Multilayer ceramic capacitor

The introduction of a dummy electrode layer in the outer layer portion addresses stress-related issues in multilayer ceramic capacitors, stabilizing internal electrode layers and improving electrical and mechanical reliability.

WO2024247504A1PCT designated stage expired Publication Date: 2024-12-05MURATA MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014543
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-04-10
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional multilayer ceramic capacitors face issues with structural defects and electrical characteristic fluctuations due to stress on internal electrode layers caused by level differences in green sheets during manufacturing, leading to potential tearing and reliability issues.

Method used

Incorporating a dummy electrode layer in the outer layer portion that does not contribute to capacitance formation, which helps absorb stress and maintain the shape and components of internal electrode layers, thereby stabilizing the capacitor's electrical characteristics.

Benefits of technology

The solution effectively prevents structural defects and maintains reliable electrical performance by absorbing stress and preventing Sn migration, enhancing the mechanical strength and high-temperature reliability of the multilayer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014543_05122024_PF_FP_ABST
    Figure JP2024014543_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a multilayer ceramic capacitor which has excellent electrical characteristics, while stably retaining the shape and components of an internal electrode layer. Provided is a multilayer ceramic capacitor 1 which is provided with: a multilayer body 10 that comprises an inner layer part 11, in which a plurality of dielectric layers 20 and internal electrode layers 30 are stacked, and outer layer parts TG, between which the inner layer part 11 is sandwiched in the stacking direction T; and an external electrode 50 which is provided on the surface of the multilayer body 10 and is electrically connected to the internal electrode layers 30. A dummy electrode layer 40, which does not contribute to the formation of a capacitance, is disposed in a region of each of the outer layer parts TG facing the internal electrode layers 30.
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer ceramic capacitors

[0001] The present invention relates to a multilayer ceramic capacitor.

[0002] Conventionally, in the manufacture of a multilayer ceramic capacitor having a laminate including an inner layer portion in which a plurality of dielectric layers and internal electrode layers are laminated, and external electrodes that are electrically connected to the internal electrode layers on the surface of the laminate, first, green sheets that will become dielectric layers and have electrode patterns that will become the internal electrode layers printed on their surfaces are prepared, and multiple green sheets are laminated and pressed together while adjusting their positions to form the inner layer portion, and then multiple green sheets that will become outer layer portions and do not have internal electrode patterns printed on them are stacked on both sides of the inner layer portion to form the laminate structure of the laminate.

[0003] However, since there is a step on the surface of the green sheet due to the printing of the electrode pattern, when the stacked green sheets are pressed in the stacking direction, the end of the electrode pattern, which forms the step, extends perpendicular to the stacking direction on the surface of the dielectric layer.

[0004] Such a stress caused by pressing is likely to be applied to the end portions (portions R shown in FIG. 5) of the internal electrode layers located in the uppermost or lowermost layers of the laminate, and such end portions of the internal electrode layers are excessively stretched, which is likely to cause fractures of the internal electrode layers or structural defects in the dielectric layers.

[0005] Furthermore, multilayer ceramic capacitors contain predetermined metal components in the internal electrode layers to improve their electrical characteristics. However, when the laminate is fired, the metal components are likely to flow out of the internal electrode layers located in the uppermost or lowermost layers to the outer layers, which can easily lead to fluctuations in the electrical characteristics and a decrease in the reliability of the multilayer ceramic capacitor.

[0006] Therefore, there is a need to develop a multilayer ceramic capacitor that has excellent electrical properties while stably maintaining the shape and composition of the internal electrode layers.

[0007] Japanese Patent Application Laid-Open No. 2001-143963

[0008] An object of the present invention is to provide a multilayer ceramic capacitor that has excellent electrical characteristics while stably maintaining the shape and components of the internal electrode layers.

[0009] The present inventors have discovered that in a multilayer ceramic capacitor comprising a laminate including an inner layer portion in which a plurality of dielectric layers and inner electrode layers are laminated, and outer layer portions sandwiching the inner layer portion in the stacking direction, and outer electrodes on the surfaces of the laminate that are electrically connected to the inner electrode layers, by arranging dummy electrode layers that do not contribute to the formation of capacitance in the regions of the outer layer portions facing the inner electrode layers, the shape and components of the inner electrode layers can be stably maintained, and have completed the present invention.

[0010] That is, the present invention provides a multilayer ceramic capacitor comprising: a laminate including an inner layer portion in which a plurality of dielectric layers and inner electrode layers are laminated; and outer layer portions sandwiching the inner layer portion in the lamination direction; and outer electrodes on the surface of the laminate that are electrically connected to the inner electrode layers; and a dummy electrode layer that does not contribute to the formation of capacitance is disposed in a region of the outer layer portion that faces the inner electrode layer.

[0011] According to the present invention, it is possible to provide a multilayer ceramic capacitor that has excellent electrical characteristics while stably maintaining the shape and components of the internal electrode layers.

[0012] FIG. 1 is an external perspective view of a multilayer ceramic capacitor. FIG. 2 is a cross-sectional view taken along line A-A of the multilayer ceramic capacitor of the present invention. FIG. 3 is a cross-sectional view taken along line B-B of the multilayer ceramic capacitor of the present invention. FIG. 4 is an exploded perspective view illustrating the stacking state of dielectric layers and internal electrode layers in the laminate of the multilayer ceramic capacitor of the present invention. FIG. 5 is a cross-sectional view taken along line A-A of a conventional multilayer ceramic capacitor. FIG. 6 is an exploded perspective view illustrating the stacking state of dielectric layers and internal electrode layers in the laminate of the conventional multilayer ceramic capacitor. FIG. 7 is a diagram illustrating a method for manufacturing the multilayer ceramic capacitor of the present invention.

[0013] Hereinafter, a multilayer ceramic capacitor will be described as an embodiment of the present invention, but the present invention is not limited thereto. Furthermore, the drawings may be drawn in a simplified schematic form to explain the contents of the invention, and the dimensional ratios of the depicted components or between the components may not match the dimensional ratios of those components described in the specification. Furthermore, components described in the specification may be omitted in the drawings, or the number of components may be omitted.

[0014] FIG. 1 is a schematic perspective view of a multilayer ceramic capacitor. FIG. 2 is a cross-sectional view of the multilayer ceramic capacitor of the present invention taken along line A-A in FIG. 1. FIG. 3 is a cross-sectional view of the multilayer ceramic capacitor of the present invention taken along line B-B in FIG. 1. FIG. 4 is an exploded perspective view illustrating the lamination state of the dielectric layers and internal electrode layers in the laminate of the multilayer ceramic capacitor of the present invention. FIG. 5 is a cross-sectional view of a conventional multilayer ceramic capacitor taken along line A-A in FIG. 1. FIG. 6 is an exploded perspective view illustrating the lamination state of the dielectric layers and internal electrode layers in the laminate of the conventional multilayer ceramic capacitor. Note that line A-A in FIG. 1 passes through the center of the multilayer ceramic capacitor in the width direction W, which will be described later. Line B-B in FIG. 1 passes through the center of the multilayer ceramic capacitor in the length direction L, which will be described later. The cross sections shown in FIGS. 2 and 5 may be referred to as LT cross sections, and the cross section shown in FIG. 3 may be referred to as WT cross sections.

[0015] (Multilayer Ceramic Capacitor) The multilayer ceramic capacitor 1 has a substantially rectangular parallelepiped shape and includes a laminate 10 and a pair of external electrodes 50 provided on both ends of the laminate 10. The laminate 10 also includes an inner layer portion 11 in which a plurality of dielectric layers 20 and internal electrode layers 30 are stacked.

[0016] In the following description, the direction in which the pair of external electrodes 50 are provided will be referred to as the length direction L, the direction in which the dielectric layers 20 and the internal electrode layers 30 are stacked will be referred to as the stacking direction T, and the direction intersecting both the length direction L and the stacking direction T will be referred to as the width direction W. In the embodiment, the length direction L, the stacking direction T, and the width direction W are mutually orthogonal.

[0017] (Laminate) The laminate 10 has a substantially rectangular parallelepiped shape. The corners and ridges of the laminate 10 are preferably rounded. A corner is a portion where three faces of the laminate 10 intersect, and a ridge is a portion where two faces of the laminate 10 intersect. Note that the dimension of the laminate 10 in the length direction L is not necessarily longer than the dimension in the width direction W. Furthermore, unevenness may be formed on part or all of the surfaces constituting the laminate 10.

[0018] The dimensions of the laminate 10 are not particularly limited, but if the dimension of the laminate 10 in the length direction L is defined as the L dimension, the L dimension is preferably 0.39 mm or more and 3.30 mm or less. If the dimension of the laminate 10 in the stacking direction T is defined as the T dimension, the T dimension is preferably 0.21 mm or more and 2.70 mm or less. If the dimension of the laminate 10 in the width direction W is defined as the W dimension, the W dimension is preferably 0.21 mm or more and 2.70 mm or less.

[0019] As shown in Figures 1 to 3, the laminate 10 has a first main surface TS1 and a second main surface TS2 that face each other in the stacking direction T, a first side surface WS1 and a second side surface WS2 that face each other in a width direction W that intersects with the stacking direction T, and a first end surface LS1 and a second end surface LS2 that face each other in a length direction L that intersects with the stacking direction T and the width direction W.

[0020] The laminate 10 has an inner layer portion 11 in which internal electrode layers 30 and dielectric layers 20 are stacked, side margin portions WG arranged on both sides of the width direction W of the inner layer portion 11, and outer layer portions TG arranged on both sides of the stacking direction T of the inner layer portion 11.

[0021] (Inner layer portion) The inner layer portion 11 is a region in the laminate 10 where the internal electrode layers 30 and the dielectric layers 20 are stacked. A capacitance is formed when the first opposing portion 31A of the first internal electrode layer 31 and the second opposing portion 32A of the second internal electrode layer 32 face each other via the dielectric layer 20. The inner layer portion 11 includes, in the stacking direction T, the internal electrode layer 30 located closest to the first main surface TS1 to the internal electrode layer 30 located closest to the second main surface TS2.

[0022] (Dielectric Layer) The plurality of dielectric layers 20 stacked in the laminate 10 can be made of a ceramic material. Examples of the ceramic material include BaTiO 3 The dielectric ceramic mainly contains the above-mentioned compound. Alternatively, the ceramic material may contain at least one of a manganese compound, an iron compound, a chromium compound, a cobalt compound, a nickel compound, and the like.

[0023] The thickness of the dielectric layer 20 is preferably 0.3 μm or more and 1.1 μm or less, and particularly preferably 0.45 μm or more and 0.55 μm or less. The number of laminated dielectric layers 20 is preferably 10 to 700. Note that this number of dielectric layers 20 is the total number of the dielectric layers of the inner layer portion 11 and the dielectric layers of the outer layer portion TG consisting of the first outer layer portion TG1 and the second outer layer portion TG2.

[0024] (Internal electrode layers) The multiple internal electrode layers 30 stacked in the laminate 10 are composed of first internal electrode layers 31 and second internal electrode layers 32. The multiple first internal electrode layers 31 are arranged on the multiple dielectric layers 20. The multiple second internal electrode layers 32 are arranged on the multiple dielectric layers 20. The multiple first internal electrode layers 31 and the multiple second internal electrode layers 32 are arranged alternately in the stacking direction T of the laminate 10.

[0025] The first internal electrode layer 31 has a first opposing portion 31A opposing the second internal electrode layer 32, and a first lead portion 31B led from the first opposing portion 31A to the first end face LS1. The first lead portion 31B is exposed at the first end face LS1.

[0026] The second internal electrode layer 32 has a second opposing portion 32A opposing the first internal electrode layer 31 and a second lead portion 32B led from the second opposing portion 32A to the second end face LS2. The second lead portion 32B is exposed at the second end face LS2.

[0027] The internal electrode layers 30 are made of an appropriate conductive material, such as a metal such as Ni, Cu, Ag, Pd, or Au, or an alloy containing at least one of these metals. When an alloy is used, the internal electrode layers 30 may be made of, for example, an Ag-Pd alloy. The internal electrode layers 30 may also contain dielectric particles having the same composition as the ceramics contained in the dielectric layers 20.

[0028] The material of the internal electrode layer 30 preferably contains Ni and Sn. Ni and Sn may include an alloyed portion. The alloying of Ni and Sn changes the state (electrical barrier height) of the internal electrode layer 30 near the interface with the dielectric layer 20, contributing to improving the high-temperature accelerated life. As a result, a multilayer ceramic capacitor 1 with excellent reliability (improved high-temperature accelerated life) when a voltage is applied can be obtained. Note that Sn may be a Sn material made of either a metal containing Sn or a Sn compound, and SnO or SnO may be used instead of Sn. 2 The tin oxide powder may be represented by the formula:

[0029] By adding Sn to Ni, which is the main component, an alloy containing Sn is formed in the internal electrode layer 30, and an interface layer containing Sn is formed at the interface between the internal electrode layer 30 and the dielectric layer 20. By providing such an interface layer, the high-temperature load life of the multilayer ceramic capacitor 1 is improved, and the reliability is enhanced.

[0030] When Ni is used as the main component and Sn is added to it, the Sn content is preferably 0.1 mol or more and 10 mol or less when the total of Ni and Sn is 100 mol. If the Sn content is less than 0.1 mol, the effect of adding Sn is difficult to achieve. On the other hand, if the Sn content exceeds 10 mol, the interface layer is formed excessively thick, and the capacitance of the multilayer ceramic capacitor 1 decreases. The above state can be achieved by adding Sn as a secondary component to Ni, the main component, in the conductive paste for forming the internal electrode layers, or by adding a Ni-Sn alloy to the conductive paste for forming the internal electrodes.

[0031] The method of including Sn is not particularly limited. For example, Sn may be previously contained in the conductive paste that will become the internal electrode layers 30, or may be mixed into the raw material powder of the dielectric ceramic that will form the dielectric layers 20 after firing. In the latter case, when SnO powder is mixed into the raw material powder of the dielectric ceramic and then fired in a reducing atmosphere at a temperature increase rate of 20° C. / min or more, SnO is reduced to Sn, which is easily absorbed into the internal electrode layers 30.

[0032] When the laminate 10 is fired, the Sn contained in the internal electrode layer 30 tends to migrate to the outer layer portion TG, and the effect expected from the alloy layer formed by Ni and Sn may not be fully exerted. However, by providing a dummy electrode layer 40 described later, it is possible to prevent the migration of Sn from the internal electrode layer 30 to the outer layer portion TG, thereby improving the function of the internal electrode layer 30 in the internal layer portion 11.

[0033] The alloy layer can be confirmed by polishing the cross section of the laminate 10 (for example, exposing the LT cross section at the center in the width direction W), checking the difference in composition by WDX analysis, and identifying the range of the alloy layer from the difference in composition. Also, the difference in composition can be confirmed in more detail by thinning a part of the cross section (including the dielectric layer 20 and the internal electrode layer 30) and performing TEM analysis.

[0034] The thickness of the internal electrode layers 30 is preferably 0.25 μm or more and 0.6 μm or less, and particularly preferably 0.4 μm or more and 0.5 μm or less. The number of the internal electrode layers 30 is preferably 5 or more and 350 or less.

[0035] (Side Margin Portion) The side margin portion WG is a region located on both sides of the inner layer portion 11 in the width direction W, and includes a first side margin portion WG1 that forms the first side surface WS1 of the multilayer ceramic capacitor 1, and a second side margin portion WG2 that forms the second side surface WS2 of the multilayer ceramic capacitor 1. The side margin portion WG can be formed of the same material as the dielectric layer 20.

[0036] (Outer layer portion) The outer layer portion TG is a region arranged on both sides of the inner layer portion 11 in the stacking direction T, and includes a first outer layer portion TG1 that forms the first main surface TS1 of the multilayer ceramic capacitor 1, and a second outer layer portion TG2 that forms the second main surface TS2 of the multilayer ceramic capacitor 1.

[0037] The outer layer portion TG can be formed from the same material as the dielectric layer 20 of the inner layer portion 11. The outer layer portion TG can also be formed by laminating a plurality of dielectric layers 20.

[0038] (Dummy Electrode Layer) A dummy electrode layer 40 is disposed in a region of the external layer portion TG facing the internal electrode layer 30. Since the dummy electrode layer 40 does not form a capacitance, it is either connected to the same external electrode 50 as the opposing internal electrode layer 30, or is not connected to the external electrode 50.

[0039] A plurality of dummy electrode layers 40 can be arranged in the stacking direction T with the dielectric layers 20 interposed therebetween. The outer layer portion TG can be formed by stacking a plurality of dielectric layers 20 in the stacking direction T, but by arranging the dummy electrode layers 40 with the dielectric layers 20 interposed therebetween, a stacked structure of the dielectric layers 20 and the dummy electrode layers 40 is formed, and the outer layer portion TG can be provided with a plurality of dummy electrode layers 40.

[0040] The dummy electrode layers 40 can be made of an appropriate conductive material, such as a metal such as Ni, Cu, Ag, Pd, or Au, or an alloy containing at least one of these metals. When an alloy is used, the dummy electrode layers 40 may be made of, for example, an Ag-Pd alloy. The dummy electrode layers 40 can be made of the same material as the internal electrode layers 30.

[0041] The material of the dummy electrode layer 40 preferably contains Ni and Sn. Ni and Sn may also contain an alloyed portion. This effectively prevents Sn from moving from the internal electrode layer 30 to the outer layer portion TG. The dummy electrode layer 40 may be made of a metal containing Sn or a Sn compound, and SnO or SnO may be used instead of Sn. 2 The tin oxide powder may be represented by the formula:

[0042] Adding Sn to the main component Ni that forms the dummy electrode layer 40 reduces the sintering temperature of the dummy electrode layer 40. As a result, when the laminate 2 is fired, the degree of shrinkage of the dummy electrode layer 40 becomes greater than that of the outer layer portion TG. Therefore, in the laminate 2 after firing, compressive stress occurs in the outer layer portion TG, which has the effect of suppressing the extension of cracks that occur due to external tensile stress when the multilayer ceramic capacitor is used, and as a result, the mechanical strength of the multilayer ceramic capacitor 1 can be improved.

[0043] When Ni is used as the main component and Sn is added to it, the Sn content is preferably 0.1 mol or more and 10 mol or less when the total of Ni and Sn is 100 mol. If the Sn content is less than 0.1 mol, the effect of adding Sn is difficult to achieve. On the other hand, if the Sn content exceeds 10 mol, the dummy electrode layer 40 shrinks too much during firing of the laminate 2, causing tensile stress in the fired dummy electrode layer 40 and making it more likely to crack. If this crack propagates to the internal electrode layer 30 located in the upper or lower layer portion of the inner layer portion 11, the high-temperature reliability of the multilayer ceramic capacitor 1 will be impaired. The above-mentioned state can be achieved by adding Sn as a secondary component to Ni, the main component, in the conductive paste for forming the dummy electrode layer, or by adding a Ni-Sn alloy to the conductive paste for forming the internal electrodes.

[0044] The method for including Sn is not particularly limited. For example, Sn may be previously included in the conductive paste that will become the dummy electrode layer 40, or may be mixed into the raw material powder of the dielectric ceramic that will form the dielectric layer 20 after firing. In the latter case, if SnO powder is mixed into the raw material powder of the dielectric ceramic and then fired in a reducing atmosphere at a temperature increase rate of 20° C. / min or more, the SnO is reduced to Sn, which is easily absorbed into the dummy electrode layer 40.

[0045] The portion where Ni and Sn are alloyed preferably has an alloy layer at the interface between the dielectric layer 20 and the dummy electrode layer 40 so as to cover the internal electrode layer 30 .

[0046] The alloy layer can be confirmed by polishing the cross section of the laminate 10 (for example, exposing the LT cross section at the center in the width direction W), checking the difference in composition by WDX analysis, and identifying the range of the alloy layer from the difference in composition. Also, the difference in composition can be confirmed in more detail by thinning a part of the cross section (including the dielectric layer 20 and the internal electrode layer 30) and performing TEM analysis.

[0047] The thickness of the dummy electrode layer 40 is preferably 0.25 μm or more and 0.6 μm or less, and more preferably 0.4 μm or more and 0.5 μm or less.

[0048] In the embodiment shown in Fig. 2, a first dummy electrode layer 40A is provided in the first outer layer portion TG1 so as to face the first internal electrode layer 31 located in the uppermost layer of the internal electrode layers 30 laminated in the internal layer portion 11. The first dummy electrode layer 40A is exposed at the first end face LS1 of the laminate 10, just like the first internal electrode layer 31 located in the uppermost layer. Fig. 2 shows a configuration in which two first dummy electrode layers 40A are arranged, but the number of first dummy electrode layers 40A arranged is not limited to two, and may be one layer or three or more layers.

[0049] 2, a second dummy electrode layer 40B is provided in the second outer layer portion TG2 so as to face the second internal electrode layer 32 located in the lowest layer of the internal electrode layers 30 laminated in the internal layer portion 11. The second dummy electrode layer 40B is exposed at the second end surface LS2 of the laminate 10, just like the second internal electrode layer 32 located in the lowest layer. While Fig. 2 shows a configuration in which two second dummy electrode layers 40B are arranged, the number of arranged second dummy electrode layers 40B is not limited to two, and may be one layer or three or more layers.

[0050] Fig. 5 is an LT cross-sectional view taken along line A-A of the conventional multilayer ceramic capacitor 1. The outer layer portion TG is formed by laminating a plurality of dielectric layers 20. Fig. 6 is an exploded perspective view illustrating the lamination state of the dielectric layers 20 and the internal electrode layers 30 in the laminate 10 of the conventional multilayer ceramic capacitor 1.

[0051] Conventionally, in the manufacture of a multilayer ceramic capacitor 1, green sheets for the dielectric layers 20, each having an electrode pattern printed on its surface to form the internal electrode layer 30, are prepared. A plurality of green sheets are laminated and pressed together while adjusting the position of the green sheets to form the inner layer portion 11. Furthermore, a plurality of green sheets, each having no internal electrode layer pattern printed thereon, are stacked on both sides of the inner layer portion 11 to form the outer layer portion TG, thereby forming the laminate structure 10. Because the surfaces of the green sheets have steps corresponding to the printed electrode patterns, when the stacked green sheets are pressed in the stacking direction, the edge portions of the electrode patterns at the edges of the steps extend perpendicularly to the stacking direction on the surfaces of the dielectric layers. In particular, stress due to such pressing is likely to be applied to the end portions (regions R shown in FIG. 5 ) of the internal electrode layers 30 located in the uppermost or lowermost layer of the laminate. The end portions (regions R shown in FIG. 5 ) of the internal electrode layers 30 located in the uppermost or lowermost layer of the laminate are excessively stretched, which can easily cause fractures of the internal electrode layers 30 or structural defects in the dielectric layers 20.

[0052] In the multilayer ceramic capacitor 1 of the present invention, dummy electrode layers 40 are formed between the dielectric layers of the outer layer portion TG in a shape corresponding to the opposing regions of the internal electrode layers 30 .

[0053] Therefore, even if the green sheet is pressed in the stacking direction T in the manufacturing process of the laminate 10, the stress is absorbed by the dummy electrode layer 40 in the outer layer portion TG or the outer layer portion TG, and partial cracks or partial peeling do not occur in the inner layer portion 11 which forms the actual capacitance, so that short circuits do not occur between the internal electrode layers and stable insulation reliability can be maintained.

[0054] That is, no internal defects are generated in the capacitance generating portion, and a high capacitance multilayer ceramic capacitor is obtained.

[0055] (External electrode 50) The external electrode 50 includes a first external electrode 50A provided on the first end face LS1 and a second external electrode 50B provided on the second end face LS2. The external electrode 50 covers not only the end face LS but also a part of the main surface TS and the side surface WS that are continuous with the end face LS.

[0056] An end of the first lead portion 31B of the first internal electrode layer 31 is exposed at the first end surface LS1 and is electrically connected to the first external electrode 50A. Also, an end of the second lead portion 32B of the second internal electrode layer 32 is exposed at the second end surface LS2 and is electrically connected to the second external electrode 50B. This results in a structure in which multiple capacitor elements are electrically connected in parallel between the first external electrode 50A and the second external electrode 50B.

[0057] The first dummy electrode layer 40A is exposed at the first end face LS1 of the laminate 10 and connected to the first external electrode 50A, just like the first internal electrode layer 31 located in the uppermost layer, and therefore does not contribute to the formation of capacitance. The first dummy electrode layer 40A can also be configured so that it is not connected to either the first external electrode 50A or the second external electrode 50B and is not electrically connected to the external electrode 50.

[0058] The second dummy electrode layer 40B is exposed at the second end face LS2 of the laminate 10 and connected to the second external electrode 50B, just like the second internal electrode layer 32 located at the bottom, and therefore does not contribute to the formation of capacitance. The second dummy electrode layer 40B can also be configured so that it is not connected to either the second external electrode 50B or the first external electrode 50A and is not electrically connected to the external electrode 50.

[0059] The external electrode 50 includes, for example, a base electrode layer and a plating layer, but it is not necessarily required that the external electrode 50 have such a layered structure.

[0060] The base electrode layer is formed by, for example, applying and baking a conductive paste containing Cu. The base electrode layer may also contain glass.

[0061] The plating layer includes a Ni plating layer disposed on the surface of the base electrode layer and a Sn plating layer disposed on the surface of the Ni plating layer, although the configuration of the plating layer is not limited thereto.

[0062] (Method for Manufacturing the Multilayer Ceramic Capacitor 1) A method for manufacturing the multilayer ceramic capacitor 1 will be described with reference to FIG.

[0063] A ceramic slurry containing ceramic powder, a binder, and a solvent is formed into a sheet on the surface of a carrier film using a die coater, a gravure coater, a microgravure coater, or the like to prepare a laminated ceramic green sheet 101 that will become the dielectric layer 20. Next, a conductive paste is printed in strips on the laminated ceramic green sheet 101 by screen printing, inkjet printing, gravure printing, or the like, and a conductive pattern 102 that will become the internal electrode layer 30 is printed on the surface of the laminated ceramic green sheet 101 to prepare a material sheet 103.

[0064] 7( a), a plurality of material sheets 103 are stacked so that the conductive patterns 102 face in the same direction and are shifted by half a pitch in the longitudinal direction between adjacent material sheets 103. This portion forms the inner layer portion 11 of the laminate 10.

[0065] Then, on the top layer of the plurality of material sheets 103 stacked with a half-pitch offset, a material sheet 103 is placed so that the conductive pattern 102 overlaps the top layer material sheet 103 when viewed from the stacking direction T. A laminate ceramic green sheet 101 without a printed conductive pattern 102 is then placed on top of the material sheet 103. This portion forms the first outer layer portion TG1 including the first dummy electrode layer 40A. While FIG. 7( a) shows a configuration in which two material sheets 103 forming the first dummy electrode layer 40A are arranged, and one laminate ceramic green sheet 101 without a printed conductive pattern 102 is arranged, the number of first dummy electrode layers 40A to be arranged is not limited to two, and one, three, or more layers may also be arranged. Furthermore, the laminate ceramic green sheet 101 without a printed conductive pattern 102 is not limited to one layer, and multiple layers may also be arranged.

[0066] Similarly, a material sheet 103 is placed under the bottom layer of a plurality of material sheets 103 stacked with a half-pitch offset such that the conductive pattern 102 overlaps the bottom layer material sheet 103 when viewed from the stacking direction T. A laminate ceramic green sheet 101 without a printed conductive pattern 102 is then placed below the bottom layer. This portion forms a second outer layer portion TG2 including the second dummy electrode layer 40B. While FIG. 7( a) shows a configuration in which two layers of material sheets 103 forming the second dummy electrode layer 40B are placed and one layer of laminate ceramic green sheet 101 without a printed conductive pattern 102 is placed, the number of second dummy electrode layers 40B placed is not limited to two, and may be one layer, or three or more layers. Furthermore, the number of laminate ceramic green sheets 101 without a printed conductive pattern 102 is not limited to one, and multiple layers may be placed.

[0067] The stacked material sheets 103 and the laminated ceramic green sheets 101 are isostatically pressed to form a mother block 110 shown in FIG. 7(b).

[0068] Next, the mother block 110 is cut along cutting lines x shown in FIG. 7B and cutting lines y intersecting with the cutting lines x, to produce a plurality of laminates 10 shown in FIG. 7C.

[0069] According to the above process, the outer layer portions TG and the side margin portions WG can be formed simultaneously with the formation of the laminate 10. Alternatively, the laminate 10 may be formed by first forming the inner layer portion 11 in which the ends of the internal electrode layers 30 in the width direction W are exposed on both sides by cutting out from a mother block member, and then attaching the side margin portions WG to both sides of the inner layer portion 11 so as to cover the exposed ends of the internal electrode layers 30. In this case, the attached side margin portions WG can be made of the same dielectric ceramic material as the dielectric layer 20. Alternatively, the side margin portions WG may be formed by applying a ceramic paste to both sides of the inner layer portion 11.

[0070] Next, a base electrode layer is formed by applying and baking a conductive paste containing Cu to the end surface LS of the laminate 10. The base electrode layer is formed so as to extend not only to the end surfaces LS on both sides of the laminate 10 but also to the main surface TS and side surface WS of the laminate 10, covering a portion of the main surface TS and side surface WS on the end surface LS side.

[0071] Next, a Ni plating layer is formed on the surface of the base electrode layer, and a Sn plating layer is formed thereon, thereby producing the multilayer ceramic capacitor 1 shown in FIG. 7(d).

[0072] Although the embodiments of the present invention have been described above, the present invention is not limited to the embodiments and can be embodied in various forms without departing from the spirit of the present invention. The present invention includes the following combinations.

[0073] <1> A multilayer ceramic capacitor comprising: a laminate including an internal layer portion in which a plurality of dielectric layers and internal electrode layers are laminated; and external layer portions sandwiching the internal layer portion in the stacking direction; and external electrodes on the surface of the laminate and electrically connected to the internal electrode layers, wherein dummy electrode layers that do not contribute to the formation of capacitance are disposed in regions of the external layer portions facing the internal electrode layers. <2> The multilayer ceramic capacitor according to <1>, wherein the internal electrode layers contain Ni and Sn. <3> The multilayer ceramic capacitor according to <2>, wherein the Sn content is 0.1 mol or more and 10 mol or less when the total of Ni and Sn is 100 mol. <4> The multilayer ceramic capacitor according to any one of <1> to <3>, wherein the internal electrode layers have a thickness in the stacking direction of 0.25 μm or more and 0.6 μm or less. <5> The multilayer ceramic capacitor according to any one of <1> to <4>, wherein the dummy electrode layers contain Ni and Sn. <6> The multilayer ceramic capacitor according to <5>, wherein the Sn content is 0.1 mol or more and 10 mol or less when the total of Ni and Sn is 100 mol. <7> The multilayer ceramic capacitor according to any one of <1> to <6>, wherein the dummy electrode layer has a thickness in the stacking direction of 0.25 μm or more and 0.6 μm or less. <8> The multilayer ceramic capacitor according to any one of <1> to <7>, wherein the dielectric layer has a thickness in the stacking direction of 0.3 μm or more and 1.1 μm or less. <9> The multilayer ceramic capacitor according to any one of <1> to <8>, wherein the length in the length direction of the laminate is 0.39 mm or more and 3.30 mm or less, the length in the stacking direction is 0.21 mm or more and 2.70 mm or less, and the length in the width direction is 0.21 mm or more and 2.70 mm or less.

[0074] REFERENCE SIGNS LIST 1 Multilayer ceramic capacitor 10 Laminate 11 Internal layer portion 20 Dielectric layer 30 Internal electrode layer 31 First internal electrode layer 31A First opposing portion 31B First lead portion 32 Second internal electrode layer 32A Second opposing portion 32B Second lead portion 40 Dummy electrode layer 40A First dummy electrode layer 40B Second dummy electrode layer 50 External electrode 50A First external electrode 50B Second external electrode TS Main surface TS1 First main surface TS2 Second main surface WS Side surface WS1 First side surface WS2 Second side surface LS End surface LS1 First end surface LS2 Second end surface TG Outer layer portion TG1 First outer layer portion TG2 Second outer layer portion WG Side margin portion WG1 First side margin WG2 Second side margin

Claims

1. A multilayer ceramic capacitor comprising: a laminate including an inner layer portion in which a plurality of dielectric layers and internal electrode layers are laminated, and outer layer portions sandwiching the inner layer portion in the stacking direction; and external electrodes on the surface of the laminate and conducting with the internal electrode layers, wherein a dummy electrode layer that does not contribute to the formation of capacitance is disposed in the region of the outer layer portion facing the internal electrode layers.

2. The multilayer ceramic capacitor according to claim 1, wherein said internal electrode layers contain Ni and Sn.

3. The multilayer ceramic capacitor according to claim 2, wherein the Sn content is from 0.1 mol to 10 mol, where the total of Ni and Sn is 100 mol.

4. The multilayer ceramic capacitor according to any one of claims 1 to 3, wherein the thickness of said internal electrode layers in said lamination direction is 0.25 µm or more and 0.6 µm or less.

5. The multilayer ceramic capacitor according to any one of claims 1 to 4, wherein the dummy electrode layers contain Ni and Sn.

6. The multilayer ceramic capacitor according to claim 5, wherein the Sn content is from 0.1 mol to 10 mol, where the total of Ni and Sn is 100 mol.

7. The multilayer ceramic capacitor according to claim 1, wherein the thickness of said dummy electrode layer in said lamination direction is not less than 0.25 μm and not more than 0.6 μm.

8. The multilayer ceramic capacitor according to claim 1, wherein the thickness of said dielectric layers in said lamination direction is not less than 0.3 μm and not more than 1.1 μm.

9. The multilayer ceramic capacitor according to any one of claims 1 to 8, wherein the length in the longitudinal direction of the laminate is not less than 0.39 mm and not more than 3.30 mm, the length in the lamination direction is not less than 0.21 mm and not more than 2.70 mm, and the length in the width direction is not less than 0.21 mm and not more than 2.70 mm.

Citation Information

Patent Citations

  • Laminated electronic component

    JP2011108966A

  • Ceramic capacitor

    JP2013197186A

  • Multilayer ceramic capacitor

    JP2018198292A

  • Multilayer ceramic capacitor

    JP2023073974A