Fiber, cement, cement paste, mortar, and concrete containing said fiber, and method for producing fiber
Incorporating EVOH fibers with a non-circular cross-section into cement pastes enables self-healing of cracks in hardened cement by promoting calcium carbonate precipitation, addressing the durability issues of existing cement materials.
Patent Information
- Application Number
- PCT/JP2024/019800
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-30
- Publication Date
- 2024-12-05
AI Technical Summary
Existing cement-based materials lack effective self-healing mechanisms for cracks that form in hardened cement bodies, leading to reduced durability and maintenance challenges.
Incorporating fibers with a non-circular cross-section and protrusions, made from ethylene-vinyl alcohol copolymer (EVOH) or phosphorylated EVOH, into cement pastes to promote self-healing by facilitating the precipitation of calcium carbonate at crack sites, thereby sealing cracks.
The EVOH fibers enhance the self-healing capability of cement-based materials by effectively precipitating calcium carbonate around the fibers, reducing crack width and promoting rapid closure of cracks without compromising the mechanical strength of the hardened cement body.
Smart Images

Figure JP2024019800_05122024_PF_FP_ABST
Abstract
Description
Fibers, cement, cement paste, mortar, and concrete containing the fibers, and methods for producing the fibers
[0001] The present invention relates to fibers, cements, cement pastes, mortars, and concretes containing the fibers, and methods for producing the fibers.
[0002] In order to promote the self-healing of cracks that occur in hardened cement paste, a technique has been proposed in which synthetic fibers having a non-circular cross section with two or more protrusions and at least a portion of the fiber surface being made of one or more resins selected from the group consisting of polyolefin resins and polyacetal resins are mixed into cement (see Patent Document 1 below).
[0003] Ethylene-vinyl alcohol copolymer (hereinafter, sometimes abbreviated as "EVOH") is a polymer that is widely used as a gas barrier material, but its applications are not limited to this. Attempts have been made to apply EVOH as a material for cooling fibers and fibers for alkaline secondary battery separators (see Patent Documents 2 and 3 listed below).
[0004] JP 2014-1129 A JP 2010-189829 A JP 2007-154402 A
[0005] The present invention provides a novel fiber that, when added to a cement paste, can promote self-healing of cracks that occur in a hardened cement body obtained from the cement paste.
[0006] The present invention includes the following aspects: [1] A fiber containing an ethylene-vinyl alcohol copolymer containing a structural unit represented by the following formula (1): [2] A fiber containing a phosphorylated ethylene-vinyl alcohol copolymer. [3] The fiber according to [1] or [2], wherein the amount of phosphorus contained per 1 g of the fiber, as measured by the molybdenum blue method, is 0.001 mg or more and 10 mg or less. [4] The fiber according to [1] or [2], wherein the amount of phosphorus contained per 1 g of the fiber, as measured by the molybdenum blue method, is 0.01 mg or more and 1 mg or less. [5] The fiber according to any one of [1] to [4], wherein the fiber length is 1 mm or more and 200 mm or less, preferably 5 mm or more and 100 mm or less. [6] The fiber according to any one of [1] to [4], wherein the fiber length is 10 mm or more and 60 mm or less. [7] A method for producing a fiber suitable as an additive to cement paste, the method comprising phosphorylating the unphosphorylated ethylene-vinyl alcohol copolymer contained in precursor fibers formed using the unphosphorylated ethylene-vinyl alcohol copolymer. [8] The method according to [7], further comprising cutting the precursor fibers to a fiber length of 1 mm or more and 200 mm or less, preferably 5 mm or more and 100 mm or less, and more preferably 10 mm or more and 60 mm or less, prior to phosphorylation of the unphosphorylated ethylene-vinyl alcohol copolymer. [9] A method for producing fibers suitable for use as an additive in cement paste, comprising cutting continuous fibers formed using a phosphorylated ethylene-vinyl alcohol copolymer to a fiber length of 1 mm or more and 200 mm or less, preferably 5 mm or more and 100 mm or less, and more preferably 10 mm or more and 60 mm or less.
[10] The method according to any of [7] to [9], wherein the fibers contain an ethylene-vinyl alcohol copolymer containing a structural unit of the following formula (1):
[11] The method according to any one of [7] to
[10] , wherein the amount of phosphorus contained per gram of the fiber, as measured by the molybdenum blue method, is 0.001 mg to 10 mg, and may be 0.01 mg-mol to 1 mg-mol.
[12] Fibers produced by the method according to any one of [7] to
[11] .
[13] Use of the fiber according to any one of [1] to [6] and
[12] as an additive to cement paste.
[14] Use of the fiber according to any one of [1] to [6] and
[12] as an agent for promoting self-healing of cracks in hardened cement paste.
[15] A cement composition comprising powdered cement and the fiber according to any one of [1] to [6] and
[12] .
[16] The cement composition according to
[15] , further comprising aggregate.
[17] A cement paste comprising the fiber according to any one of [1] to [6] and
[12] , cement, and water.
[18] Mortar comprising the cement paste according to
[17] and aggregate.
[19] Concrete containing the cement paste according to
[17] and aggregate.
[20] A hardened cement product obtained from the cement paste according to
[17] .
[0007] According to one embodiment of the present invention, there is provided a novel fiber that, when added to a cement paste, can promote self-healing of cracks that occur in a hardened cement body obtained from the cement paste.
[0008] The present invention will be described below based on examples of embodiments for carrying out the present invention, but the present invention is not limited to the embodiments described below.
[0009] Furthermore, in the present invention, when expressed as "X to Y" (X and Y are arbitrary numbers), it means "X or more and Y or less" unless otherwise specified. With regard to the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range in one stage can be arbitrarily combined with the upper limit or lower limit of a numerical range in another stage. Furthermore, in the numerical ranges described in this specification, the upper limit or lower limit of the numerical range can also be replaced with the value shown in the examples.
[0010] A fiber according to one embodiment of the present invention contains a structural unit of the following formula (1) in the EVOH forming the fiber.
[0011] In the fibers according to the present embodiment, the amount of phosphorus contained per gram of fiber, as measured by the molybdenum blue method, is preferably 0.001 mg to 10 mg, more preferably 0.005 mg to 5 mg, even more preferably 0.01 mg to 1 mg, and particularly preferably 0.05 mg to 0.5 mg. If the phosphorus content is equal to or greater than the lower limit, calcium ions tend to be more easily adsorbed onto the fiber surface, and the fiber tends to have an excellent ability to precipitate a self-healing substance such as calcium carbonate around the fiber. If the phosphorus content is equal to or less than the upper limit, the water solubility is not too high, and the fiber itself tends to be less likely to be eluted from the hardened cement paste.
[0012] The EVOH contained in the fiber according to the embodiment may be obtained by blending at least two types of EVOH having different phosphorus contents produced by different processes, one of which may be an EVOH that does not contain phosphorus.
[0013] <Unphosphorylated EVOH> The EVOH containing the structural unit of formula (1) contained in the fiber according to the embodiment can be obtained by phosphorylating unphosphorylated EVOH. Hereinafter, the unphosphorylated EVOH used in the production of the EVOH containing the structural unit of formula (1) contained in the fiber according to the embodiment may be referred to as EVOH (A). EVOH (A) is a thermoplastic polymer obtained by saponifying an ethylene-vinyl acetate copolymer, which is a copolymer of ethylene and vinyl acetate, and is water-insoluble.
[0014] The copolymerization of ethylene and vinyl acetate can be carried out by any known polymerization method, such as solution polymerization, suspension polymerization, emulsion polymerization, etc., and solution polymerization using methanol as a solvent is generally used. The resulting ethylene-vinyl acetate copolymer can also be saponified by a known method.
[0015] The EVOH (A) produced in this manner is mainly composed of ethylene units and vinyl alcohol units, and when the degree of saponification is less than 100 mol %, it contains a small amount of residual vinyl units.
[0016] The ethylene unit content of EVOH (A), measured according to ISO 14663, is usually 20 mol% to 60 mol%, preferably 20 mol% to 55 mol%, and more preferably 25 mol% to 50 mol%. When the content is equal to or greater than the lower limit, the thermal stability during fiber formation, particularly during melt spinning, tends to be excellent. Furthermore, when EVOH (A) having a content equal to or less than the upper limit is used, the fiber according to the embodiment tends to have an excellent ability to precipitate a self-healing substance such as calcium carbonate around the fiber. The ethylene unit content of EVOH (A) can be controlled by the ethylene pressure during copolymerization of vinyl acetate and ethylene.
[0017] The saponification degree of EVOH (A), measured in accordance with JIS K6726 (where EVOH (A) is a solution uniformly dissolved in a water / methanol solvent), is usually 90 mol% or more and 100 mol% or less, preferably 95 mol% or more and 100 mol% or less, and more preferably 99 mol% or more and 100 mol% or less. When the saponification degree is within the above range, the thermal stability during melt spinning tends to be excellent. The saponification degree can be controlled by the amount, temperature, time, etc. of a saponification catalyst (usually an alkaline catalyst such as sodium hydroxide is used) used when saponifying the ethylene-vinyl acetate copolymer.
[0018] The melt flow rate (MFR) (210°C, 2160 g load) of EVOH (A) is usually 0.1 g / 10 min or more and 300 g / 10 min or less, preferably 0.5 g / 10 min or more and 250 g / 10 min or less, and more preferably 1 g / 10 min or more and 200 g / 10 min or less. When the MFR is equal to or greater than the lower limit, the melt viscosity tends to be maintained at an appropriate level, which facilitates spinning. When the MFR is equal to or less than the upper limit, the tension during melt spinning tends to be maintained at an appropriate level, which facilitates stable melt spinning.
[0019] The MFR is an index of the degree of polymerization of EVOH (A), and can be adjusted by the amount of polymerization initiator and the amount of solvent used when copolymerizing ethylene and vinyl acetate.
[0020] EVOH (A) may further contain comonomer units derived from the comonomers shown below within a range that does not impair the effects of the present invention (for example, 10 mol % or less of EVOH (A)).
[0021] Examples of the comonomer include olefins such as propylene, 1-butene, and isobutene; hydroxy group-containing α-olefins such as 3-butene-1-ol, 3-butene-1,2-diol, 4-pentene-1-ol, and 5-hexene-1,2-diol, and derivatives thereof such as esters and acylation products; hydroxyalkylvinylidenes such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dipropionyloxy-2-methylenepropane; hydroxyalkylvinylidene diacetates such as 1,3-dibutyryloxy-2-methylenepropane, 1,3-dibutyryloxy-2-methylenepropane, etc.; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, (anhydrous) phthalic acid, (anhydrous) maleic acid, (anhydrous) itaconic acid, etc., or salts thereof or mono- or di-alkyl esters in which the alkyl group has 1 to 18 carbon atoms; acrylamide, N-alkylacrylamide in which the alkyl group has 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid, etc. acrylamides such as a salt thereof, acrylamidopropyldimethylamine or an acid salt or a quaternary salt thereof; methacrylamides such as methacrylamide, N-alkylmethacrylamides in which the alkyl group has 1 to 18 carbon atoms, N,N-dimethylmethacrylamide, 2-methacrylamidopropanesulfonic acid or a salt thereof, methacrylamidepropyldimethylamine or an acid salt or a quaternary salt thereof; N-vinylamides such as N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl ethers such as alkyl vinyl ethers, hydroxyalkyl vinyl ethers, and alkoxyalkyl vinyl ethers in which the alkyl group has 1 to 18 carbon atoms; halogenated vinyl compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, and vinyl bromide; vinyl silanes such as trimethoxyvinylsilane; halogenated allyl compounds such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol;Comonomers such as trimethyl-(3-acrylamido-3-dimethylpropyl)-ammonium chloride and acrylamido-2-methylpropanesulfonic acid can be used alone or in combination of two or more types.
[0022] The EVOH (A) may be post-modified as long as the effects of the present invention are not impaired. Examples of post-modification include urethanization, acetalization, cyanoethylation, and oxyalkylenation.
[0023] The EVOH (A) may be a mixture of two or more kinds of EVOH, for example, EVOHs having different degrees of saponification, different degrees of polymerization, or different copolymerization components.
[0024] <Method for producing fiber> There are two typical examples of methods for producing the fiber according to the embodiment using EVOH (A) as a starting material. <First method> A method comprising the steps of forming a precursor fiber using EVOH (A) and, after the step, phosphorylating the EVOH (A) contained in the precursor fiber to obtain the fiber according to the embodiment. <Second method> A method comprising the steps of phosphorylating EVOH (A) to produce phosphorylated EVOH and, after the step, forming the fiber according to the embodiment using the phosphorylated EVOH.
[0025] The first method will be described below by dividing it into a step of forming a precursor fiber using EVOH (A) and a step of phosphorylating EVOH (A) contained in the precursor fiber.
[0026] (Step of forming precursor fiber from EVOH (A)) The precursor fiber is formed by fiberizing EVOH (A) or a composition thereof.
[0027] The EVOH (A) composition is a composition in which one or more additives are blended with EVOH (A) within a range that does not impair the object of the present invention (for example, 5 parts by mass or less per 100 parts by mass of EVOH (A)). Examples of the additives include lubricants, inorganic salts (for example, hydrotalcite, etc.), plasticizers, heat stabilizers, light stabilizers, antioxidants, UV absorbers, colorants, antistatic agents, surfactants, antibacterial agents, antiblocking agents, slip agents, fillers (for example, inorganic fillers, etc.), and other resins (for example, polyolefins, polyamides, etc.).
[0028] The method for producing fibers from EVOH (A) or a composition thereof is not particularly limited, and examples thereof include melt spinning, wet spinning, and dry spinning. Among these, melt spinning is preferably used because of its high spinning speed and ease of spinning split fibers.
[0029] The melt spinning method is not particularly limited, but is carried out using a known melt spinning machine from a single nozzle or multiple nozzles. The spinning is carried out at a temperature at which EVOH (A) melts but does not deteriorate, and EVOH (A) is extruded at a spinning temperature of 200 to 320°C to produce spun filaments of a predetermined fineness.
[0030] (Step of Phosphorylating EVOH (A) Contained in Precursor Fiber) The EVOH (A) contained in the precursor fiber can be phosphorylated by utilizing a reaction conventionally used for producing a phosphate ester of an organic hydroxy compound. That is, by reacting the EVOH (A) contained in the precursor fiber with polyphosphoric acid, phosphorus oxychloride, or phosphorus pentoxide, some of the vinyl alcohol units contained in the EVOH (A) can be converted into the structural unit of formula (1).
[0031] The phosphorylation reaction is preferably carried out by bringing the precursor fiber into contact with a solution of the above-mentioned phosphorus compound (polyphosphoric acid, phosphorus oxychloride or phosphorus pentoxide) dissolved in a solvent that does not react with the phosphorus compound.
[0032] The content of the phosphorus compound relative to the solvent is usually 0.1% by mass or more, preferably 1.0% by mass or more, more preferably 5.0% by mass or more, even more preferably 7.0% by mass or more, and particularly preferably 9.0% by mass or more. The upper limit is usually 30% by mass or less, preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less. When the content of the phosphorus compound is within the above range, EVOH (A) can be phosphorylated.
[0033] In the second method, EVOH (A) is phosphorylated before fiber formation, thereby converting some of the hydroxyl groups of EVOH (A) into phosphate groups. Regarding the phosphorylation technique of EVOH (A) that can be used in the second method, the following literature can be referred to: "Influence of covalently bound phosphorus-containing groups on the flammability of poly(vinyl alcohol), poly(ethylene-co-vinyl alcohol) and low-density polyethylene," M. Banks et al., POLYMER, 34 (1993), pp. 4547-4556
[0034] In the second method, the fiber according to the embodiment is produced by fiberizing EVOH containing phosphorylated EVOH obtained using EVOH (A), or a composition thereof. The EVOH containing phosphorylated EVOH obtained using EVOH (A) may be a mixture of phosphorylated EVOH obtained using EVOH (A) and unphosphorylated EVOH.
[0035] <Characteristics of the fiber according to the embodiment> The fiber diameter of the fiber according to the embodiment is not particularly limited, but is usually 0.1 μm or more and 100 μm or less, preferably 0.1 μm or more and 50 μm or less, and more preferably 0.1 μm or more and 30 μm or less. When the fiber diameter is within the above range, the fiber surface area increases, and the ability to precipitate a self-healing substance per unit volume is improved. The fiber diameter here refers to the filament diameter. The same applies elsewhere in this specification, and fiber diameter refers to the filament diameter.
[0036] The fiber length of the fibers according to the present invention is not particularly limited, but is usually 1 mm to 200 mm, preferably 5 mm to 100 mm, and more preferably 10 mm to 60 mm. By keeping the fiber length within the above range, the mechanical strength of the hardened cement paste containing the fiber can be improved without making the cement paste containing the fiber difficult to handle. The fibers can be cut to lengths within the above range both before and after phosphorylation.
[0037] <Applications> The fibers according to the embodiment can be used as an additive to cement paste. Cement paste is made by adding water to cement and kneading it. Cement is a powdery composition, and typically contains quicklime, silica, alumina, iron oxide, magnesium oxide, and gypsum as components.
[0038] In the hardened cement body obtained from the cement paste to which the fibers according to the embodiment have been added, when cracks occur, a self-healing substance such as calcium carbonate is likely to precipitate in the cracks, so the cracks spontaneously close in a relatively short time. In other words, the fibers according to the embodiment act as a self-healing accelerator for cracks in the hardened cement body.
[0039] When the fibers according to the embodiment are added to a cement paste, the amount of the fibers may be 0.001 parts by mass or more, 0.005 parts by mass or more, 0.01 parts by mass or more, 0.05 parts by mass or more, 0.1 parts by mass or more, 0.5 parts by mass or more, 1 part by mass or more, or 1.5 parts by mass or more, or 60 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, 10 parts by mass or less, 5 parts by mass or less, 4 parts by mass or less, or 3 parts by mass or less, relative to 100 parts by mass of cement. Since this can promote self-healing of cracks in the hardened body obtained from the cement paste without significantly impairing the strength of the hardened body, the content of the fibers according to the embodiment is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 6 parts by mass, and even more preferably 1 to 4 parts by mass, relative to 100 parts by mass of cement.
[0040] Mortar can be obtained by kneading fine aggregate such as sand into cement paste to which the fibers according to the embodiment have been added. Alternatively, concrete can be obtained by kneading fine aggregate such as sand and coarse aggregate such as gravel into cement paste to which the fibers according to the embodiment have been added. Such hardened mortar or concrete has a structure in which the aggregates are bonded to each other by the hardened cement body containing the fibers according to the embodiment as a binder, so even if cracks occur, the cracks are closed in a relatively short time. This is because cracks also occur in the hardened cement body contained in the mortar or concrete.
[0041] In one example, a cement paste containing the fibers according to the embodiment is prepared by mixing cement, water, and the fibers immediately before use. In another example, a cement composition containing powdered cement and the fibers according to the embodiment is prepared in advance, and the cement paste is prepared by adding water to the cement composition as needed. In either example, the prepared cement paste can be further mixed with aggregate to obtain mortar or concrete.
[0042] In one example, a mortar containing a cement paste having fibers according to embodiments may be prepared by adding water to a cement composition containing powdered cement, fibers according to embodiments, and fine aggregate, and in one example, a concrete containing a cement paste having fibers according to embodiments may be prepared by adding water to a cement composition containing powdered cement, fibers according to embodiments, fine aggregate, and coarse aggregate, and in one example, a concrete containing a cement paste having fibers according to embodiments.
[0043] The cement composition containing the powdered cement and the fibers, fine aggregate, and coarse aggregate according to the embodiment may optionally contain one or more admixtures in addition to these components. Examples of admixtures include inorganic fine powder admixtures such as blast furnace slag, fly ash, and silica fume, water-reducing agents such as air-entraining agents, high-performance water-reducing agents, and high-performance air-entraining agents, air-entraining agents, foaming agents, expanding agents, and setting rate regulators.
[0044] The cement paste containing the fibers according to the embodiment, and the mortar and concrete using the cement paste can be used not only for manufacturing structures but also for repairing hardened concrete, specifically for filling cracks that have occurred in hardened concrete or for covering deteriorated surfaces of hardened concrete.
[0045] The results of the experiments conducted by the present inventors are described below.
[0046] Experiment 1: Preparation of EVOH Fiber. Hydrous EVOH pellets with an ethylene content of 38 mol%, an MFR of 50 g / 10 min (210°C, 2160 g load), and a saponification degree of 99.7 mol% were immersed in an aqueous solution containing 250 ppm sodium acetate, 260 ppm sodium dihydrogen phosphate, and 170 ppm acetic acid for 2.5 hours, rinsed with water, dried, and then used to form monofilament fibers by melt spinning. Observation with a scanning electron microscope (SEM) revealed that the diameter of the resulting fibers was approximately 27 μm.
[0047] [Preparation of Phosphorylated EVOH Fiber] The EVOH fiber obtained by the above procedure was cut to a fiber length of 51 mm and then phosphorylated as follows to prepare phosphorylated EVOH fiber. First, 40 mL of tributylamine and 13.5 g of polyphosphoric acid were dissolved in 100 mL of a mixed solvent (boiling point 90°C) consisting of acetonitrile and DMSO in a volume ratio of 7:3 (acetonitrile:DMSO). Next, 2 g of EVOH fiber was added to the solution, and the mixture was heated and stirred under reflux using a hot stage. The EVOH fiber was then removed from the reaction vessel and washed with distilled water to remove unreacted polyphosphoric acid, yielding phosphorylated EVOH fiber.
[0048] [Phosphorus Content] The amount of phosphorus contained in phosphorylated EVOH fiber was measured by the molybdenum blue method. An ascorbic acid solution was prepared by mixing 1.0 g of ascorbic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) with 5.0 mL of pure water and 5.0 mL of 4.5 M diluted sulfuric acid. A molybdic acid solution was also prepared by mixing 0.5 g of ammonium molybdate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 6.0 mL of pure water, 0.02 g of potassium antimonyl tartrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and 14 mL of 4.5 M diluted sulfuric acid. The prepared ascorbic acid solution and molybdic acid solution were added to 1 g of phosphorylated EVOH fiber and allowed to stand for 5 minutes to develop color. The absorbance at 883 nm was then measured using a spectrophotometer (U-1900, manufactured by Hitachi, Ltd.) to determine the amount of phosphoric acid (mg) per 1 g of EVOH fiber. The results are shown in Table 1 below.
[0049] [Evaluation of Self-Healing Properties of Hardened Cement Composition] Household cement (CCG1.3, manufactured by Sunhome Industries Co., Ltd.) and pure water were mixed in a mass ratio of 5:1 to obtain a cement paste. EVOH fiber was further added to 100 parts by mass of the cement paste composition to obtain a cement paste composition. The cement paste composition was then cured in pure water at 20°C for 7 days to obtain a hardened cement composition. Next, a crack approximately 60 to 70 μm wide was formed in the hardened body by striking it with a hammer, and the hardened body was then immersed in pure water and allowed to stand to examine the degree of self-healing of the crack. Specifically, the hardened body was removed from the water 3 and 7 days after immersion, and the area around the crack was observed with an optical microscope. The results are shown in Table 1. The symbols in Table 1 mean the following: ×: The crack is barely closed; △: The crack is partially closed; ○: The crack is completely closed.
[0050] [Evaluation of calcium carbonate adhesion] EVOH fibers exposed in cracks in the hardened cement composition used in the evaluation of self-healing properties were observed using a stereomicroscope, and it was visually confirmed whether calcium carbonate was attached to the fiber surface. The results are shown in Table 1. The symbols in Table 1 have the following meanings: ×: no adhesion ○: adhesion
[0051] <Experiment 2> Phosphorylated EVOH fiber was prepared in the same manner as in Experiment 1, except that phosphoryl chloride (POCl3) was used instead of polyphosphoric acid as the phosphating agent. Specifically, 16.4 g of sodium hydroxide was added to a reaction vessel containing 2 g of EVOH fiber and 200 mL of ion-exchanged water, and the mixture was stirred overnight at room temperature. After cooling the reaction solution so that the temperature did not exceed 20°C, 7.5 mL of phosphoryl chloride was added to the reaction vessel and stirred for 6 hours. The EVOH fiber was then removed from the reaction vessel and washed with distilled water to remove unreacted polyphosphoric acid, yielding phosphorylated EVOH fiber. Using the prepared phosphorylated EVOH fiber, the phosphorus content, the self-healing property of the hardened cement composition, and calcium carbonate adhesion were evaluated in the same manner as in Experiment 1. The results are shown in Table 1.
[0052] <Experiment 3> Except for using EVOH fibers without phosphate treatment, the self-healing property of the hardened cement composition and the calcium carbonate adhesion were evaluated in the same manner as in Experiment 1. The results are shown in Table 1.
[0053] <Experiment 4> Except for not using EVOH fiber, the self-healing property of the hardened cement composition was evaluated in the same manner as in Experiment 1. The results are shown in Table 1.
[0054]
[0055] A comparison of Experiments 1 and 2 with Experiment 3 shows that calcium carbonate adheres more easily to phosphorylated EVOH fiber than to unphosphorylated EVOH fiber. Furthermore, a comparison of Experiments 1 and 2 with Experiment 3 shows that phosphorylated EVOH fiber, when added to a cement composition, has a higher ability to promote self-healing of cracks that occur in the hardened body than unphosphorylated EVOH fiber.
[0056] The present invention has been described above with reference to specific embodiments. However, each embodiment is presented as an example and does not limit the scope of the present invention. Each embodiment described herein can be modified in various ways within the scope of the invention, and can be combined with features disclosed in other embodiments to the extent feasible. While specific embodiments of the present invention have been described in the above examples, these examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to be within the scope of the present invention.
[0057] The fibers according to the embodiment of the present invention can be suitably used as an additive to cement paste and as a self-healing accelerator for cracks in hardened cement paste.
Claims
1. A fiber comprising an ethylene-vinyl alcohol copolymer having a structural unit represented by the following formula (1):
2. Fibers containing phosphated ethylene-vinyl alcohol copolymer.
3. The fiber according to claim 1 or 2, wherein the amount of phosphorus contained per gram of the fiber, as measured by the molybdenum blue method, is 0.001 mg or more and 10 mg or less.
4. The fiber according to claim 1 or 2, wherein the amount of phosphorus contained per gram of the fiber, as measured by the molybdenum blue method, is 0.01 mg or more and 1 mg or less.
5. The fiber according to claim 1 or 2, wherein the fiber length is 1 mm or more and 200 mm or less.
6. The fiber according to claim 1 or 2, wherein the fiber length is 10 mm or more and 60 mm or less.
7. A method for producing fibers suitable as an additive to cement paste, comprising phosphorylating an unphosphorylated ethylene-vinyl alcohol copolymer contained in precursor fibers formed therefrom.
8. The method of claim 7, further comprising cutting the precursor fibers to a fiber length of 1 mm or more and 200 mm or less prior to phosphorylating the unphosphorylated ethylene-vinyl alcohol copolymer.
9. A method for producing fibers suitable as an additive to cement paste, comprising cutting continuous fibers formed using a phosphated ethylene-vinyl alcohol copolymer to have a fiber length of 1 mm or more and 200 mm or less.
10. The method according to claim 7 or 9, wherein the fiber contains an ethylene-vinyl alcohol copolymer containing a structural unit of the following formula (1):
11. The method according to claim 7 or 9, wherein the amount of phosphorus contained per gram of the fiber, as measured by the molybdenum blue method, is 0.001 mg or more and 10 mg or less.
12. A fiber produced by the method of claim 7 or 9.
13. Use of the fibers according to claim 1 or 2 as an additive to cement paste.
14. Use of the fiber according to claim 1 or 2 as a self-healing promoter for cracks in hardened cement bodies.
15. A cement composition comprising powdered cement and the fibers according to claim 1 or 2.
16. The cement composition of claim 15, further comprising aggregate.
17. A cement paste comprising the fibers according to claim 1 or 2, cement, and water.
18. A mortar comprising the cement paste of claim 17 and aggregate.
19. A concrete comprising the cement paste of claim 17 and aggregate.
20. A hardened cement product obtained from the cement paste according to claim 17.
Citation Information
Patent Citations
Ethylene-vinyl alcohol-based copolymer fiber
JP2007154402A
Conjugate fiber and porous fiber using the same
JP2010189829A
Synthetic fiber for self-healing of crack of cement hardened body, cement hardened body including the synthetic fiber, and method for repairing crack of cement hardened body
JP2014001129A
Fabric lettoff apparatus
JP1980001372A
Polyvinyl alcohol-based synthetic fiber and production thereof
JP1992228610A