Method for storing phosphorus fluoride and gas-filled container

By using manganese steel or chromium-molybdenum steel containers with controlled metal impurity concentrations, the storage of phosphorus fluoride is stabilized, preventing complex formation and maintaining high purity, addressing the challenge of maintaining high purity over long periods in semiconductor manufacturing.

WO2024247729A1PCT designated stage expired Publication Date: 2024-12-05RESONAC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018016
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-05-15
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Phosphorus fluoride, used in semiconductor manufacturing as a dry etching gas, is prone to reacting with metal impurities in storage containers, leading to a decrease in purity due to complex formation, which is challenging to maintain high purity over long periods.

Method used

Storing phosphorus fluoride in containers made of manganese steel or chromium-molybdenum steel, with controlled concentrations of copper, magnesium, and palladium at 3,500 mass ppb or less, measured using an inductively coupled plasma mass spectrometer, to prevent complex formation and maintain high purity.

Benefits of technology

This method effectively stabilizes the storage of phosphorus fluoride, preventing the increase of metal impurities and ensuring the gas remains at 99.90% purity or higher, even during long-term storage, thus maintaining its etching performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provide is a method which is for storing phosphorus fluoride and by which an increase in the concentration of metal impurities is less likely to occur. The phosphorus fluoride, which is at least one among phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, is stored in a container while the total concentration of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3,500 mass ppb or less.
Need to check novelty before this filing date? Find Prior Art

Description

Storage method of phosphorus fluoride and gas-filled containers

[0001] The present invention relates to a method for storing phosphorus fluoride, which is at least one of phosphorus trifluoride (PF3), phosphorus pentafluoride (PF5), and diphosphorus tetrafluoride (P2F4), and a gas-filled container thereof.

[0002] Phosphorus fluorides such as phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, as well as fluorine-containing gases such as chlorine trifluoride (ClF) and iodine heptafluoride (IF), are used as dry etching gases in semiconductor manufacturing. Stable fine processing during dry etching requires high purity dry etching gases (e.g., 99.9% by volume or higher). Furthermore, since dry etching gases are stored in a filled container, they must be kept highly pure for an extended period of time in the storage container. In particular, metal impurities, which may cause particle generation during dry etching, must be suppressed to a concentration of 1 ppm by mass or less.

[0003] Patent Document 1 discloses a technology for fluorinating the inner surface of a storage container for storing fluorine-containing gas to suppress reaction between the fluorine-containing gas and the metal material forming the storage container. The storage container is filled with fluorine-containing gas after previously carrying out a fluorination treatment to cause a reaction between the metal material forming the inner surface of the storage container and the fluorine-containing gas. This makes it difficult for the metal material forming the storage container to react with the filled fluorine-containing gas, thereby suppressing the generation of metal impurities. Therefore, a decrease in the purity of the filled fluorine-containing gas is suppressed for a long period of time.

[0004] International Publication No. 2019 / 026682

[0005] However, phosphorus fluoride is highly reactive as a ligand and can form complexes with various metal atoms. Therefore, during long-term storage, phosphorus fluoride may react with the metal material forming the storage container to form a complex, which may produce metal impurities, resulting in a decrease in the purity of the phosphorus fluoride. An object of the present invention is to provide a method for storing phosphorus fluoride and a gas-filled container that are less likely to cause an increase in the concentration of metal impurities.

[0006] In order to solve the above problems, one aspect of the present invention is as follows [1] to [8]: [1] A method for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, wherein the phosphorus fluoride is stored in a container such that the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3500 ppb by mass or less.

[0007] [2] The method for storing phosphorus fluoride according to [1], wherein the container is made of at least one of manganese steel and chromium-molybdenum steel. [3] The method for storing phosphorus fluoride according to [1] or [2], wherein the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride are measured by an inductively coupled plasma mass spectrometer. [4] The method for storing phosphorus fluoride according to any one of [1] to [3], wherein the phosphorus fluoride is stored in the container with a purity of 99.90% by volume or more.

[0008] [5] A gas-filled container in which phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, is filled in the container, wherein the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3,500 ppb by mass or less.

[0009] [6] The gas-filled container according to [5], wherein the material of the container is at least one of manganese steel and chromium-molybdenum steel. [7] The gas-filled container according to [5] or [6], wherein the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride are measured by an inductively coupled plasma mass spectrometer. [8] The gas-filled container according to any one of [5] to [7], wherein the purity of the phosphorus fluoride is 99.90% by volume or more.

[0010] When phosphorus fluoride is stored using the storage method of the present invention, the concentration of metal impurities in the phosphorus fluoride is unlikely to increase. Furthermore, the gas-filled container of the present invention is unlikely to cause an increase in the concentration of metal impurities in the phosphorus fluoride.

[0011] An embodiment of the present invention will be described below. Note that this embodiment is merely an example of the present invention, and the present invention is not limited to this embodiment. Furthermore, various modifications and improvements can be made to this embodiment, and such modifications and improvements can also be included in the present invention.

[0012] The method for storing phosphorus fluoride according to this embodiment is a method for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, in which the phosphorus fluoride is stored in a container such that the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3,500 ppb by mass or less.

[0013] Furthermore, the method for storing phosphorus fluoride according to this embodiment may be a method for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, in which the phosphorus fluoride contains at least one of copper, magnesium, calcium, and palladium, and the phosphorus fluoride is stored in a container such that the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3,500 ppb by mass or less.

[0014] The gas-filled container according to this embodiment is a gas-filled container in which phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, is filled in the container, and the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3,500 ppb by mass or less.

[0015] Furthermore, the gas-filled container according to this embodiment is a gas-filled container in which phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, is filled in the container, and the phosphorus fluoride may contain at least one of copper, magnesium, calcium, and palladium, and the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride may be 3,500 ppb by mass or less.

[0016] When phosphorus fluoride contains at least one of copper, magnesium, calcium, and palladium, the catalytic action of these metals promotes a reaction in which metal atoms contained in the metal material forming the container and phosphorus fluoride form a complex. Therefore, when phosphorus fluoride contains at least one of copper, magnesium, calcium, and palladium, the complex formation reaction proceeds during storage in a container, resulting in the generation of metal impurities and a decrease in purity.

[0017] The phosphorus fluoride storage method and gas-filled container according to this embodiment store phosphorus fluoride in a container with a total concentration of copper, magnesium, calcium, and palladium of 3500 mass ppb or less (i.e., the total concentration of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride before filling the container is 3500 mass ppb or less), so the complex formation reaction described above is unlikely to proceed even during long-term storage. As a result, metal impurities are unlikely to be generated, and the concentration of metal impurities is unlikely to increase (i.e., the purity of the phosphorus fluoride is unlikely to decrease). Therefore, phosphorus fluoride can be stored stably for long periods of time.

[0018] Examples of metals that form complexes with phosphorus fluoride include nickel (Ni), zinc (Zn), chromium (Cr), molybdenum (Mo), and tungsten (W). When phosphorus fluoride is stored using the phosphorus fluoride storage method according to this embodiment or the gas-filled container according to this embodiment, even if the metal material forming the container contains at least one of nickel, zinc, chromium, molybdenum, and tungsten, the reaction of nickel, zinc, chromium, molybdenum, and tungsten with phosphorus fluoride to form complexes is unlikely to proceed. Therefore, metal impurities are unlikely to be generated, and the concentration of metal impurities is unlikely to increase. As a result, even if phosphorus fluoride is stored in the container for a long period of time, the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten in the phosphorus fluoride can be maintained at 1,000 ppb by mass or less.

[0019] The sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten in phosphorus fluoride is preferably maintained at 1000 mass ppb or less, more preferably at 800 mass ppb or less, and even more preferably at 500 mass ppb or less. When the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten in phosphorus fluoride is 1000 mass ppb or less, deterioration of etching performance when phosphorus fluoride is used as a dry etching gas tends to be avoided. When the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten in phosphorus fluoride exceeds 1000 mass ppb, it is believed that a complex formation reaction between phosphorus fluoride and the metal forming the inner surface of the container is progressing.

[0020] The method for storing phosphorus fluoride according to this embodiment is a method for storing phosphorus fluoride in a container such that the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3500 mass ppb or less. However, the stored phosphorus fluoride may contain at least one of copper, magnesium, calcium, and palladium (i.e., the sum of the concentrations may be more than 0 mass ppb and 3500 mass ppb or less), or may not contain any of these elements at all (i.e., the sum of the concentrations may be 0 mass ppb).

[0021] Furthermore, the gas-filled container according to this embodiment is a container filled with phosphorus fluoride such that the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3500 mass ppb or less. However, the phosphorus fluoride to be filled may contain at least one of copper, magnesium, calcium, and palladium (i.e., the sum of the concentrations may be greater than 0 mass ppb and 3500 mass ppb or less), or may not contain any of these elements at all (i.e., the sum of the concentrations may be 0 mass ppb).

[0022] The phosphorus fluoride storage method according to this embodiment and the gas-filled container according to this embodiment will be described in further detail below. [Phosphorus Fluoride] As described above, the phosphorus fluoride is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride. That is, the phosphorus fluoride may be any one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, or may be a mixture of two or three of them.

[0023] When the phosphorus fluoride is a mixture of two or three of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, the content of the main component, which is the component with the largest content, is preferably 99 mol% or more, more preferably 99.9 mol% or more, and even more preferably 99.99 mol% or more. The total content of components other than the main component is preferably 0.1 mol% or less, more preferably 0.01 mol% or less, and even more preferably 0.001 mol% or less.

[0024] When storing phosphorus fluoride in a container, a gas consisting of phosphorus fluoride alone may be stored in the container, or a mixed gas containing phosphorus fluoride and a diluent gas may be stored in the container. Alternatively, a portion or all of the phosphorus fluoride may be liquefied and stored in the container. The diluent gas may be at least one selected from nitrogen gas (N), helium (He), neon (Ne), argon (Ar), krypton (Kr), and xenon (Xe). The content of the diluent gas is preferably 90% by volume or less, more preferably 50% by volume or less, of the total amount of gas stored in the container.

[0025] In the method for storing phosphorus fluoride according to this embodiment and the gas-filled container according to this embodiment, it is preferable to store phosphorus fluoride with a purity of 99.90% by volume or more in the container. If the purity of the phosphorus fluoride introduced into the container is 99.90% by volume or more, an effect is achieved in that the etching target can be etched selectively compared to the non-etching target at a sufficient etching rate.

[0026] [Container] The container for storing or filling phosphorus fluoride is not particularly limited in shape, size, material, etc., as long as it can contain and seal phosphorus fluoride, but it is preferable that the container has corrosion resistance against phosphorus fluoride. Examples of materials for the container, from the viewpoint of corrosion resistance, include manganese steel, stainless steel, chromium molybdenum steel, Hastelloy (registered trademark), Inconel (registered trademark), Monel (registered trademark), etc. The material of the container may be at least one of manganese steel and chromium molybdenum steel.

[0027] [Metals Contained in Phosphorus Fluoride] The phosphorus fluoride in the storage method for phosphorus fluoride according to this embodiment and the gas-filled container according to this embodiment may or may not contain at least one of copper, magnesium, calcium, and palladium. However, when the phosphorus fluoride contains at least one of copper, magnesium, calcium, and palladium, the sum of the concentrations of copper, magnesium, calcium, and palladium is 3500 mass ppb or less. Therefore, as described above, the complex formation reaction between the phosphorus fluoride and nickel, zinc, chromium, molybdenum, and tungsten is unlikely to proceed. Here, "not containing" refers to a case where the concentration cannot be quantified using an inductively coupled plasma mass spectrometer (ICP-MS). In other words, the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride can be measured using an inductively coupled plasma mass spectrometer. More specifically, they can be measured using the method described in the Examples.

[0028] In order to make it difficult for the complex-forming reaction between phosphorus fluoride and nickel, zinc, chromium, molybdenum, and tungsten to proceed during storage, the sum of the concentrations of copper, magnesium, calcium, and palladium contained in phosphorus fluoride needs to be 3500 mass ppb or less, preferably 2000 mass ppb or less, and more preferably 1000 mass ppb or less.

[0029] Copper, magnesium, calcium, and palladium may be contained in phosphorus fluoride as elemental metals, metal compounds, metal halides, or metal complexes. The forms of copper, magnesium, calcium, and palladium in phosphorus fluoride include fine particles, droplets, and gas. It is believed that copper, magnesium, calcium, and palladium are contaminated into phosphorus fluoride due to the raw materials, reaction catalysts, reactors, purification equipment, and the like used in synthesizing phosphorus fluoride.

[0030] [Method for producing phosphorus fluoride with low metal concentrations] As described above, in the phosphorus fluoride storage method according to this embodiment and the phosphorus fluoride filled in the gas-filled container according to this embodiment, the total concentration of copper, magnesium, calcium, and palladium contained therein must be 3500 ppb by mass or less. However, the method for producing phosphorus fluoride with low concentrations of copper, magnesium, calcium, and palladium is not particularly limited.

[0031] Examples of methods for producing phosphorus fluoride having low concentrations of copper, magnesium, calcium, and palladium include a method of removing copper, magnesium, calcium, and palladium from phosphorus fluoride having a high total concentration of copper, magnesium, calcium, and palladium. The method for removing copper, magnesium, calcium, and palladium from phosphorus fluoride is not particularly limited, and known methods can be used. Examples include a method using a filter, a method using an adsorbent, and distillation.

[0032] The material of the filter that selectively passes the phosphorus fluoride gas is preferably a resin, and particularly preferably polytetrafluoroethylene, in order to prevent metal components from being mixed into the phosphorus fluoride. The average pore size of the filter is preferably 0.01 μm or more and 30 μm or less, and more preferably 0.1 μm or more and 10 μm or less. When the average pore size is within the above range, copper, magnesium, calcium, and palladium can be sufficiently removed, and a sufficient flow rate of the phosphorus fluoride gas can be ensured, thereby achieving high productivity.

[0033] The flow rate of phosphorus fluoride gas passing through the filter is 1 cm per filter area.2 When the flow rate of the phosphorus fluoride gas is within the above range, the phosphorus fluoride gas is prevented from becoming highly pressurized, the risk of leakage of the phosphorus fluoride gas is reduced, and high productivity can be achieved.

[0034] [Pressure Conditions During Storage] The pressure conditions during storage in the phosphorus fluoride storage method according to this embodiment and the gas-filled container according to this embodiment are not particularly limited as long as the phosphorus fluoride can be stored hermetically in the container, but are preferably 0.15 MPa or more and 15 MPa or less, and more preferably 0.3 MPa or more and 9 MPa or less. If the pressure conditions are within the above range, the phosphorus fluoride can be circulated without heating when the container is connected to a dry etching device.

[0035] [Temperature Conditions During Storage] The temperature conditions during storage of the phosphorus fluoride storage method according to this embodiment and the gas-filled container according to this embodiment are not particularly limited, but are preferably -20°C or higher and 50°C or lower, and more preferably 0°C or higher and 40°C or lower. If the storage temperature is -20°C or higher, the container is less likely to deform, reducing the possibility of the container losing its airtightness and allowing oxygen, water, etc. to enter the container. If oxygen, water, etc. enters the container, the decomposition reaction of the phosphorus fluoride may be accelerated. On the other hand, if the storage temperature is 50°C or lower, the decomposition reaction of the phosphorus fluoride is suppressed.

[0036] [Etching] The phosphorus fluoride stored by the method for storing phosphorus fluoride according to this embodiment or in the gas-filled container according to this embodiment can be used as an etching gas. The phosphorus fluoride-containing etching gas stored by the method for storing phosphorus fluoride according to this embodiment or in the gas-filled container according to this embodiment can be used for both plasma etching using plasma and plasmaless etching not using plasma.

[0037] Examples of plasma etching include reactive ion etching (RIE), inductively coupled plasma (ICP) etching, capacitively coupled plasma (CCP) etching, electron cyclotron resonance (ECR) plasma etching, and microwave plasma etching. In plasma etching, the plasma may be generated in a chamber in which the member to be etched is placed, or the plasma generation chamber and the chamber in which the member to be etched is placed may be separate (i.e., remote plasma may be used).

[0038] The present invention will be described in more detail below with reference to examples and comparative examples. Phosphorus fluoride containing various concentrations of copper, magnesium, calcium, and palladium was prepared. Examples of phosphorus fluoride preparation are described below. (Preparation Example 1) One 47-liter manganese steel cylinder and four 3.4-liter sealable manganese steel cylinders were prepared. The 3.4-liter cylinders were designated Cylinder A, Cylinder B, Cylinder C, and Cylinder D, respectively. The 47-liter cylinder was filled with 5,000 g of phosphorus trifluoride (boiling point at atmospheric pressure: −101.8°C) and liquefied by cooling to −196°C, forming a liquid phase and a gas phase at approximately 100 kPa. Cylinders A, B, C, and D were depressurized to 1 kPa or less using a vacuum pump and then cooled to −196°C. The purity of the phosphorus trifluoride in the 47 L cylinder analyzed by gas chromatography was 99.95% by volume.

[0039] 500 g of phosphorus trifluoride gas was extracted from the upper outlet of a 47 L cylinder where the gas phase was present, passed through a filter, and then liquefied and collected in cylinder A under reduced pressure at -196°C. The filter was a PTFE filter manufactured by Flon Industries Co., Ltd., and had an outer diameter of 50 mm, a thickness of 80 μm, and an average pore size of 0.3 μm. The flow rate of the gas passing through the filter was controlled to 500 mL / min using a mass flow controller. The amount of phosphorus trifluoride collected in cylinder A was 499 g.

[0040] The phosphorus trifluoride collected in cylinder A is designated Sample 1-1. The phosphorus trifluoride collected in cylinder A consists of a gas phase and a liquid phase. The gas phase was extracted from the upper outlet, and the concentrations of copper, magnesium, calcium, and palladium were measured using an inductively coupled plasma mass spectrometer. The results are shown in Table 1. The details of the method for measuring the concentrations of copper, magnesium, calcium, and palladium using an inductively coupled plasma mass spectrometer are as follows.

[0041] While the liquid phase phosphorus trifluoride in cylinder A was vaporized at -78°C, phosphorus trifluoride gas was extracted from the gas phase and passed through 100 g of a 1 mol / L aqueous nitric acid solution at a flow rate of 100 mL / min, causing bubbling. This bubbling brought the phosphorus trifluoride into contact with the aqueous nitric acid solution, causing copper, magnesium, calcium, and palladium to be absorbed into the aqueous nitric acid solution. The mass of the aqueous nitric acid solution after bubbling was 98 g (M1). The mass difference of cylinder A before and after bubbling was a decrease of 24 g (M2).

[0042] After bubbling, 10 g of the nitric acid solution (M3) was collected and diluted to 100 mL (V) with ultrapure water using a measuring flask. The concentrations of various metal atoms (copper, magnesium, calcium, and palladium) in the diluted nitric acid solution were measured using an inductively coupled plasma mass spectrometer, and the concentrations of various metal atoms in phosphorus trifluoride (C, units: g / g) were calculated using the measured value (c1, units: g / mL) and the following formula: C = {(c1 × V) × (M1 / M3)} / M2

[0043]

[0044] Next, cylinder A was controlled to approximately −78°C to form a liquid phase and a gas phase, and 100 g of phosphorus trifluoride gas was extracted from the upper outlet of cylinder A, where the gas phase was present, and transferred to cylinder B, which was under reduced pressure, and collected. Furthermore, 10 g of phosphorus trifluoride gas was extracted from a 47 L cylinder, transferred to cylinder B, which was under reduced pressure, and collected. Cylinder B was then heated to room temperature in a sealed state and allowed to stand for 24 hours. The phosphorus trifluoride gas after standing was designated Sample 1-2. After standing, phosphorus trifluoride gas was extracted from the upper outlet of cylinder B, where the gas phase was present, and the concentrations of copper, magnesium, calcium, and palladium were measured using an inductively coupled plasma mass spectrometer in the same manner as above. The results are shown in Table 1.

[0045] Similarly, 100 g of phosphorus trifluoride gas was extracted from the upper outlet of cylinder A, where the gas phase was present, and transferred to cylinder C, which was under reduced pressure, and collected. Furthermore, 100 g of phosphorus trifluoride gas was extracted from a 47 L cylinder, transferred to cylinder C, which was under reduced pressure, and collected. Cylinder C was then heated to room temperature in a sealed state and allowed to stand for 24 hours. The phosphorus trifluoride gas after standing was designated Sample 1-3. After standing, phosphorus trifluoride gas was extracted from cylinder C, where the gas phase was present, and the concentrations of copper, magnesium, calcium, and palladium were measured using an inductively coupled plasma mass spectrometer in the same manner as above. The results are shown in Table 1.

[0046] Similarly, 100 g of phosphorus trifluoride gas was extracted from the upper outlet of cylinder A, where the gas phase was present, and transferred to cylinder D, which was under reduced pressure, and collected. Furthermore, 200 g of phosphorus trifluoride gas was extracted from a 47 L cylinder, transferred to cylinder D, which was under reduced pressure, and collected. Cylinder D was then heated to room temperature in a sealed state and allowed to stand for 24 hours. The phosphorus trifluoride gas after standing was designated Sample 1-4. After standing, phosphorus trifluoride gas was extracted from cylinder D, where the gas phase was present, and the concentrations of copper, magnesium, calcium, and palladium were measured using an inductively coupled plasma mass spectrometer in the same manner as above. The results are shown in Table 1.

[0047] (Preparation Example 2) Samples 2-1 to 2-4 were prepared in the same manner as in Preparation Example 1, except that phosphorus pentafluoride was used instead of the phosphorus fluoride. The concentrations of copper, magnesium, calcium, and palladium in each sample were measured using an inductively coupled plasma mass spectrometer in the same manner as in Preparation Example 1. The results are shown in Table 2.

[0048]

[0049] (Example 1) After the sealed cylinder A was allowed to stand at 23°C for 30 days, phosphorus trifluoride gas was extracted from the gas phase of the cylinder A, and the concentrations of nickel, zinc, chromium, molybdenum, and tungsten in Sample 1-1 were measured with an inductively coupled plasma mass spectrometer in the same manner as in Preparation Example 1. The results are shown in Table 3.

[0050]

[0051] (Examples 2 to 6 and Comparative Examples 1 and 2) For Samples 1-2, 1-3, and 1-4 and Samples 2-1, 2-2, 2-3, and 2-4, the concentrations of nickel, zinc, chromium, molybdenum, and tungsten were measured using an inductively coupled plasma mass spectrometer in the same manner as in Example 1. The results are shown in Table 3.

[0052] As can be seen from the results shown in Table 3, in Examples 1 to 6, the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten after storage at 23°C for 30 days was 500 ppb by mass or less. In contrast, in Comparative Examples 1 and 2, the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten after storage at 23°C for 30 days was 1000 ppb by mass or more. From these results, it is believed that in Comparative Examples 1 and 2, the catalytic action of copper, magnesium, calcium, and palladium caused the metals contained in the metal material forming the cylinder to react with phosphorus fluoride to form complexes, resulting in the generation of metal impurities.

Claims

1. A method for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, comprising storing the phosphorus fluoride in a container such that the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3,500 ppb by mass or less.

2. The method for storing phosphorus fluoride according to claim 1, wherein the container is made of at least one of manganese steel and chrome molybdenum steel.

3. A method for storing phosphorus fluoride according to claim 1 or 2, wherein the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride are measured by an inductively coupled plasma mass spectrometer.

4. A method for storing phosphorus fluoride according to claim 1 or 2, wherein the phosphorus fluoride is stored in the container with a purity of 99.90% by volume or more.

5. A gas-filled container in which phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, is filled in the container, and the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride is 3,500 ppb by mass or less.

6. A gas-filled container according to claim 5, wherein the container is made of at least one of manganese steel and chrome-molybdenum steel.

7. A gas-filled container according to claim 5 or 6, wherein the concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride are measured by an inductively coupled plasma mass spectrometer.

8. A gas-filled container according to claim 5 or 6, wherein the purity of said phosphorus fluoride is 99.90% by volume or more.

Citation Information

Patent Citations

  • METALLIC MATERIAL, AND PRESERVING CONTAINER, GAS PIPE AND APPARATUS USING THE SAME, MANUFACTURING METHOD THEREFOR, AND METHOD FOR PRESERVING ClF3

    JP2009197274A

  • Method for producing phosphorus pentafluoride and hexafluorophosphates

    JP2010042937A

  • Method for producing phosphorus pentafluoride and hexafluorophosphate

    JP2013237612A

  • Method for producing phosphorus pentafluoride and hexafluorophosphate

    JP2014001136A

  • Method for manufacturing filled containers

    JP2022159338A