Spliced lithium ribbon and method for forming same

By filling the spacer area of ​​the basic lithium strip with molten lithium and then cooling and solidifying it, the problems of connection stability and thickness consistency of spliced ​​lithium strips are solved, resulting in more stable lithium strip connections and lower production costs.

WO2024245087A1PCT designated stage expired Publication Date: 2024-12-05CHONGQING TIANQI LITHIUM CO LTD +1

Patent Information

Application Number
PCT/CN2024/094834
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing spliced ​​lithium strips have poor connection stability and are difficult to control in terms of thickness consistency, which affects the efficiency and cost of lithium strip usage.

Method used

Molten lithium is filled into the gaps between the base lithium strips and cooled and solidified in a protective gas environment to weld the base lithium strips, forming spliced ​​lithium strips.

Benefits of technology

It improves the connection stability and thickness consistency between basic lithium strips, reduces the production cost of lithium strips, and improves the utilization efficiency of lithium strips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024094834_05122024_PF_FP_ABST
    Figure CN2024094834_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of energy storage devices, and provides a spliced lithium ribbon and a method for forming same, for facilitating thickness consistency control and more stable connection between basic lithium ribbons. The method for forming the spliced lithium ribbon comprises: providing at least two basic lithium ribbons; sequentially laying the basic lithium ribbons side by side on the upper surface of a horizontally-arranged bearing layer, so that the basic lithium ribbons and the upper surface of the bearing layer are attached together, and a space is formed between adjacent basic lithium ribbons to form a solder area for the filling of a solder material; and filling the solder area with a molten lithium liquid to solder the basic lithium ribbons into a whole, so as to form the spliced lithium ribbon, wherein a protective gas is provided in the molten lithium liquid filling process, so as to protect the molten lithium liquid and cool and solidify same.
Need to check novelty before this filing date? Find Prior Art

Description

Spliced ​​lithium strip and forming method thereof

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of and priority to Chinese patent application No. CN 2023106526185, filed on June 2, 2023, and is incorporated herein by reference in its entirety for all other purposes. Technical Field

[0003] The present invention relates to the technical field of energy storage devices, and in particular to a spliced ​​and formed lithium belt and a forming method thereof. Background Art

[0004] With the increasing penetration of new energy vehicles in recent years, traditional fuel vehicles have been continuously reducing costs to consolidate their market share. To fully promote vehicle electrification, lithium-ion battery energy density must achieve breakthroughs to meet the demand for long driving ranges in new energy vehicles. As battery manufacturers continue to iterate their technologies, the next generation of high-energy-density lithium-ion batteries is gradually entering the market. Silicon-containing anode pre-lithiation and lithium metal anodes are considered the most promising for large-scale commercialization in the near future. However, the high cost of lithium metal ribbons makes the cost of pre-lithiation or direct use of lithium metal anodes significantly higher than that of traditional lithium-ion batteries, which has hindered the development of high-energy-density lithium-ion batteries. Due to the unique properties of lithium metal, the processing cost of lithium metal ribbons currently accounts for over 40% of the total cost. Therefore, improving the production and utilization efficiency of lithium metal ribbons has a significant impact on reducing costs. The width of lithium metal ribbons is a major factor limiting utilization efficiency. Mechanical extrusion methods are limited by the inner diameter of the extrusion barrel, making ultra-wide lithium metal ribbons impossible to produce. However, the current mass-produced anode electrode width can reach over one meter, far exceeding the width of existing lithium metal ribbons. To this end, Chinese patent CN210467983U and public invention patent CN112310412A mention the use of two or more basic lithium ribbons with a thickness of less than 170 mm and more than 0.2 mm to form an ultra-wide spliced ​​lithium ribbon, and the added value of the superimposed thickness at the splicing point of the spliced ​​lithium ribbon does not exceed 6% of the thickness of the basic lithium ribbon. However, this splicing method has an overlapping area of ​​1 to 3 mm, and it is difficult to reduce the thickness of the overlapping area by longitudinal rolling without affecting the morphology of the lithium ribbon in the non-spliced ​​area, and the connection stability between the basic lithium ribbons is poor. Chinese patent CN113967699A proposes a method and equipment for splicing ultra-thin lithium foil or lithium ribbon, which lays at least two basic lithium ribbons with a thickness of less than 100 μm on a support layer, and then uses a rolling mill to achieve the adhesion of the basic lithium ribbons to the support layer to achieve splicing. This method is also difficult to ensure the connection stability between the basic lithium ribbons.

[0005] Summary of the Invention

[0006] The technical problem to be solved by the present invention is to provide a spliced ​​lithium strip and a forming method thereof, which is convenient for thickness consistency control and has more stable connections between basic lithium strips.

[0007] The technical solution adopted by the present invention to solve the technical problem is: a method for forming a spliced ​​lithium strip, comprising the following steps:

[0008] providing at least two basic lithium belts;

[0009] Laying the basic lithium ribbons side by side on the upper surface of a horizontally arranged supporting layer in sequence, so that the basic lithium ribbons are attached to the upper surface of the supporting layer, and adjacent basic lithium ribbons are spaced apart to form a welding area filled with welding material;

[0010] The welding area is filled with molten lithium liquid, and the basic lithium strips are welded into a whole, thereby forming the spliced ​​formed lithium strip, wherein a protective gas is provided during the filling process of the molten lithium liquid to protect the molten lithium liquid and cool and solidify it.

[0011] Furthermore, the protective gas is argon, helium or neon.

[0012] Furthermore, the bearing layer is polyamide-imide, polyimide, polyetheretherketone, polytetrafluoroethylene, polyphenylene, polyetherimide, polyphthalamide, polyethylene terephthalate, steel belt, copper belt or aluminum belt.

[0013] Furthermore, the thickness of the base lithium strip is 0.02 to 3 mm, preferably 0.5 to 2 mm.

[0014] Furthermore, the width of the base lithium ribbon is 40 to 200 mm, preferably 90 to 160 mm.

[0015] Furthermore, the temperature of the molten lithium solution is 200-300°C.

[0016] Furthermore, the cooling rate of the molten lithium solution is 10°C / s to 30°C / s.

[0017] Furthermore, the height T2 of the molten lithium liquid after solidification satisfies: when T1≤0.1mm, |T1-T2|≤5μm; when T1≥0.1mm, |T1-T2| / T1≤%, wherein T1 is the thickness of the basic lithium strip.

[0018] Furthermore, the width of the welding zone is 5 to 15 mm.

[0019] The present invention also provides a spliced ​​and formed lithium belt, which is obtained by the above-mentioned spliced ​​and formed lithium belt forming method.

[0020] The beneficial effects of the present invention are: the spliced ​​formed lithium strips and the forming method thereof of the present invention, the spliced ​​formed lithium strips are melted by filling molten lithium liquid in the gaps (welding areas) between the basic lithium strips, and then the basic lithium strips are welded together to form a spliced ​​formed lithium strip after the lithium liquid solidifies, which can make the connection between the basic lithium strips more stable, that is, a spliced ​​formed lithium strip with a more stable morphology can be obtained, and a spliced ​​formed lithium strip with better thickness consistency can be obtained by precisely controlling the filling amount of the molten lithium liquid. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] FIG1 is a flow chart of a method for forming a lithium strip by splicing according to the present invention;

[0022] Figure 2 is a schematic diagram of the production of spliced ​​and formed lithium strips;

[0023] FIG3 is a schematic diagram of the arrangement of the basic lithium strip on the supporting layer;

[0024] FIG4 is a cross-sectional view of a spliced ​​and formed lithium ribbon;

[0025] As shown in the figure: spliced ​​and formed lithium strip 1, bearing layer 2, lithium liquid filling equipment 3, welding protection box 4, basic lithium strip roll 5, unwinding roller 6, winding roller 7, air pipe 8, dry air cooling zone 9, basic lithium strip 11, welding zone 12. DETAILED DESCRIPTION

[0026] The present invention will be further described below with reference to the accompanying drawings and examples.

[0027] As shown in FIG1 and FIG2 , the forming method of the spliced ​​lithium strip 1 of the present invention comprises the following steps:

[0028] Step 1: providing at least two basic lithium ribbons 11, wherein the basic lithium ribbons 11 can be unwound from a basic lithium ribbon roll 5 by an unwinding roller 6;

[0029] Step 2: Lay the basic lithium strips 11 side by side on the upper surface of the horizontally arranged carrier layer 2, so that the basic lithium strips 11 are attached to the upper surface of the carrier layer 2, and there is a gap between adjacent basic lithium strips 11 to form a welding area 12 filled with welding material, wherein the width of the carrier layer 2 is generally greater than the width of the spliced ​​lithium strips 1;

[0030] Step 3: Fill the welding area 12 with molten lithium liquid and weld the basic lithium strip 11 into a whole to form the spliced ​​formed lithium strip 1, wherein a protective gas is provided during the filling process of the molten lithium liquid to protect the molten lithium liquid from reacting with components in the air and cooling and solidifying it.

[0031] The protective gas in the present invention is a gas that does not react with lithium, including but not limited to argon, helium or neon.

[0032] The strength of the lithium ribbon fluctuates to a certain extent due to the production and preparation conditions. The greater the tensile strength of the lithium ribbon, the lower the thickness change due to tension during the roll-to-roll process. The optimal tensile strength σ of the basic lithium ribbon 11 is ≥1.2Mpa.

[0033] The forming method of the spliced ​​lithium strip of the present invention melts the edge of the basic lithium strip 11 by filling the gap (welding area 12) between the basic lithium strips 11 with molten lithium liquid, thereby welding the basic lithium strips 11 together to form a spliced ​​lithium strip 1 after the lithium liquid solidifies. This method can make the connection between the basic lithium strips more stable, that is, a spliced ​​lithium strip with a more stable shape can be obtained. The fracture strength of the weld can reach 1.0 MPa through experiments. In addition, this method basically does not affect the morphology of the basic lithium strip 11, such as flatness and thickness, and under the premise that the thickness fluctuation of the basic lithium strip is the same, the filling amount of the molten lithium liquid can be accurately controlled to obtain a spliced ​​lithium strip with better thickness consistency, which is beneficial to improving the unit area capacity consistency of the spliced ​​lithium strip and preventing the growth of lithium dendrites caused by local lithium excess.

[0034] The molten lithium liquid is filled into the welding area 12 specifically by a lithium liquid filling device 3. The lithium liquid filling device 3 can be an existing extrusion coating device capable of achieving precise flow control or a heating device can be added to the existing slit extrusion coating or gravure coating device commonly used in the lithium battery industry.

[0035] Specifically, the base lithium ribbon 11 can be attached to the upper surface of the carrier layer 2 by rolling, bonding, etc. In FIG2 , the unwound base lithium ribbon 11 is attached to the upper surface of the carrier layer 2 by rolling.

[0036] The bearing layer 2 mainly serves to carry the basic lithium strip 11 and the molten lithium liquid. It is understandable that the bearing layer 2 needs to withstand high temperatures to avoid being affected by the molten lithium liquid, and no relative movement can occur between the bearing layer 2 and the basic lithium strip 11 before the molten lithium liquid solidifies. In order to avoid relative movement between the bearing layer 2 and the basic lithium strip 11, specifically, both can be prohibited from being set or synchronized movement can be achieved through rollers. The bearing layer 2 can specifically be polyamide-imide, polyimide, polyetheretherketone, polytetrafluoroethylene, polyphenylene, polyetherimide, polyphthalamide, polyethylene terephthalate, steel strip, copper strip or aluminum strip. After the spliced ​​and formed lithium strip 1 is spliced, the bearing layer 2 can be removed from the spliced ​​and formed lithium strip 1, or it can be wound together with the spliced ​​and formed lithium strip 1 through the winding roller 7.

[0037] The shielding gas is mainly provided through the air pipe 8, which can be one or more air pipes, and the shielding gas is guided to the welding area 12 through the air pipe 8. In order to improve the utilization rate of the shielding gas and better protect the molten lithium liquid, the present invention passes the shielding gas into the welding protection box 4 through the air pipe 8. During welding, the base lithium strip 11 and the bearing layer 2 are passed into the welding protection box 4 together, and then the molten lithium liquid is filled into the welding area 12 in the welding protection box 4 to protect the molten lithium liquid from reacting with the components in the air and cooling and solidifying it. In the embodiment of the present invention, the molten lithium liquid is cooled to less than 100°C by the shielding gas. In order to facilitate the splicing and forming of lithium strips or improve production efficiency, after the shielding gas is cooled, a dry air cooling zone 9 can be set after the welding process to further cool the lithium in the welding area 12.

[0038] Preferably, the width of the base lithium ribbon 11 is 40 to 200 mm, and optimally 90 to 160 mm. Preferably, the thickness of the base lithium ribbon 11 is 0.02 to 3 mm, and optimally 0.5 to 2 mm. A thickness of 0.5 to 2 mm is most conducive to welding the base lithium ribbons 11 together using molten lithium.

[0039] The temperature of the molten lithium solution is generally between 180°C and 500°C, though other temperatures are possible. In the present invention, the optimal temperature of the molten lithium solution is between 200°C and 300°C. A molten lithium solution temperature of 200°C and 300°C ensures that the edges of the base lithium ribbon 11 are melted while also facilitating rapid cooling of the molten lithium solution below its freezing point, thereby minimizing the impact on the base lithium ribbon 11. In particular, when the base lithium ribbon 11 is 0.1 to 2 mm thick, a molten lithium solution temperature of 200°C and 300°C allows for a more uniform thickness and better-shaped spliced ​​lithium ribbon 1.

[0040] In order to facilitate more uniform filling of the molten lithium liquid in the welding area 12 and prevent deformation of the base lithium strip 11 due to excessively rapid cooling of the molten lithium liquid, the cooling rate of the molten lithium liquid is preferably 10° C. / s to 30° C. / s.

[0041] The thickness of lithium ribbons used for pre-lithiation of lithium-ion batteries is generally controlled within 5μm, while the thickness of lithium ribbons used in lithium metal batteries is mostly controlled within 20μm. To achieve the required thickness, the assembled lithium ribbons need to be further thinned. To minimize the absolute thickness difference when the assembled lithium ribbons are pressed to ultra-thin thicknesses, thereby preventing the risk of lithium dendrite growth caused by excess lithium, optimally, as shown in FIG4 , the height T2 of the molten lithium solution after solidification satisfies the following conditions: when T1 ≤ 0.1mm, |T1 - T2| ≤ 5μm; when T1 ≥ 0.1mm, |T1 - T2| / T1 ≤ 4%, where T1 is the thickness of the base lithium ribbon 11.

[0042] The width of the welding zone 12 can be any value greater than 0. To facilitate direct welding connection of the base lithium ribbon 11 , the width of the welding zone 12 is preferably 5 to 15 mm.

[0043] The present invention also provides a spliced ​​lithium ribbon obtained using the above method. The spliced ​​lithium ribbon is welded and spliced ​​using the above method, providing a more stable connection between the base lithium ribbons. Furthermore, the spliced ​​lithium ribbon is more uniform in thickness.

[0044] Example:

Claims

1. A method for forming a spliced ​​lithium strip, characterized in that: The following steps are involved: Providing at least two base lithium strips (11); The basic lithium strips (11) are sequentially laid side by side on the upper surface of a horizontally arranged support layer (2), so that the basic lithium strips (11) and the upper surface of the support layer (2) are bonded together, and adjacent basic lithium strips (11) are spaced apart to form a welding area (12) filled with welding material; The welding area (12) is filled with molten lithium liquid, and the basic lithium strip (11) is welded into a whole, thereby forming the spliced ​​and formed lithium strip (1), wherein a protective gas is provided during the process of filling the molten lithium liquid to protect the molten lithium liquid and cool it to solidify.

2. The method for forming a spliced ​​lithium strip according to claim 1, characterized in that: The protective gas is argon, helium or neon.

3. The method for forming a spliced ​​lithium strip according to claim 1, characterized in that: The bearing layer (2) is polyamide-imide, polyimide, polyetheretherketone, polytetrafluoroethylene, polyphenylene, polyetherimide, polyphthalamide, polyethylene terephthalate, steel strip, copper strip or aluminum strip.

4. The method for forming a spliced ​​lithium strip according to claim 1, characterized in that: The thickness of the base lithium strip (11) is 0.02 to 3 mm, preferably 0.5 to 2 mm.

5. The method for forming a spliced ​​lithium strip according to claim 1 or 4, characterized in that: The width of the base lithium belt (11) is 40 to 500 mm, preferably 150 to 350 mm.

6. The method for forming a spliced ​​lithium strip according to claim 1 or 4, characterized in that: The temperature of the molten lithium solution is 200-300°C.

7. The method for forming a spliced ​​lithium strip according to claim 5, characterized in that: The cooling speed of the molten lithium solution is 10°C / s to 30°C / s.

8. The method for forming a spliced ​​lithium strip according to claim 1, characterized in that: The height T2 of the molten lithium liquid after solidification satisfies that when T1≤0.1mm, |T1-T2|≤5μm, and when T1≥0.1mm, |T1-T2| / T1≤4%, wherein T1 is the thickness of the basic lithium strip (11).

9. The method for forming a spliced ​​lithium strip according to claim 1, characterized in that: The width of the welding area (12) is 5 to 15 mm.

10. Splicing and forming lithium belt, characterized in that: Obtained by the molding method of spliced ​​lithium strips as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for welding by fused metal filling

    CN102581497A

  • Spray welding method for metal plates

    CN103028850A

  • Spliced molded lithium strip and preparation method thereof

    CN112310412A

  • Ultrathin lithium foil and lithium strip splicing method and equipment

    CN113967699A

  • Splicing forming lithium strip and forming method thereof

    CN116646480A

Cited By

  • Large-diameter tunnel air duct production equipment

    CN119748117A