Method for producing member having recess structure, and member having recess structure
The method utilizes a catalyst material with polar functional groups and deep ultraviolet light to selectively etch surfaces, overcoming the limitations of conventional reactive ion etching in forming complex concave structures by achieving precise shape control and uniformity in concave structures.
Patent Information
- Application Number
- PCT/JP2024/012084
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional reactive ion etching methods face challenges in forming concave structures with complex shapes, particularly curved shapes, due to preferential etching on the opening side rather than the bottom surface, leading to non-uniform recess structures and mask material alteration.
A method involving the use of a catalyst material with polar functional groups on a surface exposed to deep ultraviolet light and fluorine-containing gases at elevated temperatures, which selectively etches the surface, allowing for the formation of concave structures with controlled etching rates and precise shape deviation.
Enables the easy formation of concave structures with predetermined deflections and uniform width along the depth direction, achieving high precision and preventing over-etching by controlling the etching rate through DUV irradiation conditions.
Smart Images

Figure JP2024012084_05122024_PF_FP_ABST
Abstract
Description
Method for manufacturing a member having a recessed structure and a member having a recessed structure
[0001] The present invention relates to a method for manufacturing a member having a recessed structure and a member having a recessed structure.
[0002] There is a need in various fields for microfabrication techniques that can form minute recessed structures on the surface of a sample. Various microfabrication techniques have been proposed and put to practical use.
[0003] One microfabrication technique is dry etching, in which reactants such as reactive gases, ions, and / or radicals are used to etch the surface of a sample.
[0004] For example, in reactive ion etching (RIE) methods, such as inductive coupled plasma-RIE (ICP-RIE), etching is performed by converting an etching gas into plasma and colliding it with a sample. It has been reported that such RIE methods enable extremely fine processing of samples (for example, Non-Patent Document 1).
[0005] JP 2012-42515 A
[0006] xiao Li, King Yuk Chan and Rodica Ramer, “Fabrication of Through via Holes in Ultra-Thin Fused SilicaWafers for Microwave and Millimeter-Wave Applications”, micromachines, 2018, 9, 138
[0007] In the field of microfabrication technology, it is preferable to be able to form recess structures of various shapes on the surface of a processing target object from the viewpoint of creating new optical members, etc.
[0008] However, the RIE method has a problem in that it is difficult to form recessed structures with complex shapes.
[0009] For example, Patent Document 1 describes a method for manufacturing a recess structure in which the extension axis is inclined obliquely with respect to the normal to the surface of the object to be processed by the above-mentioned RIE method.
[0010] However, in the described method, due to the etching characteristics of the RIE method, etching occurs preferentially on the opening side of the recess structure rather than on the bottom surface, which means that the recess structure tends to be wider near the opening, making it difficult to form a recess structure with a uniform width along the depth direction with high precision.
[0011] Furthermore, due to its characteristics, RIE simultaneously etches the mask material placed on the workpiece. Since the cross section of the mask material is usually rectangular or trapezoidal, etching from an oblique direction causes the shape of the mask material to change. This also creates the problem of preferential etching occurring on the opening side of the recessed structure rather than on the bottom surface.
[0012] Furthermore, with the method described in Patent Document 1, it is not easy to form a recess structure having a curved shape along the depth direction.
[0013] The present invention has been made in view of the above background, and an object of the present invention is to provide a manufacturing method that allows for relatively easy formation of a recess structure biased in a predetermined direction in a member, and to provide a member having such a recess structure.
[0014] The present invention provides a method for manufacturing a member having a recessed portion structure, the method comprising the steps of: (1) placing a catalyst material in a first region of a first surface of a workpiece, wherein the first surface is composed of elements whose fluoride boiling points are 550°C or less, and the catalyst material contains an organic compound having a polar functional group, and the catalyst material has, when viewed in a cross section of the catalyst material, i.e., a cross section perpendicular to the first surface, a first side surface having a first height H1 and a second side surface having a second height H2 that are opposed to each other, with the proviso that H1>0 μm and H2≧0 μm, and the height H1 is greater than the height H2; (2) irradiating the catalyst material with irradiation light containing deep ultraviolet light having a wavelength of 380 nm or less; and (3) exposing the workpiece to a fluorine-containing gas at 80°C or more. There is also provided a method in which, after step (3), a recess structure is formed below the first region, and the recess structure has a shape that, in the cross-sectional view, at the center of the first region, is biased toward the second side surface relative to a perpendicular line drawn from the first surface.
[0015] The present invention also provides a member having a recessed portion structure on a first surface, wherein the first surface contains at least one element selected from the group consisting of B, C, Si, P, S, Ti, V, Cr, Ge, As, Se, Nb, Mo, Tc, Ru, Rh, Sn, Sb, Te, I, Ta, W, Re, Os, Ir, Pt, and Au; the recessed portion structure has an opening formed on the first surface, a bottom surface, and a sidewall connecting the opening and the bottom surface; the recessed portion structure has a curved shape when viewed in a cross section of the recessed portion structure, i.e., a cross section perpendicular to the first surface; a ratio P2 / P1 of a dimension P2 of the bottom surface to a dimension P1 of the opening is equal to or greater than 0.99 and less than 1.1; and the center of the bottom surface is offset from the center of the opening with respect to an extension axis extending perpendicular to the first surface.
[0016] The present invention can provide a manufacturing method that allows for relatively easy formation of a recess structure biased in a predetermined direction in a member, and can also provide a member having such a recess structure.
[0017] FIG. 1 is a diagram schematically showing a reaction mechanism that may occur on the first surface of a workpiece when the organic compound does not have a polar functional group. FIG. 2 is a diagram schematically showing a reaction mechanism that may occur on the first surface of a workpiece when the organic compound has a polar functional group. FIG. 3 is a diagram schematically showing a reaction mechanism that may occur on the first surface of a workpiece when the organic compound has another polar functional group. FIG. 4 is a diagram showing the relationship between the processing temperature and the etching reaction rate during hydrogen fluoride (HF) gas etching of glass. FIG. 5 is a cross-sectional view schematically showing a process in the "basic etching technique". FIG. 6 is a cross-sectional view schematically showing a process in the "basic etching technique". FIG. 7 is a cross-sectional view schematically showing a state in which a pattern of catalytic material is provided on the first surface of a workpiece in a method according to one embodiment of the present invention. FIG. 8 is a cross-sectional view schematically showing a state in which etching progresses on the first surface of a workpiece in a method according to one embodiment of the present invention. FIG. 9 is a cross-sectional view schematically showing a state in which etching progresses on the first surface of a workpiece in a method according to one embodiment of the present invention. 11 is a perspective view showing a state in which a catalytic material is placed on a workpiece in a method for producing a member having a recessed structure according to an embodiment of the present invention. 12 is a diagram showing a cross section taken along line II in FIG. 11. 13 is a cross section showing an example of a workpiece after an etching process in a method for producing a member having a recessed structure according to an embodiment of the present invention. 14 is a schematic cross section taken along line II-II of the member according to an embodiment of the present invention shown in FIG. 14. 14 is a diagram showing a schematic cross section of a surface of a sidewall of a recessed structure in a member according to an embodiment of the present invention. 15 is a diagram showing a schematic cross section of a catalytic material formed in an embodiment of the present invention. 16 is a photograph showing an example of a cross section of a recessed structure according to an embodiment of the present invention (Sample 1). 17 is a photograph showing an example of a cross section of a recessed structure according to an embodiment of the present invention (Sample 2). 18 is a photograph showing an example of a cross section of a recessed structure according to an embodiment of the present invention (Sample 3). 19 is a photograph showing an example of a cross section of a recessed structure according to an embodiment of the present invention (Sample 4).
[0018] An embodiment of the present invention will be described below.
[0019] (Basic Etching Technology) As mentioned above, the conventional RIE method has a problem in that it is difficult to manufacture a member having a recessed structure that includes a complex shape along the depth direction.
[0020] In order to address these conventional problems, the present inventors have conducted extensive research and development and discovered a microfabrication technique that can form recessed structures having complex shapes, particularly curved shapes, along the depth direction.
[0021] Here, in order to better understand the method for manufacturing a member according to one embodiment of the present invention, first, a microfabrication technique (hereinafter referred to as "basic etching technique") that has been developed by the inventors of the present invention will be described.
[0022] The basic etching technique involves a process (hereinafter referred to as the "etching process") in which a workpiece having a catalytic material applied to a first surface thereof is exposed to a fluorine-containing gas at a processing temperature of 80° C. or higher. As will be described in detail later, by carrying out such an "etching process", the basic etching technique makes it possible to selectively etch the region on the first surface of the workpiece where the catalytic material is applied (hereinafter referred to as the "covered region").
[0023] Furthermore, in the basic etching technique, before an etching process is performed on an object to be processed, a catalytic material is irradiated with specific irradiation light, thereby controlling the etching rate in the subsequent etching process.
[0024] Here, the role of the catalyst material in the basic etching technique and the effect of the processing temperature will be explained.
[0025] It should be noted that the following description is based on the mechanism currently considered, but the actual phenomenon may occur through other mechanisms.
[0026] (Role of catalytic material) In the basic etching technique, the catalytic material includes an organic compound having a polar functional group. Such an organic compound having a polar functional group is thought to play a role in lowering the activation energy of fluoride formation on the surface of the workpiece.
[0027] This role will be explained below with reference to Figures 1 to 3. Figures 1 to 3 show a schematic diagram of the reaction that occurs on the surface of a workpiece on which a catalytic material is placed.
[0028] In the following description, the object to be treated is, for example, SiO 2 It is assumed that the surface to be processed (first surface) of the object to be processed is hydrogen-terminated.
[0029] First, FIG. 1 shows a schematic diagram of an etching mechanism that is assumed for the first surface of the object to be treated when the organic compound does not have a polar functional group.
[0030] SiO as the object to be treated 2 When hydrogen fluoride (HF) gas is supplied from the environment to the region where the catalyst material is provided on the surface, i.e., the “covered region,” HF molecules (a) nucleophilically attack Si atoms (b), as shown in (i).
[0031] However, in order for the Si atoms (b) to react with the F atoms on the surface of the workpiece, the OH groups (c) on the surface must interact with the H atoms of the HF molecules (a) to weaken the H-F bonds, as shown in (ii). In other words, unless energy is provided to break the H-F bonds in the HF molecules (a), the H 2 The Si—F bond (d) does not occur with the elimination of O (g).
[0032] However, in this reaction system, there is no substance that contributes to lowering the activation energy of the Si—F bond (d), so no significant etching reaction occurs in the coated region.
[0033] In this system, as in normal mask pattern processing, the etching rate tends to be higher in the areas of the workpiece that come into direct contact with HF gas, i.e., the areas on the surface where no catalytic material is installed (hereinafter referred to as "uncoated areas").
[0034] 2 is a schematic diagram showing a reaction mechanism on the first surface of the object to be treated when the organic compound has a polar functional group, where the polar functional group is assumed to be a hydroxy group.
[0035] In this case as well, when HF gas is supplied from the environment to the region coated with the catalytic material, HF molecules (a) undergo nucleophilic attack on Si atoms (b), as shown in (i).
[0036] In this case, however, in addition to this, the O atom in the −δ portion (e) of the polar functional group interacts with the H of the HF molecule (a), and the H atom in the +δ portion (f) of the polar functional group interacts with the OH group (c) on the surface.
[0037] Therefore, as shown in (ii), the H-F bond of the HF molecule (a) is weakened. The Si(b)-OH(c) bond is also weakened. This reduces the activation energy required for the bonding reaction between the Si atom and the F atom.
[0038] As a result, as shown in (iii), the H atom of the HF molecule (a) is taken by the O atom of the −δ part (e) of the polar functional group, and the H atom of the +δ part (f) reacts with the OH group on the surface to form H 2 Desorption of O(g) occurs.
[0039] This causes the Si atom (b) to bond with the fluorine atom. Finally, SiF is formed according to the following reaction formula (1): 4 and H 2 O is formed. SiO 2 +4HF → SiF 4 ↑ + 2H 2 O↑ (1) SiF produced by the reaction 4 and H 2 O is in a gaseous state at the treatment temperature and is quickly dispersed to the outside of the system.
[0040] By the above reaction mechanism, the area immediately below the area coated with the catalytic material in the object to be treated is selectively etched.
[0041] The above reaction is not limited to the case where the polar functional group contains a hydroxy group. For example, the same reaction can occur when the polar functional group contains at least one of an aldehyde group, a hydroxy group, a carboxy group, an amino group, a sulfo group, a thiol group, and an amide bond.
[0042] 2, the reaction mechanism has been described using an example in which the polar functional group of the organic compound contains an H atom. However, the polar functional group of the organic compound is not necessarily limited to one containing an H atom.
[0043] Figure 3 shows a schematic diagram of the reaction mechanism when the organic compound has another polar functional group. Here, the polar functional group is assumed to be a carbonyl group (>C=O) that does not have an H atom.
[0044] In this example, when HF gas is supplied from the environment to the catalytic material-coated region, the HF molecule (a) nucleophilically attacks the Si atom (b), as shown in (i). The O atom in the -δ portion (e) of the polar functional group interacts with the H atom of the HF molecule (a).
[0045] This weakens the H—F bond of the HF molecule (a), as shown in (ii).
[0046] Next, as shown in (iii), the H atom released from the HF molecule (a) by the O atom in the -δ portion (e) of the polar functional group bonds with the OH group (c), forming H 2 O(g) is generated.
[0047] In this case, too, the activation energy required for the bonding reaction between Si atoms and F atoms is reduced, resulting in the reaction shown in the above-mentioned reaction formula (1), and the area immediately below the coated region of the workpiece is selectively etched.
[0048] A similar reaction mechanism may occur, for example, when the polar functional group has at least one of a carbonyl group, a nitro group, a cyano group, an ether bond, and an ester bond.
[0049] Thus, in the basic etching technique, the presence of an organic compound with a polar functional group contained in the catalytic material promotes the fluoride production reaction in the coated region of the workpiece, allowing selective etching of the area directly below the coated region.
[0050] (Influence of Processing Temperature) Next, the influence of processing temperature will be described.
[0051] In the basic etching technique, the processing temperature is 80° C. or higher because, at temperatures below 80° C., proper etching selectivity does not occur between the coated and uncoated regions on the first surface of the workpiece.
[0052] The effect of the processing temperature will be explained in more detail below with reference to FIG.
[0053] FIG. 4 shows the relationship between the processing temperature and the etching reaction rate when etching glass with hydrogen fluoride (HF) gas, as obtained by the present inventors.
[0054] 4, the etching rate of glass gradually increases with temperature up to a processing temperature of 80° C. However, once the processing temperature reaches 80° C. or higher, the etching rate decreases rapidly. As a result, the etching rate peaks at temperatures below 80° C.
[0055] This phenomenon is thought to correspond to the association / non-association state of HF gas. That is, HF gas is in an association state below 80°C, but becomes non-associated (single molecule) at 80°C or higher. Furthermore, when HF gas is in an association state, the bonding strength of the H-F bond is relatively weak when viewed as a single molecule. Therefore, the F atom of the HF molecule is more likely to bond with the surface of the workpiece and form fluoride. It is thought that this behavior is why a high etching rate can be obtained at temperatures below 80°C.
[0056] In the basic etching technique, if the processing temperature is set to less than 80° C., the association state of the HF gas will have an effect, and the object will be etched in the uncoated area of the catalytic material, resulting in a decrease in the etching selectivity in the coated area due to the reaction mechanism described above.
[0057] In contrast, when the processing temperature is set to 80°C or higher, the high etching power of the associated HF gas can be suppressed in the non-coated region of the catalytic material. Furthermore, based on the above-mentioned reaction mechanism, etching of the workpiece is possible directly below the coated region. As a result, at processing temperatures of 80°C or higher, high etching selectivity can be obtained between the coated region and the non-coated region of the catalytic material. This also allows the coated region to be selectively etched using basic etching techniques.
[0058] (Formed Recess Structure) With basic etching techniques, recess structures having sidewalls extending substantially parallel to the perpendicular line to the surface of the object to be processed (hereinafter referred to as "vertical recess structures") can be formed relatively easily.
[0059] The reason for this will be explained below with reference to FIGS.
[0060] 5 and 6 show a schematic diagram of one step in the basic etching technique.
[0061] Fig. 5 shows a schematic diagram of a state in which a catalyst material 3 is placed on the surface of a workpiece 1. In Fig. 5 and Fig. 6, for convenience of illustration, the workpiece 1 and the catalyst material 3 are shown as being spaced apart from each other, but in reality, they are in contact with each other.
[0062] As described above, the object to be processed 1 is made of SiO 2 and the surface is assumed to be H-terminated.
[0063] The catalytic material 3 is an organic compound having a polar functional group, which is assumed to be an OH group in this example. By applying the catalytic material 3 to the surface of the workpiece 1, a coated region 8a and an uncoated region 8b are formed on the workpiece 1.
[0064] As described above, by exposing the workpiece 1 heated to 80° C. or higher to HF gas, etching proceeds selectively directly below the coating region 8 a where the catalytic material 3 is disposed, thereby forming a recessed structure directly below the coating region 8 a.
[0065] FIG. 6 shows a state in which etching of the object 1 has progressed to a certain extent and a recess structure 5 having a certain depth has been formed.
[0066] As described above, the catalytic material 3 is provided in the covering region 8a. Therefore, even as the etching reaction progresses, the catalytic material 3 remains on the bottom surface 6 of the recessed structure 5. That is, while the etching process continues, the bottom surface 6 of the recessed structure 5 continues to be in contact with the catalytic material 3. As a result, the bottom surface 6 of the recessed structure 5 continues to be etched by the above-described reaction mechanism, and the etching of the bottom surface 6 continues to progress in the depth direction.
[0067] On the other hand, when attention is focused on the sidewall 7 of the recess structure 5, once etching begins, the etching reaction proceeds in the portion of the sidewall 7 that is in contact with the catalytic material 3 according to the mechanism described above. More precisely, only the portion of the workpiece 1 that is in contact with the side surface of the catalytic material 3 is etched. As a result, a recess structure 5 defined by the sidewall 7 is formed in the portion that is in contact with the side surface of the catalytic material 3.
[0068] However, as the catalytic material 3 continues to descend deeper, after a certain point, the upper portion of the sidewall 7 no longer comes into contact with the side surface of the catalytic material 3. Hereinafter, such a sidewall 7 that is no longer in contact with the side surface of the catalytic material 3 will be referred to as the "first sidewall portion 7a."
[0069] As described above, etching does not substantially proceed in areas such as the uncoated region 8b where the catalytic material 3 is not present. In other words, the etching reaction occurs in the workpiece 1 only when the workpiece 1 is in contact with the catalytic material 3, and does not occur in other states. Therefore, once a portion of the sidewall 7, such as the first sidewall portion 7a, comes out of contact with the catalytic material 3, etching virtually stops thereafter.
[0070] In the basic etching technique, as a result of the etching stopping action at the first sidewall portion 7a that does not come into contact with the catalytic material 3, etching of the workpiece 1 proceeds selectively only directly below the catalytic material 3, ultimately forming a vertical recess structure.
[0071] That is, in the basic etching technique, a recess structure 5 is formed in which the area of the opening and the area of the bottom surface are substantially equal.
[0072] Furthermore, the basic etching technique includes a step of irradiating a catalytic material with irradiation light containing deep ultraviolet (DUV) rays having a wavelength of 380 nm or less (hereinafter referred to as a "DUV irradiation process") before performing an etching process on the object to be treated. When such a DUV irradiation process is added, it becomes possible to control the etching rate of the object to be treated during the subsequent etching process.
[0073] In the basic etching technique, the etching rate of the object to be treated can be controlled by performing an etching process after a DUV irradiation process, which is thought to be because the number of polar functional groups changes due to the DUV irradiation process.
[0074] This phenomenon will be described below with reference to FIG. 5 again.
[0075] As shown in FIG. 5, when the catalytic material 3 is placed on the surface of the object to be treated 1, a coated region 8a and an uncoated region 8b are formed on the object to be treated 1.
[0076] As described above, in the coated region 8a, the presence of the catalytic material 3 lowers the reaction barrier in reaction formula (1), and etching proceeds selectively in the coated region 8a during the etching process.
[0077] However, when the DUV irradiation process is performed, exposure to deep ultraviolet light with a wavelength of 380 nm or less results in a crosslinking reaction within the catalytic material 3. The crosslinking reaction reduces the number of polar functional groups (e.g., C—OH groups) contained in the catalytic material 3. This is thought to weaken the effect of reducing the reaction barrier in the reaction of the aforementioned reaction formula (1) during the subsequent etching process, resulting in a decrease in the etching rate.
[0078] In this case, the number of polar functional groups contained in the catalytic material 3 is also changed by changing the irradiation intensity of the irradiation light containing deep ultraviolet rays and the irradiation time of the irradiation light in the DUV irradiation process. Therefore, by changing the irradiation conditions in the DUV irradiation process, the etching rate of the workpiece 1 in the etching process can be controlled.
[0079] For example, when forming a relatively shallow recess structure, the intensity of the irradiation light in the DUV irradiation process may be increased and / or the irradiation time may be extended, which significantly reduces the etching rate in the etching process and prevents over-etching of the workpiece.
[0080] Furthermore, when forming a relatively deep recess structure, the intensity of the irradiation light in the DUV irradiation process may be weakened and / or the irradiation time may be shortened, thereby increasing the etching rate in the etching process and shortening the processing time.
[0081] Thus, the basic etching technique allows for the fabrication of components with vertical recess structures at various etching rates.
[0082] (New Microfabrication Technology Developed by the Present Inventors) The new microfabrication technology developed by the present inventors is based on this "basic etching technology."
[0083] That is, one embodiment of the present invention provides a method for manufacturing a member having a recessed portion structure, the method comprising the steps of: (1) placing a catalyst material in a first region of a first surface of a workpiece, wherein the first surface is composed of elements whose fluoride boiling points are 550°C or less, and the catalyst material contains an organic compound having a polar functional group, and the catalyst material has, when viewed in a cross section of the catalyst material, i.e., a cross section perpendicular to the first surface, a first side surface having a first height H1 and a second side surface having a second height H2 that are opposed to each other, where H1>0 μm, H2≧0 μm, and the height H1 is greater than the height H2; (2) irradiating the catalyst material with irradiation light containing deep ultraviolet light having a wavelength of 380 nm or less; and (3) exposing the workpiece to a fluorine-containing gas at 80°C or more. There is also provided a method in which, after step (3), a recess structure is formed below the first region, and the recess structure has a shape that, in the cross-sectional view, at the center of the first region, is biased toward the second side surface relative to a perpendicular line drawn from the first surface.
[0084] The shape of the recess structure that is biased toward the second side surface may be a linear shape or a curved shape.
[0085] In one embodiment of the present invention, the catalytic material placed on the first surface has, in a cross-sectional view of the catalytic material, a first side and a second side that face each other, and is characterized in that the height H1 of the first side is greater than the height H2 of the second side (H2≧0 μm).
[0086] Here, "a cross-sectional view of (the catalyst material)" means that the target member (for example, the catalyst material) is viewed in a cross section perpendicular to the first surface of the treatment target.
[0087] Alternatively, the first side of the catalyst material may have a height H1 of a certain positive value, while the second side may have a height H2 of 0. That is, in this application, the height H1 is expressed as H1>0 μm, whereas the height H2 is expressed as H1≧0 μm. Note that when H2=0, such a catalyst material may have, for example, a substantially triangular cross section.
[0088] When a catalytic material of this type is applied and then the aforementioned DUV irradiation process and etching process are performed, a recess structure having a shape biased toward the second side surface can be formed in the workpiece.
[0089] This mechanism will be described below with reference to FIGS.
[0090] 7 to 9 are schematic diagrams showing a process for forming a recess structure on a first surface of a processing target object in one embodiment of the present invention.
[0091] Fig. 7 shows a state in which a pattern of catalytic material 3 has been formed on the first surface 12 of the workpiece 1. Fig. 8 shows the state after the etching process has started (etching time t1) for the workpiece 1 after the DUV irradiation process. Fig. 9 shows the state in which the etching process for the workpiece 1 has progressed further (etching time t2, t2>t1).
[0092] In the example shown in Figure 7, catalytic material 3 having a triangular cross-sectional shape is provided on first surface 12. Catalytic material 3 has a top surface 18 and a bottom surface 19. The height of top surface 18 decreases continuously from a maximum value on the left side of Figure 7 to a minimum value (zero) on the right side.
[0093] 7 can also be said to have a configuration in which the catalyst material 3 has a first side surface 17A with a height H1 on the first side (left side of FIG. 7) and a second side surface 17B with a height H2 on the second side (right side of FIG. 7). However, in the illustrated example, H2=0. That is, while H1>0 in the present application, H2≧0.
[0094] In this state, when an etching process is performed on the object 1 to be processed after the DUV irradiation process of the catalytic material 3, the first surface 12 is etched by the catalytic material 3 in the direction of the arrow F1.
[0095] 7 , when the height of the catalytic material 3 is set to H1>H2, the amount of polar functional groups contained in the catalytic material 3 differs between the first side surface 17A and the second side surface 17B. This causes the etching rate of the workpiece 1 to differ on both sides. That is, the etching rate is higher on the first side surface 17A, which has more polar functional groups, than on the second side surface 17B.
[0096] As a result, as the etching process progresses, the recessed structure 50 formed will be deeper directly beneath the first side 17A of the catalytic material 3 than directly beneath the second side 17B, as shown in FIG.
[0097] As the etching process continues, the difference in etching rate between the first side surface 17A and the second side surface 17B becomes more pronounced. Therefore, as shown in FIG. 9 , the recessed structure 50 formed has a sidewall 57A corresponding to the first side surface 17A of the catalytic material 3 longer than a sidewall 57B corresponding to the second side surface 17B. As a result, the recessed structure 50 has a shape biased toward the second side surface 17B. For example, in the example shown in FIG. 9 , the recessed structure 50 has a non-linear shape curved toward the second side surface 17B.
[0098] As a result of the above, in one embodiment of the present invention, a member can be manufactured that has, on the underside of the first surface 12, a recess structure 5 that is biased in a predetermined direction.
[0099] 9, due to the above-described mechanism, the areas of the bottom surface 56 of the recessed portion structure 50 and the opening 52 are substantially the same at any stage of the etching process. That is, in one embodiment of the present invention, the recessed portion structure 50 formed has a characteristic that the width dimension is substantially constant in the extension direction in a cross-sectional view.
[0100] (Method for manufacturing a member having a recessed portion structure according to one embodiment of the present invention) Next, a method for manufacturing a member having a recessed portion structure according to one embodiment of the present invention will be described in more detail with reference to FIGS.
[0101] FIG. 10 shows a schematic flow of a method for manufacturing a member having a recessed portion structure according to one embodiment of the present invention (hereinafter simply referred to as "first method").
[0102] As shown in FIG. 10 , the first method includes: (1) providing a workpiece having a first surface (S110), the first surface containing an element whose fluoride boiling point is 550° C. or less; (2) placing a catalyst material in a first region of the first surface of the workpiece, the catalyst material containing an organic compound having a polar functional group; the catalyst material having, in a cross-sectional view of the catalyst material, a first side surface having a first height H1 and a second side surface having a second height H2 facing each other; the height H1 of the first side surface (H1>0 μm) being higher than the height H2 of the second side surface (H2≧0 μm); (3) irradiating the catalyst material with irradiation light including deep ultraviolet (DUV) rays having a wavelength of 380 nm or less (S130); and (4) exposing the workpiece to a fluorine-containing gas at 80° C. or higher (S140).
[0103] Each step will be explained below.
[0104] (Step S110) First, an object to be processed is prepared.
[0105] The object to be processed may be made up of a single member or multiple members.
[0106] When the object to be treated is made up of a single member, the object to be treated is made up of an element that forms a fluoride having a boiling point of 550° C. or less by reacting with fluorine (F).
[0107] For example, the object to be treated may contain at least one element selected from the group consisting of B, C, Si, P, S, Ti, V, Cr, Ge, As, Se, Nb, Mo, Tc, Ru, Rh, Sn, Sb, Te, I, Ta, W, Re, Os, Ir, Pt, and Au. The object to be treated may further contain at least one element selected from the group consisting of H, N, Cl, Br, and O.
[0108] In particular, the object to be treated is preferably made of an element that reacts with fluorine to form a fluoride having a boiling point of 200° C. or less.
[0109] For example, silicon (Si) is converted into the fluoride SiF 4 The boiling point of the silicon-containing substance is −86° C., and the silicon-containing substance can be suitably used as the substance to be treated in the first method.
[0110] Al and Ca are fluorides (AlF 3 ) and (CaF 2 ) has a boiling point exceeding 550° C. Therefore, Al and Ca cannot be said to be elements that react with fluorine (F) to form fluorides having a boiling point of 550° C. or lower.
[0111] The object to be processed may be, for example, a quartz glass substrate, a quartz substrate, or a silicon substrate.
[0112] On the other hand, when the object to be treated is composed of a laminate of a plurality of members, the object to be treated contains an element whose fluoride boiling point is 550° C. or less on the outermost surface (corresponding to the "first surface" in this application).
[0113] As mentioned above, such elements may be selected from the group consisting of, for example, B, C, Si, P, S, Ti, V, Cr, Ge, As, Se, Nb, Mo, Tc, Ru, Rh, Sn, Sb, Te, I, Ta, W, Re, Os, Ir, Pt, and Au. The first surface may further include at least one element selected from the group consisting of H, N, Cl, Br, and O.
[0114] For example, the object to be processed may have one or more films disposed on a substrate, and the outermost film may satisfy the above-described characteristics. Alternatively, the entirety of the multiple films may satisfy the above-described characteristics.
[0115] Such a film may be, for example, SiO 2 , Si 3 N 4 and SiC.
[0116] Alternatively, the substrate may have the above-described characteristics in addition to the film. In this case, the first method can be used to manufacture a member having a recessed structure formed even inside the substrate. The substrate may be, for example, a quartz glass substrate, a quartz substrate, or a silicon substrate.
[0117] In the following description, to avoid complication, it is assumed that the object to be processed is made of a single piece of quartz glass, and that a recess structure is formed on a first surface of the quartz glass.
[0118] (Step S120) Next, a catalytic material is applied to a first surface of the object to be processed in a predetermined area of the first surface.
[0119] The catalyst material includes an organic compound having a polar functional group, which may include at least one selected from the group consisting of a hydroxy group, an aldehyde group, a carboxy group, an amino group, a sulfo group, a thiol group, an amide bond, a carbonyl group, a nitro group, a cyano group, an ether bond, and an ester bond.
[0120] Representative examples of such organic compounds include phenolic resins, acrylic resins, and methacrylic resins.
[0121] The catalyst material may consist solely of the organic compound having the polar functional group described above, or may be provided as a mixture with other additives.
[0122] In the latter case, the catalyst material may include a solvent, a binder, and / or particulates, etc.
[0123] The method for disposing the catalyst material is not particularly limited.
[0124] The catalyst material may be applied to the first surface of the object to be processed by, for example, a coating method, a printing method, a spin coating method, or a spray method.
[0125] FIG. 11 is a schematic diagram showing the state in which the catalyst material is placed on the object to be treated.
[0126] 11, the workpiece 110 has a first surface 112 and a second surface 114. The catalytic material 130 is disposed on a portion of the first surface 112 of the workpiece 110.
[0127] 11, the catalytic material 130 is disposed as a pattern 131 of multiple parallel lines. However, this is merely an example, and the catalytic material 130 may be disposed in any manner depending on the required recess structure. The catalytic material 130 may be disposed, for example, as a single straight line. Alternatively, the catalytic material 130 may be disposed, for example, as a pattern of circular dots or as a single circular dot.
[0128] According to the above definition, the area of the first surface 112 where the catalyst material 130 is provided is referred to as a coated area 140a, and the other area is referred to as a non-coated area 140b.
[0129] FIG. 12 is a schematic diagram showing a part of a cross section taken along line II in FIG.
[0130] As shown in FIG. 12, each catalyst material 130 has a shape in which the thickness (height) differs between the left and right sides in cross section.
[0131] That is, each catalyst material 130 has a top surface 118, a bottom surface 119, and a first side surface 117A and a second side surface 117B of different heights. The height H1 of the first side surface 117A is configured to be higher than the height H2 of the second side surface 117B. Therefore, the top surface 118 of the catalyst material 130 has an inclined surface with the second side surface 117B side descending.
[0132] However, the shape of the catalyst material 130 is not particularly limited as long as the height H1 is greater than the height H2. For example, the catalyst material 130 may have various shapes, such as a trapezoid rotated 90 degrees as shown in Fig. 12 in cross section, or a triangle as shown in Fig. 7 above.
[0133] Furthermore, in a cross-sectional view, the upper surface 118 of the catalytic material 130 does not necessarily have to be a straight line connecting the apex of the first side surface 117A and the apex of the second side surface 117B. For example, the upper surface 118 of the catalytic material 130 may be non-linear, such as a downwardly convex curve or an upwardly convex curve, in a cross-sectional view. Alternatively, the upper surface 118 may have one or more steps.
[0134] Here, in a cross-sectional view of the catalyst material 130, the angle φ (0°<φ<90°) formed between the straight line E connecting the first side surface 117A and the second side surface 117B (which coincides with the upper surface 118 in the example shown in Figure 12) and the first surface 112 may be in the range of 1° to 80°.
[0135] φ is preferably in the range of 3° to 50°, and more preferably in the range of 5° to 15°.
[0136] Furthermore, the width W (see FIG. 12) of the catalyst material 130 is not particularly limited, but is, for example, in the range of 0.1 μm to 100 μm, and preferably in the range of 0.3 μm to 50 μm.
[0137] (Step S130) Next, the catalyst material 130 is irradiated with irradiation light. The irradiation light includes deep ultraviolet (DUV) light having a wavelength of 380 nm or less. The wavelength of the deep ultraviolet light may be in the range of 200 nm to 365 nm.
[0138] Typically, the illumination light is emitted from a light source, which may emit light of a single wavelength (or a single range of wavelengths) or multiple wavelengths (or multiple ranges of wavelengths).
[0139] The irradiation conditions, such as the irradiation intensity and irradiation time of the irradiation light, are determined based on the etching rate adopted in the subsequent step S140. That is, the higher the irradiation intensity of the irradiation light and the longer the irradiation time, the lower the maximum etching rate of the object to be processed in step S140.
[0140] However, the degree of deflection of the recessed structure formed after step S140 is determined by the difference in etching rate due to the difference in the amount of polar functional groups contained on both sides of the catalytic material (the side of side 17A and the side of second side 17B). Therefore, even if the intensity of DUV irradiation irradiated onto the entire surface of the catalytic material is changed, the degree of deflection of the recessed structure itself does not change much.
[0141] For example, the irradiation amount P (mJ / cm 2 ) is 20 mJ / cm 2 It may be more than that.
[0142] Here, the irradiation amount P of the irradiation light is expressed by the following formula (2): Irradiation amount P (mJ / cm 2 ) = Irradiation intensity of lamp A (mW / cm 2 ) × irradiation time (sec) (2) (Step S140) Next, the object 110 to be processed on which the catalytic material 130 has been placed is placed in a processing chamber. Thereafter, the inside of the processing chamber is heated to a predetermined temperature and processing gas is supplied for the etching process of the object to be processed.
[0143] The processing gas contains hydrogen fluoride gas or fluorine gas. For example, the processing gas may be adjusted to a predetermined concentration using a carrier gas such as argon gas or nitrogen gas. In this case, the concentration of the hydrogen fluoride gas or fluorine gas may be in the range of 0.1 vol % to 100 vol %, for example.
[0144] As mentioned above, the processing temperature is 80° C. or higher. The actual processing temperature varies depending on the elements contained in the object 110 (particularly the first surface 112) and the type and depth of the recessed structure, but is typically in the range of 200° C. to 450° C., and preferably in the range of 250° C. to 400° C. By setting the processing temperature to 450° C. or lower, it is possible to suppress the deterioration of the organic compounds contained in the catalyst material 130.
[0145] As described above, when the workpiece 110 is etched under such an environment, the reaction represented by the above-described reaction formula (1) occurs in the coating region 140a. The fluoride and water produced by the reaction are vaporized and dissipated outside the system. As a result, a recessed structure biased in a predetermined direction is formed in the coating region 140a of the first surface 112.
[0146] FIG. 13 shows a schematic cross section of an example of the object 110 after etching.
[0147] As shown in FIG. 13, in the first method, after step S140, a curved recess structure 150 biased to the right may be formed.
[0148] Thereafter, a step may be performed to remove the catalyst material 130 remaining on the bottom surface of the recess structure 150. For example, the catalyst material 130 may be removed by cleaning the workpiece 110 with an acid solution, an alkaline solution, an organic solvent, a corrosive gas, or plasma.
[0149] Through the above steps, the member 100 having the recessed structure 150 biased in a predetermined direction on the first surface 112 can be manufactured.
[0150] The depth of the recessed structure 150 is, for example, 10 μm or more, and may be 15 μm or more.
[0151] (Member Having a Recessed Structure According to an Embodiment of the Present Invention) Next, a member having a recessed structure according to an embodiment of the present invention will be described with reference to FIGS.
[0152] Fig. 14 shows a perspective view of a member having a recess structure according to one embodiment of the present invention (hereinafter referred to as "first member 300"), and Fig. 15 shows a schematic enlarged cross-sectional view of first member 300 taken along line II-II of Fig. 14.
[0153] 14, the first member 300 has a first surface 302 and a second surface 304 that face each other. The first member 300 also has a recessed structure 350 on the side of the first surface 302.
[0154] 14, the first surface 302 and the second surface 304 of the first member 300 are substantially rectangular. However, the shapes of the first surface 302 and the second surface 304 are not particularly limited.
[0155] 14, two recessed structures 350 are formed on the first surface 302, and the two recessed structures 350 are arranged parallel to each other. Each recessed structure 350 has a linear opening extending in one direction.
[0156] However, this is merely an example, and the number, shape, and arrangement of the recessed structures 350 are not particularly limited.
[0157] 15, the recessed structure 350 has an opening 352 in the first surface 302. The recessed structure 350 also has a bottom surface 356 and a sidewall 357.
[0158] In other words, the recess structure 350 is defined by the opening 352 , the bottom surface 356 and the sidewalls 357 .
[0159] Here, in the first member 300, the recessed structure 350 has a shape that is biased in a predetermined direction. Specifically, the recessed structure 350 has a sidewall 357 that does not extend parallel to the vertical direction but is biased to the right, and the sidewall 357 of the recessed structure 350 has a curved shape.
[0160] However, when viewed from a cross section perpendicular to the first surface 302 (i.e., a cross-sectional view), the recess structure 350 has the characteristic that the dimension P1 of the opening 352 (which may be considered to be the area of the opening 352) and the dimension P2 of the bottom surface 356 (which may be considered to be the area of the bottom surface 356) are substantially equal.
[0161] Specifically, the ratio P2 / P1 is equal to or greater than 0.90 and less than 1.1, and it is particularly preferable that the ratio P2 / P1 is in the range of 0.94 to 1.05.
[0162] Such a first member 300 can be manufactured by, for example, the first method described above.
[0163] In the first member 300, the recessed structure 350 may have a depth of 10 μm or more.
[0164] 15, the recessed portion structure 350 may have a form in which the angle α (0°<α<180°) of the sidewall 357 with respect to a plane parallel to the first surface 302 changes continuously from the opening 352 to the bottom surface 356. The angle α means the angle between the horizontal plane and a tangent to the sidewall 357 passing through the "outside" of the recessed portion structure 350. In the present application, the angle α of the sidewall 357 measured at the intersection of the sidewall 357 and the bottom surface 356 as shown in FIG. 15 is particularly referred to as "α b "
[0165] Angle α b can be any value, for example, in the range of 10° to 80°.
[0166] In particular, the recess structure 350 may have a curved shape in which the center of the opening 352 and the center of the bottom surface 356 cannot be connected by a straight line in a cross-sectional view, as shown in FIG. 21 described later.
[0167] The first member 300 is characterized in that the surface constituting the sidewall 357 of the recess structure 350 is relatively smooth and has a surface roughness Ra of 5 nm or less. In particular, the surface roughness Ra of the sidewall 357 is preferably 4.5 nm or less, and more preferably 4.0 nm or less.
[0168] This feature will be explained below.
[0169] 5 and 6, in the first method based on the basic etching technique, the covered region 8a is selectively etched by the catalytic material 3 placed on the covered region 8a. As long as the relationship between the catalytic material 3 and the covered region 8a continues, the recess structure 5 continues to grow in the depth direction.
[0170] In the case of such an etching mechanism, the sidewalls 7 of the recessed structure 5 formed by etching are affected by the state of the side surfaces of the catalyst material 3 with which the sidewalls 7 come into contact.
[0171] In general, the side surface of the catalyst material 3 is considered to be a relatively smooth surface with few irregularities. Reflecting the influence of such irregularities on the side surface of the catalyst material 3, the side wall 7 of the recessed structure 5 also has a relatively smooth surface. As a result, it is considered that the side wall 7 of the recessed structure 5 has a surface with significantly reduced surface roughness.
[0172] Such smoothness is significant and not observed in conventionally etched materials. For example, in a typical RIE process, the sidewalls of recesses can have relatively large irregularities due to the impact of ion bombardment during processing.
[0173] The first member 300 may also be characterized in that the sidewall 357 has a streak pattern that runs along the extension direction of the recessed structure 350 .
[0174] This feature will be described below with reference to FIG.
[0175] 16 is a schematic diagram showing the surface configuration of the sidewall 357 of the recess structure 350. In FIG. 16, a part of the surface of the sidewall 357 is shown schematically.
[0176] As shown in FIG. 16, in the first member 300, a continuous stripe (hereinafter referred to as a "continuous stripe") 380 is formed on the side wall 357 of the recessed portion structure 350, continuing from the opening 352 to the bottom surface 356.
[0177] 16 shows three continuous streaks 380. However, this is merely an example, and the number of continuous streaks 380 is not particularly limited.
[0178] Such a pattern of continuous streaks 380 is also thought to be formed by the mechanism described above.
[0179] That is, as shown in FIG. 6, the sidewall 7 of the recess structure 5 formed by etching in the basic etching technique is affected by the state of the side surface of the catalyst material 3 with which the sidewall 7 comes into contact.
[0180] Furthermore, in the first method, the catalyst material 3 having such irregularities on the side surface advances along the depth direction of the recess structure 5 to the bottom surface 6 of the recess structure 5. Therefore, a continuous stripe pattern corresponding to such irregularities is likely to be formed on the side wall 7 of the finally obtained recess structure 5.
[0181] As a result, it is believed that a continuous streak 380 is formed on the side wall 357 along the depth direction.
[0182] (Other Features of the First Member 300) The first member 300 may be a single member or may be configured with multiple members.
[0183] When the first member 300 is made of a single material, the first member 300 is made of an element that reacts with fluorine (F) to form a fluoride having a boiling point of 550° C. or less.
[0184] For example, the first member 300 may contain at least one element selected from the group consisting of B, C, Si, P, S, Ti, V, Cr, Ge, As, Se, Nb, Mo, Tc, Ru, Rh, Sn, Sb, Te, I, Ta, W, Re, Os, Ir, Pt, and Au. The object to be processed may further contain at least one element selected from the group consisting of H, N, Cl, Br, and O.
[0185] When the first member 300 is configured from a single member, the first member 300 may be, for example, a quartz glass substrate or a quartz crystal substrate.
[0186] On the other hand, when the first member 300 is made up of a plurality of members, the first member 300 contains, on the first surface 302, an element whose fluoride has a boiling point of 550° C. or less.
[0187] As mentioned above, such elements may be selected from the group consisting of, for example, B, C, Si, P, S, Ti, V, Cr, Ge, As, Se, Nb, Mo, Tc, Ru, Rh, Sn, Sb, Te, I, Ta, W, Re, Os, Ir, Pt, and Au. Additionally, first surface 302 may further include at least one element selected from the group consisting of H, N, Cl, Br, and O.
[0188] For example, the first member 300 may have one or more films disposed on a substrate material, with the outermost film satisfying the aforementioned characteristics, or all of the multiple films may satisfy the aforementioned characteristics.
[0189] Such a film may be, for example, SiO 2 , Si 3 N 4 Alternatively, the substrate material, along with the film, may also have the aforementioned characteristics.
[0190] The first member 300 having these characteristics can be used in a variety of applications, such as MEMS devices, microfluidic devices, semiconductor devices, optical devices, metasurface devices, resin molding molds, window glass, and cover glass.
[0191] Examples of the present invention will be described below, with Examples 1 to 4 being examples.
[0192] Example 1 A recess structure was formed on one surface (first surface) of an object to be processed by the following method.
[0193] First, a quartz glass substrate was prepared as the workpiece. A coating solution containing a catalyst material was also prepared. The catalyst material was an i-line resist, which was mixed with a solvent (ethyl lactate, n-butyl acetate) to prepare the coating solution.
[0194] The i-line resist used contains a novolac resin represented by the following chemical formula:
[0195] Therefore, the i-line resist has a hydroxy group as a polar functional group.
[0196] Next, the coating liquid was applied to the first surface of the substrate by spin coating.
[0197] A line pattern of catalytic material was then deposited on the first surface of the substrate by grayscale exposure and subsequent development.
[0198] FIG. 17 shows a schematic cross section of the formed catalyst material.
[0199] 17, catalytic material 430 has a rectangular cross section, like a trapezoid rotated 90 degrees. That is, catalytic material 430 has first and second side surfaces 417A and 417B facing each other, and a top surface 418.
[0200] The distance between the first side surface 417A and the second side surface 417B, i.e., the width W, is 10 μm. The height H1 of the first side surface 417A is approximately 1.0 μm, and the height H2 of the second side surface 417B is approximately 0.5 μm. The inclination angle of the top surface 418, i.e., the angle θr, is 2.9°.
[0201] Next, the catalyst material was irradiated with light using a low-pressure mercury lamp (hereinafter referred to as "lamp A").
[0202] Lamp A is a DUV lamp with a dominant wavelength of 254 nm, and the irradiation dose P to the catalyst material is 72000 mJ / cm 2 It was decided.
[0203] Next, the substrate was cut into pieces measuring approximately 10 mm x 10 mm, and the cut samples were placed in a processing chamber with the catalyst material side facing upward. Gas etching of the samples was carried out in the processing chamber. The processing gas was a mixture of nitrogen gas and hydrogen fluoride gas (HF / N 2 The treatment temperature was 250° C. and the treatment time was 40 minutes.
[0204] After the etching process, a recessed structure was formed on the surface. The resulting processed object is referred to as "Sample 1."
[0205] Example 2 A recess structure was formed on the first surface of a substrate using a method similar to that of Example 1. However, in Example 2, the shape of the catalyst material was changed from that of Example 1 to form the recess structure. Specifically, in Figure 17, the inclination angle θr of the upper surface 418 was set to 5.7°, and the height H2 of the second side surface 417B was set to 0. Therefore, the cross section of the catalyst material was triangular.
[0206] After the etching process, a recessed structure was formed on the surface. The resulting processed object is referred to as "Sample 2."
[0207] Example 3 A recess structure was formed on the first surface of the substrate by the same method as in Example 2. However, in Example 3, unlike Example 2, the irradiation amount of the irradiation light was 144,000 mJ / cm 2 2 It was decided.
[0208] After the etching process, a recessed structure was formed on the surface. The resulting processed object is referred to as "Sample 3."
[0209] Example 4: A recessed structure was formed on the first surface of a substrate using a method similar to that of Example 1. However, in Example 4, the shape of the catalyst material was changed from that of Example 1 to form the recessed structure. Specifically, in FIG. 17, the inclination angle θr of the upper surface 418 was set to 11.3°, and the height H2 of the second side surface 417B was set to 0. Therefore, the cross section of the catalyst material was triangular. The width of the catalyst material was 5 μm.
[0210] In Example 4, the dose P of the irradiated light was changed from that in Example 1 to form the recessed structure.
[0211] After the etching process, a recessed structure was formed on the surface. The resulting processed object is referred to as "Sample 4."
[0212] (Evaluation) In each sample, the cross section of the recessed structure was observed with a scanning electron microscope (SEM) and various dimensions of the recessed structure were measured. In particular, the angle α of the recessed structure defined as above was b and the ratio P2 / P1 was measured.
[0213] Table 1 below shows the preparation conditions and evaluation results of each sample.
[0214] 18 to 21 show examples of cross sections of recess structures obtained in Samples 1 to 4, respectively.
[0215] As shown in these figures, it can be seen that the recessed structures formed in all samples are biased to the right. In particular, Samples 1, 3, and 4 have prominent curved recessed structures.
[0216] Furthermore, from Table 1, it can be seen that in each sample, the ratio P2 / P1 was extremely close to 1. This indicates that the recessed structure formed in each sample had a substantially constant cross-sectional shape along the stretching direction.
[0217] (Aspects of the Invention) The present invention includes the following aspects.
[0218] (Aspect 1) A method for manufacturing a member having a recessed portion structure, comprising: (1) a step of placing a catalyst material in a first region of a first surface of a workpiece, wherein the first surface is composed of an element whose fluoride boiling point is 550°C or less, and the catalyst material includes an organic compound having a polar functional group, and the catalyst material has a first side surface having a first height H1 and a second side surface having a second height H2 that are opposed to each other when viewed in a cross section of the catalyst material, i.e., a cross section perpendicular to the first surface, where H1>0 μm, H2≧0 μm, and the height H1 is greater than the height H2; (2) a step of irradiating the catalyst material with irradiation light that includes deep ultraviolet light having a wavelength of 380 nm or less; and (3) a step of exposing the workpiece to a fluorine-containing gas at 80°C or more. After the step (3), a recess structure is formed below the first region, and the recess structure has a shape that, in the cross-sectional view, at the center of the first region, is biased toward the second side surface relative to a perpendicular line drawn from the first surface.
[0219] (Aspect 2) The method according to Aspect 1, wherein in step (1), the catalyst material has an angle φ (0°<φ<90°) φ between the first surface and a line connecting the top of the first side surface and the top of the second side surface in the cross-sectional view, in the range of 1° to 80°.
[0220] (Embodiment 3) The method according to embodiment 1 or 2, wherein the catalyst material has a width of 0.1 μm to 100 μm in the cross-sectional view.
[0221] (Aspect 4) The method according to any one of aspects 1 to 3, wherein the catalyst material has an upper surface whose height monotonically decreases from the first side surface to the second side surface in the cross-sectional view.
[0222] (Aspect 5) The method according to any one of aspects 1 to 4, wherein the catalytic material has a rectangular or triangular shape in cross section.
[0223] (Aspect 6) The method according to any one of Aspects 1 to 5, wherein the polar functional group includes at least one selected from the group consisting of a hydroxy group, an aldehyde group, a carboxy group, an amino group, a sulfo group, a thiol group, an amide bond, a carbonyl group, a nitro group, a cyano group, an ether bond, and an ester bond.
[0224] (Aspect 7) The method according to any one of aspects 1 to 6, wherein the fluorine-containing gas is hydrogen fluoride gas or fluorine gas.
[0225] (Aspect 8) The method according to any one of Aspects 1 to 7, wherein the step (3) is carried out at a temperature in the range of 200°C to 450°C.
[0226] (Aspect 9) The method of any one of Aspects 1 to 8, wherein the first surface includes at least one element selected from the group consisting of H, B, C, N, O, Si, P, S, Cl, Ti, V, Cr, Ge, As, Se, Br, Nb, Mo, Tc, Ru, Rh, Sn, Sb, Te, I, Ta, W, Re, Os, Ir, Pt, and Au.
[0227] (Aspect 10) The method according to any one of aspects 1 to 9, wherein the object to be processed is formed of a single member.
[0228] (Aspect 11) The object to be treated is made of SiO 2 11. The method of claim 10, comprising:
[0229] (Aspect 12) The method according to any one of aspects 1 to 9, wherein the object to be treated has one or more layers.
[0230] (Aspect 13) A component having a recessed portion structure on a first surface, wherein the first surface contains at least one element selected from the group consisting of B, C, Si, P, S, Ti, V, Cr, Ge, As, Se, Nb, Mo, Tc, Ru, Rh, Sn, Sb, Te, I, Ta, W, Re, Os, Ir, Pt, and Au, the recessed portion structure has an opening formed on the first surface, a bottom surface, and a sidewall connecting the opening and the bottom surface, the recessed portion structure has a curved shape when viewed in a cross section of the recessed portion structure, i.e., a cross section perpendicular to the first surface, a ratio P2 / P1 of a dimension P2 of the bottom surface to a dimension P1 of the opening being equal to or greater than 0.99 and less than 1.1, and the center of the bottom surface is offset from the center of the opening with respect to an extension axis extending perpendicular to the first surface.
[0231] Aspect 14: The member of aspect 13, wherein the surface of the sidewall has at least one streak extending from the opening to the bottom surface.
[0232] (Aspect 15) The member according to aspect 13 or 14, wherein the recessed structure has a depth of 10 μm or more.
[0233] (Aspect 16) The member according to any one of Aspects 13 to 15, wherein the recess structure has a sidewall with an angle α (0°<α<180°) relative to a plane parallel to the first surface that changes continuously from the opening to the bottom surface.
[0234] (Aspect 17) The member according to any one of Aspects 13 to 16, wherein the recessed portion structure has a curved shape in the cross-sectional view such that the center of the opening and the center of the bottom surface cannot be connected by a straight line.
[0235] (Aspect 18) The member according to any one of aspects 13 to 17, wherein the first surface further comprises at least one selected from the group consisting of H, N, Cl, Br, and O.
[0236] (Aspect 19) The member according to any one of Aspects 13 to 18, wherein the member is configured as a single member.
[0237] (Embodiment 20) The member according to embodiment 19, wherein the member is a quartz glass substrate or a quartz crystal substrate.
[0238] (Embodiment 21) The member according to any one of embodiments 13 to 18, wherein the member has one or more layers.
[0239] (Aspect 22) The member has a substrate and a film disposed on the substrate, and the film is made of SiO 2 19. The member of any of aspects 13-18, comprising at least one of SiN and SiC forming the first surface.
[0240] This application claims priority based on Japanese Patent Application No. 2023-089319, filed on May 31, 2023, the entire contents of which are incorporated herein by reference.
[0241] REFERENCE SIGNS LIST 1 object to be processed 3 catalytic material 5 recessed structure 6 bottom surface 7 sidewall 7a first sidewall portion 8a coated region 8b uncoated region 12 first surface 17A first side surface of catalytic material 17B second side surface of catalytic material 18 top surface of catalytic material 19 bottom surface of catalytic material 50 recessed structure 52 opening 56 bottom surface 57A, 57B sidewall 100 member 110 object to be processed 112 first surface 114 second surface 117A first side surface 117B second side surface 118 top surface 119 bottom surface 130 catalytic material 131 pattern 140a coated region 140b uncoated region 150 recessed structure 300 first member 302 first surface 304 second surface 350 recessed structure 352 Opening 356 Bottom surface 357 Side wall 380 Continuous line 430 Catalyst material 417A First side surface 417B Second side surface 418 Top surface (a) HF molecule (b) Si atom (c) OH group (d) Si-F bond (e) -δ part (f) +δ part (g) H 2 O molecule F1 Etching direction
Claims
1. A method for manufacturing a member having a recessed structure, comprising: (1) a step of placing a catalyst material in a first region of a first surface of a workpiece, the first surface being composed of elements having a fluoride boiling point of 550°C or less, the catalyst material including an organic compound having a polar functional group, the catalyst material having a first side having a first height H1 and a second side having a second height H2 opposed to each other when viewed in a cross section of the catalyst material, i.e., a cross section perpendicular to the first surface, where H1>0 μm, H2≧0 μm, and the height H1 is greater than the height H2; (2) a step of irradiating the catalyst material with irradiation light including deep ultraviolet light having a wavelength of 380 nm or less; and (3) a step of exposing the workpiece to a fluorine-containing gas at 80°C or more, A method in which, after step (3), a recess structure is formed under the first region, and the recess structure has a shape that, in the cross-sectional view, at the center of the first region, is biased toward the second side surface relative to a perpendicular line drawn from the first surface.
2. The method according to claim 1, wherein in step (1), the catalyst material has an angle φ (0°<φ<90°) between the first surface and a straight line connecting the top of the first side surface and the top of the second side surface in the cross-sectional view, the angle being in the range of 1° to 80°.
3. The method according to claim 1 or 2, wherein the catalytic material has a width in the cross-sectional view of 0.1 μm to 100 μm.
4. The method of claim 1 or 2, wherein the catalytic material has an upper surface that, in the cross-sectional view, monotonically decreases in height from the first side to the second side.
5. The method of claim 1 or 2, wherein the catalytic material has a rectangular or triangular shape in cross section.
6. The method according to claim 1 or 2, wherein the polar functional group includes at least one selected from the group consisting of a hydroxy group, an aldehyde group, a carboxy group, an amino group, a sulfo group, a thiol group, an amide bond, a carbonyl group, a nitro group, a cyano group, an ether bond, and an ester bond.
7. The method according to claim 1 or 2, wherein the fluorine-containing gas is hydrogen fluoride gas or fluorine gas.
8. The method according to claim 1 or 2, wherein step (3) is carried out at a temperature in the range of 200°C to 450°C.
9. The method of claim 1 or 2, wherein the first surface comprises at least one element selected from the group consisting of H, B, C, N, O, Si, P, S, Cl, Ti, V, Cr, Ge, As, Se, Br, Nb, Mo, Tc, Ru, Rh, Sn, Sb, Te, I, Ta, W, Re, Os, Ir, Pt, and Au.
10. The method according to claim 1 or 2, wherein the object to be processed is composed of a single member.
11. The object to be treated is SiO 2 11. The method of claim 10, comprising:
12. The method according to claim 1 or 2, wherein the workpiece has one or more layers.
13. A component having a recessed structure on a first surface, wherein the first surface contains at least one element selected from the group consisting of B, C, Si, P, S, Ti, V, Cr, Ge, As, Se, Nb, Mo, Tc, Ru, Rh, Sn, Sb, Te, I, Ta, W, Re, Os, Ir, Pt, and Au, the recessed structure has an opening formed in the first surface, a bottom surface, and a sidewall connecting the opening and the bottom surface, the recessed structure has a curved shape when viewed in a cross section of the recessed structure, i.e., a cross section perpendicular to the first surface, a ratio P2 / P1 of a dimension P2 of the bottom surface to a dimension P1 of the opening is in a range of 0.99 or more and less than 1.1, and the center of the bottom surface is offset with respect to an extension axis extending from the center of the opening in a direction perpendicular to the first surface.
14. The member of claim 13, wherein said sidewall surface has at least one streak extending from said opening to said bottom surface.
15. The member according to claim 13 or 14, wherein the recessed structure has a depth of 10 μm or more.
16. A member according to claim 13 or 14, wherein the recess structure has an angle α (0°<α<180°) of the side wall relative to a plane parallel to the first surface that changes continuously from the opening to the bottom surface.
17. A member according to claim 13 or 14, wherein the recess structure has a curved shape in the cross-sectional view such that the center of the opening and the center of the bottom surface cannot be connected by a straight line.
18. The member of claim 13 or 14, wherein the first surface further comprises at least one selected from the group consisting of H, N, Cl, Br, and O.
19. A member according to claim 13 or 14, which comprises a single member.
20. The member according to claim 19, wherein the member is a fused silica substrate or a quartz substrate.
21. The component of claim 13 or 14, wherein the component has one or more layers.
22. The member has a substrate and a film disposed on the substrate, the film being made of SiO 2 15. The member of claim 13 or 14, comprising at least one of SiN and SiC forming the first surface.
Citation Information
Patent Citations
Method of etching silicon dioxide
JP1978001198A
Method of producing semiconductor device
JP1980087436A
Method and device for dry etching
JP2000058508A
Method for forming pore in crystal substrate, and functional device having wiring and piping in crystal substrate
JP2014045030A
Manufacturing method of silicon-containing member having recess
JP2022127461A
Cited By
Method for manufacturing member having recessed structure
WO2026172947A1
Production method for member having recess structure, and member having recess structure
WO2026172954A1
Method for manufacturing member having recess structure, and member having recess structure
WO2026172960A1