Crystallized glass, heavy metal recovery material, soil modifier, crystallized glass manufacturing method, and heavy metal recovery method

Crystallized glass with magnetic crystals addresses soil contamination by efficiently adsorbing and recovering heavy metals from agricultural soils, offering a simple and cost-effective solution for soil remediation and reducing health risks.

WO2024247814A1PCT designated stage expired Publication Date: 2024-12-05NIPPON ELECTRIC GLASS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018651
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-21
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional agriculture faces challenges in managing soil contamination with heavy metals and organic substances, particularly phosphorus from fertilizers, which can lead to accumulation of heavy metals in agricultural soils and potential health risks, necessitating an efficient method for heavy metal recovery.

Method used

Development of crystallized glass containing 20-80% magnetic crystals, specifically Fe2O3, which acts as a heavy metal recovery material by adsorbing and magnetically collecting heavy metals from soil, utilizing a method that includes a melting step and crystallization process to form the glass.

Benefits of technology

The crystallized glass effectively recovers heavy metals through adsorption and magnetic collection, providing a simple and cost-effective solution for soil remediation, reducing the risk of heavy metal accumulation in the food chain and improving soil health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure 00000031_0000
    Figure 00000031_0000
Patent Text Reader

Abstract

Provided are crystallized glass from which heavy metal, etc. can be recovered using a simple method, a heavy metal recovery material, a soil modifier, a crystallized glass manufacturing method, and a heavy metal recovery method. The crystallized glass contains 20-80 mass% of Fe2O3 and includes magnetic crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Crystallized glass, heavy metal recovery material, soil conditioner, method for producing crystallized glass, and method for recovering heavy metals

[0001] The present invention relates to crystallized glass, a heavy metal recovery material, a soil conditioner, a method for producing crystallized glass, and a method for recovering heavy metals.

[0002] There are concerns that food supply will not be able to keep up with the growing food demand caused by global population growth. Vertical farming and urban farming mainly produce leafy vegetables, and they do not have the production volume or variety to meet the nutritional needs of the global population. Therefore, it can be said that we will have no choice but to rely on existing conventional agriculture to meet future population growth and expanding food demand.

[0003] One of the problems facing conventional agriculture is the contamination of agricultural soil with heavy metals and certain organic substances. For example, contaminants can be introduced from agricultural fertilizers, such as phosphorus. Phosphorus is an important nutrient, counted among the three major nutrients for agricultural crops, and it is expected that in order to meet demand from various industries, phosphorus sources with relatively high heavy metal contents will have to be used. Furthermore, while various countries have been researching and developing methods for recovering phosphorus from sewage sludge and other sources, there is a problem in that even this recycled phosphorus often contains large amounts of residual heavy metals. Therefore, regardless of the phosphorus source used, heavy metals are expected to accumulate in agricultural soil, raising concerns about the resulting increase in the amount of heavy metals accumulated in the human body and the risk of various diseases, such as kidney damage.

[0004] Against this background, methods for recovering heavy metals from phosphorus raw materials and agricultural soil have been investigated (for example, Reference 1).

[0005] JP 2012-188492 A

[0006] Although the cited document 1 considers sheet-shaped recovery materials, it does not consider a recovery method for the sheet-shaped recovery materials themselves. In order to meet the global need for heavy metal recovery, a heavy metal recovery method that takes into account the cost of the entire recovery process is required.

[0007] In view of the above, an object of the present invention is to provide crystallized glass capable of recovering heavy metals and the like in a simple manner, a heavy metal recovery material, a soil improver, a method for producing crystallized glass, and a method for recovering heavy metals.

[0008] The following describes various aspects of providing crystallized glass, a heavy metal recovery material, a soil improver, a method for producing crystallized glass, and a method for recovering heavy metals that solve the above problems.

[0009] The crystallized glass of embodiment 1 contains, in mass %, Fe 2 O 3 It contains 20 to 80% of magnetic crystals.

[0010] The crystallized glass of embodiment 2 is the same as embodiment 1, except that the crystallized glass contains, in mass %, SiO 2 0-80%, Al 2 O 3 0-80%, B 2 O 3 0-80%, P 2 O 5 0-80%, Li 2 O 0-50%, Na 2 O 0-50%, K 2 O 0-50%, MgO 0-50%, CaO 0-50%, SrO 0-50%, BaO 0-50%, ZnO 0-50%, ZrO 2 0-50%, HfO 2 0-50%, TiO 2 0-50% SnO 2 0-50%, V 2 O 5 0-50%, NiO 0-80%, Cr 2 O 3 0-80%, MoO 3 It is preferable that the content is 0 to 80%.

[0011] The crystallized glass of embodiment 3 is the same as embodiment 1 or embodiment 2, except that, in mass %, SnO 2 +Fe 2 O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3It is preferable that the content of SnO is 20% or more. 2 +Fe 2 O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3 " is SnO 2 , Fe 2 O 3 , V 2 O 5 , NiO, Cr 2 O 3 and MoO 3 It means the total amount of the contents of

[0012] The crystallized glass of Aspect 4 is any one of Aspects 1 to 3, wherein, in mass %, K 2 O / (Li 2 O + Na 2 O+K 2 O) is preferably 0.01 to 0.99. 2 O / (Li 2 O + Na 2 O+K 2 O) is K 2 The content of O is Li 2 O, Na 2 O and K 2 It means the value obtained by dividing the total content of O by the total content of O.

[0013] The crystallized glass of Aspect 5 is any one of Aspects 1 to 4, wherein, in mass %, (SiO 2 +P 2 O 5 ) / (SiO 2 +Al 2 O 3 +P 2 O 5 ) is preferably 0.01 to 0.99. 2 +P 2 O 5 ) / (SiO 2 +Al 2 O 3 +P 2 O 5 ) is SiO 2 and P 2 O 5The total content of SiO 2 , Al 2 O 3 and P 2 O 5 The value is calculated by dividing the total content of the above by the total content of the above.

[0014] The crystallized glass of Aspect 6 is any one of Aspects 1 to 5, wherein, in mass %, SiO 2 / (B 2 O 3 +P 2 O 5 + ZrO 2 +HfO 2 + TiO 2 + SnO 2 ) is preferably 0.1 to 10,000. 2 / (B 2 O 3 +P 2 O 5 + ZrO 2 +HfO 2 + TiO 2 + SnO 2 ) is SiO 2 The content of B 2 O 3 , P 2 O 5 , ZrO 2 , HfO 2 , TiO 2 and SnO 2 The value is calculated by dividing the total content of the above by the total amount of the above.

[0015] The crystallized glass of Aspect 7 is any one of Aspects 1 to 6, wherein, in mass %, SiO 2 It is preferable that the ratio of MgO to CaO is 0.1 to 10,000. 2 / (MgO+CaO+SrO+BaO+ZnO)" is SiO 2 The content of MgO, CaO, SrO, BaO and ZnO is divided by the total content of MgO, CaO, SrO, BaO and ZnO.

[0016] The crystallized glass of Aspect 8 is any one of Aspects 1 to 7, wherein, in mass %, SiO 2 / (SnO 2 +Fe 2O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3 ) is preferably 0.01 to 10. 2 / (SnO 2 +Fe 2 O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3 ) is SiO 2 The content of SnO 2 , Fe 2 O 3 , V 2 O 5 , NiO, Cr 2 O 3 and MoO 3 The value is calculated by dividing the total content of the above by the total amount of the above.

[0017] The crystallized glass of Aspect 9 is any one of Aspects 1 to 8, wherein, in mass%, MoO 3 It is preferable that the content is more than 0%.

[0018] The crystallized glass of Aspect 10, in any one of Aspects 1 to 9, preferably contains, by mass %, 100 ppm or less of Pt.

[0019] The crystallized glass of Aspect 11, in any one of Aspects 1 to 10, preferably contains, by mass %, 100 ppm or less of Rh.

[0020] The crystallized glass of Aspect 12 is any one of Aspects 1 to 11, and preferably has a β-OH value of more than 0 and up to 2 / mm before crystallization.

[0021] The crystallized glass of Aspect 13 is any one of Aspects 1 to 12, and preferably has an absolute value of Seebeck coefficient of 0.000001 V / K or more at any one temperature point between 25°C and 400°C.

[0022] The crystallized glass of Aspect 14, in any one of Aspects 1 to 13, preferably has a thermoelectric conversion index ZT of 0.00001 or more at one or more temperatures between 25°C and 400°C.

[0023] The crystallized glass of Aspect 15 is any one of Aspects 1 to 14, wherein the carrier mobility is 0.0001 cm 2 It is preferable that the voltage Vs is equal to or higher than / Vs.

[0024] The crystallized glass of Aspect 16 is preferably used as a heavy metal recovery material in any one of Aspects 1 to 15.

[0025] The heavy metal recovery material of aspect 17 comprises, in mass%, Fe 2 O 3 The glass contains 20 to 80% of magnetic crystals and is characterized by being made of crystallized glass containing magnetic crystals.

[0026] The soil improver of aspect 18 contains, in mass%, Fe 2 O 3 The glass contains 20 to 80% of magnetic crystals and is characterized by being made of crystallized glass containing magnetic crystals.

[0027] The method for producing crystallized glass of Aspect 19 is the method for producing crystallized glass of any one of Aspects 1 to 16, comprising: a glass raw material and Fe 2 O 3 The method is characterized by comprising a melting step of melting a mixture of raw materials, and a crystallization step of forming the molten glass into a predetermined shape to obtain crystallized glass.

[0028] A method for recovering heavy metals according to aspect 20 is characterized by comprising an adsorption step of adsorbing heavy metals to crystallized glass containing magnetic crystals, and a recovery step of recovering the crystallized glass after the heavy metals have been adsorbed by a magnet.

[0029] The method for recovering heavy metals of Aspect 21 is preferably the method for recovering heavy metals in Aspect 20, wherein heavy metals are recovered from soil.

[0030] According to the present invention, it is possible to provide crystallized glass capable of recovering heavy metals and the like in a simple manner, a heavy metal recovery material, a soil improver, a method for producing crystallized glass, and a method for recovering heavy metals.

[0031] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments. In the following description of the content of each component, "%" means "% by mass" unless otherwise specified.

[0032] <Glass-ceramics> The glass-ceramics of the present invention contain, in mass %, Fe 2 O 3 The glass-ceramics further contains, by mass %, 20 to 80% of SiO. 2 0-80%, Al 2 O 3 0-80%, B 2 O 3 0-80%, P 2 O 5 0-80%, Li 2 O 0-50%, Na 2 O 0-50%, K 2 O 0-50%, MgO 0-50%, CaO 0-50%, SrO 0-50%, BaO 0-50%, ZnO 0-50%, ZrO 2 0-50%, HfO 2 0-50%, TiO 2 0-50% SnO 2 0-50%, V 2 O 5 0-50%, NiO 0-80%, Cr 2 O 3 0-80%, MoO 3 It is preferable that the content is 0 to 80%. 2 O 3 Furthermore, by containing magnetic crystals, when the glass-ceramics of the present invention is used as a heavy metal recovery material, the heavy metals can be easily recovered using a magnet.

[0033] Fe 2 O 3 is a component that has the ability to adsorb heavy metals. It is also a component that can form magnetic crystals. 2 O 3 The content of Fe is 20 to 80%. 2 O 3The lower limit of the content of Fe is preferably 20% or more, 21% or more, 23% or more, particularly preferably 25% or more. 2 O 3 The upper limit of the content of Fe is preferably 80% or less, 70% or less, 60% or less, and particularly preferably 55% or less. 2 O 3 If the content of Fe is too small, it becomes difficult to include magnetic crystals in the glass-ceramics. 2 O 3 If the content is too high, the viscosity of the glass melt decreases, making it difficult to form it into a desired shape. Furthermore, when used in agricultural soil, Fe ions are more likely to be eluted, which results in a decrease in the fertility of the soil.

[0034] Here, the magnetic crystal means a crystal having properties such as superferromagnetic, ferromagnetic, paramagnetic, and ferrimagnetic. More specifically, the magnetic crystal is preferably a ferrite crystal. The ferrite crystal is preferably magnetite (Fe 3 O 4 ), maghemite (γ-Fe 2 O 3 ), manganese zinc ferrite, nickel zinc ferrite, copper zinc ferrite, (Fe 2 O 3 )10.6667[γ-Fe 2 O 3 ], or Na 0.75 Ca 0.25 Fe(Si 2 O 6 It is preferable that the glass-ceramics of the present invention contain one of the crystals other than those exemplified above, as long as the desired properties are obtained. For example, gahnite, willemite (zinc silicate), Al 2 SiO 5(aluminum silicate), zirconia, zirconia titanate, tin-containing zirconia-based oxide, titania, aluminotitanate, β-quartz solid solution, α-quartz, β-quartz, β-spodumene solid solution, spodumene, zircon, cordierite other than α-cordierite, enstatite, mica, nepheline, anorthite, lithium disilicate, lithium metasilicate, wollastonite, diopsite, cristobalite, tridymite, feldspar, spinel-based crystals, metal colloids, etc. Only one type of these crystals may be contained, or two or more types may be contained.

[0035] SiO 2 SiO forms the skeleton of the glass and can be a constituent of the crystals in the crystallized glass. It is also a component that improves the chemical durability of the glass. Furthermore, it is a component that reduces the thermal expansion coefficient, making it easier to obtain crystallized glass with excellent thermal shock resistance. 2 The content of is preferably 0 to 80%. 2 The lower limit of the content of SiO is preferably 0% or more, 1% or more, 5% or more, 10% or more, 20% or more, 25% or more, particularly preferably 29% or more. 2 The upper limit of the content of SiO is preferably 80% or less, 75% or less, 70% or less, 65% or less, and particularly preferably 60% or less. 2 If the content is too high, the meltability of the glass tends to decrease, the viscosity of the glass melt tends to increase, making fining and glass forming difficult, and the time required for crystallization tends to increase, resulting in a decrease in productivity.

[0036] Al 2 O 3 Al forms the skeleton of the glass and can be a constituent of the crystals in the crystallized glass. It also contributes to the viscosity of the glass melt and is a component that easily improves the formability. 2 O 3 The content of Al is preferably 0 to 80%. 2 O 3 The lower limit of the content of Al is preferably 0% or more, particularly preferably 1% or more. 2 O 3The upper limit of the Al content is preferably 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, and particularly preferably 15% or less. 2 O 3 If the content is too high, the chemical durability of the crystallized glass tends to decrease.

[0037] B 2 O 3 is a component that reduces the viscosity of glass and improves the melting and formability of glass. It can also be a component that forms crystals in crystallized glass. 2 O 3 The content of B is preferably 0 to 80%. 2 O 3 The lower limit of the content of B is preferably 0% or more, 1% or more, particularly preferably 2% or more. 2 O 3 The upper limit of the content of is preferably 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, and particularly preferably 10% or less. 2 O 3 If the content is too high, the B 2 O 3 The amount of evaporation increases, which increases the environmental load and also reduces the chemical durability of the crystallized glass. 2 O 3 However, B may not be substantially contained. 2 O 3 Since B is easily mixed in as an impurity, if it is attempted to be completely removed, the raw material becomes expensive and the manufacturing cost tends to increase. 2 O 3 may be contained in an amount of 0.0001% or more, 0.0003% or more, particularly 0.0005% or more. In this specification, "substantially not contained" means that the material is not intentionally contained as a raw material, and objectively refers to a content of less than 0.1%.

[0038] P 2 O 5 is a component that reduces the viscosity of glass and improves the melting and formability of glass. In some cases, it can also be a component that forms crystals in crystallized glass. 2 O5 The content of P is preferably 0 to 80%. 2 O 5 The lower limit of the content of P is preferably 0% or more, 0.5% or more, particularly preferably 1% or more. 2 O 5 The upper limit of the content of P is preferably 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly preferably 5% or less. 2 O 5 If the content is too high, the P 2 O 5 The amount of evaporation of P increases, which increases the environmental load and also reduces the chemical durability of the crystallized glass. 2 O 5 However, P may not be substantially contained. 2 O 5 Since P is easily mixed in as an impurity, if it is attempted to be completely removed, the raw material becomes expensive and the manufacturing cost tends to increase. 2 O 5 The content may be 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0039] Li 2 O is a component that reduces the viscosity of glass and improves the melting and formability of glass. In some cases, it can also be a component that forms crystals in crystallized glass. 2 The content of O is preferably 0 to 50%. 2 The lower limit of the O content is preferably 0% or more, 0.5% or more, particularly preferably 1% or more. 2 The upper limit of the O content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, particularly preferably 5% or less. 2 If the O content is too high, Li 2 The amount of evaporation of O increases, which increases the environmental load and also reduces the chemical durability of the crystallized glass. 2 It may not substantially contain O. However, Li 2Since O is easily mixed in as an impurity, if it is attempted to completely remove it, the raw material becomes expensive and the manufacturing cost tends to increase. 2 O may be contained in an amount of 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0040] Na 2 O is a component that reduces the viscosity of glass and improves the melting and formability of glass. In some cases, it can also be a component that forms crystals in crystallized glass. 2 The content of O is preferably 0 to 50%. 2 The lower limit of the O content is preferably 0% or more, 0.1% or more, 0.5% or more, particularly preferably 1% or more. 2 The upper limit of the O content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 15% or less, and particularly preferably 11% or less. 2 If the O content is too high, the Na content will increase during melting. 2 The amount of evaporation of O increases, which increases the environmental load and also reduces the chemical durability of the glass-ceramics. 2 It may be substantially free of O. However, Na 2 Since O is easily mixed in as an impurity, if it is attempted to completely remove it, the raw material becomes expensive and the manufacturing cost tends to increase. 2 O may be contained in an amount of 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0041] K 2 O is a component that reduces the viscosity of glass and improves the melting and formability of glass. In some cases, O can also be a component that forms crystals in crystallized glass. 2 The content of O is preferably 0 to 50%. 2 The lower limit of the O content is preferably 0% or more, 0.1% or more, 0.5% or more, particularly preferably 1% or more. 2 The upper limit of the O content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 15% or less, 10% or less, 5% or less, and particularly preferably 3% or less. 2 If the O content is too high, the K content during melting 2The amount of evaporation of O increases, which increases the environmental load and also reduces the chemical durability of the crystallized glass. 2 It may be substantially free of O. 2 Since O is easily mixed in as an impurity, if it is attempted to completely remove it, the raw material becomes expensive and the manufacturing cost tends to increase. 2 O may be contained in an amount of 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0042] MgO is a component that reduces the viscosity of glass and improves the meltability and formability of glass. In some cases, it can also be a constituent of crystals in crystallized glass. The MgO content is preferably 0 to 50%. More specifically, the lower limit of the MgO content is preferably 0% or more, 0.1% or more, 0.5% or more, and particularly 1% or more, and the upper limit of the MgO content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 15% or less, 10% or less, 5% or less, and particularly 4% or less. If the MgO content is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and forming, making the crystallized glass and the base glass before crystallization more likely to break. It is not necessary to substantially contain MgO. However, because MgO is easily mixed in as an impurity, attempting to completely remove MgO tends to increase the cost of raw materials and manufacturing costs. Therefore, MgO may be contained in an amount of 0.0001% or more, 0.0003% or more, and particularly 0.0005% or more.

[0043] CaO is a component that reduces the viscosity of glass and improves the meltability and formability of glass. In some cases, it can also be a constituent of crystals in crystallized glass. The CaO content is preferably 0 to 50%. More specifically, the lower limit of the CaO content is preferably 0% or more, 0.5% or more, and particularly 1% or more, and the upper limit of the CaO content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly 5% or less. If the CaO content is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and forming, making the crystallized glass and the base glass before crystallization more likely to break. It is not necessary to substantially contain CaO. However, because CaO is easily mixed in as an impurity, attempting to completely remove CaO tends to increase the cost of raw materials and manufacturing costs. Therefore, CaO may be contained in an amount of 0.0001% or more, 0.0003% or more, and particularly 0.0005% or more.

[0044] SrO is a component that reduces the viscosity of glass and improves the meltability and formability of glass. In some cases, it can also be a constituent of crystals in crystallized glass. The SrO content is preferably 0 to 50%. More specifically, the lower limit of the SrO content is preferably 0% or more, 0.5% or more, and particularly 1% or more, and the upper limit of the SrO content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly 5% or less. If the SrO content is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and forming, making the crystallized glass and the base glass before crystallization more likely to break. SrO may not be substantially contained. However, because SrO is easily mixed in as an impurity, attempting to completely remove SrO tends to increase the cost of raw materials and manufacturing costs. Therefore, SrO may be contained in an amount of 0.0001% or more, 0.0003% or more, and particularly 0.0005% or more.

[0045] BaO is a component that reduces the viscosity of glass and improves the meltability and formability of glass. In some cases, it can also be a constituent of crystals in crystallized glass. The BaO content is preferably 0 to 50%. More specifically, the lower limit of the BaO content is preferably 0% or more, 0.5% or more, and particularly 1% or more, and the upper limit of the BaO content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly 5% or less. If the BaO content is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and forming, making the crystallized glass and the base glass before crystallization more likely to break. It is not necessary to substantially contain BaO. However, because BaO is easily mixed in as an impurity, attempting to completely remove BaO tends to increase the cost of raw materials and manufacturing costs. Therefore, BaO may be contained in an amount of 0.0001% or more, 0.0003% or more, and particularly 0.0005% or more.

[0046] ZnO is a component that reduces the viscosity of glass and improves the meltability and formability of glass. In some cases, it can also be a constituent of crystals in crystallized glass. The ZnO content is preferably 0 to 50%. More specifically, the lower limit of the ZnO content is preferably 0% or more, 0.5% or more, and particularly 1% or more, and the upper limit of the ZnO content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly 5% or less. If the ZnO content is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and forming, making the crystallized glass and the base glass before crystallization more likely to break. It is not necessary to substantially contain ZnO. However, because ZnO is easily mixed in as an impurity, attempting to completely remove ZnO tends to increase the cost of raw materials and manufacturing costs. Therefore, ZnO may be contained in an amount of 0.0001% or more, 0.0003% or more, and particularly 0.0005% or more.

[0047] ZrO 2 is a component that can promote crystallization and increase the chemical durability of crystallized glass. In some cases, it can also be a component that forms the crystals in crystallized glass. 2The content of ZrO is preferably 0 to 50%. 2 The lower limit of the content of ZrO is preferably 0% or more, 0.5% or more, particularly preferably 1% or more. 2 The upper limit of the content of ZrO is preferably 50% or less, 40% or less, 30% or less, 20% or less, or 10% or less, particularly preferably 5% or less. 2 If the content of ZrO is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and molding, and the crystallized glass or the base glass before crystallization is likely to break. 2 However, ZrO 2 is easily mixed in as an impurity, so ZrO 2 If we try to completely remove ZrO, the raw materials will become expensive and the manufacturing cost will tend to increase. 2 The content may be 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0048] HfO 2 is a component that can promote crystallization and improve the Young's modulus of the crystallized glass. In some cases, it can also be a component that forms the crystals in the crystallized glass. 2 The content of HfO is preferably 0 to 50%. 2 The lower limit of the content of HfO is preferably 0% or more, 0.5% or more, particularly preferably 1% or more. 2 The upper limit of the content of HfO is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, particularly preferably 5% or less. 2 If the content of HfO is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and molding, and the crystallized glass or the raw glass before crystallization is likely to break. 2 However, HfO may not be substantially contained. 2 is easily mixed in as an impurity, 2 If we try to completely remove HfO, the raw materials will become expensive and the manufacturing cost will tend to increase. 2 The content may be 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0049] TiO 2 is a component that can promote crystallization. In some cases, it can also be a component that forms crystals in crystallized glass. 2 The content of is preferably 0 to 50%. More specifically, TiO 2 The lower limit of the content of TiO is preferably 0% or more, 0.5% or more, particularly preferably 1% or more. 2 The upper limit of the content of TiO is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly preferably 5% or less. 2 If the content of TiO is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and molding, and the crystallized glass or the base glass before crystallization is likely to break. 2 However, TiO 2 If an attempt is made to completely remove TiO, the raw material becomes expensive and the manufacturing cost tends to increase. 2 The content may be 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0050] SnO 2 At high temperatures, SnO 2 → SnO + 1 / 2O 2 The reaction occurs, and O 2 This reaction releases gas. 2 The mechanism of clarification is known as O 2 The gas has a "defoaming effect" of enlarging tiny bubbles present in the glass melt and releasing them outside the glass system, as well as a "stirring effect" of mixing the glass melt. 2 is a component that can promote crystallization and improve the Young's modulus of the crystallized glass. In some cases, it can also be a component that forms the crystals in the crystallized glass. 2 The content of SnO is preferably 0 to 50%. 2 The lower limit of the content of SnO is preferably 0% or more, 0.5% or more, particularly preferably 1% or more. 2 The upper limit of the content of SnO is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly preferably 5% or less. 2If the content of SnO is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and molding, and the crystallized glass or the base glass before crystallization is likely to break. 2 However, SnO 2 is easily mixed in as an impurity, so SnO 2 If we try to completely remove SnO, the raw materials will become expensive and the manufacturing cost will tend to increase. 2 The content may be 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0051] V 2 O 5 V is a component that reduces the viscosity of glass and improves the melting and formability of glass. In some cases, it can also be a component that forms crystals in crystallized glass. 2 O 5 The content of is preferably 0 to 50%. 2 O 5 The lower limit of the content of V is preferably 0% or more, 0.5% or more, particularly preferably 1% or more. 2 O 5 The upper limit of the content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly preferably 5% or less. 2 O 5 If the content of V is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and molding, and the crystallized glass or the raw glass before crystallization is likely to break. 2 O 5 However, V may not be substantially contained. 2 O 5 is easily mixed in as an impurity, 2 O 5 If we try to completely remove V, the raw materials will become expensive and the manufacturing cost will tend to increase. 2 O 5 The content may be 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0052] NiO is a component that reduces the viscosity of glass and improves the meltability and formability of glass. In some cases, it can also be a constituent of crystals in crystallized glass. Furthermore, under reduced conditions, it can form alloys with other metal elements, improving the magnetic properties and strength of crystallized glass. Examples of alloys include nickel-chromium alloys, nickel-copper alloys, and nickel-iron alloys. The NiO content is preferably 0 to 50%. More specifically, the lower limit of the NiO content is preferably 0% or more, 0.5% or more, and particularly 1% or more, and the upper limit of the NiO content is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly 5% or less. If the NiO content is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and forming, making the crystallized glass and the base glass before crystallization more susceptible to breakage. It is not necessary for the glass to contain substantially no NiO. However, since NiO is easily mixed in as an impurity, attempting to completely remove NiO tends to increase the cost of raw materials and manufacturing costs. Therefore, NiO may be contained in an amount of 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0053] Cr 2 O 3 is a component that reduces the viscosity of glass and improves the melting and formability of glass. In some cases, it can also be a constituent of crystals in crystallized glass. Furthermore, in a reduced state, it forms alloys with other metal elements, which can improve the magnetic properties and strength of crystallized glass. Examples of alloys include nickel-chromium-molybdenum steel, chromium-molybdenum steel, and nichrome. Cr 2 O 3 The content of Cr is preferably 0 to 50%. 2 O 3 The lower limit of the content of Cr is preferably 0% or more, 0.5% or more, particularly preferably 1% or more. 2 O 3 The upper limit of the content of Cr is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly preferably 5% or less. 2 O 3If the content of Cr is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and molding, and the crystallized glass or the raw glass before crystallization is likely to break. 2 O 3 However, Cr may not be contained substantially. 2 O 3 is easily mixed in as an impurity, 2 O 3 If we try to completely remove Cr, the raw materials will become expensive and the manufacturing cost will tend to increase. 2 O 3 The content may be 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0054] MoO 3 is a component that reduces the viscosity of glass and improves the meltability and formability of glass. It can also be a constituent of crystals in crystallized glass in some cases. Furthermore, in a reduced state, it forms alloys with other metal elements, improving the magnetic properties and strength of crystallized glass. Examples of alloys include binary molybdenum alloys, nickel-chromium-molybdenum steel, chromium-molybdenum steel, and nichrome. MoO 3 The content of MoO is preferably 0 to 50%. 3 The lower limit of the content of MoO is preferably 0% or more, more than 0%, 0.1% or more, 0.2% or more, 0.5% or more, particularly preferably 1% or more. 3 The upper limit of the content of MoO is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, particularly preferably 5% or less. 3 If the content of MoO is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and molding, and the crystallized glass or the base glass before crystallization is likely to break. 3 However, MoO 3 is easily mixed in as an impurity, so MoO 3 If we try to completely remove MoO, the raw materials will become expensive and the production cost will tend to increase. 3 The content may be 0.0001% or more, 0.0003% or more, particularly 0.0005% or more.

[0055] The crystallized glass of the present invention may further contain the following components.

[0056] MnO 2 MnO is a component that reduces the viscosity of glass and improves the melting and formability of glass. In some cases, it can also be a component of crystals in crystallized glass. Furthermore, in a reduced state, it forms alloys with other metal elements, which can improve the magnetic properties and strength of crystallized glass. Examples of alloys include ferromanganese. MnO 2 The content of MnO is preferably 0 to 50%. 2 The lower limit of the content of MnO is preferably 0% or more, 0.1% or more, 0.5% or more, particularly preferably 1% or more. 2 The upper limit of the content of MnO is preferably 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, and particularly preferably 5% or less. 2 If the content of MnO is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and molding, and the crystallized glass or the base glass before crystallization is likely to break. 2 However, MnO may not be substantially contained. 2 is easily mixed in as an impurity, so MnO 2 If we try to completely remove MnO, the raw materials will become expensive and the production cost will tend to increase. 2 is preferably 0.0001% or more, 0.0003% or more, and particularly preferably 0.0005% or more.

[0057] Sb 2 O 3 , As 2 O 3 , S.O. 3 may be added as a fining agent, and the content thereof may be 0.0001% or more, 0.0003% or more, particularly 0.0005% or more, and may be 1% or less, particularly 0.8% or less. 2 O 3 and As 2 O 3 The contents of are preferably 0.5% or less, 0.2% or less, and particularly preferably less than 0.1%, respectively.

[0058] Cl, F, Y 2 O 3 , La 2 O 3 , W.O. 3 , Ta 2 O 5 , Nd 2 O 3 , Nb 2 O 5 , RfO 2 The above components may be contained in a total amount of up to 30% as long as the desired properties are obtained. However, since the raw materials for the above components are expensive and tend to increase production costs, it is preferable that they are not substantially contained unless there are special circumstances.

[0059] Pt is a component that can promote crystallization, but since it is a precious metal, from the viewpoint of cost reduction, its content is preferably 100 ppm or less, 50 ppm or less, 20 ppm or less, 10 ppm or less, 9 ppm or less, 8 ppm or less, 7 ppm or less, 6 ppm or less, 5 ppm or less, 4 ppm or less, 3 ppm or less, 2 ppm or less, 1.6 ppm or less, 1.4 ppm or less, 1.2 ppm or less, 1 ppm or less, 0.9 ppm or less, 0.8 ppm or less, 0.7 ppm or less, 0.6 ppm or less, 0.5 ppm or less, 0.45 ppm or less, 0.40 ppm or less, 0.35 ppm or less, particularly 0.30 ppm or less. Note that Pt may be mixed in from the melting equipment, and attempting to completely remove Pt may increase production costs. Therefore, as long as the crystallized glass of the present invention can obtain desired properties, the lower limit of the Pt content is preferably 0.0001 ppm or more, 0.001 ppm or more, 0.005 ppm or more, 0.01 ppm or more, 0.02 ppm or more, 0.03 ppm or more, 0.04 ppm or more, 0.05 ppm or more, 0.06 ppm or more, particularly 0.07 ppm or more.In addition, when Pt is also used as a crystallization promoter, Pt can be used alone or can be combined with other components.In addition, when Pt is used as a crystallization promoter, the form of Pt is not particularly important.For example, the form of Pt can be colloidal or metal crystal.

[0060] Rh is a component that can promote crystallization, but since it is a precious metal, from the viewpoint of cost reduction, its content is preferably 100 ppm or less, 50 ppm or less, 20 ppm or less, 10 ppm or less, 9 ppm or less, 8 ppm or less, 7 ppm or less, 6 ppm or less, 5 ppm or less, 4 ppm or less, 3 ppm or less, 2 ppm or less, 1.6 ppm or less, 1.4 ppm or less, 1.2 ppm or less, 1 ppm or less, 0.9 ppm or less, 0.8 ppm or less, 0.7 ppm or less, 0.6 ppm or less, 0.5 ppm or less, 0.45 ppm or less, 0.40 ppm or less, 0.35 ppm or less, particularly 0.30 ppm or less. Note that Rh may be mixed in from the melting equipment, and attempting to completely remove Rh may increase production costs. Therefore, the lower limit of the Rh content is preferably 0.0001 ppm or more, 0.001 ppm or more, 0.005 ppm or more, 0.01 ppm or more, 0.02 ppm or more, 0.03 ppm or more, 0.04 ppm or more, 0.05 ppm or more, 0.06 ppm or more, particularly 0.07 ppm or more. When Rh is also used as a crystallization promoter, Rh may be used alone or in combination with other components. When Rh is used as a crystallization promoter, the form of Rh is not particularly important. For example, Rh may be in the form of a colloid or a metal crystal.

[0061] The crystallized glass of the present invention may be any of various materials, for example, H 2 , CO 2 , CO, H 2 O, He, Ne, Ar, N 2 and other minor components may be contained up to less than 0.1% each.

[0062] If As, Sb, Ag, Au, Pd, Ir, V, Cr, Sc, Ce, Pr, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Ac, Th, Pa, U are intentionally added, which tends to increase raw material costs and manufacturing costs.Therefore, the content of the above components is preferably 10% or less, 5% or less, 3% or less, 1% or less, 0.5% or less, 0.3% or less, 0.1% or less, 500 ppm or less, 300 ppm or less, 100 ppm or less, particularly 10 ppm or less.On the other hand, when glass containing Ag, Au, etc. is subjected to light irradiation or heat treatment, aggregates of these components are formed, which can be used as a starting point to promote crystallization.In addition, Pd, etc. have various catalytic effects, and by adding them, it is possible to impart unique functions to crystallized glass. In view of these circumstances, when the purpose is to promote crystallization or to impart other functions, the above components may be contained in an amount of 0.1% or more, 0.2% or more, and particularly 0.5% or more.

[0063] From the viewpoint of improving the meltability and formability of the glass, SnO 2 , Fe 2 O 3 , V 2 O 5 , NiO, Cr 2 O 3 , MoO 3 It is preferable to control the total amount of SnO. 2 +Fe 2 O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3 is preferably 20% or more, 21% or more, 23% or more, 25% or more, particularly preferably 30% or more. The upper limit is not particularly limited, but may be 90% or less, 80% or less, 70% or less, 60% or less, particularly preferably 55% or less.

[0064] Li 2 O, Na 2 O.K. 2O is a component that reduces the viscosity of glass and improves the meltability and formability of glass. Here, when the content of K cations increases, the Young's modulus and rigidity modulus of the crystallized glass tend to decrease, and the crystallized glass tends to break during processing. 2 The raw material for O is Li 2 It is cheaper than O. Also, K 2 O to Li 2 O and Na 2 When K is contained together with O, diffusion of Li cations and Na cations in the remaining glass of the crystallized glass becomes difficult, and as a result, the chemical durability of the crystallized glass may be improved. 2 O / (Li 2 O + Na 2 O+K 2 It is preferable to control K in mass % ratio. 2 O / (Li 2 O + Na 2 O+K 2 O) is preferably 0.01 to 0.99, 0.01 to 0.95, 0.01 to 0.90, 0.01 to 0.85, 0.01 to 0.80, particularly preferably 0.01 to 0.75.

[0065] Incidentally, when crystallized glass is used as a soil conditioner (described later), the remaining glass portion may be scratched when blended into the soil, and the scratch may be the starting point for breakage. Generally, in glass having many open spaces (voids, also called free volume) in the glass network, energy is consumed in structural changes of the open spaces, so scratches are unlikely to progress. From the viewpoint of providing such open spaces in the glass network, it is preferable that the crystallized glass is made of SiO 2 and / or P 2 O 5 On the other hand, since the higher the hardness of the glass, the more resistant it is to scratches, from the viewpoint of reducing open spaces in the glass network, it is preferable that the glass-ceramics contain Al. 2 O 3 That is, from the viewpoint of making the crystallized glass of the present invention less susceptible to scratches and less likely to break even if scratches are made in the remaining glass, it is preferable to contain (SiO 2 +P2 O 5 ) / (SiO 2 +Al 2 O 3 +P 2 O 5 It is preferable to control (SiO 2 +P 2 O 5 ) / (SiO 2 +Al 2 O 3 +P 2 O 5 ) is preferably 0.01 to 0.99, 0.1 to 0.99, 0.2 to 0.99, 0.3 to 0.99, 0.4 to 0.99, 0.5 to 0.99, 0.6 to 0.99, particularly preferably 0.7 to 0.99.

[0066] Incidentally, when crystals are precipitated from the base glass, a deviation in the distribution of components in the base glass may occur. Hereinafter, this state in which a deviation occurs will be referred to as a phase-separated state. By controlling this phase-separated state, it becomes easier to efficiently advance crystallization. The phase-separated state can be achieved, for example, by controlling the distribution of SiO, which is the main glass skeleton. 2 and SiO 2 It is easy to separate into areas rich in components other than B. 2 O 3 , P 2 O 5 , ZrO 2 , HfO 2 , TiO 2 , SnO 2 Since glass containing SiO is prone to phase separation, from the viewpoint of efficiently promoting crystallization, 2 / (B 2 O 3 +P 2 O 5 + ZrO 2 +HfO 2 + TiO 2 + SnO 2 It is preferable to control SiO in mass % ratio. 2 / (B 2 O 3 +P 2 O 5 + ZrO 2 +HfO 2 + TiO2 + SnO 2 ) is preferably 0.1 to 10,000, 0.1 to 8,000, 0.1 to 6,000, 0.1 to 5,000, 0.2 to 5,000, particularly preferably 0.2 to 4,000.

[0067] From the viewpoint of stable melting and forming of glass, SiO 2 It is preferable to control the SiO content of the glass-ceramics of the present invention. 2 / (MgO+CaO+SrO+BaO+ZnO) is preferably 0.1 to 10,000, 0.1 to 8,500, 0.1 to 5,000, 0.1 to 3,000, 0.1 to 1,000, 0.5 to 1,000, particularly preferably 1 to 100.

[0068] From the viewpoint of suppressing the deterioration of the crystallized glass and the elution of the constituent components, SiO 2 / (SnO 2 +Fe 2 O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3 ) is preferably controlled. More specifically, the crystallized glass of the present invention is 2 / (SnO 2 +Fe 2 O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3 ) is preferably 0.01 to 10, 0.1 to 8, 0.3 to 5, particularly preferably 0.5 to 3.

[0069] The β-OH value of the raw glass before crystallization of the crystallized glass of the present invention is preferably greater than 0 to 2 / mm. More specifically, the lower limit of the β-OH value is preferably greater than 0, 0.01 / mm or more, 0.02 / mm or more, 0.03 / mm or more, 0.04 / mm or more, 0.05 / mm or more, 0.06 / mm or more, 0.07 / mm or more, 0.08 / mm or more, 0.09 / mm or more, and particularly preferably 0.1 / mm or more. Furthermore, the upper limit of the β-OH value is preferably 2 / mm or less, 1.5 / mm or less, 1.4 / mm or less, and particularly preferably 1.3 / mm or less. When the β-OH value is within the above range, the quality of the glass is less likely to deteriorate. In other words, if the β-OH value is too small, the amount of water vapor generated when melting the glass batch is reduced. As a result, the stirring effect of the glass batch due to the generation of water vapor is reduced, making it difficult to promote the initial reaction, and the production load is likely to increase. If the β-OH value is too large, bubbles are likely to form at the interface between the molten glass and a metal member such as Pt or a refractory member, which will result in unintended voids being generated inside the crystallized glass, leading to a decrease in strength. Furthermore, the linear thermal expansion coefficient of the crystallized glass will increase, which may deteriorate its heat resistance and thermal shock resistance, making it unsuitable for use at high temperatures.

[0070] The crystallized glass of the present invention preferably has an absolute Seebeck coefficient of 0.000001 V / K or more, 0.000005 V / K or more, 0.00001 V / K or more, 0.00002 V / K or more, 0.00003 V / K or more, 0.00004 V / K or more, 0.00005 V / K or more, particularly 0.00006 V / K or more, at at least one temperature point between 25°C and 400°C. For example, the absolute value of the Seebeck coefficient preferably satisfies the above values ​​at 25°C, 100°C, 200°C, or 400°C. By having the absolute value of the Seebeck coefficient satisfy the above values, the thermoelectric conversion index ZT can be increased, thereby improving thermoelectric conversion efficiency. Furthermore, when thermoelectric conversion occurs between 25°C and 400°C, it becomes possible to generate electricity in various locations, such as oceans, rivers, mountainous regions, desert regions, residential areas, and space. Furthermore, it becomes possible to generate electricity by utilizing body heat, exhaust heat from automobiles, electronic devices, etc. There is no particular upper limit to the absolute value of the Seebeck coefficient, but it may be, for example, 0.0001 V / K or less.

[0071] The crystallized glass of the present invention preferably has a thermoelectric conversion index ZT of 0.00001 or more, 0.00005 or more, 0.0001 or more, particularly 0.0002 or more at one or more temperatures between 25°C and 400°C. For example, it is preferable that the thermoelectric conversion index ZT satisfies the above value at 400°C. Crystallized glass having a thermoelectric conversion index ZT that satisfies the above value is suitable as a thermoelectric conversion material. There is no particular restriction on the upper limit of the thermoelectric conversion index ZT, but it may be, for example, 0.01 or less, particularly 0.001 or less. The thermoelectric conversion index ZT is expressed by the following formula:

[0072] ZT = S 2 ×σ / κ where S is the Seebeck coefficient [V / K], σ is the electrical conductivity [S / m], and the thermal conductivity κ is [W / m·K].

[0073] The crystallized glass of the present invention has a carrier mobility of 0.0001 cm 2 / Vs or more, 0.001cm 2 / Vs or more, 0.01cm 2 / Vs or more, especially 0.1 cm 2 / Vs or more. Crystallized glass having a carrier mobility satisfying the above value is useful for producing semiconductor members with higher performance. The upper limit of the carrier mobility is not particularly limited, but is, for example, 1 cm 2 / Vs or less.

[0074] The crystallized glass of the present invention has a thermal expansion coefficient of 200×10 at 30 to 300° C. -7 / ℃ or less, 180 x 10 -7 / ℃ or less, 150 x 10 -7 / ℃ or less, 120 x 10 -7 / ℃ or less, 100 x 10 -7 / ℃ or less, especially 98 × 10 -7 The lower limit of the thermal expansion coefficient is not particularly limited, but is preferably 50×10 -7 / °C or more. The thermal expansion coefficient at 30 to 380°C may be 200 x 10 -7 / ℃ or less, 180 x 10 -7 / ℃ or less, 150 x 10 -7 / ℃ or less, 120 x 10 -7 / ℃ or less, 100 x 10 -7 / ℃ or less, especially 98 × 10 -7 The lower limit of the thermal expansion coefficient is not particularly limited, but is preferably 50×10 -7 / °C or more.

[0075] The glass-ceramics of the present invention are treated as a substitute for softening point, and the temperature at which the slope of the thermal expansion curve of the glass before crystallization changes is referred to as the glass transition temperature Tg. The glass transition temperature Tg is preferably 450°C or higher, 460°C or higher, 470°C or higher, 480°C or higher, 490°C or higher, 500°C or higher, 510°C or higher, and particularly 520°C or higher in the glass state before crystallization. If the glass transition temperature Tg is too low, the glass will flow too much during crystallization, making it difficult to form into the desired shape. The upper limit of the glass transition temperature Tg may be, for example, 700°C or lower. The yield point Tf is preferably 900°C or lower, 850°C or lower, 800°C or lower, and particularly 780°C or lower. If the yield temperature of the glass-ceramics exceeds 900°C, softening by reheating will be difficult to occur, and the accuracy of softening processing such as bending will tend to decrease. The lower limit of the yield point Tf may be, for example, 500°C or higher, 520°C or higher, and particularly, more than 520°C.

[0076] The crystallized glass of the present invention has a density of 2.4 to 4 g / cm after crystallization. 3 , 2.5-3.8g / cm 3 , 2.6-3.6g / cm 3 , particularly 2.7 to 3.5 g / cm 3 It is preferable that the density of the glass-ceramics is too low. If the density of the glass-ceramics is too low relative to the soil particles, it becomes difficult to mix uniformly into the soil. On the other hand, if the density of the glass-ceramics is too high, the weight per unit area becomes large, making it difficult to handle. In addition, the density of the glass-ceramics is an index for determining whether the glass is sufficiently crystallized. Specifically, the greater the difference in density between the original glass and the glass-ceramics, the more advanced the crystallization.

[0077] The crystallized glass of the present invention preferably has a crystallinity of 1% or more, 5% or more, 10% or more, 20% or more, and particularly 25% or more. If the crystallinity is too low, the mechanical strength tends to decrease. The upper limit of the crystallinity is not particularly limited, but it may be, for example, 80% or less, 70% or less, and particularly 60% or less. Here, the "crystallinity" can be evaluated by the powder method using an X-ray diffractometer (Rigaku RINT-2100). For example, after calculating the area of ​​the halo corresponding to the amorphous mass and the area of ​​the peak corresponding to the crystalline mass, it can be determined by the formula [peak area] x 100 / [peak area + halo area] (%).

[0078] The crystal grain size of the crystallized glass of the present invention is preferably 1000 nm or less, 800 nm or less, 500 nm or less, 400 nm or less, 300 nm or less, particularly 200 nm or less. This makes it easier to reduce the thermal expansion coefficient of the crystallized glass. Note that the crystal grain size can be evaluated using, for example, the analysis software installed in an X-ray diffractometer (Rigaku's fully automatic multipurpose horizontal X-ray diffractometer Smart Lab).

[0079] The Young's modulus of the crystallized glass of the present invention is preferably 60 to 120 GPa, 70 to 110 GPa, 75 to 110 GPa, or 75 to 100 GPa, particularly preferably 75 to 95 GPa. If the Young's modulus is too low or too high, the mechanical strength of the crystallized glass is likely to decrease.

[0080] The glass-ceramics of the present invention preferably have a modulus of rigidity of 25 to 40 GPa, 28 to 40 GPa, and particularly preferably 30 to 40 GPa. If the modulus of rigidity is too low or too high, the mechanical strength of the glass-ceramics is likely to decrease.

[0081] The Poisson's ratio of the crystallized glass of the present invention is preferably 0.35 or less, 0.32 or less, 0.3 or less, 0.28 or less, 0.26 or less, particularly preferably 0.25 or less.If the Poisson's ratio is too large, the mechanical strength of the crystallized glass is likely to decrease.The lower limit of the Poisson's ratio is not particularly limited, but may be, for example, 0.15 or more.

[0082] The crystallized glass of the present invention has an electrical resistance of 100,000 Ω m or less, preferably 10,000 Ω m or less, 5,000 Ω m or less, 1,000 Ω m or less, 500 Ω m or less, 1000 Ω m or less, 500 Ω m or less, 100 Ω m or less, 50 Ω m or less, 10 Ω m or less, 5 Ω m or less, 4 Ω m or less, particularly preferably Ω m or less. Because of its low electrical resistance, the crystallized glass of the present invention can be suitably used as a material for thermoelectric conversion components, semiconductor components, communication components, etc., in addition to being used as a heavy metal recovery material and soil modifier that adsorbs and recovers heavy metals, etc.

[0083] The carrier species of the crystallized glass of the present invention is preferably any one of ions, electrons, holes, or a combination thereof.In particular, when the crystallized glass of the present invention is used as a material for thermoelectric conversion components, semiconductor components, communication components, building components, chemical reaction components, heat-resistant components, space components, medical components, etc., it is preferably any one of electrons and holes, which tend to increase electrical conductivity, or a combination thereof.

[0084] The crystallized glass of the present invention has a Hall coefficient of 0.0001 cm 3 / C or more, 0.0005cm 3 / C or more, 0.001cm 3 / C or more, 0.005cm 3 / C or more, 0.01cm 3 / C or more, 0.05cm 3 / C or more, 0.1cm 3 / C or more, especially 0.5 cm 3 By doing so, the crystallized glass of the present invention can be easily used as a material for thermoelectric conversion members, semiconductor members, communication members, construction members, chemical reaction members, heat-resistant members, space members, medical members, etc.

[0085] The crystallized glass of the present invention has a carrier concentration of 1×10 15 / cm 3 , 5 x 10 15 / cm 3 , 1 x 10 16 / cm 3 , 5 x 10 16 / cm 3 , 1 x 10 17 / cm 3, 5 x 10 17 / cm 3 , especially 1 × 10 18 / cm 3 It is preferable that the sheet carrier concentration is 1×10 or more. 15 / cm 2 , 5 x 10 15 / cm 2 , 1 x 10 16 / cm 2 , 5 x 10 16 / cm 2 , especially 1 × 10 17 / cm 2 By doing so, the crystallized glass of the present invention can be easily used as a material for thermoelectric conversion members, semiconductor members, communication members, construction members, chemical reaction members, heat-resistant members, space members, medical members, etc.

[0086] The crystallized glass of the present invention has a saturation magnetization of 0.5 emμ / cm 3 Above, 1<em>μ / cm 3 Above, 5<em>μ / cm 3 Above, 10emμ / cm 3 Above, 15<em>μ / cm 3 Above, 20emμ / cm 3 Above, 25<em>μ / cm 3 Above, 30emμ / cm 3 Above, 35<em>μ / cm 3 or more, especially 40 emμ / cm 3 By doing so, after dispersing the crystallized glass of the present invention in soil or the like, the crystallized glass of the present invention can be easily recovered with a magnet or the like.

[0087] The crystallized glass of the present invention has a liquidus temperature of 1540 ° C or less, 1535 ° C or less, 1530 ° C or less, 1525 ° C or less, 1520 ° C or less, 1515 ° C or less, 1510 ° C or less, 1505 ° C or less, 1500 ° C or less, 1495 ° C or less, 1490 ° C or less, 1485 ° C or less, 1480 ° C or less, 1475 ° C or less, 1470 ° C or less, 1465 ° C or less, 1460 ° C or less, 1455 ° C or less, 1450 ° C or less, 1445 ° C or less, 1440 ° C or less, 1435 ° C or less, 1430 ° C or less, 1425 ° C or less, 1420 ° C or less, 1415 ° C or less, particularly preferably 1410 ° C or less. If the liquidus temperature is too high, it is likely to devitrify during production. Furthermore, if the liquidus temperature is 1480°C or lower, production by a roll method or the like becomes easy, if it is 1450°C or lower, production by a casting method or the like becomes easy, and if it is 1410°C or lower, production by a fusion method or the like becomes easy, which are preferable.

[0088] The crystallized glass of the present invention has a liquidus viscosity (logarithm of viscosity corresponding to the liquidus temperature) of 1.70 or more, 1.75 or more, 1.80 or more, 1.85 or more, 1.90 or more, 1.95 or more, 2.00 or more, 2.05 or more, 2.10 or more, 2.15 or more, 2.20 or more, 2.25 or more, 2.30 or more, 2.35 or more, 2.40 or more, 2.45 or more, 2.50 or more, 2.55 or more, 2.60 or more , 2.65 or more, 2.70 or more, 2.75 or more, 2.80 or more, 2.85 or more, 2.90 or more, 2.95 or more, 3.00 or more, 3.05 or more, 3.10 or more, 3.15 or more, 3.20 or more, 3.25 or more, 3.30 or more, 3.35 or more, 3.40 or more, 3.45 or more, 3.50 or more, 3.55 or more, 3.60 or more, 3.65 or more, particularly 3.70 or more are preferred. If the liquidus viscosity is too low, devitrification tends to occur during production. On the other hand, if the liquidus viscosity is 3.40 or more, production by a roll method or the like is facilitated, if it is 3.50 or more, production by a casting method or the like is facilitated, and if it is 3.70 or more, production by a fusion method or the like is facilitated, which is preferable.

[0089] <Method of Manufacturing Crystallized Glass> When manufacturing the crystallized glass of the present invention, a glass raw material and Fe are mixed. 2 O 3It is preferable that the method comprises a melting step of melting the mixture of raw materials and a crystallization step of forming the molten glass into a predetermined shape to obtain crystallized glass.

[0090] First, glass raw materials and Fe 2 O 3 The mixture of raw materials is melted (melting step). For example, the mixture can be placed in a crucible and melted in an electric furnace at 1000 to 2000°C for 3 to 5 hours. Note that the glass melting method is not limited to the above method, and flame melting using a burner or the like, melting by laser irradiation, melting by plasma, etc. can also be used as appropriate.

[0091] It is preferable to use glass cullet as a glass raw material. The type of glass cullet is not particularly limited as long as the desired glass composition can be obtained, but for example, glass cullet of residential window glass, automotive window glass, display glass, fiber glass, architectural glass, optical glass, pharmaceutical / medical glass, semiconductor material glass, and solar cell support glass is preferably used as a raw material. Since an improvement in the recycling rate of the above glasses is required, the use of glass cullet made of the above glasses can particularly contribute to the recycling and upcycling of glass. However, instead of using glass cullet, powder raw materials such as oxides, hydroxides, carbonates, and nitrates may be mixed to form a glass raw material. Alternatively, a mixture of powder raw materials and glass cullet may be used as a glass raw material. Fe 2 O 3 The raw material is Fe 2 O 3 It is preferable to use a powdered raw material.

[0092] Next, the molten glass is formed into a predetermined shape to obtain crystallized glass (crystallization step). In this process, crystallization may occur simultaneously with cooling of the molten glass, or after solidifying the glass (raw glass) into a predetermined shape, the raw glass may be heat-treated to crystallize it. Alternatively, the glass melt may be maintained at a high temperature (1000°C or higher) to crystallize it. The shape of the crystallized glass and raw glass is not particularly limited, and may be, for example, plate-like, fibrous, film-like, block-like, powder-like, spherical, or hollow. For example, a crystallized glass sample may be obtained by heat-treating the glass at 300 to less than 1000°C and then slowly cooling. Either heat treatment may be performed at a specific temperature, or may be performed stepwise by maintaining two or more temperatures, or may be performed while applying a temperature gradient. Crystallization may also be promoted by applying or irradiating sound waves or electromagnetic waves.

[0093] When wanting to obtain sufficient thermal shock resistance, it is preferable to control the cooling rate to fully carry out the structural relaxation of remaining glass phase.For example, the average cooling rate from 800 ℃ to 25 ℃ is preferably 100000 ℃ / h, 50000 ℃ / h, 20000 ℃ / h, 10000 ℃ / h, 5000 ℃ / h, 2000 ℃ / h, 1000 ℃ / h, 500 ℃ / h, 300 ℃ / h, 100 ℃ / h, 50 ℃ / h, 20 ℃ / h, 15 ℃ / h, 10 ℃ / h, 5 ℃ / h, 3 ℃ / h, 2 ℃ / h, 1 ℃ / h, 0.5 ℃ / h, particularly 0.1 ℃ / h. Furthermore, when long-term dimensional stability is desired, the cooling rate is preferably 0.05°C / h or less, 0.01°C / h or less, 0.005°C / h or less, 0.001°C / h or less, 0.0005°C / h or less, and particularly preferably 0.0001°C / h or less. Except when physical strengthening treatment such as air cooling or water cooling is performed, it is desirable that the cooling rate of the crystallized glass be similar from the surface to the part of the inner wall thickness farthest from the surface. The value obtained by dividing the cooling rate of the part of the inner wall thickness farthest from the surface by the cooling rate of the surface is preferably 0.0001 to 1, 0.001 to 1, 0.01 to 1, 0.1 to 1, 0.5 to 1, 0.8 to 1, 0.9 to 1, and particularly 1. By being close to 1, residual strain is less likely to occur at all positions in the crystallized glass, making it easier to achieve long-term dimensional stability. The surface cooling rate can be estimated using a contact thermometer or a radiation thermometer, and the internal temperature can be estimated by placing high-temperature crystallized glass in a cooling medium, measuring the heat quantity and rate of heat change of the cooling medium, and then using this numerical data and the specific heat and thermal conductivity of the crystallized glass and the cooling medium.

[0094] The crystallized glass of the present invention is not limited to the above-mentioned manufacturing method. For example, the mixture may be melted by irradiating it with a laser while floating. For example, the mixture may be melted in a continuous furnace that combines burner heating and electrical heating. For example, the up-draw method, down-draw method, slit method, overflow (fusion) method, or hand-blowing method may be used. Alternatively, the glass melt may be poured onto a liquid with a high specific gravity, and the glass composition may be solidified into a plate shape.

[0095] The crystallized glass of the present invention may be subjected to chemical strengthening or the like. The conditions for the chemical strengthening treatment may be appropriately selected by taking into consideration the glass composition, the degree of crystallization, the type of molten salt, etc., such as the treatment time and temperature. For example, the Na content that may be contained in the remaining glass may be reduced to facilitate chemical strengthening after crystallization. 2 A glass composition containing a large amount of O may be selected, or the crystallinity may be intentionally reduced. The molten salt may contain an alkali metal such as Li, Na, or K, either singly or in combination. Furthermore, multi-stage chemical strengthening may be selected in addition to the usual single-stage strengthening.

[0096] <Heavy Metal Recovery Material> The crystallized glass of the present invention can be suitably used as a heavy metal recovery material. In other words, the heavy metal recovery material of the present invention contains, in mass %, Fe 2 O 3 The glass contains 20 to 80% of Fe and is characterized by being made of glass-ceramics containing magnetic crystals. 2 O 3 By containing a large amount of , the crystallized glass of the present invention can adsorb heavy metals. The heavy metals are not particularly limited, but can be used as a recovery material for, for example, cadmium, arsenic, chromium, copper, or lead.

[0097] The form of the heavy metal recovery material is not particularly limited, and may be, for example, powder, granules, small pieces, etc. In particular, from the viewpoint of widening the contact area with the heavy metals, a powder form is preferable. The average particle size (D50) of the heavy metal recovery material is preferably, for example, 10 to 200 μm. Here, the "average particle size D50" refers to a value measured with a laser diffraction device, and represents the particle size at which the integrated amount, cumulatively from the smallest particle, is 50% of the total on a volume-based cumulative particle size distribution curve measured by laser diffraction.

[0098] The amount of heavy metal recovery material added to the heavy metal recovery source is preferably 0.1% or more, 0.5% or more, 1% or more, particularly 2% or more by weight, and preferably 10% or less, 8% or less, particularly 5% or less. If the amount of heavy metal recovery material added is too small, the heavy metal recovery effect will not be sufficient. If the amount added is too large, the recovery cost will increase. Examples of heavy metal recovery sources include soil and heavy metal-containing liquids.

[0099] <Soil Conditioner> The crystallized glass of the present invention can be particularly suitably used as a soil conditioner. In other words, the soil conditioner of the present invention contains, in mass %, Fe 2 O 3 The glass-ceramics of the present invention contain 20 to 80% Fe and are characterized by being made of glass-ceramics containing magnetic crystals. As described above, the glass-ceramics of the present invention contain magnetic crystals, so they are attracted to a magnet. 2 O 3 Because the glass-ceramics of the present invention contain a large amount of magnetic crystals, they can effectively adsorb heavy metals. Therefore, when the glass-ceramics of the present invention is spread in soil as a soil conditioner, it can be adsorbed and recovered using a magnet. Specifically, the method for recovering heavy metals of the present invention is characterized by comprising an adsorption step of adsorbing heavy metals to the glass-ceramics containing magnetic crystals, and a recovery step of recovering the glass-ceramics after adsorption of the heavy metals using a magnet. In particular, the method is suitable for recovering heavy metals from soil.

[0100] The crystallized glass of the present invention is not limited to the use of heavy metal recovery material and soil conditioner.For example, the crystallized glass of the present invention can be suitably used as a water quality improvement material, an ion exchange material, an adsorbent, or a fertilizer additive.The crystallized glass of the present invention can also be suitably used as a material for thermoelectric conversion components, semiconductor components, communication components, building components, chemical reaction components, heat-resistant components, space components, medical components, etc.

[0101] The present invention will be described below based on examples, but the present invention is not limited to the following examples.

[0102] Tables 1 and 2 show examples of the present invention (Examples 1 to 9).

[0103]

[0104]

[0105] The sample was prepared as follows: First, Fe 2 O 3The powder raw material and glass cullet were mixed to obtain a glass raw material. The obtained glass raw material was melted at 1500°C for 4 hours and then roll-formed to a thickness of 5 mm. In Examples 1 to 5 and 7 to 9, the molten glass was crystallized during roll-forming. After roll-forming, the glass was annealed at 400°C for 3 hours using a slow cooling furnace and slowly cooled to room temperature at 100°C / h to obtain a crystallized glass sample. In Example 6, the solidified raw glass after slow cooling was placed in an electric furnace heated to 900°C and held there for 5 hours to crystallize. After crystallization, the glass was annealed at 400°C for 3 hours and slowly cooled to room temperature at 100°C / h to obtain a crystallized glass sample. Note that Sn+Fe+V+Ni+Cr+Mo in Table 1 represents SnO 2 +Fe 2 O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3 K / (Li+Na+K) means K 2 O / (Li 2 O + Na 2 O+K 2 O). (Si+P) / (Si+Al+P) means (SiO 2 +P 2 O 5 ) / (SiO 2 +Al 2 O 3 +P 2 O 5 ) Si / (B+P+Zr+Hf+Ti+Sn) is SiO 2 / (B 2 O 3 +P 2 O 5 + ZrO 2 +HfO 2 + TiO 2 + SnO 2 ) Si / (Mg+Ca+Sr+Ba+Zn) is SiO 2 / (MgO+CaO+SrO+BaO+ZnO). Si / (Sn+Fe+V+Ni+Cr+Mo) means SiO 2 / (SnO 2 +Fe 2 O 3 +V 2 O 5+ NiO + Cr 2 O 3 +MoO 3 ) means

[0106] The sample composition was analyzed as follows. The Pt and Rh contents were analyzed using an ICP-MS device (Agilent 8800 manufactured by AGILEINT TECHNOLOGY). First, the prepared glass sample was crushed and wetted with pure water, and then perchloric acid, nitric acid, sulfuric acid, and hydrofluoric acid were added appropriately to melt the sample. The Pt and Rh contents of the sample were then measured by ICP-MS. The Pt and Rh contents of each measurement sample were determined based on a calibration curve created using a previously prepared Pt and Rh solution of known concentrations. The measurement mode was Pt:He gas / HMI (low mode) and Rh:HEHe gas / HMI (medium mode), and the mass numbers were Pt: 198 and Rh: 103. Note that the Li of the prepared sample 2 The O content was analyzed using an atomic absorption spectrometer (ContrAA600 manufactured by Analytik Jena). The melting process of the glass sample and the use of a calibration curve were basically the same as in the analysis of Pt and Rh. As for other components, Pt, Rh, Li 2 As with O, measurements were made by ICP-MS or atomic absorption spectrometry, or a glass sample with a known concentration previously determined using an ICP-MS or atomic absorption spectrometry was used as a calibration curve sample, and a calibration curve was then created using an XRF analyzer (RIGAKU ZSX Primus IV).The actual content of each component was then determined from the XRF analysis value of the measurement sample based on the calibration curve.During the XRF analysis, the tube voltage, tube current, exposure time, etc. were adjusted as needed depending on the component being analyzed.Table 1 shows the analytical values ​​for each sample.

[0107] The β-OH value can be measured using glass before crystallization. 2 O 3 Therefore, it is not easy to determine the β-OH value of the glass before crystallization. 2 O 3Glasses not containing β-OH were produced using the same raw material composition and manufacturing process, and the β-OH value was used to treat them as the β-OH value before crystallization in the examples. The β-OH value was calculated using the following formula by measuring the transmittance of the glass using an infrared spectrophotometer (FT-IR Frontier manufactured by Perkin Elmer). The scanning speed was 100 μm / min, and the sampling pitch was 1 cm. -1 The number of scans was 10 per measurement.

[0108] β-OH value = (1 / X) log (T1 / T2) X: glass thickness T1: transmittance at a reference wave number of 3846 cm-1 T2: minimum transmittance at an OH group absorption wave number of around 3600 cm-1

[0109] The thermal expansion coefficient was measured using a crystallized glass sample processed to 20 mm x 3.8 mmφ in the temperature ranges of 30 to 300°C and 30 to 380°C. A NETZSCH dilatometer was used for the measurements. The glass transition point (Tg) and yield point (Tf) of the crystallized glass were measured by calculating the temperature at which the slope of the thermal expansion changes in each thermal expansion curve.

[0110] The density was evaluated by the Archimedes method.

[0111] The precipitated crystals were evaluated using an X-ray diffractometer (Aeris manufactured by Spectris Co., Ltd.). The scan mode was 2θ / θ measurement, the scan type was continuous scan, the scattering slit width was 9 mm, the divergence slit width was 1 / 4°, the receiving slit was open, the measurement range was 5 to 60°, the measurement step was 0.01°, and the scan speed was 1.5° / min. The main crystals and crystal grain size were evaluated using analysis software installed in the package of the same model.

[0112] The crystallinity was evaluated by the powder method using an X-ray diffractometer (Rigaku RINT-2100). Specifically, the area of ​​the halo corresponding to the amorphous mass and the area of ​​the peak corresponding to the crystalline mass were calculated, and then the crystallinity was calculated using the formula [peak area] × 100 / [peak area + halo area] (%).

[0113] The Young's modulus, rigidity modulus, and Poisson's ratio were measured at room temperature using a free resonance type elastic modulus measuring device (JE-RT3 manufactured by Nippon Technoplus) for plate-shaped samples (40 mm × 20 mm × 20 mm) whose surfaces had been polished with a polishing solution containing dispersed No. 1200 alumina powder.

[0114] The Seebeck coefficient and electrical resistance were measured in a low-pressure helium atmosphere using a thermoelectric property evaluation device ZEM-3 manufactured by Advance Riko Co., Ltd. The thermoelectric conversion index ZT was calculated using the following formula.

[0115] ZT = S 2 ×σ / κ where S is the Seebeck coefficient [V / K], σ is the electrical conductivity [S / m], and the thermal conductivity κ is [W / m·K].

[0116] The carrier species, Hall coefficient, carrier concentration, sheet carrier concentration, and carrier mobility were measured at room temperature using ResiTest 8308 manufactured by Toyo Corporation, assuming a single carrier system.

[0117] The saturation magnetization was measured at room temperature using a vibrating sample magnetometer VSM manufactured by Toei Kogyo Co., Ltd.

[0118] To evaluate the adsorption capacity of heavy metals, etc., the amount of cadmium adsorption from a simulated contaminated aqueous solution was measured using a cadmium aqueous solution. First, the crystallized glass sample of Example 4 was crushed and sieved to 53-150 μm to prepare a powder sample. Furthermore, a cadmium standard solution (Cd 1000) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was diluted with pure water to prepare a 10 ppm cadmium aqueous solution with a pH of 7. Five grams of the powder sample was added to 200 mL of the 10 ppm cadmium aqueous solution, and the mixture was stirred at room temperature for three hours. The cadmium aqueous solution and the powder sample were then separated using a funnel and filter paper, and the cadmium ion concentration in the filtered cadmium aqueous solution was analyzed using an ICP-MS system (Agilent 8800 manufactured by AGILEINT TECHNOLOGY). The cadmium ion concentration after the test was divided by the cadmium ion concentration before the test (10 ppm), and the result was multiplied by 100 to evaluate the amount of cadmium adsorption.

[0119] As is clear from Table 2, the crystallized glass samples of Examples 1 to 9 contained magnetic crystals. More specifically, the magnetic crystals contained magnetite (Fe 3 O 4 ), maghemite (γ-Fe 2 O 3 ), (Fe 2 O 3 )10.6667[γ-Fe 2 O 3 ], Na 0.75 Ca 0.25 Fe(Si 2 O 6 The saturation magnetization was 0.7 to 54.9 emu / cm. 2 In Example 4, the amount of Cd adsorbed from the simulated contaminated aqueous solution was 1%.

[0120] In Example 5, the thermoelectric conversion index ZT was 0.0002.

[0121] The crystallized glass of the present invention can be suitably used as a heavy metal recovery material for adsorbing and recovering heavy metals and as a soil conditioner. The crystallized glass of the present invention can also be suitably used as a water quality improvement material, an ion exchange material, an adsorbent, and a fertilizer additive. Furthermore, since the crystallized glass of the present invention can have both thermoelectric conversion function and electrical conductivity, it can be suitably used as a material for thermoelectric conversion components, semiconductor components, communication components, construction components, chemical reaction components, heat-resistant components, space components, medical components, and the like. Furthermore, since the crystallized glass of the present invention can be produced using glass cullet, it can contribute to the recycling and upcycling of glass products and contribute to the realization of a sustainable society.

Claims

1. Fe, by mass% 2 O 3 A crystallized glass containing 20 to 80% magnetic crystals.

2. The crystallized glass further contains, in mass%, SiO 2 0-80%, Al 2 O 3 0-80%, B 2 O 3 0-80%, P 2 O 5 0-80%, Li 2 O 0-50%, Na 2 O 0-50%, K 2 O 0-50%, MgO 0-50%, CaO 0-50%, SrO 0-50%, BaO 0-50%, ZnO 0-50%, ZrO 2 0-50%, HfO 2 0-50%, TiO 2 0-50%, SnO 2 0-50%, V 2 O 5 0-50%, NiO 0-80%, Cr 2 O 3 0-80%, MoO 3 The crystallized glass according to claim 1, containing 0 to 80%.

3. SnO (by mass%) 2 +Fe 2 O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3 The crystallized glass according to claim 1 or 2, containing 20% ​​or more of ZnO.

4. Mass percent ratio: K 2 O / (Li 2 O+Na 2 O+K 2 3. The crystallized glass according to claim 1, wherein O) is 0.01 to 0.

99.

5. In mass percent, (SiO 2 +P 2 O 5 ) / (SiO 2 +Al 2 O 3 +P 2 O5 3. The crystallized glass according to claim 1, wherein the value of n is 0.01 to 0.

99.

6. SiO by mass percentage 2 / (B 2 O 3 +P 2 O 5 + ZrO 2 + HfO 2 + TiO 2 + SnO 2 3. The crystallized glass according to claim 1, wherein n is 0.1 to 10,000.

7. SiO by mass percentage 2 3. The crystallized glass according to claim 1, wherein / (MgO+CaO+SrO+BaO+ZnO) is 0.1 to 10,000.

8. SiO 2 / (SnO 2 +Fe 2 O 3 +V 2 O 5 + NiO + Cr 2 O 3 +MoO 3 3. The crystallized glass according to claim 1, wherein n is 0.01 to 10.

9. MoO 3 The crystallized glass according to claim 1 or 2, containing more than 0%.

10. The crystallized glass according to claim 1 or 2, containing, by mass%, 100 ppm or less of Pt.

11. The crystallized glass according to claim 1 or 2, containing, by mass%, 100 ppm or less of Rh.

12. The crystallized glass according to claim 1 or 2, wherein the β-OH value of the original glass before crystallization is greater than 0 and less than 2 / mm.

13. The crystallized glass according to claim 1 or 2, which has an absolute value of Seebeck coefficient of 0.000001 V / K or more at any one or more temperature points between 25° C. and 400° C.

14. The crystallized glass according to claim 1 or 2, which has a thermoelectric conversion index ZT of 0.00001 or more at any one or more temperature points between 25° C. and 400° C.

15. Carrier mobility is 0.0001 cm 2The crystallized glass according to claim 1 or 2, wherein Vs is greater than or equal to 1. / Vs.

16. The crystallized glass according to claim 1 or 2, which is used as a heavy metal recovery material.

17. Fe, by mass% 2 O 3 A heavy metal recovery material comprising 20-80% crystallized glass containing magnetic crystals.

18. Fe, by mass% 2 O 3 A soil conditioner comprising 20-80% crystallized glass containing magnetic crystals.

19. A method for producing crystallized glass according to claim 1 or 2, comprising the steps of: 2 O 3 A method for producing crystallized glass, comprising: a melting step of melting a mixture of raw materials; and a crystallization step of forming the molten glass into a predetermined shape to obtain crystallized glass.

20. A method for recovering heavy metals, comprising: an adsorption step of adsorbing heavy metals to crystallized glass containing magnetic crystals; and a recovery step of recovering the crystallized glass after the heavy metals have been adsorbed thereto, using a magnet.

21. The method for recovering heavy metals according to claim 20, for recovering heavy metals in soil.

Citation Information

Patent Citations

  • Ceramic heat generating substance for hot heat curing and manufacture thereof

    JP1990088059A

  • Magnetic crystallized glass

    JP2001287930A

  • Water purification using magnetic nanoparticles

    JP2012507153A

  • Magnetizable glass ceramic composition and methods thereof

    US20170341975A1