Porous molded body and gas adsorbent

A porous molded body using inorganic particles and fibrous organic compounds addresses the limitations of conventional silica bodies by achieving high mechanical strength and large pore volume, enabling efficient carbon dioxide recovery with improved durability and safety.

WO2024247513A1PCT designated stage expired Publication Date: 2024-12-05AGC INC +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014900
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-04-12
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional porous silica molded bodies have limitations in achieving high mechanical strength, large pore volume, and pore diameter due to the use of organic binders and high-temperature firing, which compromises their adsorption efficiency and durability.

Method used

A porous molded body composed of inorganic porous particles and fibrous organic compounds, specifically using nanofibers like cellulose, chitin, or chitosan, which provides high compressive strength and large pore volume without the need for high-temperature firing, and supports amine compounds for efficient carbon dioxide adsorption.

Benefits of technology

The resulting porous molded body exhibits high mechanical strength and large pore volume, enabling efficient carbon dioxide recovery from exhaust gases, reducing costs and environmental impact while maintaining ease of handling and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention provides a porous molded body having high mechanical strength and a large pore volume and pore diameter. The porous molded body of the present invention is substantially composed of inorganic porous particles and a fibrous organic compound. The gas adsorbent of the present invention uses the porous molded body of the present invention.
Need to check novelty before this filing date? Find Prior Art

Description

Porous molded body and gas adsorbent

[0001] The present invention relates to a porous molded body and a gas adsorbent using the porous molded body.

[0002] Porous molded bodies are widely used industrially as adsorbents, catalyst supports, etc. In this case, the porous molded bodies are generally used as molded bodies in the form of pellets, spheres, etc., for ease of handling and to reduce gas pressure loss.

[0003] Conventionally, such porous molded bodies have been formed from inorganic porous particles and an inorganic or organic binder. Silica, zeolite, alumina, clay compounds, and the like have been used as inorganic porous particles because of their large specific surface area, large pore volume, and excellent heat resistance. Among these, silica not only has excellent heat resistance and acid resistance, but also has the excellent feature of being able to widely adjust the pore properties, such as the specific surface area, pore volume, and pore diameter, depending on the manufacturing method and manufacturing conditions. Therefore, porous molded bodies of silica are extremely useful materials for applications such as adsorbents and catalyst supports.

[0004] Various proposals have been made for such porous silica molded bodies. For example, Patent Documents 1 and 2 disclose methods for producing a silica gel molded body by adding and mixing an organic binder or an inorganic binder to silica gel powder, molding the mixture, drying, and firing the mixture.

[0005] Furthermore, Patent Document 3 discloses the production of inorganic oxide microspheres having excellent compressive strength by extrusion molding, granulation, drying, and calcination of an inorganic oxide microparticle precursor such as silica.

[0006] Patent Document 4 discloses a silica molded body containing spherical porous silica and scaly silica, with a silica component content of 95% by mass or more.

[0007] Among the uses of such porous molded bodies, the separation and recovery of carbon dioxide, a greenhouse gas, has recently attracted attention as a measure against global warming, and examples of applications include methods for separating carbon dioxide from exhaust gases emitted by automobiles and factories, the atmosphere, etc.

[0008] In particular, attention has been focused on the development of methods using solid adsorbents. Solid adsorbents are porous materials with carbon dioxide adsorption ability imparted to the pore surface, and can be obtained, for example, by immobilizing amines on the porous material. Solid adsorbents are low in toxicity, corrosiveness, and flammability, and are environmentally friendly materials with excellent safety and ease of handling. In addition, because they can adsorb carbon dioxide with low energy consumption, they are expected to reduce costs.

[0009] Japanese Patent Application Publication No. 61-127682 Japanese Patent Application Publication No. 10-273372 Japanese Patent Application Publication No. 2005-58932 Japanese Patent Application Publication No. 2022-148340

[0010] The silica gel molded bodies described in Patent Documents 1 and 2 have insufficient porosity in the silica gel powder used as the raw material, resulting in molded bodies with relatively small pore volumes and pore diameters. Furthermore, because an organic binder is used, the molded body must be calcined at a temperature of 400°C or higher after molding and drying to remove the organic binder. The inorganic oxide microsphere molded body described in Patent Document 3 has a pore volume of 0.6 ml / g or less, which is not particularly large. Furthermore, the silica molded body described in Patent Document 4 has a large pore volume and pore diameter, but in order to obtain a molded body with high mechanical strength, it may be necessary to incorporate a large amount of flaky silica, an inorganic binder, or to calcinate at a high temperature of 600°C or higher. The use of a large amount of binder or calcination at a high temperature results in a problem of small pore volume and pore diameter of the molded body.

[0011] Therefore, an object of the present invention is to provide a porous molded body having high mechanical strength, specifically high compressive strength, and a large pore volume and pore diameter.

[0012] As a result of extensive research, the present inventors have discovered that the above problems can be solved by using a porous molded body essentially consisting of inorganic porous particles and a fibrous organic compound, and have thus completed the present invention.

[0013] The present invention relates to the following (1) to (10): (1) A porous molded body substantially consisting of inorganic porous particles and a fibrous organic compound. (2) The porous molded body according to (1) above, wherein the fibrous organic compound is at least one nanofiber selected from the group consisting of cellulose, chitin, and chitosan. (3) The porous molded body according to (1) above, wherein the inorganic porous particles include at least one selected from the group consisting of silica, zeolite, alumina, silica-alumina, titania, aluminum silicate, magnesium silicate, and clay minerals. (4) The porous molded body has a pore volume of 0.8 cm3 as determined by a nitrogen adsorption method. 3 / g or more 3.5cm 3 / g or less, the peak pore diameter is 20 nm or more and 100 nm or less, and the average pore diameter is 15 nm or more and 50 nm or less. (5) A method for producing the porous molded body according to any one of (1) to (4), comprising mixing and kneading inorganic porous particles, a fibrous organic compound, and water, shaping the mixture, optionally sizing the particles, and then drying in air at 200°C or less. (6) A gas adsorbent using the porous molded body according to any one of (1) to (4). (7) The gas adsorbent according to (6), for adsorbing carbon dioxide, in which an amine compound is supported on the porous molded body. (8) The gas adsorbent according to (7), in which the amine compound is an amine containing at least one ether-bonded oxygen atom or siloxane-bonded oxygen atom in the molecule. (9) The gas adsorbent according to (7), wherein the amine compound is an amine containing, as a partial structure, at least one selected from the group consisting of an ethylenedioxy group, an isopropylenedioxy group, a butylenedioxy group, a linear siloxane structure, and a cyclic siloxane structure in the molecule. (10) The gas adsorbent according to (7), wherein the amine compound is an amine having a boiling point of 250°C or higher at 760 mmHg.

[0014] According to the present invention, a porous molded body having high mechanical strength, specifically high compressive strength, and large pore volume and pore diameter can be obtained. Furthermore, the porous molded body of the present invention can be used as a gas adsorbent, and in particular, a gas adsorbent having an amine compound supported on the porous molded body of the present invention can efficiently capture carbon dioxide and increase the amount of carbon dioxide captured. Therefore, the gas adsorbent of the present invention can efficiently capture exhaust gases emitted from automobiles, factories, etc. and acidic gases contained in the atmosphere, particularly carbon dioxide, thereby reducing the costs associated with separating and capturing acidic gases. Furthermore, because it is a solid adsorbent, it is easy to handle and can be used safely.

[0015] The present invention will be described below, but the present invention is not limited to the examples given in the following description. In this specification, "mass" has the same meaning as "weight".

[0016] <Porous Molded Body> The porous molded body of the present invention is substantially composed of inorganic porous particles and a fibrous organic compound. The fibrous organic compound acts as a binder, and the inorganic porous particles are bound via the fibrous organic compound, causing the inorganic porous particles to aggregate, and the resulting molded body (aggregate) has excellent mechanical strength. Furthermore, because the fibrous organic compound has an extremely fine fibrous shape, it functions as a binder for the inorganic porous particles with the addition of a very small amount, thereby obtaining a porous molded body suitable as an adsorbent. In this specification, the term "substantially" means that the inclusion of components that are unavoidably contained due to the nature of the raw materials or the manufacturing process is permitted, and components other than the inorganic porous particles and the fibrous organic compound may be contained in an amount of 1 mass% or less.

[0017] The fibrous organic compound may be a fibrous natural organic polymer compound, a synthetic organic polymer compound, a semi-synthetic polymer compound, or the like, and may contain one type alone or two or more types in combination.

[0018] Examples of natural organic polymer compounds include polysaccharides (e.g., cellulose, starch, alginate, dextran, pullulane, polyhyaluronic acid, and derivatives thereof), chitin, chitosan, poly(3-hydroxyalkanoates) (e.g., poly(β-hydroxybutyrate), poly(3-hydroxyoctanoate)), poly(3-hydroxy fatty acids), fibrin, agar, and agarose.

[0019] Examples of synthetic organic polymer compounds include polyvinyl alcohol (PVA), methyl cellulose (MC), ethyl cellulose (EC), hydroxyethyl cellulose (HEC), carboxymethyl cellulose (CMC), polyethylene glycol (PEG), polypropylene glycol (PPG), polyvinylpyrrolidone (PVP), and polyacrylic acid (PAA).

[0020] Examples of semi-synthetic polymer compounds include carboxymethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and cationized guar gum.

[0021] Among the above, natural organic polymer compounds are preferred, and cellulose, chitin, and chitosan are more preferred.

[0022] Furthermore, the fibrous organic compound is preferably a nanofiber having a fiber width of 1 nm or more and 100 nm or less and an aspect ratio of 100 or more and 10,000 or less, and specifically, it is particularly preferable that the fibrous organic compound contains at least one nanofiber selected from the group consisting of cellulose, chitin, and chitosan, and it is most preferable that the fibrous organic compound contains cellulose nanofibers.

[0023] Cellulose nanofibers are obtained by mechanically defibrating pulp dispersed in water using a water jet method, and are available as aqueous slurries with fiber diameters of 10 to 50 nm and various fiber lengths. Commercially available cellulose nanofibers include "BiNFi-s" (trade name) manufactured by Sugino Machine Co., Ltd. Other examples include TEMPO-oxidized cellulose nanofibers obtained by mechanically defibrating pulp using a TEMPO catalyst. TEMPO-oxidized cellulose nanofibers are aqueous slurries of ultrafine fibers with fiber widths of 3 to 4 nm, and commercially available examples include "Cellenpia" (trade name) manufactured by Nippon Paper Industries Co., Ltd. These cellulose nanofibers act as binders for inorganic porous particles by drying at 200°C or below without calcining at a high temperature of 600°C, resulting in molded articles with sufficient mechanical strength.

[0024] Examples of raw materials for the inorganic porous particles include silica, zeolite, alumina, silica alumina, titania, aluminum silicate, magnesium silicate, clay minerals, etc. The inorganic porous particles may contain at least one selected from the group consisting of these.

[0025] The inorganic porous particles may be primary particles or secondary particles (aggregates) formed by aggregation of primary particles, and have an average particle diameter (50% particle diameter, D 50 ) is preferably 1 μm to 1 mm. If the average particle diameter of the inorganic porous particles is 1 μm or more, it is possible to prevent the pressure loss when the gas to be treated is passed through the gas adsorbent described later from increasing too much, and if it is 1 mm or less, a porous body with higher strength can be obtained. 50 ) is preferably 1 μm or more, more preferably 10 μm or more, and is preferably 1 mm or less, more preferably 500 μm or less, and even more preferably 100 μm or less.

[0026] The average particle size of inorganic porous particles can be measured using a particle size distribution analyzer or by observation with a scanning electron microscope (SEM). Examples of particle size distribution analyzers include the "Partica LA950-V2" (trade name) manufactured by Horiba, Ltd. and the "Coulter Counter III" (trade name) manufactured by Beckman Coulter. When performing SEM observation, the average particle size is determined by measuring 100 particles at random. When the number of inorganic porous particles is less than 100, the particle size is determined by measuring the particle size of all inorganic porous particles visible in the SEM image. The particle size is determined by the diameter of the circumscribed circle of the particle. Note that, when it is difficult to accurately determine the particle size due to the shape or shading of the inorganic porous particles, it is preferable to process the image using image processing software ImageJ and evaluate it. The average particle size of the inorganic porous particles in the porous molded body can also be measured using a particle size distribution analyzer or a scanning electron microscope (SEM).

[0027] Among inorganic porous particles, silica is preferred because it has various particle sizes and shapes and can produce porous particles with large pore volumes and pore sizes. Suitable examples include spherical porous silica with a particle size of 1 to 50 μm, amorphous porous silica with a particle size of 1 to 50 μm, and silica derived from rice husks.

[0028] Spherical porous silica is formed by the spherical aggregation of primary silica particles. The degree of sphericity can be defined by circularity, and in the present invention, a particle having a circularity of 0.80 or more is considered spherical. The greater the circularity and the closer to a perfect sphere, the larger the voids between the spherical porous silica particles in the molded product, allowing for larger pore volume and pore diameter of the molded product. Circularity can be calculated by determining the area and perimeter of particles from images obtained using a particle image analyzer (for example, Sysmex Corporation's "FPIA-3000S" (trade name)) using image analysis software attached to the device, and then applying this to the following formula (1): Circularity = perimeter of a circle with equal projected area / perimeter of a particle (1) In formula (1), the "perimeter of a circle with equal projected area" is the value obtained by determining the area of ​​the shadow of a particle A projected onto a flat surface below when the particle is observed from directly above, calculating a circle equal to this area, and then determining the length of the contour of that circle. The "perimeter of a particle" is the value obtained by determining the length of the contour of the shadow of a particle A projected onto a flat surface below when the particle is observed from directly above.

[0029] Rice husk-derived silica is a porous silica obtained by adding sodium hydroxide to the ash of burned rice husks to dissolve the silica component into a sodium silicate solution, which is then reacted with acid. Rice husk-derived silica has been attracting attention as a natural, environmentally friendly silica.

[0030] In the present invention, the porous molded body preferably contains inorganic porous particles in the range of 80 to 99% by mass. When the content of inorganic porous particles is 80% by mass or more, the molded body has sufficient pore volume and pore diameter, and when it is 99% by mass or less, the particles are sufficiently bonded to each other by the fibrous organic compound, resulting in a molded body with high mechanical strength. The content of inorganic porous particles is more preferably 90% by mass or more, even more preferably 95% by mass or more, and more preferably 98% by mass or less, and even more preferably 97% by mass or less.

[0031] The porous molded body preferably contains a fibrous organic compound in the range of 1 to 20% by mass. When the content of the fibrous organic compound is 1% by mass or more, the inorganic porous particles can be bonded to form aggregates, and when the content is 20% by mass or less, a molded body having sufficient pore volume and pore diameter can be formed. The content of the fibrous organic compound is more preferably 2% by mass or more, even more preferably 3% by mass or more, and more preferably 10% by mass or less, and even more preferably 5% by mass or less.

[0032] The porous molded body of the present invention is essentially composed of inorganic porous particles and a fibrous organic compound, but may contain 1% by mass or less of components that are inevitably contained due to the properties of the raw materials or the manufacturing process. Examples of components other than the inorganic porous particles and the fibrous organic compound include binders other than the fibrous organic compound, solvents, non-porous particles, etc. The content of such components is more preferably 0.5% by mass or less, and even more preferably 0.2% by mass or less.

[0033] <Method for producing porous molded body> The porous molded body is obtained by mixing and kneading inorganic porous particles, a fibrous organic compound, and water, molding the mixture, sizing the particles as necessary, and then drying the mixture in air at 200°C or lower.

[0034] First, inorganic porous particles, a fibrous organic compound, and water are mixed and kneaded, and then the kneaded mixture is molded. During molding, particle size adjustment may be performed as necessary. The inorganic porous particles are as described above, and the same applies to preferred inorganic porous particles. The fibrous organic compound is as described above, and the same applies to preferred fibrous organic compounds. The fibrous organic compound is used in the form of a water slurry, and the contents of the inorganic porous particles and the fibrous organic compound in the kneaded mixture are adjusted so that the contents of the inorganic porous particles and the fibrous organic compound in the resulting molded body are within the above-mentioned ranges in terms of solid content.

[0035] If necessary, other inorganic binders or organic binders may be added to the kneaded product, for example, to increase the mechanical strength of the molded body, or solvents such as water or alcohol may be added. Examples of inorganic binders include flaky silica, silica sol, alumina sol, and montmorillonite clay minerals. Examples of organic binders include polyvinyl alcohol, butyral resin, and acrylic resin.

[0036] The molding method is not particularly limited, and examples thereof include dry molding methods such as tableting and briquetting, as well as wet molding methods such as spray granulation, rolling granulation, stirring granulation, and extrusion molding. It is also possible to produce a molded body by injection molding. In the porous molded body of the present invention, the fibrous organic compound is in the form of a water slurry, so a wet molding method is preferred.

[0037] Among the wet molding methods, tumbling granulation is a method in which inorganic porous particles are placed in the pan of a pan granulator, and a fibrous organic compound and a solvent are added to granulate the particles while the pan is rotating at a speed of several tens of revolutions per minute. The inorganic porous particles and the fibrous organic compound aggregate due to the surface tension of the solvent and are molded into spheres, and the solvent is then dried to obtain spherical molded bodies with a diameter of 1 mm to 50 mm.

[0038] Agitation granulation is a method in which inorganic porous particles and a fibrous organic compound are placed in the container of an agitation granulator, and a solvent is added while rotating the agitator blades at a speed of several thousand revolutions per minute to granulate them. The inorganic porous particles and fibrous organic compound aggregate and form spheres due to the surface tension of the solvent, and the solvent is then dried to obtain relatively small spherical compacts with diameters of 1 mm to 10 mm.

[0039] In extrusion molding, inorganic porous particles, a fibrous organic compound, and a solvent are kneaded to form a clay-like substance, which is then extruded using an extrusion molding machine to form pellets or cylinders, for example, with a diameter of 1 mm to 10 mm and a length of 1 mm to 30 mm. The solvent is then dried to form a molded body. Spherical molded bodies can also be obtained by placing the extruded material in a granulator immediately after granulation and then drying the solvent. Alternatively, honeycomb molded bodies can be obtained by extrusion molding using a honeycomb die. Various sizes of honeycomb molded bodies can be obtained, ranging from cylindrical shapes with a diameter of 1 mm to 200 mm and a length of 10 to 500 mm, to rectangular pillars with cross-sectional dimensions of 1 mm x 1 mm to 200 mm x 200 mm and a length of 10 to 500 mm.

[0040] Examples of the shape of the molded body include general regular / irregular shapes such as spherical, elliptical, cylindrical, polygonal columnar, rod-shaped, conical, polygonal pyramidal, and irregular shapes combining these shapes, honeycomb shapes, and special shapes such as Raschig rings, Berl saddles, and Pall rings. When the packing efficiency is variable, it is preferable to use a molded body of a general shape, and when the mixing efficiency of the gas to be treated is desired to be improved, it is preferable to use a molded body of a special shape. A molded body of a special shape disrupts the gas flow to intensify mixing, increases the gas diffusion rate into the molded body, and allows the adsorbent to be uniformly distributed throughout the space even when the molded body storage space in the separation / recovery device is large. When molding a molded body into a special shape, the shape is not limited to the above-mentioned shapes as long as it can be made into a shape that increases the porosity.

[0041] Next, the obtained molded product is dried in air at a temperature of 200°C or less. This causes the inorganic porous particles to bond and aggregate with each other via the fibrous organic compound, resulting in the porous molded product of the present invention. When the drying temperature is 200°C or less, thermal decomposition of the fibrous organic compound is unlikely to occur, and the inorganic porous particles can be bound with a strong binder force. Furthermore, since there is little risk of the pores in the porous molded product disappearing, a porous molded product having a sufficiently large pore volume and pore diameter can be obtained. From the viewpoint of production efficiency, the drying temperature for the molded product is preferably 50°C or higher. That is, a range of 50 to 200°C is preferred. The drying temperature is more preferably 80°C or higher, and more preferably 150°C or lower.

[0042] <Physical Properties of Porous Molded Body> The porous molded body obtained as described above contains inorganic porous particles and a fibrous organic compound, which can be confirmed by, for example, SEM-EDS (energy dispersive X-ray spectroscopy) analysis.

[0043] The porous molded body of the present invention has a pore volume of 0.8 cm3 as determined by the nitrogen adsorption method. 3 / g or more 3.5cm 3 / g or less, the peak diameter of the pore diameter is preferably 20 nm or more and 100 nm or less, and the average pore diameter is preferably 15 nm or more and 50 nm or less. In other words, it is preferable that a molded body having a sufficiently large pore volume and a sufficiently large pore diameter is obtained. When the porous molded body has a pore volume and a pore diameter within the above range, the gas adsorbent having an amine compound supported on the porous molded body of the present invention is presumed to be able to easily allow the gas to be treated, specifically the acidic gas, to enter the pores of the adsorbent and also improve its diffusibility, thereby improving the recovery amount of the acidic gas.

[0044] The porous body has a pore volume of 0.8 cm 3 / g or more 3.5cm 3 The pore volume affects the amount of the amine compound supported in the porous molded body and the strength of the porous molded body. The larger the pore volume, the more the amine compound can be supported. 3 / g or more, the amount of adsorption of the gas to be treated can be increased. In addition, if the pore volume is too large, the strength of the porous molded body decreases, and it becomes impossible to maintain the strength required for the adsorbent. Therefore, the pore volume of the porous molded body is set to 3.5 cm 3 The lower limit of the pore volume of the porous molded body is 1.0 cm 3 / g or more, and the upper limit is 2.0 cm 3 / g or less is more preferable.

[0045] The pore volume is measured by obtaining an adsorption isotherm by nitrogen adsorption, and then measuring the amount of nitrogen gas adsorbed (BET method) when the relative pressure (adsorption equilibrium pressure / saturated vapor pressure) becomes 0.95. The pore volume of relatively large pores with a diameter of 0.2 μm or more can be measured using a mercury porosimeter. The inorganic porous particles forming the porous molded body preferably have an average particle diameter in the range of 1 μm to 1 mm. However, when particles with such a particle diameter are used, voids with a diameter of 0.2 μm or more may be formed between the particles. Pores derived from such voids can be measured using a mercury porosimeter.

[0046] Furthermore, the porous molded body preferably has a peak pore diameter of 20 nm or more and 100 nm or less, as determined by the nitrogen adsorption method. The peak pore diameter affects the diffusibility of the gas to be treated and the strength of the porous molded body. The larger the peak diameter, the more pore spaces with larger diameters there are on the surface and inside of the porous molded body, improving the diffusibility of the gas to be treated. If the peak diameter is 20 nm or more, the amount of adsorption of the gas to be treated can be increased. Furthermore, if the peak diameter is too large, the strength of the porous molded body decreases and it becomes impossible to maintain the strength required for the adsorbent, so the peak pore diameter is preferably 100 nm or less. The lower limit of the peak pore diameter of the porous molded body is more preferably 25 nm or more, and the upper limit is more preferably 50 nm or less.

[0047] The peak diameter of the pore diameter can be determined from the pore diameter that gives the peak top when the pore volume is plotted against the pore diameter as a pore diameter distribution curve obtained by a nitrogen adsorption method.

[0048] The porous molded body preferably has an average pore diameter of 15 nm or more and 50 nm or less, as determined by the nitrogen adsorption method. The average pore diameter affects the diffusibility of the gas to be treated and the strength of the porous molded body. The larger the average pore diameter, the more pore spaces of appropriate size (width) there are on the surface and inside of the porous molded body, improving the diffusibility of the gas to be treated. If the average pore diameter is 15 nm or more, the amount of adsorption of the gas to be treated can be increased. Furthermore, if the average pore diameter is too large, the strength of the porous molded body decreases and it becomes impossible to maintain the strength required for the adsorbent, so the average pore diameter of the porous molded body is preferably 50 nm or less. The lower limit of the average pore diameter of the porous body is more preferably 20 nm or more, and the upper limit is more preferably 40 nm or less.

[0049] The average pore diameter can be calculated from the specific surface area (S) of a sample determined based on an adsorption isotherm obtained by a nitrogen adsorption method and the pore volume (V) of the sample using the formula: D = 4V / S (where D represents the average pore diameter of the sample, V represents the pore volume of the sample, and S represents the specific surface area of ​​the sample).

[0050] The porous molded body has a specific surface area of ​​50 m2 as determined by a nitrogen adsorption method. 2 / g or more 1000m 2 The specific surface area affects the density of the amine compound present per specific surface area when the amine compound is supported on the porous molded body, and the diffusibility of the gas to be treated. 2 / g or less, the density per specific surface area of ​​the amine compound supported on the porous molded body becomes high, so that the amino groups of the amine compounds come close to each other, and the amino groups bond with the gas to be treated (specifically, acidic gas), thereby increasing the adsorption ability of the gas to be treated. Also, the number of very fine pores is reduced, and the pore space in the porous molded body is present at an appropriate size (width), improving the diffusibility of the gas to be treated and facilitating adsorption. If the specific surface area is too large, cracks may occur during the drying process for adjusting the porous molded body. If the specific surface area is 50 m or less, the amine compounds supported on the porous molded body become close to each other, and the amino groups bond with the gas to be treated (specifically, acidic gas), thereby increasing the adsorption ability of the gas to be treated. In addition, the number of very fine pores is reduced, and the pore space in the porous molded body is present at an appropriate size (width), improving the diffusibility of the gas to be treated and facilitating adsorption. If the specific surface area is too large, cracks may occur during the drying process for adjusting the porous molded body. 2 When the specific surface area of ​​the porous molded body is 100 m / g or more, the porous molded body can exhibit the ability to adsorb acidic gases.2 / g or more is more preferable, and the upper limit is 500m 2 / g or less is more preferable.

[0051] The specific surface area can be calculated using the BET theory after obtaining an adsorption isotherm by a nitrogen adsorption method.

[0052] The porous molded body of the present invention preferably has a compressive strength of 3.0 kgf or more. Compressive strength is an index of the mechanical strength of a porous molded body, and refers to the value obtained by applying a load to the porous molded body and measuring the load at which the porous molded body breaks. A compressive strength of 3.0 kgf or more can prevent the porous molded body from breaking and becoming powdery during handling or the operation of supporting the amine. The compressive strength is more preferably 4.0 kgf or more, even more preferably 4.5 kgf or more, and particularly preferably 5.0 kgf or more. Furthermore, since a higher compressive strength is preferable, there is no particular upper limit.

[0053] The compressive strength is measured by applying a load to a porous molded body in a dry state in a direction perpendicular to the axial direction of the porous molded body, and measuring the load at which the porous molded body breaks.

[0054] <Gas Adsorbent> The gas adsorbent of the present invention uses the porous molded body of the present invention. Examples of gases that can be adsorbed by the gas adsorbent include acidic gases, such as carbon dioxide, sulfur oxides (sulfur dioxide, sulfur trioxide, etc.), nitrogen oxides (NO, NO), and the like. 2 , NO 3 etc.), hydrogen chloride, etc.

[0055] In particular, the gas adsorbent of the present invention is preferably used as a gas adsorbent for adsorbing carbon dioxide by supporting an amine compound on a porous molded body. In this specification, such a gas adsorbent is also referred to as a carbon dioxide adsorbent. The carbon dioxide adsorbent is used to adsorb and remove carbon dioxide from a gas containing carbon dioxide (e.g., an acidic gas).

[0056] The amine compound has an amino group in its structure, and the amino group reacts with carbon dioxide to selectively adsorb carbon dioxide in the gas to be treated. Here, "supported" means that the amine compound is fixed to at least one of the surface and the inner surface of the pores of the porous molded body, or is filled into the pores of the porous molded body.

[0057] The amine compound is preferably an amine compound containing at least one ether-bonded oxygen atom or siloxane-bonded oxygen atom in the molecule. "Containing at least one ether-bonded oxygen atom or siloxane-bonded oxygen atom in the molecule" means that the amine compound has an oxygen atom derived from an ether bond (C-O-C) or an oxygen atom derived from a siloxane bond (Si-O-Si) in the molecule.

[0058] Examples of the amine compound having at least one ether-bonding oxygen atom in the molecule include amines containing an alkylenedioxy group having 1 to 20 carbon atoms as a partial structure in the molecule.

[0059] Examples of the alkylenedioxy group having 1 to 20 carbon atoms include a methylenedioxy group, an ethylenedioxy group, a propylenedioxy group, an isopropylenedioxy group, a butylenedioxy group, a 2,3-butanedioxy group, a pentylenedioxy group, a 2,4-pentanedioxy group, a 1,3-cyclopentanedioxy group, a hexanedioxy group, a 2,5-hexyldioxy group, a 1,3-cyclohexyldioxy group, a 1,4-cyclohexyldioxy group, a heptylenedioxy group, a 2,4-dimethyl-2,4-pentyldioxy group, an octylenedioxy group, Examples of such alkyl groups include a 5-dimethyl-2,5-hexyldioxy group, a 1,4-cyclohexanedimethyldioxy group, a nonanedioxy group, a 2,4-diethyl-1,5-pentanedioxy group, a 2-butyl-2-ethyl-1,3-propanedioxy group, a decanedioxy group, a 2,2-dibutyl-1,3-propylenedioxy group, a 1,12-dodecanedioxy group, a 4,4'-bicyclohexanedioxy group, a 1,14-tetradecanedioxy group, a 1,16-hexadecanedioxy group, a 1,18-octadecanedioxy group, and a 1,20-eicosanedioxy group.

[0060] Specific examples of amines containing an alkylenedioxy group having 1 to 20 carbon atoms in the molecule as a partial structure include 1,2-bis(2-aminoethoxy)ethane, 1,4-butanediol bis(3-aminopropyl)ether, diethylene glycol bis(3-aminopropyl)ether, α-(2-aminomethylethyl)-ω-(2-aminomethylethoxy)poly(oxypropylene), 1,14-diamino-3,6,9,12-tetraoxatetradecane, ethylene glycol bis(3-aminopropyl)ether, triglycolamine, PEG diamine 2000, and PEG diamine 8000.

[0061] Among these, the amine compound having at least one ether-bonding oxygen atom in the molecule is preferably an amine containing an alkylenedioxy group having 1 to 6 carbon atoms as a partial structure in the molecule, from the viewpoints of availability, amine value, boiling point, viscosity, etc., and more preferably an amine containing an ethylenedioxy group, an isopropylenedioxy group, or a butylenedioxy group as a partial structure in the molecule.

[0062] Examples of amine compounds having at least one siloxane-bonding oxygen atom in the molecule include amines containing a linear siloxane structure as a partial structure, and amines containing a cyclic siloxane structure as a partial structure.

[0063] That is, in the present invention, the amine compound is preferably an amine containing, as a partial structure in the molecule, at least one selected from the group consisting of an ethylenedioxy group, an isopropylenedioxy group, a butylenedioxy group, a linear siloxane structure, and a cyclic siloxane structure.

[0064] Examples of amines containing a linear siloxane structure as a partial structure include amines represented by the following formula (I).

[0065]

[0066] (In formula (I), R 1 ~R 6each independently represents a methyl group, a phenyl group, an aminopropyl group, an aminooctyl group, an N-2-(aminoethyl)-3-aminomethyl group, an N-2-(aminoethyl)-3-aminopropyl group, an N-2-(aminoethyl)-3-aminooctyl group, an N-phenyl-3-aminopropyl group, an N-butyl-3-aminopropyl group, or a 3,3-dimethyl-4-aminobutyl group, and n is an integer of 1 to 99. When n is 2 or more, a plurality of R 1 and R 2 may be the same or different.)

[0067] In formula (I), R 1 ~R 6 R each independently represents a methyl group, a phenyl group, an aminopropyl group, an aminooctyl group, an N-2-(aminoethyl)-3-aminomethyl group, an N-2-(aminoethyl)-3-aminopropyl group, an N-2-(aminoethyl)-3-aminooctyl group, an N-phenyl-3-aminopropyl group, an N-butyl-3-aminopropyl group, or a 3,3-dimethyl-4-aminobutyl group. 1 ~R 6 are each independently preferably a methyl group, a phenyl group, an aminopropyl group, an aminooctyl group, or an N-2-(aminoethyl)-3-aminooctyl group. 1 ~R 4 R is preferably a methyl group or a phenyl group, and from the viewpoint of the amine value and viscosity, is more preferably a methyl group. 5 and R 6 are more preferably an aminopropyl group, an aminooctyl group, or an N-2-(aminoethyl)-3-aminooctyl group, respectively, and from the viewpoint of availability, an aminopropyl group is even more preferred.

[0068] n is an integer of 1 to 99. n is preferably an integer of 1 to 50, more preferably an integer of 1 to 9, and even more preferably an integer of 1 to 4. When n is 2 or more, a plurality of R 1 and R 2 may be the same or different.

[0069] Specific examples of preferred amines represented by formula (I) include 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 1,5-bis(3-aminopropyl)hexamethyltrisiloxane, 1,7-bis(3-aminopropyl)octamethyltetrasiloxane, and 1,9-bis(3-aminopropyl)decamethylpentasiloxane.

[0070] Examples of amines containing a cyclic siloxane structure as a partial structure include amines represented by the following formula (II).

[0071]

[0072] (In formula (II), R 11 ~R 18 each independently represents a methyl group, a phenyl group, an aminopropyl group, an aminooctyl group, an N-2-(aminoethyl)-3-aminomethyl group, an N-2-(aminoethyl)-3-aminopropyl group, an N-2-(aminoethyl)-3-aminooctyl group, an N-phenyl-3-aminopropyl group, an N-methyl-3-aminopropyl group, an N-butyl-3-aminopropyl group, an N-tertiary butyl-3-aminopropyl group, an N-cyclohexyl-3-aminopropyl group, or a 3,3-dimethyl-4-aminobutyl group, p is an integer of 1 or more, and q is an integer of 0 or more. When p and q are 2 or more, a plurality of R 11 , R 12 , R 13 and R 14 may be the same or different.)

[0073] In formula (II), R 11 ~R 18 R each independently represents a methyl group, a phenyl group, an aminopropyl group, an aminooctyl group, an N-2-(aminoethyl)-3-aminomethyl group, an N-2-(aminoethyl)-3-aminopropyl group, an N-2-(aminoethyl)-3-aminooctyl group, an N-phenyl-3-aminopropyl group, an N-methyl-3-aminopropyl group, an N-butyl-3-aminopropyl group, an N-tertiary butyl-3-aminopropyl group, an N-cyclohexyl-3-aminopropyl group, or a 3,3-dimethyl-4-aminobutyl group. 11~R 18 are each independently preferably a methyl group, a phenyl group, an aminopropyl group, an aminooctyl group, or an N-2-(aminoethyl)-3-aminooctyl group. 11 ~R 16 R is preferably a methyl group or a phenyl group, and from the viewpoint of the amine value and viscosity, is more preferably a methyl group. 17 and R 18 are more preferably an aminopropyl group, an aminooctyl group, or an N-2-(aminoethyl)-3-aminooctyl group, respectively, and from the viewpoint of availability, an aminopropyl group is even more preferred.

[0074] p is an integer of 1 or more, and q is an integer of 0 or more. When p and q are 2 or more, a plurality of R 11 , R 12 , R 13 and R 14 may be the same or different. The sum of p and q is preferably 1 to 18, and more preferably 1 to 4.

[0075] Specific examples of preferred amines represented by formula (II) include 1,5-bis(3-aminopropyl)hexamethylcyclotetrasiloxane and 1,3,5,7-tetrakis(3-aminopropyl)tetramethylcyclotetrasiloxane.

[0076] The amine compound is preferably an amine that is liquid at room temperature and contains two or more of a primary amine and a secondary amine. When the amine compound contains two or more of a primary amine and a secondary amine, a sufficient amount of carbon dioxide adsorption can be obtained. Furthermore, being liquid at room temperature provides good gas diffusibility for carbon dioxide, making it suitable for use in DAC (Direct Air Capture) and for capturing carbon dioxide contained in exhaust gas. In this specification, "room temperature" means room temperature as defined in the 17th Edition of the Japanese Pharmacopoeia, specifically referring to a temperature range of 1 to 30°C.

[0077] Furthermore, the amine compound is preferably an amine having a boiling point of 250°C or higher at 760 mmHg. When the boiling point of the amine compound is 250°C or higher, it is less likely to volatilize even in a high-temperature environment, and therefore it is possible to suppress attenuation of the carbon dioxide adsorption ability when carbon dioxide is repeatedly adsorbed and desorbed. The boiling point of the amine compound is more preferably 270°C or higher, and even more preferably 300°C or higher. The upper limit is not particularly limited, as the higher the boiling point of the amine compound, the more the volatilization due to evaporation is suppressed.

[0078] The above amine compounds may be used as a single compound or as a mixture.

[0079] The method for supporting an amine compound on a porous molded body is not particularly limited, and examples thereof include the following methods (1) and (2): (1) Filling the pores of a porous molded body with an amine compound; (2) Filling the pores of a porous molded body with a precursor of an amine compound and reacting it in the pores to fill the pores with the desired amine compound. Either method (1) or method (2) may be used, or both methods may be combined.

[0080] In the method (1), the gas adsorbent of the present invention is obtained by contacting an amine compound with the porous molded body of the present invention, and if necessary, heating and maintaining the amine compound therein. The amine compound may be contacted with the porous molded body either directly in a liquid form or as an amine solution dissolved in a solvent.

[0081] Examples of the solvent include water, alcohols, ethers, esters, amines, and amides. Among them, alcohols are preferably used from the viewpoints of availability and ease of removal after contact with the porous molded body. It is more preferable to contact the amine compound directly without a solvent, from the viewpoint of eliminating the need for a solvent removal step.

[0082] The concentration of the amine compound in the amine solution is preferably 10 to 100% by mass, more preferably 25% by mass or more, and even more preferably 30% by mass or more, from the viewpoint of increasing the contact efficiency with the porous molded body and the amount supported.

[0083] The amine solution may contain other components as long as the effects of the present invention are not impaired. Examples of other components include amine compounds containing one or two amino groups in the molecule.

[0084] The contact of the amine solution with the porous molded body can be carried out by a conventionally known method, such as a method of immersing the porous molded body in the amine solution, a method of adding the amine solution dropwise or spraying it onto the porous molded body, a method of precipitating the porous molded body in the amine solution, etc. Among these, from the viewpoint of ease of operation, the method of adding the amine solution dropwise or spraying it onto the porous molded body is preferred.

[0085] After contacting the amine solution with the porous molded body, the mixture is allowed to stand at 20 to 150°C for 1 to 48 hours, with stirring optional. A reaction temperature of 20°C or higher reduces the viscosity of the amine compound, allowing the amine compound to more easily fill the pores of the porous molded body. A reaction temperature of 150°C or lower inhibits oxidation of the amine compound and prevents the amine compound from scattering before reaction. The reaction temperature is preferably 20°C or higher, more preferably 25°C or higher, and preferably 150°C or lower, more preferably 100°C or lower. A reaction time of 1 hour or longer ensures sufficient filling of the amine compound into the pores of the porous molded body, while a reaction time of 48 hours or shorter shortens the manufacturing process. The reaction time is preferably 1 hour or longer, more preferably 2 hours or longer, and preferably 48 hours or shorter, more preferably 24 hours or shorter.

[0086] After the reaction, a drying step can be carried out if necessary. Drying can be carried out at 20 to 150° C. for about 1 to 24 hours. The drying step can be carried out under reduced pressure.

[0087] In the method (2), a precursor of an amine compound is used. The gas adsorbent of the present invention can be obtained by contacting the precursor of the amine compound with the porous molded body of the present invention and reacting them by leaving them for a certain period of time or by heating. The precursor of the amine compound may be dissolved in a solvent, or multiple amine compounds may be mixed.

[0088] Examples of the solvent include water, alcohols, ethers, esters, amines, and amides. Among them, alcohols are preferably used from the viewpoints of availability and ease of removal after contact with the inorganic porous material. It is more preferable to contact the precursor of the amine compound directly without a solvent, since this eliminates the need for a removal step.

[0089] Examples of precursors of amine compounds include M- and D-aminosilane coupling agents and 2,4,6,8-tetramethylcyclotetrasiloxane. M-aminosilane coupling agents have one condensable alkoxy group, and therefore give a linear dimeric aminosiloxane compound through a condensation reaction. D-aminosilane coupling agents have two condensable alkoxy groups, and therefore give a linear aminosiloxane compound of dimer or higher, or a cyclic aminosiloxane compound of trimer or higher, through a condensation reaction. 2,4,6,8-tetramethylcyclotetrasiloxane can react with unsaturated amines in the presence of a catalyst, and give a cyclic aminosiloxane compound through the reaction.

[0090] The concentration of the amine compound precursor in the solution is preferably 20 to 100% by mass, more preferably 25% by mass or more, and even more preferably 30% by mass or more, from the viewpoint of increasing the contact efficiency with the porous molded body and the amount supported.

[0091] The solution of the precursor of the amine compound may contain other components, such as platinum, ruthenium, and rhodium, as long as the effects of the present invention are not impaired.

[0092] The contact of the amine compound precursor solution with the porous molded body can be carried out by a conventionally known method, such as a method of immersing the porous molded body in the amine compound precursor solution, a method of adding the amine compound precursor solution dropwise or spraying it onto the porous molded body, a method of precipitating the porous molded body in the amine compound precursor solution, etc. Among these, from the viewpoint of ease of operation, the method of adding the amine compound precursor solution dropwise or spraying it onto the porous molded body is preferred.

[0093] After contacting the solution of the amine compound precursor with the porous molded body, the reaction is preferably carried out at 20 to 150°C for 1 to 48 hours. A reaction temperature of 20°C or higher allows the reaction of the amine compound precursor to proceed rapidly, while a reaction temperature of 150°C or lower suppresses oxidation of the amine compound and prevents the amine compound from scattering before reacting. The reaction temperature is preferably 20°C or higher, more preferably 40°C or higher, and preferably 150°C or lower, more preferably 100°C or lower. A reaction time of 1 hour or longer allows the reaction of the amine compound precursor to proceed sufficiently, while a reaction time of 48 hours or shorter shortens the manufacturing process. The reaction time is preferably 1 hour or longer, more preferably 2 hours or longer, and preferably 48 hours or shorter, more preferably 24 hours or shorter. If reactive functional groups are present on the surface of the porous molded body, the reaction between the amine compound precursor and the surface of the porous molded body also proceeds.

[0094] After the reaction, a drying step can be carried out under reduced pressure, if necessary. Drying can be carried out at 20 to 150°C for about 1 to 24 hours.

[0095] The amount of amine compound supported in a gas adsorbent (carbon dioxide adsorbent) on which the amine compound is supported can be confirmed by the content of nitrogen atoms and oxygen atoms in the adsorbent. It is preferable that the nitrogen atom content of the amine compound in the carbon dioxide adsorbent is 1% by mass or more and 20% by mass or less, and the oxygen atom content of the amine compound in the carbon dioxide adsorbent is 1% by mass or more and 20% by mass or less. A nitrogen atom content of 1% by mass or more can improve the amount of acidic gas adsorption, and a content of 20% by mass or less can prevent the adsorbent from becoming sticky due to excess amine compound exceeding the pore volume of the porous molded body, making it easy to handle. Furthermore, a content of oxygen atoms of 1% by mass or more can improve the effective utilization rate of the amine by improving the diffusibility of acidic gases, and a content of 20% by mass or less can prevent the adsorbent from becoming sticky due to excess amine compound exceeding the pore volume of the porous molded body, making it easy to handle. The nitrogen atom content of the amine compound in the carbon dioxide adsorbent is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and preferably 20% by mass or less, more preferably 18% by mass or less, and even more preferably 15% by mass or less. The oxygen atom content of the amine compound in the adsorbent that adsorbs acidic gases is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and preferably 20% by mass or less, more preferably 18% by mass or less, and even more preferably 15% by mass or less.

[0096] The content of nitrogen atoms and oxygen atoms of the amine compound in the carbon dioxide adsorbent can be calculated from the mass ratio of nitrogen atoms or oxygen atoms to the total atomic mass of the porous molded body and the supported amine compound.

[0097] Examples of gases to be treated using the gas adsorbent of the present invention include the atmosphere, fuel exhaust gases from automobiles and factories, industrial gases such as helium gas and nitrogen gas, and gases emitted by human breathing or energy conversion in equipment in enclosed spaces such as space stations.

[0098] When a carbon dioxide-containing gas to be treated is treated using a carbon dioxide adsorbent carrying an amine compound, the concentration of carbon dioxide in the gas to be treated is not particularly limited as long as the conditions are tolerable to the carbon dioxide adsorbent, but for example, it is preferably 100% by volume or less, more preferably 50% by volume or less, and even more preferably 30% by volume or less. The lower limit is not particularly limited, but it is preferably 0.01% by volume or more. The gas to be treated may be at atmospheric pressure or may be pressurized.

[0099] Examples of methods for adsorbing and desorbing carbon dioxide include the pressure swing method (PSA method) in which adsorption and desorption are performed by utilizing a pressure difference, the thermal swing method (TSA method) in which adsorption and desorption are performed by utilizing a temperature difference, and a method in which the gas to be treated is brought into contact with a carbon dioxide adsorbent to adsorb it, and then an inert gas that does not contain carbon dioxide is brought into contact with it to desorb it.

[0100] In the PSA method, since the higher the total pressure of the atmosphere in which the carbon dioxide adsorbent is present (for example, the total pressure in a vessel containing the carbon dioxide adsorbent), the greater the amount of carbon dioxide adsorbed, it is preferable to change the total pressure in the desorption step to be lower than the total pressure in the adsorption step. The total pressure may be adjusted by pressurizing or depressurizing, or by using pressurization and depressurization in combination.

[0101] In the TSA method, for example, the temperature of the carbon dioxide adsorbent in the desorption step is set higher than that in the adsorption step. Methods for heating the carbon dioxide adsorbent include a method in which heated gas to be treated is brought into direct contact with the carbon dioxide adsorbent, a method in which the carbon dioxide adsorbent is heated by heat conduction from the heat transfer surface of a heat transfer tube or the like, and a method in which the carbon dioxide adsorbent is heated in an electric furnace or the like.

[0102] In the method of adsorption and desorption using an inert gas that does not contain carbon dioxide, the gas to be treated is brought into contact with a carbon dioxide adsorbent to adsorb the acidic gas onto the carbon dioxide adsorbent, and then the inert gas is brought into contact with the carbon dioxide adsorbent to which the carbon dioxide has been adsorbed. As a result, the acidic gas adsorbed onto the carbon dioxide adsorbent is replaced with the inert gas, and the acidic gas can be recovered. Any inert gas may be used as long as the carbon dioxide adsorbent is stable in that gas, and examples thereof include water vapor, argon, and nitrogen.

[0103] The carbon dioxide adsorbent can be reused for adsorption by undergoing a desorption step after the adsorption step.

[0104] As described above, the present specification discloses the following configurations. <1> A porous molded body substantially consisting of inorganic porous particles and a fibrous organic compound. <2> The porous molded body according to <1>, wherein the fibrous organic compound is at least one nanofiber selected from the group consisting of cellulose, chitin, and chitosan. <3> The porous molded body according to <1> or <2>, wherein the inorganic porous particles include at least one selected from the group consisting of silica, zeolite, alumina, silica-alumina, titania, aluminum silicate, magnesium silicate, and clay minerals. <4> The porous molded body has a pore volume of 0.8 cm3 as determined by a nitrogen adsorption method. 3 / g or more 3.5cm 3 The porous molded body according to any one of <1> to <3>, having a pore size of 1 / g or less, a peak pore size diameter of 20 nm or more and 100 nm or less, and an average pore size of 15 nm or more and 50 nm or less. <5> A method for producing the porous molded body according to any one of <1> to <4>, comprising mixing and kneading inorganic porous particles, a fibrous organic compound, and water, shaping the mixture, optionally sizing the particles, and then drying in air at 200°C or less. <6> A gas adsorbent using the porous molded body according to any one of <1> to <4>. <7> The gas adsorbent according to <6>, for adsorbing carbon dioxide, wherein an amine compound is supported on the porous molded body. <8> The gas adsorbent according to <7>, wherein the amine compound is an amine containing at least one ether-bonded oxygen atom or siloxane-bonded oxygen atom in the molecule. <9> The gas adsorbent according to <7> or <8>, wherein the amine compound is an amine containing at least one selected from the group consisting of an ethylenedioxy group, an isopropylenedioxy group, a butylenedioxy group, a linear siloxane structure, and a cyclic siloxane structure as a partial structure in the molecule. <10> The gas adsorbent according to any one of <7> to <9>, wherein the amine compound is an amine having a boiling point of 250°C or higher at 760 mmHg.

[0105] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" and "%" represent "parts by mass" and "% by mass", respectively. Examples 1 to 3 are working examples, and Examples 4 to 6 are comparative examples.

[0106] <Evaluation Method> The porous molded bodies and carbon dioxide adsorbents of Examples 1 to 6 were evaluated as follows.

[0107] (Average particle size) The average particle sizes of "Sunsphere (registered trademark) H32" manufactured by AGC Si-Tech Co., Ltd. and "Sunsphere (registered trademark) L123" manufactured by AGC Si-Tech Co., Ltd. were measured using a Coulter Counter (Coulter Counter III manufactured by Beckman). The average particle sizes of "Sunpera L303" manufactured by AGC Si-Tech Co., Ltd. and rice husk-derived silica were measured using a laser diffraction scattering particle size distribution analyzer (Horiba Partica LA-950V2 manufactured by Horiba, Ltd.).

[0108] (Pore volume, peak diameter, and average pore diameter of porous molded body) The pore volume, peak diameter, and average pore diameter of the porous molded body by nitrogen adsorption method were determined using a specific surface area / pore size distribution measuring device (TriStar II 3020 model, manufactured by Micromeritics Co., Ltd.) The measurements were performed by the BET method and the BJH method based on the nitrogen adsorption method.

[0109] (Compressive Strength of Porous Molded Body) The compressive strength of the porous molded body was determined using a digital hardness tester (KHT-40N model, manufactured by Fujiwara Seisakusho Co., Ltd.) A load was applied to the cylindrical molded body in a direction parallel to the circular cross section (direction perpendicular to the axial direction), and the load at which the molded body broke was read.

[0110] (Nitrogen Atom Content in Carbon Dioxide Adsorbent) The nitrogen atom content in the carbon dioxide adsorbent was determined by dividing the mass of nitrogen atoms in the supported amine compound by the sum of the atomic masses of the porous molded body and the atomic masses of the amine compound supported on the porous molded body. Nitrogen atom content (%) of amine compound = {(mass of nitrogen atoms in supported amine compound) / (sum of the atomic masses of the porous molded body and the atomic masses of the amine compound supported on the porous molded body)} × 100

[0111] (Oxygen Atom Content in Carbon Dioxide Adsorbent) The oxygen atom content of the carbon dioxide adsorbent was determined by dividing the mass of oxygen atoms in the supported amine compound by the sum of the mass of each atom in the porous molded body and the mass of each atom in the amine compound supported on the porous molded body. Oxygen atom content of amine compound (%) = {(mass of oxygen atoms in supported amine compound) / (sum of the mass of each atom in the porous molded body and the mass of each atom in the amine compound supported on the porous molded body)} × 100

[0112] (Carbon dioxide adsorption amount) Using a carbon dioxide gas cylinder, a nitrogen gas cylinder, a mass flow controller, and a plastic sample tube (inner diameter 15 mm), the change in carbon dioxide adsorption amount over time (carbon dioxide adsorption curve) was measured according to the following procedure, and the carbon dioxide adsorption amount of the adsorbent was calculated. 1. The sample tube was filled with 0.7 g of the adsorbent obtained in each example. 2. At room temperature, carbon dioxide diluted with nitrogen to a concentration of 10% by volume was introduced into the sample tube via the mass flow controller at a flow rate of 50 ml / min for 30 minutes. 3. The weight of the adsorbent was measured every 10 minutes to obtain a carbon dioxide adsorption curve for the adsorbent. The amount of carbon dioxide adsorbed by the adsorbent was calculated from the increase in weight of the adsorbent after 30 minutes.

[0113] Example 1 5.6 parts of spherical porous silica powder having an average particle size of 3 μm (manufactured by AGC Si-Tech Co., Ltd., Sunsphere (registered trademark) H32, moisture content: 4.5%), 16.9 parts of spherical porous silica powder having an average particle size of 35 μm (manufactured by AGC Si-Tech Co., Ltd., Sunspera L303, moisture content: 4.7%), 60.3 parts of cellulose nanofiber (manufactured by Nippon Paper Industries Co., Ltd., Cellenpia TC-01A, solid content: 1.1%), and 17.2 parts of ion-exchanged water were weighed into a polyethylene container having an internal volume of 150 ml, and the mixture was kneaded for 5 minutes using a kneader "Awatori Rentaro" (trade name, manufactured by Thinky Corporation) to obtain a kneaded product. The solids concentration in the kneaded product was 22.1%, and the composition of the solids was H32:L303:Cellenpia = 24.2:72.8:3.0 in mass ratio. This kneaded product was placed in a polyethylene bag equipped with a nozzle having an inner diameter of 5 mm, and the bag was squeezed to extrude the kneaded product from the tip of the nozzle into a cylindrical shape having a diameter of 5 mm. The extrudate was dried at 110°C for 2 hours and cut to a length of 5 mm after drying to obtain a cylindrical pellet-shaped porous molded product A having a diameter of 5 mm and an axial length of 5 mm. The compressive strength and pore physical properties of the obtained porous molded product A measured by a nitrogen adsorption method are shown in Table 1. Porous molded product A had a high compressive strength (4.8 kgf), and also had large pore volume, peak pore diameter, and average pore diameter measured by a nitrogen adsorption method (pore volume = 1.52 cm). 3 / g, pore diameter peak diameter = 42 nm, average pore diameter = 18 nm).

[0114] An amine compound was supported on this porous molded body A as follows to prepare a carbon dioxide adsorbent. First, 1.0 g of the porous molded body was weighed into a glass vial, and the pore volume was calculated from the mass. An amine compound (α-(2-methylethyl)-ω-(2-aminomethylethoxy)poly(oxypropylene)) equivalent to 100% of the calculated pore volume was weighed into another glass vial. 3.0 g of methanol was weighed and added to the porous molded body in the glass vial with a plastic dropper to prepare a suspension. Next, the weighed amine compound was added dropwise to the suspension with a plastic dropper, and the suspension was thoroughly shaken to achieve a uniform concentration. The suspension was then transferred to a recovery flask and the pressure was reduced for 1 hour while the temperature was maintained at 24°C using a rotary evaporator (EYELA: N-1210B model), thereby removing the methanol. The mixture was then placed in a glass bell jar, and the methanol was completely evaporated under a nitrogen gas atmosphere to obtain a carbon dioxide adsorbent. The nitrogen atom content of the amine in the obtained carbon dioxide adsorbent was 7.2%, and the oxygen atom content was 11.0%. The carbon dioxide adsorption capacity of the carbon dioxide adsorbent was 0.100 (g-CO 2 / g-adsorbent).

[0115] Example 2 23.0 parts of spherical porous silica powder (manufactured by AGC Si-Tech Co., Ltd., Sunsphere (registered trademark) L123, moisture content: 5.4%) having an average particle size of 14 μm, 61.1 parts of the same cellulose nanofibers as in Example 1, and 15.9 parts of ion-exchanged water were weighed into a 150 ml polyethylene container and kneaded for 5 minutes using a kneader "Awatori Rentaro" (trade name, manufactured by Thinky Corporation) to obtain a kneaded mixture. The solids concentration in the kneaded mixture was 22.4%, and the solid composition was L123:Cellenpia = 97.0:3.0 by mass. Pellet-shaped porous molded body B was obtained from this kneaded mixture in the same manner as in Example 1. The compressive strength and pore physical properties of the obtained porous molded body B measured by nitrogen adsorption are shown in Table 1. Porous molded body B also had high compressive strength, and the pore volume, peak pore diameter, and average pore diameter measured by nitrogen adsorption were also large.

[0116] An amine compound was supported on this porous molded body B in the same manner as in Example 1 to prepare a carbon dioxide adsorbent. The nitrogen atom content of the amine in the obtained carbon dioxide adsorbent was 6.7%, and the oxygen atom content was 10.3%. The carbon dioxide adsorption capacity of the carbon dioxide adsorbent was 0.095 (g-CO 2 / g-adsorbent).

[0117] Example 3: 20.3 parts of rice husk-derived amorphous porous silica powder (manufactured by BSB Nanotech, Biosilico, moisture content: 7.4%) with an average particle size of 8 μm, 52.9 parts of the same cellulose nanofibers as in Example 1, and 26.8 parts of ion-exchanged water were weighed into a 150 ml polyethylene container and kneaded for 5 minutes using a kneader "Awatori Rentaro" (trade name, manufactured by Thinky Corporation) to obtain a kneaded mixture. The solids concentration in the kneaded mixture was 19.4%, and the solid composition was a mass ratio of rice husk-derived silica to cellenpia = 97.0:3.0. Pellet-shaped porous molded body C was obtained from this kneaded mixture in the same manner as in Example 1. The compressive strength and pore physical properties of the obtained porous molded body C measured by nitrogen adsorption are shown in Table 1. Porous molded body C also had high compressive strength, and the pore volume, peak pore diameter, and average pore diameter measured by nitrogen adsorption were also large.

[0118] An amine compound was supported on this porous molded body C in the same manner as in Example 1 to prepare a carbon dioxide adsorbent. The nitrogen atom content of the amine in the obtained carbon dioxide adsorbent was 6.3%, and the oxygen atom content was 9.7%. The carbon dioxide adsorption capacity of the carbon dioxide adsorbent was 0.090 (g-CO 2 / g-adsorbent).

[0119] (Example 4) An attempt was made to obtain a porous molded body using scaly silica as an inorganic binder instead of the cellulose nanofibers used in Example 1. A kneaded product was obtained in the same manner as in Example 1 using 6.7 parts of spherical porous silica powder having an average particle size of 3 μm (manufactured by AGC Si-Tech Co., Ltd., Sunsphere (registered trademark) H32, moisture content: 4.5%), 20.2 parts of spherical porous silica powder having an average particle size of 35 μm (manufactured by AGC Si-Tech Co., Ltd., Sunpera L303, moisture content: 4.7%), 6.1 parts of scaly silica slurry (manufactured by AGC Si-Tech Co., Ltd., Sunlovely PN-050, moisture content: solids concentration: 13.0%), and 67.0 parts of ion-exchanged water. The solids concentration in the kneaded product was 26.5%, and the solids composition was H32:L303:scaly silica = 24.2:72.8:3.0 in mass ratio. This kneaded product was extruded into a cylindrical shape in the same manner as in Example 1, dried at 110°C for 2 hours, and cut to a length of 5 mm after drying to obtain a cylindrical pellet-shaped porous molded product D with a diameter of 5 mm and an axial length of 5 mm. The obtained porous molded product D had very low compressive strength (0.4 kgf) and was powdered during the operation of supporting the amine compound, so a carbon dioxide adsorbent could not be obtained.

[0120] Example 5 An attempt was made to obtain a porous molded body using scaly silica as an inorganic binder instead of the cellulose nanofibers used in Example 2. A kneaded product was obtained in the same manner as in Example 2 using 26.4 parts of spherical porous silica powder having an average particle size of 14 μm (Sunsphere (registered trademark) L123, moisture content: 5.4%, manufactured by AGC Si-Tech Co., Ltd.), 5.9 parts of scaly silica slurry (Sunlovely PN-050, moisture content: 13.0%, manufactured by AGC Si-Tech Co., Ltd.), and 67.7 parts of ion-exchanged water. The solids concentration in the kneaded product was 25.7%, and the solids composition was L123:scaly silica = 97.0:3.0 by mass ratio. This kneaded product was extruded into a cylindrical shape in the same manner as in Example 2, dried at 110°C for 2 hours, and cut to a length of 5 mm after drying to obtain a cylindrical pellet-shaped porous molded body E having a diameter of 5 mm and an axial length of 5 mm. The obtained porous molded body E had very low compressive strength (0.2 kgf) and was powdered during the operation of supporting the amine compound, so a carbon dioxide adsorbent could not be obtained.

[0121] (Example 6) An attempt was made to obtain a porous molded body using scaly silica as an inorganic binder instead of the cellulose nanofibers used in Example 3. A kneaded product was obtained in the same manner as in Example 3 using 19.5 parts of rice husk-derived amorphous porous silica powder (manufactured by BSB Nanotech, Biosilico, moisture content: 7.4%) with an average particle size of 8 μm, 4.3 parts of scaly silica slurry (manufactured by AGC Si-Tech Co., Ltd., Sun Lovely PN-050, moisture content: solids concentration: 13.0%), and 76.2 parts of ion-exchanged water. The solids concentration in the kneaded product was 18.6%, and the solid composition was rice husk-derived silica:scaly silica = 97.0:3.0 by mass ratio. This kneaded product was extruded into a cylindrical shape in the same manner as in Example 3, dried at 110°C for 2 hours, and cut to a length of 5 mm after drying to obtain a cylindrical pellet-shaped porous molded body F having a diameter of 5 mm and an axial length of 5 mm. The obtained porous molded body F had very low compressive strength (0.4 kgf) and was powdered during the operation of supporting the amine compound, so a carbon dioxide adsorbent could not be obtained.

[0122]

[0123] The results in Table 1 show that in Examples 1 to 3, porous molded bodies were obtained from inorganic porous particles and fibrous organic compounds, which had high mechanical strength and large pore volumes, peak pore diameters, and average pore diameters measured by nitrogen adsorption. It was found that carbon dioxide adsorbents loaded with an amine compound on these bodies had high carbon dioxide adsorption capacity and excellent carbon dioxide adsorption capacity. On the other hand, in Examples 4 to 6, no fibrous organic compound was used, and therefore the mechanical strength of the molded bodies was very weak, and no carbon dioxide adsorbents were obtained.

[0124] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made thereto without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-088126) filed on May 29, 2023, the contents of which are incorporated herein by reference.

Claims

1. A porous molded body consisting essentially of inorganic porous particles and a fibrous organic compound.

2. The porous molded body according to claim 1, wherein the fibrous organic compound is at least one nanofiber selected from the group consisting of cellulose, chitin and chitosan.

3. The porous molded body according to claim 1, wherein the inorganic porous particles comprise at least one selected from the group consisting of silica, zeolite, alumina, silica alumina, titania, aluminum silicate, magnesium silicate and clay minerals.

4. The porous molded body has a pore volume of 0.8 cm3 as determined by a nitrogen adsorption method. 3 / g or more 3.5cm 3 2. The porous molded body according to claim 1, wherein the pore diameter is 20 nm or more and 100 nm or less, and the average pore diameter is 15 nm or more and 50 nm or less.

5. A method for producing a porous molded body according to any one of claims 1 to 4, comprising mixing and kneading inorganic porous particles, a fibrous organic compound and water, molding the mixture, sizing the particles as necessary, and then drying the mixture in air at 200°C or lower.

6. A gas adsorbent using the porous molded body according to any one of claims 1 to 4.

7. The gas adsorbent according to claim 6, for adsorbing carbon dioxide, wherein an amine compound is supported on the porous molded body.

8. The gas adsorbent according to claim 7, wherein the amine compound is an amine containing at least one ether-bonding oxygen atom or siloxane-bonding oxygen atom in the molecule.

9. The gas adsorbent according to claim 7, wherein the amine compound is an amine containing at least one structure selected from the group consisting of an ethylenedioxy group, an isopropylenedioxy group, a butylenedioxy group, a linear siloxane structure, and a cyclic siloxane structure as a partial structure within the molecule.

10. The gas adsorbent according to claim 7, wherein the amine compound is an amine having a boiling point of 250° C. or higher at 760 mmHg.

Citation Information

Patent Citations

  • Method for treating exhaust gas

    JP2004261670A

  • Environment cleaning agent, environment cleaning method, and production method for environment cleaning agent

    JP2017047135A

  • Renewable Adsorbents for Modified Amines on Solid Supports

    JP2018509280A

  • Amine containing fibrous structure for adsorption of co2 from atmoshperic air

    WO2010091831A1

  • Carbon dioxide absorbent and method for producing same, and carbon dioxide separation system

    WO2018207633A1