Graphite sheet

By integrating carbon particles with a specific aspect ratio within the graphite sheet to align carbon crystals in the thickness direction, the thermal conductivity of the graphite sheet is enhanced, addressing the low thermal conductivity issue in existing graphite sheets and improving heat dissipation performance.

WO2024247565A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016051
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-04-24
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Graphite sheets with thermal conductivity in the thickness direction remain low due to the alignment of graphite layers in the plane direction during film formation, and the hard surface layer formed on thermally decomposed polyimide films increases contact thermal resistance, making it difficult to enhance thermal conductivity in this direction.

Method used

Incorporating carbon particles with an aspect ratio of 4 or less between and within the graphite layers, which are aligned to have a thickness direction component, improves thermal conductivity by allowing carbon crystals to be oriented parallel to the thickness direction, enhancing heat transfer.

Benefits of technology

The graphite sheet achieves increased thermal conductivity in the thickness direction, effectively improving heat dissipation performance when used as a thermally conductive sheet between heating and heat radiating elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016051_05122024_PF_FP_ABST
    Figure JP2024016051_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a graphite sheet that allows an increase in the thermal conductivity in the thickness direction. A graphite sheet (1) has a plurality of graphite layers (10) and a plurality of carbon particles (20) present between the graphite layers (10) and in at least some of the graphite layers. The carbon particles (20) have an aspect ratio of 4 or less. Due to this configuration, it is thought that the graphite layers (10) follow the shape of the carbon particles (20) in the vicinity of the carbon particles (20) and are arranged in a direction having the thickness direction component, thereby allowing improvement in the thermal conductivity in the thickness direction of the graphite sheet (1).
Need to check novelty before this filing date? Find Prior Art

Description

Graphite Sheet

[0001] The present disclosure relates to graphite sheets, and more particularly to graphite sheets having graphite layers.

[0002] In recent years, the number of electric vehicles and hybrid vehicles that use electric motors as a driving source for traveling has been increasing. In the inverters that control these vehicles, power modules such as insulated gate bipolar transistors (IGBTs) are heat-generating elements that generate a large amount of heat. These heat-generating elements are attached to a heat sink or other heat sink to dissipate the heat generated during operation. In this case, a sheet of thermal interface material (TIM) is sandwiched between the heat-generating element and the heat sink to smoothly transfer heat from the heat-generating element to the heat sink. A graphite sheet is used as this heat-conducting sheet.

[0003] Patent Document 1 discloses a thermally conductive sheet using a graphite sheet obtained by pyrolyzing an organic film such as polyimide.

[0004] JP 2013-222918 A

[0005] A thermally conductive sheet is required to have a high thermal conductivity in the thickness direction. However, thermally conductive sheets obtained by pyrolysis of polyimide films, such as those described in Patent Document 1, have the problem of high contact thermal resistance due to the hard layer formed on the surface. Graphite sheets obtained by reducing graphene oxide through firing have low thermal conductivity in the thickness direction because the graphite layers are aligned in the plane direction during the self-organization process during film formation. Furthermore, even if flake-shaped graphite powder is added to the graphite sheet, the alignment of the graphite layers does not change much from the plane direction, making it difficult to increase the thermal conductivity in the thickness direction.

[0006] An object of the present disclosure is to provide a graphite sheet that can increase thermal conductivity in the thickness direction.

[0007] A graphite sheet according to one embodiment of the present disclosure includes a plurality of graphite layers and a plurality of carbon particles present at least partially between and within the graphite layers, the carbon particles having an aspect ratio of 4 or less.

[0008] According to the graphite sheet of the present disclosure, it is possible to provide a graphite sheet that can increase thermal conductivity in the thickness direction.

[0009] Fig. 1 is a schematic cross-sectional view showing a graphite sheet according to an embodiment of the present disclosure. Fig. 2 is an enlarged cross-sectional view of a carbon particle 20 and its vicinity in the graphite sheet according to an embodiment of the present disclosure. Fig. 3 is an electron microscope photograph of a cross-section of the graphite sheet according to Example 1.

[0010] 1. Overview Graphite sheets according to embodiments of the present disclosure will be described below. Note that the following embodiment is merely one of various embodiments of the present disclosure. The following embodiment can be modified in various ways depending on the design as long as the object of the present disclosure can be achieved.

[0011] Graphite sheets are used as thermally conductive sheets that smoothly transfer heat generated by the heating element to the heat sink by, for example, sandwiching them between a heating element and a heat sink and fastening them with screws or the like, compressing the graphite sheet and bringing it into close contact with the heating element and the heat sink. When graphite sheets are produced by firing organic films or graphene oxide, the resulting graphite layers are mostly aligned in the plane direction, resulting in very high thermal conductivity in the plane direction. However, when used as a thermally conductive sheet, the thermal conductivity in the thickness direction, which is the direction of heat conduction, remains low.

[0012] In response to this, the inventors have conducted extensive research into improving thermal conductivity in the thickness direction by controlling the arrangement of graphite layers in a graphite sheet, and have found that the thermal conductivity in the thickness direction can be improved by having carbon particles in the graphite sheet and using carbon particles with a specific shape, thereby completing the present disclosure.

[0013] FIG. 1 is a schematic cross-sectional view showing a graphite sheet 1 according to an embodiment of the present disclosure. FIG. 2 is an enlarged cross-sectional view of a carbon particle 20 and its vicinity in the graphite sheet 1 according to the embodiment of the present disclosure. The graphite sheet 1 according to the embodiment has a plurality of graphite layers 10 and a plurality of carbon particles 20 present at least partially between and within the graphite layers 10. The aspect ratio of the carbon particles 20 is 4 or less. The direction in which the graphite layers 10 are stacked in the graphite sheet 1 is defined as the z-axis. A plane perpendicular to the z-axis is defined as the x-y plane, and the x-axis and y-axis are set to be orthogonal to each other. The x-axis, y-axis, and z-axis define an xyz Cartesian coordinate system. FIG. 1 is a cross-sectional view taken along a plane perpendicular to the y-axis, i.e., a plane parallel to the xz plane.

[0014] Graphite sheet 1 can increase the thermal conductivity in the thickness direction. The reason why graphite sheet 1 having the above configuration exhibits the above effect is not entirely clear, but can be speculated, for example, as follows. When flake-shaped carbon particles are contained between or within graphite layers 10 in graphite sheet 1, the flake-shaped carbon particles are oriented in the direction of the long sides of the flakes due to their large aspect ratio. Therefore, the carbon crystals constituting graphite layer 10 are aligned in a direction parallel to the xy plane, i.e., in the direction D1, and not aligned in the direction of the z-axis. On the other hand, in this embodiment, between or within graphite layers 10 in graphite sheet 1, carbon particles 20 with an aspect ratio of 4 or less have crystals aligned in the thickness direction of graphite sheet 1 (a direction parallel to the z-axis). Therefore, in graphite layer 10, near carbon particle 20, it is believed that the carbon crystals constituting graphite layer 10 are arranged so as to have a tilt component toward the z-axis so as to follow the shape of carbon particle 20. In other words, it is believed that the carbon crystals constituting graphite layer 10 are arranged in the direction of D2. This is believed to improve the thermal conductivity in the thickness direction of graphite sheet 1. Note that the direction parallel to the z-axis is also the thickness direction, so the vector indicating the direction of D2 includes the thickness direction as a component. Hereinafter, the direction of D2 will be referred to as the "direction having a component in the thickness direction." The "aspect ratio" will be explained later.

[0015] 2. Details <Graphite Sheet> Graphite sheet 1 has a plurality of graphite layers 10 and a plurality of carbon particles 20. The plurality of graphite layers 10 are stacked in the thickness direction of graphite sheet 1. The plurality of carbon particles 20 are present at least partially between and within the plurality of graphite layers 10.

[0016] 1 , in graphite sheet 1, a portion of graphite layer 10 preferably extends in the plane direction of graphite sheet 1, and a portion of graphite layer 10 preferably extends in a direction having a component in the thickness direction of graphite sheet 1 near a plurality of carbon particles 20. In this case, the thermal conductivity of graphite sheet 1 in the thickness direction can be further increased.

[0017] The average thickness of graphite sheet 1 is, for example, 1 μm or more and 150 μm or less, preferably 10 μm or more and 120 μm or less, and more preferably 20 μm or more and 100 μm or less. The "average thickness" refers to the arithmetic mean value of thicknesses measured at multiple points (e.g., 10 points) on graphite sheet 1.

[0018] [Graphite Layer] The "graphite layer" is a layer made of graphite (black lead) that forms a single cleavage plane. The graphite layer 10 typically includes one or more graphene layers (layers in which carbon atoms are arranged in a hexagonal honeycomb lattice pattern, typically a single layer).

[0019] The average thickness of graphite layer 10 is, for example, 0.001 μm or more and 20 μm or less, and preferably 0.01 μm or more and 10 μm or less.

[0020] Graphite layer 10 is preferably formed from graphene oxide. When graphite layer 10 is formed from graphene oxide mainly having a single-layer structure, it is believed that a higher proportion of the graphite oxide is arranged in the thickness direction, thereby enabling graphite sheet 1 to have a higher thermal conductivity in the thickness direction. Graphene oxide is graphene modified with oxygen-containing groups such as carboxyl groups, carbonyl groups, and hydroxyl groups.

[0021] [Carbon Particles] Carbon particles 20 refer to particles mainly composed of simple carbon. The aspect ratio of the carbon particles 20 is 4 or less. The "aspect ratio" refers to the ratio of the maximum diameter to the minimum diameter determined from an electron microscope photograph of the cross section of the carbon particle 20. Taking FIG. 2 as an example, it represents the ratio (L1 / L2) of the maximum diameter L1 to the minimum diameter L2. The "aspect ratio" is also the arithmetic average value for, for example, any 10 carbon particles 20. Note that, for the carbon particles 20, the direction of the maximum diameter L1 is not necessarily perpendicular to the thickness direction, and the direction of the minimum diameter L2 is not necessarily parallel to the thickness direction.

[0022] The aspect ratio of carbon particles 20 is preferably 3.5 or less, more preferably 3 or less, even more preferably 2.5 or less, and particularly preferably 2 or less. The lower limit of the aspect ratio of carbon particles 20 is, for example, 1 or more, preferably 1.3 or more, and more preferably 1.6 or more. By setting the aspect ratio of carbon particles 20 within this range, the thermal conductivity of graphite sheet 1 in the thickness direction can be further increased.

[0023] As long as the aspect ratio of carbon particles 20 is equal to or less than the specific value, the shape of carbon particles 20 may be, for example, spherical, approximately spherical, or other spherical shape; polyhedral shape, such as tetrahedron or hexahedron; flat shape, such as scale, flake, or other flaky shape; rod-like shape; or fibrous shape. Carbon particles 20 may also be granular, lumpy, or porous, such as spongy, or have an uneven surface. The shape of carbon particles 20 is preferably spherical or approximately spherical. In this case, the thermal conductivity of graphite sheet 1 in the thickness direction can be further increased. The term "spherical" refers to a cross-sectional circularity (= 4π × area / perimeter) of, for example, 0.6 or more, preferably 0.8 or more.

[0024] Examples of the carbon particles 20 include graphite particles, carbon fibers, carbon nanotubes, and graphene. "Graphite" is one of the allotropes of carbon and is also called graphite. However, graphite particles are different from the graphite layer 10. The carbon particles 20 preferably include graphite particles.

[0025] Examples of graphite particles include natural graphite particles such as graphite stone and graphite minerals, and artificial graphite particles (synthetic graphite particles) such as highly oriented pyrolytic graphite. The graphite particles preferably include artificial graphite particles. In this case, the thermal conductivity of graphite sheet 1 in the thickness direction can be further increased.

[0026] It is preferable that at least a portion of the plurality of carbon particles 20 is bonded to at least a portion of graphite layer 10. In this case, carbon particles 20 are prevented from being expelled from graphite sheet 1 even when cut, and the thermal conductivity in the thickness direction of graphite sheet 1 can be increased. Examples of such bonds include covalent bonds between carbon atoms of carbon particles 20 and carbon atoms of graphite layer 10.

[0027] The average particle size of the plurality of carbon particles 20 is preferably larger than the distance between the layers of graphite layer 10. Furthermore, the distance between the layers of graphite layer 10 is preferably 25 μm or less. In this case, a larger proportion of graphite layer 10 is arranged to avoid carbon particles 20, thereby further increasing the thermal conductivity in the thickness direction of graphite sheet 1. The "average particle size of carbon particles" refers to the volume-based median diameter (50% cumulative distribution diameter (D50)) of a plurality of (e.g., 10) carbon particles 20.

[0028] The average particle size of the plurality of carbon particles 20 is preferably 1 μm or more and 100 μm or less. By setting the average particle size of carbon particles 20 within this range, the thermal conductivity in the thickness direction of graphite sheet 1 can be further increased. The average particle size of carbon particles 20 is more preferably 2 μm or more and 60 μm or less, even more preferably 3 μm or more and 40 μm or less, and particularly preferably 10 μm or more and 30 μm or less.

[0029] The average particle size of the plurality of carbon particles 20 in the thickness direction of graphite sheet 1 (hereinafter also referred to as the average particle size in the thickness direction) is preferably 0.05 to 0.8 times the average thickness of graphite sheet 1. By setting the average particle size in the thickness direction of carbon particles 20 within this range, the thermal conductivity of graphite sheet 1 in the thickness direction can be further increased. The average particle size in the thickness direction of carbon particles 20 is more preferably 0.07 to 0.6 times, even more preferably 0.08 to 0.5 times, and particularly preferably 0.1 to 0.4 times. The "average particle size in the thickness direction of graphite sheet 1" of carbon particles 20 can be determined by measuring the maximum diameter in the thickness direction of graphite sheet 1 for a plurality of (e.g., 10) carbon particles 20 in an electron microscope photograph of a cross section in the thickness direction of graphite sheet 1, and then calculating the arithmetic mean of these measured values.

[0030] It is preferable that the plurality of carbon particles 20 have a single peak in the particle size distribution. In this case, since there is little mixing of carbon particles 20 with various particle sizes, the proportion of carbon particles 20 aligned in a direction having a component in the thickness direction of graphite layer 10 can be increased, thereby increasing the thermal conductivity of graphite sheet 1 in the thickness direction. "Having a single peak in the particle size distribution" means that no valleys between peaks are observed in the particle size distribution curve of carbon particles 20. Note that the proportion of carbon particles aligned in a direction having a component in the thickness direction of graphite layer 10 means that a high proportion of carbon particles are aligned in the thickness direction of graphite layer 10.

[0031] When a plurality of carbon particles 20 have a single peak in the particle size distribution, the coefficient of variation at the single peak is preferably 10% or more and 60% or less, and more preferably 20% or more and 50% or less, of the average particle size of carbon particles 20. By setting this coefficient of variation within the above range, the thermal conductivity in the thickness direction of graphite sheet 1 can be further increased. The "coefficient of variation" is the value obtained by dividing the standard deviation of the measured particle size distribution by the average value, and the "coefficient of variation at a single peak" means the ratio (%) of the standard deviation (nm) of the particle size distribution at the single peak to the average particle size (nm) of the carbon particles.

[0032] The proportion of carbon particles 20 in graphite sheet 1 is preferably 1% by mass or more and 70% by mass or less. In this case, it is believed that it is possible to increase the number of locations in graphite layer 10 where carbon particles are aligned in a direction having a thickness direction component, thereby increasing the thermal conductivity in the thickness direction of graphite sheet 1. The proportion of carbon particles 20 is more preferably 5% by mass or more and 60% by mass or less, even more preferably 8% by mass or more and 50% by mass or less, and particularly preferably 10% by mass or more and 40% by mass or less.

[0033] [Graphite Sheet] The compression ratio of graphite sheet 1 when compressed in the thickness direction at 600 kPa is preferably greater than the compression ratio of carbon particles 20. In this case, when graphite sheet 1 is compressed, graphite layers 10 are aligned in a direction that follows the shape of carbon particles 20 and further has a component in the thickness direction, so that graphite sheet 1 can have a higher thermal conductivity in the thickness direction when compressed. The "compressibility" of graphite sheet 1 and carbon particles 20 is the value of 1-T1 / T0, expressed as a percentage, where T0 is the initial thickness of graphite sheet 1 or the initial particle size of carbon particles 20, and T1 is the thickness or particle size after applying a pressure of 600 kPa.

[0034] Furthermore, the porosity of graphite sheet 1 when graphite sheet 1 is compressed in the thickness direction at 600 kPa is preferably 40% or less. In this case, by having the porosity when graphite sheet 1 is compressed be equal to or less than a specific value, the arrangement of graphite layers 10 in a direction having a thickness direction component can be maintained during compression, thereby further increasing the thermal conductivity of graphite sheet 1 in the thickness direction. This porosity is preferably 30% or less, and more preferably 25% or less. There is no particular limitation on the lower limit of this porosity, but it is, for example, 1% or more, and preferably 5% or more. The "porosity" can be determined from an electron microscope photograph of a cross section of graphite sheet 1.

[0035] The thermal conductivity of graphite sheet 1 in the thickness direction is preferably 1.5 W / mK or more, more preferably 2 W / mK or more, even more preferably 2.5 W / mK or more, and particularly preferably 3 W / mK or more. In this case, the thermal conductivity of graphite sheet 1 in the thickness direction can be sufficiently increased. The higher the thermal conductivity of graphite sheet 1 in the thickness direction, the more preferable it is. There is no particular upper limit to the thermal conductivity, but it is, for example, 7 W / mK or less, and preferably 6 W / mK or less.

[0036] <Graphite Sheet Manufacturing Method> Graphite sheet 1 of the present embodiment described above can be manufactured by, for example, a manufacturing method including the following first, second, and third steps.

[0037] Each step will be described below.

[0038] (First Step) In the first step, a solution or suspension (hereinafter also referred to as liquid (X)) containing graphene oxide, carbon particles 20, and a surfactant is prepared.

[0039] The carbon particles 20 have an aspect ratio of 4 or less.

[0040] The term "surfactant" refers to a substance that acts on the interface of a substance and changes its properties, and usually has a structure that contains both hydrophilic and hydrophobic parts in the molecule.

[0041] Examples of surfactants include ionic surfactants such as anionic surfactants and cationic surfactants, nonionic surfactants, etc. The surfactant preferably contains an ionic surfactant, and more preferably contains an anionic surfactant.

[0042] Examples of anionic surfactants include sulfonic acids or salts thereof, carboxylic acids or salts thereof, etc. Examples of sulfonic acid salts and carboxylic acid salts include alkali metal salts such as lithium salts, sodium salts, and potassium salts of sulfonic acids and carboxylic acids, alkaline earth metal salts such as magnesium salts, calcium salts, and barium salts, and amine salts such as triethanolamine salts.

[0043] Examples of sulfonic acids include aliphatic sulfonic acids and aromatic sulfonic acids.

[0044] Examples of aliphatic sulfonic acids include octanesulfonic acid, dodecylsulfonic acid, etc. Examples of salts of aliphatic sulfonic acids include sodium octanesulfonate, sodium dodecylsulfonate, etc.

[0045] Examples of aromatic sulfonic acids include aromatic sulfonic acids having an alkyl group such as dodecylbenzenesulfonic acid, and aromatic sulfonic acids having no alkyl group such as naphthalenetrisulfonic acid. Examples of salts of aromatic sulfonic acids include salts of aromatic sulfonic acids having an alkyl group such as sodium dodecylbenzenesulfonate, and salts of aromatic sulfonic acids having no alkyl group such as trisodium naphthalenetrisulfonate.

[0046] Examples of carboxylic acids include tetradecanoic acid (myristic acid), hexadecanoic acid (palmitic acid), octadecanoic acid (stearic acid), etc. Examples of carboxylic acid salts include sodium myristate, sodium palmitate, sodium stearate, etc.

[0047] Examples of the alkyl group include linear alkyl groups such as n-octyl, n-dodecyl, n-tetradecyl, n-hexadecyl, n-octadecyl, and n-icosyl groups, and branched alkyl groups such as isooctyl and isododecyl groups. As the alkyl group, linear alkyl groups are preferred, and n-dodecyl groups are more preferred.

[0048] The liquid (X) in the first step can be prepared, for example, by adding an aqueous solution of graphene oxide to an aqueous solution of a surfactant, and stirring the resulting mixture using, for example, a stirring defoamer.

[0049] (Second Step) In the second step, a precursor membrane is formed using the liquid (X) prepared in the first step.

[0050] The precursor film in the second step can be formed, for example, by applying the liquid (X) obtained in the first step to a substrate such as PET (polyethylene terephthalate) using a device such as a coater to a predetermined thickness, followed by drying. The coating thickness is, for example, 0.1 mm or more and 3 mm or less. The drying temperature is, for example, 30°C or more and 80°C or less.

[0051] (Third Step) In the third step, the precursor film formed in the second step is heat-treated.

[0052] The heat treatment in the third step can be performed, for example, by firing the precursor film formed in the second step. This firing is usually performed under load. The firing temperature is, for example, 2000°C or higher and 3000°C or lower, and preferably 2500°C or higher and 2800°C or lower.

[0053] In this manner, graphite sheet 1 can be obtained.

[0054] Hereinafter, the present disclosure will be described more specifically with reference to examples, but the present disclosure is not limited to only these examples.

[0055] <Production of Graphite Sheet> [Examples 1 to 9 and Comparative Examples 1 and 2] Graphite sheets were produced according to the following procedure.

[0056] Carbon particles having the aspect ratios and average particle sizes shown in Table 1 below were placed in a small bottle to a predetermined content ratio, and 12 g of an aqueous solution of sodium dodecylbenzenesulfonate (1.5% by mass) was added and stirred. Next, 45 g of a graphene oxide aqueous dispersion (solid content: 1.8% by mass) was added to the bottle and stirred with a stirrer / defoamer to prepare a raw material solution. This raw material solution was then applied to a PET substrate using a coater with a 1.5 mm gap. The resulting coating was dried at 60°C to form a precursor film (raw material sheet before firing). The resulting precursor films were then sandwiched between graphite plates one by one, loaded with a high-density graphite plate, and heat-treated by firing at 2700°C to obtain a graphite sheet.

[0057] The aspect ratio and average particle size of each carbon particle used are shown below.

[0058] Aspect ratio: 1.8, average particle size along the long axis: 20 μm Aspect ratio: 2.2, average particle size along the long axis: 9 μm Aspect ratio: 4.5, average particle size along the long axis: 20 μm An electron microscope photograph of a cross section of the graphite sheet of Example 1 is shown in Figure 3. As can be seen from this electron microscope photograph, the obtained graphite sheet has a high proportion of graphite layers that are aligned in a direction having a component in the thickness direction.

[0059] <Evaluation> The thermal conductivity (W / mK) of the graphite sheet in the thickness direction was measured by the following method.

[0060] According to a method in accordance with ASTM D5470, a graphite sheet was sandwiched between two metal blocks so that the graphite sheet was pressed in the thickness direction at a predetermined pressure, and the steady-state thermal resistance from one metal block to the other was measured. The temperature of each metal block was measured with a thermocouple. The thermal resistance value was calculated using the following formula (1):

[0061] Thermal resistance (Kcm 2 / W) = temperature difference ΔT (K) × surface area of ​​graphite sheet (cm 2 ) / amount of heat passing (W) (1) This thermal resistance was measured by changing the pressure to 50 kPa, 100 kPa, 200 kPa, 300 kPa, 500 kPa, and 600 kPa, and the average thickness of the graphite sheet (arithmetic mean value of 10 points) was also measured in each case.

[0062] The thermal conductivity of the graphite sheet in the thickness direction can be calculated by the following formula (2).

[0063] Thermal conductivity (W / mK) = average thickness (μm) / (thermal resistance (Kcm 2 / W)×100) (2) Based on the formula (2), the thermal resistance and average thickness values ​​obtained by the measurements were plotted, and the thermal conductivity value was calculated from the slope of the resulting straight line.

[0064] The aspect ratio, average particle size in the thickness direction (average particle size of carbon particles in the thickness direction of the graphite sheet) and content of the carbon particles used in producing the graphite sheet, as well as the thermal conductivity of the graphite sheet in the thickness direction are shown in Table 1. *1 in the average particle size in the thickness direction for Comparative Example 2 in Table 1 indicates that the average particle size of the carbon particles in the thickness direction could not be measured.

[0065]

[0066] As can be seen from the results in Table 1 above, the graphite sheets of the examples were able to increase the thermal conductivity in the thickness direction, whereas the graphite sheets of the comparative examples were unable to increase the thermal conductivity in the thickness direction.

[0067] (Summary) As is clear from the above-described embodiments and examples, the present disclosure includes the following aspects.

[0068] A graphite sheet (1) according to a first aspect of the present disclosure has a plurality of graphite layers (10) and a plurality of carbon particles (20) present at least partially between and within the graphite layers (10). The carbon particles (20) have an aspect ratio of 4 or less.

[0069] According to the first aspect, by setting the aspect ratio of the carbon particles (20) to a specific value or less, the carbon particles (20) can be arranged in a direction having a component in the thickness direction of the graphite layer (10), and the thermal conductivity of the graphite sheet (1) in the thickness direction can be increased.

[0070] In the graphite sheet (1) according to the second aspect of the present disclosure, the carbon particles (20) have a spherical or nearly spherical shape in the first aspect.

[0071] According to the second aspect, by forming the carbon particles (20) into a specific shape, it is possible to increase the proportion of the carbon particles (20) aligned in a direction having a component in the thickness direction of the graphite layer (10), and to increase the thermal conductivity of the graphite sheet (1) in the thickness direction.

[0072] In the graphite sheet (1) according to the third aspect of the present disclosure, in the first or second aspect, the proportion of carbon particles (20) in the graphite sheet (1) is 1% by mass or more and 70% by mass or less.

[0073] According to the third aspect, it is possible to increase the portion of the graphite layer (10) that is aligned in a direction having a component in the thickness direction, and to increase the thermal conductivity of the graphite sheet (1) in the thickness direction.

[0074] In the graphite sheet (1) according to the fourth aspect of the present disclosure, in any one of the first to third aspects, the plurality of carbon particles (20) have a single peak in the particle size distribution.

[0075] According to the fourth aspect, by using carbon particles (20) having a single-peak particle size distribution, there is little mixing of carbon particles (20) of various particle sizes, and therefore the proportion of carbon particles (20) aligned in a direction having a component in the thickness direction in the graphite layer (10) can be increased, and the thermal conductivity of the graphite sheet (1) in the thickness direction can be increased.

[0076] In the graphite sheet (1) according to a fifth aspect of the present disclosure, in any one of the first to fourth aspects, the compressibility of the graphite sheet (1) when compressed in the thickness direction at 600 kPa is greater than the compressibility of the carbon particles (20).

[0077] According to the fifth aspect, by making the compression ratio of the graphite sheet (1) larger than that of the carbon particles (20), when the graphite sheet (1) is compressed, the graphite layers (10) are aligned in a direction that follows the shape of the carbon particles (20) and further has a component in the thickness direction, and therefore, when the graphite sheet (1) is compressed, the thermal conductivity in the thickness direction can be made larger.

[0078] In a graphite sheet (1) according to a sixth aspect of the present disclosure, in any one of the first to fifth aspects, the porosity of the graphite sheet (1) when compressed in the thickness direction at 600 kPa is 40% or less.

[0079] According to the sixth aspect, by setting the porosity of the graphite sheet (1) when compressed to a specific value or less, the arrangement of the graphite layer (10) in a direction having a component in the thickness direction can be maintained when compressed, and the thermal conductivity of the graphite sheet (1) in the thickness direction can be further increased.

[0080] The graphite sheet of the present disclosure can increase thermal conductivity in the thickness direction. Therefore, when the graphite sheet of the present disclosure is attached to a heat dissipating body such as a heat sink, the heat dissipation performance of the heat dissipating body can be improved. Thus, the graphite sheet of the present disclosure is industrially useful.

[0081] 1 Graphite sheet 10 Graphite layer 20 Carbon particles

Claims

1. A graphite sheet having a plurality of graphite layers and a plurality of carbon particles present at least partially between and within the graphite layers, the carbon particles having an aspect ratio of 4 or less.

2. The graphite sheet according to claim 1, wherein the carbon particles are spherical or nearly spherical in shape.

3. The graphite sheet according to claim 1 or 2, wherein the proportion of the carbon particles in the graphite sheet is 1 mass % or more and 70 mass % or less.

4. The graphite sheet according to claim 1 or 2, wherein the plurality of carbon particles have a single peak in particle size distribution.

5. The graphite sheet according to claim 1 or 2, wherein the graphite sheet has a compression ratio greater than the compression ratio of the carbon particles when compressed in a thickness direction at 600 kPa.

6. The graphite sheet according to claim 1 or 2, wherein the graphite sheet has a porosity of 40% or less when compressed in the thickness direction at 600 kPa.

Citation Information

Patent Citations

  • Flexible carbon electrode and application thereof in lithium ion battery

    CN107994208A

  • Electrode for capacitor and manufacturing method thereof, and capacitor

    JP2020161708A

  • Highly heat-conductive member, method for producing same, and heat dissipating system using same

    WO2005019132A1