Poly(carbazole phosphonic acid) material, preparation method, and use in photoelectric device
By polymerizing carbazole phosphate material and adopting specific preparation methods, the coverage and stability of carbazole phosphate small molecules on the conductive substrate are solved, efficient hole transmission and stable photoelectric device performance are achieved, and pertitanium is improved Efficiency and stability of mine solar cells.
Patent Information
- Application Number
- PCT/CN2024/096042
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-29
- Publication Date
- 2024-12-05
AI Technical Summary
Small carbazole phosphate molecules have high hole transport resistance, poor coverage and diffusion problems on conductive substrates, resulting in low stability and efficiency of perovskite solar cells.
By polymerizing small molecule carbazole phosphate, increasing molecular weight, forming a polycarbazole phosphate material with multiple repeat units, and using halogenated phosphate carbazole for catalytic polycondensation reaction, combined with halosilanes and alcohols for hydrolysis, it was prepared A polycarbazole phosphate material with excellent stability and film forming properties.
Improve the film forming and stability of carbazole phosphate material, solve the problems of poor density and easy diffusion of traditional carbazole phosphate small molecules, realize efficient hole transmission in optoelectronic devices, and improve perovskite solar cells. photoelectric conversion efficiency and stability.
Smart Images

Figure CN2024096042_05122024_PF_FP_ABST
Abstract
Description
A polyphosphoric acid carbazole material, preparation method and application in optoelectronic devices Technical Field
[0001] The present invention belongs to the field of material preparation, and more specifically relates to a polyphosphate carbazole material and a preparation method and application thereof. Background Art
[0002] Small molecule phosphate carbazole (PACz) is a recently developed hole transport material with the advantage of solution processability. It can form a monolayer on conductive substrates (ITO and FTO). Compared to PTAA-based polytriphenylamine hole transport layer materials, perovskite films have better wettability on phosphate carbazole, facilitating large-area coating of perovskite films and achieving efficient hole transport in trans-perovskite photovoltaics. Currently, phosphate carbazole has become a commonly used hole transport material in trans-perovskite solar cells. Despite its excellent hole transport properties, the small molecule carbazole has been plagued by problems with its compactness and stability. Efficient hole transport requires the formation of a dense, uniform monolayer on a conductive substrate. However, during actual solution processing, the small molecule carbazole forms localized multilayers, increasing resistance to hole extraction. The small molecule carbazole also diffuses into the perovskite active layer under photothermal conditions. Furthermore, on some rough conductive substrates, such as FTO, the carbazole phosphate small molecule cannot completely cover the entire conductive substrate, resulting in direct contact between the perovskite film and the conductive substrate. This situation not only causes local leakage, but also induces the decomposition of the perovskite, causing the degradation of perovskite solar cells (Science 2020, 370, 1300-1309; Nature 2023, Nature https: / / doi.org / 10.1038 / s41586-41023-05992-y; Joule 2020, 4, 850-864; Nature Energy 2023, https: / / doi.org / 10.1038 / s41560-41023-01227-41566). Developing new hole transport layer materials to address the current problems of carbazole phosphate small molecules is an important step in improving the stability of inverse perovskite photovoltaic devices and promoting their industrialization.
[0003] Summary of the Invention
[0004] The technical problem to be solved by the present invention is the high hole resistance, poor coverage, and diffusion problems encountered when small molecule carbazole phosphate is applied to conductive substrates. The present invention provides a polycarbazole phosphate material having good film-forming properties, excellent stability, and low diffusion resistance. Another technical problem to be solved by the present invention is to provide a method for preparing the polycarbazole phosphate material. Another technical problem to be solved by the present invention is to provide the application of the polycarbazole phosphate material in organic solar cells and perovskite solar cells.
[0005] During the research process of this patent, it was found that by polymerizing small molecule carbazole phosphate to increase the molecular weight, its film-forming property on the surface of the conductive substrate can be effectively improved, and a stable hole transport layer with a suitable thickness can be formed.
[0006] A polyphosphoric acid carbazole material comprises a plurality of repeating units, wherein the repeating unit structure is as follows:
[0007] In the formula, the benzene ring on the phosphate carbazole unit does not contain or contains a substituent;
[0008] In the polyphosphoric acid carbazole structure of this patent, as long as the small molecule phosphoric acid carbazole can be polymerized to a certain extent and the molecular weight is increased, the film-forming property of the coating after coating can be effectively improved. The number of repeating units in the polymer material can be 2 to 10,000,000, preferably the number of repeating units is greater than 5, 8, 10, 15, 20, 25, 30, 50, 80, 100, 200, 500, 1000, 2000, 5000, etc., and can also be a parameter range composed of any integers in this range.
[0009] The polycarbazole phosphate used in this patent is formed by the polymerization of small molecules. The small molecule carbazole phosphate here can adopt the structure disclosed in the prior art. In this patent, the molecular weight is increased by polymerizing it. As long as it is a small molecule carbazole phosphate with certain hole transport properties, it can achieve the purpose of the present invention. It can also be modified by some substituents to adjust and improve its performance.
[0010] When containing substituents, the benzene ring contains single or multiple independent substituents, which are selected from:
[0011] 1)H;
[0012] 2) halogen groups;
[0013] 3) cyano;
[0014] 4) alkyl;
[0015] 5) aromatic groups;
[0016] 6) cyclic groups;
[0017] The value range of n is 1-40, the polymerization site of polycarbazole phosphate is at any position on the benzene ring, and the molecular weight range is 300-10,000,000. The value of n here can be 1, 2, 3, 5, 10, 15, 20, or any integer within this range. The molecular weight here is increased after polymerization, and the value can also be greater than 500, 800, 1000, 1500, 2000, 3000, 5000, 8000, 10000, 15000, 20000, 30000, 50000, 100000, 200000, etc., or any integer within this range.
[0018] The alkyl group is selected from (C1-C40) linear alkyl, (C3-C40) branched alkyl or (C3-C40) cycloalkyl.
[0019] The annulation group is used to annulate the benzene ring to form a macrocycle such as naphthalene and anthracene.
[0020] The halogen group is F, Cl, Br or I.
[0021] The aromatic group is selected from one or more of aryl, heteroaryl, aryloxy, heteroaryloxy, arylcarbonyl, heteroarylcarbonyl, arylcarbonyloxy, heteroarylcarbonyloxy, aryloxycarbonyl and heteroaryloxycarbonyl.
[0022] The repeating unit structure is one of the following structural formulas:
[0023] wherein m ranges from 2 to 10,000,000, and R1, R2, and R3 are H or the substituents mentioned above.
[0024] The polyphosphate carbazole material provided in this patent with or without substituents is obtained by polymerizing a small molecule phosphate carbazole and hydrolyzing the ester group. The polymerization site is at any position on the benzene ring. In order to realize the synthesis of the polymer material, the present invention provides the following synthesis idea: polymerization is achieved by catalytic polycondensation of phosphate carbazole. In the reaction, halogenated phosphate carbazole can be used for polycondensation, wherein the halogenated group can be at any position on the benzene ring. In this case, phosphate carbazole modified with some substituents can also be used for the reaction; in addition, the corresponding halogenated compound can be added to copolymerize with the phosphate carbazole during the polycondensation reaction, and then a halogenated silane and an alcohol compound are added to hydrolyze the polyphosphate carbazole into polyphosphate carbazole.
[0025] The preparation method of the polyphosphoric acid carbazole material comprises the following steps:
[0026] Step 1, copolymerizing halogenated phosphate carbazole in a solvent with or without adding other halogenated compounds;
[0027] Step 2: adding halogenated silane and alcohol to carry out hydrolysis to obtain polyphosphoric acid carbazole material.
[0028] The other halogenated compounds are selected from halogenated aromatic hydrocarbons or halogenated thiophenes with or without substituents.
[0029] The aromatic group in the halogenated aromatic hydrocarbon is selected from one or more of aryl, heteroaryl, aryloxy, heteroaryloxy, arylcarbonyl, heteroarylcarbonyl, arylcarbonyloxy, heteroarylcarbonyloxy, aryloxycarbonyl or heteroaryloxycarbonyl.
[0030] The halophosphate carbazole polymerizes by itself without the addition of other halogenated compounds.
[0031] When other halogenated compounds are added, the halogenated phosphate carbazole and the other halogenated compounds are polymerized; the mass ratio of the phosphate carbazole to the halogenated compound is 1:0.01-10.0, the polymerization reaction takes 0.1-72 hours, and the reaction temperature is 0-300°C.
[0032] The catalyst used in the catalytic polymerization reaction is selected from nickel-based catalysts.
[0033] The phosphate carbazole comprises one or more of the following unit structures:
[0034] The value range of n is 1-40.
[0035] Rx are independently selected from:
[0036] 1)H;
[0037] 2) halogen groups;
[0038] 3) cyano;
[0039] 4) alkyl;
[0040] 5) aromatic groups;
[0041] 6) cyclic groups;
[0042] The halogen group is F, Cl, Br or I.
[0043] The alkyl group is selected from (C1-C40) linear alkyl, (C3-C40) branched alkyl or (C3-C40) cycloalkyl.
[0044] In the alkyl group, one or more non-adjacent C atoms are optionally replaced by -O-, -S-, -C(O)-, -C(O-)-O-, -OC(O)-, -OC(O)-O-, -CR 0 =CR 00 - or -C≡C- substitution, where R 0 and R 00 are independently straight-chain alkyl, branched-chain alkyl or cycloalkyl.
[0045] In the alkyl group, one or more H atoms are optionally replaced by F, Cl, Br, I or CN.
[0046] The aromatic group is selected from aryl, heteroaryl, aryloxy, heteroaryloxy, arylcarbonyl, heteroarylcarbonyl, arylcarbonyloxy, heteroarylcarbonyloxy, aryloxycarbonyl or heteroaryloxycarbonyl, and has 4 to 30 ring atoms.
[0047] In one embodiment, dibromocarbazole phosphate is used as a raw material, and a catalytic polymerization reaction is performed to obtain polycarbazole phosphate; polycarbazole phosphate and trimethylsilyl bromide are stirred and reacted in a solvent, and then excess methanol is added for hydrolysis to obtain a polycarbazole phosphate material; the reaction equation is as follows:
[0048] In one embodiment, dibromocarbazole phosphate and aromatic groups are used as raw materials to catalyze a reaction to obtain polycarbazole phosphate; polycarbazole phosphate and trimethylsilyl bromide are stirred in a solvent for reaction, and then excess methanol is added for hydrolysis to obtain a polycarbazole phosphate material; the reaction equation is as follows:
[0049] In the formula, n is an integer not greater than 40, m is an integer from 2 to 10,000,000, and Ar is an aromatic group.
[0050] Application of polycarbazole phosphate materials in the preparation of optoelectronic device structures.
[0051] The optoelectronic device structure comprises a solar cell, a field effect transistor, a photodetector, a ray detector, and a light emitting diode. The solar cell comprises an organic solar cell and a perovskite solar cell.
[0052] The polyphosphoric acid carbazole material is used as a hole transport layer material in an organic solar cell or a perovskite solar cell, or is used for interface modification on the basis of an original hole transport layer.
[0053] In the application, the battery structure is selected from one of the following:
[0054] The perovskite light-absorbing layer includes a metal halide perovskite having the chemical formula ABX3, wherein A includes, but is not limited to, methylamine ion, formamidinium ion, cesium, rubidium, potassium, sodium, ammonium ion, ethylamine, propylamine, butylamine, aniline, benzylamine, phenylethylamine, or a combination thereof; B includes lead, tin, cadmium, germanium, zinc, nickel, or a combination thereof; and X is a fluorine, chlorine, bromine, iodine anion, or a combination thereof.
[0055] Specifically, the solar cell electrode contains one or more of gold, silver, copper, aluminum, carbon, and chromium. The hole transport layer includes PTAA, Spiro-OMeTAD, PEDOT:PSS, NiO, MoO3, V2O5, Poly-TPD, EH44, P3HT or a combination of the above materials. The electron transport layer includes C 60 ,BCP,TiO2,SnO2,PCBM,ICBA,ZnO,ZrAcac,LiF,TPBi,PFN,Nb2O5 or a combination of the above materials.
[0056] Specifically, perovskite solar cells have a photoelectric conversion efficiency of 1% to 30%.
[0057] Organic solar cells have a photoelectric conversion efficiency of 1% to 20%. Beneficial effects
[0058] 1) The polycarbazole phosphate polymer material provided by the present invention has better stability and film-forming properties. The interaction between its polymer chains can effectively solve the problems of poor density and easy diffusion of traditional small molecules of carbazole phosphate, thereby realizing stable optoelectronic devices based on polycarbazole phosphate.
[0059] 2) The synthesis method of the polyphosphate carbazole is simple and rapid, and the reaction conditions are mild. The obtained polyphosphate carbazole material is dissolved in a single or mixed solvent such as toluene, chlorobenzene, chloroform, dichloromethane, methanol, ethanol, isopropanol, etc., and processed into a thin film by spin coating, blade coating, slit coating, dip coating, spraying, etc. to prepare optoelectronic devices based on the polyphosphate carbazole material, including perovskite solar cells, organic solar cells, field-effect transistors, light-emitting diodes, photodetectors, radiation detectors, etc.
[0060] 3) This invention has both important scientific significance and extremely high industrial value. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 shows the stacking morphology and conductive atomic force microscopy current distribution of small molecule phosphate carbazole (left) and polyphosphate carbazole (right) materials on conductive ITO.
[0062] FIG2 is a graph showing the current-voltage curve of a polyphosphate carbazole perovskite solar cell as a function of annealing temperature;
[0063] FIG3 is a graph showing the current-voltage curve of a carbazole phosphate small molecule perovskite solar cell as a function of annealing temperature;
[0064] FIG4 is a graph showing the current-voltage curve of a polycarbazole phosphate perovskite solar cell as a function of concentration;
[0065] FIG5 is a graph showing the current-voltage curve of a carbazole phosphate small molecule perovskite solar cell as a function of concentration;
[0066] FIG6 is a current-voltage curve of the optimal perovskite solar cell of polycarbazole phosphate on an ITO / FTO substrate.
[0067] FIG7 is a long-term stability test curve. DETAILED DESCRIPTION
[0068] Example 1
[0069] Dissolve 3.25g of 3,6-dibromocarbazole and 2.1g of potassium carbonate in 20mL of 1,4-dibromobutane, add 0.485g of tetrabutylammonium bromide, followed by 5.2mL of 50% potassium hydroxide, and stir at 60°C for 12 hours. After cooling to room temperature, concentrate under reduced pressure and filter the product. Purify it through a column to obtain 4.1g of 3,6-dibromo-9-(4-bromobutyl)-9H-carbazole (3,6-dibromo-9-(4-bromobutyl)-9-hydrogen-carbazole), with the following structural formula:
[0070] 1 H NMR (400MHz, CDCl3, ppm): 8.15 (d, J=1.9Hz, 2H), 7.55 (dd, J=8.6Hz, 2.0Hz, 2H), 7.25 (d, 2.1Hz 2H),4.30(t,7.3Hz,2H),3.37(t,6.4Hz,2H),2.07–1.99(m,2H),1.91–1.85(m,2H). 13 C NMR (400MHz, CDCl3, ppm): 139.21, 129.21, 123.58, 123.41, 112.25, 110.28, 42.52, 32.84, 30.06.
[0071] Example 2
[0072] Dissolve 1 g of 3,6-dibromo-9-(4-bromobutyl)-9H-carbazole in 10 mL of triethyl phosphite and heat with stirring at 140°C for 12 hours. Remove the triethyl phosphite by distillation under reduced pressure and purify with a column to obtain diethyl(4-(3,6-dibromo-9H-carbazol-9-yl)butyl)phosphonate, with the following structural formula:
[0073] 1 H NMR (400MHz, CDCl3, ppm): 8.12 (d, 2.1Hz, 2H), 7.54 (dd, J = 8.7Hz, 1.9Hz, 2H), 7.25 (d, 8.9H z,2H),4.25(t,J=7.9Hz,2H),3.96–4.06(m,4H),1.61–1.96(m,6H),1.25(t,J=7.1Hz,6H). 13 C NMR (400MHz, CDCl3, ppm): 139.22, 129.13, 123.53, 123.33, 112.15, 110.33, 61.63, 42.68, 26.12, 24.78, 20.46, 16.46.
[0074] Example 3
[0075] Dissolve 0.8g of Ni(Cod)2, 0.286g of bipyridine, and 0.23mL of 1,5-cyclooctadiene in 10mL of DMF and heat with stirring at 80°C for half an hour. Dissolve 0.5g of (4-(3,6-dibromo-9H-carbazol-9-yl)butyl)phosphonate in 10mL of DMF and slowly add dropwise to the reaction system. Stir at 80°C for 24 hours. After the reaction is complete, cool to room temperature. Slowly add dilute hydrochloric acid dropwise while stirring until the solution dissolves into a transparent green solution. Filter and collect the suspended solids. The final product is a brown polyphosphate carbazole powder with the following structural formula:
[0076] Example 4
[0077] Dissolve 0.12g of polyphosphate carbazole in 20mL of dichloromethane, add 2mL of 0.1g / mL trimethylsilyl bromide dropwise, and stir at room temperature for 24 hours. After the reaction is complete, add excess methanol to the reaction mixture to remove excess trimethylsilyl bromide. Concentrate the solution by vacuum distillation, precipitate in ether, and filter and rinse with ether. The final product is polyphosphate carbazole powder with a number average molecular weight of approximately 1800 and a weight average molecular weight of approximately 2300. The structural formula is as follows:
[0078] Example 5
[0079] The ITO conductive glass was placed in a UV ozone cleaning machine for 15 minutes, and then different concentrations (0.3 mg / ml to 3 mg / ml) of small molecule carbazole phosphate or polycarbazole phosphate were scraped on it and annealed at 100 degrees Celsius, 150 degrees Celsius, and 200 degrees Celsius. 0.7 FA 0.3 PbI3 perovskite polycrystalline film, after thermal annealing, 25nm C is evaporated on its surface 60 , 5nm BCP and 100nm copper electrode to complete the preparation of perovskite solar cells.
[0080] Comparative experiment: In order to compare the performance of polycarbazole phosphate, the small molecule carbazole phosphate (Me-4PACz) shown in the figure below was used for comparison, and the carbazole phosphate prepared in Example 2 was used.
[0081] Small molecule carbazole phosphate (Me-4PACz) and polycarbazole phosphate (Poly-4PACz) were scraped onto ITO conductive glass. As shown in Figure 1, small molecule carbazole phosphate showed poor coverage on the ITO, with localized multilayer accumulation, resulting in low current and high resistance in conductive atomic force microscopy tests. In contrast, polycarbazole phosphate exhibited excellent coverage and film-forming properties on the ITO, resulting in high current and low resistance in conductive atomic force microscopy tests, facilitating hole extraction.
[0082] The research results on the annealing temperature of small molecule carbazole phosphate (Me-4PACz) or polycarbazole phosphate (Poly-PACz) are shown in Figures 2, 3 and Table 1. Figure 2 is a current-voltage curve of polycarbazole phosphate perovskite solar cell as a function of annealing temperature, and Figure 3 is a current-voltage curve of carbazole phosphate small molecule perovskite solar cell as a function of annealing temperature. It can be clearly found that small molecule carbazole phosphate is more sensitive to annealing temperature, while polycarbazole material is not sensitive to annealing temperature.
[0083] Table 1 Device parameters of polycarbazole phosphate and carbazole phosphate small molecule perovskite solar cells at different annealing temperatures
[0084] The results of the study on the concentration / thickness of small molecule carbazole phosphate or polycarbazole phosphate are shown in Figures 4, 5 and Table 2. Figure 4 shows the current-voltage curve of the polycarbazole phosphate perovskite solar cell as a function of concentration; Figure 5 shows the current-voltage curve of the carbazole phosphate small molecule perovskite solar cell as a function of concentration. It can be clearly found that small molecule carbazole phosphate is more sensitive to concentration / thickness, while polycarbazole phosphate material is not sensitive to concentration / thickness.
[0085] Table 2 Device parameters of polycarbazole phosphate and carbazole phosphate small molecule perovskite solar cell at different concentrations
[0086] It can be seen that the perovskite solar cell based on polycarbazole phosphate can achieve a photoelectric conversion efficiency of 22.64%, which exceeds the control group based on polycarbazole phosphate small molecules, and the perovskite solar cell based on polycarbazole phosphate is insensitive to the concentration of polycarbazole phosphate and annealing temperature.
[0087] Example 6
[0088] The ITO conductive glass was placed in a UV-ozone cleaning machine for 15 minutes, and then a 5-10 nm thick polyphosphate carbazole was spin-coated on it, followed by a PM6:Y6 active layer, and finally a 5 nm PDINN was spin-coated and a 100 nm silver electrode was evaporated to complete the preparation of the organic solar cell.
[0089] Example 7
[0090] The FTO conductive glass was placed in a UV ozone cleaning machine for 15 minutes, and then polyphosphate carbazole (1 mg / ml) was scraped on it and annealed at 150 degrees Celsius. 0.7 FA 0.3 PbI3 perovskite polycrystalline film, after thermal annealing, 25nm C is evaporated on its surface 60 , 5nm BCP and 100nm copper electrodes are used to complete the fabrication of a perovskite solar cell. Figure 6 shows the current-voltage curve of the optimal perovskite solar cell with polycarbazole phosphate on an ITO / FTO substrate. Table 3 shows the device parameters of polycarbazole phosphate perovskite solar cells based on ITO and FTO. It can be clearly seen that polycarbazole phosphate achieves good photoelectric conversion efficiency on both ITO and FTO substrates.
[0091] Table 3 Device parameters of polyphosphate carbazole perovskite solar cells based on ITO and FTO
[0092] Example 8
[0093] Perovskite solar cells based on the small molecule carbazole phosphate (Me-4PACz) and polycarbazole phosphate (Poly-4PACz) were packaged and placed under a solar simulator for stability testing at the solar cell's maximum power point. After over 100 hours of testing (Figure 7), the polycarbazole-based perovskite solar cell showed no significant efficiency degradation, while the carbazole-based perovskite solar cell exhibited significant degradation, demonstrating that the polycarbazole-based material possesses superior light stability compared to the carbazole-based material.
Claims
1. A polyphosphoric acid carbazole material comprising a plurality of repeating units, characterized in that: The repeating unit structure is as follows: In the formula, the benzene ring on the phosphate carbazole unit does not contain or contains a substituent; When containing substituents, the benzene ring contains single or multiple independent substituents, which are selected from: 1)H; 2) halogen groups; 3) cyano; 4) alkyl; 5) Aromatic groups; 6) Cyclic groups; The value range of n is 1-40, the polymerization site of polycarbazole phosphate is at any position on the benzene ring, and the value range of its molecular weight is 300-10000000.
2. The polyphosphoric acid carbazole material according to claim 1, characterized in that: The alkyl group is selected from (C1-C40) straight-chain alkyl, (C3-C40) branched alkyl or (C3-C40) cycloalkyl; the annular group is used to annulate the benzene ring into a macrocycle such as naphthalene and anthracene; the halogen group is F, Cl, Br or I; the aromatic group is selected from one or more of aryl, heteroaryl, aryloxy, heteroaryloxy, arylcarbonyl, heteroarylcarbonyl, arylcarbonyloxy, heteroarylcarbonyloxy, aryloxycarbonyl or heteroaryloxycarbonyl; and the number of repeating units is 2-10000000.
3. The polyphosphoric acid carbazole material according to claim 1, characterized in that: The repeating unit structure is one of the following structural formulas: wherein m ranges from 2 to 10,000,000, and R1, R2, and R3 are H or the substituents mentioned above.
4. The method for preparing the polyphosphoric acid carbazole material according to claim 1, characterized in that: The steps include: Step 1, a halogenated phosphate carbazole is copolymerized in a solvent with or without the addition of other halogenated compounds; Step 2, adding halogenated silane and alcohol to carry out hydrolysis to obtain polyphosphoric acid carbazole material.
5. The preparation method according to claim 4, characterized in that: The other halogenated compounds are halogenated aromatic hydrocarbons or halogenated thiophenes with or without substituents; the aromatic group in the halogenated aromatic hydrocarbon is selected from one or more of aryl, heteroaryl, aryloxy, heteroaryloxy, arylcarbonyl, heteroarylcarbonyl, arylcarbonyloxy, heteroarylcarbonyloxy, aryloxycarbonyl or heteroaryloxycarbonyl; the halogenated phosphate carbazole is polymerized by itself without adding other halogenated compounds; when other halogenated compounds are added, the halogenated phosphate carbazole and the other halogenated compounds are polymerized; the mass ratio of phosphate carbazole to halogenated compound is 1:0.01-10.0, the polymerization reaction takes 0.1-72 hours, and the reaction temperature is 0-300°C.
6. The method for preparing the polyphosphoric acid carbazole material according to claim 4, characterized in that: The phosphate carbazole comprises one or more of the following unit structures: The value range of n is 1-40.
7. The method for preparing the polyphosphoric acid carbazole material according to claim 6, characterized in that: Rx is independently selected from: 1)H; 2) halogen groups; 3) cyano; 4) alkyl; 5) Aromatic groups; 6) Cyclic groups; The halogen group is F, Cl, Br or I; The alkyl group is selected from (C1-C40) straight chain alkyl, (C3-C40) branched chain alkyl or (C3-C40) cycloalkyl; In the alkyl group, one or more non-adjacent C atoms are optionally replaced by -O-, -S-, -C(O)-, -C(O-)-O-, -OC(O)-, -OC(O)-O-, -CR 0 =CR 00 - or -C≡C- substitution, where R 0 and R 00 are independently straight chain alkyl, branched chain alkyl or cycloalkyl; In the alkyl group, one or more H atoms are optionally replaced by F, Cl, Br, I or CN; The aromatic group is selected from aryl, heteroaryl, aryloxy, heteroaryloxy, arylcarbonyl, heteroarylcarbonyl, arylcarbonyloxy, heteroarylcarbonyloxy, aryloxycarbonyl or heteroaryloxycarbonyl, and has 4 to 30 ring atoms.
8. Application of polycarbazole phosphate materials in the preparation of optoelectronic device structures.
9. The use according to claim 8, characterized in that: The optoelectronic device structure is a solar cell, a field effect transistor, a photodetector, a radiation detector, and a light emitting diode. The solar cell includes an organic solar cell and a perovskite solar cell. The polyphosphoric acid carbazole material is used as a hole transport layer material in an organic solar cell or a perovskite solar cell, or is used for interface modification on the basis of an original hole transport layer.
10. The use according to claim 9, characterized in that: The battery structure is selected from one of the following:
Citation Information
Patent Citations
Hole transport layers for organic electroluminescent devices
CN101091417A
Triphenylamine conjugated polymer containing phosphate and application thereof
CN102399359A
Carbazole polymer
CN104066766A
Organic room-temperature phosphorescent polymer, preparation thereof and application of organic room-temperature phosphorescent polymer in X-ray imaging
CN114539472A
Self-assembled monomolecular layer hole transport material based on carbazole derivative and synthesis method and application thereof
CN114716476A