Cylindrical secondary battery
The cylindrical secondary battery employs a strategically distributed filler layer with resin particles to prevent positive electrode extension, addressing capacity loss concerns and maintaining efficiency.
Patent Information
- Application Number
- PCT/JP2024/018803
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-22
- Publication Date
- 2024-12-05
AI Technical Summary
Cylindrical secondary batteries face the challenge of suppressing the extension of the positive electrode in the width direction during charge/discharge cycles without compromising battery capacity, as increased resin particles in the separator filler layer can lead to decreased capacity.
A cylindrical secondary battery design where the separator has a filler layer with resin particles forming convex portions that protrude towards the positive electrode, with a specific area ratio distribution across the electrode facing range, optimizing the placement and quantity of resin particles to enhance adhesion and resistance while maintaining capacity.
Effectively suppresses the elongation of the positive electrode while minimizing the decrease in battery capacity by strategically distributing resin particles, ensuring increased resistance without compromising overall performance.
Smart Images

Figure JP2024018803_05122024_PF_FP_ABST
Abstract
Description
Cylindrical secondary battery
[0001] The present disclosure relates to a cylindrical secondary battery.
[0002] Patent Document 1 describes a cylindrical secondary battery. The cylindrical secondary battery is a battery in which an electrode assembly, in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, is housed in a cylindrical outer can. The positive electrode and the negative electrode each have a current collector and a mixture layer disposed on the surface of the current collector, and the mixture layer contains an active material capable of reversibly absorbing and releasing Li ions.
[0003] Japanese Patent Application Publication No. 10-261439
[0004] During charging, in cylindrical secondary batteries, lithium migrates to the negative electrode, absorbing Li ions into the carbon, causing expansion. However, the positive electrode, which remains almost constant in volume, is pressed against the negative electrode and stretches. In particular, in cylindrical secondary batteries, the inner peripheral portion of the electrode assembly exerts a high surface pressure on the positive electrode, potentially causing the inner peripheral portion of the positive electrode to stretch significantly in the width direction, corresponding to the winding axis direction of the electrode assembly. To prevent this stretch, a separator may be provided with a filler layer facing the positive electrode, and the filler layer may contain resin particles that form protrusions toward the positive electrode. However, the greater the amount of resin particles, the lower the battery capacity.
[0005] An object of the present disclosure is to provide a cylindrical secondary battery that can suppress the extension of the positive electrode in the width direction while suppressing a decrease in battery capacity.
[0006] a cylindrical secondary battery according to one embodiment of the present disclosure, the cylindrical secondary battery including: an electrode assembly in which a positive electrode and a negative electrode are wound with a separator interposed therebetween; a non-aqueous electrolyte; and a cylindrical outer can accommodating the electrode assembly and the non-aqueous electrolyte; the positive electrode has a positive electrode current collector and a positive electrode mixture layer disposed on the surface of the positive electrode current collector; the separator includes a base layer and a filler layer disposed on the surface of the base layer facing the positive electrode; the filler layer has resin particles that form convex portions that protrude toward the positive electrode; and the cylindrical secondary battery includes a positive electrode facing range on the surface of the separator from a position facing the winding start end of the positive electrode mixture layer to a position facing the winding end end of the positive electrode mixture layer, a first region that extends from the winding start end of the positive electrode facing range to one-third of the total length of the positive electrode facing range in the longitudinal direction, and a second region that extends to the remaining range of the positive electrode facing range.
[0007] According to the cylindrical secondary battery according to the present disclosure, it is possible to suppress the elongation of the positive electrode while suppressing the decrease in battery capacity.
[0008] 1 is a longitudinal cross-sectional view of a cylindrical secondary battery that is an example of an embodiment. 2 is a front view showing a developed state of a positive electrode and a negative electrode that constitute an electrode body provided in the cylindrical secondary battery of FIG. 1. 3 is a cross-sectional view of the electrode body cut along the positive electrode longitudinal direction, schematically showing the arrangement of the positive electrode, negative electrode, and separator that constitute the electrode body shown in FIG. 2. 4 is a cross-sectional view of the electrode body cut along the positive electrode width direction, showing (a) the arrangement state of the positive electrode, negative electrode, and separator that constitute the inner peripheral side portion of the electrode body of a cylindrical secondary battery of a comparative example before charge / discharge cycles and (b) the arrangement state after a predetermined number of charge / discharge cycles have been repeated. 5 is a cross-sectional view of the electrode body cut along the positive electrode width direction, showing (a) the arrangement state of the positive electrode, negative electrode, and separator that constitute the inner peripheral side portion of the electrode body of a cylindrical secondary battery of an embodiment before charge / discharge cycles and (b) the arrangement state after a predetermined number of charge / discharge cycles have been repeated.
[0009] In cylindrical secondary batteries, it is believed that the positive electrode is pushed by the negative electrode and expands significantly in the radial direction during charge-discharge cycles. To suppress this widthwise expansion of the positive electrode, a separator may be provided with a filler layer facing the positive electrode, and the filler layer may contain resin particles that form protrusions that protrude toward the positive electrode. However, the greater the amount of resin particles, the lower the battery capacity. The inventors conducted extensive research and found that, on the surface of a separator, the positive electrode-facing region extends from the position facing the winding start end of the positive electrode mixture layer to the position facing the winding end end of the positive electrode mixture layer, the region extending from the winding start end of the positive electrode-facing region to one-third of the longitudinal length of the positive electrode-facing region is defined as a first region, and the remaining region of the positive electrode-facing region is defined as a second region. By increasing the area ratio of the resin particles forming the protrusions in the first region compared to the area ratio of the resin particles forming the protrusions in the second region, it is possible to suppress expansion of the positive electrode while suppressing a decrease in battery capacity.
[0010] An example of an embodiment of a cylindrical secondary battery according to the present disclosure will be described in detail below with reference to Figures 1 to 3. In the following description, specific shapes, materials, numerical values, directions, etc. are examples for facilitating understanding of the present invention and can be appropriately changed according to the specifications of the cylindrical secondary battery. Furthermore, when multiple embodiments and variations are included in the following description, it is assumed from the beginning that their characteristic features will be used in appropriate combination. Furthermore, in this specification, the term "substantially" is used to mean, for example, not only when something is completely the same, but also when it can be considered to be substantially the same.
[0011] Fig. 1 is a longitudinal cross-sectional view of a cylindrical secondary battery 10 (hereinafter referred to as secondary battery 10) according to an embodiment. In the secondary battery 10 shown in Fig. 1, an electrode assembly 14 and a non-aqueous electrolyte (not shown) are housed in an outer can 16. For ease of explanation, the following description will be given with the sealing body 17 side referred to as "top" and the bottom side of the outer can 16 referred to as "bottom."
[0012] The electrode assembly 14 has a wound structure in which the positive electrode 11 and the negative electrode 12 are wound with a separator 13 interposed therebetween. The positive electrode 11, the negative electrode 12, and the separator 13 are all long strips, and are spirally wound so as to be alternately stacked in the radial direction of the electrode assembly 14. The separator 13 is formed to be slightly larger than the positive electrode 11 and the negative electrode 12, and two separators 13 are arranged to sandwich the positive electrode 11.
[0013] As the non-aqueous solvent (organic solvent) of the non-aqueous electrolyte, carbonates, lactones, ethers, ketones, esters, etc. can be used, and two or more of these solvents can be mixed and used. When two or more solvents are mixed and used, it is preferable to use a mixed solvent containing a cyclic carbonate and a chain carbonate. For example, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used as the cyclic carbonate, and dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), etc. can be used as the chain carbonate. As the electrolyte salt of the non-aqueous electrolyte, LiPF 6 , LiBF 4 , LiCF 3 SO 3 The amount of electrolyte salt dissolved in the non-aqueous solvent may be, for example, 0.5 mol / L or more and 2.0 mol / L or less.
[0014] The sealing body 17 seals the opening at the top end of the outer can 16, thereby sealing the interior of the secondary battery 10. An upper insulating plate 18 and a lower insulating plate 19 are provided above and below the electrode body 14. The positive electrode tab 20 extends vertically through a through-hole in the upper insulating plate 18 and connects a terminal plate 23, which is the bottom plate of the sealing body 17, to the positive electrode 11 included in the electrode body 14. This connects the positive electrode 11 to the sealing body 17, and in the secondary battery 10, the cap 27, which is the top plate of the sealing body 17 and is electrically connected to the terminal plate 23, serves as the positive electrode terminal. The positive electrode tab 20 is, for example, an aluminum tab. On the other hand, the negative electrode tab 21 extends through a through-hole in the lower insulating plate 19 toward the bottom of the outer can 16 and is welded to the inner bottom surface of the outer can 16. This connects the negative electrode 12 to the outer can 16, and in the secondary battery 10, the outer can 16 serves as the negative electrode terminal. The negative electrode tab 21 is, for example, a nickel tab.
[0015] The positive electrode tab 20 is provided in the longitudinal center of the positive electrode 11 at a position away from the winding start end and winding end end of the electrode body 14 .
[0016] The negative electrode tab 21 is provided at one longitudinal end of the negative electrode 12 located on the winding start side of the negative electrode 12. The negative electrode 12 has a first negative electrode exposed portion 42 (see FIG. 2 ) that is provided at the winding start end and exposes the negative electrode current collector 40. The negative electrode tab 21 is joined to the first negative electrode exposed portion 42.
[0017] The negative electrode 12 is disposed on the outermost peripheral surface of the electrode assembly 14, and a second negative electrode exposed portion 44 is provided where the surface of the negative electrode current collector 40 is exposed. The negative electrode exposed portion 44 abuts against the inner peripheral surface of the outer can 16. The abutment of the negative electrode exposed portion 44 with the inner peripheral surface of the outer can 16, which serves as the negative electrode terminal, electrically connects both longitudinal ends of the negative electrode 12 to the outer can 16, ensuring good current collection. The negative electrode exposed portion 44 may be provided on a portion of the outermost peripheral surface of the electrode assembly 14, but is preferably provided over the entire outermost peripheral surface. For example, the negative electrode exposed portion is provided on both sides of the negative electrode current collector 40 over a length of at least one revolution of the electrode assembly 14 from the winding end of the negative electrode 12.
[0018] The position of the negative electrode tab is not limited to the examples shown in FIGS. 1 and 2 , and the negative electrode tab may be provided only near the winding end of the negative electrode 12, or may be provided near both the winding start end and the winding end end of the negative electrode 12.
[0019] The exterior can 16 is a cylindrical metal container with a bottom and an opening on one axial side. A gasket 28 is provided between the exterior can 16 and the sealing body 17 to ensure the sealing of the interior of the secondary battery 10. The exterior can 16 has a grooved portion 22 that supports the sealing body 17 and is formed, for example, by pressing the side surface from the outside. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior can 16, and supports the sealing body 17 on its upper surface.
[0020] The sealing body 17 includes a terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27, which are stacked in this order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disk or ring shape, and all components except for the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, with the insulating member 25 interposed between their respective peripheral edges. If the internal pressure of the battery increases due to abnormal heat generation, for example, the lower valve body 24 may break, causing the upper valve body 26 to bulge toward the cap 27 and separate from the lower valve body 24, thereby cutting off the electrical connection between them. If the internal pressure continues to increase, the upper valve body 26 may break, and gas may be released from the opening of the cap 27.
[0021] Next, the positive electrode 11 and the negative electrode 12 will be described with reference to Fig. 2. Fig. 2 is a front view showing the positive electrode 11 and the negative electrode 12 constituting the electrode body 14 provided in the secondary battery 10 of Fig. 1 in a developed state. As shown in Fig. 2, the negative electrode 12 is generally formed to have dimensions slightly larger than the positive electrode 11 in order to prevent lithium precipitation. That is, the negative electrode 12 is formed to be longer than the positive electrode 11 in the longitudinal and width directions.
[0022] The positive electrode 11 has a positive electrode current collector 30 and a positive electrode mixture layer 31 disposed on the surface of the positive electrode current collector 30. In addition, a positive electrode exposed portion 34 where the positive electrode current collector 30 is exposed is disposed in the longitudinal center of the positive electrode 11.
[0023] A foil of a metal such as aluminum that is stable in the potential range of the positive electrode, a film having such a metal disposed on the surface layer, or the like can be used for the positive electrode current collector 30. The thickness of the positive electrode current collector 30 is, for example, 10 μm or more and 30 μm or less.
[0024] The positive electrode mixture layer 31 is preferably formed on both sides of the positive electrode current collector 30. The thickness of the positive electrode mixture layer 31 is, for example, 10 μm or more and 150 μm or less on one side of the positive electrode current collector 30. The positive electrode mixture layer 31 includes, for example, a positive electrode active material, a conductive agent, and a binder. The positive electrode can be produced, for example, by applying a positive electrode mixture slurry including a positive electrode active material, a conductive agent, a binder, etc. to both sides of the positive electrode current collector 30, drying the coating, and then rolling the coating using a roller or the like.
[0025] The positive electrode active material contained in the positive electrode mixture layer 31 can be, for example, a lithium transition metal composite oxide containing a transition metal element such as Co, Mn, or Ni. x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co y Ni 1-y O 2 , Li x Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn 2 O 4 , Li x Mn 2-y M y O 4 , LiMPO 4 , Li 2 MPO 4 F (M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, and 0<x≦1.2, 0<y≦0.9, and 2.0≦z≦2.3). These may be used alone or in combination.
[0026] The positive electrode active material preferably contains a lithium nickel composite oxide, since this can increase the capacity of the secondary battery 10. The lithium nickel composite oxide is preferably Li x NiO 2 , Li x Co y Ni 1-y O 2 , Li x Ni 1-y M y O z (M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B; 0<x≦1.2, 0<y≦0.9, 2.0≦z≦2.3) The higher the Ni content of the lithium nickel composite oxide, the higher the capacity.
[0027] Examples of the conductive agent contained in the positive electrode mixture layer 31 include carbon-based particles such as carbon black (CB), acetylene black (AB), ketjen black, carbon nanotubes (CNT), graphene, and graphite. These may be used alone or in combination of two or more.
[0028] Examples of the binder contained in the positive electrode mixture layer 31 include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, polyolefin-based resins, etc. These may be used alone or in combination of two or more.
[0029] The negative electrode 12 has a negative electrode current collector 40 and a negative electrode mixture layer 41 disposed on the surface of the negative electrode current collector 40. The negative electrode current collector 40 may be a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a film having such a metal disposed on its surface. The thickness of the negative electrode current collector 40 is, for example, 5 μm or more and 30 μm or less.
[0030] The negative electrode mixture layer 41 is preferably formed on both sides of the negative electrode current collector 40. The thickness of the negative electrode mixture layer 41 is, for example, 10 μm or more and 150 μm or less on one side of the negative electrode current collector 40. The negative electrode mixture layer 41 contains, for example, a negative electrode active material and a binder. The negative electrode can be produced, for example, by applying a negative electrode mixture slurry containing the negative electrode active material, the binder, and the like to both sides of the negative electrode current collector 40, drying the coating, and then rolling the coating using a roller or the like.
[0031] The negative electrode active material contained in the negative electrode mixture layer 41 is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, a carbon material such as graphite is used. The graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, and artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads.
[0032] As the negative electrode active material, metals that can be alloyed with Li, such as Si and Sn, metal compounds containing Si, Sn, etc., and lithium-titanium composite oxides may be used. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.
[0033] Examples of the binder contained in the negative electrode mixture layer 41 include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.
[0034] Next, the separator 13 will be described with reference to Fig. 3. The separator 13 isolates the positive electrode 11 and the negative electrode 12 from each other and prevents the positive electrode 11 and the negative electrode 12 from coming into contact with each other, thereby preventing a short circuit from occurring. Fig. 3 is a cross-sectional view of the electrode assembly 14 taken along the longitudinal direction of the positive electrode, for illustrating the arrangement of the positive electrode 11, the negative electrode 12, and the separator 13 that constitute the electrode assembly 14 shown in Fig. 2.
[0035] 3 , the separator 13 has a substrate layer 50 and a filler layer 52 disposed on the surface of the substrate layer 50 facing the positive electrode 11. In this embodiment, the filler layer 52 is disposed on only one surface of the substrate layer 50, with the filler layer 52 facing the positive electrode 11 and the substrate layer 50 facing the negative electrode 12. Note that the form of the separator 13 is not limited to the example shown in FIG. 3 , and the filler layer 52 may be disposed on both surfaces of the substrate layer 50.
[0036] The substrate layer 50 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of porous sheets include a microporous thin film, a woven fabric, and a nonwoven fabric. The material of the substrate layer 50 is not particularly limited, but examples include polyolefins such as polyethylene, polypropylene, and copolymers of polyethylene and α-olefins, acrylic resins, polystyrene, polyesters, cellulose, polyimides, polyphenylene sulfide, polyether ether ketones, and fluororesins. The substrate layer 50 may have a single-layer structure or a multi-layer structure. The thickness of the substrate layer 50 is preferably 3 μm or more and 20 μm or less, and more preferably 5 μm or more and 15 μm or less.
[0037] The filler layer 52 includes resin particles 54, inorganic particles, and a binder. The filler layer 52 also has protrusions 56 formed by the resin particles 54, and the protrusions 56 protrude from the positive electrode side surface of an inorganic particle layer 57 of the filler layer 52 formed by inorganic particles and a binder. As a result, the protrusions 56 protruding toward the positive electrode 11 side are formed on the surface of the filler layer 52. The resin particles 54 forming the protrusions 56 may be in contact with the base layer 50 of the separator 13.
[0038] Examples of inorganic particles include metal oxide particles, metal nitride particles, metal fluoride particles, and metal carbide particles. Examples of metal oxide particles include aluminum oxide, titanium oxide, magnesium oxide, zirconium oxide, nickel oxide, silicon oxide, and manganese oxide. Examples of metal nitride particles include titanium nitride, boron nitride, aluminum nitride, magnesium nitride, and silicon nitride. Examples of metal fluoride particles include aluminum fluoride, lithium fluoride, sodium fluoride, magnesium fluoride, calcium fluoride, and barium fluoride. Examples of metal carbide particles include silicon carbide, boron carbide, titanium carbide, and tungsten carbide. Furthermore, inorganic particles include zeolite (M 2/n O.Al 2 O 3 xSiO 2 ・yH 2 O, M is a metal element, n is the valence of M, x≧2, y≧0), porous aluminosilicates such as talc (Mg 3 Si 4 O 10 (OH) 2 ), layered silicates such as barium titanate (BaTiO 3 ), strontium titanate (SrTiO 3 ), or other minerals. These may be used alone or in combination of two or more. The binder is preferably a polymer material, and examples thereof include fluorine-based resins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE), polyimide-based resins, polyamide-based resins, acrylic resins, polyolefin-based resins, styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof, and polyvinyl alcohol (PVA). These may be used alone or in combination of two or more.
[0039] Examples of materials for the resin particles 54 include acrylic resins made of ethylenically unsaturated carboxylic acid alkyl esters such as methyl acrylate, butyl acrylate, ethyl acrylate, and 2-ethylhexyl acrylate; resins made of cyano group-containing ethylenically unsaturated monomers such as acrylonitrile; and resins made of ethylenically unsaturated carboxylic acids and salts thereof such as acrylic acid, methacrylic acid, and maleic acid.
[0040] The resin particles 54 have adhesive properties with the positive electrode 11, and in the secondary battery 10, the resin particles 54 are preferably adhered to the positive electrode. By adhering the resin particles 54 to the positive electrode 11, movement of the positive electrode 11 due to charge and discharge is significantly suppressed. As a result, even when the expansion of the negative electrode during charge causes the positive electrode 11, particularly the inner peripheral portion thereof, to be pushed by the negative electrode 12 and tends to expand in the width direction, the effect of suppressing expansion of the positive electrode 11 in the width direction is significant. The resin particles 54 exhibit adhesive properties to the positive electrode 11, for example, when a non-aqueous electrolyte is held therein.
[0041] On the surface of the separator 13 facing the filler layer 52, a positive electrode-facing region 60 extends from a position facing the winding start end S of the positive electrode mixture layer 31 to a position facing the winding end E of the positive electrode mixture layer 31. A first region 58 extends from the winding start end S of the positive electrode-facing region 60 to one-third of the total length L of the positive electrode-facing region 60, and a second region 59 extends the remaining region of the positive electrode-facing region 60. In this case, an area ratio S1 of the area occupied by the resin particles 54 in the first region 58 is greater than an area ratio S2 of the area occupied by the resin particles 54 in the second region 59 (S1 > S2). When the electrode body 14 is formed, a boundary C between the first region and the second region is located approximately in the radial center between the inner and outer circumferential surfaces of the electrode body.
[0042] By making S1 > S2, the contact area of the protrusions 56 formed by the resin particles 54 in the first region 58 with the positive electrode 11 can be increased, thereby increasing the resistance to movement of the positive electrode 11. This makes it possible to suppress the expansion of the positive electrode 11 in the width direction. At the same time, the amount of resin particles 54 provided over the entire separator 13 can be suppressed, thereby suppressing a decrease in battery capacity.
[0043] S1 is preferably 2% or more and 20% or less, more preferably 4% or more and 16% or less, and S2 is preferably 0% or more and 10% or less, more preferably 0% or more and 8% or less.
[0044] During production of the separator 13, for example, the average particle size (D50) of the resin particles 54 contained in the first region 58 can be made larger than the D50 of the resin particles 54 contained in the second region 59, thereby making S1 > S2. Furthermore, during production of the separator 13, for example, the average particle sizes (D50) of the resin particles 54 contained in the first region 58 and the second region 59 can be made substantially the same, while the number of resin particles 54 contained in the first region 58 can be made larger than the number of resin particles 54 contained in the second region 59, thereby making S1 > S2. The D50 of the resin particles used during production of the separator 13 is, for example, 1 μm or more and 10 μm or less. In this specification, the average particle size (D50) refers to the particle size at which the cumulative frequency of the smallest particle size in a volume-based particle size distribution is 50%, and is also referred to as the median diameter. The particle size distribution of the resin particles is measured by dispersing the resin particles in a dispersion medium using a laser diffraction particle size distribution measuring device (for example, MT3000II manufactured by Microtrac Bell).
[0045] The average particle area of the protrusions 56 in the first region 58 is preferably larger than the average particle area of the protrusions 56 in the second region 59. The average particle area of the protrusions 56 in the first region 58 is, for example, 500 μm 2 2000 μm or more 2 The average grain area of the convex portion 56 in the second region 59 is, for example, 0 μm 2 1500 μm or more 2 Here, the average particle area refers to the average area per resin particle measured using the separator 13 removed from the secondary battery 10. Specifically, the surface of the filler layer 52 is observed with a scanning electron microscope (e.g., SU8220 manufactured by Hitachi High-Technologies Corporation), and the average particle area is calculated by averaging the sum of the areas of all the convex portions in portions of a predetermined area at multiple randomly selected positions in each of the first region 58 and the second region 59 by the number of convex portions, and then averaging the average particle area by the number of portions of the predetermined area for each of the regions 58 and 59.
[0046] Next, the effects obtained by the secondary battery 10 of the embodiment will be described in comparison with a secondary battery of a comparative example using Figures 4 and 5. Figures 4 and 5 are cross-sectional views of the electrode body 14 taken along the width direction of the positive electrode, showing the arrangement of the positive electrode 11, negative electrode 12, and separator 13 constituting the inner peripheral portion of the electrode body 14 of the secondary battery 10 before charge-discharge cycles (a) and the arrangement after a predetermined number of charge-discharge cycles (b) in the comparative example and the embodiment, respectively.
[0047] 4 , in the secondary battery of the comparative example, the separator 13 a has a base material layer 50 and a filler layer 52 disposed on the surface of the base material layer 50 facing the positive electrode 11, but the filler layer 52 does not contain resin particles but contains inorganic particles and a binder. The other configurations of the cylindrical secondary battery of the comparative example are similar to those of the cylindrical secondary battery 10 of the embodiment.
[0048] In such a comparative example, as shown in Fig. 4(a), the widthwise length of the negative electrode 12 is greater than the widthwise length of the positive electrode 11. On the other hand, in a state after a predetermined number of charge-discharge cycles have been repeated, as shown in Fig. 4(b), the electrodes, particularly the negative electrode 12, expand during charging, increasing the stress and surface pressure applied to the inner periphery of the electrode body in particular, and this may cause the positive electrode 11 to be pressed from both radial sides by the negative electrode 12 via the separator 13a, resulting in an increased widthwise extension D1.
[0049] On the other hand, in this embodiment, as shown in FIG. 5A , convex portions 56 formed of resin particles 54 protrude from the filler layer 52 of the separator 13 facing the positive electrode 11 toward the positive electrode 11 and are pressed against the positive electrode 11. This suppresses widthwise movement of the positive electrode 11 due to the adhesiveness of the convex portions 56, etc. In particular, the area ratio S1 of the area occupied by the resin particles 54 in the first region 58 corresponding to the approximately inner circumferential portion of the electrode body is greater than the area ratio S2 of the area occupied by the resin particles 54 in the second region 59 corresponding to the approximately outer circumferential portion. This increases the resistance of the convex portions 56 to the widthwise movement of the positive electrode 11 in the inner circumferential portion of the electrode body. This suppresses widthwise expansion of the positive electrode 11, and the widthwise expansion amount D2 can be made smaller than the widthwise expansion amount D1 in the comparative example.
[0050] Furthermore, by making the area ratio S2 of the resin particles 54 contained in the substantially outer peripheral portion of the electrode body smaller than the area ratio S1 of the resin particles 54 contained in the substantially inner peripheral portion of the electrode body, it is possible to suppress an increase in the outer diameter due to the protrusions 56 of the electrode body, and therefore it is possible to suppress a decrease in battery capacity.
[0051] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0052] Example 1 [Preparation of Positive Electrode] As the positive electrode active material, LiNi 0.88 Co 0.09 Al 0.03 O 2 Aluminum-containing lithium nickel cobalt oxide represented by the formula (I) was used. 100 parts by mass of the positive electrode active material, 1 part by mass of acetylene black (AB), and 0.9 parts by mass of polyvinylidene fluoride (PVDF) were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry was applied to both sides of a strip-shaped positive electrode current collector made of aluminum foil with a thickness of 15 μm, so that a positive electrode exposed portion was formed. This coating was dried in a dryer at a temperature of 100 to 150 °C, and the NMP was removed, followed by rolling using a roll press. The resulting electrode was then cut to a predetermined electrode plate size to produce a positive electrode with a positive electrode mixture layer formed on both sides of the positive electrode current collector. The positive electrode had a thickness of 0.144 mm, a width of 62.6 mm, and a length of 861 mm. An aluminum positive electrode tab was then welded to the positive electrode exposed portion.
[0053] [Preparation of Negative Electrode] 95 parts by mass of graphite powder and 5 parts by mass of Si oxide (SiO ) were mixed, followed by mixing 1 part by mass of sodium carboxymethyl cellulose (CMC-Na) and 1 part by mass of styrene butadiene rubber (SBR), and an appropriate amount of water was added to prepare a negative electrode mixture slurry. Next, the negative electrode mixture slurry was applied to both sides of a strip-shaped negative electrode current collector made of copper foil with a thickness of 8 μm, dried, and then rolled using a roller. Thereafter, it was cut to a predetermined electrode plate size to prepare a negative electrode in which a negative electrode mixture layer was formed on both sides of the negative electrode current collector. The negative electrode had a thickness of 0.160 mm, a width of 64.2 mm, and a length of 959 mm. Thereafter, a negative electrode exposed portion where no mixture layer was present and the current collector surface was exposed was provided at the end of the winding start side of the negative electrode, and a nickel negative electrode tab was welded to the negative electrode exposed portion.
[0054] [Preparation of separator] Alumina (α-Al) was used as inorganic particles having an average particle size (D50) of 0.7 μm. 2 O 3 A first dispersion was prepared by mixing acrylic resin particles having a D50 of 4 μm, acrylic resin particles as resin particles, and an acrylic acid ester-based binder emulsion in a solids mass ratio of 100:2:3, and then adding an appropriate amount of water to adjust the solids concentration to 10% by mass. A second dispersion was prepared in the same manner as the first dispersion, except that the amount of acrylic resin particles added was changed from 2 parts by mass to 1 part by mass.
[0055] A 12 μm-thick porous polyethylene substrate was used as the substrate layer. On the surface of the porous substrate serving as the substrate layer, a first dispersion was applied to a first region 58, which was a region from the winding start end of the positive electrode facing region 60 to one-third of the total length in the longitudinal direction. A second dispersion was applied to a second region 59, which was the remaining region of the positive electrode facing region 60. The coating was then dried by heating in an oven at 50° C. for 4 hours, forming a filler layer in which acrylic resin particles protruded from the surface of a 3 μm-thick inorganic particle layer formed by the binder.
[0056] [Preparation of non-aqueous electrolyte] 5 parts by mass of vinylene carbonate (VC) was added to 100 parts by mass of a mixed solvent in which ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed at a volume ratio of 1:3, to prepare a non-aqueous electrolyte solution containing lithium hexafluorophosphate (LiPF6 A non-aqueous electrolyte was prepared by dissolving 1.5 mol / L of ammonium hydroxide in water.
[0057] [Fabrication of Secondary Battery] A wound electrode assembly was fabricated by spirally winding the positive and negative electrodes with a separator interposed therebetween. At this time, the filler layer of the separator faced the positive electrode. Insulating plates were placed on the top and bottom of the electrode assembly, respectively, and the electrode assembly was housed in an outer can. The negative electrode tab was welded to the bottom of a cylindrical outer can with a bottom, and the positive electrode tab was welded to a sealing member. After injecting a nonaqueous electrolyte into the outer can using a reduced pressure method, the opening of the outer can was sealed with a sealing member via a gasket, and the cylindrical secondary battery of Example 1 was fabricated.
[0058] [Charge-Discharge Cycle Test] The secondary battery was charged at a constant current of 0.3 It (1380 mA) in a 25°C environment until the battery voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current reached 0.02 It (92 mA). After a 20-minute pause, the battery was discharged at a constant current of 0.5 It (2300 mA) until the battery voltage reached 2.5 V. The discharge capacity at this time was defined as the initial capacity. The initial capacity of Example 1 was 4600 mAh. This charge-discharge cycle was repeated 100 times, with a 20-minute pause between each cycle.
[0059] [Evaluation of electrode plate elongation] The secondary battery after the above charge / discharge cycle test was charged at a constant current of 0.3 It (1380 mA) until the battery voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current reached 0.02 It (92 mA). Thereafter, the secondary battery was subjected to cross-sectional observation along the winding axis direction of the electrode body using an X-ray CT device (Shimadzu Corporation, SMX-225CT FPD HR) to evaluate whether or not elongation in the width direction of the positive electrode had occurred, and if so, the level of the amount of elongation.
[0060] Comparative Example 1 A secondary battery was produced and evaluated in the same manner as in Example 1, except that in the preparation of the separator, the amount of acrylic resin particles added in the second dispersion was changed from 1 part by mass to 2 parts by mass.
[0061] Comparative Example 2 A secondary battery was produced and evaluated in the same manner as in Example 1, except that in the preparation of the separator, the amount of acrylic resin particles added in the first dispersion was changed from 2 parts by mass to 1 part by mass.
[0062] Comparative Example 3 A secondary battery was produced and evaluated in the same manner as in Example 1, except that in producing the separator, acrylic resin particles were not added to the first dispersion liquid and the second dispersion liquid.
[0063] Table 1 shows the evaluation results of the secondary batteries according to the examples and comparative examples. The level of the positive electrode elongation was divided into three levels, with the minimum level designated as A, the maximum level designated as C, and the intermediate level designated as B. Table 1 also shows the occupied area ratio of the resin particles contained in the first region and the occupied area ratio of the resin particles contained in the second region, measured using a separator removed from a cylindrical secondary battery after a charge-discharge cycle test. The occupied area ratio was determined by calculating the area ratio of the resin particles in a plurality of randomly selected predetermined area portions in each of the first and second regions, and averaging the area ratios by the number of predetermined area portions. Table 1 also shows the measurement results of the initial capacity (battery capacity) of the secondary batteries according to the examples and comparative examples. In Table 1, the values are shown relative to the battery capacity of Comparative Example 3, which is set to 100.
[0064]
[0065] In the secondary batteries of Example 1 and Comparative Example 1, the positive electrode elongation level was Level A. This is thought to be due to the large occupied area ratio of the resin particles in the first region of the separator, at 16%. On the other hand, the occupied area ratio of the resin particles in the first region was small, at 8%, in Comparative Example 2, and 0% in Comparative Example 3, resulting in poorer positive electrode elongation levels, at Level B and Level C. Furthermore, in the secondary battery of Example 1, the occupied area ratio of the resin particles in the second region of the separator was small, at 8%, so the decrease in battery capacity was suppressed to 2%, which is approximately the same as that of Comparative Example 3, in which no resin particles were added to the separator. On the other hand, in Comparative Example 1, in which the occupied area ratio of the resin particles in the second region was large, at 16%, the battery capacity was significantly reduced compared to Comparative Example 3.
[0066] The present disclosure will be further described by the following embodiments. Configuration 1: A cylindrical secondary battery including an electrode assembly in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, a non-aqueous electrolyte, and a cylindrical outer can accommodating the electrode assembly and the non-aqueous electrolyte, wherein the positive electrode has a positive electrode current collector and a positive electrode mixture layer disposed on a surface of the positive electrode current collector, the separator includes a base layer and a filler layer disposed on a surface of the base layer facing the positive electrode, and the filler layer has resin particles that form protrusions protruding toward the positive electrode, A cylindrical secondary battery in which, on the surface of the separator, a positive electrode-facing range is defined as a position facing the winding start end of the positive electrode mixture layer to a position facing the winding end end of the positive electrode mixture layer, a first region is defined as a range from the winding start end of the positive electrode-facing range to one-third of the total length of the positive electrode-facing range in the longitudinal direction, and a second region is defined as the remaining range of the positive electrode-facing range, the area ratio occupied by the resin particles in the first region is larger than the area ratio occupied by the resin particles in the second region. Configuration 2: The cylindrical secondary battery according to Configuration 1, in which the area ratio occupied by the resin particles in the first region is 2% or more and 20% or less, and the area ratio occupied by the resin particles in the second region is 0% or more and 10% or less. Configuration 3: The cylindrical secondary battery according to Configuration 1 or Configuration 2, in which the average particle area of the resin particles included in the first region is larger than the average particle area of the resin particles included in the second region. Configuration 4: The average particle area of the resin particles contained in the first region is 500 μm 2 2000 μm or more 2 the average particle area of the resin particles contained in the second region is 0 μm or less; 2 1500 μm or more 2 4. The cylindrical secondary battery according to claim 3, wherein:
[0067] REFERENCE SIGNS LIST 10 (cylindrical) secondary battery, 11 positive electrode, 12 negative electrode, 13, 13a separator, 14 electrode body, 16 outer can, 17 sealing body, 18 upper insulating plate, 19 lower insulating plate, 20 positive electrode tab, 21 negative electrode tab, 22 grooved portion, 23 terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 30 positive electrode current collector, 31 positive electrode mixture layer, 34 positive electrode exposed portion, 40 negative electrode current collector, 41 negative electrode mixture layer, 42 first negative electrode exposed portion, 44 second negative electrode exposed portion, 50 substrate layer, 52 filler layer, 54 resin particles, 56 convex portion, 58 first region, 59 second region, 60 positive electrode facing area.
Claims
1. A cylindrical secondary battery comprising an electrode assembly in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, a non-aqueous electrolyte, and a cylindrical exterior can accommodating the electrode assembly and the non-aqueous electrolyte, wherein the positive electrode comprises a positive electrode current collector and a positive electrode mixture layer disposed on a surface of the positive electrode current collector, the separator comprises a base layer and a filler layer disposed on a surface of the base layer facing the positive electrode, the filler layer comprises resin particles forming convex portions that protrude toward the positive electrode, and a positive electrode facing range on the surface of the separator is defined as a range from a position facing the winding start end of the positive electrode mixture layer to a position facing the winding end end of the positive electrode mixture layer, a range from the winding start end of the positive electrode facing range to a position facing the winding end end of the positive electrode facing range in the longitudinal direction is defined as a first region, and the remaining range of the positive electrode facing range is defined as a second region, the area ratio occupied by the resin particles in the first region is greater than the area ratio occupied by the resin particles in the second region, Cylindrical secondary battery.
2. The cylindrical secondary battery according to claim 1, wherein the area ratio of the resin particles in the first region is 2% or more and 20% or less, and the area ratio of the resin particles in the second region is 0% or more and 10% or less.
3. The cylindrical secondary battery according to claim 1, wherein an average particle area of the resin particles contained in the first region is larger than an average particle area of the resin particles contained in the second region.
4. The average particle area of the resin particles contained in the first region is 500 μm 2 2000 μm or more 2 The average particle area of the resin particles contained in the second region is 0 μm or less. 2 1500 μm or more 2 The cylindrical secondary battery according to claim 3 , wherein:
Citation Information
Patent Citations
Separator for lithium secondary battery and a method of making the same
KR1020160118979A
Non-aqueous electrolyte secondary battery and method of manufacturing non-aqueous electrolyte secondary battery
WO2019181286A1
Functional layer for electrochemical elements, separator with functional layer for electrochemical elements, and electrochemical element
WO2020175079A1
Separator, preparation method therefor, and related secondary battery thereof, and battery module, battery pack, and device
WO2022110227A1
Nonaqueous electrolyte secondary battery
WO2024043145A1