Battery and battery manufacturing method
The battery design with a Li and O-containing interface compound addresses the low performance issues of all-solid-state lithium batteries by enhancing coulombic efficiency and cycle performance through improved lithium ion conductivity and safety.
Patent Information
- Application Number
- PCT/JP2024/019239
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-29
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
All-solid-state lithium batteries face challenges with low coulombic efficiency and cycle performance due to the limitations of existing solid electrolytes, particularly those based on sulfide materials which react with moisture and generate hydrogen sulfide gas, and oxide-based materials that have lower lithium ion conductivity.
A battery design incorporating a positive electrode, a negative electrode with a specific active material, and a solid electrolyte layer where an additional compound containing Li and O is present at the interface, enhancing coulombic efficiency and cycle performance by suppressing reductive decomposition and improving lithium ion conductivity.
The proposed battery configuration achieves high coulombic efficiency and cycle performance by generating an interfacial product that acts as a decomposition-inhibiting layer, ensuring stable charging and discharging while maintaining high lithium ion conductivity and safety.
Smart Images

Figure JP2024019239_05122024_PF_FP_ABST
Abstract
Description
Battery and method for manufacturing the battery
[0001] This application claims the benefit of priority from Japanese Patent Application No. JP2023-87889 filed on May 29, 2023, and Japanese Patent Application No. JP2023-138734 filed on August 29, 2023, the entire disclosures of which are incorporated herein by reference.
[0002] In recent years, with the development of portable devices such as personal computers and mobile phones, the demand for batteries as their power sources has expanded significantly. Batteries used for such applications have traditionally used organic electrolytes, in which electrolytes are dissolved in flammable organic solvents, as a medium for ion transfer. Batteries containing organic electrolytes may pose safety issues.
[0003] To solve these problems and ensure intrinsic safety, all-solid-state batteries that use solid electrolytes instead of organic electrolytes are being developed. In all-solid-state batteries, the electrolyte is a non-flammable material, making them intrinsically safe lithium (Li) ion batteries.
[0004] Furthermore, some solid electrolytes, such as sulfides, are widely known to react with water to generate hydrogen sulfide gas. On the other hand, oxide-based solid electrolytes, which do not generate gas like hydrogen sulfide, are also being developed widely, but the lithium ion conductivity of these materials is lower than that of sulfides, making it difficult to improve battery output (extract large current).
[0005] For example, in "Unlocking the Potential of Fluoride-Based Solid Electrolytes for Solid-State Lithium Batteries" by Max Feinauer and three others (ACS Appl. Energy Mater., 2019, Vol. 2, pp. 7196-7203) (Reference 1), β-Li is used as a solid electrolyte. 3 AlF 6 In FIG. 5(a), an all-solid-state lithium ion battery using Li as the anode and LiMn as the cathode is disclosed.2 O 4 The charge-discharge curve at 100°C when using a lithium-ion battery is shown. In this charge-discharge curve, the charge-discharge capacity from the second charge onwards is significantly smaller than the initial charge-discharge capacity, and cycle performance is poor. In addition, Japanese Patent Laid-Open Publication No. 2023-41247 (Document 2) discloses a coated negative electrode active material having a Si-based active material and a coating layer containing lithium oxide that coats at least a portion of the surface of the Si-based active material. In addition, International Publication No. 2022 / 210482 (Document 3) discloses Li a+d M b X c A e O f (wherein M is an element that becomes trivalent as a cation, X is a halogen element, and A is sulfur or phosphorus element.) Figure 2 in "Interface Stability in Solid-State Batteries" by William D. Richards and four others (ACS Chem. Mater., 2016, Vol. 28, pp. 266-273) (Reference 4) shows the electrochemical stability ranges of various solid electrolyte materials.
[0006] As mentioned above, the battery of Reference 1 has poor cycle performance. Even when the inventors of the present application performed experiments by changing the electrodes of the battery to an NCM positive electrode and a graphite negative electrode, the cycle performance was poor. Furthermore, the coulombic efficiency (the ratio of charge and discharge capacities) during the initial charge and discharge was low, and the discharge capacity was also small. Therefore, a battery with high coulombic efficiency and high cycle performance is desired.
[0007] An object of the present invention is to provide a battery having high coulombic efficiency and high cycle performance.
[0008] A first aspect of the invention is a battery comprising: a positive electrode; a negative electrode including a negative electrode active material and a solid electrolyte; and a solid electrolyte layer provided between the positive electrode and the negative electrode; wherein in the negative electrode, another compound is present at the interface between the negative electrode active material and the solid electrolyte, and the other compound includes Li and O.
[0009] According to the present invention, a battery having high coulombic efficiency and high cycle performance can be provided.
[0010] A second aspect of the invention is the battery of the first aspect, wherein the negative electrode active material is 2.0 V (vs. Li / Li + ) is an active material that operates at a potential below
[0011] A third aspect of the invention is the battery of the first or second aspect, wherein the negative electrode active material is 1.0 V (vs. Li / Li + ) is an active material that operates at a potential below
[0012] A fourth aspect of the invention is the battery according to any one of the first to third aspects, wherein the other compound is present in the form of a layer at the interface, and the thickness of the other compound is 1 to 1000 nm.
[0013] A fifth aspect of the invention is the battery according to any one of the first to fourth aspects, wherein the solid electrolyte contains Li and O.
[0014] A sixth aspect of the invention is the battery of the fifth aspect, wherein the solid electrolyte further contains X which is a halogen element.
[0015] A seventh aspect of the present invention is the battery of the fifth or sixth aspect, wherein the solid electrolyte further contains S.
[0016] An eighth aspect of the invention is the battery of any one of the fifth to seventh aspects, wherein the solid electrolyte further contains Al.
[0017] A ninth aspect of the invention is the battery according to any one of the fifth to eighth aspects, wherein the solid electrolyte has a composition formula of Li a+d M b X c S e O f (wherein M is an element that becomes trivalent as a cation, and X is a halogen element), and 0.8c≦(a+3b)≦1.2c and 1.6f≦(d+n×e)≦2.4f (wherein n is 4 or 6) are satisfied.
[0018] A tenth aspect of the present invention is the battery according to any one of the first to ninth aspects, wherein the other compounds do not contain Ti.
[0019] An eleventh aspect of the invention is the battery according to any one of the first to tenth aspects, wherein the solid electrolyte contains S and the other compound does not contain S.
[0020] A twelfth aspect of the invention is the battery of any one of the first to eleventh aspects, wherein the negative electrode active material is carbon.
[0021] The present invention is also directed to a method for manufacturing a battery.
[0022] A thirteenth aspect of the invention is a method for manufacturing the battery of any one of the first to twelfth aspects, comprising: a) preparing a battery by stacking a positive electrode, a solid electrolyte layer, and a negative electrode containing a negative electrode active material and a solid electrolyte; and b) charging the battery, wherein the solid electrolyte of the negative electrode contains Li and O.
[0023] A fourteenth aspect of the invention is a method for manufacturing the battery of any one of the first to twelfth aspects, comprising: a) a step of preparing a battery by stacking a positive electrode, a solid electrolyte layer, and a negative electrode containing a negative electrode active material and a solid electrolyte; and b) a step of charging the battery, wherein the a) step is performed in an oxygen-containing atmosphere, and in the b) step, Li ions migrate from the positive electrode to the negative electrode.
[0024] The above and other objects, features, aspects and advantages will become more apparent from the following detailed description of the invention which proceeds with reference to the accompanying drawings.
[0025] FIG. 1 is a longitudinal sectional view showing an all-solid-state battery. FIG. 2 is a diagram schematically showing a cross section of a negative electrode layer. FIG. 3 is a diagram showing a flow of manufacturing an all-solid-state battery. FIG. 4 is a diagram showing the results of a charge-discharge test for an all-solid-state battery of Experimental Example 1. FIG. 5 is a diagram showing the results of a charge-discharge test for an all-solid-state battery of Experimental Example 2. FIG. 6 is a diagram showing the results of an analysis of a cross section of the negative electrode by FE-SEM / EDX for an all-solid-state battery of Experimental Example 2 after charge-discharge. FIG. 7 is a diagram showing the results of an analysis of a cross section of the negative electrode by FE-SEM / EDX for an all-solid-state battery of Experimental Example 2 before charge-discharge. FIG. 8 is a diagram showing the results of an analysis of a cross section of the negative electrode by AES for an all-solid-state battery of Experimental Example 2 after charge-discharge.
[0026] FIG. 1 is a longitudinal cross-sectional view showing an all-solid-state battery 1. The all-solid-state battery 1 in this embodiment is an all-solid-state lithium-ion battery, and is a chargeable and dischargeable secondary battery. The all-solid-state battery 1 has, from the top of FIG. 1 , a positive electrode 11, a solid electrolyte layer 13, and a negative electrode 12. The solid electrolyte layer 13 is provided between the positive electrode 11 and the negative electrode 12. The solid electrolyte layer 13 also serves as a separator layer. The solid electrolyte layer 13 is made of or includes a solid electrolyte 22 described below.
[0027] The positive electrode 11 includes a current collector 111 and a positive electrode layer 112. The positive electrode layer 112 is in contact with the solid electrolyte layer 13 and includes a positive electrode active material. The positive electrode active material of the positive electrode layer 112 preferably includes a lithium composite oxide. A preferred positive electrode active material is a lithium composite oxide having a layered rock salt structure, such as NCM (Li(Ni, Co, Mn)O 2 The positive electrode active material may be other lithium composite oxides, for example, NCA (Li(Ni, Co, Al)O) having a layered rock salt structure. 2 ), LCO (LiCoO 2 ), LNMO (Li(Ni,Mn)O) with a spinel structure 4 ), LFP (LiFePO) having an olivine structure 4 ) or the like. The positive electrode layer 112 includes a solid electrolyte 22 described below in addition to the positive electrode active material. The positive electrode layer 112 may further include an electron conduction assistant (carbon black, etc.). An example of the positive electrode layer 112 is one in which these materials are integrated by applying pressure or heat.
[0028] The current collector 111 is disposed on the opposite side of the positive electrode layer 112 from the solid electrolyte layer 13, and is in contact with the positive electrode layer 112. The current collector 111 is formed of, for example, copper, stainless steel, nickel, aluminum, silver, gold, chromium, iron, tin, lead, tungsten, molybdenum, titanium, zinc, or an alloy containing any of these. The same applies to the current collector 121 of the negative electrode 12, which will be described later.
[0029] The anode 12 includes a current collector 121 and an anode layer 122. The anode layer 122 is in contact with the solid electrolyte layer 13 and includes an anode active material 21 and a solid electrolyte 22, which will be described later. The anode layer 122 may further include an electron conduction additive (carbon black, etc.). An example of the anode layer 122 is formed by integrating these materials by applying pressure or heat. The current collector 121 is disposed on the opposite side of the anode layer 122 from the solid electrolyte layer 13, and is in contact with the anode layer 122.
[0030] FIG. 2 is a diagram schematically illustrating a cross section of the negative electrode layer 122, showing the interface between the negative electrode active material 21 and the solid electrolyte 22 and the vicinity thereof. The negative electrode active material 21 is, for example, carbon (C), and preferably graphite. The negative electrode active material 21 has a potential of 2.0 V (vs. Li / Li + The potential at which the negative electrode active material 21 operates is preferably 1.5 V (vs. Li / Li + ) or less, and more preferably 1.0 V (vs. Li / Li + ) or less. The negative electrode active material 21 may be, in addition to graphite, hard carbon, SiO (silicon monoxide), Si (silicon) metal, an alloy containing Si, Sn (tin) metal, an alloy containing Sn, Li metal, an alloy containing Li, or the like.
[0031] The particle size of the negative electrode active material 21 is, for example, 5 to 20 μm. For example, the particle size of the negative electrode active material 21 can be measured by observing the cross section of a mirror-polished negative electrode with a scanning electron microscope (SEM) and calculating the average of the major axes of the particles of the negative electrode active material 21.
[0032] The solid electrolyte 22 is a lithium ion conductive material. The solid electrolyte 22 contains, for example, Li and O (oxygen). The solid electrolyte 22 may further contain at least one element selected from the group consisting of halogen elements X, S (sulfur), and Al (aluminum). The solid electrolyte 22 may also contain all of X, S, and Al.
[0033] A preferred example of the solid electrolyte 22 is a solid electrolyte having a composition formula of Li a+d M b X c Se O f (wherein M is an element that is trivalent as a cation, and X is a halogen element) In this composition formula, 0.8c≦(a+3b)≦1.2c and 1.6f≦(d+n×e)≦2.4f (wherein n is 4 or 6) are satisfied. Such a solid electrolyte 22 has high lithium ion conductivity and high-temperature stability. It also does not generate hydrogen sulfide gas, thereby increasing safety. The main component is the component with the largest mass ratio among the components contained in the solid electrolyte 22. The mass ratio of the main component in the solid electrolyte 22 is preferably 80 mass% or more, and more preferably 90 mass% or more.
[0034] An example of the solid electrolyte 22 in this embodiment is a Li-based solid electrolyte containing Li, Al, and F (fluorine). 3 AlF 6 and Li containing Li, S, and O 2 SO 4 (lithium sulfate). 3 AlF 6 and Li 2 SO 4 In the solid electrolyte 22 containing 3 AlF 6 The reason for this is not clear, but one possible reason is that the solid electrolyte 22 is produced by a mechanical milling process, which will be described later, and Li 3 AlF 6 And Li 2 SO 4 It is considered that an interface layer with high lithium ion conductivity is formed at the particle interface between the solid electrolyte 22 and Li. 3 AlF 6 and LiPO 3 The same applies to mixtures of the above.
[0035] The particle size of the solid electrolyte 22 is, for example, smaller than the particle size of the negative electrode active material 21. The particle size of the solid electrolyte 22 is, for example, 5 μm or less, preferably 4.5 μm or less, and more preferably 4 μm or less. When the particle size of the solid electrolyte 22 is sufficiently small, the gap at the interface between the negative electrode active material 21 and the solid electrolyte 22 is reduced, facilitating adhesion between the two. As a result, the discharge capacity of the all-solid-state battery 1 is increased and the interfacial product 23 described below can be appropriately generated. The lower limit of the particle size of the solid electrolyte 22 is not particularly limited, but is, for example, 0.3 μm, preferably 0.5 μm, and more preferably 1 μm. For example, the particle size of the solid electrolyte 22 can be measured by observing a mirror-polished cross section of the negative electrode with a scanning electron microscope (SEM) and calculating the average major axis of each particle of the solid electrolyte 22.
[0036] 2 , in the anode layer 122, another compound 23 is present at the interface between the anode active material 21 and the solid electrolyte 22. The compound 23 is a compound not contained in the anode active material 21 or the solid electrolyte 22, and contains Li and O. As will be described later, the other compound 23 is produced by performing a charging operation on the all-solid-state battery 1, and therefore will be referred to as an "interface product 23" in the following description.
[0037] The interface product 23 is typically an oxide containing Li (Li oxide), and preferably Li 2 The interface product 23 may contain other elements in addition to Li and O, such as Li, 2The interface product 23 is not limited to O. When the solid electrolyte 22 contains at least one element of X (a halogen element), S, and Al, the interface product 23 may or may not contain any of the at least one element. In other words, when the solid electrolyte 22 contains X, the interface product 23 may or may not contain X. When the solid electrolyte 22 contains S, the interface product 23 may or may not contain S. When the solid electrolyte 22 contains Al, the interface product 23 may or may not contain Al. Furthermore, when the negative electrode active material 21 is carbon, it is preferable that the interface product 23 does not contain C. The interface product 23 also does not contain Ti (titanium), which is often used as a constituent element of negative electrode active materials.
[0038] Typically, the interface product 23 exists in the form of a layer at the interface between the negative electrode active material 21 and the solid electrolyte 22. The interface product 23 may also exist at a position slightly separated from the interface. In this specification, the expression "the interface product 23 exists at the interface between the negative electrode active material 21 and the solid electrolyte 22" includes not only the case where the interface product 23 is strictly present at the interface, but also the case where the interface product 23 is present near the interface. For example, if the shortest distance between the interface product 23 and the interface is 1 μm or less, it can be said that the interface product 23 is present near the interface. In an all-solid-state battery 1 in which the interface product 23 exists at the interface between the negative electrode active material 21 and the solid electrolyte 22, it is believed that the interface product 23 functions as a decomposition-suppressing layer that suppresses reductive decomposition of the solid electrolyte 22 during charging. As a result, high coulombic efficiency and high cycle performance are achieved.
[0039] The thickness of the layered interface product 23 is, for example, 1 nm or more, preferably 10 nm or more, and more preferably 30 nm or more. This more reliably suppresses reductive decomposition of the solid electrolyte 22. The thickness of the interface product 23 is, for example, 1000 nm or less, preferably 750 nm or less, and more preferably 500 nm or less. This prevents a decrease in conductivity in the negative electrode 12. As described below, the thickness of the interface product 23 can be measured by calculating the average maximum thickness of each layer having a higher O concentration than the solid electrolyte 22 in an O (oxygen) element mapping image (see the lower part of Figure 6 described below) obtained using an EDX (energy dispersive X-ray analyzer) on a mirror-polished cross section of the negative electrode. Depending on the design of the all-solid-state battery 1, the thickness of the interface product 23 may be less than 1 nm or greater than 1000 nm.
[0040] 3 is a diagram showing the flow of manufacturing the all-solid-state battery 1. The all-solid-state battery 1 is manufactured in an oxygen-containing atmosphere, such as a dry room with a dew point of −40° C. or less. In the manufacturing of the all-solid-state battery 1, first, a solid electrolyte 22 to be used in the positive electrode 11, the solid electrolyte layer 13, and the negative electrode 12 is prepared (step S11). The solid electrolyte 22 contains, for example, Li and O. In this processing example, Li 3 AlF 6 and Li 2 SO 4 The solid electrolyte 22 is prepared by mixing the above. 3 AlF 6 and Li 2 SO 4 The solid electrolyte 22 is not limited to a mixture of the above. In addition, the solid electrolyte 22 does not have to contain O.
[0041] In the preparation of the solid electrolyte 22, Li 3 AlF 6 powder and Li 2 SO 4 Powders of Li are prepared. 3 AlF 6 In preparing the powder, for example, commercially available LiF (lithium fluoride) powder and commercially available AlF 3(aluminum fluoride) powder is weighed and mixed. The resulting mixture is then heat-treated (e.g., at 900°C) and then pulverized to obtain Li 3 AlF 6 A powder of Li is obtained. 3 AlF 6 Powders of Li may be produced by other methods. 2 SO 4 The powder is commercially available. 2 SO 4 The powder may be produced by known techniques.
[0042] Next, Li 3 AlF 6 powder and Li 2 SO 4 The powder is mixed with Li 3 AlF 6 Amount of substance and Li 2 SO 4 The amount of Li in the total amount of 2 SO 4 The ratio of the amount of the substances is, for example, 5 to 85%. The mixture is then subjected to mechanical milling (mechanochemical milling). Here, as an example of mechanical milling, a planetary ball mill is used. In a planetary ball mill, the pot rotates on its axis while the stage on which the pot is placed revolves, making it possible to generate very high impact energy. The mechanical milling may also be performed using other types of grinders. By the mechanical milling, Li 3 AlF 6 -Li 2 SO 4 A powder is obtained as the solid electrolyte 22. In this example, the mechanical milling process is carried out at room temperature, but the conditions such as temperature may be changed as appropriate.
[0043] Once the powder of the solid electrolyte 22 is produced, a laminate of the positive electrode layer 112, the solid electrolyte layer 13, and the negative electrode layer 122 is produced. The positive electrode layer 112 is produced by mixing a powder of the positive electrode active material and a powder of the solid electrolyte 22 and then pressure-molding the mixture. An electronic conduction aid may be further mixed into the positive electrode layer 112. Typically, the particle size of the electronic conduction aid is sufficiently smaller than that of the powder of the positive electrode active material and the powder of the solid electrolyte 22 (the same applies to the production of the negative electrode layer 122). The negative electrode layer 122 is produced by mixing a powder of the negative electrode active material 21 and a powder of the solid electrolyte 22 and then pressure-molding the mixture. The particle size of the negative electrode active material 21 is, for example, 5 to 20 μm, and the particle size of the solid electrolyte 22 is, for example, 0.3 to 5 μm. The electronic conduction aid may be further mixed into the negative electrode layer 122. The solid electrolyte layer 13 is produced by pressure-molding the powder of the solid electrolyte 22. The positive electrode layer 112, the solid electrolyte layer 13, and the negative electrode layer 122 may be integrally pressure-molded. Then, the current collector 111 is attached to the positive electrode layer 112, and the current collector 121 is attached to the negative electrode layer 122. In this way, the all-solid-state battery 1 including the positive electrode 11, the solid electrolyte layer 13, and the negative electrode 12 is fabricated and prepared (step S12). The positive electrode layer 112, the solid electrolyte layer 13, and the negative electrode layer 122 may be housed in a sealed case.
[0044] When the all-solid-state battery 1 is prepared, the current collectors 111 and 121 are connected to a power source, and a charging operation is performed on the all-solid-state battery 1. As a result, in the anode 12, another compound containing Li and O, i.e., an interface product 23, is generated at the interface between the anode active material 21 and the solid electrolyte 22 (step S13). The reason why the interface product 23 is generated is not clear, but it is thought that, for example, the solid electrolyte 22 contains Li. 3 AlF 6 -Li 2 SO 4 In the case of powder, Li is reacted with Li by the reaction of formula (1) described below. 2 It is believed that O is generated. In addition, O mixed into the negative electrode 12 during the production of the all-solid-state battery 1 2There is a possibility that the gas has reacted with Li ions. The above processes complete the production of the all-solid-state battery 1. Note that, when the positive electrode layer 112, the solid electrolyte layer 13, and the negative electrode layer 122 are housed in a case, step S13 may be performed in the atmosphere.
[0045] Next, experimental examples of the all-solid-state battery 1 will be described. Table 1 shows the configurations of the all-solid-state batteries of Experimental Examples 1 to 4 and the results of charge / discharge tests. Experimental Example 1 is a comparative example, and Experimental Examples 2 to 4 are examples of the present invention. The following experiments were carried out in a glove box or a dry room with a dew point of -40°C or below.
[0046]
[0047] (Experimental Example 1) Commercially available LiF powder and commercially available AlF were used as raw materials. 3 The raw materials were prepared as LiF:AlF powders. 3 The resulting mixture was heated at 900°C and then pulverized in a mortar to obtain the solid electrolyte powder of Experimental Example 1, Li 3 AlF 6 A powder was obtained.
[0048] NCM: Li(Ni,Co,Mn)O 2 and a solid electrolyte powder (Li 3 AlF 6 A positive electrode powder was obtained by weighing and mixing a graphite active material powder, a solid electrolyte powder, and an electron conduction aid powder. A negative electrode powder was obtained by weighing and mixing a graphite active material powder, a solid electrolyte powder, and an electron conduction aid powder. The solid electrolyte powder was placed in a mold consisting of a PEEK resin sleeve and SUS upper and lower punches, and uniaxial press molding was performed under a pressure of 150 MPa. The positive electrode powder was placed on top of the pressed solid electrolyte powder and integrated under a pressure of 150 MPa. The negative electrode powder was placed on the pressed solid electrolyte powder opposite the positive electrode and integrated under a pressure of 150 MPa. This produced an all-solid-state battery consisting of a positive electrode layer, a solid electrolyte layer, and a negative electrode layer.
[0049] (Experimental Example 2) The above Li 3 AlF 6 In addition to powder, commercially available Li2 SO 4 The two were weighed to have a molar ratio of 1:1, and mechanically milled using a planetary ball mill to obtain Li powder. 3 AlF 6 -Li 2 SO 4 Then, Li was used as a solid electrolyte powder. 3 AlF 6 -Li 2 SO 4 An all-solid-state battery was fabricated in the same manner as in Experimental Example 1, except that powder was used.
[0050] (Experimental Example 3) The above Li 3 AlF 6 powder and Li 2 SO 4 In addition to powder, commercially available Li 2 SiF 6 Powder was prepared. 3 AlF 6 Powder, Li 2 SO 4 powder and Li 2 SiF 6 The powders were weighed to have a molar ratio of 8:2:1 and mechanically milled using a planetary ball mill to obtain Li 3 AlF 6 -Li 2 SO 4 -Li 2 SiF 6 Then, Li was used as a solid electrolyte powder. 3 AlF 6 -Li 2 SO 4 -Li 2 SiF 6 An all-solid-state battery was fabricated in the same manner as in Experimental Example 1, except that powder was used.
[0051] (Experimental Example 4) The above Li 3 AlF 6 In addition to powder, commercially available LiPO 3 Powder was prepared. 3 AlF 6 Powder and LiPO 3The powders were weighed to have a molar ratio of 9:1 and subjected to mechanical milling using a planetary ball mill to obtain Li 3 AlF 6 -LiPO 3 Then, Li was used as a solid electrolyte powder. 3 AlF 6 -LiPO 3 An all-solid-state battery was fabricated in the same manner as in Experimental Example 1, except that powder was used.
[0052] <Charge-Discharge Test> Conductive wires were connected to the upper and lower punches, and the above-described all-solid-state battery was placed in a thermostatic chamber at 100°C to perform a cc-cv (constant current-constant voltage) charge-discharge test. In the charge-discharge test, a cc current density of 300 μA / cm was used. 2 , cv current density 30μA / cm 2 The cutoff voltage was set to 4.15-2.00V.
[0053] Fig. 4 shows the results of a charge / discharge test for the all-solid-state battery of Experimental Example 1, and Fig. 5 shows the results of a charge / discharge test for the all-solid-state battery of Experimental Example 2. In Fig. 4 and Fig. 5, the initial charge curves are labeled L11 and L21, the initial discharge curves are labeled L12 and L22, the fourth charge curves are labeled L13 and L23, and the fourth discharge curves are labeled L14 and L24. In Table 1, the "Initial Discharge Amount" column shows the discharge capacity in the initial discharge, the "Initial Coulombic Efficiency" column shows the Coulombic efficiency (discharge capacity / charge capacity) in the initial charge / discharge, and the "3-cycle Capacity Retention Rate" column shows the ratio of the fourth discharge capacity to the initial discharge capacity.
[0054] As is clear from Fig. 4, Fig. 5 and Table 1, the all-solid-state batteries of Experimental Examples 2 to 4 had higher initial discharge amounts and coulombic efficiencies than the all-solid-state battery of Experimental Example 1. In addition, the 3-cycle capacity retention rate was also higher, and it was confirmed that the all-solid-state batteries of Experimental Examples 2 to 4 had higher cycle performance than the all-solid-state battery of Experimental Example 1.
[0055] <Analysis of Negative Electrode Interface of All-Solid-State Battery> The all-solid-state battery of Experimental Example 2 that was not charged and discharged was used as the all-solid-state battery before charge and discharge, and the all-solid-state battery of Experimental Example 2 that was charged and discharged was used as the all-solid-state battery after charge and discharge. The cross section of the mirror-polished negative electrode of each of the all-solid-state batteries before and after charge and discharge was observed using a field emission scanning electron microscope (FE-SEM). Element mapping of the cross section was also performed using an energy dispersive X-ray analyzer (EDX).
[0056] 6 and 7 are diagrams showing the results of analysis of a cross section of a negative electrode by FE-SEM / EDX. FIG. 6 shows the analysis results for the all-solid-state battery of Experimental Example 2 after charge and discharge, and FIG. 7 shows the analysis results for the all-solid-state battery of Experimental Example 2 before charge and discharge. The upper rows of FIGS. 6 and 7 show images observed by FE-SEM. The lower rows of FIGS. 6 and 7 show the results of element mapping of C, O, S, F, and Al, with the higher the density of white, the higher the concentration of each element.
[0057] In the all-solid-state battery after charge and discharge shown in FIG. 6, the presence of an oxide layer containing O and not containing C, S, F, or Al was confirmed at the interface between the negative electrode active material containing C and the solid electrolyte containing O, S, F, and Al. In FIG. 6, the position of the oxide layer (product) is indicated by a white arrow. The thickness of the oxide layer was in the range of 1 to 1000 nm. On the other hand, in the all-solid-state battery before charge and discharge shown in FIG. 7, the presence of the oxide layer (i.e., an oxide layer containing O and not containing C, S, F, or Al) could not be confirmed. In FIG. 7, the Al used in producing the solid electrolyte powder was 2 O 3 Fragments of boulders were found to be mixed in, and the location of the fragments was marked as "Al 2 O 3 It states, "Contamination of boulders and stones."
[0058] Next, in the all-solid-state battery after charge / discharge, the mirror-polished cross section of the negative electrode was analyzed by AES (Auger electron spectroscopy). FIG. 8 shows the results of the AES analysis of the cross section of the negative electrode. The upper part of FIG. 8 is an image showing the cross section of the negative electrode, and the lower part is a diagram showing the Auger electron spectrum at the position marked with the symbol P3 in the upper image. Position P3 corresponds to the oxide layer, and the presence of Li was confirmed at position P3. Therefore, the oxide layer contains Li, and it can be said that the oxide layer is a compound (interface product) containing Li and O. It should be noted that in the all-solid-state batteries of Experimental Examples 3 and 4, it was confirmed that a compound (interface product) containing Li and O was present at the interface between the negative electrode active material and the solid electrolyte after charge / discharge.
[0059] <Consideration 1 on Interface Products> The above-mentioned compounds containing Li and O (interface products) are formed by reacting with some of the components contained in the solid electrolyte (for example, Li 2 SO 4 ) is reductively decomposed and is generated as a reduction product at the interface between the negative electrode active material and the solid electrolyte. 2 SO 4 When the lithium ion battery contains lithium, the reduction reaction that can be considered at the negative electrode during charging when lithium and electrons are supplied from the positive electrode is as shown in the following formula (1): 2 SO 4 +8Li + +8e - →4Li 2 O + Li 2 S... (1)
[0060] The compounds containing Li and O in the above examples (Li 2 O), low operating potentials (e.g., 2.0 V (vs. Li / Li + ) or less, and preferably 1.0 V (vs. Li / Li +Even when a negative electrode active material having the following structure is used, reductive decomposition does not occur (see Figure 2 in "Interface Stability in Solid-State Batteries" by William D. Richards and four others, ACS Chem. Mater., 2016, Vol. 28, pp. 266-273 (reference 4)). Furthermore, the compound is in a passive state with no electrical conductivity. Therefore, it is believed that the presence of the compound at the interface between the negative electrode active material and the solid electrolyte functions as a decomposition suppressing layer that suppresses the reductive decomposition of the solid electrolyte. As a result, in an all-solid-state battery, stable charge and discharge can be performed using a negative electrode active material with a low operating potential, achieving high coulombic efficiency and high cycle performance. The solid electrolyte does not necessarily contain Li. 2 SO 4 It is not necessary for the solid electrolyte to contain Li and O, and any solid electrolyte that generates other compounds containing Li and O at the interface with the negative electrode active material during charging may be used. Typically, the solid electrolyte contains Li and O, and the operating potential is 2.0 V (vs. Li / Li + ) or less (preferably, 1.0 V (vs Li / Li + ) below), it is believed that the above-mentioned compounds containing Li and O (interface products) are produced.
[0061] <Consideration 2 on interface products> Depending on various conditions, Li that has migrated from the positive electrode to the negative electrode during charging of the all-solid-state battery may be present as shown in the following formula (2). + Ions and electrons e - and O contained in the negative electrode 2 Gas (O mixed into the negative electrode during the production of the all-solid-state battery) 2 gas) to form a compound containing Li and O (Li 2 O) is also considered to be generated. This can occur when the fabrication (and charge / discharge) of an all-solid-state battery is carried out, for example, in a dry room with a dew point of −40° C. or less. 2 SO 4 Even when the mixture does not contain other compounds containing Li or O, that is, does not contain O element, it is believed that the compound containing Li and O (interface product) is generated. 2+4Li + +4e - →2Li 2 O...(2)
[0062] As described above, the all-solid-state battery 1 includes the positive electrode 11, the negative electrode 12 including the negative electrode active material 21 and the solid electrolyte 22, and the solid electrolyte layer 13 provided between the positive electrode 11 and the negative electrode 12. In the negative electrode 12, another compound is present at the interface between the negative electrode active material 21 and the solid electrolyte 22, and this other compound includes Li and O. In such an all-solid-state battery 1, the other compound can suppress continuous reductive decomposition of the solid electrolyte 22, thereby achieving high coulombic efficiency and high cycle performance.
[0063] Preferably, the other compound is present in the form of a layer at the interface, and the thickness of the other compound is 1 to 1,000 nm. When the thickness of the other compound is 1 nm or more, reductive decomposition of the solid electrolyte 22 can be more reliably suppressed. Furthermore, when the thickness is 1,000 nm or less, a decrease in the conductivity of the negative electrode 12 can be prevented.
[0064] Preferably, the negative electrode active material 21 is 2.0 V (vs. Li / Li + ) or less, and more preferably, the negative electrode active material 21 is an active material that operates at a potential of 1.0 V (vs. Li / Li + ) or less. This allows the other compounds to be produced more reliably by charging the all-solid-state battery 1. Furthermore, since the solid electrolyte 22 contains Li and O, the other compounds can be produced by temporary reductive decomposition of the solid electrolyte 22.
[0065] A preferred method for manufacturing the all-solid-state battery 1 includes the steps of: preparing a battery by stacking a positive electrode 11, a solid electrolyte layer 13, and a negative electrode 12 including a negative electrode active material 21 and a solid electrolyte 22 (step S12); and charging the battery (step S13). The solid electrolyte 22 of the negative electrode 12 contains Li and O. Alternatively, step S12 is performed in an oxygen-containing atmosphere, and Li ions migrate from the positive electrode 11 to the negative electrode 12 in step S13. This allows other compounds containing Li and O to be easily generated at the interface between the negative electrode active material 21 and the solid electrolyte 22 in the negative electrode 12.
[0066] In the above embodiment, Li 3 AlF 6 And Li 2 SO 4 The solid electrolyte 22 is obtained by mechanical milling the above. The solid electrolyte 22 is a compound Li containing Li, a metal element M which becomes trivalent as a cation, and a halogen element X. a M b X c and a compound containing Li, S, and O, Li d S e O f (where a to f are all greater than 0). In this case, Li, M, and X are monovalent cations, trivalent cations, and monovalent anions, respectively, so that a + 3b = c is satisfied. a M b X c Li 3 AlF 6 In addition, for example, Li 3 YF 6 , Li 3 LaF 6 , Li 3 GaF 6 , Li 3 YCl 6 , Li 3 YBr 6 , Li 3 InCl 6 , Li 3 LaI 6 , LiYF 4, LiYbF 4 , LiLaF 4 , LiBiF 4 , LiAlCl 4 , LiGaCl 4 etc. Also, since Li, S, and O are monovalent cations, tetravalent or hexavalent cations, and divalent anions, respectively, d + 4e = 2f or d + 6e = 2f is satisfied. In other words, d + n × e = 2f (where n is 4 or 6) is satisfied. Li 2 SO 4 The above compounds other than Li d S e O f For example, Li 2 SO 3 (lithium sulfite), etc.
[0067] Compound Li a M b X c and the compound Li d S e O f The composition formula of the solid electrolyte 22 is a+d M b X c S e O f The solid electrolyte 22 satisfies the above-mentioned conditions of a + 3b = c and d + n × e = 2f (where n is 4 or 6). Taking into account measurement errors and the like, it is sufficient that 0.8c ≦ (a + 3b) ≦ 1.2c and 1.6f ≦ (d + n × e) ≦ 2.4f are satisfied. Preferably, 0.9c ≦ (a + 3b) ≦ 1.1c and 1.8f ≦ (d + n × e) ≦ 2.2f are satisfied. The solid electrolyte 22 has a composition formula of Li a+d M b X c S e O f The solid electrolyte 22 represented by the formula (I) has high lithium ion conductivity and high temperature stability. 3 AlF 6 -Li 2 SO 4 In the preparation of 3 AlF 6 Without generating LiF, AlF 3 and Li2 SO 4 It is also possible to mix these materials and subject them to mechanical milling.
[0068] The unknown solid electrolyte is Li a+d M b X c S e O f When confirming whether the unknown solid electrolyte is a solid electrolyte 22 expressed by the formula (I), chemical analysis is performed on the unknown solid electrolyte to confirm whether its constituent elements are Li, M, X, S, and O. When the constituent elements are Li, M, X, S, and O, and the molar ratio values a to f of the constituent elements satisfy 0.8c≦(a+3b)≦1.2c and 1.6f≦(d+n×e)≦2.4f (where n is 4 or 6), the unknown solid electrolyte is determined to be Li, M, X, S, and O. a+d M b X c S e O f For example, Li, Al, and S can be quantified using an ICP-optical emission spectrometer. F can be quantified using an ion chromatograph. O can be quantified by oxygen-nitrogen gas analysis. When the solid electrolyte contains an element M other than Al and an element X other than F, a measurement method capable of quantifying the elements M and X is appropriately selected.
[0069] The all-solid-state battery 1 can be modified in various ways.
[0070] The interface product 23 may be generated by a method other than the charging operation of the all-solid-state battery 1. In this case, when the negative electrode active material 21 is charged to 2.0 V (vs. Li / Li + ) The solid electrolyte 22 may or may not contain O.
[0071] Solid electrolyte layer 13 may contain other substances in addition to solid electrolyte 22. Furthermore, the solid electrolytes contained in solid electrolyte layer 13 and positive electrode 11 may be different from solid electrolyte 22 contained in negative electrode 12. Solid electrolyte 22 may be produced by a method other than mechanical milling.
[0072] The configurations in the above-described embodiment and each modification may be combined as appropriate as long as they are not mutually contradictory.
[0073] While the invention has been particularly illustrated and described, it should be understood that the foregoing description is illustrative and not restrictive, and that numerous modifications and variations are possible without departing from the scope of the invention.
[0074] REFERENCE SIGNS LIST 1 all-solid-state battery 11 positive electrode 12 negative electrode 13 solid electrolyte layer 21 negative electrode active material 22 solid electrolyte 23 compound (interface product) S11 to S13 steps
Claims
1. A battery comprising: a positive electrode; a negative electrode including a negative electrode active material and a solid electrolyte; and a solid electrolyte layer provided between the positive electrode and the negative electrode, wherein in the negative electrode, another compound is present at the interface between the negative electrode active material and the solid electrolyte, and the other compound includes Li and O.
2. The battery according to claim 1, wherein the negative electrode active material is 2.0 V (vs Li / Li + ) A battery whose active material operates at a potential below 3. The battery according to claim 1, wherein the negative electrode active material is 1.0 V (vs Li / Li + ) A battery whose active material operates at a potential below 4. A battery according to claim 1, wherein the other compound is present in the form of a layer at the interface, and the thickness of the other compound is 1 to 1000 nm.
5. The battery according to claim 1, wherein the solid electrolyte comprises Li and O.
6. The battery according to claim 5, wherein said solid electrolyte further contains X which is a halogen element.
7. The battery according to claim 5, wherein the solid electrolyte further contains S.
8. The battery according to claim 5, wherein the solid electrolyte further contains Al.
9. The battery according to claim 5, wherein the solid electrolyte has a composition formula of Li a+d M b X c S e O f (wherein M is an element that becomes trivalent as a cation, and X is a halogen element) and in which 0.8c≦(a+3b)≦1.2c and 1.6f≦(d+n×e)≦2.4f (wherein n is 4 or 6) are satisfied.
10. A battery according to claim 1, wherein said other compound does not contain Ti.
11. A battery according to claim 1, wherein the solid electrolyte contains S, and the other compound does not contain S.
12. The battery according to any one of claims 1 to 11, wherein the negative electrode active material is carbon.
13. A method for manufacturing a battery according to any one of claims 1 to 11, comprising: a) preparing a battery by stacking a positive electrode, a solid electrolyte layer, and a negative electrode containing a negative electrode active material and a solid electrolyte; and b) performing a charging operation on the battery, wherein the solid electrolyte of the negative electrode contains Li and O.
14. A method for manufacturing a battery as defined in any one of claims 1 to 11, comprising: a) a step of preparing a battery by stacking a positive electrode, a solid electrolyte layer, and a negative electrode containing a negative electrode active material and a solid electrolyte; and b) a step of performing a charging operation on the battery, wherein the step a) is performed in an oxygen-containing atmosphere, and in the step b), Li ions move from the positive electrode to the negative electrode.
Citation Information
Patent Citations
Negative electrode active material and method for manufacturing the same, and all-solid lithium secondary battery and method for manufacturing the same
JP2011150942A
Positive electrode material and battery
WO2019135322A1
Electrode material and battery
WO2019146308A1