Separator, preparation method for separator, and electrochemical device

By setting the base film and gel film on both sides of the adhesive layer of the isolation film, an integral structure is formed, which solves the problem of the lithium battery isolation film being prone to rupture in the vertical direction, improves the stability and safety of the battery, and extends the Battery lifespan.

WO2024244425A1PCT designated stage expired Publication Date: 2024-12-05CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/140738
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2023-12-21
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The isolation film of lithium batteries is easily cracked by the pressure of lithium dendrites in the vertical direction, resulting in short-circuiting of the cathode and anode and short-circuiting of the battery. The prior art is difficult to effectively solve this problem.

Method used

Design an isolation film, including an adhesive layer, a base film and a gel film disposed on both sides of the adhesive layer, and a base film and gel film are bonded into a whole by providing a base film and gel film on both sides of the adhesive layer. Enhance the deformation and puncture resistance of the isolation film and delay the rupture time.

Benefits of technology

It improves the puncture resistance of the isolation film and the stability and safety of the battery, extends the service life of the battery, and reduces the risk of positive and negative electrode shorting caused by heat shrinkage of the isolation film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023140738-FTAPPB-I100001
    Figure PCTCN2023140738-FTAPPB-I100001
  • Figure PCTCN2023140738-FTAPPB-I100002
    Figure PCTCN2023140738-FTAPPB-I100002
Patent Text Reader

Abstract

Disclosed in the present application are a separator, a preparation method for a separator, and an electrochemical device. The separator comprises a bonding layer, and a base film and a gel film which are respectively arranged on two sides of the bonding layer. In the present application, the gel film has relatively good ductility and deformation resistance, is not prone to being pierced or still completely covers a pierced position after being pierced, such that the separator still plays a role in separating positive and negative electrodes; and the base film has relatively good shape-retaining capability and self-supporting performance. The base film and the gel film are respectively provided on the two sides of the bonding layer, such that the gel film and the base film are bonded into a whole under the bonding action of the bonding layer, and thus when there is an external force acting in the vertical direction of the separator, the separator deforms but is not prone to breaking, thereby delaying the breakage of the separator, and improving the stability and safety of a battery.
Need to check novelty before this filing date? Find Prior Art

Description

Isolation membrane, method for preparing isolation membrane, and electrochemical device

[0001] Citation of Related Applications

[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on May 26, 2023, with application number 202310609508.0 and invention name “Isolation membrane, method for preparing isolation membrane and electrochemical device”, the entire contents of which are incorporated by reference into the application. Technical Field

[0003] The present application relates to the field of battery technology, and in particular to an isolation membrane, a method for preparing the isolation membrane, and an electrochemical device. Background Art

[0004] The separator of lithium batteries is mostly made of polyolefin separator, which has a low degree of physical deformation in the direction perpendicular to the membrane surface and is easy to rupture under certain external forces in the vertical direction. However, during the use of the battery, the accumulation of lithium dendrites will cause a series of physical damage to the separator in the vertical direction, causing a short circuit between the anode and cathode and a battery short circuit.

[0005] Summary of the Invention

[0006] The present application is made in view of the above-mentioned problems, and its purpose is to provide an isolation membrane to improve the puncture resistance of the isolation membrane, reduce the physical damage of the isolation membrane, and improve the stability of the battery.

[0007] In order to achieve the above objectives, embodiments of the present application provide an isolation membrane, a method for preparing the isolation membrane, and an electrochemical device.

[0008] In a first aspect, an embodiment of the present application provides an isolation film, comprising an adhesive layer and a base film and a gel film respectively disposed on both sides of the adhesive layer.

[0009] Therefore, in the technical solution of the embodiment of the present application, the gel film has good ductility and deformation resistance, is not easy to be punctured, or after being punctured, it still completely covers the punctured area, so that the isolation membrane still plays the role of isolating the positive and negative electrodes; the base film has good shape retention ability and self-supporting performance; by arranging the base film and the gel film on both sides of the adhesive layer respectively, the gel film and the base film are bonded into a whole under the bonding action of the adhesive layer, so that when an external force is applied in the vertical direction of the isolation membrane, the isolation membrane is deformed but not easy to rupture, thereby delaying the rupture time of the isolation membrane and improving the stability and safety of the battery.

[0010] In any embodiment, the thickness of the bonding layer is δ1, wherein 0.5 μm ≤ δ1 ≤ 6 μm, optionally, 0.5 μm ≤ δ1 ≤ 3 μm, the thickness of the bonding layer affects the energy density of the battery core and thus affects the service life of the battery core, and also affects the heat resistance of the separator. When the thickness of the bonding layer is less than 0.5 μm, the heat resistance of the separator is reduced. When the thickness of the bonding layer is greater than 6 μm, the energy density of the battery core is reduced, affecting the service life of the battery core; and / or,

[0011] The thickness of the base film is δ2, wherein 3μm≤δ2≤12μm, optionally, 3μm≤δ2≤8μm. The thickness of the base film affects the energy density of the battery cell and the shape retention performance of the isolation membrane. When the thickness of the base film is less than 3μm, the base film is too thin, the thickness of the isolation membrane is too thin, and the shape retention ability of the isolation membrane is reduced. When the thickness of the base film is greater than 12μm, the base film is too thick, which reduces the energy density of the battery cell and thus reduces the service life of the battery cell; and / or,

[0012] The thickness of the gel film is δ3, wherein 1μm≤δ3≤12μm, optionally, 1μm≤δ3≤8μm. The thickness of the gel film affects the energy density of the battery cell and the puncture resistance of the isolation membrane. When the thickness of the gel film is less than 1μm, the gel film is too thin, and the thickness of the isolation membrane is too thin, which reduces the puncture resistance of the isolation membrane. When the thickness of the gel film is greater than 12μm, the gel film is too thick, which reduces the energy density of the battery cell and thereby reduces the service life of the battery cell.

[0013] In any embodiment, the material of the base film includes but is not limited to at least one of polyolefin, polyether, polyetherketone, polyimide, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymer and copolymer containing CF bond, and the base film made of the above materials can provide better shape retention ability; and / or,

[0014] The material of the gel film includes but is not limited to at least one of polyurethane and polyurethane. The gel film made of the above materials can provide better deformation ability.

[0015] In any embodiment, the bonding layer includes inorganic particles and a binder. The inorganic particles and the binder can provide good shape retention and bonding capabilities.

[0016] In any embodiment, the inorganic particles include but are not limited to any one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, yttrium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate and magnesium fluoride. The use of the above inorganic particles can improve the barrier effect and shape retention ability; and / or,

[0017] The binder includes but is not limited to at least one of acrylate, acrylic acid and carboxymethyl cellulose. Adopting the above binder can improve the bonding performance.

[0018] In any embodiment, the mass proportion of the inorganic particles in the bonding layer is 30% to 50%; optionally, the mass proportion of the inorganic particles in the bonding layer is 35% to 45%. The mass proportion of the inorganic particles in the bonding layer affects the ion transmission capacity and the heat resistance of the isolation membrane. When the mass proportion of the inorganic particles in the bonding layer is less than 30%, the bonding layer is too thin and the heat resistance is reduced, thereby affecting the cycle performance of the battery cell. When the mass proportion of the inorganic particles in the bonding layer is greater than 50%, the ion transmission capacity is reduced, thereby affecting the cycle performance of the battery cell.

[0019] In any embodiment, the mass proportion of the adhesive in the adhesive layer is 10-20%; optionally, the mass proportion of the adhesive in the adhesive layer is 13-18%. The mass proportion of the adhesive in the adhesive layer affects the bonding performance. When the mass proportion of the adhesive in the adhesive layer is less than 10%, the bonding force is insufficient. When the mass proportion of the adhesive in the adhesive layer is greater than 20%, the bonding force is too large and the coating is uneven.

[0020] In any embodiment, the average particle size of the inorganic particles is 0.1 to 10 nm; optionally, the average particle size of the inorganic particles is 0.2 to 0.8 nm. The average particle size of the inorganic particles affects the coating performance. When the average particle size of the inorganic particles is less than 0.1 nm, it is easy to clog the pores and reduce the ion transmission capacity. When the average particle size of the inorganic particles is greater than 10 nm, it is easy to disperse unevenly, affecting the heat resistance.

[0021] In any embodiment, the specific surface area of ​​the inorganic particles is 5 to 15 g / m 2 Optionally, the specific surface area of ​​the inorganic particles is 6 to 9 g / m 2 The specific surface area of ​​inorganic particles affects the surface tension. When the specific surface area of ​​inorganic particles is less than 5g / m 2 When the surface tension is insufficient, the bonding is not strong. When the specific surface area of ​​the inorganic particles is greater than 15g / m 2 When the surface tension is too large, it is difficult to apply evenly during coating.

[0022] In any embodiment, the air permeability of the separator is 300-500 s / 100 cc; optionally, the air permeability of the separator is 400-450 s / 100 cc. The air permeability of the separator affects the porosity of the separator, thereby affecting the ion transmission capacity and puncture resistance of the separator. When the air permeability of the separator is less than 300 s / 100 cc, the ion transmission capacity is weakened. When the air permeability of the separator is greater than 500 s / 100 cc, the puncture resistance of the separator is reduced.

[0023] In any embodiment, the porosity of the separator is 25% to 65%, and optionally, the porosity of the separator is 40% to 50%. Maintaining a certain porosity of the separator can improve the separator's deformation resistance and puncture resistance, and at the same time improve the ion transmission capacity. When the separator's porosity is less than 25%, the ion transmission capacity is reduced. When the separator's porosity is greater than 65%, the separator's puncture resistance is reduced.

[0024] In any embodiment, the porosity of the base membrane is 30% to 70%. Optionally, the porosity of the base membrane is 50% to 60%. Maintaining a certain porosity of the base membrane can improve the ion transmission capacity and puncture resistance of the isolation membrane, and at the same time improve the ion transmission capacity. When the porosity of the base membrane is less than 30%, the ion transmission capacity is weak. When the porosity of the base membrane is greater than 70%, the puncture resistance of the isolation membrane decreases; and / or,

[0025] The porosity of the gel membrane is 40% to 80%. Optionally, the porosity of the gel membrane is 50% to 60%. Maintaining a certain porosity of the gel membrane can improve the ion transmission ability and puncture resistance of the isolation membrane, and at the same time improve the ion transmission ability. When the porosity of the gel membrane is less than 40%, the ion transmission ability will be reduced. When the porosity of the gel membrane is greater than 80%, the puncture resistance of the isolation membrane decreases.

[0026] In any embodiment, the pores of the base membrane have a pore size of 100 to 800 nm; optionally, the pores of the base membrane have a pore size of 200 to 600 nm. The pore size of the base membrane affects the puncture resistance and ion transmission capacity of the isolation membrane, and can also improve the ion transmission capacity. When the pore size of the base membrane is less than 100 nm, the ion transmission capacity is reduced. When the pore size of the base membrane is greater than 800 nm, the puncture resistance of the isolation membrane decreases; and / or,

[0027] The pore size of the gel membrane is 200 to 1000 nm; optionally, the pore size of the gel membrane is 200 to 600 nm. The pore size of the gel membrane affects the ion transmission capacity and puncture resistance of the isolation membrane. When the pore size of the gel membrane is less than 200 nm, the ion transmission capacity will be reduced. When the pore size of the gel membrane is greater than 1000 nm, the puncture resistance of the isolation membrane will decrease.

[0028] In any embodiment, the surface density of the base film is 2 to 10 g / m 2 Optionally, the surface density of the base film is 3 to 8 g / m 2 The surface density of the base film affects the shape retention and ion transmission ability of the isolation membrane. When the surface density of the base film is less than 2g / m 2 When the surface density of the base film is greater than 10g / m 2 When the ion transmission capacity is reduced; and / or,

[0029] The surface density of the gel film is 2 to 10 g / m 2 Optionally, the surface density of the gel film is 4 to 8 g / m 2 The surface density of the gel film affects the puncture resistance and ion transmission capacity of the isolation membrane. When the surface density of the gel film is less than 2g / m 2 When the surface density of the gel film is greater than 10g / m 2 When the ion transport capacity is reduced, the cycle performance of the battery cell will be affected; and / or,

[0030] The specific surface area of ​​the bonding layer is 1.0 to 6.0 g / m 2 Optionally, the specific surface area of ​​the adhesive layer is 2.0 to 4.0 g / m 2 The specific surface area of ​​the bonding layer affects the surface tension. When the specific surface area of ​​the bonding layer is less than 2g / m 2 When the surface tension is insufficient, the bonding is not strong. When the specific surface area of ​​the bonding layer is greater than 10g / m 2 When the surface tension is too large, it is difficult to apply evenly during coating.

[0031] In any embodiment, the heat shrinkage rate of the separator is less than 2%, and optionally, the heat shrinkage rate of the separator is less than 1%. By limiting the heat shrinkage rate of the separator, the separator's ability to retain its shape is improved, reducing the possibility of shorting the positive and negative electrodes and battery short circuits caused by the separator's heat shrinkage.

[0032] In any embodiment, the tensile deformation rate of the isolation membrane is greater than 400%, and optionally, the tensile deformation rate of the isolation membrane is greater than 600%. By limiting the tensile deformation rate of the isolation membrane, the isolation membrane's deformation resistance is improved, the probability of isolation membrane damage is reduced, and the time of isolation membrane damage is delayed.

[0033] In any embodiment, the puncture resistance of the separator is ≥350 gf. Optionally, the puncture resistance of the separator is ≥500 gf. By limiting the puncture resistance of the separator, the time for the separator to rupture is delayed, thereby improving the safety and stability of the battery.

[0034] In any embodiment, the transverse tensile strength of the separator is greater than 1000 kg / cm 2 The transverse tensile properties of the separator affect its deformation resistance. The transverse tensile strength of the separator is greater than 1000kg / cm 2 can provide better deformation ability; and / or,

[0035] The longitudinal tensile strength of the isolation film is greater than 1200 kg / cm 2 The longitudinal tensile strength of the isolation membrane affects the isolation membrane's ability to resist deformation. The longitudinal tensile strength of the isolation membrane is greater than 1200kg / cm 2 It can provide better deformation ability.

[0036] In a second aspect, an embodiment of the present application provides a method for preparing an isolation film, which is used to prepare the isolation film of the first aspect of the present application, comprising the following steps:

[0037] providing a base film,

[0038] An adhesive layer is arranged on one side of the base film, and a gel film is arranged on the side of the adhesive layer facing away from the base film to obtain an isolation film.

[0039] By setting an adhesive layer on one side of the base film and setting a gel film on the side of the adhesive layer away from the base film, the stable shape of the base film provides support for the adhesive layer, and the adhesive film bonds the base film and the gel film into a whole to obtain an isolation film.

[0040] In any embodiment, the step of providing a base film comprises:

[0041] The base film is prepared by melt extrusion and heat stretching. The base film prepared by melt extrusion and heat stretching has good shape retention ability.

[0042] In any embodiment, the steps of providing an adhesive layer on one side of the base film and providing a gel film on the side of the adhesive layer facing away from the base film to obtain the isolation film include:

[0043] preparing a bonding layer slurry, and coating the bonding layer slurry on one side of the base film to obtain a base film containing a bonding layer;

[0044] A gel film is arranged on the side of the adhesive layer of the base film containing the adhesive layer facing away from the base film, and the film is dried and pressed to obtain an isolation film.

[0045] Wherein, the bonding layer slurry includes inorganic particles, a binder and a solvent. By configuring the bonding layer slurry and coating the bonding layer slurry on one side of the base film, a base film containing a bonding layer is obtained, which can make the bonding layer slurry evenly dispersed on the base film, providing uniform bonding ability. By containing inorganic particles, a binder and a solvent, the inorganic particles and the binder are dispersed in the solvent, which is convenient for coating. In some embodiments of the present invention, the solvent includes water. And / or,

[0046] The drying temperature is 30-40°C; optionally, the drying temperature is 33-37°C. The drying temperature affects the adhesion performance of the base film and the gel film to the adhesive layer. When the drying temperature is less than or equal to 30°C, the adhesion is not strong. When the drying temperature is less than or equal to 40°C, the adhesion temperature is too high and the adhesion is uneven. And / or,

[0047] The drying time is 1 to 10 seconds; optionally, the drying time is 3 to 7 seconds. The drying time affects the adhesion performance of the base film and the gel film to the adhesive layer. If the drying time is less than 1 second, the adhesion is not tight enough. If the drying time is greater than 10 seconds, the adhesion is not tight enough. And / or,

[0048] The pressing pressure is 5 to 20 N; optionally, the pressing pressure is 8 to 15 N. The pressing pressure affects the adhesion performance of the base film and the gel film to the adhesive layer. When the pressing pressure is less than 5 N, the adhesion of the base film and the gel film to the adhesive layer is not tight enough. When the pressing pressure is greater than 20 N, the isolation film will be compressed, increasing the probability of inorganic particles damaging the isolation film.

[0049] In a third aspect, an embodiment of the present application provides an electrochemical device comprising the isolation membrane of the first aspect of the present application.

[0050] In any embodiment, the electrochemical device comprises a capacitor, a primary battery, or a secondary battery. DETAILED DESCRIPTION

[0051] The following specifically discloses the embodiments of the isolation film, the method for preparing the isolation film, the solar power generation device, and the power-consuming device of the present application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0052] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0053] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0054] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0055] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0056] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0057] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0058] An isolation membrane is usually set between the positive and negative electrodes of the battery to reduce the short circuit between the positive and negative electrodes and reduce the probability of battery short circuit. Therefore, the isolation membrane needs to have a certain shape retention ability. Usually, the isolation membrane with shape retention ability has the problem of poor puncture resistance in the direction perpendicular to the isolation membrane. During the use of the battery, the accumulation of lithium dendrites will compress the isolation membrane in the vertical direction and puncture the isolation membrane, increasing the risk of short circuit between the positive and negative electrodes.

[0059] Therefore, research on the short circuit between the positive and negative electrodes caused by separator damage is constantly emerging. For example, a microporous polyolefin lithium battery separator includes: a laminated, dry-process prepared, microporous multi-layer separator, which includes at least two outer layers and at least one inner layer, each of the outer layers comprising polyethylene, polyethylene blends, polyethylene copolymers, or mixtures thereof, and the inner layer comprising polypropylene, polypropylene blends, polypropylene copolymers, or mixtures thereof. PP / PE is hot-pressed into various structures, which can slightly improve the heat resistance and strength of the separator. However, the thickness is increased too much, and the air permeability of the separator after hot-pressing is severely reduced, the pore structure is blocked, affecting the energy density of the battery and hindering the transfer of Li+ in the battery.

[0060] Surprisingly, by configuring the isolation membrane to include an adhesive layer and a base membrane and a gel membrane disposed on both sides of the adhesive layer, the stability of the isolation membrane is maintained while improving ion transmission, thereby improving the puncture resistance of the isolation membrane.

[0061] Based on this, the present application provides an isolation membrane, a method for preparing the isolation membrane, a positive electrode sheet, a method for preparing the positive electrode sheet, and an electrochemical device.

[0062] In a first aspect, an embodiment of the present application provides an isolation film, comprising an adhesive layer and a base film and a gel film respectively disposed on both sides of the adhesive layer.

[0063] Therefore, in the technical solution of the embodiment of the present application, the gel film has good ductility and deformation resistance, is not easy to be punctured, or after being punctured, it still completely covers the punctured area, so that the isolation membrane still plays the role of isolating the positive and negative electrodes; the base film has good shape retention ability and self-supporting performance; by arranging the base film and the gel film on both sides of the adhesive layer respectively, the gel film and the base film are bonded into a whole under the bonding action of the adhesive layer, so that when an external force acts in the vertical direction of the isolation membrane, the isolation membrane is deformed but not easy to rupture, thereby delaying the rupture time of the isolation membrane and improving the stability and safety of the battery.

[0064] In any embodiment, the heat shrinkage rate of the separator is less than 2%, and optionally, the heat shrinkage rate of the separator is less than 1%. By limiting the heat shrinkage rate of the separator, the separator's ability to retain its shape is improved, reducing the possibility of shorting the positive and negative electrodes and battery short circuits caused by the separator's heat shrinkage.

[0065] In any embodiment, the tensile deformation rate of the isolation membrane is greater than 400%, and optionally, the tensile deformation rate of the isolation membrane is greater than 600%. By limiting the tensile deformation rate of the isolation membrane, the isolation membrane's deformation resistance is improved, the probability of isolation membrane damage is reduced, and the time of isolation membrane damage is delayed.

[0066] In any embodiment, the puncture resistance of the separator is ≥350 gf. Optionally, the puncture resistance of the separator is ≥500 gf. By limiting the puncture resistance of the separator, the time for the separator to rupture is delayed, thereby improving the safety and stability of the battery.

[0067] In any embodiment, the transverse tensile strength of the separator is greater than 1000 kg / cm 2 The transverse tensile properties of the separator affect its deformation resistance. The transverse tensile strength of the separator is greater than 1000kg / cm 2 can provide better deformation ability; and / or,

[0068] The longitudinal tensile strength of the isolation film is greater than 1200 kg / cm 2 The longitudinal tensile strength of the isolation membrane affects the isolation membrane's ability to resist deformation. The longitudinal tensile strength of the isolation membrane is greater than 1200kg / cm 2 It can provide better deformation ability.

[0069] In any embodiment, the thickness of the bonding layer is δ1, wherein 0.5μm≤δ1≤6μm, and the thickness δ1 of the bonding layer can be 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, or 5.5μm. Optionally, 0.5μm≤δ1≤3μm, and the thickness of the bonding layer affects the energy density of the battery cell and thus affects the service life of the battery cell, and also affects the heat resistance of the isolation membrane. When the thickness of the bonding layer is less than 0.5μm, the heat resistance of the isolation membrane will be reduced. When the thickness of the bonding layer is greater than 6μm, the energy density of the battery cell will be reduced, affecting the service life of the battery cell; and / or,

[0070] The thickness of the base film is δ2, wherein 3μm≤δ2≤12μm, and the thickness δ2 of the base film can be 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm, 10μm, 10.5μm, 11μm, 11.5μm, or 12μm. Optionally, 3μm≤δ2≤8μm, and the thickness of the base film affects the energy density of the battery cell and the shape retention performance of the isolation membrane. When the thickness of the base film is less than 3μm, the base film is too thin, and the thickness of the isolation membrane is too thin, which reduces the shape retention ability of the isolation membrane. When the thickness of the base film is greater than 12μm, the base film is too thick, which reduces the energy density of the battery cell and thus reduces the service life of the battery cell; and / or,

[0071] The thickness of the gel film is δ3, wherein 1μm≤δ3≤12μm. The thickness δ3 of the gel film can be 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm, 10μm, 10.5μm, 11μm, 11.5μm, or 12μm. Optionally, 1μm≤δ3≤8μm. The thickness of the gel film affects the energy density of the battery cell and the puncture resistance of the separator. When the thickness of the gel film is less than 1μm, the gel film is too thin, the separator thickness is too thin, and the puncture resistance of the separator is reduced. When the thickness of the gel film is greater than 12μm, the gel film is too thick, which reduces the energy density of the battery cell and thus reduces the service life of the battery cell.

[0072] In any embodiment, the material of the base film includes but is not limited to at least one of polyolefin, polyether, polyetherketone, polyimide, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymer and copolymer containing CF bond, and the base film made of the above materials can provide better shape retention ability; and / or,

[0073] The material of the gel film includes but is not limited to at least one of polyurethane and polyurethane. The gel film made of the above materials can provide better deformation ability.

[0074] In any embodiment, the bonding layer includes inorganic particles and a binder. The inorganic particles and the binder can provide good shape retention and bonding capabilities.

[0075] In any embodiment, the inorganic particles include but are not limited to any one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, yttrium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate and magnesium fluoride. The use of the above inorganic particles can improve the barrier effect and shape retention ability; and / or,

[0076] The binder includes but is not limited to at least one of acrylate, acrylic acid and carboxymethyl cellulose. Adopting the above binder can improve the bonding performance.

[0077] In any embodiment, the mass proportion of the inorganic particles in the bonding layer is 30% to 50%, and the mass proportion of the inorganic particles in the bonding layer can be 30%, 33%, 35%, 38%, 40%, 42%, 45%, 47%, or 50%; optionally, the mass proportion of the inorganic particles in the bonding layer is 35% to 45%, and the mass proportion of the inorganic particles in the bonding layer affects the ion transmission capacity and the heat resistance of the isolation membrane. When the mass proportion of the inorganic particles in the bonding layer is less than 30%, the bonding layer is too thin and the heat resistance is reduced, thereby affecting the cycle performance of the battery cell. When the mass proportion of the inorganic particles in the bonding layer is greater than 50%, the ion transmission capacity is reduced, thereby affecting the cycle performance of the battery cell.

[0078] In any embodiment, the mass proportion of the adhesive in the adhesive layer is 10-20%, and the mass proportion of the adhesive in the adhesive layer can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%; optionally, the mass proportion of the adhesive in the adhesive layer is 13-18%. The mass proportion of the adhesive in the adhesive layer affects the bonding performance. When the mass proportion of the adhesive in the adhesive layer is less than 10%, the bonding force is insufficient. When the mass proportion of the adhesive in the adhesive layer is greater than 20%, the bonding force is too large and the coating is uneven.

[0079] In any embodiment, the average particle size of the inorganic particles is 0.1 to 10 nm, and the average particle size of the inorganic particles can be 0.1 nm, 0.2 nm, 0.3 nm, 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1.0 nm, 2.0 nm, 3.0 nm, 4.0 nm, 5.0 nm, 6.0 nm, 7.0 nm, 8.0 nm, 9.0 nm, or 10.0 nm; optionally, the average particle size of the inorganic particles is 0.2 to 0.8 nm, and the average particle size of the inorganic particles affects the coating performance. When the average particle size of the inorganic particles is less than 0.1 nm, the pores are easily blocked, reducing the ion transmission capacity. When the average particle size of the inorganic particles is greater than 10 nm, uneven dispersion is easily caused, affecting the heat resistance.

[0080] In any embodiment, the specific surface area of ​​the inorganic particles is 5 to 15 g / m 2 The specific surface area of ​​the inorganic particles can be 5g / m 2 , 6g / m 2 , 7g / m 2 , 8g / m 2 , 9g / m 2 , 10g / m 2 , 11g / m 2 , 12g / m 2 , 13g / m 2 , 14g / m 2 , 15g / m 2 Optionally, the specific surface area of ​​the inorganic particles is 6 to 9 g / m 2 The specific surface area of ​​inorganic particles affects the surface tension. When the specific surface area of ​​inorganic particles is less than 5g / m 2 When the surface tension is insufficient, the bonding is not strong. When the specific surface area of ​​the inorganic particles is greater than 15g / m 2 When the surface tension is too large, it is difficult to apply evenly during coating.

[0081] In any embodiment, the air permeability of the separator is 300-500 s / 100 cc. The air permeability of the separator can be 300 s / 100 cc, 320 s / 100 cc, 350 s / 100 cc, 380 s / 100 cc, 400 s / 100 cc, 420 s / 100 cc, 450 s / 100 cc, 470 s / 100 cc, or 500 s / 100 cc. Optionally, the air permeability of the separator is 400-450 s / 100 cc. The air permeability of the separator affects the porosity of the separator, thereby affecting the ion transmission capacity and puncture resistance of the separator. When the air permeability of the separator is less than 300 s / 100 cc, the ion transmission capacity is weakened. When the air permeability of the separator is greater than 500 s / 100 cc, the puncture resistance of the separator is reduced.

[0082] In any embodiment, the porosity of the separator is 25% to 65%. The porosity of the separator can be 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, or 65%. Optionally, the porosity of the separator is 40% to 50%. Maintaining a certain porosity of the separator can improve the separator's deformation resistance and puncture resistance, while also improving ion transmission capacity. When the separator's porosity is less than 25%, the ion transmission capacity is reduced. When the separator's porosity is greater than 65%, the separator's puncture resistance is reduced.

[0083] In any embodiment, the porosity of the base membrane is 30% to 70%, and the porosity of the base membrane can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, or 70%. Optionally, the porosity of the base membrane is 50% to 60%. Maintaining a certain porosity of the base membrane can improve the ion transmission capacity and puncture resistance of the isolation membrane, and at the same time improve the ion transmission capacity. When the porosity of the base membrane is less than 30%, the ion transmission capacity will be reduced. When the porosity of the base membrane is greater than 70%, the puncture resistance of the isolation membrane will decrease; and / or,

[0084] The porosity of the gel membrane is 40% to 80%. The porosity of the gel membrane can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 7540%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%. Optionally, the porosity of the gel membrane is 50% to 60%. Maintaining a certain porosity of the gel membrane can improve the ion transmission capacity and puncture resistance of the isolation membrane, and at the same time improve the ion transmission capacity. When the porosity of the gel membrane is less than 40%, the ion transmission capacity will be reduced. When the porosity of the gel membrane is greater than 80%, the puncture resistance of the isolation membrane decreases.

[0085] In any embodiment, the pore size of the base membrane is 100-800 nm, and the pore size of the base membrane may be 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm, or 800 nm; optionally, the pore size of the base membrane is 200-600 nm, and the pore size of the base membrane affects the puncture resistance and ion transmission capacity of the isolation membrane, and can also improve the ion transmission capacity. When the pore size of the base membrane is less than 100 nm, the ion transmission capacity will be reduced. When the pore size of the base membrane is greater than 800 nm, the puncture resistance of the isolation membrane decreases; and / or,

[0086] The pore size of the gel membrane is 200-1000nm. The pore size of the gel membrane can be 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm, 750nm, 800nm, 850nm, 900nm, 950nm, 1000nm; optionally, the pore size of the gel membrane is 200-600nm. The pore size of the gel membrane affects the ion transmission ability and puncture resistance of the isolation membrane. When the pore size of the gel membrane is less than 200nm, the ion transmission ability will be reduced. When the pore size of the gel membrane is greater than 1000nm, the puncture resistance of the isolation membrane will decrease.

[0087] In any embodiment, the surface density of the base film is 2 to 10 g / m 2 The surface density of the base film can be 2g / m 2 , 3g / m 2 , 4g / m 2 , 5g / m 2 , 6g / m 2 , 7g / m 2 , 8g / m 2 , 9g / m 2 , 10g / m 2 Optionally, the surface density of the base film is 3 to 8 g / m 2 The surface density of the base film affects the shape retention and ion transmission ability of the isolation membrane. When the surface density of the base film is less than 2g / m 2 When the surface density of the base film is greater than 10g / m 2 When the ion transmission capacity is reduced; and / or,

[0088] The surface density of the gel film is 2 to 10 g / m 2 The surface density of the gel film can be 2g / m2 , 3g / m 2 , 4g / m 2 , 5g / m 2 , 6g / m 2 , 7g / m 2 , 8g / m 2 , 9g / m 2 , 10g / m 2 Optionally, the surface density of the gel film is 4 to 8 g / m 2 The surface density of the gel film affects the puncture resistance and ion transmission capacity of the isolation membrane. When the surface density of the gel film is less than 2g / m 2 When the surface density of the gel film is greater than 10g / m 2 When the ion transport capacity is reduced, the cycle performance of the battery cell will be affected; and / or,

[0089] The specific surface area of ​​the bonding layer is 1.0 to 6.0 g / m 2 The specific surface area of ​​the adhesive layer can be 1g / m 2 , 2g / m 2 , 3g / m 2 , 4g / m 2 , 5g / m 2 , 6g / m 2 Optionally, the specific surface area of ​​the adhesive layer is 2.0 to 4.0 g / m 2 The specific surface area of ​​the bonding layer affects the surface tension. When the specific surface area of ​​the bonding layer is less than 2g / m 2 When the surface tension is insufficient, the bonding is not strong. When the specific surface area of ​​the bonding layer is greater than 10g / m 2 When the surface tension is too large, it is difficult to apply evenly during coating.

[0090] In a second aspect, an embodiment of the present application provides a method for preparing an isolation film, which is used to prepare the isolation film of the first aspect of the present application, comprising the following steps:

[0091] providing a base film,

[0092] An adhesive layer is arranged on one side of the base film, and a gel film is arranged on the side of the adhesive layer facing away from the base film to obtain an isolation film.

[0093] By setting an adhesive layer on one side of the base film and setting a gel film on the side of the adhesive layer away from the base film, the stable shape of the base film provides support for the adhesive layer, and the adhesive film bonds the base film and the gel film into a whole to obtain an isolation film.

[0094] In any embodiment, the step of providing a base film comprises:

[0095] The base film is prepared by melt extrusion and heat stretching. The base film prepared by melt extrusion and heat stretching has good shape retention ability.

[0096] In any embodiment, the steps of providing an adhesive layer on one side of the base film and providing a gel film on the side of the adhesive layer facing away from the base film to obtain the isolation film include:

[0097] preparing a bonding layer slurry, and coating the bonding layer slurry on one side of the base film to obtain a base film containing a bonding layer;

[0098] A gel film is arranged on the side of the adhesive layer of the base film containing the adhesive layer facing away from the base film, and the film is dried and pressed to obtain an isolation film.

[0099] Wherein, the bonding layer slurry includes inorganic particles, a binder and a solvent. By configuring the bonding layer slurry and coating the bonding layer slurry on one side of the base film, a base film containing a bonding layer is obtained, which can make the bonding layer slurry evenly dispersed on the base film, providing uniform bonding ability. By containing inorganic particles, a binder and a solvent, the inorganic particles and the binder are dispersed in the solvent, which is convenient for coating. In some embodiments of the present invention, the solvent includes water. And / or,

[0100] The drying temperature is 30-40°C, and the drying temperature can be 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, or 40°C; optionally, the drying temperature is 33-37°C. The drying temperature affects the adhesion properties of the base film and the gel film to the adhesive layer. When the drying temperature is less than or equal to 30°C, the adhesion is not strong. When the drying temperature is less than or equal to 40°C, the adhesion temperature is too high and the adhesion is uneven. And / or,

[0101] The drying time is 1 to 10 seconds, and the drying time can be 1 second, 2 seconds, 3 seconds, 4 seconds, 5 seconds, 6 seconds, 7 seconds, 8 seconds, 9 seconds, or 10 seconds; optionally, the drying time is 3 to 7 seconds. The drying time affects the adhesion performance of the base film and the gel film to the adhesive layer. If the drying time is less than 1 second, the adhesion is not tight enough, and if the drying time is greater than 10 seconds, the adhesion is not tight enough; and / or,

[0102] The pressing pressure is 5 to 20N, and the pressing pressure can be 5N, 8N, 10N, 12N, 15N, 18N, and 20N; optionally, the pressing pressure is 8 to 15N. The pressing pressure affects the adhesion performance of the base film and the gel film to the bonding layer. When the pressing pressure is less than 5N, the adhesion of the base film and the gel film to the bonding layer is not tight enough. When the pressing pressure is greater than 20N, the isolation film will be compressed, increasing the probability of inorganic particles damaging the isolation film.

[0103] In a third aspect, an embodiment of the present application provides an electrochemical device comprising the isolation membrane of the first aspect of the present application.

[0104] In any embodiment, the electrochemical device comprises a capacitor, a primary battery, or a secondary battery.

[0105] The technical solutions of the present invention are further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0106] The parameters of the isolation membranes of Examples 1 to 28 of the present application are as shown in Table 1.

[0107] Comparative Example 1

[0108] A separation film comprises an adhesive layer and base films arranged on both sides of the adhesive layer.

[0109] Comparative Example 2

[0110] An isolation film comprises an adhesive layer and gel films arranged on both sides of the adhesive layer.

[0111] The isolation films of Examples 1 to 28 and Comparative Examples 1-2 were tested as follows:

[0112] Destruction resistance test

[0113] 1) Sample preparation: Cut a sample with a diameter greater than 65 mm and lay it flat on the testing machine;

[0114] 2) Testing:

[0115] Install a puncture fixture on the tensile testing machine with a needle diameter of 1mm. Click the test button until the diaphragm is punctured. The tensile testing machine display shows the test value.

[0116] Thermal shrinkage test

[0117] 1) Sample preparation: Use a punch to punch out samples with a width of 50 mm and a length of 100 mm. 5-10 parallel samples are placed on a glass plate and fixed with paper clips on all four sides.

[0118] 2) Testing:

[0119] Set the temperature of the forced air oven to 250°C. After the temperature reaches the set temperature and stabilizes for 60 minutes, place the glass plate in the oven and time it for 1 hour. Measure the length and width of the diaphragm and mark the values ​​as a and b respectively.

[0120] 3) Calculation:

[0121] Lengthwise shrinkage A = (100-a) / 100*100%;

[0122] Width direction shrinkage B = (50-b) / 50*100%;

[0123] Record the values ​​of A and B respectively.

[0124] Room temperature cycle performance test of secondary batteries

[0125] The secondary batteries prepared in Examples 1 to 28 and Comparative Examples 1 to 2 were charged and discharged for the first time at 25°C. The process was as follows: after standing for 30 minutes at 25°C, the secondary batteries were charged to 4.35V at a constant current of 1C, and then charged at a constant voltage until the current was ≤0.05C; then, the batteries were discharged to 2.8V at a constant current of 1C, and the discharge capacity C1 of the first cycle was recorded.

[0126] The battery was then subjected to repeated charge and discharge cycles at a rate of 0.33C1 / 1C1 over a voltage range of 3.3V to 4.3V, and the discharge capacity was recorded. The capacity retention rate at the Nth cycle = (discharge capacity at the Nth cycle / discharge capacity at the first cycle) × 100%. The capacity retention rate of the secondary battery was tested after 1000 cycles at 25°C.

[0127] The performance test results of Examples 1 to 28 are shown in Table 1, and the performance test results of Comparative Examples 1 and 2 are shown in Table 2.

[0128] Table 2 Performance test results of Comparative Example 1 and Comparative Example 2

[0129] It can be seen from the data in Tables 1 and 2 that by arranging the base film and the gel film on both sides of the adhesive layer, the gel film and the base film are bonded into a whole under the bonding action of the adhesive layer. When an external force is applied in the vertical direction of the isolation membrane, the isolation membrane is deformed but not easily ruptured, thereby delaying the rupture time of the isolation membrane and improving the stability and safety of the battery. Therefore, the puncture resistance, heat shrinkage resistance and battery cycle performance of the isolation membranes of Examples 1 to 28 are better than those of Comparative Examples 1 and 2.

[0130] From Examples 8 to 12, it can be seen that the surface density of the gel film affects the puncture resistance and ion transmission capacity of the separator. When the surface density of the gel film is less than 2 g / m 2 When the surface density of the gel film is greater than 10g / m 2 When the battery is heated, the ion transmission capacity will be reduced, thus affecting the cycle performance of the battery.

[0131] It can be seen from Examples 12 to 17 that the mass proportion of inorganic particles in the bonding layer affects the ion transmission capacity and the heat resistance of the isolation membrane. When the mass proportion of inorganic particles in the bonding layer is less than 30%, the bonding layer is too thin and the heat resistance is reduced, which in turn affects the cycle performance of the battery cell. When the mass proportion of inorganic particles in the bonding layer is greater than 50%, the ion transmission capacity is reduced, which in turn affects the cycle performance of the battery cell.

[0132] It can be seen from Examples 16 to 21 that the thickness of the bonding layer affects the energy density of the battery cell and thus affects the service life of the battery cell, and also affects the heat resistance of the isolation membrane. When the thickness of the bonding layer is less than 0.5μm, the heat resistance of the isolation membrane will be reduced. When the thickness of the bonding layer is greater than 6μm, the energy density of the battery cell will be reduced, affecting the service life of the battery cell.

[0133] It can be seen from Examples 20 to 25 that the thickness of the base film affects the energy density of the battery cell and the morphology retention performance of the isolation membrane. When the thickness of the base film is less than 3 μm, the base film is too thin, and the thickness of the isolation membrane is too thin, which reduces the morphology retention ability of the isolation membrane. When the thickness of the base film is greater than 12 μm, the base film is too thick, which reduces the energy density of the battery cell and thus reduces the service life of the battery cell.

[0134] It can be seen from Examples 24 to 28 that the thickness of the gel film affects the energy density of the battery cell and the puncture resistance of the isolation membrane. When the thickness of the gel film is less than 1 μm, the gel film is too thin, and the thickness of the isolation membrane is too thin, which reduces the puncture resistance of the isolation membrane. When the thickness of the gel film is greater than 12 μm, the gel film is too thick, which reduces the energy density of the battery cell and thus reduces the service life of the battery cell.

[0135] In summary, in the isolation membrane proposed in the present application, the gel membrane has good ductility and deformation resistance, is not easy to be punctured, or after being punctured, it still completely covers the punctured area, so that the isolation membrane still plays the role of isolating the positive and negative electrodes; the base membrane has good shape retention ability and self-supporting performance; by arranging the base membrane and the gel membrane on both sides of the bonding layer respectively, the gel membrane and the base membrane are bonded into a whole under the bonding action of the bonding layer, so that when an external force is applied in the vertical direction of the isolation membrane, the isolation membrane is deformed, but is not easy to rupture, thereby delaying the rupture time of the isolation membrane and improving the stability and safety of the battery.

[0136] The above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Those skilled in the art will readily appreciate that the present invention is susceptible to various modifications and variations. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention shall be included within the scope of the present invention.

Claims

1. A separation film, characterized in that: The invention comprises an adhesive layer and a base film and a gel film which are respectively arranged on both sides of the adhesive layer.

2. The isolation film according to claim 1, characterized in that The thickness of the bonding layer is δ1, wherein 0.5 μm≤δ1≤5 μm, optionally, 1 μm≤δ1≤3 μm; and / or, The thickness of the base film is δ2, wherein 3 μm≤δ2≤12 μm, optionally, 3 μm≤δ2≤7 μm; and / or, The thickness of the gel film is δ3, wherein 1 μm≤δ3≤12 μm, optionally, 1 μm≤δ3≤8 μm.

3. The isolation film according to claim 1 or 2, characterized in that: The material of the base film includes at least one of polyolefin, polyether, polyetherketone, polyimide, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymer and copolymer containing CF bond; and / or, The material of the gel film includes at least one of polyurethane and polyurethane.

4. The isolation membrane according to any one of claims 1 to 3, characterized in that: The bonding layer includes inorganic particles and a bonding agent.

5. The isolation film according to claim 4, characterized in that The inorganic particles include any one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, yttrium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate and magnesium fluoride; and / or, The binder includes at least one of acrylate, acrylic acid and carboxymethyl cellulose.

6. The isolation film according to claim 4 or 5, characterized in that: The mass proportion of the inorganic particles in the bonding layer is 30% to 50%; optionally, the mass proportion of the inorganic particles in the bonding layer is 35% to 45%; and / or, The mass proportion of the adhesive in the adhesive layer is 10-20%; optionally, the mass proportion of the adhesive in the adhesive layer is 13-18%.

7. The isolation membrane according to any one of claims 4 to 6, characterized in that: The average particle size of the inorganic particles is 0.1 to 10 nm; The diameter is 0.2 to 0.8 nm; and / or, The specific surface area of ​​the inorganic particles is 5 to 15 g / m 2 Optionally, the specific surface area of ​​the inorganic particles is 6 to 9 g / m 2 .

8. The isolation membrane according to any one of claims 1 to 7, characterized in that: The transverse tensile strength of the isolation film is greater than 1000 kg / cm 2 and / or, The longitudinal tensile strength of the isolation film is greater than 1200 kg / cm 2 and / or, The air permeability of the isolation membrane is 300-500s / 100cc; optionally, the air permeability of the isolation membrane is 400-450s / 100cc; and / or, The porosity of the isolation membrane is 25% to 65%, and optionally, the porosity of the isolation membrane is 40% to 50%; and / or, The porosity of the base film is 30% to 70%, and optionally, the porosity of the base film is 50% to 60%; and / or, The porosity of the gel film is 40% to 80%. Optionally, the porosity of the gel film is 50% to 60%.

9. The isolation membrane according to any one of claims 1 to 8, characterized in that: The pores of the base film have a pore size of 100 to 800 nm; optionally, the pores of the base film have a pore size of 200 to 600 nm; and / or, The pores of the gel membrane have a pore size of 200 to 1000 nm; optionally, the pores of the gel membrane have a pore size of 200 to 600 nm.

10. The isolation film according to any one of claims 1 to 9, characterized in that: The surface density of the base film is 2 to 10 g / m 2 Optionally, the surface density of the base film is 4 to 8 g / m 2 and / or, The surface density of the gel film is 2 to 10 g / m 2 Optionally, the surface density of the gel film is 4 to 8 g / m 2 and / or, The specific surface area of ​​the bonding layer is 1.0 to 6.0 g / m 2 Optionally, the specific surface area of ​​the bonding layer is 2.0 to 4.0 g / m 2 .

11. A method for preparing an isolation film according to any one of claims 1 to 10, characterized in that: The following steps are involved: providing a base film, An adhesive layer is arranged on one side of the base film, and a gel film is arranged on the side of the adhesive layer away from the base film to obtain an isolation From the membrane.

12. The method for preparing an isolation film according to claim 11, characterized in that: The step of providing a base film comprises: The base film was prepared by melt extrusion and heat stretching.

13. The method for preparing a separator according to claim 11 or 12, characterized in that: The steps of providing an adhesive layer on one side of the base film and providing a gel film on the side of the adhesive layer away from the base film to obtain the isolation film include: Prepare a bonding layer slurry, and apply the bonding layer slurry on one side of the base film to obtain a base film containing a bonding layer; A gel film is arranged on the side of the adhesive layer of the base film containing the adhesive layer facing away from the base film, and the film is dried and pressed to obtain a separation film; Wherein, the bonding layer slurry comprises inorganic particles, a binder and a solvent; and / or, The drying temperature is 30-40°C; optionally, the drying temperature is 33-37°C; and / or, The drying time is 1 to 10 seconds; optionally, the drying time is 3 to 7 seconds; and / or, The pressing pressure is 5-20N; optionally, the pressing pressure is 8-15N.

14. An electrochemical device, characterized in that: The invention comprises the isolation film according to any one of claims 1 to 10.

15. The electrochemical device according to claim 14, characterized in that The electrochemical device includes a capacitor, a primary battery, or a secondary battery.

Citation Information

Patent Citations

  • Lithium ion battery composite isolating membrane

    CN109546063A

  • Lithium battery composite diaphragm as well as preparation method and application thereof

    CN114335904A

  • Microporous polymeric membrane, battery separator and battery

    EP2111915A1

  • Separator for lithium-ion battery, manufacturing method therefor, and lithium-ion battery

    WO2017008286A1