Active ray-curable composition and cured film
The actinic radiation-curable composition, with specific (meth)acrylates and inorganic fillers, addresses the lack of mechanical properties in existing compositions by forming a cured film with enhanced adhesiveness, refractive index, and stability, ensuring high transparency and resistance to yellowing.
Patent Information
- Application Number
- PCT/JP2024/017372
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-10
- Publication Date
- 2024-12-05
AI Technical Summary
Existing actinic radiation curable compositions for optical devices lack both mechanical properties like bending resistance and storage stability, despite achieving high refractive indices and transparency.
An actinic radiation-curable composition comprising (meth)acrylate with a hydroxy group, alkyl (meth)acrylate, a photopolymerization initiator, and an inorganic filler, with the inorganic filler content between 10-50% by mass and a viscosity of 5-200 mPa·s, using zirconium oxide or titanium oxide fillers with a refractive index of 1.9-3.0 and average particle size of 100 nm or less, and excluding sulfur-containing components.
The composition forms a cured film with improved adhesiveness, high refractive index, bending resistance, and storage stability, maintaining transparency and avoiding yellowing issues.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Actinic radiation curable composition and cured film
[0001] The present invention relates to an actinic radiation-curable composition and a cured film. In particular, the present invention relates to an actinic radiation-curable composition and a cured film using the same that have, as physical properties after film formation, adhesiveness, high transparency, and refractive index, as well as bending resistance and storage stability.
[0002] It is known that a high refractive index layer is used to improve the light extraction efficiency of optical devices such as liquid crystal displays and organic electroluminescence (organic EL) displays (hereinafter also referred to as "OLEDs"). Recently, techniques have been disclosed for improving the optical properties, such as high refractive index and high transparency, of each layer for foldable devices.
[0003] For example, Patent Document 1 discloses a technology relating to a curable composition containing high refractive index particles, a (meth)acrylate having two or more ethylenically unsaturated groups and having an alicyclic structure, an aromatic ring structure, or a combination thereof, and a polymerization initiator.
[0004] Patent Document 2 discloses a technology for applying a high refractive index acrylic formulation with embedded metal oxide nanocrystals of less than 10 nm to a high refractive index, highly transparent coating for various optical applications including OLED lighting.
[0005] U.S. Patent No. 5,999,629 discloses a formulation comprising metal oxide nanocrystals and a matrix comprising at least one monomer, oligomer, or polymer, which is used to produce high refractive index, high transparency nanocomposites for various optical applications, including OLED lighting and display applications.
[0006] On the other hand, in recent years, in addition to the optical properties, bending resistance and storage stability have also become important, and there is a demand for achieving both of these. However, although the techniques described in the above Patent Documents 1 to 3 mention inkjet suitability, optical properties, and refractive index, they do not mention the concept of mechanical properties such as adhesive function and bending resistance.
[0007] Japanese Patent Application Laid-Open No. 2017-61606 Special Publication No. 2019-507221 Special Publication No. 2022-507821
[0008] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide an actinic radiation-curable composition and a cured film that are adhesive, have high bending resistance and storage stability, and are capable of forming a cured film with a high refractive index, and the composition and the cured film.
[0009] The present inventors have investigated the causes of the above problems in order to solve them. As a result, an actinic radiation-curable composition contains a (meth)acrylate having a hydroxy group, an alkyl (meth)acrylate, a photopolymerization initiator, and an inorganic filler, and the content of the inorganic filler and the viscosity of the actinic radiation-curable composition before curing are set within specific ranges. The present inventors have found that such a configuration makes it possible to form a cured film that is adhesive, has high bending resistance and storage stability, and has a high refractive index. That is, the above problems of the present invention are solved by the following means.
[0010] 1. An actinic radiation-curable composition that is cured by actinic radiation, comprising a (meth)acrylate having a hydroxy group, an alkyl (meth)acrylate, a photopolymerization initiator, and an inorganic filler, wherein the content of the inorganic filler is within the range of 10 to 50 mass% based on the total amount of the actinic radiation-curable composition, and the viscosity of the actinic radiation-curable composition before curing is within the range of 5 to 200 mPa·s at 25°C.
[0011] 2. The actinic radiation-curable composition according to item 1, wherein the refractive index of the inorganic filler at a wavelength of 589 nm is in the range of 1.9 to 3.0.
[0012] 3. The actinic radiation-curable composition according to item 1, wherein the inorganic filler is either zirconium oxide or titanium oxide.
[0013] 4. The actinic radiation-curable composition according to item 1, wherein the inorganic filler has an average primary particle size of 100 nm or less.
[0014] 5. The actinic radiation-curable composition according to item 1, wherein the (meth)acrylate contained in the actinic radiation-curable composition as a whole does not contain sulfur element.
[0015] 6. The actinic radiation-curable composition according to item 1, containing the (meth)acrylate having a hydroxy group in an amount of 5 to 50% by mass, the alkyl (meth)acrylate in an amount of 5 to 50% by mass, and the photopolymerization initiator in an amount of 0.1 to 5% by mass, based on the total amount of the actinic radiation-curable composition.
[0016] 7. The actinic radiation-curable composition according to item 1, wherein the alkyl group of the alkyl (meth)acrylate has 8 to 24 carbon atoms.
[0017] 8. The actinic radiation-curable composition according to item 1, which is used in an ink-jet ink.
[0018] 9. A cured film which is a cured product of the actinic radiation-curable composition according to any one of items 1 to 8.
[0019] The above-described means of the present invention can provide an actinic radiation-curable composition and a cured film using the same, which exhibit adhesiveness, high transparency, and refractive index as physical properties after film formation, as well as bending resistance and storage stability. While the mechanism by which the effects of the present invention manifest or function is unclear, the following speculation is made. The actinic radiation-curable composition of the present invention contains a (meth)acrylate having a hydroxy group, an alkyl (meth)acrylate, and a photopolymerization initiator. It has been known that alkyl (meth)acrylates can become adhesive by polymerization alone. However, in the present invention, the addition of a (meth)acrylate having a hydroxy group as a comonomer more stably maintains the wet state, which is a property of adhesives, after polymerization. This is thought to improve adhesive properties by making it easier to fill irregularities on the surface of the adherend. It has also been known that the addition of an inorganic filler increases the refractive index. A low inorganic filler content may not achieve a sufficient effect of increasing the refractive index, while a high inorganic filler content may achieve a high refractive index. However, the rigidity of the inorganic filler, which has properties opposite to adhesiveness, results in a loss of adhesiveness. Therefore, in the present invention, by setting an appropriate amount of inorganic filler, the surface state of the inorganic filler, such as its charge and hydrophilicity, can be maintained in a consistent dispersed state even after the actinic radiation-curable composition is cured. As a result, the present invention is believed to be able to improve the average refractive index of the entire material while maintaining adhesiveness and high transparency. Generally, yellowing during storage is accelerated by the addition of moisture and temperature. In the present invention, it is believed that yellowing is caused by the formation of sulfur oxides formed by the oxidation of sulfur, or chromophores formed by some reaction between sulfur oxides and the actinic radiation-curable composition or between sulfur oxides and the adherend. Therefore, in the present invention, by configuring the actinic radiation-curable composition to be sulfur-free, it is believed that excellent storage stability can be achieved. As described above, the actinic radiation-curable composition of the present invention contains the (meth)acrylate having a hydroxy group and the (meth)acrylate alkyl ester, and thereby exhibits adhesiveness in the cured product cured by actinic radiation. Furthermore, mechanical strength can be achieved by the inorganic filler while exhibiting adhesiveness.Furthermore, it is believed that the balance between adhesiveness and mechanical strength can be achieved, thereby achieving bending resistance.
[0020] Schematic diagram showing an exemplary configuration of a cured film manufacturing apparatus according to one embodiment of the present invention. Schematic diagram showing an exemplary configuration of a cured film manufacturing apparatus according to one embodiment of the present invention. Schematic diagram showing an exemplary configuration of a cured film manufacturing apparatus according to one embodiment of the present invention.
[0021] The actinic radiation-curable composition of the present invention is an actinic radiation-curable composition that is cured by actinic radiation, and contains a (meth)acrylate having a hydroxy group, an alkyl (meth)acrylate, a photopolymerization initiator, and an inorganic filler, the content of the inorganic filler being 10 to 50 mass % based on the total amount of the actinic radiation-curable composition, and the viscosity of the actinic radiation-curable composition before curing is within the range of 5 to 200 mPa s at 25° C. This feature is a technical feature common to or corresponding to each of the following embodiments.
[0022] In an embodiment of the present invention, the refractive index of the inorganic filler at a wavelength of 589 nm is preferably in the range of 1.9 to 3.0. When the refractive index of the inorganic filler is in the range of 1.9 to 3.0, the effect of increasing the refractive index is high even if the content of the inorganic filler is small.
[0023] It is preferable that the inorganic filler contains at least one of zirconium oxide and titanium oxide in order to achieve a high refractive index.
[0024] It is preferable that the inorganic filler has an average primary particle size of 100 nm or less in terms of high transparency.
[0025] It is preferable that the (meth)acrylate contained in the entire actinic radiation curable composition does not contain sulfur element in terms of excellent storage stability.
[0026] It is more preferable that the actinic radiation-curable composition contains the (meth)acrylate having a hydroxy group in an amount of 5 to 50 mass %, the alkyl (meth)acrylate in an amount of 5 to 50 mass %, and the photopolymerization initiator in an amount of 0.1 to 5 mass %, based on the entire actinic radiation-curable composition, in terms of adhesiveness, a high refractive index, bending resistance, and storage stability.
[0027] In terms of ensuring higher transparency in the configuration of the present invention, it is preferable that the alkyl group of the alkyl (meth)acrylate has 8 to 24 carbon atoms. The actinic radiation-curable composition of the present invention is suitably used for inkjet inks.
[0028] The cured film of the present invention is characterized by being obtained by curing the actinic radiation-curable composition with actinic radiation, thereby forming a cured film that has adhesiveness, high bending resistance, high storage stability, and a high refractive index.
[0029] The present invention, its components, and embodiments and modes for carrying out the present invention will be described below. In this application, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0030] [Outline of Actinic Ray-Curable Composition of the Present Invention] The actinic ray-curable composition of the present invention is an actinic ray-curable composition that is cured by actinic rays, and contains a (meth)acrylate having a hydroxy group, an alkyl (meth)acrylate, a photopolymerization initiator, and an inorganic filler, the content of the inorganic filler being 10 to 50 mass % based on the total amount of the actinic ray-curable composition, and the viscosity of the actinic ray-curable composition before curing is within the range of 5 to 200 mPa s at 25°C.
[0031] In the present invention, "(meth)acrylate" means acrylate or methacrylate, "(meth)acryloyl group" means acryloyl group or methacryloyl group, and "(meth)acrylic" means acrylic or methacrylic.
[0032] The actinic radiation-curable composition of the present invention is a composition that can be cured by actinic radiation. "Actinic radiation" refers to radiation that can impart energy to generate initiating species in the curable composition upon irradiation, and includes α-rays, γ-rays, X-rays, ultraviolet rays, electron beams, etc. Among these, ultraviolet rays and electron beams are preferred from the viewpoints of curing sensitivity and ease of equipment availability, and ultraviolet rays are more preferred.
[0033] <Viscosity> The viscosity of the actinic radiation-curable composition before curing is in the range of 5 to 200 mPa·s at 25°C. In the present invention, the "viscosity of the actinic radiation-curable composition before curing" refers to the viscosity obtained by measuring the actinic radiation-curable composition before curing with actinic radiation under the following conditions. The viscosity was measured using a rheometer MCR302 (manufactured by Anton Paar Japan KK) and a cone plate CP75-1 (manufactured by Anton Paar Japan KK) with a diameter of 75 mm and an angle of 1° at 25°C at a shear rate of 1000 (S -1 )
[0034] The viscosity of the actinic radiation-curable composition before curing is preferably within the range of 5 to 200 mPa·s, particularly preferably within the range of 10 to 100 mPa·s, at 25° C. In order to make the viscosity of the actinic radiation-curable composition before curing within the above range, the total content of the (meth)acrylate having a hydroxy group, the alkyl (meth)acrylate, and the other acrylate may be set within the range of 50 to 90% by mass based on the total amount of the actinic radiation-curable composition.
[0035] [Constitution of actinic radiation-curable composition] The actinic radiation-curable composition of the present invention contains a (meth)acrylate having a hydroxy group, a (meth)acrylate alkyl ester, a photopolymerization initiator, and an inorganic filler. Hereinafter, the (meth)acrylate having a hydroxy group, the (meth)acrylate alkyl ester, the photopolymerization initiator, the inorganic filler, etc. will be described.
[0036] <(Meth)acrylate Having a Hydroxy Group> Examples of the (meth)acrylate having a hydroxy group according to the present invention include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-chloropropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, ethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, propylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, cyclohexyldimethanol mono(meth)acrylate, and caprolactone acrylate. These (meth)acrylates may be used alone or in combination of two or more. In the present invention, it is particularly preferable to use 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate as the (meth)acrylate having a hydroxy group.
[0037] <Alkyl (meth)acrylate> Examples of alkyl (meth)acrylates according to the present invention include linear alkyl (meth)acrylates such as n-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; isobutyl (meth)acrylate; s-butyl (meth)acrylate; Examples of the (meth)acrylate include branched (meth)acrylates such as (meth)acrylate, t-butyl (meth)acrylate, isoamyl (meth)acrylate, ethylhexyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, and isostearyl (meth)acrylate, and cyclic (meth)acrylates such as isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate. These (meth)acrylates may be used alone or in combination of two or more.
[0038] The number of carbon atoms in the alkyl group of the alkyl (meth)acrylate is preferably 8 to 24. As the alkyl (meth)acrylate, it is particularly preferable to use a straight-chain type such as octyl (meth)acrylate (number of carbon atoms: 8) or behenyl (meth)acrylate (number of carbon atoms: 22), or a branched type such as isostearyl (meth)acrylate (number of carbon atoms: 18), but the alkyl (meth)acrylate is not limited thereto.
[0039] In terms of excellent storage stability, it is preferable that the (meth)acrylates contained in the entire actinic radiation-curable composition of the present invention do not contain sulfur element. Specifically, it is preferable that the (meth)acrylate having a hydroxy group and the alkyl (meth)acrylate do not contain sulfur element. It is also preferable that (meth)acrylates other than the (meth)acrylate having a hydroxy group and the alkyl (meth)acrylate do not contain sulfur.
[0040] The content of the hydroxyl group-containing (meth)acrylate is preferably within a range of 5 to 50 mass % based on the total amount of the actinic radiation-curable composition, from the viewpoints of adhesiveness, a high refractive index, bending resistance, and storage stability. The content of the alkyl (meth)acrylate is preferably within a range of 5 to 50 mass % based on the total amount of the actinic radiation-curable composition, from the viewpoints of adhesiveness, a high refractive index, bending resistance, and storage stability.
[0041] <Photopolymerization initiator> The photopolymerization initiator is a radically polymerizable photopolymerization initiator. The photopolymerization initiator may be an intramolecular bond cleavage type radical polymerization initiator or an intramolecular hydrogen abstraction type radical polymerization initiator. Of these, an intramolecular bond cleavage type radical polymerization initiator is less likely to initiate polymerization initiated from the hydroxy group of a hydroxy group-containing (meth)acrylate compared to an intramolecular hydrogen abstraction type radical polymerization initiator. Therefore, an intramolecular bond cleavage type radical polymerization initiator makes it more difficult to form a crosslinked structure due to polymerization initiated from the hydroxy group, making the cured film more flexible and more sufficiently improving the durability of the cured film when bent.
[0042] Examples of the intramolecular bond cleavage type radical polymerization initiator include acetophenone-based initiators such as diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl-phenyl ketone, 2-methyl-2-morpholino(4-methylthiophenyl)propan-1-one, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone; benzoins such as benzoin methyl ether and benzoin isopropyl ether; acylphosphine oxide-based initiators such as 2,4,6-trimethylbenzoindiphenylphosphine oxide; and benzyl and methylphenyl glyoxyesters.
[0043] Among these intramolecular bond cleavage type radical polymerization initiators, acylphosphine oxide-based polymerization initiators are preferred because they have sufficient curability (polymerization initiation ability) even when a UV-LED light source is used in order to reduce damage to the substrate. The intramolecular bond cleavage type radical polymerization initiators may be used alone or in combination of two or more.
[0044] Examples of the intramolecular hydrogen abstraction type radical polymerization initiator include benzophenone-based initiators such as benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, acrylated benzophenone, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthone-based initiators such as 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone; aminobenzophenone-based initiators such as Michler's ketone and 4,4'-diethylaminobenzophenone; 10-butyl-2-chloroacridone, 2-ethylanthraquinone, 9,10-phenanthrenequinone, and camphorquinone. The intramolecular hydrogen abstraction type radical polymerization initiators may be used alone or in combination of two or more.
[0045] The content of the polymerization initiator may be within a range that allows the actinic radiation-curable composition to be sufficiently cured, and is preferably within a range of 0.01 to 10 mass % relative to the total mass of the actinic radiation-curable composition. The content of the polymerization initiator is preferably within a range of 0.1 to 5 mass % relative to the total mass of the actinic radiation-curable composition.
[0046] <Inorganic Filler> Examples of inorganic fillers according to the present invention include silicon monoxide (nano SiO silicon monoxide powder: Xinglu Chemicals), zirconium oxide (Zirconeo-Cp, Zirconeo-Rp: ITEC Corporation, Zircostar ZP-153, Zircostar HR-101: Nippon Shokubai Co., Ltd.), titanium oxide (AMT-100, AMT-600, TKP-101, TKP-102: Teika Corporation, ultrafine particle titanium oxide TTO series: Ishihara Sangyo Kaisha, Ltd.), tantalum pentoxide (Hongwu International Group Co., Ltd.), and the like. Ltd.), niobium pentoxide (Bailar series: Nb-G6000, Nb-G6100, Nb-G6600: Taki Chemical Co., Ltd.), cerium oxide (ITEC Co., Ltd.), silicon (Si nanoparticles: Nissin Chemical Co., Ltd.), and germanium (Hongwu International Group Ltd.). These inorganic fillers may be used alone or in combination of two or more. They may also contain multiple metal oxides within a single particle, such as a core-shell type. In the present invention, the inorganic filler preferably contains one or more of silicon monoxide, zirconium oxide, titanium oxide, tantalum pentoxide, niobium pentoxide, cerium oxide, silicon elemental, and germanium elemental. It is particularly preferable that the inorganic filler contains one or more of zirconium oxide and titanium oxide.
[0047] The refractive index of the inorganic filler at a wavelength of 589 nm is preferably in the range of 1.9 to 3.0, since a high refractive index can be achieved even with a small inorganic filler content. The refractive index of the inorganic filler is measured by the following method. A thin film of inorganic filler having a thickness of 1 μm or less is formed on a substrate such as glass or a silicon wafer by a sputtering method or the like. Then, the refractive index is measured using, for example, a spectroscopic ellipsometer M-2000 (J.A. Woollam Japan Co., Ltd.).
[0048] The average primary particle size of the inorganic filler is preferably 100 nm or less in order to ensure optical transparency, and more preferably within the range of 1 to 50 nm. The average primary particle size of the inorganic filler was measured as follows: A liquid sample before curing was introduced into a glass cell (manufactured by Malvern Panalytical) using a ZetaSizer Nano ZS (manufactured by Malvern Panalytical) that uses dynamic light scattering as its measurement principle, and the Z-average value was taken as the average primary particle size.
[0049] The inorganic filler according to the present invention is contained in a range of 10 to 50% by mass relative to the total amount of the actinic radiation-curable composition (total amount of acrylic monomer and inorganic filler). If the content of the inorganic filler is less than 10% by mass, its contribution to increasing the refractive index will be minimal. On the other hand, if the content of the inorganic filler is 50% by mass or less, adhesiveness can be maintained. The content of the inorganic filler is preferably in a range of 20 to 50% by mass, more preferably in a range of 25 to 50% by mass.
[0050] <Other Acrylates> The actinic radiation curable composition of the present invention may contain an aromatic ring-containing monomer, a polyfunctional monomer, a crosslinking agent, or the like for improving the refractive index, elastic modulus, or adhesiveness.
[0051] The aromatic ring-containing monomer may be any compound having an aromatic ring and one ethylenically unsaturated group in the molecule. Examples of the functional group containing such an ethylenically unsaturated group include a (meth)acryloyl group, a crotonoyl group, a vinyl group, and an allyl group. Among these, a (meth)acryloyl group is preferred because of its excellent reactivity.
[0052] Examples of such aromatic rings include a benzene ring, a naphthalene ring, an anthracene ring, a biphenyl ring, and a fluorene ring. The number of aromatic rings may be one or more. However, in terms of balancing the adhesive properties, a compound containing one aromatic ring is preferred, and in terms of efficiently controlling the refractive index and birefringence of the adhesive layer, a compound containing two aromatic rings is preferred.
[0053] Examples of the aromatic ring-containing monomer include benzyl (meth)acrylate, benzyloxyethyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, ethylene oxide-modified cresol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, biphenyloxyethyl (meth)acrylate, styrene, etc., and among these, benzyl (meth)acrylate and phenoxyethyl (meth)acrylate are preferred. These may be used alone or in combination of two or more.
[0054] The polyfunctional monomer may be any compound having two or more (meth)acrylic groups in the molecule. Polyfunctional (meth)acrylates can appropriately increase the hardness of the cured film. Examples of polyfunctional (meth)acrylates include triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, bisphenol A PO adduct di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, polytetramethylene glycol ... Examples of the acrylates include difunctional (meth)acrylates such as polyethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate, trifunctional (meth)acrylates such as trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate, trifunctional or higher (meth)acrylates such as pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerin propoxy tri(meth)acrylate, and pentaerythritol ethoxy tetra(meth)acrylate, and modified products thereof. Examples of the modified products include ethylene oxide-modified (EO-modified) (meth)acrylates having an ethylene oxide group inserted therein, and propylene oxide-modified (PO-modified) (meth)acrylates having propylene oxide inserted therein. These may be used alone or in combination of two or more.
[0055] <Other Components> The actinic radiation-curable composition of the present invention may contain the following components within the range that does not impair the effects of the present invention. Examples of such components include antistatic agents, other acrylic adhesives, and other adhesives. Examples of such components include tackifiers such as urethane resins, rosin, rosin esters, hydrogenated rosin esters, phenolic resins, aromatic-modified terpene resins, aliphatic petroleum resins, alicyclic petroleum resins, styrene-based resins, and xylene-based resins. Examples of such components include various additives such as colorants, fillers, antioxidants, UV absorbers, and functional dyes, as well as compounds that develop or change color upon exposure to UV or radiation. In addition to the above additives, the composition may contain small amounts of impurities contained in the raw materials used to produce the components of the actinic radiation-curable composition. The amounts of these additives added may be appropriately determined so as to achieve desired physical properties.
[0056] <Uses> The actinic radiation-curable composition of the present invention can be used as a so-called inkjet ink that can be discharged from an inkjet head, for forming a cured film in various applications that use a cured film formed by an inkjet method.
[0057] The actinic radiation-curable composition of the present invention is suitable for use in transparent layers of image display devices because the cured film has high adhesion and sufficiently high transparency. In particular, it is used to form transparent layers for bonding various components of the image display device. Examples of the transparent layer include transparent layers for bonding a transparent electrode formed on a substrate to a transparent protective layer made of glass or resin, transparent layers for bonding various panels such as liquid crystal display panels, organic EL display panels, and touch panels to transparent protective layers, transparent layers for bonding display panels such as liquid crystal display panels and organic EL display panels to touch panels, and transparent layers for bonding various other components.
[0058] [Cured Film] The cured film of the present invention is characterized by being obtained by curing the actinic radiation-curable composition of the present invention described above with actinic radiation.
[0059] <Physical Properties> The refractive index of the cured film of the present invention at 25°C and a wavelength of 589 nm is preferably 1.5 or more, and more preferably 1.55 or more. The refractive index can be measured as follows. First, an actinic radiation-curable composition is set on the prism of an Abbe refractometer (NAR-1T SOLID: manufactured by Atago Co., Ltd.). Next, an ultraviolet irradiation device (manufactured by Phoseon) is used to irradiate the cured film with ultraviolet light having a wavelength of 395 nm at an intensity of 2000 mW / cm. 2 , cumulative light intensity 1000 mJ / cm 2 The refractive index (nD) of the cured film can be measured at 25° C. and a wavelength of 589 nm by irradiating the film with light at this temperature.
[0060] The total light transmittance of the cured film of the present invention is preferably 80% or more, more preferably 90% or more, and particularly preferably 95% or more. The total light transmittance can be measured as follows. An actinic radiation curable composition is applied to a quartz substrate (manufactured by Matsunami Glass Co., Ltd.) measuring 50 mm x 50 mm x 1 mm thick to a film thickness of 50 μm. After sandwiching the composition between similar quartz substrates, an ultraviolet irradiation device (manufactured by Phoseon) is used to irradiate the composition with ultraviolet light having a wavelength of 395 nm at an intensity of 2000 mW / cm. 2 , cumulative light intensity 1000 mJ / cm 2 The total light transmittance of the resulting cured film is measured using a haze meter NDH-5000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7361-1.
[0061] [Method for forming cured film] The cured film of the present invention is obtained by applying the actinic ray-curable composition to a substrate or one of the members to be bonded, and curing the actinic ray-curable composition by irradiating it with actinic rays.
[0062] The method for applying the actinic radiation-curable composition is not particularly limited, and known methods such as spray coating, dipping, screen printing, gravure printing, offset printing, and inkjet printing can be used. The above-mentioned application methods may be used alone or in combination of two or more. Among these, the inkjet method is preferred from the viewpoint of accurately forming a fine cured film to form a high-definition pattern (image, etc.) or applying the composition to a curved portion.
[0063] The actinic radiation-curable composition may be applied to various substrates, or when two members are bonded together, it may be applied to one of the members to be bonded. The material of the substrate or member to which the actinic radiation-curable composition is applied is not particularly limited, and may be an inorganic material such as glass, metal, or ceramic, or an organic material such as a resin film. The actinic radiation-curable composition can adhere well to any of these materials, regardless of their types.
[0064] At this time, the applied actinic ray-curable composition may be temporarily cured by irradiating it with actinic rays to an extent that does not completely cure it.
[0065] When forming a transparent layer for bonding two different members, the other member is bonded to the applied (or provisionally cured) actinic radiation-curable composition, at least one of the two members to be bonded being a member that transmits actinic radiation.
[0066] Examples of the member that transmits actinic rays include members formed from materials such as glass, (meth)acrylic resin, polyethylene terephthalate resin, polyethylene naphthalate resin, polycarbonate resin, polyimide resin, cycloolefin polymer, etc. Members formed from these materials may have a transparent functional member such as a transparent electrode formed thereon.
[0067] Examples of members that are opaque to actinic rays include liquid crystal display panels, organic EL display panels, protective panels, touch panels, organic EL elements, and members on which color filters and the like are formed.
[0068] After lamination, these members may be pressed appropriately to ensure close contact or to make the thickness of the actinic radiation-curable composition uniform.
[0069] The actinic radiation-curable composition is then irradiated with actinic radiation to cure (or main cure) the composition, thereby obtaining a cured film. The actinic radiation may be any actinic radiation such as electron beams, ultraviolet radiation, α-rays, γ-rays, or X-rays, but from the viewpoint of suppressing damage to other components, ultraviolet radiation is more preferable. Furthermore, from the viewpoint of suppressing damage to other components due to radiant heat, ultraviolet radiation emitted from a light-emitting diode (UV-LED) that emits ultraviolet radiation is more preferable.
[0070] The cured film formed from the actinic radiation-curable composition of the present invention in this manner has high adhesiveness and maintains good adhesiveness even in high-temperature, high-humidity environments and low-temperature environments. Therefore, when used to bond two components, these components are less likely to separate, especially during long-term use. Furthermore, the adhesiveness of the cured film is less likely to decrease even when repeatedly folded. Therefore, even when used in flexible displays, the components are less likely to separate, especially during long-term use. Therefore, devices having the cured film, such as image display devices having the cured film, can be used for long periods of time.
[0071] [Apparatus for Producing Cured Film] FIGS. 1A to 1C are schematic diagrams showing the configuration of an apparatus for producing a cured film for carrying out the above-described method for producing a cured film.
[0072] The cured film manufacturing apparatus 100 has an application section 120 that applies the above-mentioned actinic radiation-curable composition to the surface of one of the members 110, and an irradiation section 130 that irradiates the surface of the one of the members 110 to which the actinic radiation-curable composition has been applied with actinic radiation.
[0073] In this embodiment, the application unit 120 applies the actinic radiation-curable composition by an inkjet method. The application unit 120 ejects the actinic radiation-curable composition from a nozzle 121 and applies the actinic radiation-curable composition 122 to the surface of one member 110 at a position where a cured film is to be formed (see FIG. 1A ).
[0074] Thereafter, the laminating unit may apply the other member 150 to the surface of the applied actinic radiation curable composition 122, thereby laminating the one member 110 and the other member 150. In this embodiment, the laminating unit feeds the other member 150, which is a transparent film, using a feed roller 142 and applies it to the surface of the actinic radiation curable composition. Then, pressure is applied by a pressure roller 144 to bring the one member 110 and the other member 150 into close contact with each other (see FIG. 1B ).
[0075] In addition, when one member 110 is a member that transmits actinic rays and the other member 150 is a member that does not transmit actinic rays, the manufacturing apparatus 100 may have an inversion unit that inverts them.
[0076] The irradiation unit 130 irradiates the surface of the one member 110 on which the actinic ray curable composition 122 is applied with actinic rays. In this way, the irradiation unit 130 cures the actinic ray curable composition 122 applied to the surface of the one member 110 to form a cured film. In this embodiment, the irradiation unit 130 irradiates the actinic ray curable composition 122 with actinic rays that have passed through the other member 150 (see FIG. 1C ).
[0077] In the above description, the actinic ray-curable composition is applied to the surface of one of the members 110 by an inkjet method. However, the method for applying the actinic ray-curable composition is not particularly limited, and any known method such as a spray coating method, a dipping method, a screen printing method, a gravure printing method, or an offset printing method can be used.
[0078] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, operations were carried out at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0079] [Preparation of Actinic Radiation Curable Composition 4] The materials shown below were added and heated at 90°C for 1 hour to prepare Actinic Radiation Curable Composition 1. Alkyl (meth)acrylate: octyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd., linear structure, carbon number 4) 9 parts by mass (meth)acrylate having a hydroxy group: 4-hydroxybutyl acrylate (manufactured by Osaka Organic Chemical Industry Ltd.) 9 parts by mass Inorganic filler: DZM-003 (ZrO 2 Contains 60 mass% of ZrO 2 Primary particle size of: 10 nm, manufactured by Daiken Chemical Co., Ltd.) 79 parts by mass Polymerization inhibitor: bis(2,2,6,6-tetramethyl-4-piperidyl-1-oxyl) sebacate (manufactured by Tokyo Chemical Industry Co., Ltd.) 0.02 parts by mass Photopolymerization initiator: bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resin) 3 parts by mass Note that ZrO contained in the DZM-003 at 60% by mass 2 is contained in the actinic radiation-curable composition in an amount of 79 parts by mass×0.6=47.4 parts by mass based on the total amount of the actinic radiation-curable composition.
[0080] [Preparation of Actinic Radiation Curable Compositions 2 to 23] Each actinic radiation curable composition was prepared in the same manner as in the preparation of Actinic Radiation Curable Composition 4, except that the types and contents of the alkyl (meth)acrylate, (meth)acrylate having a hydroxy group, inorganic filler, polymerization inhibitor, and photopolymerization initiator were changed as shown in the table below. The compounds shown in the table below are as follows: Octyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd., linear structure, 8 carbon atoms) Isostearyl acrylate (manufactured by Osaka Organic Chemical Industry Ltd., branched structure, 18 carbon atoms) Behenyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd., linear structure, 22 carbon atoms) 2-Hydroxyethyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) Caprolactone acrylate (manufactured by Miwon Specialty Chemical Co., Ltd.) 9869 ZR (ZrO2 Contains 20% by mass, ZrO 2 Primary particle size: 63 nm, manufactured by Tokushiki Co., Ltd.) NS483 (TiO 2 Contains 20% by mass, TiO 2 Primary particle size: 6.8 nm, manufactured by Teika Corporation)
[0081] The sulfur-containing acrylate (compound 1) used in the preparation of actinic radiation-curable composition 16 was synthesized as follows.
[0082] <Synthesis of Compound 1> The following materials were added to a 300 ml three-necked round-bottom flask: 47.5 g of 2-(octylthio)ethanol (manufactured by Fluorochem Ltd.), 29.7 g of triethylamine (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.01 g of salicylaldoxime (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.01 g of 2,3,5,6-tetramethyl-1,4-phenylenediamine (manufactured by Tokyo Chemical Industry Co., Ltd.), and 430 g of t-butyl methyl ether (manufactured by Tokyo Chemical Industry Co., Ltd.). The flask containing the mixture was heated to 40°C in a water bath, and 24.4 g of acryloyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise to the reaction mixture. The reaction was maintained at 40°C for 1 hour to complete the reaction, and then cooled to room temperature. 400 g of water was added to the flask. Further, 5 g of hydrochloric acid (35-37%, manufactured by Kanto Chemical Co., Inc.) was added and thoroughly stirred, after which the aqueous phase was separated. The organic phase was washed with a mixture of 300 g of water and 30 g of sodium carbonate (manufactured by Tokyo Chemical Industry Co., Ltd.), and then with a mixture of 300 g of water and 30 g of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd.). The solvent was removed using a rotary evaporator to obtain 45 g of a pale yellow liquid sulfur-containing acrylate (Compound 1).
[0083]
[0084] <Viscosity> The viscosity of each actinic radiation-curable composition prepared was measured as follows: The viscosity was measured at 25°C at a shear rate of 1000 (S) using a rheometer MCR302 (manufactured by Anton Paar Japan K.K.) and a cone plate CP75-1 (manufactured by Anton Paar Japan K.K.) with a diameter of 75 mm and an angle of 1°. -1 The viscosity of the actinic radiation-curable composition was measured at each of the temperatures. The measurement results are shown in the table below.
[0085] <Refractive Index> The refractive index of the cured film of each actinic radiation-curable composition prepared was measured as follows: The actinic radiation-curable composition was set on the prism of an Abbe refractometer (NAR-1T SOLID, manufactured by Atago Co., Ltd.). An ultraviolet irradiation device (manufactured by Phoseon) was used to irradiate ultraviolet light with a wavelength of 395 nm at an intensity of 2000 mW / cm. 2 , cumulative light intensity 1000 mJ / cm 2 After irradiation at 25°C, the refractive index (nD) of the cured film was measured at a wavelength of 589 nm. The refractive index obtained was evaluated on a three-level scale of AA, A, and B. "AA" and "A" were deemed acceptable for practical use. (Criteria) AA: (nD) ≥ 1.55 A: 1.50 ≤ (nD) < 1.55 B: (nD) < 1.50
[0086] <Adhesive Strength> In this specification, adhesive strength refers to adhesive strength to a glass plate, and was measured as follows. An inkjet head (KM1024iLHE-30, manufactured by Konica Minolta, Inc.) was attached to an inkjet image forming apparatus (manufactured by Tritec Corporation). Each actinic radiation-curable composition was applied to a 75 μm-thick PET film Lumirror T60 (manufactured by Toray Industries, Inc.) at a resolution of 360 dpi x 360 dpi to a film thickness of 50 μm. Thereafter, ultraviolet light having a wavelength of 395 nm was applied at an intensity of 2000 mW / cm using an ultraviolet irradiation device (manufactured by Phoseon). 2 , cumulative light intensity 1000 mJ / cm 2A cured film was formed by irradiating the film with light at a rate of 1000 nm. The obtained PET film with the cured film was sampled to a size of 25 mm x 100 mm, attached to the surface of a clean soda glass plate (manufactured by Matsunami Glass Co., Ltd.), and pressed twice with a 2 kg pressure roller. After 24 hours at room temperature, the film was peeled at a tensile speed of 300 mm / min according to the 180-degree peel test method specified in JIS-Z-0237, and the adhesive strength (N / 25 mm) was measured using a peel tester VPA-H200 (manufactured by Kyowa Interface Science Co., Ltd.). The obtained adhesive strength was evaluated on a four-level scale: AAA, AA, A, and B. "AAA," "AA," and "A" were considered acceptable for practical use. (Standards) AAA: (Adhesive force) ≧ 30 [N / 25 mm] AA: 20 [N / 25 mm] ≦ (Adhesive force) < 30 [N / 25 mm] A: 10 [N / 25 mm] ≦ (Adhesive force) < 20 [N / 25 mm] B: (Adhesive force) < 10 [N / 25 mm]
[0087] <Transmittance> The transmittance of the cured film was evaluated as follows. Each actinic radiation-curable composition was applied to a quartz substrate (manufactured by Matsunami Glass Co., Ltd.) measuring 50 mm x 50 mm x 1 mm thick, using the same method as in the measurement method for <Adhesive Strength> above, to a film thickness of 50 μm. After sandwiching the composition between the same quartz substrates, an ultraviolet irradiation device (manufactured by Phoseon) was used to irradiate the composition with ultraviolet light having a wavelength of 395 nm at an intensity of 2000 mW / cm. 2 , cumulative light intensity 1000 mJ / cm 2 A cured film was formed by irradiating the sample with light at a rate of 1000 W at a temperature of 100° C. The total light transmittance of the cured film was measured using a haze meter NDH-5000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7361-1. The total light transmittance was evaluated using a four-level scale of AAA, AA, AA, and B. "AAA", "AA", and "A" were deemed acceptable for practical use. (Criteria) AAA: (total light transmittance) ≧ 95% AA: 90% ≦ (total light transmittance) < 95% A: 80% ≦ (total light transmittance) < 90% B: (total light transmittance) < 80%
[0088] <Storage Stability> Storage stability was evaluated as follows. Each actinic radiation-curable composition was applied to a 75 μm-thick PET film Lumirror X10S (manufactured by Toray Industries, Inc.) in the same manner as in <Adhesive Strength> above, so that the film thickness was 50 μm. After sandwiching the composition between similar PET films, an ultraviolet irradiation device (manufactured by Phoseon) was used to irradiate the composition with ultraviolet light having a wavelength of 395 nm at an intensity of 2000 mW / cm. 2 , cumulative light intensity 1000 mJ / cm 2 The sample was irradiated at a temperature of 100°C to form a cured film sandwiched between PET films on both sides. The sample with the cured film formed was left in an environmental test chamber (manufactured by Espec Corporation) at 85°C and 85% RH for 1000 hours. The change in color was calculated using the color evaluation program on a UV-Vis-Near-Infrared Spectrophotometer V-780 (manufactured by JASCO Corporation). The yellowness index ΔYI (= YI2 - YI1) was calculated from the yellowness index YI1 immediately after the formation of the cured film and the yellowness index YI2 after the film was left in the environmental test chamber. The obtained yellowness index was evaluated on a four-level scale of AAA, AA, A, and B. "AAA", "AA", and "A" were considered acceptable for practical use. (Criteria) AAA: ΔYI<1.0 AA: 1.0≦ΔYI<3.0 A: 3.0≦ΔYI<5.0 B: 5.0≦ΔYI
[0089] <Bending Resistance> The bending resistance was evaluated as follows. Each actinic radiation-curable composition was applied to a PET film Lumirror T60 (manufactured by Toray Industries, Inc.) measuring 200 mm x 200 mm x 75 μm in thickness in the same manner as in <Adhesive Strength> above, so as to have a film thickness of 50 μm. After sandwiching the composition between similar PET films, an ultraviolet irradiation device (manufactured by Phoseon) was used to irradiate the composition with ultraviolet light having a wavelength of 395 nm at an intensity of 2000 mW / cm. 2 , cumulative light intensity 1000 mJ / cm 2The sample was irradiated at a rate of 100,000 times to form a cured film sandwiched between PET films on both sides. The sample sandwiched between PET films on both sides was set in a clamshell type bending tester (manufactured by Yuasa System Equipment Co., Ltd.). The sample was bent at a bending radius of 2 mm at a speed of 20 reciprocations / minute, and the change in appearance after 100,000 reciprocations was evaluated on a three-level scale of AA, A, and B. "AA" and "A" were deemed to be acceptable for practical use. (Criteria) AA: No cracks or white discoloration were observed. A: Cracks or white discoloration were observed in one or two places. B: Cracks or white discoloration were observed in three or more places, or the cured film protruded outside the PET film.
[0090]
[0091]
[0092]
[0093] From the results shown in Tables I to III, it can be seen that actinic radiation-curable compositions 1 to 18 (inventions 1 to 18) not only have a high refractive index but also are excellent in bending resistance and storage stability while maintaining high transparency as a physical property after film formation, compared to actinic radiation-curable compositions 19 to 23 (comparison examples 1 to 5). In other words, it can be seen that the actinic radiation-curable composition of the present invention exhibits adhesiveness in the cured film obtained by ultraviolet irradiation due to the combination of specific acrylates, and that the effects of the present invention described above can be achieved by further combining these acrylates with a specific inorganic filler.
[0094] Furthermore, as in actinic radiation curable compositions 4 to 18, it is recognized that the type and proportion of the monofunctional acrylate, the chain length of the monofunctional alkyl acrylate, and the proportion of the acrylate containing elemental sulfur also have a slight effect on the physical properties.
[0095] On the other hand, in actinic radiation-curable compositions 19 and 20 (Comparative Examples 1 and 2), the refractive index was low at 1.48 due to the absence or small amount of inorganic filler. Furthermore, because actinic radiation-curable compositions 19 and 20 were too soft, the cured film protruded from the PET film during the bending resistance test, indicating that sufficient bending resistance was not achieved. Furthermore, actinic radiation-curable composition 21 (Comparative Example 3) failed to achieve adhesive strength, and the cured film was too hard during the bending resistance test, resulting in cracks and white discoloration in some areas. Actinic radiation-curable composition 22 (Comparative Example 4) did not contain an acrylate having a hydroxy group and contained only an alkyl acrylate, but poor compatibility resulted in reduced transparency. In actinic radiation-curable composition 23 (Comparative Example 5), the cohesive strength of the cured film was insufficient, resulting in no adhesive strength and insufficient bending resistance.
[0096] INDUSTRIAL APPLICABILITY The present invention can be used for an actinic radiation-curable composition and a cured film using the same that have, as physical properties after film formation, adhesiveness, high transparency, and refractive index, as well as bending resistance and storage stability.
[0097] REFERENCE SIGNS LIST 100 Cured film manufacturing apparatus 110 One member 120 Application section 122 Actinic radiation curable composition 130 Irradiation section 142 Delivery roller 144 Pressure roller 150 Other member
Claims
1. An actinic radiation curable composition that is cured by actinic radiation, comprising a (meth)acrylate having a hydroxyl group, an alkyl (meth)acrylate, a photopolymerization initiator, and an inorganic filler, the content of the inorganic filler being within the range of 10 to 50 mass% of the total actinic radiation curable composition, and the viscosity of the actinic radiation curable composition before curing being within the range of 5 to 200 mPa·s at 25°C.
2. The actinic radiation-curable composition according to claim 1, wherein the refractive index of the inorganic filler at a wavelength of 589 nm is within the range of 1.9 to 3.
0.
3. The actinic radiation curable composition according to claim 1, wherein the inorganic filler is either zirconium oxide or titanium oxide.
4. The actinic radiation curable composition according to claim 1, wherein the inorganic filler has an average primary particle size of 100 nm or less.
5. The actinic radiation curable composition according to claim 1, wherein the (meth)acrylate contained in the entire actinic radiation curable composition does not contain elemental sulfur.
6. The actinic radiation curable composition according to claim 1, comprising, relative to the entire actinic radiation curable composition, within the ranges of 5 to 50 mass % of the (meth)acrylate having a hydroxy group, 5 to 50 mass % of the alkyl (meth)acrylate, and 0.1 to 5 mass % of the photopolymerization initiator.
7. The actinic radiation-curable composition according to claim 1, wherein the alkyl group of the alkyl (meth)acrylate has 8 to 24 carbon atoms.
8. The actinic radiation curable composition according to claim 1, which is used in an ink-jet ink.
9. A cured film which is a cured product of the actinic radiation curable composition according to any one of claims 1 to 8.
Citation Information
Patent Citations
Active energy ray-polymerizable adhesive for optical use, and optical laminate
JP2020041108A
Active energy ray-curable adhesive composition, laminated polarization film and method for producing the same, laminated optical film and image display device
JP2021073335A
Self-adhesive film, optical member including the same, and optical display device including the same
JP2023043872A
Adhesive, cured product thereof and optical member
WO2019244959A1