Method for producing silicon nitride sintered body
The method of producing a silicon nitride sintered body by creating a temporary sintered body with a specific density range for easier processing and subsequent main firing addresses the challenges of achieving high accuracy and yield, resulting in a product with enhanced surface and dimensional precision.
Patent Information
- Application Number
- PCT/JP2024/018194
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-16
- Publication Date
- 2024-12-05
AI Technical Summary
The existing methods for manufacturing silicon nitride sintered bodies face challenges in achieving high dimensional and surface accuracy due to the high hardness of the material, which makes processing difficult, leading to increased manufacturing costs and potential product yield loss, along with issues in suppressing surface irregularities and voids during phase transition.
A method involving the production of a temporary sintered body with a specific density range of 2.5 to 2.9 g/cm³, allowing for easier processing and polishing, followed by main firing to achieve excellent surface and dimensional accuracy, using a green body with 60% or more β-type silicon nitride powder and appropriate sintering aids, and employing specific firing and removal processing techniques.
This approach enhances the workability of the silicon nitride sintered body during processing, reduces damage and distortion, and results in a product with improved surface smoothness and dimensional accuracy, while maintaining high yield and reducing the need for large processing margins.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Method for manufacturing silicon nitride sintered body
[0001] The present invention relates to a novel method for producing a silicon nitride sintered body, and more specifically to a method for producing a silicon nitride sintered body that can reduce the labor required for processing into a desired shape and that can produce a sintered body with high dimensional accuracy.
[0002] In recent years, silicon nitride sintered bodies, which have high strength, high hardness, high thermal conductivity, and high toughness, are used as components for various industrial equipment such as circuit boards for power semiconductors, jigs for semiconductor manufacturing equipment, and bearing balls, due to their characteristics such as resistance to cracking.
[0003] On the other hand, in the manufacturing method of a molded body made of silicon nitride sintered body, since silicon nitride sintered body has high hardness, it takes a long time to process the silicon nitride sintered body into a molded body having the desired shape and dimensions, which becomes a bottleneck and leads to an increase in manufacturing costs.
[0004] Generally, silicon nitride sintered bodies are produced by molding a raw material containing silicon nitride powder, a sintering aid, and a binder into a green body, decomposing and removing (degreasing) the binder from the green body, and then firing the green body.
[0005] Several methods have been proposed to solve the problems associated with processing the sintered body in the above-mentioned manufacturing methods. For example, there is a method for manufacturing a silicon nitride sintered body that serves as a wafer fork, in which a green body is laser-machined into a desired shape, followed by degreasing and firing (see Patent Document 1), a method for manufacturing a silicon nitride sintered body that serves as a ball, in which a green body is polished to approximate a perfect sphere, followed by degreasing and firing (see Patent Document 2), and a method for manufacturing an assembly of sintered bodies consisting of multiple parts, in which a primary molded body for each part is produced by cutting a molded body that has been hardened by reducing the plasticizer content of the green body, and then assembling and firing the individual parts (see Patent Document 3).
[0006] The conventional manufacturing methods described above process pre-sintered green bodies or debound bodies to easily obtain the desired shape. However, due to the low strength of the green bodies and debound bodies, they are prone to breakage during processing, resulting in concerns about reduced product yield. Furthermore, external forces applied during processing can cause dents and uneven density. Furthermore, density variations in the green and debound bodies at the stage of sintering lead to significant distortion during sintering. Therefore, it is difficult to predict such dimensional changes during processing before sintering, and a significant dimensional margin is required after sintering. This necessitates extensive processing to correct for these margins after sintering. Furthermore, when using α-type silicon nitride powder as a raw material, it is difficult to suppress the surface irregularities and voids that occur when the α-phase silicon nitride transforms to the β-phase during sintering.
[0007] JP 6-53303, JP 1-130908, JP 6-116007
[0008] Therefore, an object of the present invention is to provide a manufacturing method that can produce silicon nitride sintered bodies that have a high yield of molded bodies obtained by sintering and that have significantly excellent surface precision, dimensional precision, etc., without sacrificing the processability that is present in the conventional methods.
[0009] The inventors have conducted extensive research to solve the above-mentioned problems, and as a result have found that a pre-sintered body, which is obtained by stopping the firing so that the density falls within a specific range during the firing process to obtain a silicon nitride sintered body, is easy to process and remove by polishing, etc., and has sufficiently high strength during processing, so there is no problem with breakage. Furthermore, when the pre-sintered body is further fired after processing to obtain a sintered body, changes due to subsequent sintering are suppressed, and a silicon nitride sintered body with significantly excellent surface precision, dimensional precision, etc. can be obtained, which has led to the completion of the present invention.
[0010] That is, according to the present invention, a green body containing silicon nitride powder and a sintering aid is formed into a sintered body having a density of 2.5 to 2.9 g / cm 3 The pre-sintered body was then subjected to removal processing and then fired to a density of 3.0 g / cm. 3There is provided a method for producing a silicon nitride sintered body, characterized in that firing is carried out so as to achieve the above (hereinafter also referred to as "main firing").
[0011] In the above manufacturing method, it is particularly advantageous to use β-type silicon nitride powder in an amount of 60 mass % or more of the silicon nitride powder, since this reduces the occurrence of voids due to phase transition.
[0012] According to the manufacturing method of the present invention, by performing removal processing on a pre-sintered body having a specific density, the resulting body has workability comparable to that of the green body used in the conventional method. Furthermore, by performing removal processing on a pre-sintered body having a higher strength than a green body or a degreased body, it is possible to reduce breakage during processing and achieve a high yield. Furthermore, since the pre-sintered body is almost completely sintered, the sintered body obtained by further firing it has an extremely small change rate from the pre-sintered body, making it possible to produce a silicon nitride sintered body with significantly excellent surface smoothness, dimensional accuracy, etc.
[0013] The manufacturing method of the present invention is to form a green body containing silicon nitride powder and a sintering aid into a sintered body having a density of 2.5 to 2.9 g / cm 3 The method is characterized in that a pre-sintered body is obtained by pre-sintering so as to obtain a pre-sintered body, and then the pre-sintered body is subjected to removal processing, and then sintered at a temperature higher than that of the pre-sintering.
[0014] In the present invention, the green body basically contains silicon nitride powder and a sintering aid, and may also contain additives such as a binder to improve the strength of the green body.
[0015] Any known silicon nitride powder may be used without particular limitation, but in order to reduce surface irregularities after the removal process described below, it is preferable to use a powder containing preferably 60 mass % or more, more preferably 80 mass % or more of β-type silicon nitride powder, with the remainder being α-type silicon nitride powder. Whether the silicon nitride powder is β-type or not can be confirmed by X-ray diffraction measurement.
[0016] The silicon nitride powder preferably has an average particle size of 0.4 to 1.6 μm, and more preferably 0.8 to 1.2 μm. The average particle size is the 50% value (D50) on a volume-based cumulative curve showing the particle size distribution measured by a laser diffraction scattering method.
[0017] Furthermore, with regard to metal impurities, Al and Fe are preferably 75 ppm or less, particularly 50 ppm or less, and Ca is preferably 100 ppm or less, particularly 70 ppm or less. The amount of metal impurities can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES) or the like.
[0018] In addition, known sintering aids can be used without any particular restrictions. For example, Al 2 O 3 , MgO, Y 2 O 3 , ZrO 2 These may be used alone or in combination as required, and metals such as titanium, tungsten, molybdenum, etc. or their oxides may be added as colorants.
[0019] Furthermore, any known binder may be used without any particular limitation, and examples thereof include organic polymers (acrylic resins, polyvinyl alcohol, etc.), which may be used alone or in combination as required.
[0020] The amounts of the sintering aid, the binder used as needed, and the colorant used relative to the silicon nitride powder are not particularly limited, and known amounts may be used without any particular restrictions. Specifically, relative to 100 parts by mass of the silicon nitride powder, the sintering aid is preferably 4 to 15 parts by mass, more preferably 6 to 12 parts by mass, the binder is preferably 1 to 30 parts by mass, more preferably 1 to 5 parts by mass, and the colorant is preferably 0 to 3 parts by mass.
[0021] The green body is formed into the shape of the desired sintered body by the removal processing of the pre-sintered body described below, so its shape is not particularly limited. However, in order to reduce the amount of removal processing of the pre-sintered body, it is preferable to form it into a shape similar to the shape of the sintered body. That is, taking into account shrinkage due to sintering, it is preferable to form it into a shape close to the shape of the desired silicon nitride sintered body. Specifically, if the desired silicon nitride sintered body is a plate-like body, it is preferable to form it into a plate-like shape, and if it is a sphere, it is preferable to form it into a sphere or a cube. Furthermore, if a complex shape is desired, it is preferable to form it into a shape such as a cube or rectangular parallelepiped that includes that shape.
[0022] The green body can be formed by any known method without any particular limitation. For example, in the case of a plate-like shape, methods such as a doctor blade method and a T-die method (extrusion molding) can be used, and in the case of a sphere, cube, or rectangular parallelepiped, methods such as press molding and injection molding can be used.
[0023] Furthermore, when an organic substance is used as a binder, the green body is generally degreased. The degreasing conditions can be any known method for decomposing the binder, and are not particularly limited. For example, the binder is decomposed and removed at 500 to 600°C in the presence of oxygen, such as in air. When the green body contains an organic binder, it is preferable to degrease the green body to form a degreased body, and then calcinate it.
[0024] The pre-firing conditions for the green body or degreased body may be any known firing conditions without any particular restrictions. Specifically, the firing is preferably carried out in the presence of nitrogen. The firing temperature during pre-firing is preferably 1400 to 1650°C, and more preferably 1450 to 1550°C, although the appropriate temperature needs to be adjusted depending on the particle size of the raw materials and the amount of auxiliary agents. The pressure may be reduced, normal pressure, or increased pressure, without any particular restrictions.
[0025] The greatest feature of the present invention is that in the above-mentioned calcination, the density of the calcined body is 2.5 to 2.9 g / cm 3 , preferably 2.6 to 2.8 g / cm 3In this state, the firing is interrupted, the pre-sintered body is removed, and the pre-sintered body is subjected to removal processing. That is, if the density of the pre-sintered body is higher than the above range, the removal processing becomes difficult because it takes a long time to process or requires special processing techniques. Also, if the density of the pre-sintered body is lower than the above range, the strength of the pre-sintered body decreases, leading to a decrease in yield during removal processing and large dimensional changes during the subsequent firing, which adversely affects the precision of the resulting sintered body. Furthermore, shavings from the removal processing may adhere firmly to the pre-sintered body, causing poor appearance of the resulting sintered body.
[0026] The pre-sintered body having the above density has a lower Vickers hardness than a sintered body after sintering, but a higher Vickers hardness than a general green body or a degreased body. For example, the Vickers hardness (Hv) measured with an indentation weight of 20 kgf is preferably 800 or less, more preferably about 300 to 600.
[0027] Furthermore, since the pre-sintered body is one in which sintering is almost complete, the sintered body obtained by further firing it will have an extremely small change rate from the pre-sintered body, making it possible to produce a silicon nitride sintered body with significantly excellent surface smoothness, dimensional accuracy, etc.
[0028] In the pre-firing, the means for adjusting the density of the pre-sintered body to fall within the above range is not particularly limited, but it is preferable to confirm the relationship between the density of the sintered body and the sintering temperature and time in advance through experiments, and then remove the pre-sintered body from the firing furnace after firing at a temperature and time that results in the density falling within the above range.
[0029] In the present invention, the removal processing of the pre-sintered body can be performed by any known processing method, such as grinding, cutting, polishing, etc., without any particular limitation. Specifically, known removal processing methods such as surface grinding using a grinding wheel, lapping, polishing, barrel processing, cylindrical grinding, grinder processing, lathe processing using cemented carbide, milling, etc. can be mentioned, and methods suitable for the desired finished shape can be used alone or in combination as appropriate.
[0030] The removal process may be performed by either a dry method or a wet method. For wet removal, the liquid used for the process, such as an abrasive liquid containing abrasive grains, must be easy to clean afterwards, and it is preferable to select a liquid that does not inhibit sintering during the firing process. Specifically, it is preferable to use an aqueous liquid containing little organic matter, specifically a liquid containing less than 60% by mass of organic matter. Furthermore, it is more preferable to use a silicon carbide GC (green carborundum) grinding stone as the grinding stone used for the removal process, as it leaves little abrasive grains and does not inhibit sintering during the firing process.
[0031] Representative embodiments of the removal process are shown below.
[0032] (1) When producing a plate-shaped silicon nitride sintered body: A method in which a plate-shaped body of a predetermined thickness is produced as a pre-sintered body from the target silicon nitride sintered body, taking into consideration the removal processing allowance and the shrinkage allowance due to main firing, and one or both sides of the pre-sintered body are then removed.
[0033] - A method in which a rectangular or cubic block is manufactured as a pre-sintered body, and then the desired silicon nitride sintered body is cut into a plate-like body of a specified thickness by milling, lathe processing, etc., taking into account the removal processing allowance and the shrinkage allowance due to main sintering, and one or both sides are further removed using a grinding stone as necessary.
[0034] (2) When producing a ball-shaped silicon nitride sintered body: A method in which a spherical body of a predetermined size is produced as a pre-sintered body from the target silicon nitride sintered body, taking into consideration the removal processing allowance and the shrinkage allowance due to main firing, and then the pre-sintered body is removed to approximate a perfect sphere.
[0035] - A method in which a rectangular or cubic block is manufactured as a pre-sintered body, and then cut into a spherical body of a specified size using a lathe, taking into account the amount of removal processing and the amount of shrinkage due to firing, and then removing processing is performed using a grinding stone to make it closer to a perfect sphere.
[0036] Furthermore, when producing a plate-shaped silicon nitride sintered body, the above-mentioned removal processing not only allows for adjustment of dimensional accuracy, etc., but also makes it possible to reduce warping of the plate-shaped body by setting a large amount of grinding processing.
[0037] In the present invention, the slag generated by the removal process can be pulverized, re-nitrided, etc., as necessary, and reused as a raw material for the sintered body, thereby improving the utilization rate of the silicon nitride powder.
[0038] In the present invention, the pre-sintered body after the grinding process is further sintered to obtain the desired silicon nitride sintered body. The sintering conditions for the sintering are as follows: the density of the obtained sintered body is 3.0 g / cm 3 More specifically, 3.2 g / cm 3 It is preferable to perform firing so that the density of the sintered body obtained by firing is equal to or greater than 3.5 g / cm. 3 The firing conditions for the main firing may be the same as those for the pre-firing, but in order to increase the density of the resulting sintered body as much as possible, it is preferable to perform firing at a temperature higher than the temperature (firing temperature) used in the pre-firing. Specifically, it is preferable to perform the main firing at a temperature higher than the pre-firing temperature by 5°C or more, preferably by 10°C or more, and at a temperature not exceeding 1800°C, which is the decomposition temperature of silicon nitride under normal pressure, and even in the case of pressurization, it is preferable to perform the main firing at a temperature lower than 1900°C so as to prevent voids from being generated due to evaporation of the sintering aid.
[0039] In the present invention, the silicon nitride sintered body obtained after the main firing may be subjected to removal processing in order to finely adjust the dimensions to the desired size or to further improve the smoothness of the surface.
[0040] Examples will be given below to explain the present invention more specifically, but the present invention is not limited to these examples. As typical examples, two patterns, a plate-like body and a spherical body, will be exemplified.
[0041] Example 1 (Plate) β-type silicon nitride powder (average particle size 0.9 μm) and yttrium oxide powder and aluminum oxide powder as sintering aids were prepared. A water-soluble acrylic binder, a dispersant, and water were added to this raw material powder to prepare a raw material slurry. The mass% of each component when the total of the silicon nitride powder, yttrium oxide powder, and aluminum oxide powder was taken as 100 mass% is shown in the mixed raw material column in Table 1.
[0042] Next, the prepared raw material slurry was granulated by a spray drying method, and the obtained granules were pressure-molded using a mold molding machine to obtain a green body, which was a plate-like body having a length of 20 mm, a width of 20 mm, a thickness of 8 mm, and a density shown in Table 1. The green body was degreased to obtain a degreased body.
[0043] The degreased body was then placed in a firing furnace, the atmosphere in the furnace was replaced with nitrogen gas, and the degreased body was fired at 1520°C for 10 hours under a pressure of approximately 0.8 MPa to obtain a pre-sintered body having the density shown in Table 1.
[0044] The obtained pre-sintered body was subjected to removal processing (grinding processing) only in the thickness direction using a GC grindstone. The target value for the grinding processing was set taking into account the shrinkage rate with respect to the final target thickness of 6.50 mm. Water was used as the grinding processing fluid. The dimensions of the pre-sintered body obtained by removal processing and the time required for removal processing are shown in Table 1.
[0045] After the grinding process, the substrate was subjected to ultrasonic cleaning using pure water to remove grinding powder, and then dried.
[0046] The pre-sintered body was then placed in a sintering furnace, the atmosphere in the furnace was replaced with nitrogen gas, and the temperature was raised to 1850°C under a pressure of approximately 0.8 MPa and maintained for 10 hours to produce a plate-shaped sintered body. The thickness (final target thickness: 6.5 mm) and density of the obtained sintered body are shown in Table 1.
[0047] Furthermore, when the surface of the sintered body was observed under an SEM at 3000 magnifications, no voids of 10 μm or larger were observed on the surface.
[0048] <Examples 2 to 4 (plate-shaped body)> Sintered bodies were produced in the same manner as in Example 1, except that the density of the pre-sintered body was changed by changing the amount of sintering aid and the temperature during pre-sintering as shown in Table 1. The results are shown in Table 1.
[0049] Comparative Example 1 (Plate) A green body was obtained in the same manner as in Example 1, except that the amount of sintering aid was changed as shown in Table 1. The obtained green body was then subjected to the same grinding and cleaning as in Example 1 without being degreased or pre-fired. However, the shape was distorted, and the desired sintered body shape could not be obtained.
[0050] Comparative Example 2 (Plate) A degreased body was obtained in the same manner as in Example 1, except that the amount of sintering aid was changed as shown in Table 1. The obtained degreased body was then ground and washed in the same manner as in Example 1 without being pre-fired. However, the shape was distorted, and the desired sintered body shape could not be obtained.
[0051] Comparative Example 3 (Plate) A sintered body was produced in the same manner as in Example 1, except that the density of the pre-sintered body was changed by adjusting the amount of sintering aid and changing the temperature during pre-sintering, as shown in Table 1. In this example, the target thickness after removal processing was set to 6.58 mm, taking into account the shrinkage rate, but even after 20 hours of grinding processing, the target thickness was 7.18 mm, which was not achieved. The results are shown in Table 1.
[0052] Examples 5 and 6 (spherical bodies) Granules were prepared in the same manner as in Example 1, except that the amount of sintering aid was changed as shown in Table 1. The resulting granules were then pressure-molded using a mold molding machine to form granules with a diameter of 15 mm and a density of 2.2 g / cm. 3 The green bodies were degreased to obtain degreased bodies having the densities shown in Table 1.
[0053] Next, the degreased body was placed in a firing furnace, and after replacing the atmosphere in the firing furnace with nitrogen gas, the body was calcined under the conditions shown in Table 1 to obtain a calcined body. 3 , 2.78 g / cm 3 It was.
[0054] The obtained pre-sintered body was subjected to removal processing (grinding / polishing) on the entire surface using a GC grinding wheel. The grinding / polishing target value was set taking into account the shrinkage rate with respect to the final target diameter of 13.0 mm. Water was used as the grinding / polishing liquid. The dimensions of the pre-sintered body obtained by removal processing and the time required for grinding / polishing are shown in Table 1. After the above grinding / polishing processing, ultrasonic cleaning was performed using pure water to remove grinding / polishing scum, and then the body was dried.
[0055] The pre-sintered body was then placed in a sintering furnace, the atmosphere in the furnace was replaced with nitrogen gas, and the body was then sintered under the conditions shown in Table 1 to produce a spherical sintered body. The density and thickness (final target diameter: 13.0 mm) of the obtained sintered body are shown in Table 1.
[0056] As in this example, after obtaining a pre-sintered body, removal processing is carried out, and then main firing is carried out, making it possible to easily obtain a sintered body close to the target dimensions in a short time.
[0057]
Claims
1. A green body containing silicon nitride powder and a sintering aid is sintered to a density of 2.5 to 2.9 g / cm 3 After the calcination was performed to obtain a calcined body, the calcined body was subjected to a removing process, and then the calcined body was subjected to a removing process to obtain a calcined body having a density of 3.0 g / cm 3 A method for producing a silicon nitride sintered body, comprising the steps of:
2. The method for producing sintered silicon nitride according to claim 1, wherein 60 mass % or more of said silicon nitride powder is β-type silicon nitride powder.
3. A method for producing a silicon nitride sintered body according to claim 1 or 2, wherein the sintering temperature for obtaining the silicon nitride sintered body is higher than the sintering temperature for obtaining the pre-sintered body.
4. The method for producing a silicon nitride sintered body according to claim 1 or 2, wherein the green body contains a binder.
5. A method for producing a silicon nitride sintered body according to claim 4, wherein the green body is degreased to obtain a degreased body, and then fired to obtain the pre-sintered body.
Citation Information
Patent Citations
Efficient precision processing method for manufacturing high-hardness Si3N4 ceramic radome
CN109608204A
Manufacture of ceramic product
JP1984096912A
Manufacture of ceramics sintered body
JP1985011261A
Manufacturing method of ceramic-made micro-precision component
JP2009215141A
Method for manufacturing silicon nitride powder
WO2019167879A1