Power storage device and power storage device external packaging material

The use of heat-fusible resin films in the sealant layer of energy storage device exterior materials addresses the issue of insufficient gas barrier and sealing strength, ensuring effective prevention of water vapor and oxygen intrusion and maintaining device integrity at high temperatures.

WO2024247865A1PCT designated stage expired Publication Date: 2024-12-05RESONAC PACKAGING CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018948
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing exterior materials for all-solid-state batteries and other energy storage devices have insufficient gas barrier properties against water vapor and oxygen, particularly at the fused portions, and lack sufficient sealing strength, especially when exposed to high temperatures.

Method used

A sealant layer composed of heat-fusible resin films, such as polyvinylidene chloride, ethylene-vinyl alcohol copolymer, or high-density polyethylene, with specific permeability and sealing strength properties, is used to enhance gas barrier properties and ensure reliable sealing, preventing water vapor and oxygen intrusion.

Benefits of technology

The solution provides excellent gas barrier properties and sufficient sealing strength, preventing defects and harmful gas generation, even at high temperatures, while allowing for diverse packaging forms of energy storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018948_05122024_PF_FP_ABST
    Figure JP2024018948_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a power storage device external packaging material that has excellent gas barrier properties and that can ensure sufficient seal strength. A power storage device external packaging material 1 according to the present invention comprises: a resin substrate layer 11; a metal foil layer 12 that is laminated to an inner surface side of the substrate layer 11; and a sealant layer 13 that is laminated to an inner surface side of the metal foil layer 12 with an adhesive layer 22 therebetween. The sealant layer 13 has gas barrier properties with respect to water vapor and / or oxygen, has heat-resistant seal properties, and is constituted by a thermally fusible resin film, excluding polypropylene-based films.
Need to check novelty before this filing date? Find Prior Art

Description

Electricity storage device and exterior material for the same

[0001] The present invention relates to an electricity storage device such as an all-solid-state battery used as a high-power battery such as an in-vehicle battery, a battery for portable devices such as a mobile electronic device, or a battery for storing regenerative energy, and an exterior material for the electricity storage device.

[0002] In recent years, packaging materials with gas barrier properties that prevent the permeation of water vapor and oxygen have been used in the packaging fields of foods, beverages, pharmaceuticals, electronic components, etc., from the perspective of long-term storage and maintaining the quality of the contents, and in the display field, to prevent deterioration of display elements that are sensitive to water vapor and oxygen.

[0003] Meanwhile, development of all-solid-state batteries is progressing as one of the promising electronic components for the future. Because all-solid-state batteries use a solid electrolyte, they do not leak or produce dendrites, and their separators are not destroyed. Therefore, there is no risk of fire due to separator destruction, and they are attracting much attention from the perspective of safety. The basic structure of an exterior material for this all-solid-state battery includes a metal foil layer, a substrate layer laminated on the outside of the metal foil layer via an adhesive layer, and a sealant layer (thermal seal layer) laminated on the inside of the metal foil layer via the adhesive layer. For example, the all-solid-state battery body is sandwiched from above and below between a pair of exterior materials with the sealant layer sides facing each other, and the outer peripheries of the sealant layers are thermally sealed to encapsulate the all-solid-state battery body.

[0004] However, when a sulfide-based all-solid-state battery is enclosed as the all-solid-state battery main body, a problem occurs in that moisture entering from the outside reacts with the sulfide-based all-solid-state battery, generating hydrogen sulfide gas.

[0005] Therefore, as shown in the following Patent Documents 1 to 5, all-solid-state battery packaging materials with gas barrier properties have been proposed. The packaging material for all-solid-state batteries shown in Patent Document 1 is composed of a transparent gas barrier film and a sealant layer laminated thereon via a fluorine-based adhesive resin layer. Furthermore, the packaging material for all-solid-state batteries shown in Patent Document 2 uses a sealant layer with high hydrogen sulfide gas permeability to actively discharge hydrogen sulfide gas generated inside the battery to the outside and suppress an increase in internal pressure. Furthermore, the packaging material for all-solid-state batteries shown in Patent Document 3 uses a sealant layer with low hydrogen sulfide gas permeability to suppress leakage of hydrogen sulfide gas. Furthermore, the packaging material for all-solid-state batteries shown in Patent Document 4 contains a moisture absorbent and a gas absorbent in the sealant layer. Furthermore, the packaging material for all-solid-state batteries shown in Patent Document 5 has a gas barrier vapor deposition film layer laminated on the inner surface of the sealant layer, thereby providing a measure against the intrusion of oxygen and moisture from the outside.

[0006] Japanese Patent Application Publication No. 2011-230454, Japanese Patent No. 6777276, Japanese Patent No. 6747636, Japanese Patent Application Publication No. 2020-187855, Japanese Patent Application Publication No. 2020-187835

[0007] However, in the packaging materials for all-solid-state batteries shown in Patent Documents 1 to 4, the sealant layer is made of an olefin-based film such as unstretched polypropylene (CPP), and therefore there arises a problem that the gas barrier properties against the penetration of water vapor and oxygen from the outer peripheral edge face between the fused sealant layers along the fused portion between the sealant layers are insufficient.

[0008] Furthermore, in the packaging material for an all-solid-state battery shown in Patent Document 5, a gas barrier vapor deposition film is provided on the surface of the sealant, and therefore, the gas barrier property against water vapor and the like from the outer peripheral end face is good, but there is a problem in that the sealing strength at high temperatures is insufficient.

[0009] The above describes the issues with all-solid-state batteries, but similar issues may arise in other power storage devices.

[0010] The preferred embodiments of the present invention have been made in light of the above and / or other deficiencies in the related art, and provide significant improvements over existing methods and / or apparatus.

[0011] The present invention has been made in view of the above-mentioned problems, and aims to provide an electricity storage device and an exterior material for an electricity storage device that have excellent gas barrier properties against water vapor and oxygen and can ensure sufficient sealing strength between sealant layers.

[0012] Other objects and advantages of the present invention will be apparent from the following preferred embodiments.

[0013] In order to solve the above problems, the present invention comprises the following means.

[0014] [1] An exterior packaging material for an electricity storage device, comprising: a resin base layer; a metal foil layer laminated on the inner surface of the base layer; and a sealant layer laminated on the inner surface of the metal foil layer via an adhesive layer, wherein the sealant layer has gas barrier properties against water vapor and / or oxygen, and heat-resistant sealing properties, and is made of a heat-fusible resin film other than a polypropylene-based film.

[0015] [2] The sealant layer has a water vapor permeability of 5 g / m at 40°C and 90% RH. 2 The packaging material for an electricity storage device according to item 1, wherein the surface roughness is 24 hr / 15 μm or less.

[0016] [3] The sealant layer has an oxygen permeability of 5 cm at 20°C and 90% RH. 3 / m 2 3. The electrical storage device packaging material according to item 1 or 2, wherein the electrical resistance is 24 hr·atm / 15 μm or less.

[0017] [4] The packaging material for an electricity storage device according to any one of items 1 to 3, wherein the sealant layer has a seal strength of 30 N / 15 mm or more at 80°C.

[0018] [5] The exterior packaging material for an electricity storage device according to any one of items 1 to 4, wherein the resin constituting the sealant layer is composed of at least one resin selected from the group consisting of polyvinylidene chloride resin, ethylene-vinyl alcohol copolymer, and high-density polyethylene resin.

[0019] [6] The packaging material for an electricity storage device according to any one of items 1 to 5, wherein the sealant layer is made of a resin that can be heat-sealed to the resin that constitutes the base material layer.

[0020] [7] An electricity storage device comprising: the packaging material for an electricity storage device according to any one of items 1 to 6; and an electricity storage device main body packaged with the packaging material for an electricity storage device.

[0021] According to the packaging material for an electricity storage device of invention [1], the sealant layer has gas barrier properties against water vapor and oxygen and also has heat-resistant sealing properties, so that defects due to the intrusion of water vapor and oxygen can be prevented and sufficient sealing strength can be ensured between the sealant layers. In particular, because the sealant layer is made of a heat-sealable resin film other than a polypropylene film, gas barrier properties against water vapor and oxygen that intrude along the fused portion from the outer peripheral end face of the fused sealant layer can be reliably obtained.

[0022] According to the packaging material for an electricity storage device of the invention [2], gas barrier properties against water vapor can be more reliably obtained.

[0023] According to the packaging material for an electricity storage device of the invention [3], gas barrier properties against oxygen can be more reliably obtained.

[0024] According to the packaging material for an electricity storage device of the invention [4], the sealing strength between the sealant layers can be more reliably ensured.

[0025] According to the packaging material for an electricity storage device of the invention [5], the above-mentioned effects can be obtained more reliably.

[0026] According to the exterior packaging material for an electricity storage device of the invention [6], it is possible to produce cases for electricity storage devices in various forms.

[0027] According to the electricity storage device of the invention [7], similarly to the above, not only is the gas barrier property excellent, but also sufficient sealing strength can be ensured.

[0028] Fig. 1 is a schematic cross-sectional view showing an all-solid-state battery packaging material as a packaging material for an electricity storage device according to an embodiment of the present invention. Fig. 2 is a schematic cross-sectional view showing an all-solid-state battery produced using the packaging material of the embodiment. Fig. 3 is a diagram showing a case for an all-solid-state battery produced using the packaging material of the embodiment, where Fig. 3(a) is a schematic cross-sectional view showing a first example case, Fig. 3(b) is a schematic cross-sectional view showing a second example case, and Fig. 3(c) is a schematic cross-sectional view showing a third example case. Fig. 4 is a diagram showing a fourth example case for an all-solid-state battery according to the embodiment, where Fig. 4(a) is a schematic perspective view, and Fig. 4(b) is a cross-sectional view taken along line A-A in Fig. 4(a).

[0029] Fig. 1 is a schematic cross-sectional view showing an all-solid-state battery packaging material 1 as a packaging material for an electricity storage device according to an embodiment of the present invention. As shown in the figure, the packaging material 1 of this embodiment is composed of a laminate (laminate material) and includes a base material layer 11 disposed on the outermost side, a metal foil layer 12 laminated and bonded to the inner side of the base material layer 11 via a first adhesive layer 21, and a sealant layer (thermally fused resin layer) 13 laminated and bonded to the inner side of the metal foil layer 12 via a second adhesive layer 22. In the present invention, when describing the positions of the layers constituting the packaging material 1 in terms of directions, the direction toward the base material layer 11 (upper side in Fig. 1 ) is referred to as the outside, and the direction toward the sealant layer 13 (lower side in Fig. 1 ) is referred to as the inside.

[0030] The substrate layer 11 has a thickness set to 3 μm to 50 μm, and is made of a heat-resistant resin coating or a heat-resistant resin film.

[0031] Suitable resins that can be used to form the base layer 11 include oriented polyamide, oriented polyester (PET, PBT, PEN, etc.), oriented polyolefin (PE, PP, etc.), polyvinylidene chloride (PVDC), ethylene-vinyl alcohol copolymer (EVOH), and high-density polyethylene (HDPE).

[0032] The metal foil layer 12 has a thickness set to 9 μm to 40 μm and has a function (barrier property) of blocking the penetration of oxygen and moisture from the surface (outer surface) side. The metal that constitutes this metal foil layer 12 can be suitably aluminum (Al), copper (Cu), iron (Fe), or an alloy thereof.

[0033] The sealant layer 13 is made of a resin film having a thickness set to 12 μm to 50 μm.

[0034] In this embodiment, the resin constituting the sealant layer 13 is one that has gas barrier properties against at least one of water vapor and oxygen, and preferably against both gases. In other words, the sealant layer 13 is made of a material that has excellent water vapor permeability and oxygen permeability. Specifically, the sealant layer 13 is made of a material that has a water vapor permeability of 5 g / m 2 It is preferable to use one with an oxygen permeability of 5 cm or less, and a permeability of 24 hr / 15 μm (40°C, 90% RH) or less. 3 / m 2 It is preferable to use a material with a resistance of 24 hr·atm / 15 μm (20° C., 90% RH) or less.

[0035] Furthermore, a material having heat-resistant sealing properties is used as the sealant layer 13. Specifically, it is preferable to use a sealant layer 13 having a seal strength of 40 N / 15 mm or more under normal conditions, and preferably a seal strength of 30 N / 15 mm or more at 80°C.

[0036] In this embodiment, the resin film constituting the sealant layer 13 is made of a heat-sealable resin film other than a polypropylene-based film.

[0037] Specifically, the resin film for the sealant layer 13 can be suitably made of a polyvinylidene chloride (PVDC) film, an ethylene-vinyl alcohol copolymer (EVOH) film, or an HDPE film.

[0038] As the PVDC film, a copolymer with vinyl chloride (PVC) or acrylonitrile, etc. can be suitably used. The melting point of this copolymer varies depending on the copolymerization ratio, but those with a melting point in the range of 140°C to 180°C can be suitably used.

[0039] The melting point of the EVOH film varies depending on the ethylene content (25 mol % to 50 mol %), but films with a melting point in the range of 155° C. to 190° C. can be suitably used.

[0040] The melting point of HDPE film varies depending on the density (0.94 to 0.965), but films with a melting point in the range of 120° C. to 140° C. can be suitably used.

[0041] In this embodiment, it is particularly preferable to use a PVDC film that exhibits gas barrier properties against both carbon dioxide and nitrogen gases.

[0042] In this embodiment, it is preferable to use a material having insulating properties as the sealant layer 13. Specifically, the volume resistivity is 1×10 14 It is preferable to use a resin film having a resistance of Ωcm or more.

[0043] Furthermore, in the present embodiment, the resin constituting the sealant layer 13 may be composed of a resin that is heat-sealable to the resin constituting the base material layer 11. For example, the resin for the sealant layer 13 and the resin for the base material layer 11 may be composed of the same type of resin or the same resin. In this case, as will be described later, it is possible to diversify the shapes of all-solid-state battery cases produced using the exterior material 1.

[0044] Two-component curing dry lamination adhesives such as polyurethane adhesives, acrylic adhesives, polyacrylate adhesives, modified polypropylene adhesives, polyester adhesives, polyamide adhesives, and epoxy adhesives can be suitably used for the first adhesive layer 21 that bonds between the base material layer 11 and the metal foil layer 12, and the second adhesive layer 21 that bonds between the metal foil layer 12 and the sealant layer 13. The thicknesses of the first and second adhesive layers 21, 22 are preferably set to 1 μm to 6 μm.

[0045] An all-solid-state battery (all-solid-state battery case) is produced using the all-solid-state battery exterior material 1 having the above-described configuration. For example, as shown in Fig. 2 , a pair (two sheets) of exterior materials 1 are arranged with their sealant layer 13 sides facing each other, and the all-solid-state battery body 3 is sandwiched between the pair of exterior materials 1 from above and below. The outer peripheral edges of the sealant layers 13 are heat-fused (thermally bonded) together to exterior and encapsulate the all-solid-state battery body 3 with the exterior material 1, thereby producing an all-solid-state battery. In the all-solid-state battery of Fig. 2 , the two heat-fused exterior materials 1 form an all-solid-state battery case 10.

[0046] In this embodiment, the exterior packaging material 1 may be subjected to molding or other forming processes to form a molded sheet, and the molded sheet may be used to manufacture the all-solid-state battery case 10.

[0047] In this embodiment, it is also possible to manufacture an all-solid-state battery case using a single exterior material 1. For example, as shown in Fig. 3(a) , a cylindrical all-solid-state battery case 10 may be manufactured by rolling the exterior material 1 into a cylindrical shape, folding opposing edges outward to make the sealant layers 13 face each other, and heat-sealing the opposing sealant layers 13 to each other.

[0048] Furthermore, as shown in FIG. 3( b), a cylindrical all-solid-state battery case 10 may be produced by rolling one sheet of exterior material 1 into a cylindrical shape, folding one edge outward, and overlapping the other edge with the folded portion of the one edge, so that the sealant layers 13 on the one edge and the other edge face each other, and then heat-sealing the opposing sealant layers 13 to each other.

[0049] Furthermore, in the present embodiment, when the resin for the sealant layer 13 and the resin for the base material layer 11 are configured to be heat-sealable as described above, a cylindrical all-solid-state battery case 10 may be produced by rolling one sheet of packaging material 1 into a cylindrical shape, superimposing the sealant layer 13 on one edge of the base material layer 11 on the other edge of the packaging material 1, and heat-sealing the base material layer 1 and the sealant layer 13 on the superimposed edges of the packaging material 1 to each other, as shown in FIG. 3( c).

[0050] 4( a) and 4(b) , it is also possible to produce an all-solid-state battery case 10 using a long tape-shaped (strip-shaped) exterior material 1. That is, the tape-shaped exterior material 1 may be spirally wound in one direction (upward), and for each turn, the sealant layer 13 at the lower edge of the upper exterior material 1 may be superimposed on the base material layer 11 at the upper edge of the lower exterior material 1 in adjacent exterior materials 1, and the base material layers 1 and sealant layers 13 at the superimposed edges may be heat-sealed to produce a rectangular cylindrical all-solid-state battery case 10. Note that openings at both ends in the cylindrical axis direction may be closed by heat-sealing other exterior materials 1 as necessary (the same applies to the all-solid-state battery case 10 in FIG. 3 ).

[0051] In the above example, the case where the all-solid-state battery case 10 is produced using one or two exterior materials 1 has been described as an example, but the present invention is not limited thereto, and the all-solid-state battery case may be produced using three or more exterior materials.

[0052] As described above, in the all-solid-state battery of this embodiment, the sealant layer 13 of the exterior packaging material 1 has gas barrier properties against water vapor and oxygen and heat-resistant sealing properties, so that the intrusion of water vapor and oxygen can be prevented and sufficient sealing strength can be ensured between the sealant layers 13. In particular, in this embodiment, the sealant layer 13 is made of a heat-sealable resin film other than a polypropylene-based film, so that gas barrier properties against water vapor and oxygen that intrude along the fused portion from the outer peripheral end surface of the fused sealant layer 13 can be reliably obtained. Since the intrusion of water vapor and oxygen can be prevented in this way, it is possible to prevent the generation of harmful hydrogen sulfide gas due to a reaction between moisture intruded from the outside and the all-solid-state battery body 3, such as a sulfide-based all-solid-state battery.

[0053]

[0054] Example 1 When producing an exterior material, a chemical conversion treatment solution containing polyacrylic acid, a trivalent chromium compound, water, and alcohol was applied to both sides of an aluminum foil made of A8021-O specified in JIS H4160 with a thickness of 35 μm as a metal foil layer, and the resulting coating was dried at 180° C. to a chromium deposition amount of 10 mg / m per side. 2 A metal foil layer member was prepared by subjecting it to chemical conversion treatment so as to have the following properties.

[0055] As shown in Table 1, a 12 μm-thick biaxially oriented PET film (substrate layer film) was bonded to one surface (outer surface) of the metal foil layer member via a two-component curing polyester-polyurethane adhesive applied to a thickness of 2 μm as an outer adhesive layer. A 15 μm-thick polyvinylidene chloride film (sealant layer film: melting point 180° C.) was bonded to the other surface (inner surface) of the metal foil layer with the substrate layer via a two-component curing polyester-polyurethane adhesive applied to a thickness of 2 μm as an inner adhesive layer to prepare a laminate for an exterior packaging material.

[0056] The laminate for the packaging material was subjected to heat aging treatment at 40° C. for 10 days to prepare a packaging material (laminate) of Example 1.

[0057] Example 2 An exterior packaging material of Example 2 was produced in the same manner as in Example 1 above, except that a vinylidene chloride film (melting point 180° C.) having a thickness of 25 μm was used as the sealant layer.

[0058] Example 3 An exterior packaging material of Example 3 was produced in the same manner as in Example 1 above, except that a 15 μm thick ethylene-vinyl alcohol copolymer film (melting point 161.5° C.) was used as the sealant layer.

[0059] Example 4 An exterior packaging material of Example 4 was produced in the same manner as in Example 1, except that a vinylidene chloride film (melting point 180° C.) having a thickness of 15 μm was used as the substrate layer.

[0060] Example 5 An exterior packaging material of Example 5 was produced in the same manner as in Example 1 above, except that a 30 μm thick ethylene-vinyl alcohol copolymer film (melting point 161.5° C.) was used as the sealant layer and a 15 μm thick ethylene-vinyl alcohol copolymer film (melting point 161.5° C.) was used as the base layer.

[0061] Example 6 An exterior packaging material of Example 6 was produced in the same manner as in Example 1 above, except that a 30 μm thick high-density polyethylene film (melting point 140° C.) was used as the sealant layer and a 20 μm thick high-density polyethylene film (melting point 140° C.) was used as the base layer.

[0062] Comparative Example 1 As a sealant layer, silica (silicon oxide: SiO ) was formed by electron beam heating silicon monoxide on one side (inner surface) of a 30 μm-thick unstretched polypropylene (CPP) film. 2 ) vapor-deposited film (thickness: 0.1 μm) was laminated on the gas barrier layer (vapor-deposited film), and a sealant layer (CPP / SiO 2 An exterior material of Comparative Example 1 was produced in the same manner as in Example 1, except that a non-oriented polypropylene film (barrier film) was prepared, and the other side (outer surface) of this non-oriented polypropylene film and the metal foil layer were bonded together using a two-component curing polyester-polyurethane adhesive.

[0063] Comparative Example 2 An exterior packaging material of Comparative Example 2 was produced in the same manner as in Example 1, except that a 30 μm thick unstretched polypropylene film was used as the sealant layer.

[0064] <Preparation of Packaging Material Samples> Using the packaging material of Example 1, a pair (two sheets) of packaging material samples (100 mm × 100 mm) were stacked together, and three of the four peripheral sides were sealed by heat sealing, leaving one side open, to prepare two three-sided bags.

[0065] Heat sealing was performed using a heat sealing device (TP-701-A) manufactured by Tester Sangyo Co., Ltd. and an aluminum seal bar with a seal width of 5 mm, by heating both sides under the conditions of a heat sealing temperature of 200°C, a sealing pressure of 0.2 MPa (gauge pressure), and a sealing time of 2 seconds, and three sides were heat sealed.

[0066] Next, in an environment inside a glove box purged with dry nitrogen, an oxygen detector was placed inside one of the two three-sided bags, and the open side (one opening) was sealed under reduced pressure using the same heat sealing conditions to prepare oxygen evaluation samples for Example 1.

[0067] The oxygen detector is a type that changes color predominantly to pink when the oxygen concentration is low and to blue when the oxygen concentration is high.

[0068] Cobalt chloride paper (moisture detecting agent) was placed in the other three-sided bag, and one opening was similarly sealed to prepare a sample for moisture evaluation in Example 1.

[0069] Cobalt chloride paper (moisture detector) changes color from blue to pink when it comes into contact with water or moisture.

[0070] In Examples 2 to 6 and Comparative Examples 1 and 2, samples for evaluating oxygen and samples for evaluating moisture were prepared in the same manner as above.

[0071] <Evaluation of moisture penetration>

[0072]

[0073] The moisture evaluation sample was left to stand for 60 days in an environment of 40°C and 90 RH (relative humidity). Thereafter, the discoloration of the moisture evaluation agent was visually observed to evaluate whether moisture (humidity) had penetrated into the sample. The results are shown in Table 2. In Table 2, when the color of the cobalt chloride paper (moisture detection agent) was blue, the gas barrier property against moisture (water vapor) was evaluated as "○ (pass)," and when it was pink, it was evaluated as "× (fail)."

[0074] <Evaluation of oxygen intrusion> The oxygen evaluation sample was left to stand at room temperature for 30 days. Thereafter, the oxygen detector was removed, and the degree of discoloration of the oxygen detector was visually observed to evaluate whether oxygen had intruded into the sample. The results are shown in Table 2. In Table 2, when the color of the oxygen detector was pink, the gas barrier property against oxygen was evaluated as "○ (pass)", and when it was blue, it was evaluated as "× (fail)".

[0075] <Evaluation of seal strength> A pair (two sheets) of packaging material samples measuring 15 mm wide x 150 mm long was cut out from the packaging material of Example 1, and this pair of packaging material samples was overlapped so that their inner surfaces (sealant layers) were in contact with each other. Using a heat sealing device (TP-701-A) manufactured by Tester Sangyo Co., Ltd., heat sealing was performed by heating on both sides under the following conditions: heat sealing temperature: 200°C, sealing pressure: 0.2 MPa (gauge display pressure), and sealing time: 2 seconds, to prepare a sample for measuring heat seal strength.

[0076] In Examples 2 to 6 and Comparative Examples 1 and 2, samples for measuring heat seal strength were prepared in the same manner as above.

[0077] Next, the heat seal strength measurement sample was measured in accordance with JIS Z0238-1998 using a Strograph (AGS-5kNX) manufactured by Shimadzu Access Co., Ltd., at the sealant layer portion, which is the seal portion of a pair of packaging material samples, when peeled at 180 degrees at a tensile strength of 100 mm / min, and this was taken as the seal strength (N / 15 mm width). The results are shown in Table 2.

[0078] In measuring the hot seal strength at 80°C, the sample for measuring the heat seal strength was set in a thermostatic chamber of the same Shimadzu Strograph, and then held in an 80°C environment for 1 minute, after which the peel strength was measured when the sample was allowed to naturally peel at a tensile strength of 100 mm / min. The results are shown in Table 2.

[0079] In Table 2, the evaluation criteria for room temperature seal strength are "◯ (pass)" for those of 40 N / 15 mm or more, and "× (fail)" for those of less than 40 N / 15 mm.

[0080] In the evaluation criteria for 80° C. seal strength, a value of 30 N / 15 mm or more is rated "◯ (pass)", and a value of less than 30 N / 15 mm is rated "× (fail)".

[0081] <Confirmation of heat-sealing properties: presence or absence of heat-sealing properties between base layer and sealant layer> The base layer film and sealant film used in Example 1 were each cut into a size of 15 mm wide x 150 mm long. The cut-out base layer film and sealant layer film were overlapped, and aluminum foils with a thickness of 80 μm were further overlapped on the top and bottom of the overlapped resin films to prepare a heat-sealing sample.

[0082] The above heat-sealable sample was heat-sealed by heating on both sides using a heat-sealing device (TP-701-A manufactured by Tester Sangyo Co., Ltd.) under the conditions of a heat-sealing temperature of 200°C, a sealing pressure of 0.2 MPa (gauge pressure), and a sealing time of 2 seconds, to obtain a sample for evaluating seal strength to confirm heat-bonding properties.

[0083] In Examples 2 to 6 and Comparative Examples 1 and 2, samples for evaluating the seal strength to check the heat-sealing properties were prepared in the same manner as above.

[0084] The seal strength evaluation sample was measured for its peel strength at 180° peeling at a tensile speed of 100 mm / min using a Strograph (AGS-5kNX) manufactured by Shimadzu Access Co., Ltd. in accordance with JIS Z0238-1998, and this was taken as the seal strength (N / 15 mm width). The evaluation criteria were as follows: "◯" in this evaluation criteria indicates a seal strength of 2 N / 15 mm or more, and "×" indicates a seal strength of less than 2 N / 15 mm.

[0085] As is clear from Table 2, all of the samples of the examples were highly rated in seal strength, and most were also highly rated in water vapor barrier property and oxygen barrier property. In contrast, the samples of the comparative examples were unable to receive high ratings in either seal strength or gas barrier property (water vapor barrier property, oxygen barrier property).

[0086] Regarding the thermal adhesiveness, the evaluations of the samples of the examples were mixed, but it was confirmed that the desired evaluation could be obtained by selecting the materials for the base layer and the sealant layer.

[0087] This application claims priority from Japanese Patent Application No. 2023-90217, filed on May 31, 2023, the disclosure of which is incorporated herein by reference in its entirety.

[0088] It should be understood that the terms and expressions used herein are used for the purpose of explanation and not for limiting interpretation, and do not exclude any equivalents of the features shown and described herein, but also allow various modifications within the claimed scope of the present invention.

[0089] The exterior packaging material for an electricity storage device of the present invention can be suitably used as a material for a battery case (casing) for accommodating an all-solid-state battery main body such as an all-solid-state battery.

[0090] 1: Exterior material 11: Base material layer 12: Metal foil layer 13: Sealant layer 3: All-solid-state battery body

Claims

1. An exterior material for an electricity storage device comprising: a resin base layer; a metal foil layer laminated on the inner surface side of the base layer; and a sealant layer laminated on the inner surface side of the metal foil layer via an adhesive layer, wherein the sealant layer has gas barrier properties against water vapor and / or oxygen, and has heat-resistant sealing properties, and is made of a heat-fusible resin film other than a polypropylene-based film.

2. The sealant layer has a water vapor permeability of 5 g / m at 40°C and 90% RH. 2 The exterior material for an electricity storage device according to claim 1, which has a hardness of 24 hr / 15 μm or less.

3. The sealant layer has an oxygen permeability of 5 cm at 20°C and 90% RH. 3 / m 2 The exterior material for an electricity storage device according to claim 1 or 2, which has a hardness of 24 hr·atm / 15 μm or less.

4. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the sealant layer has a seal strength of 30 N / 15 mm or more at 80°C.

5. The exterior packaging material for an electricity storage device according to any one of claims 1 to 4, wherein the resin constituting the sealant layer is composed of at least one resin selected from the group consisting of polyvinylidene chloride resin, ethylene-vinyl alcohol copolymer, and high-density polyethylene resin.

6. The packaging material for an electricity storage device according to any one of claims 1 to 5, wherein the sealant layer is made of a resin that can be thermally fused to the resin that constitutes the base layer.

7. An electricity storage device comprising: the exterior material for an electricity storage device according to any one of claims 1 to 6; and an electricity storage device main body that is exteriorly covered with the exterior material for an electricity storage device.

Citation Information

Patent Citations

  • Electrochemical device and method for manufacturing the same

    JP2005191288A

  • Laminated material for secondary battery container and secondary battery container

    JP2012084377A

  • Laminate film for battery outer packaging and method for producing the same

    JP2014026778A

  • Exterior material for lithium ion battery

    WO2012050182A1