Negative electrode active material for nonaqueous electrolyte secondary batteries, method for producing same, and aqueous negative electrode slurry composition

The use of silicon compound particles coated with carbon and specific ionic substances in lithium-ion batteries addresses stability issues, reducing gas generation and enhancing performance, particularly in high-temperature conditions, resulting in improved capacity and efficiency.

WO2024247938A1PCT designated stage expired Publication Date: 2024-12-05SHIN ETSU CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019293
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-24
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries using silicon as the negative electrode material face challenges with stability in aqueous solvents, leading to inadequate performance in industrial applications due to gas generation during high-temperature storage, which affects the battery's cycle characteristics and capacity retention.

Method used

The development of negative electrode active material particles made from silicon compounds (SiOx) with a carbon and ionic substance coating, where the carbon coating amount is between 0.3% to 10% by mass, and the ionic substance consists of elements from specific groups in the periodic table, enhancing stability and conductivity, and suppressing interfacial reactions.

Benefits of technology

This approach significantly reduces gas generation during high-temperature storage, improves battery capacity, and maintains high cycle characteristics and initial efficiency, making the batteries suitable for industrial use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019293_05122024_PF_FP_ABST
    Figure JP2024019293_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a negative electrode active material for nonaqueous electrolyte secondary batteries, the negative electrode active material: comprising silicon compound particles which are formed of a silicon compound (SiOx, wherein 0.5 ≤ x ≤ 1.6) that contains an Li compound; containing an Si0-4 component in the surface in XAFS analysis; containing a carbon material and an ionic substance as constituent materials; and having a structure in which at least a part thereof is coated with the carbon material and at least a part of the carbon material and each of the silicon compound particles are coated with the ionic substance, or a structure in which at least a part thereof is coated with the ionic substance and at least a part of the ionic substance and each of the silicon compound particles are coated with the carbon material, wherein the carbon material has a coating amount within a specific range, and the cations and anions of the ionic substance are composed of ions each containing specific elements. Consequently, the present invention provides a negative electrode active material which is capable of stabilizing an aqueous negative electrode slurry, and is capable of improving the initial charge / discharge characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode active material for non-aqueous electrolyte secondary battery, method for producing the same, and aqueous negative electrode slurry composition

[0001] The present invention relates to a negative electrode active material for a non-aqueous electrolyte secondary battery, a method for producing the same, and an aqueous negative electrode slurry composition.

[0002] In recent years, small electronic devices such as mobile terminals have become widespread, and there is a strong demand for further miniaturization, weight reduction, and longer life. In response to such market demands, development of secondary batteries that are small, lightweight, and capable of achieving high energy density has been progressing. The application of these secondary batteries is being considered not only for small electronic devices but also for large electronic devices such as automobiles and power storage systems such as those for homes.

[0003] Among these, lithium-ion secondary batteries are attracting great attention because they can be easily made small and have a high capacity, and can provide a higher energy density than lead batteries and nickel-cadmium batteries.

[0004] The lithium ion secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte solution, and the negative electrode contains a negative electrode active material involved in charge and discharge reactions.

[0005] While carbon-based active materials are widely used as negative electrode active materials, recent market demands have led to a demand for further improvements in battery capacity. To improve battery capacity, the use of silicon as a negative electrode active material has been considered. This is because the theoretical capacity of silicon (4199 mAh / g) is more than 10 times greater than that of graphite (372 mAh / g), and a significant improvement in battery capacity can be expected. The development of silicon materials as negative electrode active materials is being considered not only for silicon itself, but also for alloys and compounds such as oxides. Furthermore, the active material shape is being considered, ranging from the standard coated type for carbon-based active materials to an integrated type in which the material is deposited directly on the current collector.

[0006] However, when silicon is used as the primary raw material for the negative electrode active material, the negative electrode active material expands and contracts during charging and discharging, making it prone to cracking, primarily near the surface of the negative electrode active material. Furthermore, ionic substances are generated within the active material, making it prone to cracking. When the surface layer of the negative electrode active material cracks, a new surface is created, increasing the reactive area of ​​the active material. At this time, the electrolyte decomposes on the new surface, and a coating of the electrolyte decomposition product is formed on the new surface, consuming the electrolyte. This can lead to a deterioration in cycle performance.

[0007] To date, various studies have been conducted on negative electrode active materials and electrode configurations for lithium-ion secondary batteries that are primarily made of silicon materials in order to improve the initial battery efficiency and cycle characteristics.

[0008] Specifically, to achieve good cycle characteristics and high safety, silicon and amorphous silicon dioxide are simultaneously deposited using a vapor-phase method (see, for example, Patent Document 1). Furthermore, to achieve high battery capacity and safety, a carbon material (electron conductor) is provided on the surface of silicon oxide particles (see, for example, Patent Document 2). Furthermore, to improve cycle characteristics and achieve high input / output characteristics, an active material containing silicon and oxygen is prepared, and an active material layer with a high oxygen ratio near the current collector is formed (see, for example, Patent Document 3). Furthermore, to improve cycle characteristics, oxygen is incorporated into the silicon active material, and the silicon active material is formed so that the average oxygen content is 40 at% or less and the oxygen content is higher near the current collector (see, for example, Patent Document 4).

[0009] In addition, in order to improve the initial charge / discharge efficiency, Si phase, SiO 2 , M y In order to improve cycle characteristics, nanocomposites containing SiO2 and metal oxides are used (see, for example, Patent Document 5). x(0.8≦x≦1.5, particle size range = 1 μm to 50 μm) is mixed with a carbon material and fired at a high temperature (see, for example, Patent Document 6). To improve cycle characteristics, the molar ratio of oxygen to silicon in the negative electrode active material is set to 0.1 to 1.2, and the active material is controlled so that the difference between the maximum and minimum molar ratios near the interface between the active material and the current collector is 0.4 or less (see, for example, Patent Document 7). To improve battery load characteristics, a lithium-containing metal oxide is used (see, for example, Patent Document 8). To improve cycle characteristics, a hydrophobic layer such as a silane compound is formed on the surface of the silicon material (see, for example, Patent Document 9).

[0010] In addition, in order to improve cycle characteristics, silicon oxide is used and a graphite coating is formed on the surface thereof to impart conductivity (see, for example, Patent Document 10). In Patent Document 10, the shift value obtained from the RAMAN spectrum of the graphite coating is 1330 cm -1 and 1580 cm -1 A broad peak appears at the peak intensity ratio I 1330 / I 1580 is 1.5<I 1330 / I 1580 <3. In order to achieve high battery capacity and improved cycle characteristics, particles having a silicon microcrystalline phase dispersed in silicon dioxide are used (see, for example, Patent Document 11). In addition, in order to improve overcharge and overdischarge characteristics, silicon oxide is used in which the atomic ratio of silicon to oxygen is controlled to 1:y (0<y<2) (see, for example, Patent Document 12).

[0011] When using a silicon material, high initial efficiency and capacity retention can be achieved by using a silicon material doped with Li. However, Li-doped silicon materials have low stability in aqueous solvents, which reduces the stability of the aqueous negative electrode slurry prepared by mixing the silicon material with the material during negative electrode fabrication, making them unsuitable for industrial use. To improve the stability of aqueous negative electrode slurries, water resistance has been enhanced by attaching phosphate to the outermost layer of the Li-doped silicon material (see, for example, Patent Document 13). However, the stability of aqueous negative electrode slurries has been insufficient, as evidenced by gas generation during high-temperature storage of the aqueous negative electrode slurry. Therefore, a technology has been reported that suppresses gas generation during high-temperature storage of aqueous negative electrode slurries by optimizing the amount of phosphate (see, for example, Patent Document 14). However, although optimizing the amount of phosphate reduces the amount of gas generation, there have been cases where gas generation of more than 1 ml has been observed within 7 days.

[0012] JP 2001-185127 A JP 2002-042806 A JP 2006-164954 A JP 2006-114454 A JP 2009-070825 A JP 2008-282819 A JP 2008-251369 A JP 2008-177346 A JP 2007-234255 A JP 2009-212074 A JP 2009-205950 A JP 06-325765 A JP 2017-152358 A JP 2020-77510 A

[0013] As mentioned above, in recent years, small electronic devices such as mobile terminals have become more powerful and multifunctional, and the lithium-ion secondary batteries that serve as their main power sources are required to have larger battery capacities. One method to solve this problem is to develop lithium-ion secondary batteries with a negative electrode that uses silicon as the main material.

[0014] Furthermore, when using a silicon material, high initial efficiency and capacity retention can be obtained by using a silicon material doped with Li, but on the other hand, the Li-doped silicon material has low stability in aqueous solvents, which reduces the stability of the aqueous negative electrode slurry prepared by mixing the silicon material during negative electrode production, making it industrially unsuitable. To stabilize the aqueous negative electrode slurry, surface treatment of the Li-doped silicon material has been performed, but the stability of the aqueous negative electrode slurry is still insufficient.

[0015] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a negative electrode active material for a non-aqueous electrolyte secondary battery that can stabilize an aqueous negative electrode slurry prepared during the preparation of a negative electrode of a secondary battery and can improve initial charge-discharge characteristics when used as the negative electrode active material for a secondary battery. Another aim is to provide an aqueous negative electrode slurry composition that is stable during the preparation of a negative electrode. Another aim is to provide a method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery that can stabilize the slurry prepared during the preparation of a negative electrode and can improve initial charge-discharge characteristics.

[0016] In order to achieve the above object, the present invention provides a negative electrode active material particle, which is a silicon compound (SiO x : 0.5≦x≦1.6), wherein XAFS analysis reveals that Si is present on the surface of the silicon compound particles. 0~+4The negative electrode active material particles contain a carbon material and an ionic material as constituent materials, and the negative electrode active material particles are at least partially coated with the carbon material, and have a structure in which the silicon compound particles and the carbon material are at least partially coated with the ionic material, or the negative electrode active material particles are at least partially coated with the ionic material, and have a structure in which the silicon compound particles and the ionic material are at least partially coated with the carbon material, and the amount of the carbon material coated is equal to or greater than the amount of the silicon compound particles and the amount of the carbon material coated. The negative electrode active material for a non-aqueous electrolyte secondary battery is characterized in that the carbon material accounts for 0.3 mass % or more and 10 mass % or less of the total amount of the coating layer, the cation of the ionic substance is an ion containing at least one element selected from Group 1 elements, Group 2 elements, Group 4 elements, and Group 13 elements of the periodic table, and the anion of the ionic substance is an ion of an oxide containing at least one element selected from Group 4 elements, Group 5 elements, Group 13 elements, Group 14 elements, and Group 15 elements of the periodic table, or an ion of a halide containing at least one element selected from Group 17 elements of the periodic table.

[0017] The negative electrode active material (also referred to as silicon-based active material) of the present invention contains negative electrode active material particles (also referred to as silicon-based active material particles) containing silicon compound particles, thereby improving battery capacity. Furthermore, the silicon compound particles contain a Li compound, which reduces irreversible capacity generated during charging. This improves initial efficiency. Furthermore, since the negative electrode active material contains a carbon material and an ionic substance, when the negative electrode active material is mixed with an aqueous negative electrode slurry composition (also referred to as aqueous negative electrode slurry) during the negative electrode manufacturing process, it suppresses Li ions eluted from the silicon compound particles and also suppresses interfacial reactions between the particles and the aqueous solution, thereby significantly suppressing the amount of gas generation in the aqueous slurry even under high-temperature storage conditions.

[0018] Furthermore, by ensuring that the amount of carbon coating on the negative electrode active material particles is 0.3 mass % or more and 10 mass % or less, the interfacial reaction can be suppressed and sufficient conductivity can be ensured, resulting in better battery characteristics.

[0019] As described above, the cations of the ionic substance in the surface layer of the silicon-based active material particle are composed of ions containing at least one element selected from Groups 1, 2, 4, and 13 of the Periodic Table. Oxides or fluorides of these elements have low solubility in water, which can suppress interfacial reactions in aqueous slurries and therefore suppress gas generation. Furthermore, when the negative electrode active material is formed into an electrode to fabricate a battery, the charge / discharge behavior is not adversely affected.

[0020] As described above, the anions of the ionic substance in the surface layer of the silicon-based active material particle are ions of an oxide containing at least one element selected from Groups 4, 5, 13, 14, and 15 of the Periodic Table, or ions of a halide containing at least one element selected from Group 17 of the Periodic Table. This allows the ionic substance formed with the cation to have low solubility in water, suppressing interfacial reactions in aqueous slurries and thereby suppressing gas generation. Furthermore, this does not adversely affect the charge / discharge behavior when the negative electrode active material is used to fabricate a battery.

[0021] In this case, the amount of the ionic substance coated is preferably 0.5% by mass or more and 10% by mass or less based on the total amount of the silicon compound particles and the carbon coating layer.

[0022] By controlling the amount of ionic substance within the above range, it is possible to obtain an aqueous negative electrode slurry that is more stable even when stored at high temperatures without impairing the battery characteristics.

[0023] Furthermore, it is preferable that the intensity ratio Id / Ig of the D band to the G band in Raman spectroscopy of the negative electrode active material is 0.5≦Id / Ig≦2.0.

[0024] In this way, if 0.5≦Id / Ig≦2.0, peeling of the carbon film due to expansion and contraction and side reactions on the carbon surface can be suppressed, and therefore better battery characteristics can be obtained.

[0025] In addition, the ratio ISi / Ig of the Si peak intensity to the G band intensity in Raman spectroscopy of the negative electrode active material is preferably 0≦ISi / Ig≦2.0.

[0026] Thus, if 0≦ISi / Ig≦2.0, surface exposure of silicon-based compound particles can be suppressed and gas generation in the aqueous slurry can be delayed, resulting in better battery characteristics.

[0027] The negative electrode active material particles have a specific surface area of ​​0.3 m 2 / g or more 5.0m 2 / g or less is preferable.

[0028] Specific surface area is 0.3m 2 / g or more 5.0m 2 / g or less, the negative electrode active material particles can be uniformly covered with the binder component when preparing the aqueous slurry, and the interfacial reaction with water can be suppressed, thereby suppressing gas generation in the aqueous slurry.

[0029] In addition, Li obtained by X-ray diffraction of the negative electrode active material 2 SiO 3 The crystallite size calculated from the peak at about 2θ=18.7° by the Scherrer equation is preferably 3 nm or more and 10 nm or less.

[0030] Thus, the Li obtained by X-ray diffraction 2 SiO 3 When the crystallite size calculated using the Scherrer equation from the peak at around 2θ=18.7° due to the above is 3 nm or more and 10 nm or less, the elution of alkaline components into the aqueous slurry can be suppressed, and better battery characteristics can be obtained.

[0031] The crystallite size resulting from the Si (220) crystal plane obtained by X-ray diffraction of the negative electrode active material is preferably 0.5 nm or more and 5 nm or less.

[0032] Thus, if the crystallite size resulting from the Si(220) crystal plane is within the above range, better battery characteristics can be obtained.

[0033] The silicon compound particles preferably have a median diameter of 0.5 μm or more and 20 μm or less.

[0034] If the median diameter is 0.5 μm or more, the area where side reactions occur on the surface of the negative electrode active material particles is small, so that excess Li is not consumed and the battery cycle retention rate can be maintained high. Furthermore, if the median diameter is 20 μm or less, expansion during Li insertion is small, making the particles less likely to break and crack. Furthermore, because the expansion of the negative electrode active material particles is small, for example, a negative electrode active material layer made by mixing a commonly used silicon-based active material with a carbon active material is less likely to be destroyed.

[0035] It is preferable that the Group 1 element of the periodic table constituting the cation is Li, Na, or K; that the Group 2 element of the periodic table constituting the cation is Mg or Ca; that the Group 4 element of the periodic table constituting the cation is Zr; or that the Group 13 element of the periodic table constituting the cation is Al.

[0036] If the elements constituting the cations are of this type, the battery characteristics will be good and a more stable ionic substance can be formed at the particle interface, which is preferable.

[0037] It is preferred that the Group 4 element of the periodic table of the oxide constituting the anion is Ti, the Group 5 element of the periodic table of the oxide constituting the anion is Nb, the Group 13 element of the periodic table of the oxide constituting the anion is B or Al, the Group 14 element of the periodic table of the oxide constituting the anion is C or Si, the Group 15 element of the periodic table of the oxide constituting the anion is P, or the Group 17 element of the periodic table of the halide constituting the anion is F.

[0038] If the element constituting the anion is such, it is preferable because it can provide good battery characteristics and form a more stable ionic substance at the particle interface.

[0039] It is preferable that a carbon precursor is present that originates from Si in the silicon compound particles, Li or Al among the elements constituting the cation, or Al or Si among the elements constituting the anion.

[0040] The presence of carbon-forming substances originating from these elements is more preferable because it improves the electrical conductivity of the silicon compound particle surface and improves the battery characteristics.

[0041] The carbon material is preferably a fibrous carbon compound or a carbon nanotube.

[0042] Such a carbonaceous material is more preferable because it improves the electrical conductivity of the surface of the silicon compound particles and improves the battery characteristics.

[0043] The present invention also provides an aqueous negative electrode slurry composition for a non-aqueous electrolyte secondary battery, which comprises the above-mentioned negative electrode active material.

[0044] Such a slurry composition is preferable because it generates little gas when stored under high temperature conditions and enables the industrial production of non-aqueous electrolyte secondary batteries with an advantage.

[0045] In order to achieve the above object, the present invention also provides a non-aqueous electrolyte secondary battery comprising any one of the above negative electrode active materials for a non-aqueous electrolyte secondary battery.

[0046] A nonaqueous electrolyte secondary battery containing such a negative electrode active material for a nonaqueous electrolyte secondary battery has a high battery capacity, and also has good cycle characteristics and initial efficiency.

[0047] Furthermore, the present invention provides a mobile terminal, an electric rickshaw, and a power storage system that include the nonaqueous electrolyte secondary battery.

[0048] The mobile terminal, electric power vehicle, and power storage system equipped with the nonaqueous electrolyte secondary battery are preferable because the nonaqueous electrolyte secondary battery has a high battery capacity, good cycle characteristics, and good initial efficiency.

[0049] The present invention also provides a silicon compound (SiO xa step of coating the silicon compound particles with a carbon material; and a step of inserting Li into the silicon compound particles, the method comprising the steps of preparing negative electrode active material particles having the silicon compound particles and the carbon material, and producing a negative electrode active material for a non-aqueous electrolyte secondary battery comprising the negative electrode active material particles, the method comprising the steps of: coating the silicon compound particles with a carbon material; and intercalating Li into the silicon compound particles; and coating the silicon compound particles with an ionic substance, the cations of which are ions containing at least one element selected from Group 1, Group 2, Group 4, and Group 13 elements of the periodic table, and the anions of which are ions of an oxide containing at least one element selected from Group 4, Group 5, Group 13, Group 14, and Group 15 elements of the periodic table, or ions of a halide containing at least one element selected from Group 17 elements of the periodic table, on the silicon compound particles prior to the step of coating the carbon material. or, after the carbonaceous material coating step, forming a coating of an ionic substance on the surface of at least one of the silicon compound particles and the carbonaceous material, the cations of which are ions containing at least one element selected from Groups 1, 2, 4, and 13 of the Periodic Table of Elements, and the anions of which are ions of an oxide containing at least one element selected from Groups 4, 5, 13, 14, and 15 of the Periodic Table of Elements, or ions of a halide containing at least one element selected from Group 17 of the Periodic Table of Elements; and preparing the negative electrode active material particles so that the amount of the carbonaceous material coating is 0.3% by mass or more and 10% by mass or less, based on the total amount of the silicon compound particles and the carbonaceous material coating layer.

[0050] Such a method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery can provide a non-aqueous negative electrode active material that has a high battery capacity and a good cycle retention rate by taking advantage of the inherent properties of silicon oxide modified with Li, and in which gas generation is significantly suppressed even during high-temperature storage in an aqueous slurry.

[0051] As described above, the negative electrode active material for a non-aqueous electrolyte secondary battery of the present invention can improve the stability of the slurry prepared during secondary battery production, and by using this slurry, an industrially usable coating film can be formed, thereby substantially improving the battery capacity, cycle characteristics, and initial charge / discharge characteristics. Furthermore, the secondary battery of the present invention containing this negative electrode active material for a non-aqueous electrolyte secondary battery can be produced industrially advantageously, and exhibits good battery capacity, cycle characteristics, and initial charge / discharge characteristics. Furthermore, similar effects can be obtained in electronic devices, power tools, electric vehicles, power storage systems, etc. that use the non-aqueous electrolyte secondary battery of the present invention.

[0052] Furthermore, the method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery of the present invention can produce a negative electrode material that can improve the stability of the slurry prepared during the production of the secondary battery and can also improve the battery capacity, cycle characteristics, and initial charge / discharge characteristics.

[0053] 1 is a cross-sectional view showing an example of the configuration of a negative electrode for a non-aqueous electrolyte secondary battery including the negative electrode active material of the present invention; 2 is an in-bulk reforming apparatus that can be used when producing the negative electrode active material of the present invention; 3 is an exploded view showing an example of the configuration of a lithium ion secondary battery (laminate film type) including the negative electrode active material of the present invention;

[0054] As mentioned above, one method for increasing the battery capacity of lithium-ion secondary batteries has been investigated: using a negative electrode primarily made of silicon-based active materials. Lithium-ion secondary batteries primarily made of silicon-based active materials are expected to have initial efficiencies and cycle characteristics comparable to those of lithium-ion secondary batteries using carbon materials (carbon-based negative electrode active materials). However, no negative electrode materials have been proposed that exhibit cycle stability comparable to that of nonaqueous electrolyte secondary batteries using carbon materials. Furthermore, oxygen-containing silicon compounds, in particular, have lower initial efficiencies compared to carbon materials, limiting the improvement in battery capacity. While Li-doping modification treatment has shown improvements in initial efficiency, gas generation in aqueous slurries has been an issue. This gas generation, particularly when aqueous slurries are stored under high-temperature conditions, has been particularly problematic.

[0055] Therefore, the present inventors have conducted extensive research to obtain a negative electrode active material that can easily produce a nonaqueous electrolyte secondary battery having a high battery capacity, good cycle characteristics, and good initial efficiency, and that suppresses gas generation even when an aqueous slurry is stored at high temperatures, and have arrived at the present invention.

[0056] Hereinafter, the present invention will be described in detail with reference to the preferred embodiments, but the present invention is not limited to these.

[0057] [Negative electrode active material of the present invention] The negative electrode active material has particles of a silicon compound (SiO x 1. A negative electrode active material for a non-aqueous electrolyte secondary battery, comprising silicon compound particles each having a surface containing silicon dioxide particles and a silicon monoxide particle, wherein the surface is found to contain silicon dioxide particles by XAFS analysis. 0~+4 components, the negative electrode active material particles contain a carbon material and an ionic material as constituent materials, the negative electrode active material particles are at least partially coated with the carbon material, and have a structure in which the silicon compound particles and at least a portion of the carbon material are coated with the ionic material, or the negative electrode active material particles are at least partially coated with the ionic material, and have a structure in which the silicon compound particles and at least a portion of the ionic material are coated with the carbon material, the amount of the carbon material coated is 0.3 mass % or more and 10 mass % or less with respect to the total of the silicon compound particles and the coating layer of the carbon material, and the cation of the ionic material is composed of an ion containing at least one element selected from Group 1 elements, Group 2 elements, Group 4 elements and Group 13 elements of the periodic table, The anion of the ionic substance satisfies the requirement that it is an ion of an oxide containing at least one element selected from Group 4 elements, Group 5 elements, Group 13 elements, Group 14 elements, and Group 15 elements of the periodic table, or an ion of a halide containing at least one element selected from Group 17 elements of the periodic table.

[0058] Such a negative electrode active material has a high battery capacity because it contains negative electrode active material particles containing a silicon compound. In addition, the silicon compound contains SiO, which becomes unstable when lithium is inserted and extracted during charging and discharging of the battery. 2Since the component portion is pre-modified into a different Li compound, irreversible capacity generated during charging can be reduced. Furthermore, the negative electrode active material particles have appropriate electrical conductivity due to the inclusion of a carbon coating, thereby improving capacity retention and initial efficiency. Furthermore, the negative electrode active material particles contain an ionic substance with low solubility in water, which is composed of a cation containing at least one element selected from Groups 1, 2, 4, and 13 of the Periodic Table, and an anion consisting of an oxide ion containing at least one element selected from Groups 4, 5, 13, 14, and 15 of the Periodic Table, or a halide ion containing at least one element selected from Group 17 of the Periodic Table. This allows the negative electrode active material particles to maintain a stable state without generating gas even in an aqueous slurry, resulting in improved initial efficiency and capacity retention. In particular, the aqueous slurry can be maintained in a stable state even during high-temperature storage.

[0059] [Configuration of Negative Electrode] Next, the configuration of the negative electrode of a secondary battery containing such a negative electrode active material of the present invention will be described.

[0060] Fig. 1 shows a cross-sectional view of a negative electrode containing the negative electrode active material of the present invention. As shown in Fig. 1, a negative electrode 10 has a negative electrode active material layer 12 on a negative electrode current collector 11. This negative electrode active material layer 12 may be provided on both sides or only one side of the negative electrode current collector 11. Furthermore, if the negative electrode active material for a non-aqueous electrolyte secondary battery of the present invention is used, the negative electrode current collector 11 may be omitted.

[0061] [Negative electrode current collector] The negative electrode current collector 11 is made of a highly conductive material that has excellent mechanical strength. Examples of conductive materials that can be used for the negative electrode current collector 11 include copper (Cu) and nickel (Ni). This conductive material is preferably a material that does not form an intermetallic compound with lithium (Li).

[0062] The negative electrode current collector 11 preferably contains carbon (C) and sulfur (S) in addition to the main elements. This is because the physical strength of the negative electrode current collector is improved. In particular, when the current collector has an active material layer that expands during charging, if the current collector contains the above elements, it has the effect of suppressing deformation of the electrode including the current collector. The content of the above contained elements is not particularly limited, but is preferably 100 ppm or less. This is because a higher deformation suppression effect can be obtained.

[0063] The surface of the negative electrode current collector 11 may be roughened or may not be roughened. A roughened negative electrode current collector is, for example, a metal foil that has been subjected to electrolytic treatment, embossing treatment, or chemical etching treatment. A non-roughened negative electrode current collector is, for example, a rolled metal foil.

[0064] [Negative Electrode Active Material Layer] The negative electrode active material layer 12 may contain multiple types of negative electrode active materials, such as silicon-based active material particles and carbon-based active materials. Furthermore, depending on the battery design, other materials such as a thickener (also referred to as a "binding agent" or "binder") and a conductive additive may be included. The negative electrode active material may be in the form of particles.

[0065] As described above, the negative electrode active material of the present invention is a SiO x (0.5≦x≦1.6). The silicon-based active material particles are made of silicon oxide material (SiO x (x: 0.5≦x≦1.6), and it is preferable that x is close to 1 in the composition, because this results in high cycle characteristics. Note that the composition of the silicon oxide material in the present invention does not necessarily mean 100% purity, and it may contain trace amounts of impurity elements and Li.

[0066] Furthermore, in the present invention, the lower the crystallinity of the silicon compound (crystallinity of Si crystallites), the better. Specifically, when the negative electrode active material particles are measured by X-ray diffraction using Cu-Kα radiation, the crystallite size resulting from the Si (220) crystal plane obtained by the X-ray diffraction is preferably 5 nm or less. Furthermore, it is preferable that the half-width of the diffraction peak resulting from the (220) crystal plane obtained by X-ray diffraction is 1.5° or more. In particular, it is preferable that the diffraction peak is broad and has no clear peak. In this way, particularly low crystallinity and a small amount of Si crystals not only improves battery characteristics but also enables the production of stable Li compounds.

[0067] The crystallite size resulting from this Si (220) crystal plane cannot be calculated by ordinary analysis, but can be calculated by XRD peak analysis. Calculation of crystallite size by XRD can be performed, for example, under the following conditions. For broad peaks, analysis can be performed using the analysis software TOPAS, for example, under the following conditions. XRD Measurement Apparatus: Bruker D2 PHASER X-ray source: Cu Divergence slit: 0.5° Incident side solar: 4° Receiving side solar: 4° Calculation of Crystallite Size Analysis Software: DIFFRAC. TOPAS Analysis Method: Peak fitting method Emission Profile: CuKa5. lam Function: FP (First Principle) function Refinement Option: Select "Calculate Error" and "Use Extrapolation"

[0068] The median diameter of the silicon compound particles is not particularly limited, but is preferably 0.5 μm or more and 20 μm or less (volume basis). This range facilitates the absorption and release of lithium ions during charging and discharging, and the silicon-based active material particles are less likely to crack. If the median diameter is 0.5 μm or more, the surface area is not too large, making it less likely for side reactions to occur during charging and discharging, and reducing the irreversible capacity of the battery. On the other hand, if the median diameter is 20 μm or less, the silicon-based active material particles are less likely to crack and new surfaces are less likely to appear, making this preferable.

[0069] Furthermore, in the present invention, the silicon-based active material contains Li as the Li compound contained in the silicon compound. 2 SiO 3 It is preferable to include Li 4 SiO 4 and Li 6 Si 2 O 7 Li may be present. 2 SiO 3 In addition to Li 4 SiO 4 , Li 6 Si 2 O 7 Li silicates such as these are relatively more stable than other Li compounds, and therefore silicon-based active materials containing these Li compounds can achieve more stable battery characteristics. 2 It can be obtained by selectively changing a part of the components to Li compounds and modifying silicon compounds.

[0070] The amount of Li compounds inside the negative electrode active material particles and silicon compound particles can be quantified by NMR (nuclear magnetic resonance) and XPS (X-ray photoelectron spectroscopy).

[0071] In addition, in the present invention, when modifying the silicon compound, electrochemical methods, modification by oxidation-reduction reaction, and physical methods such as thermal doping can be used. In particular, when the silicon compound is modified using electrochemical methods and oxidation-reduction modification, the battery characteristics of the negative electrode active material are improved. Furthermore, in the modification, not only the insertion of Li into the silicon compound but also the stabilization of the Li compound by heat treatment and the desorption of Li from the silicon compound are preferably performed. This further improves the stability of the negative electrode active material against slurry, such as its water resistance.

[0072] As described above, in the present invention, the silicon compound particles in the silicon-based active material particles may be at least partially coated with the carbon material, and have a structure in which the silicon compound particles and at least a portion of the carbon material are coated with the ionic material, or may be at least partially coated with the ionic material, and have a structure in which the silicon compound particles and at least a portion of the ionic material are coated with the carbon material, and the amount of the carbon material coated is 0.3 mass % or more and 10 mass % or less with respect to the total of the silicon compound particles and the coating layer of the carbon material, and the cation of the ionic material may be an ion containing at least one element selected from Groups 1, 2, 4, and 13 of the Periodic Table, and the anion of the ionic material may be an ion of an oxide containing at least one element selected from Groups 4, 5, 13, 14, and 15 of the Periodic Table, or an ion of a halide containing at least one element selected from Group 17 of the Periodic Table.

[0073] In this way, the presence of the carbon material and the ionic material outside the negative electrode active material particles can suppress gas generation during high-temperature storage of the aqueous slurry. Furthermore, the presence of the carbon material can provide appropriate electrical conductivity. The relationship between the carbon material and the ionic material may be such that at least a portion of the silicon-based compound is coated with a carbon film, and at least a portion of the silicon-based compound and the carbon film is coated with an ionic material, or such that at least a portion of the silicon-based compound is coated with an ionic material, and at least a portion of the silicon-based compound and the ionic material is coated with a carbon material.

[0074] In the negative electrode active material of the present invention, the amount of the ionic substance coated is preferably 0.5% by mass or more and 10% by mass or less based on the total amount of the silicon compound particles and the carbon coating layer. By controlling the amount of the ionic substance within the above range, it is possible to obtain an aqueous negative electrode slurry that is more stable even when stored at high temperatures without impairing the battery characteristics.

[0075] In addition, in the negative electrode active material of the present invention, when the negative electrode active material particles are measured by X-ray diffraction using Cu-Kα rays, the Li obtained by the X-ray diffraction2 SiO 3 It is preferable that the crystallite size calculated from the half width of the peak at about 2θ = 18.7° due to the above is 3 nm or more and 10 nm or less. 2 SiO 3 When the crystallite size calculated from the half width of the peak at around 2θ=18.7° due to the above is 3 nm or more and 10 nm or less, the elution of alkaline components into the aqueous slurry can be suppressed, and better battery characteristics can be obtained.

[0076] In the negative electrode active material of the present invention, the amount of carbon coating on the negative electrode active material particles is 0.3% by mass or more and 10% by mass or less of the total of the silicon compound and the carbon coating layer. Thus, when the amount of carbon coating on the negative electrode active material particles is 0.3% by mass or more and 10% by mass or less, sufficient conductivity can be ensured, resulting in better battery characteristics.

[0077] In the negative electrode active material of the present invention, the negative electrode active material particles have a specific surface area of ​​0.3 m 2 / g or more 5.0m 2 The specific surface area here is determined by the BET method. 2 / g or more 5.0m 2 / g or less, the negative electrode active material particles can be uniformly covered with the binder component when preparing the aqueous slurry, and the interfacial reaction with water can be suppressed, thereby suppressing gas generation in the aqueous slurry.

[0078] In the negative electrode active material of the present invention, the intensity ratio Id / Ig of the D band to the G band as determined by Raman spectroscopy of the negative electrode active material particles is preferably 0.5≦Id / Ig≦2.0, where 0.5≦Id / Ig≦2.0 can suppress peeling of the carbon film due to expansion and contraction and side reactions on the carbon surface, thereby achieving better battery characteristics.

[0079] In the negative electrode active material of the present invention, the intensity ratio ISi / Ig of the Si peak intensity to the G band in Raman spectroscopy of the negative electrode active material particles is preferably 0≦ISi / Ig≦2.0. If 0≦ISi / Ig≦2.0, surface exposure of the silicon-based compound particles can be suppressed and gas generation in the aqueous slurry can be delayed, resulting in better battery characteristics.

[0080] In addition, in the negative electrode active material of the present invention, it is preferable that carbon precursors originating from Si in the silicon compound particles, Li or Al among the elements constituting the cations, or Al or Si among the elements constituting the anions are present, which is more preferable because the presence of carbon precursors originating from these elements improves the conductivity of the silicon compound particle surface and improves the battery characteristics.

[0081] The carbon material is preferably a fibrous carbon compound or a carbon nanotube, since such a carbon material improves the electrical conductivity of the silicon compound particle surface and improves the battery characteristics.

[0082] [Manufacturing Method of Negative Electrode] Next, an example of a manufacturing method of the negative electrode of the nonaqueous electrolyte secondary battery of the present invention will be described.

[0083] First, we will explain how to manufacture the negative electrode material contained in the negative electrode. x (0.5≦x≦1.6) x Silicon compound particles containing 0.5≦x≦1.6 are prepared. Next, at least a portion of the silicon compound particles may be coated with a carbon material. Next, Li is inserted into the silicon compound particles to modify the silicon compound particles. During this Li insertion, Li may also be removed. This Li insertion results in Li 2 SiO 3At the same time, a Li compound can be formed inside or on the surface of the silicon compound particles. Then, an ion source containing at least one element selected from Groups 1, 2, 4, and 13 of the Periodic Table of Elements, and an anion source containing an oxide containing at least one element selected from Groups 4, 5, 13, 14, and 15 of the Periodic Table of Elements, or a halide containing at least one element selected from Group 17 of the Periodic Table, are added, followed by heat treatment, thereby forming an ionic substance on the surface of the silicon compound particles, or on the surface of the silicon compound particles and the carbon coating. After forming the ionic substance on the surface of the silicon compound particles, the silicon compound particles may be coated with a carbon material. In this case, the carbon material is present in an amount of 0.3% by mass or more and 10% by mass or less. A negative electrode material and a negative electrode can be produced using negative electrode active material particles containing such silicon compound particles, for example by mixing them with a conductive additive or binder.

[0084] The element of Group 1 of the periodic table that constitutes the cation is preferably Li, Na, or K.

[0085] The element of Group 2 of the periodic table that constitutes the cation is preferably Mg or Ca.

[0086] The element of Group 4 of the periodic table that constitutes the cation is preferably Zr.

[0087] The element of Group 13 of the periodic table that constitutes the cation is preferably Al.

[0088] The element of Group 4 of the periodic table of the oxide constituting the anion component is preferably Ti.

[0089] The element of Group 5 of the periodic table of the oxide constituting the anion component is preferably Nb.

[0090] The element of Group 13 of the periodic table of the oxide constituting the anion component is preferably B or Al.

[0091] The element of Group 14 of the periodic table of the oxide constituting the anion component is preferably C or Si.

[0092] The element of Group 15 of the periodic table of the oxide constituting the anion component is preferably phosphorus.

[0093] The element of Group 17 of the periodic table of the halide constituting the anion component is preferably F.

[0094] More specifically, the negative electrode active material is produced, for example, by the following procedure.

[0095] First, a raw material that generates silicon oxide gas is heated in the presence of an inert gas or under reduced pressure at a temperature range of 900°C to 1600°C to generate silicon oxide gas. In this case, the raw material is a mixture of metallic silicon powder and silicon dioxide powder. Considering the surface oxygen of the metallic silicon powder and the presence of trace oxygen in the reactor, the molar ratio of the mixture is preferably in the range of 0.8 < metallic silicon powder / silicon dioxide powder < 1.3. The Si crystallites in the particles are controlled by changing the feeding range and vaporization temperature, as well as by heat treatment after generation. The generated gas is deposited on an adsorption plate. The temperature inside the reactor is lowered to below 100°C, and the deposit is removed and pulverized using a ball mill, jet mill, or the like.

[0096] Next, a carbon coating may be formed on the surface of the resulting silicon oxide powder material (silicon compound particles). The carbon coating is effective in further improving the battery characteristics of the negative electrode active material. Note that the carbon coating may be performed at the end of the process, as described below.

[0097] The method of forming a carbon coating on the surface of a powder material is preferably pyrolysis CVD or pyrolysis of an organic compound. In pyrolysis CVD, silicon oxide powder is placed in a furnace, which is filled with hydrocarbon gas and the temperature inside the furnace is raised. The decomposition temperature is not particularly limited, but is preferably 1200°C or less. More preferably, it is 950°C or less, which makes it possible to suppress unintended disproportionation of silicon oxide. The hydrocarbon gas is not particularly limited, but is preferably C n H mIn the composition, 2≧n is desirable because it results in low production costs and good physical properties of the decomposition products. In the thermal decomposition of organic compounds, coal tar or pitch is applied to the surface of silicon compound particles, which are then placed in a furnace and the temperature inside the furnace is raised. The coal tar or pitch is thermally decomposed to form carbon, which is then formed on the surface of the silicon compound particles. There are no particular restrictions on the decomposition temperature, but it is desirable that it be 1200°C or lower, as in thermal decomposition CVD. A temperature of 950°C or lower is more desirable, as it is possible to suppress unintended disproportionation of silicon oxides.

[0098] Next, Li was inserted into the negative electrode active material particles containing the silicon active material particles prepared as described above, and Li 2 SiO 3 The insertion of Li is preferably carried out by an electrochemical method or a redox method.

[0099] In the electrochemical reforming, the structure of the apparatus is not particularly limited. For example, in-bulk reforming can be performed using an in-bulk reforming apparatus 20 shown in FIG. 2 . The in-bulk reforming apparatus 20 includes a bath 27 filled with an organic solvent 23, a positive electrode (lithium source, reforming source) 21 disposed in the bath 27 and connected to one side of a power supply 26, a powder storage container 25 disposed in the bath 27 and connected to the other side of the power supply 26, and a separator 24 disposed between the positive electrode 21 and the powder storage container 25. The powder storage container 25 stores silicon oxide powder 22. The powder storage container stores a silicon compound (silicon oxide particles), and a voltage is applied from the power supply between the powder storage container containing the silicon oxide particles and the positive electrode (lithium source). This allows lithium to be inserted into and removed from the silicon compound particles, thereby reforming the silicon oxide powder 22. The resulting silicon oxide is dispersed in a solvent again, and the desired cation and anion components are supplied to form ionic substances on the surfaces of the silicon compound particles. After the ionic substances are formed, the Li compound can be stabilized by heat treatment at 200 to 800°C.

[0100] As the organic solvent 23 in the bath 27, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, fluoromethyl methyl carbonate, difluoromethyl methyl carbonate, or the like can be used. In addition, as the electrolyte salt contained in the organic solvent 23, lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ) etc. can be used.

[0101] The positive electrode 21 may be made of Li foil or a Li-containing compound such as lithium carbonate, lithium oxide, lithium cobalt oxide, lithium iron olivine, lithium nickel oxide, or lithium vanadium phosphate.

[0102] After the electrochemical Li-doping modification, the slurry may be washed with alkaline water containing lithium carbonate, lithium oxide, or lithium hydroxide dissolved therein, alcohol, a weak acid, or pure water. By washing, excess alkaline components can be eluted, improving the stability of the slurry.

[0103] When the cation species is lithium, lithium ions inserted by modification can be used as the ion source. Alternatively, lithium ions can be newly supplied as nitrates or the like.

[0104] In the formation of an ionic substance, when the cationic species is other than lithium, it is preferable to supply it in a specified amount as a nitrate.

[0105] When selecting an anionic species for forming an ionic substance, it is preferable to use an anhydride. When selecting phosphorus from Group 15, phosphoric anhydride, which is an anhydride, is preferable. When selecting carbon from Group 14, carbon dioxide, which is an anhydride, is preferable. When selecting silicon, silicon oxide is preferable. When selecting boron from Group 13, boric acid anhydride, which is an anhydride, or a mixture of oxalic acid and boric acid anhydride is preferable. When selecting fluorine from Group 17, aluminum trifluoride is preferable. When selecting titanium from Group 4, titanium oxide is preferable. When selecting niobium from Group 5, niobium oxide is preferable.

[0106] In the oxidation-reduction modification, for example, lithium can be intercalated by first immersing silicon active material particles in Solution A, which contains lithium dissolved in an ether-based solvent. This Solution A may also contain a polycyclic aromatic compound or a linear polyphenylene compound. The resulting silicon oxide can be dispersed again in a solvent and the desired cation and anion components added to form ionic substances on the surface of the silicon compound particles. After forming the ionic substances, the resulting silicon oxide can be heat-treated at 400 to 800°C to stabilize the Li compound. After lithium intercalation, the silicon active material particles may be immersed in Solution B, which contains a polycyclic aromatic compound or a linear polyphenylene compound or a derivative thereof, to desorb active lithium from the silicon active material particles. The solvent for Solution B may be, for example, an ether-based solvent, a ketone-based solvent, an ester-based solvent, an alcohol-based solvent, an amine-based solvent, or a mixture thereof. Washing may also be performed with alkaline water, alcohol, weak acid, or pure water containing lithium carbonate, lithium oxide, or lithium hydroxide dissolved therein. By washing, excess alkaline components can be eluted, improving the stability of the slurry.

[0107] Examples of ether solvents that can be used in solution A include diethyl ether, tert-butyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and mixtures thereof. Among these, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, and diethylene glycol dimethyl ether are particularly preferred. These solvents are preferably dehydrated and deoxygenated.

[0108] Furthermore, the polycyclic aromatic compound contained in solution A may be one or more of naphthalene, anthracene, phenanthrene, naphthalene, pentacene, pyrene, triphenylene, coronene, chrysene, and derivatives thereof, and the linear polyphenylene compound may be one or more of biphenyl, terphenyl, and derivatives thereof.

[0109] The polycyclic aromatic compound contained in solution B may be one or more of naphthalene, anthracene, phenanthrene, pentacene, pyrene, triphenylene, coronene, chrysene, and derivatives thereof.

[0110] The ether solvent for solution B may be diethyl ether, tertbutyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, or a mixture thereof.

[0111] As the ketone solvent, acetone, acetophenone, etc. can be used.

[0112] As the ester solvent, methyl formate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, and the like can be used.

[0113] As the alcohol solvent, methanol, ethanol, propanol, isopropyl alcohol, and the like can be used.

[0114] As the amine solvent, methylamine, ethylamine, ethylenediamine, etc. can be used.

[0115] Alternatively, Li may be inserted into the negative electrode active material particles by thermal doping. In this case, for example, the negative electrode active material particles can be modified by mixing them with LiH powder or Li powder and heating them in a non-oxidizing atmosphere. Examples of the non-oxidizing atmosphere include an Ar atmosphere. More specifically, LiH powder or Li powder is first thoroughly mixed with silicon oxide powder in an Ar atmosphere, sealed, and homogenized by stirring the sealed container. The mixture is then heated at a temperature ranging from 600°C to 750°C for modification. To remove Li from the silicon compound, the heated powder may be thoroughly cooled and washed with alkaline water containing lithium carbonate, lithium oxide, or lithium hydroxide, alcohol, a weak acid, or pure water. Washing can dissolve excess alkaline components, improving the slurry stability.

[0116] Subsequently, the desired cation species and anion species are mixed with the negative electrode active material particles containing the silicon compound particles, and the resulting mixture is heat-treated at 300° C. to 800° C., thereby forming ionic substances on the surfaces of the silicon compound particles. At this time, the surfaces of the silicon compound particles may be coated with carbon.

[0117] It is preferable to produce a negative electrode active material in which the ionic substance is contained in an amount of 0.5% by mass or more and 10% by mass or less based on the total amount of the silicon compound particles and the carbon coating layer.

[0118] The mixing method may be wet mixing in which a cation source and an anion source are supplied to silicon compound particles dispersed in a solution, or dry mixing such as stirring mixing, tumbling mixing, or shear mixing may be used.

[0119] In this case, it is preferable that the ionic substance has low solubility in water.

[0120] A carbon coating may be formed on silicon-based compound particles containing an ionic substance on the surface thereof, which is effective in further improving the battery characteristics of the negative electrode active material.

[0121] As described above, the method for forming a carbon coating on the surface of the powder material may be pyrolysis CVD or carbonization of an organic compound.

[0122] In the case of pyrolytic CVD, the process is as described above.

[0123] In the case of carbonization of an organic compound, powder particles and an organic compound are mixed in a predetermined ratio, and the resulting mixture is heat-treated, whereby the organic substance is decomposed and carbonized, forming a carbon coating on the surface of the powder particles.

[0124] Examples of organic compounds include, but are not limited to, fractions obtained in a tar distillation process such as gas light oil, creosote oil, anthracene oil, and naphtha cracked tar oil; conductive polymers such as polyaniline, polyacetylene, and polyphenylene; and sugars such as glucose.

[0125] The mixing method with the organic compound may be dry mixing such as stirring mixing, rolling mixing, or shear mixing, or may be wet mixing with the organic compound dispersed in a solution.

[0126] The heat treatment temperature is preferably 300 to 800°C, more preferably 350 to 700°C, further preferably 400 to 650°C, and particularly preferably 400 to 600°C.

[0127] Furthermore, as described above, in the negative electrode active material of the present invention, it is preferable that a carbon product originating from Si in the silicon compound particles, Li or Al among the elements constituting the cations, or Al or Si among the elements constituting the anions is present, and this can be formed by performing a pyrolytic CVD treatment under conditions in which Si in the silicon compound particles, Li or Al among the elements constituting the cations, or Al or Si among the elements constituting the anions are present on the outermost surface. Under the heating conditions during the pyrolytic CVD treatment, radical species consisting of the elements present on the outermost surface are generated, and the product reacts with the hydrocarbon gas during the pyrolytic CVD treatment to form a carbon product.

[0128] <Water-based negative electrode slurry composition> The negative electrode active material prepared as described above is mixed with other materials such as a negative electrode binder and a conductive additive, as needed, and then water is added (an organic solvent or the like can also be added in addition to water), thereby obtaining a water-based negative electrode slurry composition.

[0129] Such an aqueous negative electrode slurry composition can minimize changes over time due to gas generation during storage, etc., and therefore has a high degree of freedom in the manufacturing process and is suitable for industrialization. Furthermore, by producing a negative electrode using the aqueous negative electrode slurry composition, a secondary battery with high capacity and good initial charge-discharge characteristics can be obtained.

[0130] Next, the aqueous negative electrode slurry composition is applied to the surface of the negative electrode current collector and dried to form a negative electrode active material layer. At this time, hot pressing or the like may be performed as necessary. In this manner, the negative electrode can be produced.

[0131] <Lithium Ion Secondary Battery> Next, a laminate film type lithium ion secondary battery will be described as a specific example of the nonaqueous electrolyte secondary battery of the present invention.

[0132] [Configuration of Laminate Film Type Secondary Battery] The laminate film type lithium ion secondary battery 30 shown in Fig. 3 mainly comprises a wound electrode body 31 housed inside a sheet-like exterior member 35. This wound electrode body 31 has a separator between the positive and negative electrodes and is wound. There are also cases where the electrode body is not wound, but instead houses a laminate having a separator between the positive and negative electrodes. In either type of electrode body, a positive electrode lead 32 is attached to the positive electrode, and a negative electrode lead 33 is attached to the negative electrode. The outermost periphery of the electrode body is protected by protective tape.

[0133] The positive and negative electrode leads 32, 33 are, for example, led out in one direction from the inside to the outside of the exterior member 35. The positive electrode lead 32 is formed of a conductive material such as aluminum, and the negative electrode lead 33 is formed of a conductive material such as nickel or copper.

[0134] The exterior member 35 is, for example, a laminate film in which a fusion layer, a metal layer, and a surface protection layer are laminated in this order, and the outer peripheral edges of the fusion layers of the two films of this laminate film are fused together or attached with an adhesive or the like so that the fusion layer faces the electrode body 31. The fusion portion is, for example, a film such as polyethylene or polypropylene, and the metal portion is, for example, aluminum foil. The protection layer is, for example, nylon or the like.

[0135] An adhesive film 34 is inserted between the exterior member 35 and the positive and negative electrode leads to prevent outside air from entering, and is made of, for example, polyethylene, polypropylene, or polyolefin resin.

[0136] The positive electrode has a positive electrode active material layer on one or both sides of a positive electrode current collector, similar to the negative electrode 10 in FIG. 1, for example.

[0137] The positive electrode current collector is made of a conductive material such as aluminum.

[0138] The positive electrode active material layer contains one or more positive electrode materials capable of absorbing and releasing lithium ions, and may contain other materials such as a positive electrode binder, a positive electrode conductive additive, a dispersant, etc. In this case, details regarding the positive electrode binder and the positive electrode conductive additive are the same as, for example, the negative electrode binder and the negative electrode conductive additive already described.

[0139] The positive electrode material is preferably a lithium-containing compound. Examples of the lithium-containing compound include a composite oxide made of lithium and a transition metal element, or a phosphate compound containing lithium and a transition metal element. Among these positive electrode materials, compounds containing at least one of nickel, iron, manganese, and cobalt are preferred. Their chemical formulas are, for example, Li x M 1 O 2 Or Li y M 2 P.O. 4 In the formula, M 1 , M 2 represents at least one transition metal element. The values ​​of x and y vary depending on the charge / discharge state of the battery, but are generally expressed as 0.05≦x≦1.10 and 0.05≦y≦1.10.

[0140] Examples of composite oxides containing lithium and transition metal elements include lithium cobalt composite oxide (Li x CoO 2 ), lithium nickel composite oxide (Li x NiO 2 ), lithium nickel cobalt composite oxide, etc. Examples of the lithium nickel cobalt composite oxide include lithium nickel cobalt aluminum composite oxide (NCA) and lithium nickel cobalt manganese composite oxide (NCM).

[0141] Examples of phosphate compounds containing lithium and a transition metal element include lithium iron phosphate compounds (LiFePO 4 ) or lithium iron manganese phosphate compound (LiFe 1-u Mn u P.O. 4 (0<u<1)). By using these positive electrode materials, it is possible to obtain a high battery capacity and also excellent cycle characteristics.

[0142] [Negative Electrode] The negative electrode has a configuration similar to that of the lithium-ion secondary battery negative electrode 10 shown in Fig. 1, and has, for example, negative electrode active material layers on both sides of a current collector. This negative electrode preferably has a negative electrode charge capacity greater than the electrical capacity (charge capacity as a battery) obtained from the positive electrode active material. This can suppress the deposition of lithium metal on the negative electrode.

[0143] The positive electrode active material layer is provided on a portion of both sides of the positive electrode current collector, and similarly, the negative electrode active material layer is provided on a portion of both sides of the negative electrode current collector. In this case, for example, the negative electrode active material layer provided on the negative electrode current collector has a region where the opposing positive electrode active material layer is not present. This is for the purpose of designing a stable battery.

[0144] The region where the negative electrode active material layer and the positive electrode active material layer do not face each other is hardly affected by charging and discharging, and therefore the state of the negative electrode active material layer is maintained as it was immediately after formation, allowing the composition of the negative electrode active material to be accurately determined with good reproducibility, regardless of whether charging and discharging are performed.

[0145] [Separator] The separator separates the positive electrode and the negative electrode, prevents current short circuit due to contact between the electrodes, and allows lithium ions to pass through. This separator is formed of a porous film made of, for example, a synthetic resin or ceramic, and may have a laminate structure in which two or more types of porous film are laminated. Examples of synthetic resins include polytetrafluoroethylene, polypropylene, and polyethylene.

[0146] [Electrolyte Solution] At least a portion of the active material layer or the separator is impregnated with a liquid electrolyte (electrolyte solution). This electrolyte solution contains an electrolyte salt dissolved in a solvent and may contain other materials such as additives.

[0147] The solvent can be, for example, a non-aqueous solvent. Examples of non-aqueous solvents include ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 1,2-dimethoxyethane, and tetrahydrofuran. Among these, it is desirable to use at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. This is because better properties can be obtained. In this case, more advantageous properties can be obtained by combining a high-viscosity solvent such as ethylene carbonate or propylene carbonate with a low-viscosity solvent such as dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate. This is because the dissociation property and ion mobility of the electrolyte salt are improved.

[0148] It is preferable that the solvent additive contains an unsaturated carbon-bond cyclic carbonate. This is because a stable coating is formed on the negative electrode surface during charge and discharge, and the decomposition reaction of the electrolyte can be suppressed. Examples of the unsaturated carbon-bond cyclic carbonate include vinylene carbonate and vinylethylene carbonate.

[0149] It is also preferable that the solvent additive contains sultone (cyclic sulfonic acid ester), which improves the chemical stability of the battery. Examples of sultones include propane sultone and propene sultone.

[0150] Furthermore, it is preferable that the solvent contains an acid anhydride, because this improves the chemical stability of the electrolyte solution. Examples of acid anhydrides include propanedisulfonic acid anhydride.

[0151] The electrolyte salt may include, for example, one or more light metal salts such as lithium salts. Examples of the lithium salt include lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ) etc.

[0152] The content of the electrolyte salt is preferably 0.5 mol / kg or more and 2.5 mol / kg or less relative to the solvent, because this allows high ionic conductivity to be obtained.

[0153] Furthermore, the present invention provides a mobile terminal, an electric power vehicle, and a power storage system including the nonaqueous electrolyte secondary battery. Such a mobile terminal, an electric power vehicle, and a power storage system including the nonaqueous electrolyte secondary battery are preferable because the nonaqueous electrolyte secondary battery has a high battery capacity, as well as good cycle characteristics and initial efficiency.

[0154] [Method for manufacturing laminate film-type secondary battery] First, a positive electrode is fabricated using the above-described positive electrode material. First, a positive electrode active material is mixed with, if necessary, a positive electrode binder, a positive electrode conductive additive, etc. to form a positive electrode mixture, which is then dispersed in an organic solvent to form a positive electrode mixture slurry. Next, the mixture slurry is applied to a positive electrode current collector using a coating device such as a knife roll or a die coater having a die head, and then dried with hot air to obtain a positive electrode active material layer. Finally, the positive electrode active material layer is compression-molded using a roll press or the like. Heating may be performed during this process, and compression may be repeated multiple times.

[0155] Next, using the same procedure as in the production of the negative electrode 10 for a lithium ion secondary battery described above, a negative electrode active material layer is formed on the negative electrode current collector to produce a negative electrode.

[0156] When preparing the positive and negative electrodes, active material layers are formed on both sides of the positive and negative electrode current collectors, respectively, and the lengths of the active material applied on both sides of each electrode may be offset (see FIG. 1).

[0157] Next, an electrolyte solution is prepared. Next, a positive electrode lead 32 is attached to the positive electrode current collector by ultrasonic welding or the like, and a negative electrode lead 33 is attached to the negative electrode current collector. Next, the positive electrode and the negative electrode are laminated or wound with a separator interposed therebetween to prepare a wound electrode body 31, and a protective tape is adhered to the outermost periphery. Next, the wound body is molded into a flat shape. Next, the wound electrode body is sandwiched between folded film-like exterior members 35, and the insulating portions of the exterior members are bonded together by a heat fusion method, and the wound electrode body is encapsulated with only one side open. Next, an adhesive film is inserted between the positive electrode lead and the negative electrode lead and the exterior member. Next, a predetermined amount of the prepared electrolyte solution is poured through the open portion, and vacuum impregnation is performed. After impregnation, the open portion is sealed by a vacuum heat fusion method. In this manner, a laminate film-type secondary battery 30 can be manufactured.

[0158] In the nonaqueous electrolyte secondary battery of the present invention, such as the laminate film type secondary battery 30 fabricated above, the negative electrode utilization rate during charge and discharge is preferably 93% or more and 99% or less. If the negative electrode utilization rate is in the range of 93% or more, the initial charge efficiency does not decrease and the battery capacity can be significantly improved. Furthermore, if the negative electrode utilization rate is in the range of 99% or less, Li does not precipitate and safety can be ensured.

[0159] EXAMPLES The present invention will be explained in more detail below by showing examples and comparative examples of the present invention, but the present invention is not limited to these examples.

[0160] Example 1-1 A laminate film type secondary battery 30 shown in FIG. 3 was fabricated by the following procedure.

[0161] First, the positive electrode was prepared. The positive electrode active material was lithium nickel cobalt aluminum composite oxide (LiNi 0.7 Co 0.25 Al 0.05A positive electrode mixture was prepared by mixing 95 parts by mass of a positive electrode conductive additive (acetylene black), 2.5 parts by mass of a positive electrode binder (polyvinylidene fluoride, PVDF). The positive electrode mixture was then dispersed in an organic solvent (N-methyl-2-pyrrolidone, NMP) to form a paste-like slurry. The slurry was then applied to both sides of the positive electrode current collector using a coating device with a die head and dried using a hot air dryer. A positive electrode current collector with a thickness of 15 μm was used. Finally, compression molding was performed using a roll press.

[0162] Next, a negative electrode was prepared. First, a silicon-based active material was prepared as follows. A raw material (vaporized starting material) containing a mixture of silicon metal and silicon dioxide was placed in a reactor, vaporized in a vacuum atmosphere of 10 Pa, and deposited on an adsorption plate. After sufficient cooling, the deposit was removed and pulverized in a ball mill. After adjusting the particle size, if carbon was selected for the first layer, a carbon coating was formed by thermal CVD. Next, lithium was inserted into the silicon compound particles coated with the carbon coating using an oxidation-reduction method to modify them. First, the negative electrode active material particles were immersed in a solution (Solution A) in which lithium flakes and the aromatic compound naphthalene were dissolved in tetrahydrofuran (hereinafter referred to as THF). Naphthalene was dissolved in the THF solvent at a concentration of 0.2 mol / L, and then 12% by mass of lithium flakes were added to the THF and naphthalene mixture to prepare Solution A. The temperature of the solution when the negative electrode active material particles were immersed was 20° C., and the immersion time was 20 hours. Thereafter, the negative electrode active material particles were collected by filtration. By the above treatment, lithium was intercalated into the negative electrode active material particles.

[0163] The resulting silicon compound particles were dispersed in tetrahydrofuran, and an ion source was then added to form an ionic substance on the surface. Since the target cation component was lithium, the lithium inserted into the silicon compound particles was used as the ion source. A predetermined amount of phosphoric anhydride was added as an anion source, and the lithium ions reacted with the phosphoric anhydride on the surface to form an ionic substance coating of lithium phosphate on the silicon compound particle surface.

[0164] The obtained silicon compound particles were heat treated in an argon atmosphere at 650° C. or less for 24 hours to stabilize the Li compound.

[0165] In this way, the negative electrode active material particles (silicon-based active material particles) were modified. Negative electrode active material particles were produced by the above-described process. The negative electrode active material particles had a Li content of 10.0 mass %, a carbon coverage of 3 mass %, and a median diameter (volume basis, D50) of 9.0 μm.

[0166] XRD measurement of the obtained negative electrode active material particles, 29 Si-NMR measurement, Raman spectroscopic analysis, particle size distribution measurement, and XAFS analysis were carried out.

[0167] The XAFS (X-ray absorption fine structure) measurement conditions are as follows: Measurement facility: Aichi Synchrotron Light Center Acceleration energy: 1.2 GeV Accumulation current value: 300 mA Monochromatization conditions: White X-rays from a bending magnet are monochromatized using a double crystal monochromator and used for measurement Focusing conditions: Focusing in the vertical and horizontal directions using a Ni-coated bend cylindrical mirror Upstream slit opening: 7.0 mm horizontal x 3.0 mm vertical Beam size: 2.0 mm horizontal x 1.0 mm vertical Angle of incidence on the sample: Normal incidence (incident angle 0 degrees) Energy calibration: K 2 SO 4 The peak position at the S-K edge of is calibrated to 2481.70 eV. Measurement method: Total electron yield method by measuring the sample current. 0 Measurement method: Au-mesh during XANES (X-ray absorption near edge structure) measurement; Al-mesh during EXAFS (extended X-ray absorption fine structure) measurement. Sample environment: Transported without exposure to air using a transfer vessel. Vacuum degree: 5 x 10 -7 Pa

[0168] As a result of the XAFS measurement, the negative electrode active material particles have Si on their surfaces. 0~+4 It contained ingredients.

[0169] The silicon-based active material prepared as described above was mixed with a carbon-based active material in a mass ratio of 2:8 to prepare a negative electrode active material. The carbon-based active material used was a mixture of pitch-coated natural graphite and artificial graphite in a mass ratio of 5:5. The median diameter of the carbon-based active material was 20 μm.

[0170] Next, the prepared negative electrode active material, conductive additive 1 (carbon nanotubes, CNT), conductive additive 2 (carbon fine particles with a median diameter of approximately 50 nm), styrene butadiene rubber (styrene butadiene copolymer, hereinafter referred to as SBR), and carboxymethyl cellulose (hereinafter referred to as CMC) were mixed in a dry mass ratio of 92.5:1:1:2.5:3, and then diluted with pure water to form a negative electrode mixture slurry. The above SBR and CMC are negative electrode binders (negative electrode binders). Here, in order to measure the stability of the negative electrode mixture slurry, 10 g of a portion of the prepared negative electrode mixture slurry was taken separately from that used for preparing the secondary battery, sealed in an aluminum laminate pack, and stored at 40 ° C. The volume after 5 days was measured by the Archimedes method. The calculation method for the value in the column for gas generation amount in Table 1 is as follows. The volume [cc] immediately after sealing in the aluminum laminate pack was used as a reference value, and the reference value was subtracted from the volume value [cc] after 5 days, and the obtained value was divided by the slurry weight of 10 g to obtain the amount of gas generated [cc / g].

[0171] The negative electrode current collector was made of electrolytic copper foil (thickness: 15 μm). Finally, the negative electrode mixture slurry was applied to the negative electrode current collector and dried at 100°C for 1 hour in a vacuum atmosphere. After drying, the deposition amount of the negative electrode active material layer per unit area on one side of the negative electrode (also referred to as area density) was 5 mg / cm. 2 It was.

[0172] Next, fluoroethylene carbonate (FEC), ethylene carbonate (EC), and diethyl carbonate (DEC) were mixed as a solvent, and then an electrolyte salt (lithium hexafluorophosphate: LiPF 6An electrolyte solution was prepared by dissolving the above-mentioned compounds in a solvent with a volume ratio of FEC:EC:DEC=1:2:7, and the content of the electrolyte salt relative to the solvent was 1.0 mol / kg. Furthermore, 1.5% by mass of vinylene carbonate (VC) was added to the obtained electrolyte solution.

[0173] Next, a secondary battery was assembled as follows. First, an aluminum lead was ultrasonically welded to one end of the positive electrode current collector, and a nickel lead was welded to the negative electrode current collector. Next, the positive electrode, separator, negative electrode, and separator were stacked in this order and wound longitudinally to obtain a wound electrode assembly. The end of the winding was secured with PET protective tape. The separator was a 12 μm laminated film sandwiched between a film primarily composed of porous polypropylene and a film primarily composed of porous polyethylene. Next, the electrode assembly was sandwiched between exterior components, and the outer edges, excluding one side, were heat-sealed to encase the electrode assembly inside. The exterior component was an aluminum laminate film laminated with nylon film, aluminum foil, and polypropylene film. Next, the prepared electrolyte was injected through the opening, impregnated under a vacuum atmosphere, and then heat-sealed to seal.

[0174] The cycle characteristics and initial charge / discharge characteristics of the secondary battery fabricated as described above were evaluated.

[0175] The cycle characteristics were investigated as follows. First, to stabilize the battery, two cycles of charge and discharge were performed at 0.2 C in an atmosphere of 25°C, and the discharge capacity at the second cycle was measured. Next, charge and discharge were performed until the total number of cycles reached 499, and the discharge capacity was measured each time. Finally, the discharge capacity at the 500th cycle obtained by 0.2 C charge and discharge was divided by the discharge capacity at the second cycle to calculate the capacity retention rate (hereinafter also simply referred to as retention rate). For normal cycles, i.e., from the third cycle to the 499th cycle, charge and discharge were performed at 0.7 C and 0.5 C, respectively.

[0176] When investigating the initial charge-discharge characteristics, the initial efficiency (hereinafter sometimes referred to as initial efficiency) was calculated. The initial efficiency was calculated using the formula: initial efficiency (%) = (initial discharge capacity / initial charge capacity) × 100. The ambient temperature was the same as when investigating the cycle characteristics. The initial efficiency was calculated based on the discharge capacity up to 1.2 V.

[0177] (Examples 1-2 to 1-4, Comparative Example 1-1) As shown in Table 1, the modified SiO x A secondary battery was fabricated under the same conditions as in Example 1-1, except that the surface of Example 1-1 was adjusted, and evaluations were performed. For Example 1-2, the order of coating the carbon material (carbon) and ionic substance in Example 1-1 was changed, for Example 1-3, Al, a Group 13 element of the periodic table, was further added to the cation component of Example 1-1, and for Example 1-4, Al, a Group 13 element of the periodic table, was further added to the cation component of Example 1-1, and F, a Group 17 element of the periodic table, was further added to the anion component. For Comparative Example 1-1, only the carbon material (carbon) was coated, and no ionic substance was coated.

[0178] As shown in Table 1, SiO x In the silicon-based oxide represented by the formula (I), the surface is a two-layer structure consisting of a carbon material (carbon) and an ionic substance, which significantly suppresses the amount of gas generated on day 5 even at a high temperature of 40°C, resulting in excellent results. The surface layer was composed of either a first layer on the material side (silicon compound particle side) and an outer second layer, each consisting of carbon and an ionic substance, or an ionic substance and carbon. Such a surface layer structure can suppress Li ions eluting from the silicon-based oxide when the aqueous slurry is made, thereby suppressing gas generation even at a high temperature of 40°C. On the other hand, when the ionic substance was not included, the amount of gas generated during storage of the aqueous slurry at 40°C became significant, as shown in Comparative Example 1-1.

[0179] (Examples 2-1 to 2-4, Comparative Examples 2-1 to 2-3) The amount of carbon coating was adjusted as shown in Table 2. This adjustment was performed by adjusting the CVD conditions during carbon coating formation. Secondary batteries were also fabricated under the same conditions as in Example 1-1, and each evaluation was performed, and the results are shown in Table 2.

[0180] When the carbon coating amount was 0.2% by mass, a decrease in battery characteristics was observed. This is thought to be due to the fact that the small carbon coating amount makes it difficult to establish a conductive path during charging and discharging. When the carbon coating amount is greater than 0.2% by mass, the amount of gas generated during storage of the aqueous slurry can be suppressed. On the other hand, when the carbon coating amount is greater than 10% by mass, there is no problem with the battery characteristics, but the capacity per unit weight decreases, thereby compromising the benefits of the silicon-based active material.

[0181] [Examples 3-1 to 3-4, Comparative Examples 3-1 to 3-3] As shown in Table 3, secondary batteries were produced under the same conditions as in Example 1-2, except that the carbon coating amount was adjusted and the intensity ratio Id / Ig of the D band peak and the G band peak obtained by Raman spectroscopy was adjusted. Each evaluation was performed and shown in Table 3.

[0182] When the carbon coating amount was 0.2% by mass, a decrease in battery characteristics was observed. This is thought to be due to the fact that the small carbon coating amount makes it difficult to establish a conductive path during charging and discharging. When the carbon coating amount is more than 0.2% by mass, the amount of gas generated during storage of the aqueous slurry can be suppressed. When the carbon coating amount is more than 10% by mass, the amount of gas generated during storage of the aqueous slurry deteriorated.

[0183] (Examples 4-1 to 4-8) Negative electrode active material particles were produced in the same manner as in Example 1-1, except that the amount of ionic components was adjusted as shown in Table 4. The amount of ionic components can be adjusted by adjusting the blending amount of the target ion source. In addition, secondary batteries were produced under the same conditions as in Example 1-1, and various evaluations were performed, and the results are shown in Table 4.

[0184] When the ionic component is 0.3% by mass or more, the amount of gas generated during storage of the aqueous slurry at 40° C. can be sufficiently suppressed. On the other hand, when the ionic component is present in an amount of 10% by mass or less, an increase in the amount of gas generated during storage of the aqueous slurry at 40° C. is suppressed. This is thought to be because such a coating amount can suppress the ionic component from extracting the alkaline component from the inside of the silicon-based compound particles.

[0185] (Examples 5-1 to 5-9) Negative electrode active material particles were prepared in the same manner as in Example 1-1, except that the intensity ratio Id / Ig of the D band peak to the G band peak obtained by Raman spectroscopy was adjusted as shown in Table 5. This intensity ratio Id / Ig can be adjusted by adjusting the thermal CVD conditions (gas type, pressure, temperature, time, etc.). In addition, secondary batteries were prepared under the same conditions as in Example 1-1, and various evaluations were performed, and the results are shown in Table 5.

[0186] If the intensity ratio Id / Ig is 0.5 or higher, the sp2 carbon, which is the G-band peak component, is adequate, and the battery can follow the expansion and contraction of the silicon-based oxide during charge and discharge, resulting in good battery characteristics after long-term cycling. On the other hand, if the intensity ratio Id / Ig is 2.0 or lower, the progression of side reactions on the carbon surface is suppressed, and this does not lead to a decrease in the initial efficiency.

[0187] (Examples 6-1 to 6-6) Negative electrode active material particles were produced in the same manner as in Example 1-1, except that the specific surface area of ​​the negative electrode active material particles was adjusted as shown in Table 6. The specific surface area of ​​the negative electrode active material particles can be adjusted by adjusting the thermal CVD conditions (gas type, pressure, temperature, time, etc.). In addition, secondary batteries were produced under the same conditions as in Example 1-1, and various evaluations were performed, and the results are shown in Table 6.

[0188] Specific surface area is 0.3m 2 / g or more, the amount of gas generated during storage of the aqueous slurry at 40°C is suppressed, and good battery characteristics can be obtained. 2 When the specific surface area was 5.0 m / g or less, the amount of gas generated during storage of the aqueous slurry at 40°C was suppressed, and the battery characteristics were also sufficiently good. 2 / g or less, the binder is not used in excess on the particle surface, and can be uniformly applied to the entire particle, which is thought to result in good slurry properties and battery properties.

[0189] (Examples 7-1 to 7-7) As shown in Table 7, the Li of the negative electrode active material particles 2 SiO 3 Negative electrode active material particles were prepared in the same manner as in Example 1-1, except that the crystallite size calculated from the Si-derived peak and the crystallite size calculated from the Si-derived peak were adjusted. This adjustment can be performed by adjusting the temperature during heat treatment. In addition, secondary batteries were prepared under the same conditions as in Example 1-1, and various evaluations were performed, and the results are shown in Table 7.

[0190] Li 2 SiO 3 When the crystallite size calculated from the Li-derived peak was 3 nm or more and the crystallite size calculated from the Si-derived peak was 0.5 nm or more, both the amount of gas generated during storage of the aqueous slurry at 40°C and the battery characteristics were particularly good. 2 SiO 3 When the crystallite size calculated from the Si-derived peak is 3 nm or more, it is considered that Li is stabilized and its elution into water is suppressed, and as a result, the amount of gas generated during storage of the aqueous slurry at 40 ° C. is suppressed. At this time, the crystallite size calculated from the Si-derived peak is about 0.5 nm. 2 SiO 3 When the crystallite size calculated from the Si-derived peak is 10 nm or less, the crystallite size calculated from the Si-derived peak is kept small, at 5 nm or less, and the charge / discharge cycle characteristics of the battery when made into the battery are good.

[0191] (Examples 8-1 to 8-8) Negative electrode active material particles were prepared in the same manner as in Example 1-1, except that the median diameter of the silicon-based compound particles was adjusted as shown in Table 8. Secondary batteries were also prepared under the same conditions as in Example 1-1, and the results are shown in Table 8.

[0192] When the median diameter of the silicon-based compound particles is 0.5 μm or more, both the amount of gas generated during storage of the aqueous slurry at 40° C. and the battery characteristics are good. On the other hand, when the median diameter is 20 μm or less, the particles are less likely to crack during charging, and a solid electrolyte interface (SEI) due to newly formed surfaces is less likely to form during charging and discharging, thereby suppressing reversible Li loss. Furthermore, when the median diameter of the silicon compound particles is 20 μm or less, the amount of expansion of the silicon compound particles during charging does not become too large, preventing physical and electrical breakdown of the negative electrode active material layer due to expansion.

[0193] (Examples 9-1 to 9-13) Negative electrode active material particles were prepared in the same manner as in Example 1-1, except that the constituent elements of the ionic component were adjusted as shown in Table 9. At this time, the adjustment was made by selecting the ion source to be supplied during the treatment with the ionic component. In addition, secondary batteries were prepared under the same conditions as in Example 1-1, and various evaluations were performed, and the results are shown in Table 9.

[0194] When the anion element was phosphorus or phosphorus and F, i.e., the anion substance was phosphoric acid or F, both the amount of gas generated during storage of the aqueous slurry at 40°C and the battery characteristics were good. In this case, the cation element can be selected from Li, Al, Na, K, Ca, Mg, and Zr.

[0195] (Examples 10-1 to 10-5) As shown in Table 10, negative electrode active materials were prepared in the same manner as in Example 1-2, except that the constituent elements of the ionic component were adjusted. In addition, secondary batteries were prepared under the same conditions as in Example 1-1, and various evaluations were performed, and the results are shown in Table 10. Secondary batteries were prepared under the same conditions as in Example 1-1, and various evaluations were performed. The components of the first layer and the second layer can be changed by changing the treatment order. The adjustment was made by selecting the ion source supplied during treatment with the ionic component.

[0196] When the anion element was phosphorus or phosphorus and F, i.e., the anion substance was phosphoric acid or F, both the amount of gas generated during storage of the aqueous slurry at 40°C and the battery characteristics were good. In this case, the cation element can be selected from Li, Al, and Na.

[0197] (Examples 11-1 to 11-5) Negative electrode active material particles were prepared in the same manner as in Example 1-1, except that the constituent elements of the ionic component were adjusted as shown in Table 11. The adjustment was made by selecting the ion source supplied during treatment with the ionic component. In addition, secondary batteries were prepared under the same conditions as in Example 1-1, and various evaluations were performed, and the results are shown in Table 11.

[0198] When the anion element was carbon or carbon and F, i.e., the anion substance was carbonate or F, both the amount of gas generated during storage of the aqueous slurry at 40°C and the battery characteristics were good. In this case, the cation element can be selected from Li, Al, and Na.

[0199] (Examples 12-1 to 12-10) As shown in Table 12, negative electrode active materials were prepared in the same manner as in Example 1-2, except that the constituent elements of the ionic component were adjusted. The components of the first and second layers could be changed by changing the treatment order. The adjustment was made by selecting the ion source supplied during the treatment with the ionic component. In addition, secondary batteries were prepared under the same conditions as in Example 1-1, and various evaluations were performed, and the results are shown in Table 12.

[0200] When the anion element was carbon, boron, or carbon and fluorine, i.e., the anion substance was carbonic acid, boric acid, bisoxalatoboric acid, or F, both the amount of gas generated during storage of the aqueous slurry at 40°C and the battery characteristics were good. In this case, Li, Al, or Na can be selected as the cationic element.

[0201] (Examples 13-1 to 13-6) Negative electrode active material particles were prepared in the same manner as in Example 1-1, except that the constituent elements of the ionic component were adjusted as shown in Table 13. The adjustment was made by selecting the ion source supplied during treatment with the ionic component. In addition, secondary batteries were prepared under the same conditions as in Example 1-1, and various evaluations were performed, and the results are shown in Table 13.

[0202] When the cation component was Li or Li and Al, both the amount of gas generated during storage of the aqueous slurry at 40° C. and the battery characteristics were good. The anion substance in this case can be selected from boric acid, carbonate, silicic acid, fluoride ion, titanic acid, and niobic acid.

[0203] (Examples 14-1 to 14-8) As shown in Table 14, negative electrode active materials were prepared in the same manner as in Example 1-1, except that the constituent elements of the ion component were adjusted and the type of carbon precursor was changed. Furthermore, this carbon precursor can be formed by pyrolysis CVD treatment under conditions in which Si in the silicon compound particles, Li or Al among the elements constituting the cation, or Al or Si among the elements constituting the anion, are present on the outermost surface. The type of carbon precursor (whether a fibrous carbon compound or a carbon nanotube) can be changed by changing the element present on the outermost surface. Secondary batteries were prepared using these negative electrode active materials under the same conditions as in Example 1-1, and the evaluations were performed, as shown in Table 14.

[0204] The negative electrode active material of the present invention may have a fibrous carbon compound or carbon nanotubes on the surface, which actually improves the conductivity of the silicon compound particle surface, resulting in improved battery characteristics.

[0205] The present specification includes the following aspects: [1]: A negative electrode active material particle is included, and the negative electrode active material particle is a silicon compound (SiO x : 0.5≦x≦1.6), wherein XAFS analysis reveals that Si is present on the surface. 0~+4components, the negative electrode active material particles contain a carbon material and an ionic material as constituent materials, the negative electrode active material particles are at least partially coated with the carbon material, and have a structure in which the silicon compound particles and at least a portion of the carbon material are coated with the ionic material, or the negative electrode active material particles are at least partially coated with the ionic material, and have a structure in which the silicon compound particles and at least a portion of the ionic material are coated with the carbon material, the amount of the carbon material coated is 0.3 mass % or more and 10 mass % or less with respect to the total of the silicon compound particles and the coating layer of the carbon material, and the cation of the ionic material is composed of an ion containing at least one element selected from Group 1 elements, Group 2 elements, Group 4 elements and Group 13 elements of the periodic table, a negative electrode active material for a non-aqueous electrolyte secondary battery, wherein the anion of the ionic substance is an ion of an oxide containing at least one element selected from Groups 4, 5, 13, 14, and 15 of the Periodic Table, or an ion of a halide containing at least one element selected from Group 17 of the Periodic Table; [2]: The negative electrode active material for a non-aqueous electrolyte secondary battery according to [1] above, wherein the coating amount of the ionic substance is 0.5% by mass or more and 10% by mass or less based on the total of the silicon compound particles and the carbon coating layer; [3]: The negative electrode active material for a non-aqueous electrolyte secondary battery according to [1] or [2] above, wherein the intensity ratio Id / Ig of the D band to the G band measured by Raman spectroscopy analysis of the negative electrode active material is 0.5≦Id / Ig≦2.0; [4]: The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to [3], wherein the intensity ratio ISi / Ig of the Si peak intensity to the G band in Raman spectroscopic analysis of the negative electrode active material is 0≦ISi / Ig≦2.0. [5]: The negative electrode active material particles have a specific surface area of ​​0.3 m 2 / g or more 5.0m 2 [6]: The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to [4], wherein the Li 2 SiO 3The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to [5] above, wherein the crystallite size calculated by the Scherrer equation from a peak at around 2θ = 18.7° due to a peak is 3 nm or more and 10 nm or less. [7]: The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to [6] above, wherein the crystallite size due to a Si (220) crystal plane obtained by X-ray diffraction of the negative electrode active material is 0.5 nm or more and 5 nm or less. [8]: The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to [7] above, wherein the silicon compound particles have a median diameter of 0.5 μm or more and 20 μm or less. [9]: The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to [8] above, wherein the Group 1 element of the Periodic Table of the cation is Li, Na, or K, the Group 2 element of the Periodic Table of the cation is Mg or Ca, the Group 4 element of the Periodic Table of the cation is Zr, or the Group 13 element of the Periodic Table of the cation is Al.

[10] : The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to [9] above, wherein the Group 4 element of the Periodic Table of the oxide constituting the anion is Ti, the Group 5 element of the Periodic Table of the oxide constituting the anion is Nb, the Group 13 element of the Periodic Table of the oxide constituting the anion is B or Al, the Group 14 element of the Periodic Table of the oxide constituting the anion is C or Si, the Group 15 element of the Periodic Table of the oxide constituting the anion is P, or the Group 17 element of the Periodic Table of the halide constituting the anion is F.

[11] : The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to

[10] above, wherein a carbon precursor is present, the carbon precursor originating from Si in the silicon compound particles, Li or Al among the elements constituting the cation, or Al or Si among the elements constituting the anion.

[12] : The negative electrode active material for a non-aqueous electrolyte secondary battery according to

[12] above, wherein the carbon precursor is a fibrous carbon compound or a carbon nanotube.

[13] : A slurry composition for a non-aqueous electrolyte secondary battery, comprising the negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to

[12] above.

[14] : A non-aqueous electrolyte secondary battery, comprising the negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of [1] to

[12] above.

[15] : A mobile terminal comprising the nonaqueous electrolyte secondary battery of

[14] above.

[16] : An electric rickshaw comprising the nonaqueous electrolyte secondary battery of

[14] above.

[17] : A power storage system comprising the nonaqueous electrolyte secondary battery of

[14] above.

[18] : A silicon compound (SiO. x a step of coating the silicon compound particles with a carbon material; and a step of inserting Li into the silicon compound particles, the method comprising the steps of preparing negative electrode active material particles having the silicon compound particles and the carbon material, and producing a negative electrode active material for a non-aqueous electrolyte secondary battery comprising the negative electrode active material particles, the method comprising the steps of: forming a coating of an ionic substance on the surfaces of the silicon compound particles, the cations of which are ions containing at least one element selected from Group 1 elements, Group 2 elements, Group 4 elements, and Group 13 elements of the periodic table, and the anions of which are ions of an oxide containing at least one element selected from Group 4 elements, Group 5 elements, Group 13 elements, Group 14 elements, and Group 15 elements of the periodic table, or ions of a halide containing at least one element selected from Group 17 elements of the periodic table, before the step of coating the carbon material. and forming a coating of an ionic substance on at least one surface of the silicon compound particles and the carbon material, the cations being ions containing at least one element selected from Group 1, 2, 4, and 13 elements of the periodic table, and the anions being ions of an oxide containing at least one element selected from Group 4, 5, 13, 14, and 15 elements of the periodic table, or ions of a halide containing at least one element selected from Group 17 elements of the periodic table, after the step of coating the silicon compound particles and the carbon material, the method comprising producing the negative electrode active material particles so that the amount of the carbon material coating is 0.3 mass % or more and 10 mass % or less of the total of the silicon compound particles and the coating layer of the carbon material.

[0206] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

Claims

1. A negative electrode active material particle is provided, and the negative electrode active material particle is a silicon compound (SiO x : 0.5≦x≦1.6), wherein the surface of the silicon compound particles is found to have Si 0~+4 components, the negative electrode active material particles contain a carbon material and an ionic material as constituent materials, the negative electrode active material particles are at least partially coated with the carbon material, and have a structure in which the silicon compound particles and at least a portion of the carbon material are coated with the ionic material, or the negative electrode active material particles are at least partially coated with the ionic material, and have a structure in which the silicon compound particles and at least a portion of the ionic material are coated with the carbon material, the amount of the carbon material coated is 0.3 mass % or more and 10 mass % or less with respect to the total of the silicon compound particles and the coating layer of the carbon material, and a cation of the ionic material is composed of an ion containing at least one element selected from Group 1 elements, Group 2 elements, Group 4 elements, and Group 13 elements of the periodic table, a negative electrode active material for a nonaqueous electrolyte secondary battery, wherein the anion of the ionic substance is an ion of an oxide containing at least one element selected from the group consisting of elements in groups 4, 5, 13, 14, and 15 of the periodic table, or an ion of a halide containing at least one element selected from elements in group 17 of the periodic table.

2. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that the amount of the ionic substance coated is 0.5 mass % or more and 10 mass % or less based on the total amount of the silicon compound particles and the carbon coating layer.

3. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that the intensity ratio Id / Ig of D band to G band in Raman spectroscopic analysis of said negative electrode active material is 0.5≦Id / Ig≦2.

0.

4. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that the intensity ratio ISi / Ig of the Si peak intensity to the G band by Raman spectroscopy of the negative electrode active material satisfies 0≦ISi / Ig≦2.

0.

5. The negative electrode active material particles have a specific surface area of ​​0.3 m 2 / g or more 5.0m 2 2. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the molecular weight of the negative electrode active material is 1 / g or less.

6. Li obtained by X-ray diffraction of the negative electrode active material 2 SiO 3 2. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the crystallite size calculated from a peak at about 2θ=18.7° by Scherrer's formula is 3 nm or more and 10 nm or less.

7. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that the crystallite size due to the Si (220) crystal plane obtained by X-ray diffraction of the negative electrode active material is 0.5 nm or more and 5 nm or less.

8. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that the median diameter of the silicon compound particles is 0.5 μm or more and 20 μm or less.

9. The negative electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, characterized in that the Group 1 element of the periodic table constituting the cation is Li, Na or K, the Group 2 element of the periodic table constituting the cation is Mg or Ca, the Group 4 element of the periodic table constituting the cation is Zr, or the Group 13 element of the periodic table constituting the cation is Al.

10. The negative electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, characterized in that a Group 4 element of the periodic table of the oxide constituting the anion is Ti; a Group 5 element of the periodic table of the oxide constituting the anion is Nb; a Group 13 element of the periodic table of the oxide constituting the anion is B or Al; a Group 14 element of the periodic table of the oxide constituting the anion is C or Si; a Group 15 element of the periodic table of the oxide constituting the anion is P; or a Group 17 element of the periodic table of the halide constituting the anion is F.

11. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that a carbon precursor is present, the carbon precursor originating from Si in the silicon compound particles, Li or Al among the elements constituting the cation, or Al or Si among the elements constituting the anion.

12. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 11, wherein the carbon material is a fibrous carbon compound or a carbon nanotube.

13. A slurry composition for a non-aqueous electrolyte secondary battery, comprising the negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1.

14. A non-aqueous electrolyte secondary battery comprising the negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 12.

15. A mobile terminal comprising the nonaqueous electrolyte secondary battery according to claim 14.

16. An electric power vehicle comprising the nonaqueous electrolyte secondary battery according to claim 14.

17. A power storage system comprising the nonaqueous electrolyte secondary battery according to claim 14.

18. Silicon compounds (SiO xa step of preparing a negative electrode active material particle having the silicon compound particle and the carbon material, and a step of producing a negative electrode active material for a non-aqueous electrolyte secondary battery comprising the negative electrode active material particle, the method comprising the steps of: preparing silicon compound particles containing a silicon compound having a cation ion containing at least one element selected from Groups 1, 2, 4 and 13 of the periodic table, and anion ions of an oxide containing at least one element selected from Groups 4, 5, 13, 14 and 15 of the periodic table, or ions of a halide containing at least one element selected from Group 17 of the periodic table, before the step of coating with the carbon material, forming a coating of an ionic material on the surface of the silicon compound particle. and forming a coating of an ionic substance on at least one surface of the silicon compound particles and the carbon material, the cations being ions containing at least one element selected from Groups 1, 2, 4, and 13 of the periodic table, and the anions being ions of an oxide containing at least one element selected from Groups 4, 5, 13, 14, and 15 of the periodic table, or ions of a halide containing at least one element selected from Group 17 of the periodic table, after the step of coating the silicon compound particles and the carbon material, the method comprising producing the negative electrode active material particles such that the amount of the carbon material coating is 0.3 mass % or more and 10 mass % or less with respect to the total amount of the silicon compound particles and the coating layer of the carbon material.

Citation Information

Patent Citations

  • Silicon-based negative electrode material and preparation method and application thereof

    CN113381021A

  • Negative electrode material for non-aqueous electrolyte secondary battery, method of manufacturing the same, and lithium-ion secondary battery

    JP2011096455A

  • Negative electrode active material for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, method for manufacturing negative electrode material for nonaqueous electrolyte secondary battery, and method for manufacturing nonaqueous electrolyte secondary battery

    JP2017073302A

  • Negative electrode active material, mixture negative electrode active material, water type negative electrode slurry composition, and manufacturing method of the negative electrode active material

    JP2020077510A

  • Negative electrode for non-aqueous electrolyte secondary battery and method for manufacturing the same