Austenitic stainless steel and method for producing same
The austenitic stainless steel manufacturing method, involving specific composition and hot rolling processes, addresses the low strength and corrosion issues of existing austenitic stainless steel, achieving high low-temperature strength and corrosion resistance without solution heat treatment, enhancing its suitability for hydrogen storage applications.
Patent Information
- Application Number
- PCT/JP2024/018558
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-20
- Publication Date
- 2024-12-05
AI Technical Summary
Austenitic stainless steel used in storage tanks for hydrogen and liquefied gases has low strength due to solution heat treatment, which increases costs and compromises corrosion resistance, making it unsuitable for large-scale hydrogen storage applications.
Austenitic stainless steel with a specific composition and manufacturing process that includes hot rolling and water cooling, eliminating the need for solution heat treatment, resulting in high low-temperature strength and sufficient corrosion resistance.
The method provides austenitic stainless steel with a yield stress of 1000 MPa at -269°C and excellent corrosion resistance, suitable for extreme low-temperature environments, reducing manufacturing costs and improving structural integrity.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Austenitic stainless steel and its manufacturing method
[0001] The present disclosure relates to austenitic stainless steels and methods for producing the same.
[0002] To achieve carbon neutrality, it is desirable to utilize hydrogen as an energy source. To ensure a stable supply of hydrogen, hydrogen storage tanks are necessary. To achieve a large-scale supply of hydrogen, large storage tanks are required. To realize large storage tanks, improved storage tank strength is required. Austenitic stainless steel is sometimes used as a material for storage tank structures for liquid hydrogen, liquid helium, liquefied gas, etc. However, austenitic stainless steel generally undergoes solution heat treatment to restore corrosion resistance, which poses the issue of low strength. Therefore, high-strength austenitic stainless steel is desired.
[0003] Patent Document 1 discloses an austenitic stainless steel and a method for producing the same, which has a chemical composition, in mass %, of C: 0.005 to 0.07%, Si: 0.1 to 1.2%, Mn: 3.2 to 6.5%, Ni: 9 to 14%, the total of at least one of Cu and Co: 0.005% or more and less than 3%, Cr: 19 to 24%, Mo: 1 to 4%, Nb: 0.05 to 0.4%, N: 0.15 to 0.50%, The austenitic stainless steel contains 0.05% or less Al, 0.03% or less P, 0.002% or less S, 0.02% or less O, 0-0.5% V, 0-0.5% Ti, 0-0.01% B, 0-0.05% Ca, 0-0.05% Mg, 0-0.5% REM, and the balance is Fe and impurities. The amount of Nb analyzed as an electrolytic extraction residue is 0.01-0.3% by mass. Patent Document 1 discloses that this austenitic stainless steel has excellent strength, ductility, and weldability, and discloses, for example, a tensile strength of 690 MPa or more at room temperature. Patent Document 1 also discloses that the strength and ductility of austenitic stainless steel are related to the amount of Nb analyzed as an electrolytic extraction residue, i.e., the amount of Nb-containing precipitates.
[0004] International Publication No. 2017 / 056619
[0005] The austenitic stainless steel described in Patent Document 1 requires a solution heat treatment process in addition to a hot working process as a manufacturing process. Therefore, although the austenitic stainless steel has good corrosion resistance, it does not have sufficient strength in a low-temperature environment (hereinafter referred to as low-temperature strength), which results in high costs.
[0006] The present disclosure has been made in view of the above circumstances, and its object is to provide an austenitic stainless steel that is low cost and has both high low-temperature strength and sufficient corrosion resistance, and a method for producing the same.
[0007] In order to achieve the above object, the austenitic stainless steel and the method for producing the same according to the present disclosure are as follows.
[0008] [1] A component composition containing, in mass%, C: 0.050% or more and 0.100% or less, Si: 0.05% or more and 1.00% or less, Mn: 5.0% or more and 20.0% or less, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% or more and 3.5% or less, Ni: 5.0% or more and 10.0% or less, Cr: 11.0% or more and 20.0% or less, N: 0.05% or more and 0.20% or less, W: 0.05% or more and 0.50% or less, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less, with the balance being Fe and unavoidable impurities; The average crystal grain size is less than 30 μm, and the dislocation density is 1.0×10 14 m -2 or more, and having a microstructure in which the amount of precipitated Cr is less than 1.0 mass %, and mechanical properties in which the yield stress in a tensile test at -269°C is 1000 MPa or more.
[0009] [2] The austenitic stainless steel according to [1] above, wherein the chemical composition further contains, in mass%, one or more elements selected from the group consisting of Mo: 2.0% or less, V: 0.5% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less.
[0010] [3] In mass%, C: 0.050% or more and 0.100% or less, Si: 0.05% or more and 1.00% or less, Mn: 5.0% or more and 20.0% or less, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% or more and 3.5% or less, Ni: 5.0% or more and 10.0% or less, Cr: 11.0% or more and 20.0% or less, N: 0.05% or more and 0.20% or less, W: 0.05% or more and 0.50% or less, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less. and the balance consisting of Fe and unavoidable impurities, to a temperature range of 1000°C or more and 1300°C or less; a hot rolling process of hot rolling the steel material after the heating process; and a cooling process of cooling the steel material after the hot rolling, wherein the hot rolling process includes: (i) a first rolling process of hot rolling the steel material at 950°C or more to a total rolling reduction of 52% or more; and (ii) a second rolling process which is carried out after the first rolling process and involves hot rolling the steel material at less than 900°C for one or more passes, wherein the finish rolling end temperature is 800°C or more; and wherein the cooling process involves water cooling at an average water cooling rate of 10°C / s or more from a cooling start temperature which is in a temperature range of at least a temperature which is 100°C lower than the finish rolling end temperature, to a cooling stop temperature which is in a temperature range of 600°C or less.
[0011] [4] The method for producing an austenitic stainless steel according to [3] above, wherein the chemical composition further contains, in mass%, one or more elements selected from the group consisting of Mo: 2.0% or less, V: 0.5% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less.
[0012] According to the present disclosure, it is possible to provide an austenitic stainless steel that combines high low-temperature strength and sufficient corrosion resistance at low cost, and a method for producing the same.
[0013] An austenitic stainless steel and a method for producing the same according to an embodiment of the present disclosure will be described.
[0014] The austenitic stainless steel according to this embodiment has a component composition containing, in mass%, C: 0.050% or more and 0.100% or less, Si: 0.05% or more and 1.00% or less, Mn: 5.0% or more and 20.0% or less, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% or more and 3.5% or less, Ni: 5.0% or more and 10.0% or less, Cr: 11.0% or more and 20.0% or less, N: 0.05% or more and 0.20% or less, W: 0.05% or more and 0.50% or less, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less, with the balance being Fe and unavoidable impurities. The austenitic stainless steel according to this embodiment has an average grain size of less than 30 μm and a dislocation density of 1.0×10 14 m -2 The austenitic stainless steel according to this embodiment has a microstructure in which the amount of precipitated Cr is less than 1.0 mass %. The austenitic stainless steel according to this embodiment has mechanical properties in which the yield stress in a tensile test at −269° C. is 1000 MPa or more.
[0015] The method for producing an austenitic stainless steel according to this embodiment includes a heating step of heating a steel material having the chemical composition described in the previous paragraph to a temperature range of 1000°C to 1300°C, a hot rolling step of hot-rolling the steel material after the heating step, and a cooling step of cooling the hot-rolled steel material. The hot rolling step includes (i) a first rolling step of hot-rolling the steel material at 950°C or higher to a total reduction of 52% or more, and (ii) a second rolling step, which is performed after the first rolling step, of hot-rolling the steel material at less than 900°C in one or more passes, and the finish rolling end temperature is 800°C or higher. The cooling step involves water cooling at an average water cooling rate of 10°C / s or higher from a cooling start temperature in a temperature range of at least 100°C lower than the finish rolling end temperature to a cooling stop temperature in a temperature range of at most 600°C.
[0016] The austenitic stainless steel according to this embodiment can be manufactured at low cost because it does not require a solution heat treatment step in its manufacturing process. Furthermore, in this embodiment, by optimizing the manufacturing conditions, such as adopting a predetermined chemical composition and adopting a predetermined slab heating temperature and hot rolling conditions without performing solution heat treatment, a structure with a predetermined average grain size and dislocation density can be obtained, thereby achieving high low-temperature strength. Furthermore, in this embodiment, by optimizing the manufacturing conditions, such as adopting a predetermined C content and Cr content and adopting a predetermined finish rolling end temperature and water cooling conditions, sufficient corrosion resistance can be ensured without performing solution heat treatment.
[0017] The austenitic stainless steel and the method for producing the same according to this embodiment will be described in detail below.
[0018] The austenitic stainless steel according to this embodiment is particularly suitable as a structural steel for use in extremely low temperature environments, such as tanks for storing liquid hydrogen, liquid helium, liquefied gases, and the like.
[0019] The chemical composition of the austenitic stainless steel according to this embodiment will be described. The austenitic stainless steel according to this embodiment has the chemical composition described above. As described above, the steel material used to manufacture the austenitic stainless steel according to this embodiment also has the same chemical composition as the austenitic stainless steel according to this embodiment.
[0020] In the following description, the designation "%" regarding the chemical composition means "mass %" unless otherwise specified. Hereinafter, austenitic stainless steels and steel materials used in the production thereof will be collectively referred to simply as steel materials.
[0021] The C content in the steel material is 0.050% or more and 0.100% or less. C is an inexpensive austenite stabilizing element and is an important element for obtaining austenite. C also has the effect of dissolving in steel to strengthen the steel material through solid solution strengthening. To fully obtain this effect, the steel material contains 0.050% or more of C. If the steel material contains more than 0.100% of C, excessive Cr precipitates are formed, reducing the corrosion resistance of the steel material. The C content in the steel material is preferably 0.060% or more and preferably 0.090% or less.
[0022] The Si content in the steel material is 0.05% or more and 1.00% or less. Si not only acts as a deoxidizer and is necessary for steelmaking, but also has the effect of dissolving in steel to strengthen the steel material through solid solution strengthening. To achieve this effect, the steel material contains 0.05% or more Si. If the steel material contains more than 1.00% Si, non-thermal stress increases excessively, resulting in a deterioration in the low-temperature toughness of the steel material. The Si content in the steel material is preferably 0.07% or more and preferably 0.80% or less.
[0023] The Mn content in the steel material is 5.0% or more and 20.0% or less. Mn is an inexpensive austenite stabilizing element and is an important element for obtaining austenite. It also has the effect of dissolving in steel to strengthen the steel material through solid solution strengthening. To fully obtain this effect, the steel material contains 5.0% or more Mn. If the steel material contains more than 20.0% Mn, manufacturability and cuttability may deteriorate. The Mn content in the steel material is preferably 6.0% or more and preferably 19.0% or less.
[0024] The P content in the steel material is 0.030% or less. If the P content in the steel material exceeds 0.030%, the hot ductility of the steel material may decrease, which may result in an increase in intergranular cracking. For this reason, it is desirable to reduce the P content in the steel material as much as possible. The P content in the steel material is preferably 0.028% or less. Note that an excessive reduction in P content increases refining costs and is economically disadvantageous, so the P content in the steel material is preferably 0.002% or more.
[0025] The S content in the steel material is 0.0050% or less. If the S content in the steel material exceeds 0.0050%, the hot ductility of the steel material may decrease, which may result in an increase in intergranular cracking. For this reason, it is desirable to reduce the S content in the steel material as much as possible. The S content in the steel material is preferably 0.0045% or less. Note that excessive reduction of S content increases refining costs and is economically disadvantageous, so the S content in the steel material is preferably 0.0010% or more.
[0026] The Al content in the steel material is 0.070% or less. Al acts as a deoxidizer and is most commonly used in the molten steel deoxidation process. To obtain this effect, the steel material preferably contains 0.010% or more Al. If the steel material contains more than 0.070% Al, the hot ductility of the steel material may decrease, which may increase the occurrence of intergranular cracking. The Al content in the steel material is preferably 0.060% or less.
[0027] The Cu content in the steel material is 1.5% or more and 3.5% or less, and the Ni content is 5.0% or more and 10.0% or less. Cu and Ni are austenite-stabilizing elements and are important elements for obtaining austenite, and also increase the strength of the steel material through solid solution strengthening. To fully obtain these effects, the steel material contains 1.5% or more of Cu and 5.0% or more of Ni. If the steel material contains excessive amounts of these elements, the surface quality may deteriorate during rolling of the steel material and the manufacturing cost may be increased. Therefore, the Cu content in the steel material is 3.5% or less and the Ni content is 10.0% or less. Preferably, the Cu content in the steel material is 2.0% or more and 3.0% or less. Also, preferably, the Ni content in the steel material is 6.0% or more and 9.0% or less.
[0028] The Cr content in the steel material is 11.0% or more and 20.0% or less. Cr is an element necessary for ensuring the corrosion resistance of stainless steel. To achieve this effect, the steel material contains 11.0% or more of Cr. If the steel material contains Cr more than 20.0%, excessive Cr precipitates are formed, reducing the corrosion resistance of the steel material. The Cr content in the steel material is preferably 12.0% or more and preferably 19.0% or less.
[0029] The N content in the steel material is 0.05% or more and 0.20% or less. N is an inexpensive austenite stabilizing element. N is an important element for obtaining austenite, and also has the effect of dissolving in steel and strengthening the steel material through solid solution strengthening. To achieve this effect, the steel material contains 0.05% or more N. If the steel material contains more than 0.20% N, the nitrides or carbonitrides in the steel material may become coarse, and the low-temperature toughness of the steel material may decrease. The N content in the steel material is preferably 0.06% or more and preferably 0.19% or less.
[0030] The W content in the steel material is 0.05% or more and 0.50% or less. W contributes to improving the strength of the steel material and also contributes to improving the corrosion resistance of the steel material. To achieve these effects, the steel material contains 0.05% or more of W. If the steel material contains W in excess of 0.50%, the manufacturing cost of the steel material will be increased. The W content in the steel material is preferably 0.10% or more and preferably 0.40% or less.
[0031] The O content in the steel material is 0.0050% or less. O forms oxides, which deteriorates the low-temperature toughness of the steel material. The O content in the steel material is preferably 0.0045% or less. Note that excessive reduction of O increases the refining cost and is economically disadvantageous, so the O content in the steel material is preferably 0.0010% or more.
[0032] The Ti content in the steel material is 0.005% or less, and the Nb content is 0.005% or less. Ti and Nb form high-melting point carbonitrides in the steel material, which may reduce the low-temperature toughness of the steel material. Ti and Nb are components mixed in from raw materials, etc. Generally, the Ti content is mixed into the steel material in the range of more than 0.005% to 0.010%, and the Nb content is mixed into the steel material in the range of more than 0.005% to 0.010%. Therefore, it is necessary to avoid the mixing of Ti and Nb into the steel material and to limit the Ti and Nb contents to 0.005% or less, respectively, according to the melting method described below. By limiting the Ti and Nb contents in the steel material to 0.005% or less, respectively, the adverse effects of the carbonitrides can be eliminated, and excellent low-temperature toughness and ductility can be ensured in the steel material. The Ti content in the steel material is preferably 0.003% or less. In addition, the Nb content in the steel material is preferably 0.003% or less. Of course, the Ti and Nb contents in the steel material may be 0.000% or 0.001% or more.
[0033] The steel material in this embodiment is composed of iron (Fe) and inevitable impurities other than the above-mentioned components. Examples of inevitable impurities include H and B, and a total content of each element of 0.01% or less is acceptable. In this embodiment, inevitable impurities refer to impurities that are inevitably mixed in from raw materials, manufacturing processes, manufacturing equipment, etc., and are acceptable to be present within a range that does not impair the objectives of the present invention. Examples of raw materials include iron ore, reduced iron, and scrap.
[0034] The steel material in this embodiment may contain the elements described below as optional components as necessary.
[0035] The Mo content in the steel material may be 2.0% or less. The V content in the steel material may be 0.5% or less. Mo and V contribute to stabilizing austenite and improving the strength of the steel material. To achieve these effects, the steel material preferably contains Mo and V in an amount of 0.1% or more each. If the steel material contains Mo and V in an amount exceeding 2.0% and 0.5%, respectively, the manufacturing cost may be increased.
[0036] The Ca content in the steel material may be 0.0100% or less. The Mg content in the steel material may be 0.0100% or less. The REM (rare earth metal) content in the steel material may be 0.0200% or less. Ca, Mg, and REM are elements useful for controlling the morphology of inclusions. Controlling the morphology of inclusions means converting elongated sulfide-based inclusions into granular inclusions. Through this control of the morphology of inclusions, the ductility, low-temperature toughness, and sulfide stress corrosion cracking resistance of the steel material are improved. To achieve these effects, the steel material preferably contains 0.0005% or more of Ca and Mg and 0.0010% or more of REM. If the steel material contains excessive amounts of these elements, the amount of non-metallic inclusions may increase, which may actually reduce the ductility, low-temperature toughness, or sulfide stress corrosion cracking resistance of the steel material. This may also be economically disadvantageous. It is preferable that the Ca content be 0.0080% or less, the Mg content be 0.0080% or less, and the REM content be 0.0150% or less.
[0037] Next, the microstructure of the austenitic stainless steel according to this embodiment will be described.
[0038] The austenitic stainless steel according to this embodiment has an average grain size of less than 30 μm and a dislocation density of 1.0×10 14 m -2 When the grain size of the austenitic stainless steel is coarse and / or the dislocation density is low, the yield stress of the steel becomes insufficient. The average grain size is set to be less than 30 μm and the dislocation density is set to be less than 1.0 × 10 14 m -2 This is a necessary condition for achieving excellent low-temperature strength with a yield stress of 1000 MPa or more in a tensile test at −269° C. Keeping the amount of precipitated Cr below 1.0 mass % is a necessary condition for ensuring sufficient corrosion resistance.
[0039] The average grain size of the austenitic stainless steel according to this embodiment is preferably 27 μm or less, and more preferably 25 μm or less. There is no particular lower limit for the average grain size of the austenitic stainless steel according to this embodiment. To improve the toughness of the austenitic stainless steel according to this embodiment, the average grain size is preferably 18 μm or more, and more preferably 20 μm or more. The average grain size of the austenitic stainless steel according to this embodiment is a value measured by the method described in the examples below.
[0040] The dislocation density of the austenitic stainless steel according to this embodiment is preferably 2.0 × 10 14 m -2 More preferably, 3.0 × 10 14 m -2 That is all. The upper limit of the dislocation density of the austenitic stainless steel according to this embodiment is not particularly specified. In order to improve the toughness of the austenitic stainless steel according to this embodiment, the dislocation density should be 9.0 × 10 14 m -2 Preferably, the following is 8.0 x 10 14 m -2 The following is more preferable: The dislocation density of the austenitic stainless steel according to this embodiment is a value measured by the method described in the examples below.
[0041] The amount of precipitated Cr in the austenitic stainless steel according to this embodiment is preferably 0.8 mass% or less, and more preferably 0.5 mass% or less. The lower limit of the amount of precipitated Cr in the austenitic stainless steel according to this embodiment is not particularly specified, and the lower the better, and it can be 0.0 mass%. The amount of precipitated Cr in the austenitic stainless steel according to this embodiment is a value measured by the method described in the examples below.
[0042] In this embodiment, the average grain size and dislocation density of the austenitic stainless steel according to this embodiment can be controlled within the above-mentioned numerical ranges by heating and hot-rolling the steel material according to the conditions described below, and not performing a solution heat treatment, and as a result, the austenitic stainless steel according to this embodiment can achieve the above-mentioned low-temperature strength.
[0043] In this embodiment, the austenitic stainless steel may be a steel plate having a thickness of 10 mm or more. When the austenitic stainless steel according to this embodiment is a steel plate, the thickness of the steel plate is preferably 12 mm or more from the viewpoint of suitable use as a structural steel material used in extremely low-temperature environments. The upper limit of the thickness of the steel plate is not particularly limited and can be any thickness, but it is preferably 30 mm or less.
[0044] Next, an example of a method for producing the austenitic stainless steel according to this embodiment will be described.
[0045] First, molten steel having the above-mentioned composition is obtained by melting using a known melting method such as a converter or an electric furnace, etc. Secondary refining may also be carried out in a vacuum degassing furnace.
[0046] When obtaining the austenitic stainless steel according to this embodiment, in order to limit the contents of Ti and Nb, which hinder structural control, to the above-mentioned numerical ranges, it is necessary to take measures to prevent Ti and Nb from being mixed in raw materials as much as possible and to reduce their contents. For example, the basicity of the slag in the refining stage may be reduced to concentrate these alloys in the slag and discharge them, thereby reducing the concentrations of Ti and Nb in the slab product. Alternatively, oxygen may be blown into the molten steel to oxidize it, and the Ti and Nb alloy may be floated and separated during reflux.
[0047] Thereafter, it is preferable to produce a steel material such as a slab of a predetermined size by a known casting method such as a continuous casting method or an ingot-making and blooming rolling method.
[0048] The method for producing austenitic stainless steel according to this embodiment will be described in detail below.
[0049] In the method for producing austenitic stainless steel according to this embodiment, the heating step, the hot rolling step, and the cooling step are carried out as described above.
[0050] In the following description, unless otherwise specified, the temperature indicated in "°C" refers to the surface temperature of the steel material or steel plate (austenitic stainless steel). In each process described below, the temperature is controlled based on the surface temperature of the steel material or steel plate. The surface temperature can be measured, for example, with a radiation thermometer.
[0051] In the heating step, the steel material is heated to 1000°C or higher and 1300°C or lower. If the heating temperature of the steel material is lower than 1000°C, it may not be possible to achieve a total reduction of 52% or higher at 950°C or higher in the hot rolling step described below. If the heating temperature of the steel material exceeds 1300°C, the crystal grains may become excessively coarse, and high yield stress may not be obtained after the steel material is made into an austenitic stainless steel. The heating temperature of the steel material is preferably 1130°C or higher and 1270°C or lower.
[0052] The hot rolling process includes a first rolling process and a second rolling process that is performed after the first rolling process.
[0053] In the first rolling step, the steel material after the heating step is hot-rolled at 950°C or higher. In the first rolling step, the total reduction is set to 52% or higher. As described above, in the present disclosure, it is important to maintain an average grain size of less than 30 μm in the microstructure of the austenitic stainless steel. If the structure of the steel material cannot be made equiaxed in the first rolling step, i.e., rolling in the recrystallization region, the coarse grains will remain in the subsequent rolling (second rolling step). Therefore, in the first rolling step, it is effective to ensure a total reduction of 52% or higher in the temperature range of 950°C or higher, which is the recrystallization region. In the first rolling step, the total reduction is preferably 55% or higher. The upper limit of the temperature of the steel material in the first rolling step is not particularly limited, but the temperature can be 1300°C or lower. The upper limit of the total reduction in the first rolling step, i.e., in the recrystallization region, is not limited. However, in order to ensure the strength of the austenitic stainless steel, the total reduction in the first rolling step is preferably 80% or less, and more preferably 70% or less.
[0054] In the second rolling step, the steel material is hot-rolled at a temperature of less than 900°C for one or more passes. The finish rolling temperature is set to be 800°C or higher. That is, the hot rolling of the steel material in the second rolling step is performed at a temperature of 800°C or higher and lower than 900°C.
[0055] In the second rolling step, in order to refine the equiaxed grains formed in the steel material in the first rolling step, it is important to perform one or more hot rolling passes at temperatures below 900°C, which is the non-recrystallized region. The number of hot rolling passes in the second rolling step, i.e., at temperatures below 900°C, is preferably two or more. There is no particular upper limit on the number of hot rolling passes below 900°C, but from the viewpoint of preventing the finish rolling end temperature from decreasing excessively, the number of passes is preferably five or less.
[0056] If hot rolling is performed at a temperature below 800°C in the second rolling step, precipitated Cr is generated, reducing the corrosion resistance of the austenitic stainless steel, so the finish rolling temperature in the second rolling step is set to 800°C or higher. The finish rolling temperature (the temperature of the steel material at the last rolling pass in the second rolling step) is preferably 820°C or higher. The finish rolling temperature is lower than 900°C.
[0057] The cooling step is performed after the second rolling step. In the cooling step, the steel material is water-cooled. In the cooling step, the steel material is water-cooled at an average water-cooling rate of 10°C / s or more from a cooling start temperature in a temperature range equal to or higher than a temperature 100°C lower than the finish rolling end temperature (finish rolling end temperature -100°C) to a cooling stop temperature in a temperature range equal to or lower than 600°C. This suppresses the generation of precipitated Cr, and sufficient corrosion resistance can be ensured without performing solution heat treatment. The upper limit of the cooling start temperature is not particularly limited, but the cooling start temperature can be 870°C or less. The lower limit of the cooling stop temperature is not particularly limited, but the cooling stop temperature can be 250°C or more. The upper limit of the average water-cooling rate is not particularly limited, but the average water-cooling rate can be 40°C / s or less.
[0058] In the method for producing austenitic stainless steel according to this embodiment, no solution heat treatment is performed after the cooling step. Solution heat treatment for austenitic stainless steel involves heating the austenitic stainless steel, in which precipitated Cr has formed, to 1000 to 1100°C, maintaining the temperature until a single-phase austenite structure is formed, and then rapidly cooling the stainless steel in water, thereby resolving the precipitated Cr and restoring corrosion resistance.
[0059] In this manner, an austenitic stainless steel and a method for producing the same can be provided.
[0060] The present disclosure will be described below based on examples. Note that the following examples are preferred examples of the present disclosure, and the present disclosure is not limited to these examples.
[0061] Steel slabs (Steel Nos. 1 to 22) having the chemical compositions shown in Table 1 were produced using a converter-ladle refining (secondary refining)-continuous casting process. The symbol "-" in Table 1 indicates that a component is not intentionally added, and includes not only cases where the component is not contained (0%) but also cases where the component is inevitably contained. In Table 1, Steel Nos. 1 to 10, 21, and 22 have the chemical compositions according to this embodiment. The steel slabs were then heated and hot-rolled under the conditions shown in Table 2 (see "Steel Plate Manufacturing Method" in Table 2), followed by water cooling, to produce austenitic stainless steel plates (Sample Nos. 1 to 31) having thicknesses of 10 to 30 mm. Sample No. 29 underwent solution heat treatment at 1010°C after water cooling. In Table 2, the steel plates of Samples 1 to 10, 30, and 31 are austenitic stainless steels according to the invention that satisfy the ranges of this embodiment. In Tables 1 and 2, underlined values indicate that the values are outside the range defined in this embodiment.
[0062]
[0063]
[0064] The obtained steel sheets were evaluated in the following manner.
[0065] (1) The crystal grain size was determined as follows.
[0066] The cross section of the obtained hot-rolled steel sheet perpendicular to the sheet width direction was polished and etched, and the electron backscatter diffraction (EBSD) pattern was measured in a scanning electron microscope (SEM) at the center position of the sheet thickness. The measurement area was 1 mm x 1 mm. The measured EBSD data was analyzed using OIM-Analysis to determine the average crystal grain size (μm). These average crystal grain sizes are also shown in Table 2.
[0067] (2) The dislocation density was determined as follows.
[0068] For the obtained hot-rolled steel sheets, a sample of 10 mm length × 10 mm width × 1.0 mm thickness was taken from the center position of the sheet thickness, mirror polished, and electrolytically polished, and then a diffraction pattern was obtained using an X-ray diffraction device, and dislocation density analysis was performed. The dislocation densities obtained thereby are also shown in Table 2.
[0069] (3) The amount of precipitated Cr was determined as follows.
[0070] For the obtained hot-rolled steel sheets, samples for electrolytic extraction were taken from the center position of the sheet thickness, and the precipitates extracted by electrolytic extraction using a 10% AA (10% acetylacetone-1% tetramethylammonium chloride-methanol) solution were measured for the Cr content in the precipitates by ICP atomic emission spectrometry. These precipitated Cr contents are also shown in Table 2.
[0071] (4) Low temperature strength was evaluated as follows.
[0072] From each of the obtained steel plates, JIS No. 4 tensile test pieces were taken from steel plates having a thickness exceeding 15 mm (except for sample Nos. 5, 7, 18, and 31), and a tensile test was carried out at −269° C. to determine the yield stress.
[0073] For the steel plates of Sample Nos. 5, 7, 18, and 31, which had a plate thickness of 15 mm or less, round bar tensile test specimens having a parallel portion diameter of 6 mm and a gauge length of 25 mm were taken and subjected to a tensile test at −269°C to determine the yield stress. Note that the temperature at which the tensile test was performed in this example (−269°C) corresponds to the boiling point of liquid helium.
[0074] The yield stress at −269°C determined as described above is also shown in Table 2. When the yield stress is 1000 MPa or more, it is determined that the target performance is satisfied and the low-temperature strength is excellent. That is, in this embodiment, excellent low-temperature strength means that the yield stress is 1000 MPa or more in an environment of −269°C, which is the boiling point of liquid helium.
[0075] (5) Corrosion resistance was evaluated as follows.
[0076] A corrosion resistance test was carried out in accordance with the Slow Strain Rate Test Method (hereinafter referred to as the SSRT test) of NACE Standard TM0111-2011. Specifically, Type A notched round bar test specimens were used, and the specimens were immersed in artificial seawater (chloride ion concentration: 18,000 ppm) at a temperature of 23°C under a strain rate of 4 × 10. -7 A constant velocity tensile test was carried out at 1000 kJ / s. Here, a specimen with a breaking stress of 600 MPa or more was judged to have excellent corrosion resistance and satisfy the target performance, and was judged to be "good." A specimen with a breaking stress of less than 600 MPa was judged to have poor corrosion resistance and not satisfy the target performance, and was judged to be "poor." The results of the corrosion resistance evaluations as described above are also shown in Table 2.
[0077] As shown in Table 2, the austenitic stainless steel according to this embodiment (samples Nos. 1 to 10, 30, and 31) has an average crystal grain size in the microstructure of less than 30 μm and a dislocation density of 1.0×10 14 m -2 or more, and the amount of precipitated Cr is less than 1.0 mass %.
[0078] In these austenitic stainless steels according to this embodiment, the yield stress in the tensile test at −269° C. was 1000 MPa or more, satisfying the target performance.
[0079] Furthermore, the austenitic stainless steel according to this embodiment also had good corrosion resistance and satisfied the target performance.
[0080] In contrast, the steel sheets of Samples No. 11 to 29, which are outside the scope of the present disclosure, could not satisfy the above target performance regardless of the values of the average grain size, dislocation density, and amount of precipitated Cr.
[0081] As shown in the above examples, the austenitic stainless steel according to this embodiment can be produced at low cost because it does not require a solution heat treatment step in its production process. Furthermore, the austenitic stainless steel according to this embodiment has high strength and excellent corrosion resistance in low-temperature environments. Therefore, the austenitic stainless steel according to this embodiment can be suitably used as a material for steel structures (such as tanks for liquefied gas storage) used in low-temperature environments. This can significantly contribute to improving the safety and lifespan of such steel structures. Furthermore, the method for producing the austenitic stainless steel according to this embodiment is economical because it does not result in a decrease in productivity or an increase in production costs.
[0082] It should be noted that the embodiments disclosed in this specification are merely examples, and the embodiments of the present disclosure are not limited to these, and can be modified as appropriate within the scope of the purpose of the present disclosure.
[0083] The present disclosure is applicable to austenitic stainless steels and methods for making same.
Claims
1. A component composition containing, by mass%, C: 0.050% to 0.100%, Si: 0.05% to 1.00%, Mn: 5.0% to 20.0%, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% to 3.5%, Ni: 5.0% to 10.0%, Cr: 11.0% to 20.0%, N: 0.05% to 0.20%, W: 0.05% to 0.50%, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less, with the balance being Fe and unavoidable impurities; The average grain size is less than 30 μm, and the dislocation density is less than 1.0×10 14 m -2 or more, and having a microstructure in which the amount of precipitated Cr is less than 1.0 mass %, and mechanical properties in which the yield stress in a tensile test at -269°C is 1000 MPa or more.
2. The austenitic stainless steel according to claim 1, wherein the chemical composition further contains, in mass percent, one or more elements selected from the group consisting of Mo: 2.0% or less, V: 0.5% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less.
3. In mass%, C: 0.050% or more and 0.100% or less, Si: 0.05% or more and 1.00% or less, Mn: 5.0% or more and 20.0% or less, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% or more and 3.5% or less, Ni: 5.0% or more and 10.0% or less, Cr: 11.0% or more and 20.0% or less, N: 0.05% or more and 0.20% or less, W: 0.05% or more and 0.50% or less, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less. and the balance consisting of Fe and unavoidable impurities, a heating step of heating a steel material having a composition comprising: a steel material with a composition of 1,000°C or more and 1,300°C or less; a hot rolling step of hot rolling the steel material after the heating step; and a cooling step of cooling the steel material after the hot rolling, wherein the hot rolling step includes: (i) a first rolling step of hot rolling the steel material at 950°C or more to a total rolling reduction of 52% or more; and (ii) a second rolling step which is performed after the first rolling step and which performs one or more passes of hot rolling the steel material at less than 900°C, wherein a finish rolling end temperature is 800°C or more, and the cooling step includes water cooling at an average water cooling rate of 10°C / s or more from a cooling start temperature which is in a temperature range of 100°C lower than the finish rolling end temperature to a cooling stop temperature which is in a temperature range of 600°C or less.
4. A method for producing an austenitic stainless steel as described in claim 3, wherein the chemical composition further contains, in mass percent, one or more selected from the group consisting of Mo: 2.0% or less, V: 0.5% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less.
Citation Information
Patent Citations
Austenitic stainless steels plate having high strength and high toughness at very low temperature
JP1986270356A
Production of high mn non-magnetic steel plate excellent in toughness at low temperature
JP1994293920A
HIGH Mn STEEL MATERIAL FOR CRYOGENIC USE
JP2016196703A
Austenitic alloy for cryogenic applications
WO2010013083A1
Steel, and method for producing same
WO2021033693A1
Cited By
High-corrosion-resistance and high-ductility stainless steel and preparation method thereof
CN120330600A
Nanometer composite precipitation strengthening austenite superhard steel and preparation method thereof