Method for manufacturing superconducting wire connection structure, and superconducting wire connection structure
The method of applying a raw material solution using rotating rollers with grooves for superconducting wire connection structures addresses the challenge of uniform thickness, achieving stable and uniformly thick bonding layers with low surface roughness, effectively bonding oxide superconductor films.
Patent Information
- Application Number
- PCT/JP2024/016794
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-01
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional methods for manufacturing superconducting wire connection structures face challenges in forming a bonding layer with uniform thickness due to variations in coating film thickness caused by low viscosity raw material solutions, particularly in die coating and inkjet methods.
A method involving the application of a raw material solution using rotating rollers with grooves to ensure uniform coating film thickness, followed by calcination and pressure heating to form a stable bonding layer with REBa2Cu3Ox crystals, achieving a uniform thickness and low arithmetic mean roughness.
This method stably forms a bonding layer with uniform thickness and small surface roughness, ensuring consistent superconducting bonding between oxide superconductor films, overcoming the thickness variations inherent in previous techniques.
Smart Images

Figure JP2024016794_05122024_PF_FP_ABST
Abstract
Description
Manufacturing method of superconducting wire joint structure and superconducting wire joint structure
[0001] The present disclosure relates to a method for manufacturing a superconducting wire connection structure and a superconducting wire connection structure. This application claims priority to Japanese Patent Application No. 2023-088984, filed on May 30, 2023. The entire contents of this Japanese patent application are incorporated herein by reference.
[0002] For example, International Publication No. 2016 / 129469 (Patent Document 1) describes a superconducting wire connection structure, which includes a first superconducting wire, a second superconducting wire, and a joining layer.
[0003] The first superconducting wire has a first metal substrate, a first intermediate layer disposed on the first metal substrate, and a first oxide superconducting film disposed on the first intermediate layer. The first superconducting wire has a first end in the longitudinal direction of the first superconducting wire. The second superconducting wire has a second metal substrate, a second intermediate layer disposed on the second metal substrate, and a second oxide superconducting film disposed on the second intermediate layer. The second superconducting wire has a second end in the longitudinal direction of the second superconducting wire.
[0004] The first and second superconducting wires are arranged such that the first oxide superconductor film at the first end and the second oxide superconductor film at the second end face each other with a bonding layer interposed therebetween. The constituent materials of the first oxide superconductor film, the constituent materials of the second oxide superconductor film, and the constituent materials of the bonding layer are REBa. 2 Cu 3 O x where RE is a rare earth element. The first oxide superconductor film at the first end and the second oxide superconductor film at the second end are superconductively joined by a joining layer.
[0005] International Publication No. 2016 / 129469
[0006] A manufacturing method for a superconducting wire connection structure according to the present disclosure includes the steps of preparing a first superconducting wire and a second superconducting wire. The first superconducting wire has a first substrate, a first intermediate layer disposed on the first substrate, and a first superconducting layer disposed on the first intermediate layer. The first superconducting wire has a first end in the longitudinal direction of the first superconducting wire. The second superconducting wire has a second substrate, a second intermediate layer disposed on the second substrate, and a second superconducting layer disposed on the second intermediate layer. The second superconducting wire has a second end in the longitudinal direction of the second superconducting wire. The constituent materials of the first superconducting layer and the second superconducting layer are oxide superconductors. The method for manufacturing a superconducting wire connection structure further includes the steps of: applying a raw material solution containing constituent elements of the first superconducting layer to form a coating film on the first superconducting layer at a first end; firing the coating film to form a calcined layer containing crystals of a precursor of an oxide superconductor; arranging the first superconducting wire and the second superconducting wire so that the first superconducting layer at the first end and the second superconducting layer at the second end face each other with the calcined layer interposed therebetween; and heating the calcined layer while applying pressure to form a joining layer that superconductively joins the first superconducting layer at the first end and the second superconducting layer at the second end. The application of the raw material solution is performed by rotating a first roller to directly or indirectly transfer the raw material solution supplied to the outer peripheral surface of the first roller onto the first superconducting layer at the first end.
[0007] FIG. 1 is a plan view of a superconducting wire connection structure 100. FIG. 2 is a cross-sectional view taken along line II-II in FIG. 1. FIG. 3A is a cross-sectional view of a superconducting wire connection structure 100 according to a first modified example. FIG. 3B is a cross-sectional view of a superconducting wire connection structure 100 according to a second modified example. FIG. 4 is a manufacturing process diagram of the superconducting wire connection structure 100. FIG. 5 is a cross-sectional view illustrating the coating film forming step S2. FIG. 6 is a cross-sectional view illustrating the calcined layer forming step S3.
[0008] [Problem to be Solved by the Present Disclosure] The superconducting wire connection structure described in Patent Document 1 is manufactured by the following method. First, a first superconducting wire and a second superconducting wire are prepared. Second, a raw material solution is applied to form a coating film on the first oxide superconductor film at the first end. The raw material solution contains constituent materials of the first oxide superconductor film.
[0009] Third, by baking the coating, REBa 2 Cu 3 O x Fourth, the first superconducting wire and the second superconducting wire are arranged so that the first oxide superconductor film at the first end and the second oxide superconductor film at the second end face each other with the calcined film interposed therebetween. Fifth, the calcined film is heated while being pressurized, thereby forming a calcined film containing crystals of the precursor of REBa. 2 Cu 3 O x crystals grow epitaxially from the first oxide superconductor film at the first end and the second oxide superconductor film at the second end, whereby the calcined film becomes a bonding layer, forming a superconducting bond between the first oxide superconductor film at the first end and the second oxide superconductor film at the second end.
[0010] In the manufacturing method of the superconducting wire connection structure described in Patent Document 1, the raw material solution is applied by a die coating method or an inkjet method. With the die coating method, it is necessary to apply the solution over a long distance until the coating film reaches a predetermined thickness. With the inkjet method, the viscosity of the raw material solution is low, so the thickness of the coating film is likely to vary greatly. In other words, with conventional application methods, it is time-consuming to form a coating film of uniform thickness, which can result in large variations in the thickness of the bonding layer.
[0011] The present disclosure has been made in view of the above-described problems of the conventional art. More specifically, the present disclosure provides a method for manufacturing a superconducting wire connection structure that can stably form a bonding layer with a uniform thickness.
[0012] Effect of the Present Disclosure According to the method for manufacturing a superconducting wire connection structure of the present disclosure, it is possible to stably form a bonding layer with a uniform thickness.
[0013] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described.
[0014] (1) A manufacturing method of a superconducting wire connection structure according to an embodiment includes a step of preparing a first superconducting wire and a second superconducting wire. The first superconducting wire has a first substrate, a first intermediate layer disposed on the first substrate, and a first superconducting layer disposed on the first intermediate layer. The first superconducting wire has a first end in the longitudinal direction of the first superconducting wire. The second superconducting wire has a second substrate, a second intermediate layer disposed on the second substrate, and a second superconducting layer disposed on the second intermediate layer. The second superconducting wire has a second end in the longitudinal direction of the second superconducting wire. The constituent materials of the first superconducting layer and the second superconducting layer are oxide superconductors. The method for manufacturing a superconducting wire connection structure further includes the steps of applying a raw material solution containing constituent elements of the first superconducting layer to form a coating film on the first superconducting layer at the first end, firing the coating film to form a calcined layer containing crystals of a precursor of an oxide superconductor, arranging the first superconducting wire and the second superconducting wire so that the first superconducting layer at the first end and the second superconducting layer at the second end face each other with the calcined layer interposed therebetween, and heating the calcined layer while applying pressure to form a joining layer that superconductively joins the first superconducting layer at the first end and the second superconducting layer at the second end. The application of the raw material solution is performed by rotating the first roller to directly or indirectly transfer the raw material solution supplied to the outer peripheral surface of the first roller onto the first superconducting layer at the first end. The method for manufacturing a superconducting wire connection structure described above in (1) enables the stable formation of a joining layer of uniform thickness.
[0015] (2) In the manufacturing method of the superconducting wire connection structure described in (1) above, the application of the raw material solution may be performed by rotating the first roller to transfer the raw material solution supplied to the outer surface to the outer surface of the second roller, and by rotating the second roller to transfer the raw material solution transferred to the outer surface of the second roller onto the first superconducting layer at the first end.
[0016] (3) In the method for manufacturing a superconducting wire connection structure according to (1) or (2) above, the viscosity of the raw material solution may be 100 mPa·s or less.
[0017] (4) In the manufacturing method of the superconducting wire connection structure described above in (1) to (3), the width of the coating film in the longitudinal direction of the first superconducting wire may be 1.5 times or less the overlapping distance between the first superconducting layer at the first end and the second superconducting layer at the second end.
[0018] (5) In the above-mentioned methods for manufacturing a superconducting wire according to (1) to (4), the constituent material of the first superconducting layer and the constituent material of the second superconducting layer are REBa. 2 Cu 3 O x may be.
[0019] (6) A superconducting wire connection structure according to an embodiment includes a first superconducting wire, a second superconducting wire, and a joining layer. The first superconducting wire has a first substrate, a first intermediate layer disposed on the first substrate, and a first superconducting layer disposed on the first intermediate layer. The first superconducting wire has a first end in the longitudinal direction of the first superconducting wire. The second superconducting wire has a second substrate, a second intermediate layer disposed on the second substrate, and a second superconducting layer disposed on the second intermediate layer. The second superconducting wire has a second end in the longitudinal direction of the second superconducting wire. The first superconducting wire and the second superconducting wire are arranged such that the first superconducting layer at the first end and the second superconducting layer at the second end face each other with the joining layer interposed therebetween. The constituent material of the first superconducting layer, the constituent material of the second superconducting layer, and the constituent material of the bonding layer are REBa. 2 Cu 3 O x where RE is a rare earth element. The bonding layer superconductively bonds the first superconducting layer at the first end and the second superconducting layer at the second end. The arithmetic mean roughness on the surface of the bonding layer is 100 nm or less. According to the superconducting wire connection structure of (6) above, it is possible to stably form a bonding layer with a small arithmetic mean roughness on the surface, i.e., a bonding layer with a uniform thickness.
[0020] (7) In the superconducting wire connection structure of (6) above, the width of the joining layer in the longitudinal direction of the first superconducting wire may be 1.5 times or less the distance over which the first superconducting layer at the first end and the second superconducting layer at the second end overlap.
[0021] [Details of the embodiment of the present disclosure] Next, details of the embodiment of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are designated by the same reference numerals, and redundant description will not be repeated. A superconducting wire connection structure according to the embodiment is referred to as a superconducting wire connection structure 100.
[0022] (Configuration of Superconducting Wire Connection Structure 100) The configuration of the superconducting wire connection structure 100 will be described below with reference to Figs.
[0023] As shown in FIGS. 1 and 2 , the superconducting wire connection structure 100 includes a first superconducting wire 10 , a second superconducting wire 20 , and a joining layer 30 .
[0024] First superconducting wire 10 has first substrate 11, first intermediate layer 12, and first superconducting layer 13. First superconducting wire 10 has first end 10a. First end 10a is an end of first superconducting wire 10 in the longitudinal direction.
[0025] The first substrate 11 is a clad material having, for example, a stainless steel tape member, a copper (Cu) layer disposed on the tape member, and a nickel (Ni) layer disposed on the copper layer. The crystals of the copper layer are oriented. The crystals of the nickel layer are also oriented along the crystals of the copper layer.
[0026] The first substrate 11 is not limited to this. The first substrate 11 may be, for example, Hastelloy (registered trademark). The first substrate 11 may be a tape member made of a biaxially oriented metal material or a tape member made of a non-oriented metal material. Note that even if the material making up the first substrate 11 is made of a non-oriented metal material, it is sufficient that the crystals of the first intermediate layer 12 are oriented.
[0027] The first intermediate layer 12 is disposed on the first substrate 11. More specifically, the first intermediate layer 12 is disposed on the nickel layer of the first substrate 11. The first intermediate layer 12 is formed of, for example, yttria-stabilized zirconia (YSZ), magnesium oxide (MgO), cerium oxide (CeO 2 ), yttrium oxide (Y 2 O 3), lanthanum manganese oxide (LaMnO 3 ), gadolinium zirconate (Gd 2 Zr 2 O 7 ) and strontium titanate (SrTiO 3 The first intermediate layer 12 is formed by, for example, magnetron sputtering or ion beam assisted deposition (IBAD).
[0028] The layer structure of the first intermediate layer 12 is not limited to this. As described above, since the crystals of the nickel layer of the first base material 11 are oriented, the crystals of each layer of the first intermediate layer 12 are also oriented. The first intermediate layer 12 may have a two-layer structure or a single-layer structure.
[0029] The first superconducting layer 13 is disposed on the first intermediate layer 12. Since the crystals of the first intermediate layer 12 are oriented as described above, the c-axis of the crystals of the first superconducting layer 13 is oriented along the crystals of the first intermediate layer 12. The first superconducting layer 13 is, for example, a material (for example, REBa described later) that is a material having a c-axis oriented along the crystals of the first intermediate layer 12. 2 Cu 3 O x ) is oriented so that the c-axis of the crystal is along the normal direction to the surface of the first superconducting layer 13.
[0030] Second superconducting wire 20 has second substrate 21, second intermediate layer 22, and second superconducting layer 23. Second superconducting wire 20 has second end 20a. Second end 20a is an end of second superconducting wire 20 in the longitudinal direction.
[0031] The second substrate 21 is, for example, a clad material having a stainless steel tape member, a copper layer disposed on the tape member, and a nickel layer disposed on the copper layer. The crystals of the copper layer are oriented. The crystals of the nickel layer are also oriented along the crystals of the copper layer. The second substrate 21 is not limited to this. The second substrate 21 may be, for example, Hastelloy. The second substrate 21 may be a tape member made of a biaxially oriented metal material or a tape member made of a non-oriented metal material. Note that, as with the first superconducting wire 10, even if the material constituting the second substrate 21 is made of a non-oriented metal material, it is sufficient that the crystals of the second intermediate layer 22 are oriented.
[0032] The second intermediate layer 22 is disposed on the second substrate 21. The details of the second intermediate layer 22 are similar to those of the first intermediate layer 12.
[0033] The second superconducting layer 23 is disposed on the second intermediate layer 22. Since the crystals of the second intermediate layer 22 are oriented as described above, the c-axis of the crystals of the second superconducting layer 23 is also oriented along the crystals of the second intermediate layer 22. The second superconducting layer 23 is, for example, made of a material (for example, REBa described later) 2 Cu 3 O x ) is oriented so that the c-axis of the crystal is along the normal direction to the surface of the second superconducting layer 23.
[0034] The first superconducting wire 10 and the second superconducting wire 20 are arranged so that the longitudinal direction of the first superconducting wire 10 is aligned with the longitudinal direction of the second superconducting wire 20, and so that the first superconducting layer 13 at the first end 10a and the second superconducting layer 23 at the second end 20a face each other with a joining layer 30 interposed therebetween. The first superconducting layer 13 at the first end 10a and the second superconducting layer 23 at the second end 20a are superconductively joined by the joining layer 30.
[0035] The width of the joining layer 30 in the longitudinal direction of the first superconducting wire 10 is defined as width W1. The distance over which the first end 10a and the second end 20a overlap in the longitudinal direction of the first superconducting wire 10 is defined as distance DIS. Width W1 may be 1.5 times or less of distance DIS. Width W1 may be 1.2 times or less of distance DIS. In other words, the value obtained by subtracting distance DIS from width W1 may be smaller than distance DIS. When width W1 is 1 time or more of distance DIS, the first superconducting layer 13 and the second superconducting layer 23 are firmly joined by the joining layer 30.
[0036] The thickness of the bonding layer 30 between the first superconducting layer 13 at the first end 10a and the second superconducting layer 23 at the second end 20a is defined as thickness T. The average value of thickness T is, for example, 15 nm or more and 1.8 μm or less. The average value of thickness T may be, for example, 15 nm or more and 1 μm or less, or 15 nm or more and 500 nm or less.
[0037] The arithmetic mean roughness (Ra) of the surface of the bonding layer 30 is, for example, 100 nm or less. The arithmetic mean roughness of the surface of the bonding layer 30 is measured in accordance with JIS B 0601. More specifically, first, a measurement direction is set. The measurement direction may be the longitudinal direction of the first superconducting wire 10 or the width direction of the first superconducting wire 10 (a direction perpendicular to the longitudinal direction of the first superconducting wire 10). Second, a roughness curve of the surface of the bonding layer 30 along the measurement direction is obtained using a stylus surface roughness measuring instrument. The length over which the roughness curve is measured (evaluation length) is set to 1.25 mm. Third, Ra is calculated at any 0.25 mm (reference length) within the evaluation length based on the following formula. This Ra is regarded as the arithmetic mean roughness of the surface of the bonding layer 30. In the following equation, f(x) is the roughness curve, l is the reference length, and the x-axis direction is the measurement direction.
[0038]
[0039] If the thickness of the bonding layer 30 varies greatly, the variation is reflected in the arithmetic mean roughness of the surface of the bonding layer 30. Therefore, by evaluating the arithmetic mean roughness of the surface of the bonding layer 30, it is possible to evaluate the variation in the thickness of the bonding layer 30.
[0040] The constituent material of the first superconducting layer 13, the constituent material of the second superconducting layer 23, and the constituent material of the joining layer 30 are oxide superconductors. 2 Cu 3 O x Here, RE is a rare earth element. Examples of rare earth elements include gadolinium (Gd), yttrium (Y), and europium (Eu). However, the rare earth elements are not limited to these. REBa 2 Cu 3 O x Specific examples of oxide superconductors other than those mentioned above include bismuth-based oxide superconductors.
[0041] 3A , the first superconducting wire 10 may further include a first protective layer 14 and a first stabilizing layer 15. The first protective layer 14 is disposed on the first superconducting layer 13. The first stabilizing layer 15 is disposed on the first protective layer 14. However, the first protective layer 14 and the first stabilizing layer 15 are removed from the first end 10 a. The first protective layer 14 is made of, for example, silver (Ag) or a silver alloy. The first stabilizing layer 15 is made of, for example, copper or a copper alloy.
[0042] The second superconducting wire 20 may further include a second protective layer 24 and a second stabilizing layer 25. The second protective layer 24 is disposed on the second superconducting layer 23. The second stabilizing layer 25 is disposed on the second protective layer 24. However, the second protective layer 24 and the second stabilizing layer 25 are removed at the second end 20a. The second protective layer 24 is made of, for example, silver or a silver alloy. The second stabilizing layer 25 is made of, for example, copper or a copper alloy.
[0043] 3B, width W1 may be 1 time distance DIS. In other words, bonding layer 30 may not have a portion that protrudes in the longitudinal direction of first superconducting wire 10 from the portion where first end 10a and second end 20a overlap, and width W1 may be equal to distance DIS.
[0044] (Method for Manufacturing Superconducting Wire Connection Structure 100) Hereinafter, a method for manufacturing the superconducting wire connection structure 100 will be described with reference to Figs.
[0045] 4, the method for manufacturing the superconducting wire connection structure 100 includes a preparation step S1, a coating film formation step S2, a calcination layer formation step S3, and a joining step S4. The coating film formation step S2 is performed after the preparation step S1. The calcination layer formation step S3 is performed after the coating film formation step S2. The joining step S4 is performed after the calcination layer formation step S3.
[0046] As shown in FIG. 5 , in the coating film forming step S2, a coating film 31 is formed on the first superconducting layer 13 at the first end 10a by applying a raw material solution. The raw material solution contains a solvent and constituent elements of the first superconducting layer 13. The viscosity of the raw material solution is, for example, 100 mPa·s or less. The viscosity of the raw material solution is measured using a commercially available rotational viscometer. When the viscosity of the raw material solution is 100 mPa·s or less, the raw material solution spreads easily but also flows easily, which makes the thickness of the coating film 31 prone to become uneven. Therefore, the raw material solution is applied using a first roller 40 and a second roller 41. The first roller 40 is cylindrical and has an outer peripheral surface 40a. In this example, a groove 40b is formed in the outer peripheral surface 40a of the first roller 40. The axial portion of the first roller 40 excluding both axial ends of the first roller 40 is referred to as the middle portion of the first roller 40. Groove 40b is formed in the outer peripheral surface 40a in the middle portion of first roller 40. Groove 40b is formed over the entire circumference of outer peripheral surface 40a in the middle portion of first roller 40. That is, in this example, the bottom surface of groove 40b forms outer peripheral surface 40a in the middle portion of first roller 40. Second roller 41 is cylindrical and has outer peripheral surface 41a.
[0047] The first roller 40 is disposed so that the outer peripheral surface 40a contacts the outer peripheral surface 41a. The second roller 41 is disposed so that the outer peripheral surface 41a contacts the surface of the first superconducting layer 13 at the first end 10a. In applying the raw material solution, first, the raw material solution is supplied to the first roller 40. More specifically, the raw material solution is supplied into the groove 40b.
[0048] Second, as the first roller 40 and the second roller 41 are rotated, the raw solution in the grooves 40b is transferred to the outer peripheral surface 41a. Third, as the second roller 41 is rotated, the raw solution transferred to the outer peripheral surface 41a is applied to the first superconducting layer 13 at the first end 10a to form the coating film 31. Fourth, the coating film 31 is dried to volatilize the solvent. The width of the coating film 31 in the longitudinal direction of the first superconducting wire 10 is defined as width W2. Width W2 is 1.5 times or less the distance DIS. Width W2 may be 1.2 times or less the distance DIS. Width W2 is ideally equal to distance DIS. The difference between width W2 and distance DIS is within the tolerance range when applying the raw solution.
[0049] In the above example, the raw material solution in the groove 40b is applied onto the first superconducting layer 13 at the first end 10a via the second roller 41, but the raw material solution in the groove 40b may be transferred directly onto the first superconducting layer 13 at the first end 10a without using the second roller 41.
[0050] By forming the coating film 31 in the above manner, it is possible to form the coating film 31 with a uniform thickness even when the viscosity of the raw material solution is 100 mPa·s or less. As a result, the thickness of the finally obtained bonding layer 30 also tends to be uniform, and the arithmetic mean roughness of the surface of the bonding layer 30 becomes small as described above.
[0051] As shown in Fig. 6, in the calcined layer forming step S3, the coating film 31 is heat-treated to form the calcined layer 32. 2 Cu 3 O x This precursor contains crystals of REBa. 2 Cu 3 O x The material may be subjected to a heat treatment for forming polycrystals or a heat treatment for promoting decomposition of the raw material.
[0052] In the joining step S4, heating is performed while applying pressure, thereby turning the calcined layer 32 into the joining layer 30. More specifically, in the joining step S4, first, the first superconducting wire 10 and the second superconducting wire 20 are arranged so that the first superconducting layer 13 at the first end 10a and the second superconducting layer 23 at the second end 20a face each other with the calcined layer 32 interposed therebetween.
[0053] Second, the first end 10a and the second end 20a are clamped with a jig or the like to apply pressure to the calcined layer 32, and heating is performed in this state. This heating is performed in an oxygen-containing atmosphere at a temperature higher than that in the calcined layer forming step S3. 2 Cu 3 O x The crystals grow epitaxially from the first superconducting layer 13 at the first end 10 a and the second superconducting layer 23 at the second end 20 a to form the bonding layer 30 .
[0054] Methods for applying the raw material solution include a die coating method and an inkjet method. With the die coating method, it is necessary to apply the raw material solution over a long distance until the thickness of the coating film 31 stabilizes. With the inkjet method, it is difficult to stabilize the thickness of the coating film 31 because the viscosity of the raw material solution is low. That is, with these application methods, it is difficult to stabilize the thickness of the coating film 31, and as a result, the thickness (thickness T) of the bonding layer 30 becomes unstable.
[0055] On the other hand, in the manufacturing method of the superconducting wire connection structure 100, the first roller 40 is rotated to directly or indirectly transfer the raw material solution in the groove 40b onto the first superconducting layer 13 at the first end 10a. With this method, the thickness of the coating film 31 can be stabilized even if the width (width W2) over which the raw material solution is applied is small and the viscosity of the raw material solution is low. Therefore, with the manufacturing method of the superconducting wire connection structure 100, it is possible to obtain a joining layer 30 with a stable thickness T.
[0056] In the above, an example has been described in which the grooves 40b are formed on the outer peripheral surface 40a of the first roller 40, but the grooves 40b do not have to be formed on the outer peripheral surface 40a of the first roller 40. In this case, by arranging weir members (not shown) at both ends of the first roller 40 in the axial direction, it is possible to maintain the state in which the raw material solution is supplied onto the outer peripheral surface 40a of the first roller 40.
[0057] The embodiments disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims, not by the above-described embodiments, and is intended to include all modifications within the meaning and scope of the claims.
[0058] 10 First superconducting wire, 10a First end, 11 First substrate, 12 First intermediate layer, 13 First superconducting layer, 14 First protective layer, 15 First stabilization layer, 20 Second superconducting wire, 20a Second end, 21 Second substrate, 22 Second intermediate layer, 23 Second superconducting layer, 24 Second protective layer, 25 Second stabilization layer, 30 Joining layer, 31 Coating film, 32 Calcined layer, 40 First roller, 40a Outer circumferential surface, 40b Groove, 41 Second roller, 41a Outer circumferential surface, 100 Superconducting wire connection structure, DIS Distance, S1 Preparation process, S2 Coating film forming process, S3 Calcined layer forming process, S4 Joining process, T Thickness, W1, W2 Width.
Claims
1. A method for producing a superconducting wire, comprising the steps of: preparing a first superconducting wire and a second superconducting wire; the first superconducting wire has a first base material, a first intermediate layer disposed on the first base material, and a first superconducting layer disposed on the first intermediate layer; the first superconducting wire has a first end in a longitudinal direction of the first superconducting wire; the second superconducting wire has a second base material, a second intermediate layer disposed on the second base material, and a second superconducting layer disposed on the second intermediate layer; the second superconducting wire has a second end in a longitudinal direction of the second superconducting wire; a constituent material of the first superconducting layer and a constituent material of the second superconducting layer are oxide superconductors; applying a raw material solution containing constituent elements of the first superconducting layer to form a coating film on the first superconducting layer located at the first end; and firing the coating film to form a calcined layer containing crystals of a precursor of an oxide superconductor. a step of arranging the first superconducting wire and the second superconducting wire so that the first superconducting layer at the first end and the second superconducting layer at the second end face each other with the calcined layer interposed therebetween; and a step of forming a joining layer that superconductively joins the first superconducting layer at the first end and the second superconducting layer at the second end by heating the calcined layer while applying pressure thereto, wherein the application of the raw material solution is performed by rotating a first roller to directly or indirectly transfer the raw material solution supplied to the outer peripheral surface of the first roller onto the first superconducting layer at the first end.
2. A method for manufacturing a superconducting wire connection structure as described in claim 1, wherein the application of the raw material solution is performed by rotating the first roller to transfer the raw material solution supplied to the outer peripheral surface to the outer peripheral surface of the second roller, and by rotating the second roller to transfer the raw material solution transferred to the outer peripheral surface of the second roller onto the first superconducting layer at the first end.
3. A method for manufacturing a superconducting wire connection structure according to claim 1 or 2, wherein the viscosity of the raw material solution is 100 mPa·s or less.
4. A method for manufacturing a superconducting wire connection structure described in any one of claims 1 to 3, wherein the width of the coating in the longitudinal direction of the first superconducting wire is 1.5 times or less the overlapping distance between the first superconducting layer at the first end and the second superconducting layer at the second end.
5. The constituent material of the first superconducting layer and the constituent material of the second superconducting layer are REBa 2 Cu 3 O x The method for producing a superconducting wire connection structure according to claim 1 , wherein RE is a rare earth element.
6. A superconducting wire comprising: a first superconducting wire; a second superconducting wire; and a bonding layer; the first superconducting wire has a first base material, a first intermediate layer disposed on the first base material, and a first superconducting layer disposed on the first intermediate layer; the first superconducting wire has a first end in a longitudinal direction of the first superconducting wire; the second superconducting wire has a second base material, a second intermediate layer disposed on the second base material, and a second superconducting layer disposed on the second intermediate layer; the second superconducting wire has a second end in a longitudinal direction of the second superconducting wire; the first superconducting wire and the second superconducting wire are arranged such that the first superconducting layer at the first end and the second superconducting layer at the second end face each other with the bonding layer interposed therebetween; The first superconducting layer, the second superconducting layer, and the bonding layer are made of REBa. 2 Cu 3 O x RE is a rare earth element, the joining layer superconductively joins the first superconducting layer at the first end and the second superconducting layer at the second end, and an arithmetic mean roughness of a surface of the joining layer is 100 nm or less.
7. A superconducting wire connection structure as described in claim 6, wherein the width of the joining layer in the longitudinal direction of the first superconducting wire is 1.5 times or less the overlapping distance between the first superconducting layer at the first end and the second superconducting layer at the second end.
Citation Information
Patent Citations
Formation of superconductive thin film
JP1988279524A
Production of superconductor
JP1988285157A
Superconducting composite with high sheath resistivity
JP2002528848A
Connection structure of superconducting wire rod and method for connecting superconducting wire rod
JP2017117523A
Connection structure
JP2018170173A