Composition, transfer film, semiconductor package, and method for producing semiconductor package

The composition of polysilsesquioxane and a metal-interacting compound with a polymerization initiator addresses the need for films with low linear expansion and strong metal adhesion, improving semiconductor package performance.

WO2024247627A1PCT designated stage expired Publication Date: 2024-12-05FUJIFILM CORP

Patent Information

Application Number
PCT/JP2024/017074
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-08
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current materials for forming insulating films in semiconductor packages and display devices lack a small coefficient of linear expansion and excellent adhesion to metals, which are essential for advanced electronic devices with diverse and high-performance applications.

Method used

A composition comprising polysilsesquioxane with a functional group that interacts with metals, combined with a compound X having a metal-interacting functional group, and a polymerization initiator, which forms a film with a small coefficient of linear expansion and excellent adhesion to metals.

Benefits of technology

The composition effectively forms films with a low linear expansion coefficient and superior metal adhesion, addressing the limitations of existing resin systems and enhancing the performance of semiconductor packages and display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017074_05122024_PF_FP_ABST
    Figure JP2024017074_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a composition capable of forming a film having a small linear expansion coefficient and excellent adhesion to a metal; a transfer film related to the composition; a semiconductor package; and a method for producing the semiconductor package. A composition according to the present invention contains a polysilsesquioxane and satisfies at least one of requirement 1 and requirement 2. Requirement 1: The polysilsesquioxane has a functional group that interacts with a metal. Requirement 2: The composition further includes a compound X having a functional group that interacts with a metal, the compound being different from the polysilsesquioxane.
Need to check novelty before this filing date? Find Prior Art

Description

Composition, transfer film, semiconductor package, and method for manufacturing semiconductor package

[0001] The present invention relates to a composition, a transfer film, a semiconductor package, and a method for manufacturing a semiconductor package.

[0002] In semiconductor packages and build-up boards of multilayer printed circuit boards, insulating films are provided between wiring and between layers for the purposes of forming and protecting circuit wiring, etc. Also, in display devices (e.g., organic electroluminescence (EL) display devices and liquid crystal display devices) equipped with touch panels such as capacitance-type input devices, insulating films are provided for the purposes of forming and protecting conductive patterns such as electrode patterns corresponding to sensors in the recognition section, and wiring in peripheral wiring and lead-out wiring.

[0003] As a composition capable of forming the above insulating film, for example, Patent Document 1 discloses a composition containing a photopolymerizable compound having an ethylenically unsaturated bond, a photopolymerization initiator, and an epoxy resin.

[0004] Japanese Patent Application Laid-Open No. 2019-066510

[0005] Recently, with the diversification and high performance of devices, there is a demand for the development of new material systems capable of forming films that exhibit desired effects. Properties required for films used in semiconductor packages and the like include, for example, a small coefficient of linear expansion and excellent adhesion to metals contained in wiring and the like.

[0006] Under these circumstances, an object of the present invention is to provide a novel composition that can form a film having a small linear expansion coefficient and excellent adhesion to metals. Another object of the present invention is to provide a transfer film, a semiconductor package, and a method for manufacturing the semiconductor package, which are related to the composition.

[0007] As a result of extensive research into solving the above problems, the present inventors have found that the problems can be solved by the following configuration.

[0008] [1] A composition containing a polysilsesquioxane, satisfying at least one of Requirement 1 and Requirement 2. Requirement 1: The polysilsesquioxane has a functional group that interacts with a metal. Requirement 2: The composition further contains a compound X that is a compound different from the polysilsesquioxane and has a functional group that interacts with a metal. [2] The composition according to [1], further containing a polymerization initiator, wherein the polysilsesquioxane contains a polysilsesquioxane having a polymerizable group. [3] The composition according to [1] or [2], wherein the polysilsesquioxane contains a cage polysilsesquioxane. [4] The composition according to any one of [1] to [3], wherein the polysilsesquioxane has a chain hydrocarbon group. [5] The composition according to any one of [1] to [4], wherein the polysilsesquioxane has a weight-average molecular weight of 5,000 to 50,000. [6] The composition according to any one of [1] to [5], wherein the content of the polysilsesquioxane is 50 to 99% by mass, based on the total solid content of the composition. [7] The composition according to [2], wherein the polymerization initiator is a radical polymerization initiator. [8] The composition according to [2] or [8], wherein the content of the polymerization initiator is 0.01 to 10% by mass, based on the total solid content of the composition. [9] The composition according to any one of [1] to [8], wherein the compound X is at least one selected from the group consisting of a compound represented by formula (1) described below, a hydrolyzate of a compound represented by formula (1), and a hydrolysis condensate of a compound represented by formula (1).

[10] The composition according to any one of [1] to [9], wherein the content of the compound X is 0.01 to 10% by mass, based on the total solid content of the composition.

[11] A transfer film having a temporary support and a composition layer formed using the composition according to any one of [1] to

[10] .

[12] A semiconductor package having an insulating layer formed using the composition according to any one of [1] to

[10] .

[13] A method for manufacturing a semiconductor package, comprising: Step 1: forming a composition layer on a substrate using the composition according to any one of [1] to

[10] ; Step 2: forming a pattern including vias in the composition layer; and Step 3: subjecting the pattern to a curing treatment.

[0009] The present invention provides a composition capable of forming a film having a small linear expansion coefficient and excellent adhesion to metal. The present invention also provides a transfer film, a semiconductor package, and a method for manufacturing a semiconductor package, which are related to the composition.

[0010] FIG. 2 is a schematic diagram illustrating an example of a layer structure of a transfer film.

[0011] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.

[0012] In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits. Furthermore, in this specification, when two or more types of a certain component are present, the "content" of that component means the total content of those two or more components. In this specification, in a numerical range described in stages, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in a numerical range described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the Examples. In this specification, a combination of two or more preferred embodiments is a more preferred embodiment.

[0013] The term "step" in this specification includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved.

[0014] In this specification, unless otherwise specified, the temperature condition may be 25° C. For example, the temperature when performing each of the above steps may be 25° C. unless otherwise specified.

[0015] In this specification, "transparent" means that the average transmittance of visible light in the wavelength range of 400 to 700 nm is 80% or more, and preferably 90% or more. The average transmittance of visible light is a value measured using a spectrophotometer, and can be measured using, for example, a spectrophotometer U-3310 manufactured by Hitachi, Ltd.

[0016] In this specification, "actinic rays" or "radiation" refers to, for example, the bright line spectrum of a mercury lamp, such as g-rays, h-rays, and i-rays, far ultraviolet rays typified by excimer lasers, extreme ultraviolet rays (EUV light), X-rays, and electron beams (EB). Furthermore, in the present invention, light refers to actinic rays or radiation. In this specification, "exposure" refers to not only exposure using far ultraviolet rays typified by mercury lamps and excimer lasers, extreme ultraviolet rays, and X-rays, but also exposure using particle beams such as electron beams and ion beams, unless otherwise specified.

[0017] In this specification, the "solid content" of a composition refers to the components that form a film formed using the composition. Typically, when the composition contains a solvent (e.g., an organic solvent and water), it refers to all components excluding the solvent. In addition, liquid components that form a film are also considered to be solid content.

[0018] In this specification, unless otherwise specified, the content ratio of each repeating unit of the polymer is a molar ratio. In this specification, unless otherwise specified, the molecular weight when there is a molecular weight distribution is the weight average molecular weight (Mw). In this specification, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are values ​​obtained by gel permeation chromatography (GPC) in terms of polystyrene.

[0019] In this specification, "(meth)acrylic acid" is a concept that encompasses both acrylic acid and methacrylic acid, "(meth)acryloyl group" is a concept that encompasses both acryloyl group and methacryloyl group, "(meth)acrylate" is a concept that encompasses both acrylate and methacrylate, and "(meth)acrylamide group" is a concept that encompasses both acrylamide group and methacrylamide group.

[0020] In this specification, the bonding direction of a divalent group (e.g., —CO—O—) is not limited unless otherwise specified. For example, when Y is —CO—O— in a compound represented by the formula “X-Y-Z,” the compound may be “X-O-CO-Z” or “X-CO-O-Z.”

[0021] In this specification, unless otherwise specified, the thickness (film thickness) of a layer is the average thickness measured using a scanning electron microscope (SEM) for thicknesses of 0.5 μm or more, and the average thickness measured using a transmission electron microscope (TEM) for thicknesses of less than 0.5 μm. The average thickness is obtained by cutting a sample to be measured using an ultramicrotome, measuring the thickness at any five points, and calculating the arithmetic average of the thicknesses.

[0022] [Composition] The composition of the present invention will be described in detail below. The composition of the present invention (hereinafter also simply referred to as "composition") contains a polysilsesquioxane and satisfies at least one of Requirement 1 and Requirement 2. Requirement 1: The polysilsesquioxane has a functional group that interacts with a metal. Requirement 2: The composition further contains a compound X that is a compound different from the polysilsesquioxane and has a functional group that interacts with a metal.

[0023] Although the reason why the composition having the above configuration can solve the problems of the present invention is not entirely clear, the inventors speculate as follows. The following speculation does not limit the mechanism by which the effect is obtained. In other words, even if the effect is obtained by a mechanism other than the one described below, it is still within the scope of the present invention. By including polysilsesquioxane in the composition of the present invention, a film formed by the composition of the present invention has a small linear expansion coefficient, and by satisfying at least one of Requirement 1 and Requirement 2, the film has excellent adhesion to metal. In this way, the composition of the present invention can form a film exhibiting desired properties from a material different from existing resin systems (e.g., epoxy resins). Hereinafter, regarding the characteristics of the composition of the present invention, a film formed by the composition having a small linear expansion coefficient will be referred to simply as "a smaller linear expansion coefficient," a film formed by the composition having excellent adhesion to metal will be referred to simply as "excellent adhesion to metal," and achieving at least one of an excellent linear expansion coefficient and excellent adhesion to metal will be referred to as "excellent effects of the present invention."

[0024] [Polysilsesquioxane] The composition of the present invention contains a polysilsesquioxane. In this specification, polysilsesquioxane refers to a polymer having a structural unit in which one silicon atom is bonded to one organic group and three oxygen atoms. The skeleton structure of the polysilsesquioxane is not particularly limited, and may be any of cage polysilsesquioxane, ladder polysilsesquioxane, double-decker polysilsesquioxane, and random polysilsesquioxane, with ladder polysilsesquioxane or cage polysilsesquioxane being preferred. The cage polysilsesquioxane may be any of complete cage polysilsesquioxane and incomplete cage polysilsesquioxane, with complete cage polysilsesquioxane being preferred. The cage polysilsesquioxane is a T consisting of eight structural units T3, which will be described later. 8 Polysilsesquioxane, T consisting of 10 constitutional units T3 described below 10 T consisting of polysilsesquioxane and 12 of the structural units T3 described below 12In terms of achieving superior effects of the present invention, the composition preferably contains at least one selected from ladder-type polysilsesquioxanes and cage-type polysilsesquioxanes, more preferably contains a cage-type polysilsesquioxane, and even more preferably contains a ladder-type polysilsesquioxane and a cage-type polysilsesquioxane. The skeletal structure of the polysilsesquioxane can be determined based on the molecular weight obtained by GPC and 29 The structure can be identified from the structural units determined from the peak positions in Si-NMR spectrum measurement. Specifically, for example, the cage polysilsesquioxane has a peak top molecular weight of T 8 Polysilsesquioxane, T 10 Polysilsesquioxane or T 12 The molecular weight of each of the cage polysilsesquioxanes is calculated appropriately depending on the substituents possessed by the cage polysilsesquioxane, and is often detected as a peak corresponding to a weight average molecular weight (Mw) of 300 to 4,000.

[0025] <Functional Group That Interacts with Metals (Interactive Groups)> When the composition does not contain a compound X described below, the polysilsesquioxane has a functional group that interacts with metals (interactive groups). Even when the composition contains a compound X described below, the polysilsesquioxane may have an interactive group. The mode of interaction between the interactive group and the metal is not particularly limited, and examples include a covalent bond, a coordinate bond, an ionic bond, a hydrogen bond, an acid-base interaction, a van der Waals bond, and a metallic bond, with a coordinate bond being preferred. The interactive group can be appropriately selected depending on the metal to be interacted with and the mode of interaction, but a group containing a nitrogen atom, an oxygen atom, or a sulfur atom is preferred. Specific examples of the interactive group include an amino group (—NR N 2 ), epoxy group, thiol group (-SH), cyano group (-CN), nitrogen-containing heterocyclic group, hydrazine group, guanidine group, phosphate group (-PO 4 H 2 ), a phosphonic acid group (—PO3 H 2 ), carboxylic acid group (-COOH), sulfo group (-SO 3 H), hydroxy group (—OH), phosphonate ester bond-containing group, sulfonate ester bond-containing group, boronic acid group (—BO 2 H 2 ), a thioether bond-containing group, and a disulfide bond-containing group are exemplified, and an amino group, an epoxy group, or a thiol group is preferred.

[0026] R N each independently represents a hydrogen atom, an alkyl group, or an aryl group. The alkyl group preferably has 1 to 6 carbon atoms, and more preferably 1 to 3 carbon atoms. The alkyl group may have a substituent, and examples of the substituent include a hydroxy group, a halogen atom, and an aryl group described below. The aryl group preferably has 4 to 12 carbon atoms, and a phenyl group is preferred as the aryl group. The aryl group may have a substituent, and examples of the substituent include a hydroxy group, a halogen atom, and the alkyl group described above.

[0027] Examples of the nitrogen-containing heterocyclic group include nitrogen-containing aromatic heterocyclic groups such as a pyridyl group, an oxazolyl group, a triazine group, a pyrrole group, a pyrazole group, an imidazole group, a pyrazole group, a triazole group, a benzimidazole group, and a benztriazole group, and nitrogen-containing aliphatic heterocyclic groups such as an imidazolidinyl group, a pyrrolidinyl group, a pyrazolidinyl group, a piperidinyl group, and a piperazinyl group, and a pyridyl group, an oxazolyl group, an imidazolidinyl group, or a pyrrolidinyl group is preferred.

[0028] The acidic groups such as the phosphate group, phosphonate group, carboxylate group, and sulfo group may be in the form of a salt in the composition, such as a salt with a metal cation or a salt with an ammonium cation.

[0029] The hydroxy group may be either an alcoholic hydroxy group (a hydroxy group bonded to an aliphatic group) or a phenolic hydroxy group (a hydroxy group bonded to an aromatic ring group), with a phenolic hydroxy group being preferred.

[0030] Examples of metals with which the interactive group interacts include copper (Cu), silver (Ag), gold (Au), cobalt (Co), ruthenium (Ru), tungsten (W), titanium (Ti), tantalum (Ta), molybdenum (Mo), germanium (Ge), zirconium (Zr), tin (Sn), nickel (Ni), palladium (Pd), aluminum (Al), indium (In), iron (Fe), zinc (Zn), and platinum (Pt), with copper or silver being preferred, and copper being more preferred. That is, the interactive group is preferably a functional group that interacts with copper.

[0031] The polysilsesquioxane preferably has a polymerizable group, since the film formed from the composition has a smaller linear expansion coefficient and better thermocycling resistance. Examples of the polymerizable group include known polymerizable groups such as radically polymerizable groups, epoxy groups, oxetanyl groups, methylol groups, and alkoxymethyl groups, with radically polymerizable groups being preferred. Examples of the radically polymerizable group include a group having an ethylenically unsaturated double bond, such as a vinyl group, a styryl group, a (meth)acryloyl group, a (meth)acrylamide group, an allyl group, and a vinyl ether group. Examples of the group having an ethylenically unsaturated double bond include a vinyl group, a styryl group, or a (meth)acryloyl group, with a styryl group being more preferred. The polymerizable group may also function as the interactive group described above.

[0032] The polysilsesquioxane preferably has a chain-like hydrocarbon group, since this allows the film formed from the composition to have better conformability to unevenness and the composition to be suitably used as a transfer film. Examples of the chain-like hydrocarbon group include a chain-like alkyl group, a chain-like alkenyl group, and a chain-like alkynyl group, with a chain-like alkyl group being preferred. The chain-like hydrocarbon group may be either linear or branched, with a linear group being preferred. The number of carbon atoms in the chain-like hydrocarbon group is preferably 1 to 20, more preferably 2 to 15, and even more preferably 4 to 12.

[0033] The polysilsesquioxane preferably contains a structural unit selected from the structural unit T1 represented by formula (T1), the structural unit T2 represented by formula (T2), and the structural unit T3 represented by formula (T3), more preferably contains a structural unit selected from the structural unit T2 and the structural unit T3, and even more preferably contains the structural unit T3. The structural units T1 to T3 belong to the so-called T units. Formula (T1): R 1 -Si(OX 1 ) 2 O 1/2 Formula (T2): R 1 -Si(OX 1 ) O 2/2 Formula (T3): R 1 -SiO 3/2 In formulas (T1) to (T3), R 1 each independently represents a monovalent organic group. 1 Each of R independently represents a hydrogen atom or an alkyl group. 1 may be the same or different. In other words, the polysilsesquioxane may contain different R 1 The copolymer may be a copolymer containing a plurality of structural units having the following structure:

[0034] In formulas (T1) to (T3), R 1each independently represents a monovalent organic group. Examples of the monovalent organic group include a hydrocarbon group and a heteroatom-containing group. The hydrocarbon group may be either an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be either chain-like or cyclic, with chain-like being preferred. The chain-like aliphatic hydrocarbon group may be either linear or branched, with linear being preferred. The aliphatic hydrocarbon group preferably has 1 to 20 carbon atoms, more preferably 1 to 15, and even more preferably 3 to 12. The aromatic hydrocarbon group preferably has 4 to 20 carbon atoms, more preferably 5 to 12, and even more preferably 5 to 6. Examples of the heteroatom-containing group include groups in which one or more carbon atoms of the hydrocarbon group are substituted with heteroatoms. The heteroatom is preferably an oxygen atom, a nitrogen atom, or a sulfur atom. The hydrocarbon group and the heteroatom-containing group may have a substituent. Examples of the substituent include a halogen atom, an alkyl group, an alkoxy group, an aryl group, the above-mentioned interactive group, and the above-mentioned polymerizable group.

[0035] R 1 The monovalent organic group represented by R is preferably a group selected from the group consisting of an interactive group-containing group, a polymerizable group-containing group, and a chain hydrocarbon group. 1 The monovalent organic group represented by the formula (I) may be, for example, a group having both an interactive group and a polymerizable group.

[0036] The interactive group-containing group is a monovalent organic group containing an interactive group, and -L Z -Z R A group represented by the following formula is preferred. R represents an interactive group. The definition and preferred embodiments of the interactive group are as described above. Z represents a single bond or a divalent linking group. Examples of the divalent linking group include a divalent aliphatic hydrocarbon group (preferably having 1 to 6 carbon atoms), a divalent aromatic ring group (preferably a phenylene group), -O-, -CO-, and groups combining these. The divalent aliphatic hydrocarbon group and the divalent aromatic ring group may have a substituent. The substituent is preferably the above-mentioned interactive group. L Zis preferably a divalent aliphatic hydrocarbon group having 1 to 6 carbon atoms, —O—, or a group formed by combining these.

[0037] The polymerizable group-containing group is a monovalent organic group containing a polymerizable group, and -L P -P R A group represented by the following formula is preferred. R represents a polymerizable group. The definition and preferred embodiments of the polymerizable group are the same as those of the polymerizable group that is preferably possessed by the polysilsesquioxane described above. P represents a single bond or a divalent linking group. Examples of the divalent linking group include L Z Examples of the divalent linking group represented by the formula: P is preferably a single bond, a divalent aliphatic hydrocarbon group having 1 to 6 carbon atoms, -O-, or a group formed by combining these.

[0038] The definition and preferred embodiments of the chain hydrocarbon group are the same as the chain hydrocarbon group that is preferably contained in the polysilsesquioxane described above.

[0039] In formulas (T1) to (T3), X 1 represents a hydrogen atom or an alkyl group. The number of carbon atoms in the alkyl group is preferably 1 to 10, more preferably 1 to 6, still more preferably 1 to 4, and particularly preferably 1 to 3. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, and an n-butyl group.

[0040] The polysilsesquioxane preferably contains a structural unit selected from the structural unit T2 and the structural unit T3. The total content of the structural units selected from the structural unit T2 and the structural unit T3 is preferably 50 mol% or more, more preferably 70 mol% or more, based on the total of all structural units of the polysilsesquioxane. There is no particular upper limit, and it may be 100 mol%. The content of each of the above structural units may be, for example, 29 It can be calculated from the peak positions and peak area ratios in Si-NMR spectrum measurement.

[0041] In order to obtain a more excellent effect of the present invention, it is preferable that the polysilsesquioxane contains a structural unit having a polymerizable group. As the structural unit having a polymerizable group, R 1 is a polymerizable group-containing group. The content of the polymerizable group-containing structural unit is preferably 10 to 90 mol %, more preferably 30 to 70 mol %, and even more preferably 40 to 60 mol %, relative to the total of all structural units of the polysilsesquioxane. In terms of superior suitability for transfer films, it is also preferable that the polysilsesquioxane contains a structural unit having a chain hydrocarbon group. Examples of structural units having a chain hydrocarbon group include those represented by R 1 is a chain hydrocarbon group. The content of the chain hydrocarbon group-containing structural unit is preferably 10 to 90 mol %, more preferably 30 to 70 mol %, and even more preferably 40 to 60 mol %, relative to the total content of all structural units of the polysilsesquioxane.

[0042] Polysilsesquioxane can be synthesized by a known method. Specifically, for example, a method of polycondensing a compound represented by formula (M1) in the presence of a polycondensation catalyst can be mentioned. Known acid catalysts and alkali catalysts can be used as the polycondensation catalyst. 1 -SiX 2 3 In formula (M1), R 1 represents a monovalent organic group. 2 each independently represents a hydrolyzable group.

[0043] In formula (M1), R 1 is R in the above formulas (T1) to (T3). 1 The same definition and preferred embodiments are also the same.

[0044] In formula (M1), X 2 each independently represents a hydrolyzable group. Examples of the hydrolyzable group include an alkoxy group, an aryloxy group, and a halogen atom, and an alkoxy group is preferred. Examples of the alkoxy group include -OX 1 A group represented by the following formula is preferred. X 1represents X in formula (T1) and formula (T2). 1 The meanings and preferred embodiments are the same as those of the above. The aryl group in the aryloxy group is preferably a phenyl group. The halogen atom includes, for example, a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and a chlorine atom is preferred.

[0045] The weight-average molecular weight (Mw) of the polysilsesquioxane is preferably 1,000 to 150,000, more preferably 3,000 to 100,000, and even more preferably 5,000 to 50,000. The number-average molecular weight (Mn) of the polysilsesquioxane is preferably 500 to 100,000, more preferably 1,000 to 10,000, and even more preferably 2,500 to 7,000. The polysilsesquioxane typically has a polydispersity index (PDI, Mw / Mn) of 1.0 or more, preferably 1.0 to 8.0, and more preferably 1.5 to 6.0. The weight-average molecular weight and number-average molecular weight of the polysilsesquioxane can be determined by detecting with a differential refractometer using a GPC analyzer equipped with a column of TSKgel Super HM-H (trade name of Tosoh Corporation) and a solvent of PFP (pentafluorophenol) / chloroform=1 / 2 (mass ratio), and converting the molecular weight using polystyrene as a standard substance.

[0046] The polysilsesquioxane may be used alone or in combination of two or more. The composition preferably contains a polysilsesquioxane having a polymerizable group. For example, the polysilsesquioxane may be a combination of a polysilsesquioxane having a polymerizable group and a polysilsesquioxane not having a polymerizable group. The content of the polysilsesquioxane having a polymerizable group is preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more, based on the total mass of the polysilsesquioxane. The upper limit is not particularly limited, and may be 100% by mass. The content of the polysilsesquioxane is preferably 50 to 99% by mass, more preferably 75 to 99% by mass, and even more preferably 85 to 99% by mass, based on the total solid content of the composition.

[0047] [Compound X] When the polysilsesquioxane does not have an interactive group, the composition contains compound X, which is a compound different from the polysilsesquioxane and has a functional group (interactive group) that interacts with a metal. The composition may contain compound X even when the polysilsesquioxane has an interactive group. The definition and preferred embodiments of the interactive group possessed by compound X are the same as those of the interactive group that may be possessed by the polysilsesquioxane described above. The number of interactive groups possessed by compound X is not particularly limited as long as it is 1 or more, but 1 to 3 is preferred.

[0048] The molecular weight of compound X is preferably 100 to 2,000, more preferably 150 to 1,000, and even more preferably 180 to 600.

[0049] The compound X preferably has a group that interacts with the polysilsesquioxane, which is different from the interactive group. The group that interacts with the polysilsesquioxane is preferably a group that forms a covalent bond with a functional group that the polysilsesquioxane has, and the Si—OX group that the polysilsesquioxane has is preferably a group that forms a covalent bond with a functional group that the polysilsesquioxane has. 1 A group that forms a covalent bond with the X group is more preferred. 1 is as described above.

[0050] In terms of achieving better effects of the present invention, compound X is preferably at least one selected from the group consisting of a compound represented by formula (1), a hydrolyzate of a compound represented by formula (1), and a hydrolysis condensate of a compound represented by formula (1). Formula (1): Z-L-Si(X) 3 In formula (1), each X independently represents a hydroxy group or a hydrolyzable group, L represents a single bond or a divalent linking group, and Z represents a functional group that interacts with a metal (interactive group).

[0051] In formula (1), each X independently represents a hydroxy group or a hydrolyzable group. Examples of the hydrolyzable group include an alkoxy group, an aryloxy group, and a halogen atom. The number of carbon atoms in the alkyl group in the alkoxy group is preferably 1 to 10, more preferably 1 to 6, still more preferably 1 to 4, and particularly preferably 1 to 3. The aryl group in the aryloxy group is preferably a phenyl group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, with a chlorine atom being preferred.

[0052] In formula (1), L represents a single bond or a divalent linking group. Examples of the divalent linking group include a divalent aliphatic hydrocarbon group, a divalent aromatic ring group, -O-, -CO-, and a group formed by combining these. However, -Si(X) 3 and the group adjacent thereto is a divalent aliphatic hydrocarbon group or a divalent aromatic ring group. The divalent aliphatic hydrocarbon group preferably has 1 to 12 carbon atoms, more preferably 1 to 6, and still more preferably 2 to 4. The divalent aromatic ring group preferably has 4 to 12 carbon atoms, more preferably 4 to 8, and preferably 6. The divalent linking group is preferably a divalent aliphatic hydrocarbon group having 1 to 6 carbon atoms, or a group formed by combining a divalent aliphatic hydrocarbon group having 1 to 6 carbon atoms with -O-.

[0053] In formula (1), Z represents a functional group (interactive group) that interacts with a metal. The definition and preferred embodiments of the interactive group represented by Z are the same as the definition and preferred embodiments of the interactive group contained in compound X.

[0054] Examples of the compound represented by formula (1) include organotrialkoxysilane compounds and organotrichlorosilane compounds, with organotrialkoxysilane compounds being preferred.

[0055] The hydrolyzate of the compound represented by formula (1) may be a complete hydrolyzate in which all of the hydrolyzable groups are hydrolyzed, a partial hydrolyzate in which only a portion of the hydrolyzable groups are hydrolyzed, or a mixture thereof. The hydrolyzate may undergo dehydration condensation with silanol groups in the system to form a hydrolyzed condensate. The hydrolyzed condensate may be a complete hydrolyzed condensate in which all of the hydrolyzed groups are condensed, a partial hydrolyzed condensate in which only a portion of the hydrolyzed groups are condensed, or a mixture thereof. In the composition, the hydrolyzate may be condensed with polysilsesquioxane.

[0056] Examples of compound X that can be used include KBM-585, KBM-303, KBM-803, KBM-802, KBM-402, KBM-403, KBM-903, KBM-603, KBM-602, KBM-573, KBM-903, and X-12-1214A (manufactured by Shin-Etsu Chemical Co., Ltd.). Known silane coupling agents can also be used as compound X.

[0057] The compound X may be used singly or in combination of two or more. The content of compound X is preferably 0.005 to 20.0 mass% and more preferably 0.01 to 10 mass% (10.0 mass%) relative to the total solid content of the composition. The mass ratio of the content of compound X to the content of polysilsesquioxane is preferably 0.0001 to 0.3 and more preferably 0.001 to 0.1.

[0058] [Requirements 1 and 2] The composition satisfies at least one of requirements 1 and 2. Requirement 1: The polysilsesquioxane has a functional group that interacts with a metal. Requirement 2: The composition further includes a compound X that is a compound different from the polysilsesquioxane and has a functional group that interacts with a metal.

[0059] [Polymerization initiator] The composition may contain a polymerization initiator. When the polysilsesquioxane has a polymerizable group or when the composition contains a polymerizable compound described below, the composition preferably contains a polymerization initiator. The polymerization initiator may be any of a radical polymerization initiator, an anionic polymerization initiator, and a cationic polymerization initiator, and a radical polymerization initiator is preferred. The polymerization initiator may be any of a thermal polymerization initiator and a photopolymerization initiator.

[0060] The radical polymerization initiator includes a thermal radical polymerization initiator and a photoradical polymerization initiator.

[0061] Examples of the thermal radical polymerization initiator include azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl-2,2'-azobis(2-methylpropionate), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(N-butyl-2-methylpropionamide), dimethyl-1,1'-azobis(1-cyclohexanecarboxylate), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride; Examples of the peroxide include organic peroxides such as t-butylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 2,2-di(4,4-di-(t-butylperoxy)cyclohexyl)propane, t-hexylperoxyisopropyl monocarbonate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, dicumyl peroxide, di-t-butyl peroxide, t-butylperoxy-2-ethylhexanoate, t-hexylperoxy-2-ethylhexanoate, cumene hydroperoxide, and t-butyl hydroperoxide; and inorganic peroxides such as potassium persulfate, ammonium persulfate, and hydrogen peroxide.

[0062] Examples of the photoradical polymerization initiator include oxime ester compounds (photopolymerization initiators having an oxime ester structure), aminoacetophenone compounds (photopolymerization initiators having an aminoacetophenone structure), hydroxyacetophenone compounds (photopolymerization initiators having a hydroxyacetophenone structure), acylphosphine oxide compounds (photopolymerization initiators having an acylphosphine oxide structure), and bistriphenylimidazole compounds (photopolymerization initiators having a bistriphenylimidazole structure).

[0063] Examples of the oxime ester compound include 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)] (trade name: IRGACURE OXE-01, manufactured by BASF), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) (trade name: IRGACURE OXE-02, manufactured by BASF), [8-[5-(2,4,6-trimethylphenyl)-11-(2-ethylhexyl)-11H-benzo[a]carbazol-3-yl]-[2-(2,2,3,3-tetrafluoropropoxy)phenyl]methanone-(O-acetyloxime) (trade name: IRGACURE OXE-03, manufactured by BASF), and OXE-03, manufactured by BASF), 1-[4-[4-(2-benzofuranylcarbonyl)phenyl]thio]phenyl]-4-methylpentanone-1-(O-acetyloxime) (trade name: IRGACURE OXE-04, manufactured by BASF and trade name: Lunar 6, manufactured by DKSH Japan Co., Ltd.), 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(O-benzoyloxime) (trade name: TR-PBG-305, manufactured by Changzhou New Power Electronic Materials Co., Ltd.), 1,2-propanedione,3-cyclohexyl-1-[9-ethyl-6-(2-furanylcarbonyl)-9H-carbazol-3-yl]-,2-(O-acetyloxime) (trade name: TR-PBG-326, manufactured by Changzhou New Power Electronic Materials Co., Ltd.), and 3-cyclohexyl-1-(6-(2-(benzoyloxyimino)hexanoyl)-9-ethyl-9H-carbazol-3-yl)-propane-1,2-dione-2-(O-benzoyloxime) (trade name: TR-PBG-391, manufactured by Changzhou New Power Electronic Materials Co., Ltd.).

[0064] Examples of aminoacetophenone compounds include 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone (trade name: Omnirad 379EG, Omnirad series, manufactured by IGM Resins B.V.), 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (trade name: Omnirad 907), and APi-307 (1-(biphenyl-4-yl)-2-methyl-2-morpholinopropan-1-one, manufactured by Shenzhen UV-ChemTech Ltd.).

[0065] Examples of the photoradical polymerization initiator include 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one (trade name: Omnirad 127), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (trade name: Omnirad 369), 2-hydroxy-2-methyl-1-phenyl-propan-1-one (trade name: Omnirad 1173), 1-hydroxy-cyclohexyl-phenyl-ketone (trade name: Omnirad 184), 2,2-dimethoxy-1,2-diphenylethan-1-one (trade name: Omnirad 651), 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (trade name: Omnirad TPO), H), and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (trade name: Omnirad 819).

[0066] Examples of the photopolymerization initiator include the photopolymerization initiators described in paragraphs 0031 to 0042 of JP-A No. 2011-095716 and paragraphs 0064 to 0081 of JP-A No. 2015-014783.

[0067] The polymerization initiator may be used alone or in combination of two or more. The content of the polymerization initiator is preferably 0.005 to 20.0 mass %, more preferably 0.01 to 10 mass %, based on the total solid content of the composition.

[0068] [Surfactant] The composition may contain a surfactant. Examples of the surfactant include a fluorine-based surfactant, a hydrocarbon-based surfactant, and a silicone-based surfactant. The surfactant is preferably a silicone-based surfactant. From the viewpoint of improving environmental compatibility, it is also preferable that the surfactant does not contain a fluorine atom.

[0069] Examples of fluorosurfactants include acrylic compounds that have a molecular structure containing a functional group having a fluorine atom, and when heated, the functional group having the fluorine atom is cleaved, causing the fluorine atom to volatilize. Examples of such fluorosurfactants include the Megafac DS series (manufactured by DIC Corporation, Chemical Daily (February 22, 2016), Nikkei Business Daily (February 23, 2016), and Megafac DS-21). Furthermore, the fluorosurfactant may be a polymer of a fluorine-containing vinyl ether compound having a fluorinated alkyl group or a fluorinated alkylene ether group, and a hydrophilic vinyl ether compound. The fluorosurfactant may be a block polymer. The fluorosurfactant may also be a fluorine-containing polymer compound containing a repeating unit derived from a (meth)acrylate compound having a fluorine atom and a repeating unit derived from a (meth)acrylate compound having two or more (preferably five or more) alkyleneoxy groups (preferably ethyleneoxy groups or propyleneoxy groups). Further, examples of fluorine-based surfactants include fluorine-containing polymers having a group with an ethylenically unsaturated double bond in the side chain, such as Megafac RS-101, RS-102, RS-718K, and RS-72-K (all manufactured by DIC Corporation).

[0070] As the fluorine-based surfactant, from the viewpoint of improving environmental compatibility, surfactants derived from alternative materials to compounds having a linear perfluoroalkyl group having 7 or more carbon atoms, such as perfluorooctanoic acid (PFOA) and perfluorooctanesulfonic acid (PFOS), are preferred.

[0071] Commercially available fluorine-based surfactants include, for example, Megafac F-171, F-172, F-173, F-176, F-177, F-141, F-142, F-143, F-144, F-437, F-475, F-477, F-479, F-482, F-551-A, F-552, F-554, F-555-A, F-556, F-557, F-558, F-559, F-560, F-561, F-565, F-563, F-568, F-575, and F-780 (all manufactured by DIC Corporation); EXP. MFS-324, EXP. MFS-330, EXP. MFS-578, EXP. MFS-578-2, EXP. MFS-579, EXP. MFS-586, EXP. MFS-587, EXP. MFS-628, EXP. MFS-631, EXP. MFS-603, R-41, R-41-LM, R-01, R-40, R-40-LM, RS-43, TF-1956, RS-90, R-94, RS-72-K, and DS-21 (all manufactured by DIC Corporation); Fluorad FC430, FC431, and FC171 (all manufactured by Sumitomo 3M Limited); Surflon S-382, SC-101, SC-103, SC-104, SC-105, SC-1068, SC-381, SC-383, S-393, and KH-40 (all manufactured by AGC); PolyFox Examples of such products include PF636, PF656, PF6320, PF6520, and PF7002 (manufactured by OMNOVA); Ftergent 710FL, 710FM, 610FM, 601AD, 601ADH2, 602A, 215M, 245F, 251, 212M, 250, 209F, 222F, 208G, 710LA, 710FS, 730LM, 650AC, 681, and 683 (manufactured by NEOS Corporation); and U-120E (manufactured by Unichem).

[0072] Examples of hydrocarbon surfactants include glycerol, trimethylolpropane, trimethylolethane, and their ethoxylates and propoxylates (e.g., glycerol propoxylate and glycerol ethoxylate), polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyethylene glycol dilaurate, polyethylene glycol distearate, and sorbitan fatty acid ester. Commercially available hydrocarbon surfactants include, for example, Pluronic (registered trademark) L10, L31, L61, L62, 10R5, 17R2, and 25R2, Tetronic 304, 701, 704, 901, 904, and 150R1, and HYDROPALAT WE 3323 (all manufactured by BASF); Solsperse 20000 (manufactured by Lubrizol Japan Corporation); NCW-101, NCW-1001, and NCW-1002 (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.); Paionin D-1105, D-6112, D-6112-W, and D-6315 (all manufactured by Takemoto Yushi Co., Ltd.); Olfine E1010, Surfynol 104, 400, and 440 (all manufactured by Nissin Chemical Industry Co., Ltd.).

[0073] Examples of silicone surfactants include linear polymers consisting of siloxane bonds, modified siloxane polymers with organic groups introduced into the side chains and / or terminals, and polymers having a repeating unit with a hydrophilic group in the side chain and a repeating unit with a group having a siloxane bond in the side chain.Preferred silicone surfactants are polymers having a repeating unit with a hydrophilic group in the side chain and a repeating unit with a group having a siloxane bond in the side chain.The polymers may be either random copolymers or block copolymers.

[0074] The repeating unit having a group having a siloxane bond in the side chain is preferably a repeating unit represented by formula (SX1) or a repeating unit represented by formula (SX2).

[0075]

[0076] In formula (SX1), each R independently represents an alkyl group having 1 to 3 carbon atoms. 1 represents a hydrogen atom or a methyl group. 1 represents a single bond or a divalent organic group. When a plurality of R's are present, the R's may be the same or different.

[0077]

[0078] In formula (SX2), R 1 represents a hydrogen atom or a methyl group. 2 represents an alkylene group having 1 to 10 carbon atoms. 3 represents an alkyl group having 1 to 4 carbon atoms, and n represents an integer of 5 to 50.

[0079] The repeating unit having a hydrophilic group in the side chain is preferably a repeating unit represented by formula (SX3).

[0080]

[0081] In formula (SX3), R 4 and R 5 each independently represents a hydrogen atom or a methyl group, n represents an integer of 1 to 4, and m represents an integer of 1 to 100.

[0082] Commercially available silicone surfactants include, for example, EXP. S-309-2, EXP. S-315, EXP. S-503-2, EXP. S-505-2, and S-506 (all manufactured by DIC Corporation); DOWSIL 8032 ADDITIVE, Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, and Toray Silicone SH8400 (all manufactured by Dow Corning Toray Co., Ltd.); X-22-4952, X-22-4272, and X-22-6266. , KF-351A, K354L, KF-355A, KF-945, KF-640, KF-642, KF-643, X-22-6191, X-22-4515, KF-6004, KF-6001, K F-6002, KP-101KP-103, KP-104, KP-105, KP-106, KP-109, KP-109, KP-112, KP-120, KP-121, KP-124, KP-125 , KP-301, KP-306, KP-310, KP-322, KP-323, KP-327, KP-341, KP-368, KP-369, KP-611, KP-620, KP-621, KP-626, and KP-652 (all manufactured by Shin-Etsu Silicone Co., Ltd.); F-4440, TSF-4300, TSF-4445, TSF-4460, and TSF-4452 (all manufactured by Momentive Perform BYK300, BYK306, BYK307, BYK310, BYK320, BYK323, BYK325, BYK330, BYK313, BYK315N, BYK331, BYK333, BYK345, BYK347, BYK348, BYK349, BYK370, BYK377, BYK378, and BYK323 (all manufactured by BYK-Chemie).

[0083] Other examples of the surfactant include nonionic surfactants other than those mentioned above, such as those described in paragraph 0017 of Japanese Patent No. 04502784 and paragraphs 0060 to 0071 of JP-A-2009-237362.

[0084] The surfactant may be used alone or in combination of two or more. The content of the surfactant is preferably 0.01 to 3.0 mass %, more preferably 0.05 to 1.0 mass %, and still more preferably 0.1 to 0.8 mass %, based on the total solid content of the composition.

[0085] [Polymerizable Compound] The composition may contain a polymerizable compound. The polymerizable compound is a compound different from the various components described above. The polymerizable compound is a compound having one or more polymerizable groups in the molecule. Examples of the polymerizable group include the polymerizable groups that the polysilsesquioxane described above may have. A group having an ethylenically unsaturated double bond is preferred, a (meth)acryloyl group, a vinyl group, or a styryl group is more preferred, and a (meth)acryloyl group is even more preferred.

[0086] The number of polymerizable groups in the polymerizable compound is preferably 1 or 2 or more, more preferably 2 to 10, and even more preferably 2 to 6. Examples of the polymerizable compound include a polymerizable compound having one polymerizable group in one molecule (hereinafter also referred to as a "monofunctional polymerizable compound"), a polymerizable compound having two polymerizable groups in one molecule (hereinafter also referred to as a "bifunctional polymerizable compound"), and a polymerizable compound having three or more polymerizable groups in one molecule (hereinafter also referred to as a "trifunctional or higher functional polymerizable compound"). The polymerizable compound is preferably a bifunctional polymerizable compound or a trifunctional or higher functional polymerizable compound.

[0087] Examples of bifunctional polymerizable compounds include polyethylene glycol (meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, tricyclodecane dimenanol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and 1,6-hexanediol di(meth)acrylate. Commercially available bifunctional polymerizable compounds include, for example, diethylene glycol dimethacrylate (2G, manufactured by Shin-Nakamura Chemical Co., Ltd.), triethylene glycol dimethacrylate (3G, manufactured by Shin-Nakamura Chemical Co., Ltd.), polyethylene glycol #200 dimethacrylate (4G, manufactured by Shin-Nakamura Chemical Co., Ltd.), tricyclodecane dimethanol diacrylate (A-DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), tricyclodecane dimenanol dimethacrylate (DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,9-nonanediol diacrylate (A-NOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,6-hexanediol diacrylate (A-HD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), SR205NS (manufactured by Sartomer Inc.), and SR209 (manufactured by Sartomer Inc.).

[0088] Examples of trifunctional or higher functional polymerizable compounds include dipentaerythritol (tri / tetra / penta / hexa)(meth)acrylate, pentaerythritol (tri / tetra)(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, isocyanuric acid (meth)acrylate, and (meth)acrylate compounds with a glycerin tri(meth)acrylate skeleton. "(Tri / tetra / penta / hexa)(meth)acrylate" is a concept that encompasses tri(meth)acrylate, tetra(meth)acrylate, penta(meth)acrylate, and hexa(meth)acrylate, and "(tri / tetra)(meth)acrylate" is a concept that encompasses tri(meth)acrylate and tetra(meth)acrylate.

[0089] Examples of the polymerizable compound include caprolactone-modified (meth)acrylate compounds (KAYARAD (registered trademark) DPCA-20, etc., manufactured by Nippon Kayaku Co., Ltd., and A-9300-1CL, etc., manufactured by Shin-Nakamura Chemical Co., Ltd.), alkylene oxide-modified (meth)acrylate compounds (KAYARAD RP-1040, etc., manufactured by Nippon Kayaku Co., Ltd., ATM-35E and A-9300, etc., manufactured by Shin-Nakamura Chemical Co., Ltd., and EBECRYL (registered trademark) 135, etc., manufactured by Daicel-Allnex Corporation), and ethoxylated glycerin triacrylate (A-GLY-9E, etc., manufactured by Shin-Nakamura Chemical Co., Ltd.).

[0090] Examples of the polymerizable compound include urethane (meth)acrylates (preferably tri- or higher functional urethane (meth)acrylates). The number of polymerizable groups in the urethane (meth)acrylate is preferably 6 or more, and more preferably 8 or more. The upper limit is preferably 20 or less. Examples of tri- or higher functional urethane (meth)acrylates include 8UX-015A (manufactured by Taisei Fine Chemical Co., Ltd.); UA-32P, U-15HA, and UA-1100H (all manufactured by Shin-Nakamura Chemical Co., Ltd.); AH-600 (manufactured by Kyoeisha Chemical Co., Ltd.); UA-306H, UA-306T, UA-306I, UA-510H, and UX-5000 (all manufactured by Nippon Kayaku Co., Ltd.).

[0091] The polymerizable compound may be used alone or in combination of two or more. The content of the polymerizable compound is preferably 0.1 to 15.0 mass %, more preferably 1.0 to 10.0 mass %, based on the total solid content of the composition.

[0092] [Other Additives] The composition may contain other additives in addition to those described above. Examples of the other additives include solvents, fillers, heterocyclic compounds, aliphatic thiol compounds, thermally crosslinkable compounds, polymerization inhibitors, hydrogen donor compounds, impurities, plasticizers, sensitizers, and maleimide compounds.

[0093] <Solvent> The composition may contain a solvent. The solvent is not particularly limited as long as it can dissolve or disperse various components that may be contained in the composition other than the solvent. Examples of solvents include water, alkylene glycol ether solvents, alkylene glycol ether acetate solvents, alcohol solvents (e.g., methanol, ethanol, etc.), ketone solvents (e.g., acetone, methyl isobutyl ketone, methyl ethyl ketone, etc.), aromatic hydrocarbon solvents (e.g., toluene, etc.), aprotic polar solvents (e.g., N,N-dimethylformamide, etc.), cyclic ether solvents (e.g., tetrahydrofuran, etc.), ester solvents (e.g., n-propyl acetate, etc.), amide solvents, lactone solvents, and solvents containing two or more of these. The solvents may be used alone or in combination. The content of the solvent is preferably 50 to 1900 parts by mass, more preferably 100 to 1200 parts by mass, and even more preferably 100 to 900 parts by mass, relative to 100 parts by mass of the total solids content of the composition.

[0094] <Filler> The composition may contain a filler. The average particle diameter of the filler is preferably 500 nm or less, more preferably 300 nm or less, and even more preferably 150 nm or less. The lower limit of the average particle diameter of the filler is more than 0 nm, preferably 5 nm or more, and more preferably 10 nm or more. The average particle diameter of the filler is also preferably 5 to 300 nm, and more preferably 10 to 150 nm. The average particle diameter of the filler is a value calculated by the following particle diameter measurement method. Particle diameter measurement method: A rectangular region of 3 μm × 10 μm in a cross section taken along the normal direction to the surface of a composition layer formed using the composition is observed with a scanning electron microscope, and the major axes of all fillers observed within the region are measured at five different locations in the composition layer. The average value of the major axes of all fillers measured in each measurement is defined as the average particle diameter of the filler.

[0095] The particle size measurement method is described in detail below. The composition is applied to a substrate (preferably a glass substrate) to form a composition layer. The thickness of the composition layer is preferably 3 μm or more. Furthermore, to form the composition layer, a drying treatment may be performed, if necessary, after the composition is applied. A cross section of the resulting composition layer along the normal direction of its surface (the surface opposite the substrate side) is cut out, and a rectangular region of 3 μm x 10 μm on the cross section is observed using a scanning electron microscope, and the major axes of all fillers observed within the region are measured. The scanning electron microscope used is an S-4800 manufactured by Hitachi High-Tech Corporation. The magnification used for observation is 50,000x. The above procedure is performed at five different locations on the composition layer, and the average (arithmetic mean) of the major axes of all fillers measured in each procedure is taken as the average particle size of the filler. The major axis refers to the length of the longest line segment connecting any two points on the outline of the filler's outer shape in the observed image. Furthermore, when fillers are aggregated to form aggregates in the observed image, the major axis of each filler constituting the aggregate is measured.

[0096] The filler is preferably an inorganic filler. Examples of the filler include silicon dioxide (silica); silicates such as kaolinite, kaolin clay, calcined clay, talc, and glass fillers such as chion-doped glass; alumina, barium sulfate, mica powder, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum borate, barium titanate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, barium zirconate, calcium zirconate, zirconium phosphate, cordierite, zirconium tungstate, and manganese nitride. The filler preferably contains at least one selected from the group consisting of silicon dioxide (silica), boron nitride, barium sulfate, and silicates, and more preferably contains silicon dioxide (silica).

[0097] The shape of the filler may be either spherical or non-spherical (e.g., crushed or fibrous), with spherical being preferred. The filler may be surface-treated. Examples of surface treatments include treatments to introduce functional groups and treatments using known surface treatment agents. Examples of the functional groups include polymerizable groups (such as polymerizable groups that polysilsesquioxane may have) and hydrophobic groups. Examples of surface treatment agents include silane coupling agents, silazane compounds, and titanate-based coupling agents. Examples of methods for surface treatment of the filler include a dry method in which surface treatment is performed in a gas phase and a wet method in which surface treatment is performed in a liquid phase.

[0098] Examples of fillers include NHM-5N (manufactured by Tokuyama Corporation, silicon dioxide, solid content concentration 100% by mass), NHM-3N (manufactured by Tokuyama Corporation, silicon dioxide, solid content concentration 100% by mass), Seahoster KE-S30 (manufactured by Nippon Shokubai Co., Ltd., silicon dioxide, solid content concentration 100% by mass), YA050C-MJE (manufactured by Admatechs Co., Ltd., silicon dioxide, solid content concentration 50% by mass MEK slurry), SFP-20M (manufactured by Denka Co., Ltd., silicon dioxide), PMA-ST (manufactured by Nissan Chemical Industries, Ltd., silicon dioxide), and M Examples of such an emulsion include EK-ST-L (manufactured by Nissan Chemical Industries, Ltd., silicon dioxide), MEK-AC-5140Z (manufactured by Nissan Chemical Industries, Ltd., silicon dioxide), MEK-EC-2430Z (manufactured by Nissan Chemical Industries, Ltd., solids concentration 30% by mass), barium sulfate (manufactured by Nippon Solvay K.K., solids concentration 100% by mass), Y50SP-AM1 (manufactured by Admatechs Co., Ltd., silicon dioxide, MEK slurry with a solids concentration of 50% by mass), and Y50SZ-AM1 (manufactured by Admatechs Co., Ltd., silicon dioxide, MEK slurry with a solids concentration of 50% by mass).

[0099] The filler may be used alone or in combination of two or more. The content of the filler is preferably 10 to 90 mass %, more preferably 30 to 80 mass %, based on the total solid content of the composition.

[0100] Examples of the heterocyclic compound, aliphatic thiol compound, thermal crosslinking compound, polymerization inhibitor, and hydrogen donor compound include the various components described in WO 2022 / 039027. Examples of the plasticizer and sensitizer include those described in paragraphs 0097 to 0119 of WO 2018 / 179640. Examples of the maleimide compound (compound having a maleimide ring) include known maleimide compounds and the maleimide compounds described in WO 2022 / 102756.

[0101] The composition may contain impurities. Examples of impurities include sodium, potassium, magnesium, calcium, iron, manganese, copper, aluminum, titanium, chromium, cobalt, nickel, zinc, tin, halogens, and ions thereof. Because halide ions, sodium ions, and potassium ions are easily mixed in as impurities, the following contents are preferred.

[0102] The content of impurities is preferably 80 ppm by mass or less, more preferably 10 ppm by mass or less, and even more preferably 2 ppm by mass or less, relative to the total mass of the composition. The lower limit is often 0 ppb by mass or more, but may be 1 ppb by mass or more, or 0.1 ppm by mass or more, relative to the total mass of the composition.

[0103] Methods for adjusting the content of impurities include, for example, using raw materials with low impurity contents as raw materials for the various components that may be contained in the composition, purifying the various components that may be contained in the composition before use, and preventing the inclusion of impurities when preparing the composition.

[0104] The content of impurities can be determined by known methods such as ICP (Inductively Coupled Plasma) emission spectroscopy, atomic absorption spectroscopy, and ion chromatography.

[0105] The content of compounds such as benzene, formaldehyde, trichloroethylene, 1,3-butadiene, carbon tetrachloride, chloroform, N,N-dimethylformamide, N,N-dimethylacetamide, and hexane in the composition is preferably low. Specifically, the content of each of these compounds is preferably 100 ppm by mass or less, more preferably 20 ppm by mass or less, and even more preferably 4 ppm by mass or less, relative to the total mass of the composition. The lower limit may be 10 ppb by mass or more, or 100 ppb by mass or more, relative to the total mass of the composition. The content of these compounds can be adjusted using the same method as for the impurities described above. Furthermore, these compounds can be quantified using known measurement methods.

[0106] [Film] The composition of the present invention can form a film. The method for forming the film is not particularly limited, and examples include a method in which the composition is applied to a substrate, dried, and then cured. Examples of the curing treatment include the curing treatment used in step 3 of the semiconductor package manufacturing method described below. That is, the film is preferably a cured film of the composition. In the cured film, some or all of the components contained in the composition may have reacted (e.g., condensation of unreacted silanol groups in the polysilsesquioxane, polymerization of polymerizable groups, and reaction of the polysilsesquioxane with compound X) through the curing treatment, or some of the components contained in the composition (e.g., solvent) may have been removed.

[0107] The average thickness of the film is preferably 0.5 μm or more, more preferably 1.0 μm or more, even more preferably 3.0 μm or more, and particularly preferably 5.0 μm or more, from the viewpoint of superior insulating properties, and is preferably 40 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, and particularly preferably 19 μm or less, from the viewpoint of superior pattern resolution.

[0108] [Transfer Film] The transfer film of the present invention has a temporary support and a composition layer formed using the above-described composition.

[0109] FIG. 1 is a cross-sectional schematic diagram showing an example of an embodiment of a transfer film. The transfer film 100 shown in FIG. 1 has a configuration in which a temporary support 12, a composition layer 14, and a cover film 16 are laminated in this order. Although the transfer film 100 shown in FIG. 1 has the cover film 16, the transfer film may have no cover film 16. Furthermore, as described below, the transfer film may further have an intermediate layer and / or a thermoplastic resin layer. Each component of the transfer film will be described in detail below.

[0110] [Temporary Support] The transfer film has a temporary support, which is a member that supports the composition layer and is ultimately removed by a peeling treatment.

[0111] The temporary support may have either a single-layer structure or a multi-layer structure. The temporary support is preferably a film, more preferably a resin film. The temporary support is also preferably a film that is flexible and does not significantly deform, shrink, or stretch under pressure, or under pressure and heat. Examples of the film include polyethylene terephthalate (PET) films (e.g., biaxially oriented polyethylene terephthalate films), polymethyl methacrylate films, cellulose triacetate films, polystyrene films, polyimide films, and polycarbonate films, with polyethylene terephthalate films being preferred. Furthermore, the temporary support is preferably free of deformations such as wrinkles and scratches.

[0112] The temporary support preferably has high transparency in order to enable pattern exposure through the temporary support. Specifically, the transmittance at each of the wavelengths of 313 nm, 365 nm, 405 nm, and 436 nm is preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, and most preferably 90% or more. The upper limit is preferably less than 100%. Preferred values ​​of the transmittance at each of the above wavelengths include, for example, 87%, 92%, and 98%. In terms of the pattern formability during pattern exposure through the temporary support and the transparency of the temporary support, the haze of the temporary support is preferably small. Specifically, the haze value of the temporary support is preferably 2% or less, more preferably 0.5% or less, and even more preferably 0.1% or less. The lower limit is preferably 0% or more. In terms of the pattern formability during pattern exposure through the temporary support and the transparency of the temporary support, the number of fine particles, foreign matter, and defects contained in the temporary support is preferably small. The number of particles, foreign matter, and defects with a diameter of 1 μm or more on the temporary support is 50 / 10 mm. 2 Preferably, 10 pieces / 10 mm or less 2 More preferably, 3 pieces / 10 mm or less 2 More preferably, 0 pieces / 10 mm or less 2 is particularly preferred.

[0113] The thickness of the temporary support is preferably 5 to 200 μm, and from the viewpoint of ease of handling and versatility, more preferably 5 to 150 μm, still more preferably 5 to 50 μm, and particularly preferably 5 to 35 μm. The thickness of the temporary support can be calculated as the average value of any five points measured by cross-sectional observation using an SEM (scanning electron microscope).

[0114] In order to improve the adhesion between the temporary support and the composition layer, the surface of the temporary support that comes into contact with the composition layer may be surface-modified by UV irradiation, corona discharge, plasma, etc. When the surface is modified by UV irradiation, the exposure dose of UV irradiation is 10 to 2000 mJ / cm. 2 is preferred, and 50 to 1000 mJ / cm 2Examples of light sources for UV irradiation include low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, and light-emitting diodes that emit light in the wavelength range of 150 to 450 nm. The lamp output and illuminance can be adjusted as appropriate.

[0115] Examples of the temporary support include a biaxially oriented polyethylene terephthalate film having a thickness of 16 μm, a biaxially oriented polyethylene terephthalate film having a thickness of 12 μm, and a biaxially oriented polyethylene terephthalate film having a thickness of 9 μm. The temporary support may be a recycled product. Examples of the recycled product include a film obtained by cleaning and chipping used films. Examples of commercially available recycled products include the Ecouse series (manufactured by Toray Industries, Inc.).

[0116] Examples of temporary supports include those described in paragraphs 0017 to 0018 of JP-A-2014-085643, paragraphs 0019 to 0026 of JP-A-2016-027363, paragraphs 0041 to 0057 of WO 2012 / 081680, and paragraphs 0029 to 0040 of WO 2018 / 179370, the contents of which are incorporated herein by reference.

[0117] The temporary support may have a layer containing fine particles (lubricant layer) on one or both sides of the temporary support for the purpose of imparting handleability. The diameter of the fine particles contained in the lubricant layer is preferably 0.05 to 0.8 μm. The film thickness of the lubricant layer is preferably 0.05 to 1.0 μm. Commercially available temporary supports include Lumirror 16FB40, Lumirror 16KS40, Lumirror #38-U48, Lumirror #75-U34, and Lumirror #25T60 (all manufactured by Toray Industries, Inc.); and Cosmoshine A4100, Cosmoshine A4160, Cosmoshine A4300, Cosmoshine A4360, and Cosmoshine A8300 (all manufactured by Toyobo Co., Ltd.).

[0118] [Composition Layer] The composition layer is a layer formed using the above composition. The various components that can be contained in the composition layer are synonymous with the various components that can be contained in the above composition, and the preferred embodiments are also the same. However, the preferred numerical ranges for the contents of the various components in the composition layer are the same as the preferred ranges obtained by replacing the above "contents (% by mass) of the various components relative to the total solid content of the composition" with "contents (% by mass) of the various components relative to the total mass of the composition layer." Specifically, the statement "The content of the polysilsesquioxane is preferably 5.0% by mass or more relative to the total solid content of the composition" should be replaced with "The content of the polysilsesquioxane is preferably 5.0% by mass or more relative to the total mass of the composition layer."

[0119] The composition layer preferably further contains a solvent. The solvent has the same meaning as the solvent that may be contained in the composition, and the preferred embodiments are also the same.

[0120] The average thickness of the composition layer is preferably 0.5 μm or more, more preferably 1.0 μm or more, even more preferably 3.0 μm or more, and particularly preferably 5.0 μm or more. In terms of excellent pattern resolution, the average thickness of the composition layer is preferably 40 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, and particularly preferably 19 μm or less.

[0121] The transfer film may have layers other than those described above.

[0122] [Intermediate layer and thermoplastic resin layer] The transfer film may have an intermediate layer and / or a thermoplastic resin layer. Examples of the intermediate layer and the thermoplastic resin layer include those described in paragraphs 0164 to 0204 of WO 2021 / 166719, the contents of which are incorporated herein by reference.

[0123] [Cover Film] The transfer film may have a cover film. The number of fisheyes having a diameter of 80 μm or more contained in the cover film is 5 / m. 2 The following are preferred: Fisheyes are foreign matter, undissolved matter, and / or oxidized and deteriorated matter of the material that is introduced into the film when the material is thermally melted and then kneaded, extruded, and / or biaxially stretched, cast, or other methods are used to produce the film.

[0124] The number of particles with a diameter of 3 μm or more contained in the cover film is 30 / mm 2 Preferably, 10 pieces / mm or less 2 More preferably, 5 or less pieces / mm 2 The following is more preferable: This can suppress defects caused by the transfer of irregularities due to particles contained in the cover film to the composition layer.

[0125] The arithmetic mean roughness Ra of the surface of the cover film is preferably 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.03 μm or more.If Ra is within this range, for example, when the transfer film is long, the winding property of the transfer film is excellent.In addition, from the viewpoint of suppressing defects during transfer, Ra is preferably less than 0.50 μm, more preferably 0.40 μm or less, and even more preferably 0.30 μm or less.

[0126] Examples of the cover film include polyethylene terephthalate film, polypropylene film, polystyrene film, and polycarbonate film, and examples of the cover film include the cover films described in paragraphs 0083 to 0087 and 0093 of JP-A No. 2006-259138.

[0127] Examples of cover films include Alphan (registered trademark) FG-201 (manufactured by Oji F-Tex Co., Ltd.), Alphan (registered trademark) E-201F (manufactured by Oji F-Tex Co., Ltd.), Therapeel (registered trademark) 25WZ (manufactured by Toray Advanced Film Co., Ltd.), and Lumirror (registered trademark) 16QS62 (16KS40) (manufactured by Toray Industries, Inc.). The cover film may be a recycled product. Examples of recycled products include those obtained by cleaning and chipping used films and then forming the resulting material into films. Examples of commercially available recycled products include the Ecouse series (manufactured by Toray Industries, Inc.).

[0128] The transfer film may include other layers in addition to the above-described layers. Examples of the other layers include a high refractive index layer. Examples of the high refractive index layer include those described in paragraphs 0168 to 0188 of International Publication No. 2021 / 187549, the contents of which are incorporated herein by reference.

[0129] [Method for manufacturing transfer film] A known manufacturing method can be applied to the manufacturing method of the transfer film. In the manufacturing method of the transfer film, it is preferable to coat a composition on a temporary support to form a composition layer, and it is more preferable to dry a coating film of the composition to form a composition layer. Examples of the coating method include slit coating, spin coating, curtain coating, and inkjet coating.

[0130] For example, a method for manufacturing the transfer film 100 shown in Fig. 1 includes a step of applying a composition to the surface of a temporary support 12 to form a coating film, and then drying this coating film to form a composition layer 14. Furthermore, the transfer film 100 shown in Fig. 1 is manufactured by pressing a cover film 16 onto the composition layer of the transfer film manufactured by the above manufacturing method. Furthermore, the transfer film 100 shown in Fig. 1 may be wound up after manufacturing and stored as a roll-form transfer film 100. The roll-form transfer film 100 can be provided in its original form for the lamination step with a substrate in a roll-to-roll system described below.

[0131] As described above, the transfer film may have an intermediate layer and / or a thermoplastic resin layer between the temporary support and the composition layer. Examples of the intermediate layer-forming composition, the method for forming the intermediate layer, the thermoplastic resin layer-forming composition, and the method for forming the thermoplastic resin layer are described in paragraphs 0133 to 0136 and 0143 to 0144 of International Publication No. 2021 / 033451, the contents of which are incorporated herein by reference.

[0132] [Applications] Films formed using the composition or transfer film can be used in a variety of applications. For example, they can be used in insulating films, electrode protective films, planarizing films, overcoat films, hard coat films, passivation films, partitions, spacers, microlenses, optical filters, anti-reflection films, etching resists, and plated members. More specifically, they can be used in protective or insulating films for touch panel electrodes, protective or insulating films for printed wiring boards, protective or insulating films for TFT substrates, interlayer insulating films in build-up substrates for semiconductor packages, organic interposers, color filters, overcoat films for color filters, and etching resists for wiring formation. In particular, the composition and transfer film can be suitably used to form insulating films, and the insulating films are preferably used as insulating layers for semiconductor packages. That is, the composition and transfer film are preferably used to form insulating layers for semiconductor packages.

[0133] [Method for manufacturing a semiconductor package] The method for manufacturing a semiconductor package of the present invention includes the following steps: Step 1: forming a composition layer on a substrate using a composition Step 2: forming a pattern including vias in the composition layer Step 3: subjecting the pattern to at least one of heating and exposure Each step of the method for manufacturing a semiconductor package will be described in detail below.

[0134] [Step 1] Step 1 is a step of forming a composition layer on a substrate using a composition. Methods for forming the composition layer include a method of applying the composition and a method using a transfer film. Examples of methods for applying the composition include the composition application method in the above-mentioned method for producing a transfer film. The composition layer may be formed by drying a coating of the composition. A specific example of a method for forming a composition layer using a transfer film is a method in which the surface of the composition layer in the transfer film opposite the temporary support side is brought into contact with the substrate and the transfer film and substrate are laminated together. Examples of lamination methods include known transfer methods and lamination methods. Preferred methods include a method in which the substrate is laminated on the surface of the composition layer and pressure and heat are applied using a roll or the like. Examples of lamination methods include known laminators such as vacuum laminators and auto-cut laminators. The lamination temperature is not particularly limited, but is preferably 70 to 130°C. When a transfer film is used, Step 1 is preferably performed using a roll-to-roll system. The substrate to which the transfer film is laminated is preferably a resin film or a resin film having a conductive layer. The roll-to-roll method refers to a method in which a substrate that can be wound up and unwound is used as the substrate, and includes a step of unwinding the substrate before any of the steps included in the method for producing a laminate of the present invention, and a step of winding the substrate after any of the steps, and at least any of the steps (preferably all of the steps or all of the steps other than the heating step) is performed while the substrate is being transported. As the unwinding method in the unwinding step and the winding method in the winding step, any method known in the art for production methods that apply the roll-to-roll method may be used.

[0135] <Substrate> The substrate is preferably a substrate containing a metal. The metal is a metal that interacts with the above-mentioned interactive group, and is preferably copper or silver, and more preferably copper. The form of the metal contained in the substrate is not particularly limited, and examples thereof include simple metals, alloys, nitrides, oxides, and silicides, and simple metals or alloys are preferred, and simple metals are more preferred. Examples of the alloy include alloys containing two or more of the metals exemplified as metals that interact with the above-mentioned interactive group, and alloys containing copper are preferred. The metal may also be present as a conductive metal oxide. Examples of conductive metal oxides include ITO (indium tin oxide), IZO (indium zinc oxide), and SiO 2 The conductivity is such that the volume resistivity is 1×10 6 It means that the volume resistivity is less than 1×10 4 It is preferably less than Ωcm.

[0136] The substrate is preferably a substrate having the above metal as a conductive layer. Examples of substrates having a conductive layer include glass substrates, glass epoxy substrates, silicon substrates, and resin substrates. The substrate may be composed of a light-transmitting substrate such as a glass substrate, and tempered glass, such as Corning Gorilla Glass, can also be used. Materials contained in the substrate include, for example, materials used in JP 2010-086684 A, JP 2010-152809 A, and JP 2010-257492 A. When the substrate includes a resin substrate, a resin film with low optical distortion and / or high transparency is more preferred. Specific examples include polyethylene terephthalate (PET), polyethylene naphthalate, polycarbonate, triacetyl cellulose, cycloolefin polymer, and polyimide.

[0137] The substrate having a conductive layer is preferably a resin substrate having a conductive layer, and more preferably a resin film having a conductive layer, because it can be produced by a roll-to-roll process. The substrate having a conductive layer may be a laminate obtained by the above-mentioned method for producing a laminate.

[0138] The conductive layer in the substrate having a conductive layer may be one layer or two or more layers. When the substrate having a conductive layer includes two or more conductive layers, the conductive layers may be made of different materials.

[0139] The conductive layer may be patterned. Examples of methods for producing a patterned conductive layer include subtractive methods such as etching and additive methods. Examples of etching methods include wet etching methods described in paragraphs 0048 to 0054 of JP 2010-152155 A and known dry etching methods such as plasma etching. The etching method may also be a method using an etching resist.

[0140] [Step 2] Step 2 is a step of forming a pattern having vias in the composition layer. The pattern having vias may be formed only in the composition layer, or may be formed in both the composition layer and the substrate. The pattern including vias may be either a through hole or a via hole. Examples of the shape of the via include a square, trapezoid, and inverted trapezoid cross-sectional shape; and a circle or square front shape (the shape when the via is observed from the direction in which the via bottom is visible). In view of improving the adhesion of plated copper to the via wall surface, an inverted trapezoid cross-sectional shape is preferred. The via size (diameter) is preferably 300 μm or less, more preferably 100 μm or less, even more preferably 50 μm or less, and particularly preferably 5 μm or less. The lower limit is preferably 1 μm or more. The number of vias may be 1 or more, and preferably 2 or more.

[0141] Methods for forming a pattern having vias include, for example, methods using a drill, a laser, and plasma.

[0142] Furthermore, when the composition layer is photosensitive, the method for forming a pattern having vias preferably includes the steps of exposing the composition layer to light in a pattern and developing the exposed composition layer using a developer to form a pattern.

[0143] In the step of patternwise exposure, the composition layer may be exposed from the side opposite to the substrate, or from the substrate side of the composition layer.

[0144] The light source used for exposure may be any light source that irradiates light in a wavelength range (e.g., light in wavelength ranges of 254 nm, 313 nm, 365 nm, and 405 nm) to which various photosensitive components (e.g., photopolymerization initiators) in the composition layer are sensitive. Specific examples include ultra-high pressure mercury lamps, high pressure mercury lamps, metal halide lamps, and LEDs (Light Emitting Diodes). The exposure dose is 5 to 200 mJ / cm. 2 is preferred, and 10 to 200 mJ / cm 2 is more preferred.

[0145] When the composition layer is formed using a transfer film, the layer may be exposed after peeling off the temporary support, or may be exposed through the temporary support before peeling off the temporary support, and then the temporary support may be peeled off. In order to prevent mask contamination due to contact between the composition layer and the mask and to avoid the influence of foreign matter attached to the mask on the exposure, it is preferable to perform pattern exposure without peeling off the temporary support. The pattern exposure may be exposure through a mask or direct exposure using a laser or the like. Examples of masks include quartz masks, soda-lime glass masks, and film masks. Quartz masks are preferred because of their excellent dimensional accuracy, and film masks are preferred because they can be easily made into large sizes. As a material for the film mask, polyester film is preferred, and polyethylene terephthalate film is more preferred. As a material for the film mask, for example, XPR-7S SG (manufactured by Fujifilm Global Graphic Systems Co., Ltd.) is exemplified.

[0146] [Step 3] Step 3 is a step of performing a curing treatment on the pattern. An insulating film derived from the composition is formed by Step 3. Examples of the curing treatment include a heating treatment and an exposure treatment, and the curing treatment preferably includes at least a heating treatment.

[0147] The temperature and time of the heat treatment can be appropriately selected depending on the components of the composition. The heat treatment temperature is preferably 120 to 400°C, more preferably 150 to 400°C, and even more preferably 180 to 350°C. The heat treatment time is preferably 0.5 to 24 hours, more preferably 1 to 12 hours, and even more preferably 1 to 9 hours. The heat treatment may be carried out in either an air environment or a nitrogen-substituted environment. The atmospheric pressure in the heat treatment environment is preferably 8.1 kPa or more, more preferably 50.66 kPa or more. The upper limit is preferably 121.6 kPa or less, more preferably 111.46 kPa or less, and even more preferably 101.3 kPa or less.

[0148] The light source and exposure dose for the exposure treatment can be appropriately selected depending on the type of photosensitive component (e.g., photopolymerization initiator) in the composition layer. Examples of light sources include ultra-high pressure mercury lamps, high pressure mercury lamps, metal halide lamps, and LEDs (Light Emitting Diodes). The exposure dose is 5 to 1,000 mJ / cm. 2 is preferred, and 10 to 200 mJ / cm 2 is more preferred.

[0149] [Step 4] The method for manufacturing a semiconductor package preferably includes step 4, in which a circuit pattern is formed on the pattern after step 3. A semi-additive process is preferred as a method for forming the circuit pattern, as it allows for the formation of fine wiring. Examples of semi-additive processes include the following: First, after step 3, the via bottoms, via walls, and the entire surface of the pattern are subjected to electroless copper plating using a palladium catalyst or the like to form a seed layer. The seed layer serves to form a power supply layer for electrolytic copper plating, and the seed layer thickness is preferably 0.1 to 2.0 μm. A seed layer thickness of 0.1 μm or more tends to suppress a decrease in connection insulation reliability during electrolytic copper plating. A seed layer thickness of 2.0 μm or less tends to eliminate the need for a large etching amount when flash etching the seed layer between wirings, thereby suppressing damage to the wiring during etching. Electroless copper plating is performed by depositing metallic copper on the surface of a pattern having vias through a reaction between copper ions and a reducing agent. Examples of electroless plating methods and electrolytic plating methods include known plating methods. The catalyst used in the electroless plating process is preferably a palladium-tin mixed catalyst. The average primary particle size of the mixed catalyst is preferably 10 nm or less. The plating composition used in the electroless plating process preferably contains hypophosphorous acid as a reducing agent. Commercially available electroless copper plating solutions include, for example, "MSK-DK" manufactured by Atotech Japan and the "Sulcup (registered trademark) PEA ver. 4" series manufactured by Uemura Kogyo Co., Ltd.

[0150] After electroless copper plating, it is preferable to thermocompress the surface of the composition layer of the transfer film opposite the temporary support onto the electroless copper plating using a roll laminator. The thickness of the composition layer is preferably 5 to 30 μm, since it can be made thicker than the wiring height after electrolytic copper plating. After thermocompression bonding of the transfer film, the composition layer is exposed to light, for example, through a mask on which a desired wiring pattern is drawn. Examples of the exposure method include the exposure method in step 2. After exposure, the temporary support of the transfer film is peeled off, and the exposed composition layer is developed using an alkaline developer to form a pattern. After forming the pattern, development residues of the composition may be removed using plasma or the like. After development, electrolytic copper plating is performed to form a copper circuit layer and via filling. After electrolytic copper plating, the pattern is peeled off using an alkaline aqueous solution or an amine-based stripper. After peeling the pattern, the seed layer between the wiring is removed (flash etching). Flash etching is performed, for example, using an oxidizing solution containing sulfuric acid and an acidic solution such as hydrogen peroxide. Examples of oxidizing solutions include "SAC" manufactured by JCU Corporation and "CPE-800" manufactured by Mitsubishi Gas Chemical Co., Ltd. After flash etching, palladium and other materials adhering to the portions between the wirings are removed as necessary. Palladium can be removed using an acidic solution such as nitric acid and hydrochloric acid.

[0151] After the pattern is removed or after the flash etching step, a post-baking treatment is preferably performed. The post-baking treatment sufficiently cures any unreacted thermosetting components, thereby improving the electrical insulation reliability, curing characteristics, and adhesive strength with plated copper. The preferred thermosetting conditions are a curing temperature of 150 to 240°C and a curing time of 15 to 500 minutes.

[0152] The method for manufacturing a semiconductor package may include a roughening step of roughening a pattern having vias. The roughening step is preferably performed after step 3 and before step 4. By performing the roughening step, the surface of the pattern can be roughened to improve adhesion to the circuit wiring. Smears can also be removed at the same time. Examples of the roughening step include known desmearing treatments, and treatments involving contact with a roughening liquid are preferred. Examples of roughening liquids include a roughening liquid containing chromium and sulfuric acid, a roughening liquid containing an alkaline permanganate (e.g., a sodium permanganate roughening liquid, etc.), and a roughening liquid containing sodium fluoride, chromium, and sulfuric acid.

[0153] The above-described steps are repeated depending on the number of layers required to manufacture a semiconductor package. It is preferable to form a solder resist on the outermost layer.

[0154] [Semiconductor Package] The semiconductor package is not particularly limited as long as it includes an insulating layer formed from the composition, and is preferably manufactured by the above-mentioned semiconductor package manufacturing method. In the semiconductor package, the film formed from the composition may be used as an insulating film, or may be used as an organic interposer or insulating film in a so-called build-up substrate.

[0155] The present invention will be described in more detail below based on examples. The materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the examples shown below. In the following examples, "%" means "% by mass" unless otherwise specified.

[0156] [Preparation of Composition] Various components were mixed to prepare a mixture in the amounts (solid content ratio) shown in the table below. Methyl isobutyl ketone was then added to the mixture to dilute it to a solid content of 40% by mass. The various components contained in the composition are shown below.

[0157] [Polysilsesquioxane] Polysilsesquioxane A-1 was synthesized by the following method. Styrylmethoxysilane (0.15 mol), hexyltrimethoxysilane (0.15 mol), and 75.0 g of methyl isobutyl ketone were mixed in a 300 mL three-neck flask and stirred while heating at an external temperature of 80°C. 18.0 g of a 0.1% by mass aqueous potassium hydroxide solution was added dropwise at a constant rate over 5 minutes, and the mixture was heated and stirred for 5 hours. During heating, the reaction was carried out while refluxing methanol was removed from the system using a Dean-Stark apparatus. After stopping the stirring and cooling to room temperature (25°C) in a water bath, 150 g of methyl isobutyl ketone and 150 g of 5% by mass saline were added, and the organic phase was extracted. The organic phase was washed once with 150 g of 5% by mass saline and twice with 150 g of pure water, successively, and then dried over 45 g of magnesium sulfate. The mixture was then concentrated under reduced pressure at 50°C and 35 mmHg to obtain a methyl isobutyl ketone solution of polysilsesquioxane A-1. Polysilsesquioxane A-1 had an Mw of 43,700 and an Mn of 8,900, and contained a cage polysilsesquioxane. In addition, in GPC measurement, T 8 Polysilsesquioxane, T 10 Polysilsesquioxane, and T 12 When a peak corresponding to at least one molecular weight of the polysilsesquioxane was confirmed, it was determined that the polysilsesquioxane contained a cage polysilsesquioxane. GPC measurement was performed by the method described above. Polysilsesquioxanes other than polysilsesquioxane A-1 were synthesized by the same procedure except that the styrylmethoxysilane and hexyltrimethoxysilane were replaced with the following materials, and their molecular weights and structures were as follows:

[0158] A-2: Polysilsesquioxane synthesized using styrylmethoxysilane (0.15 mol) and decyltrimethoxysilane (0.15 mol). Mw was 17,600, Mn was 7,900, and it contained a cage polysilsesquioxane. A-3: Polysilsesquioxane synthesized using phenylmethoxysilane (0.15 mol) and hexyltrimethoxysilane (0.15 mol). Mw was 10,500, Mn was 4,400, and it contained a cage polysilsesquioxane. A-4: Polysilsesquioxane synthesized using hexyltrimethoxysilane (0.30 mol). Mw was 20,000, Mn was 4,000, and it contained a cage polysilsesquioxane. A-5: Acrylic resin with the following structure. The Mw was 27,000 and the Mn was 5,500. A-6: Polysilsesquioxane synthesized using decyltrimethoxysilane (0.30 mol). The Mw was 1,7000 and the Mn was 6,000, and it contained a cage polysilsesquioxane.

[0159]

[0160] [Compound X]

[0161]

[0162] [Polymerization initiators] Dicumyl peroxide: thermal polymerization initiator Oxe-01: photopolymerization initiator, Irgacure OXE-01, manufactured by BASF Api307: photopolymerization initiator, manufactured by Shenzhen UV-ChemTech Ltd.

[0163] [Surfactants] S-506: Silicone surfactant, manufactured by DIC Corporation F-551A: Megafac (registered trademark) F551A, fluorine-based surfactant, manufactured by DIC Corporation

[0164] [Other additives] A-NOD-N: polymerizable compound, 1,9-nonanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.

[0165] [Evaluation] Using the compositions obtained in each of the Examples and Comparative Examples, the linear expansion coefficient, adhesion, dielectric properties, and thermocycling resistance of the films formed from the compositions, as well as the suitability of the compositions for transfer films, were evaluated.

[0166] [Linear expansion coefficient] A copper-clad polyimide film (Metalloyal, manufactured by Toray Industries, Inc.) was used as a substrate, and the prepared composition was applied to the substrate and dried to obtain a laminate having a composition layer of 30.0 μm in thickness on the substrate. In Examples 59 and 60, before the heat treatment described below, the obtained laminate was exposed to light (high-pressure mercury lamp, cumulative illuminance of 100 mJ / cm measured with an illuminometer at a wavelength of 365 nm) from the side opposite to the substrate side of the composition layer. 2 ) was measured. Next, the laminate was heated in an oven (200°C, 1.5 hours), immersed in 2M hydrochloric acid for 8 hours for a peeling treatment, rinsed (in pure water at room temperature for 1 hour), and then peeled off from the substrate to obtain a free-standing film derived from the composition layer. If the free-standing film could not be peeled off by the above peeling treatment, it was further immersed in 2M hydrochloric acid for about 1 week for peeling. The obtained free-standing film was cut into strips (19 mm x 5 mm), and the linear expansion coefficient was measured using a TMA (thermomechanical analyzer, "TMA450EM" manufactured by TA Instruments). The measurement conditions were a heating rate of 10°C / min, a chuck distance of 10 mm, and a load of 40 mN. The linear expansion coefficient was measured as a value (ppm / K) in the temperature range of 50°C to 150°C during heating, and was calculated as the average of three measurements. The obtained linear expansion coefficient was evaluated according to the following evaluation criteria.

[0167] <Evaluation criteria> A: 30 ppm / K or less B: More than 30 ppm / K, 50 ppm / K or less C: More than 50 ppm / K

[0168] [Adhesion] A copper-clad polyimide film (Metalloyal, manufactured by Toray Industries, Inc.) was used as a substrate, and the prepared composition was applied to the substrate and dried to obtain a laminate having a composition layer of 10.0 μm in thickness on the substrate. In Examples 59 and 60, before the heat treatment described below, the obtained laminate was exposed to light (high-pressure mercury lamp, integrated illuminance of 100 mJ / cm measured with an illuminometer at a wavelength of 365 nm) from the side opposite to the substrate side of the composition layer. 2Next, the laminate was heated in an oven (200°C, 1.5 hours) to obtain an evaluation sample. The evaluation sample was subjected to a cross-cut test in accordance with JIS K5600-5-6, and the adhesion between the film formed from the composition and copper was evaluated according to the following evaluation criteria.

[0169] <Evaluation criteria> A: The area of ​​peeled areas is 35% or less of the cross-cut test range. B: The area of ​​peeled areas is more than 35% and less than 50% of the cross-cut test range. C: The area of ​​peeled areas is more than 50% of the cross-cut test range.

[0170] [Dielectric Properties] The freestanding films obtained in the same manner as in the [Linear Expansion Coefficient] above were measured for average dielectric loss tangent using a 28 GHz split cylinder resonator (manufactured by Kanto Electronics Application Development Co., Ltd.). Measurements were performed on three samples, and the average value was taken as the dielectric loss tangent. The dielectric properties were evaluated from the obtained dielectric loss tangent according to the following evaluation criteria.

[0171] <Evaluation criteria> A: Dielectric loss tangent is 0.01 or less B: Dielectric loss tangent is more than 0.01

[0172] [Thermocycling Resistance] A silicon wafer having a 5 μm thick copper pattern (line / space = 30 μm / 30 μm) formed in a comb-like pattern was used as the substrate, and a composition was applied to the substrate and dried to form a composition layer, thereby obtaining a laminate. The film thickness of the composition layer was adjusted so that the film thickness on the copper pattern was 20 μm. In Examples 59 and 60, before the heat treatment described below, the obtained laminate was exposed to light (high-pressure mercury lamp, cumulative illuminance of 100 mJ / cm2 measured with an illuminometer at a wavelength of 365 nm) from the side opposite to the substrate side of the composition layer. 2 ) was then subjected to a heat treatment in an oven (200°C, 1.5 hours) to obtain an evaluation sample. A thermocycle test was performed on the evaluation sample using a gas-phase thermal tester, in which the evaluation sample was left in a gas phase at a temperature of -40°C for 30 minutes and then in a gas phase at 180°C for 30 minutes, with this cycle being repeated 100 times. Thereafter, a 5 cm x 5 cm area of ​​the evaluation sample was observed, and the thermocycle resistance was evaluated according to the following evaluation criteria.

[0173] <Evaluation criteria> A: The number of cracks is 10 or less. B: The number of cracks is more than 10 and less than 20. C: The number of cracks is more than 20.

[0174] [Suitability for Transfer Films] The prepared composition was applied to a temporary support (QS62, manufactured by Toray Industries, Inc., 31 μm thick PET film) and dried at 100°C to form a composition layer. The film thickness of the composition layer was adjusted to 25 μm after drying. Next, a protective film (FG-201, polypropylene film manufactured by Oji F-Tex Co., Ltd., 30 μm thick) was attached to the side of the composition layer opposite the temporary support to obtain a transfer film. The protective film was peeled off from the resulting transfer film, and the film was laminated (rubber roller temperature 100°C, conveying speed 1 m / min, linear pressure 0.6 MPa) onto a copper-clad polyimide film (Metalloyal, manufactured by Toray Industries, Inc.) substrate. The temporary support was then peeled off from the substrate at an angle of 90° and a speed of 2 m / min, after which the composition layer was observed and the suitability for transfer films was evaluated according to the following criteria. The better the temporary support releasability, the more suitable it is for use as a transfer film, i.e., the better the suitability for transfer films.

[0175] <Evaluation Criteria> A: The area of ​​the composition layer remaining on the substrate is 60% or more of the area of ​​the peeled temporary support. B: The area of ​​the composition layer remaining on the substrate is less than 60% of the area of ​​the peeled temporary support.

[0176] [Results] The contents of various components in the compositions and the evaluation results are shown below. In the table, "amount" indicates the content (% by mass) relative to the total solid content of the composition.

[0177]

[0178]

[0179]

[0180] From the results shown in the above table, it was confirmed that the composition of the present invention can form a film that has a small linear expansion coefficient and excellent adhesion to metals.

[0181] Comparison of Example 62 with the other Examples confirmed that when the composition contained polysilsesquioxane having a polymerizable group, the heat resistance and thermocycling resistance were superior.

[0182] The transfer film of each example was laminated on both sides of a glass epoxy substrate (CCL-EL190T, thickness 1.0 mm, manufactured by Mitsubishi Gas Chemical Co., Ltd.) on which a circuit pattern had been formed, and composition layers were formed on both sides of the glass epoxy substrate. Lamination was performed using a vacuum laminator manufactured by MCK Corporation under conditions of a substrate temperature of 50°C, a rubber roller temperature of 100°C, a linear pressure of 3 N / cm, and a conveying speed of 2 m / min. A pattern having vias with a diameter of 80 μm was formed at predetermined positions on the composition layer and subjected to a heat treatment (200°C, 1.5 hours). Residues were then removed using an aqueous sodium permanganate solution as a roughening solution, and electroless plating was performed. Next, a resist pattern was formed at predetermined positions using a known dry film resist, and electrolytic plating was performed. The resist pattern was then stripped using a stripping solution. Finally, a seed layer etching treatment was performed, followed by a heat treatment (180°C, 1 hour) to form copper wiring on the insulating film formed from the composition. The above process from lamination to heat treatment was repeated three times. Finally, a solder resist was formed as the outermost layer, and a semiconductor element was sealed and mounted to produce a semiconductor package. The resulting semiconductor package was mounted in a predetermined position on a printed wiring board to obtain a semiconductor package substrate. The resulting semiconductor package substrate was confirmed to operate normally.

[0183] 12: Temporary support 14: Composition layer 16: Cover film 100: Transfer film

Claims

1. A composition containing a polysilsesquioxane, which satisfies at least one of Requirement 1 and Requirement 2. Requirement 1: The polysilsesquioxane has a functional group that interacts with a metal. Requirement 2: The composition further contains a compound X, which is a compound different from the polysilsesquioxane and has a functional group that interacts with a metal.

2. The composition according to claim 1, further comprising a polymerization initiator, and the polysilsesquioxane comprises a polysilsesquioxane having a polymerizable group.

3. The composition of claim 1, wherein the polysilsesquioxane comprises a cage-type polysilsesquioxane.

4. The composition according to claim 1, wherein the polysilsesquioxane has a linear hydrocarbon group.

5. The composition according to claim 1, wherein the weight average molecular weight of the polysilsesquioxane is from 5,000 to 50,000.

6. The composition according to claim 1, wherein the content of the polysilsesquioxane is 50 to 99 mass % based on the total solid content of the composition.

7. The composition according to claim 2, wherein the polymerization initiator is a radical polymerization initiator.

8. The composition according to claim 2, wherein the content of the polymerization initiator is 0.01 to 10% by mass based on the total solid content of the composition.

9. The composition according to claim 1, wherein the compound X is at least one selected from the group consisting of a compound represented by formula (1), a hydrolysate of a compound represented by formula (1), and a hydrolysis condensate of a compound represented by formula (1). Formula (1): Z-L-Si(X) 3 In formula (1), each X independently represents a hydroxy group or a hydrolyzable group, L represents a single bond or a divalent linking group, and Z represents a functional group that interacts with a metal.

10. The composition according to claim 1, wherein the content of said compound X is 0.01 to 10% by mass based on the total solid content of said composition.

11. A transfer film having a temporary support and a composition layer formed by using the composition according to any one of claims 1 to 10.

12. A semiconductor package having an insulating layer formed using the composition according to any one of claims 1 to 10.

13. A method for manufacturing a semiconductor package, comprising: step 1 forming a composition layer on a substrate using the composition according to any one of claims 1 to 10; step 2 forming a pattern including vias in the composition layer; and step 3 performing a curing treatment on the pattern.

Citation Information

Patent Citations

  • Negative type photoresist

    JP1987284352A

  • Curable composition for NANO inprint, cured product using the same, and member for liquid crystal display

    JP2010013513A

  • Curable composition for nano-imprint, cured product using the same, and member for liquid crystal display device

    JP2010013514A

  • Transfer film, and in-mold molded article

    JP2018192704A

  • Ultraviolet curable organopolysiloxane composition and use thereof

    WO2020090346A1

Cited By

  • Organopolysiloxane, composition, transfer film, cured product, semiconductor package, and method for producing semiconductor package

    WO2026172932A1

  • Organopolysiloxane, transfer film, cured product, semiconductor package, and method for producing semiconductor package

    WO2026172934A1