current collector 31; if there is a primer layer 33 between the current collector 31 and the active material layer 32, the total coating mass of the material laid on the surface of the current collector 31 facing the active material layer 32 includes the sum of the total mass of the active material layer 32 coated on one side of the current collector 31 and the total mass of the primer layer 33 coated between the current collector 31 and the active material layer 32.

[0175] It should be understood that, when the total coating mass M of the material laid on the surface of the current collector 31 facing the active material layer 32 is constant, if the proportional coefficient N is too large, the average compaction density Y of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 will be too large. Correspondingly, the average compaction density of the portion 322 of the active material layer 32 laid on the edge 312 of the current collector 31 will be even greater, which will increase the difficulty of processing the electrode sheet 3 and increase the processing cost of the electrode sheet 3. Conversely, if the proportional coefficient N is too small, the average compaction density Y of the portion 321 of the active material layer 32 laid on the middle portion 311 of the current collector 31 will be too small, which will not meet the design requirements of the electrode sheet 3, will reduce the performance of the electrode sheet 3, and further reduce the performance of the electrode assembly 22 formed by the electrode sheet 3.

[0176] Therefore, the value of the proportional coefficient N should not be too large or too small. For example, the proportional coefficient N can be specifically set to 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5 or 7 to improve the performance of the pole piece 3.

[0177] In the embodiment of the present application, the total coating mass M of the material laid on the surface of the current collector 31 facing the active material layer 32 can be set according to the actual application. For example, if the electrode 3 is a positive electrode, the value range of the total coating mass M can be set to [0.2g / 1540.25mm 2, 0.4g / 1540.25mm 2 ] Specifically, the total coating mass M can be set to 0.2g / 1540.25mm 2 、0.23g / 1540.25mm 2 , 0.25g / 1540.25mm 2 、0.28g / 1540.25mm 2 、0.3g / 1540.25mm 2 、0.33g / 1540.25mm 2 , 0.35g / 1540.25mm 2 、0.38g / 1540.25mm 2 or 0.4g / 1540.25mm 2 For another example, if the electrode 3 is a negative electrode, the value range of the total coating mass M can be set to [0.1g / 1540.25mm 2 , 0.2g / 1540.25mm 2 ] Specifically, the total coating mass M can be set to 0.1g / 1540.25mm 2 、0.11g / 1540.25mm 2 , 0.12g / 1540.25mm 2 、0.13g / 1540.25mm 2 、0.14g / 1540.25mm 2 、0.15g / 1540.25mm 2 、0.16g / 1540.25mm 2 、0.17g / 1540.25mm 2 、0.18g / 1540.25mm 2 、0.19g / 1540.25mm 2 or 0.2g / 1540.25mm 2 .

[0178] In the embodiment of the present application, the average compaction density of the portion 321 of the active material layer 32 of the pole piece 3, which is laid on the middle portion 311 of the current collector 31, is less than the average compaction density of the portion 322 laid on the edge 312 of the current collector 31. That is, the porosity of the portion 321 of the active material layer 32 located in the middle is greater than the porosity of the portion 322 located at the edge. In this way, the central area of ​​the pole piece 3 can accommodate more electrolyte, which can effectively solve the problem of lithium deposition caused by the electrolyte being easily squeezed out of the central area. That is, it can effectively reduce the lithium deposition phenomenon, thereby improving the performance and cycle life of the battery cell 20.

[0179] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and components may be substituted with equivalents without departing from the scope of the present application. In particular, the various technical features described in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but encompasses all technical solutions within the scope of the claims.

Claims

1. A pole piece, characterized in that: include: Current collector(31); An active material layer (32) is laid on the surface of the current collector (31); The average compaction density of a portion (321) of the active material layer (32) laid on the middle portion (311) of the current collector (31) is smaller than the average compaction density of a portion (322) laid on the edge (312) of the current collector (31).

2. The pole piece according to claim 1, characterized in that: The average thickness of a portion (321) of the active material layer (32) laid on the middle portion (311) of the current collector (31) is greater than the average thickness of a portion (322) laid on the edge (312) of the current collector (31).

3. The pole piece according to claim 1 or 2, characterized in that: The middle part (311) of the current collector (31) is provided with a first groove (313) opening toward the active material layer (32), and the average thickness of the bottom wall of the first groove (313) is smaller than the average thickness of the edge (312) of the current collector (31).

4. The pole piece according to any one of claims 1 to 3, characterized in that: The pole piece further comprises: a base coating layer (33) disposed in at least a portion of the region between the current collector (31) and the active material layer (32).

5. The pole piece according to claim 4, characterized in that: The middle part (311) of the current collector (31) is in direct contact with the active material layer (32), and the primer layer (33) is provided between the edge (312) of the current collector (31) and the active material layer (32).

6. The pole piece according to claim 4, characterized in that: The primer layer (33) is disposed in the entire region between the current collector (31) and the active material layer (32).

7. The pole piece according to claim 6, characterized in that: A portion (331) of the primer layer (33) corresponding to the middle portion (311) of the current collector (31) is provided with a second groove (333) opening toward the active material layer (32).

8. The pole piece according to claim 7, characterized in that: The average thickness of the bottom wall of the second groove (333) is smaller than the average thickness of the portion (332) of the primer layer (33) corresponding to the edge (312) of the current collector (31).

9. The pole piece according to any one of claims 1 to 8, characterized in that: The edge (312) of the current collector (31) includes a first portion (3121) and a second portion (3122), wherein the first portion (3121) is located at one end of the current collector (31) in the width direction of the pole piece, and the second portion (3122) is located at the other end of the current collector (31) in the width direction of the pole piece, and the middle portion (311) of the current collector (31) is located between the first portion (3121) and the second portion (3122).

10. The pole piece according to claim 9, characterized in that: The edge (312) of the current collector (31) comprises a third portion (3123) and a fourth portion (3124), wherein the third portion (3123) is located at one end of the current collector (31) in the length direction of the pole piece; the fourth portion (3124) is located at the other end of the current collector (31) in the length direction of the pole piece, and the middle portion (311) of the current collector (31) is located between the third portion (3123) and the fourth portion (3124).

11. The pole piece according to claim 9 or 10, characterized in that: Along the width direction of the pole piece, the ratio of the average width of the middle portion (311) of the current collector (31) to the average width of the pole piece is in the range of [1 / 3, 2 / 3].

12. The pole piece according to claim 11, characterized in that: Along the width direction of the pole piece, the ratio of the average width of the middle portion (311) of the current collector (31) to the average width of the pole piece is in the range of [40%, 60%].

13. The pole piece according to any one of claims 1 to 12, characterized in that: Along the thickness direction of the electrode sheet, the difference between the average thickness of a portion (321) of the active material layer (32) laid on the middle portion (311) of the current collector (31) and the average thickness of a portion (322) laid on the edge (312) of the current collector (31) and the ratio of the average thickness of the portion (322) of the active material layer (32) laid on the edge (312) of the current collector (31) is in the range of [1%, 3%].

14. The pole piece according to any one of claims 1 to 13, characterized in that: Along the thickness direction of the electrode sheet, the difference between the average thickness of the portion (321) of the active material layer (32) laid on the middle portion (311) of the current collector (31) and the average thickness of the portion (322) laid on the edge (312) of the current collector (31) is H, and the unit of H is μm. The average compaction density of the portion (321) of the active material layer (32) laid on the middle portion (311) of the current collector (31) is Y, and the unit of Y is g / cm 3 , H and Y satisfy Y=KH, where the value range of K is [0.1, 0.4].

15. The pole piece according to any one of claims 1 to 14, characterized in that: The average compaction density of the portion (321) of the active material layer (32) laid on the middle portion (311) of the current collector (31) is Y, and the unit of Y is g / cm 3 The total coating mass of the material laid on the surface of the current collector (31) facing the active material layer (32) is M, and the unit of M is g / 1540.25 mm 2 , Y and M satisfy Y=NM, where the value range of N is [1, 7].

16. The pole piece according to any one of claims 1 to 15, characterized in that: The average thickness of the middle portion of the pole piece is substantially equal to the average thickness of the edge of the pole piece.

17. The pole piece according to any one of claims 1 to 16, characterized in that: The pole piece comprises two layers of active material layers (32), and the current collector (31) is located between the two layers of active material layers (32).

18. An electrode assembly, characterized in that: include: A positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet and / or the negative electrode sheet comprises a sheet as claimed in any one of claims 1 to 17.

19. The electrode assembly according to claim 18, characterized in that The positive electrode sheet and the negative electrode sheet are wound to form the electrode assembly.

20. The electrode assembly according to claim 19, characterized in that The electrode assembly is a cylinder.

21. A battery cell, characterized in that: include: An electrode assembly as claimed in any one of claims 18 to 20.

22. A battery, characterized in that: include: A plurality of battery cells, wherein the battery cells are the battery cells as claimed in claim 21.

23. An electrical equipment, characterized in that: include: The battery as claimed in claim 22, wherein the battery is used to provide electrical energy.

Citation Information

Patent Citations

  • Pole piece, battery cell and battery

    CN111540910A

  • Pole piece and lithium ion battery

    CN116093247A

  • Pole piece, battery monomer, battery and electric device

    CN217606853U

  • Battery

    JP2001015146A

  • Lithium ion secondary battery and manufacturing method of the same

    JP2005038612A

Cited By

  • Battery pole piece, winding battery and electric equipment

    CN119833527A