Method for storing phosphorus fluoride, storage container, and gas-loaded storage container
By using containers made from metal materials with controlled copper, magnesium, and palladium concentrations, the storage of phosphorus fluoride is stabilized, preventing impurity generation and maintaining high purity, addressing the reactivity issues and ensuring effective dry etching performance.
Patent Information
- Application Number
- PCT/JP2024/018017
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-15
- Publication Date
- 2024-12-05
AI Technical Summary
Phosphorus fluoride compounds, such as phosphorus trifluoride and phosphorus pentafluoride, are prone to reacting with metal impurities in storage containers, leading to a decrease in purity and the generation of metal impurities during long-term storage, which is problematic for maintaining high-purity dry etching gases in semiconductor manufacturing.
Storing phosphorus fluoride in containers made from metal materials with a total concentration of copper, magnesium, and palladium of 0.8% by mass or less, specifically using manganese steel or chrome-molybdenum steel, and ensuring the purity of phosphorus fluoride is maintained at 99.90% by volume or more, thereby minimizing complex formation reactions and impurity generation.
This approach effectively stabilizes the storage of phosphorus fluoride, maintaining low concentrations of metal impurities like nickel, zinc, chromium, molybdenum, and tungsten at 1000 mass ppb or less, ensuring high-purity storage and preventing decreases in etching performance over time.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Storage method, storage container, and gas-filled storage container for phosphorus fluoride
[0001] The present invention relates to a method for storing phosphorus fluoride, which is at least one of phosphorus trifluoride (PF3), phosphorus pentafluoride (PF5), and diphosphorus tetrafluoride (P2F4), a storage container, and a gas-filled storage container.
[0002] Phosphorus fluorides such as phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, as well as fluorine-containing gases such as chlorine trifluoride (ClF) and iodine heptafluoride (IF), are used as dry etching gases in semiconductor manufacturing. Stable fine processing during dry etching requires high purity dry etching gases (e.g., 99.9% by volume or higher). Furthermore, since dry etching gases are stored in a filled container, they must be kept highly pure for an extended period of time in the storage container. In particular, metal impurities, which may cause particle generation during dry etching, must be suppressed to a concentration of 1 ppm by mass or less.
[0003] Patent Document 1 discloses a technology for fluorinating the inner surface of a storage container for storing fluorine-containing gas to suppress reaction between the fluorine-containing gas and the metal material forming the storage container. The storage container is filled with fluorine-containing gas after previously carrying out a fluorination treatment to cause a reaction between the metal material forming the inner surface of the storage container and the fluorine-containing gas. This makes it difficult for the metal material forming the storage container to react with the filled fluorine-containing gas, thereby suppressing the generation of metal impurities. Therefore, a decrease in the purity of the filled fluorine-containing gas is suppressed for a long period of time.
[0004] International Publication No. 2019 / 026682
[0005] However, phosphorus fluoride is highly reactive as a ligand and can form complexes with various metal atoms. Therefore, during long-term storage, phosphorus fluoride may react with the metal material forming the storage container to form a complex, which may generate metal impurities, resulting in a decrease in the purity of the phosphorus fluoride. An object of the present invention is to provide a storage method, storage container, and gas-filled storage container for phosphorus fluoride that are less likely to cause an increase in the concentration of metal impurities.
[0006] In order to solve the above problems, one aspect of the present invention is as follows [1] to
[10] : [1] A method for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, comprising storing the phosphorus fluoride in a storage container having a portion that comes into contact with the phosphorus fluoride formed of a metal material, and wherein the sum of concentrations of copper, magnesium, calcium, and palladium contained in the metal material is 0.8 mass % or less.
[0007] [2] The method for storing phosphorus fluoride according to [1], wherein the metal material is at least one of manganese steel and chromium-molybdenum steel. [3] The method for storing phosphorus fluoride according to [1] or [2], wherein the concentrations of copper, magnesium, calcium, and palladium contained in the metal material are measured by X-ray photoelectron spectroscopy. [4] The method for storing phosphorus fluoride according to any one of [1] to [3], wherein the purity of the phosphorus fluoride is 99.90% by volume or more and the phosphorus fluoride is stored in the storage container.
[0008] [5] A storage container for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, wherein a portion that comes into contact with the phosphorus fluoride is formed of a metal material, and the total concentration of copper, magnesium, calcium, and palladium contained in the metal material is 0.8 mass % or less. [6] The phosphorus fluoride storage container according to [5], wherein the metal material is at least one of manganese steel and chromium molybdenum steel.
[0009] [7] A gas-filled storage container in which phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, is filled in the storage container, wherein a portion of the storage container that comes into contact with the phosphorus fluoride is formed of a metal material, and the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the metal material is 0.8 mass% or less.
[0010] [8] The gas-filled storage container according to [7], wherein the metal material is at least one of manganese steel and chromium-molybdenum steel. [9] The gas-filled storage container according to [7] or [8], wherein the concentrations of copper, magnesium, calcium, and palladium contained in the metal material are measured by X-ray photoelectron spectroscopy.
[10] The gas-filled storage container according to any one of [7] to [9], wherein the purity of the phosphorus fluoride is 99.90% by volume or more.
[0011] When phosphorus fluoride is stored in the phosphorus fluoride storage method, storage container, and gas-filled storage container according to the present invention, the concentration of metal impurities in the phosphorus fluoride is unlikely to increase.
[0012] An embodiment of the present invention will be described below. Note that this embodiment is merely an example of the present invention, and the present invention is not limited to this embodiment. Furthermore, various modifications and improvements can be made to this embodiment, and such modifications and improvements can also be included in the present invention.
[0013] The method for storing phosphorus fluoride according to this embodiment is a method for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, in which the phosphorus fluoride is stored in a storage container whose contact parts are made of a metal material, and the total concentration of copper, magnesium, calcium, and palladium contained in the metal material is 0.8 mass% or less.
[0014] The phosphorus fluoride storage container according to the present embodiment is a storage container for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, and is a container in which a portion that comes into contact with the phosphorus fluoride is formed of a metal material, and the total concentration of copper, magnesium, calcium, and palladium contained in this metal material is 0.8 mass% or less.
[0015] Furthermore, the gas-filled storage container of this embodiment is a gas-filled storage container in which phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, is filled in the storage container, and the portion of the storage container that comes into contact with the phosphorus fluoride is formed of a metal material, and the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the metal material is 0.8 mass% or less.
[0016] When the metal material forming the portion of the storage container that comes into contact with phosphorus fluoride contains at least one of copper, magnesium, calcium, and palladium, the catalytic action of these metals promotes a reaction in which metal atoms contained in the metal material and phosphorus fluoride form a complex. Therefore, if phosphorus fluoride is stored in a storage container made of a metal material containing at least one of copper, magnesium, calcium, and palladium, the complex formation reaction may progress during storage in the storage container, resulting in the generation of metal impurities and a decrease in the purity of the phosphorus fluoride.
[0017] In the phosphorus fluoride storage method, storage container, and gas-filled storage container according to this embodiment, the total concentration of copper, magnesium, calcium, and palladium contained in the metal material forming the portion of the storage container that comes into contact with the phosphorus fluoride is 0.8 mass% or less, so the complex formation reaction described above is unlikely to proceed even during long-term storage. As a result, metal impurities are unlikely to be generated, and the concentration of metal impurities is unlikely to increase (i.e., the purity of the phosphorus fluoride is unlikely to decrease). Therefore, the phosphorus fluoride can be stored stably for long periods of time.
[0018] Examples of metals that form complexes with phosphorus fluoride include nickel (Ni), zinc (Zn), chromium (Cr), molybdenum (Mo), and tungsten (W). When phosphorus fluoride is stored using the phosphorus fluoride storage method, storage container, and gas-filled storage container according to this embodiment, even if the metal material forming the portion of the storage container that comes into contact with the phosphorus fluoride contains at least one of nickel, zinc, chromium, molybdenum, and tungsten, the reaction of nickel, zinc, chromium, molybdenum, and tungsten with phosphorus fluoride to form complexes is unlikely to proceed. Therefore, metal impurities are unlikely to be generated, and the concentration of metal impurities is unlikely to increase. As a result, even if phosphorus fluoride is stored in the storage container for a long period of time, the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten in the phosphorus fluoride can be maintained at 1,000 ppb by mass or less.
[0019] The sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten in the phosphorus fluoride is preferably maintained at 1000 mass ppb or less, more preferably 800 mass ppb or less, and even more preferably 500 mass ppb or less. When the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten in the phosphorus fluoride is 1000 mass ppb or less, deterioration of etching performance when the phosphorus fluoride is used as a dry etching gas tends to be avoided. When the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten in the phosphorus fluoride exceeds 1000 mass ppb, it is thought that a complex formation reaction between the phosphorus fluoride and the metal material forming the contact portion of the storage container is progressing in the contact portion between the phosphorus fluoride and the metal material forming the contact portion.
[0020] In addition, the phosphorus fluoride storage method, storage container, and gas-filled storage container of this embodiment are configured so that the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the metal material that forms the part of the storage container that stores phosphorus fluoride and that comes into contact with the phosphorus fluoride is 0.8 mass% or less. However, the metal material may contain at least one of copper, magnesium, calcium, and palladium (i.e., the sum of the concentrations may be more than 0 mass% and 0.8 mass% or less), or may not contain any of these elements at all (i.e., the sum of the concentrations may be 0 mass%).
[0021] The phosphorus fluoride storage method, storage container, and gas-filled storage container according to this embodiment will be described in further detail below. [Phosphorus Fluoride] As described above, the phosphorus fluoride is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride. That is, the phosphorus fluoride may be any one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, or a mixture of two or three of them.
[0022] When the phosphorus fluoride is a mixture of two or three of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, the content of the main component, which is the component with the largest content, is preferably 99 mol% or more, more preferably 99.9 mol% or more, and even more preferably 99.99 mol% or more. The total content of components other than the main component is preferably 0.1 mol% or less, more preferably 0.01 mol% or less, and even more preferably 0.001 mol% or less.
[0023] When storing phosphorus fluoride in a storage container, a gas consisting of only phosphorus fluoride may be stored in the storage container, or a mixed gas containing phosphorus fluoride and a diluent gas may be stored in the storage container. Alternatively, a portion or all of the phosphorus fluoride may be liquefied and stored in the storage container. The diluent gas may be at least one selected from nitrogen gas (N), helium (He), neon (Ne), argon (Ar), krypton (Kr), and xenon (Xe). The content of the diluent gas is preferably 90% by volume or less, and more preferably 50% by volume or less, of the total amount of gas stored in the storage container.
[0024] In the phosphorus fluoride storage method, storage container, and gas-filled storage container according to the present embodiment, it is preferable to store phosphorus fluoride with a purity of 99.90% by volume or more in the storage container. If the purity of the phosphorus fluoride introduced into the storage container is 99.90% by volume or more, an effect is achieved in that the etching target can be selectively etched at a sufficient etching rate compared to the non-etching target.
[0025] [Storage Container] The shape, size, etc. of a storage container for storing or filling phosphorus fluoride are not particularly limited as long as the container can contain and seal phosphorus fluoride, the portion that comes into contact with the phosphorus fluoride is formed of a metal material, and the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the metal material is 0.8 mass% or less. The material of the portion of the storage container that does not come into contact with the phosphorus fluoride is also not particularly limited. However, it is preferable that the storage container be corrosion-resistant to phosphorus fluoride. Examples of the metal material include manganese steel, stainless steel, chromium-molybdenum steel, Hastelloy (registered trademark), Inconel (registered trademark), Monel (registered trademark), etc., from the viewpoint of corrosion resistance. The metal material may be at least one of manganese steel and chromium-molybdenum steel.
[0026] Examples of manganese steel storage containers and chromium-molybdenum steel storage containers include containers manufactured from steel pipes specified in JIS G3429 (seamless steel pipes for high-pressure gas containers) STH11 and STH12 (manganese steel pipes) and STH21 and STH22 (chromium-molybdenum steel pipes) of the JIS standard.
[0027] However, these standards do not include a section on copper, and the copper concentration in manganese steel and chromium-molybdenum steel is unknown, so simply meeting these standards is insufficient. Analysis of the inner surfaces of several commercially available cylinders that meet the STH12 standard revealed that the copper concentration varied depending on the cylinder. Therefore, when using containers made of general manganese steel or chromium-molybdenum steel as storage containers in the present invention, it is necessary to select those with a total concentration of copper, magnesium, calcium, and palladium of 0.8 mass% or less.
[0028] The storage container also includes a valve, which is preferably made of manganese steel, stainless steel, or chrome-molybdenum steel, just like the storage container. Valves made of brass or copper alloys such as Monel (registered trademark) can also be used as long as they are designed to avoid direct contact with phosphorus fluoride.
[0029] [Copper, Magnesium, Calcium, and Palladium Contained in the Metallic Material] The metallic material in the phosphorus fluoride storage method, storage container, and gas-filled storage container according to this embodiment may or may not contain at least one of copper, magnesium, calcium, and palladium. However, when the metallic material contains copper, magnesium, calcium, and palladium, the sum of the concentrations of copper, magnesium, calcium, and palladium is 0.8 mass% or less. Therefore, as described above, the complex formation reaction between phosphorus fluoride and nickel, zinc, chromium, molybdenum, and tungsten is unlikely to proceed. Here, "not containing" refers to a case where the amounts cannot be quantified by X-ray photoelectron spectroscopy (XPS analysis). That is, the concentrations of copper, magnesium, calcium, and palladium contained in the metallic material can be measured by X-ray photoelectron spectroscopy. More specifically, they can be measured by the method described in the Examples.
[0030] In order to make it difficult for the complex-forming reaction between phosphorus fluoride and nickel, zinc, chromium, molybdenum, and tungsten to proceed during storage, the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the metal material needs to be 0.8 mass% or less, preferably 0.4 mass% or less, and more preferably 0.2 mass% or less. Note that copper, magnesium, calcium, and palladium are thought to be contaminated into the storage container due to the metal material that is the raw material for the storage container, the storage container manufacturing equipment used in manufacturing the storage container, etc.
[0031] [Method for producing phosphorus fluoride with low metal concentration] In the phosphorus fluoride storage method according to this embodiment and the gas-filled storage container according to this embodiment, the phosphorus fluoride filled in the storage container (phosphorus fluoride before filling) also preferably contains low concentrations of copper, magnesium, calcium, and palladium.
[0032] Examples of methods for producing phosphorus fluoride having low concentrations of copper, magnesium, calcium, and palladium include a method of removing copper, magnesium, calcium, and palladium from phosphorus fluoride having a high total concentration of copper, magnesium, calcium, and palladium. The method for removing copper, magnesium, calcium, and palladium from phosphorus fluoride is not particularly limited, and known methods can be used. Examples include a method using a filter, a method using an adsorbent, and distillation.
[0033] The material of the filter that selectively passes the phosphorus fluoride gas is preferably a resin, and particularly preferably polytetrafluoroethylene, in order to prevent metal components from being mixed into the phosphorus fluoride. The average pore size of the filter is preferably 0.01 μm or more and 30 μm or less, and more preferably 0.1 μm or more and 10 μm or less. When the average pore size is within the above range, copper, magnesium, calcium, and palladium can be sufficiently removed, and a sufficient flow rate of the phosphorus fluoride gas can be ensured, thereby achieving high productivity.
[0034] The flow rate of phosphorus fluoride gas passing through the filter is 1 cm per filter area. 2 The flow rate of the phosphorus fluoride gas is preferably 3 mL / min or more and 300 mL / min or less, and more preferably 10 mL / min or more and 50 mL / min or less. If the flow rate of the phosphorus fluoride gas is within the above range, the phosphorus fluoride gas is prevented from becoming highly pressurized, the risk of leakage of the phosphorus fluoride gas is reduced, and high productivity can be achieved. The concentrations of copper, magnesium, calcium, and palladium contained in the phosphorus fluoride can be quantified using an inductively coupled plasma mass spectrometer (ICP-MS).
[0035] [Pressure Conditions During Storage] The pressure conditions during storage in the phosphorus fluoride storage method according to this embodiment and the gas-filled storage container according to this embodiment are not particularly limited as long as the phosphorus fluoride can be stored in a sealed state within the storage container, but are preferably 0.15 MPa or more and 15 MPa or less, and more preferably 0.3 MPa or more and 9 MPa or less. If the pressure conditions are within the above range, the phosphorus fluoride can be circulated without heating when the storage container is connected to a dry etching device.
[0036] [Temperature Conditions During Storage] The temperature conditions during storage in the phosphorus fluoride storage method according to this embodiment and the gas-filled storage container according to this embodiment are not particularly limited, but are preferably -20°C or higher and 50°C or lower, and more preferably 0°C or higher and 40°C or lower. If the storage temperature is -20°C or higher, the storage container is less likely to deform, reducing the possibility of the storage container losing its airtightness and allowing oxygen, water, etc. to enter the storage container. If oxygen, water, etc. enters the storage container, the decomposition reaction of phosphorus fluoride may be accelerated. On the other hand, if the storage temperature is 50°C or lower, the complex formation reaction between phosphorus fluoride and nickel, zinc, chromium, molybdenum, and tungsten is less likely to proceed.
[0037] [Etching] The phosphorus fluoride stored in the storage method, storage container, and gas-filled storage container according to the present embodiment can be used as an etching gas. The phosphorus fluoride-containing etching gas stored in the storage method, storage container, and gas-filled storage container according to the present embodiment can be used for both plasma etching using plasma and plasmaless etching not using plasma.
[0038] Examples of plasma etching include reactive ion etching (RIE), inductively coupled plasma (ICP) etching, capacitively coupled plasma (CCP) etching, electron cyclotron resonance (ECR) plasma etching, and microwave plasma etching. In plasma etching, the plasma may be generated in a chamber in which the member to be etched is placed, or the plasma generation chamber and the chamber in which the member to be etched is placed may be separate (i.e., remote plasma may be used).
[0039] The present invention will be explained in more detail below with reference to examples and comparative examples. (Example 1) A seamless container with a capacity of 10 L made of manganese steel was prepared. Its inner surface was shot blasted, acid washed, and washed with water in the order listed, and then dried. A valve was then attached to the dried container to prepare a storage container. The valve was made of SUS316L, which has a total concentration of copper, magnesium, calcium, and palladium of less than 0.005% by mass.
[0040] The storage container was heated to 160°C, and the pressure inside the storage container was reduced to a vacuum using a vacuum pump. The storage container, whose interior was evacuated, was then connected to a gas filling line equipped with a cylinder filled with phosphorus trifluoride. The cylinder filled with phosphorus trifluoride was made of SUS316 stainless steel, in which the total concentration of copper, magnesium, calcium, and palladium was less than 0.005% by mass.
[0041] The phosphorus trifluoride packed in the cylinder was analyzed by gas chromatography and found to have a purity of 99.95% by volume. The phosphorus trifluoride packed in the cylinder was also analyzed by inductively coupled plasma mass spectrometry and found to have a total concentration of copper, magnesium, calcium, and palladium of 3,500 ppb by mass or less.
[0042] Next, the gas filling line was subjected to a purging process in which the inside was filled with nitrogen gas and then the inside was depressurized using a vacuum pump to create a vacuum state. Then, 1 kg of phosphorus trifluoride was sent from the cylinder to the storage container through the purged gas filling line, resulting in a gas-filled storage container in which phosphorus trifluoride was filled. The internal pressure (gauge pressure) of the resulting gas-filled storage container was 2.84 MPaG.
[0043] The gas-filled storage container thus obtained was filled with phosphorus trifluoride and then allowed to stand at 23°C for 30 days, after which the gas phase in the gas-filled storage container was extracted from the upper outlet. The concentrations of metal impurities contained in the extracted phosphorus trifluoride, i.e., the concentrations of nickel, zinc, chromium, molybdenum, and tungsten, were measured using an inductively coupled plasma mass spectrometer. The results are shown in Table 1. The details of the method for measuring the concentrations of nickel, zinc, chromium, molybdenum, and tungsten using an inductively coupled plasma mass spectrometer are as follows.
[0044] While the liquid phase phosphorus trifluoride in the gas-filled storage container was vaporized at -78°C, the phosphorus trifluoride gas was extracted from the gas phase and passed through 100 g of a 1 mol / L aqueous nitric acid solution at a flow rate of 100 mL / min, followed by bubbling. This bubbling brought the phosphorus trifluoride into contact with the aqueous nitric acid solution, causing nickel, zinc, chromium, molybdenum, and tungsten to be absorbed into the aqueous nitric acid solution. The mass of the aqueous nitric acid solution after bubbling was 99 g (M1). The mass difference between the gas-filled storage container before and after bubbling was a decrease of 23 g (M2).
[0045] After bubbling, 10 g of the nitric acid aqueous solution (M3) was collected and diluted to 100 mL (V) with ultrapure water using a measuring flask. The concentrations of various metal atoms (nickel, zinc, chromium, molybdenum, and tungsten) in the diluted nitric acid aqueous solution were measured using an inductively coupled plasma mass spectrometer, and the concentration of various metal atoms in phosphorus trifluoride (C, unit: g / g) was calculated using the measured value (c1, unit: g / mL) and the following formula: C = {(c1 × V) × (M1 / M3)} / M2
[0046]
[0047] After measuring the concentrations of various metal atoms in the phosphorus trifluoride, the phosphorus trifluoride was extracted from the gas-filled storage container, and the storage container from which the phosphorus trifluoride had been extracted was subjected to a purging process in which the inside of the storage container was filled with nitrogen gas and then reduced in pressure using a vacuum pump to create a vacuum state, which was repeated 30 times.
[0048] Next, the purged storage container was cut using a laser cutting machine to obtain square pieces with sides of 2 cm. Using these pieces as measurement samples, X-ray photoelectron spectroscopy was performed on the inner surface of the storage container to measure the concentrations of copper, magnesium, calcium, and palladium in the metal material forming the portion of the storage container that came into contact with the phosphorus fluoride. The results are shown in Table 1.
[0049] The analytical equipment, analytical conditions, and sputtering conditions used in the XPS analysis are as follows: Analytical equipment: X-ray photoelectron spectrometer PHI5000VersaProbeII manufactured by ULVAC-PHI, Inc. Atmosphere: vacuum (1.0 × 10 6 Pa or less) X-ray source: Monochromated Al Ka (1486.6 eV) Spectrometer: Electrostatic concentric hemispherical spectrometer X-ray beam diameter: 100 μm (25 W, 15 kV) Signal acceptance angle: 45.0° Pass energy: 23.5 eV Measurement energy range: Cu2p 933-953 eV Mg2p 50 eV Ca2p 347-351 eV Pd3d 335-340 eV Sputtering ion source: Ar2,500+ Sputtering acceleration voltage: 10 kV Sputtering area: 2 mm x 2 mm Sputtering time: 10 minutes
[0050] (Examples 2 and 3 and Comparative Examples 1 and 2) The same procedures as in Example 1 were carried out, except that the concentrations of copper, magnesium, calcium, and palladium in the manganese steel forming the seamless container used as the storage container were different as shown in Table 1. After leaving the gas-filled storage container at 23°C for 30 days, the metal impurity concentrations of the phosphorus trifluoride gas were measured using an inductively coupled plasma mass spectrometer. The results are shown in Table 1. The concentrations of copper, magnesium, calcium, and palladium in the manganese steel were measured by XPS analysis of the inner surface of the storage container in the same manner as in Example 1.
[0051] (Examples 4, 5, 6 and Comparative Examples 3, 4) The same procedure as in Example 1 was carried out, except that a 10 L seamless container made of chromium-molybdenum steel was fitted with a valve to serve as a storage container. After leaving the container at 23°C for 30 days, the metal impurity concentrations of the phosphorus trifluoride gas in the gas-filled storage container were measured using an inductively coupled plasma mass spectrometer. The results are shown in Table 1. The concentrations of copper, magnesium, calcium, and palladium in the chromium-molybdenum steel were measured by XPS analysis of the inner surface of the storage container in the same manner as in Example 1, and the values obtained are as shown in Table 1.
[0052] (Examples 7 and 8 and Comparative Examples 5 and 6) The same procedures as in Example 1 were carried out, except that the type of phosphorus fluoride filled in the storage container and the seamless container used as the storage container were different as shown in Table 1. After leaving the gas-filled storage container at 23°C for 30 days, the concentrations of metal impurities in the phosphorus pentafluoride gas were measured using an inductively coupled plasma mass spectrometer. The results are shown in Table 1. The concentrations of copper, magnesium, calcium, and palladium in the manganese steel and chromium-molybdenum steel were measured by XPS analysis of the inner surface of the storage container in the same manner as in Example 1.
[0053] As can be seen from the results shown in Table 1, in Examples 1 to 8, the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten after storage at 23°C for 30 days was 500 ppb by mass or less. In contrast, in Comparative Examples 1 to 6, the sum of the concentrations of nickel, zinc, chromium, molybdenum, and tungsten after storage at 23°C for 30 days was 1000 ppb by mass or more. From these results, it is believed that in Comparative Examples 1 to 6, the catalytic action of copper, magnesium, calcium, and palladium caused the metals contained in the metal material forming the storage container to react with phosphorus fluoride to form complexes, resulting in the generation of metal impurities.
Claims
1. A method for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, comprising storing the phosphorus fluoride in a storage container in which a portion with which the phosphorus fluoride comes into contact is formed of a metal material, and the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the metal material is 0.8 mass% or less.
2. The method for storing phosphorus fluoride according to claim 1, wherein the metallic material is at least one of manganese steel and chrome molybdenum steel.
3. A method for storing phosphorus fluoride as described in claim 1 or 2, wherein the concentrations of copper, magnesium, calcium, and palladium contained in the metal material are measured by X-ray photoelectron spectroscopy.
4. A method for storing phosphorus fluoride according to claim 1 or 2, wherein the phosphorus fluoride is stored in the storage container with a purity of 99.90% by volume or more.
5. A storage container for storing phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, wherein a portion that comes into contact with the phosphorus fluoride is formed of a metal material, and the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the metal material is 0.8 mass% or less.
6. A phosphorus fluoride storage container according to claim 5, wherein said metallic material is at least one of manganese steel and chrome molybdenum steel.
7. A gas-filled storage container in which phosphorus fluoride, which is at least one of phosphorus trifluoride, phosphorus pentafluoride, and diphosphorus tetrafluoride, is filled in the storage container, wherein a portion of the storage container that comes into contact with the phosphorus fluoride is formed of a metal material, and the sum of the concentrations of copper, magnesium, calcium, and palladium contained in the metal material is 0.8 mass% or less.
8. The gas-filled storage vessel of claim 7, wherein said metallic material is at least one of manganese steel and chrome-molybdenum steel.
9. A gas-filled storage container as described in claim 7 or 8, wherein the concentrations of copper, magnesium, calcium, and palladium contained in the metal material are measured by X-ray photoelectron spectroscopy.
10. A gas-filled storage container according to claim 7 or 8, wherein the purity of the phosphorus fluoride is 99.90% by volume or more.
Citation Information
Patent Citations
High strength steel and gas storing cylinder made therefrom
JP1985070165A
Safety handling device for gas cylinder
JP1989069900A
Deposition film forming method
JP1989307229A
Corrosion resistant vessel and gas supply system
JP2003500551A
Method for supplying high-pressure gas
JP2012154429A