Zeolite-containing activated carbon composition and method for producing same

By using carboxymethyl cellulose ammonium salt as a binder to stabilize zeolite particles on activated carbon, the composite composition achieves improved stability and lead removal efficiency, addressing adhesion and detachment issues in water purification.

WO2024248068A1PCT designated stage expired Publication Date: 2024-12-05KOWA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019808
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing composite compositions of activated carbon and zeolite for water purification face challenges in maintaining stability and preventing zeolite detachment when using finer zeolite particles, due to differences in specific gravity and adhesion issues, which affect their lead removal efficiency.

Method used

Incorporating carboxymethyl cellulose ammonium salt as a binder to adhere zeolite particles to activated carbon, with a specific particle size range and heating process to create a stable composite with high mechanical strength and improved lead adsorption ability.

Benefits of technology

The resulting composite maintains stability and effectively retains zeolite particles, enhancing lead removal capacity and mechanical strength, suitable for water purification applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019808_05122024_PF_FP_ABST
    Figure JP2024019808_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing: an activated carbon-containing composite composition which exhibits excellent stability during the production thereof and in which zeolite is hardly desorbed from activated carbon; and a method for producing the composition. The activated carbon-containing composite composition comprises activated carbon particles, zeolite particles, and carboxymethyl cellulose. The activated carbon-containing composite composition can be produced by a method including a step for mixing activated carbon particles, zeolite particles, and carboxymethyl cellulose ammonium salt together to produce a mixture and a step for heating the mixture to 150°C or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Zeolite-containing activated carbon composition and method for producing same

[0001] The present invention relates to an activated carbon-containing composite composition suitable for water purification applications.

[0002] Due to its excellent adsorption capacity, activated carbon is an adsorbent widely used for water purification. Due to growing concerns about the safety and hygiene of tap water, there is a high demand for water purification cartridges using activated carbon as a means of easily removing chlorine, trihalomethanes, and other contaminants from tap water. In addition, in recent years, there has been an increasing demand for the removal of heavy metals from tap water. Lead, in particular, is harmful to the human body and has a tendency to accumulate, so it is necessary to reduce intake, and there is a growing demand for as much lead removal as possible from tap water. Zeolite is known to have excellent lead adsorption capacity. When preparing a water purification composition, simply mixing activated carbon and zeolite can result in the zeolite easily flowing out of the filter when water is passed through, and the difference in specific gravity between activated carbon and zeolite makes it difficult to mix them uniformly. Therefore, it is common to combine the two. In order to bind and fix the zeolite to the activated carbon during such a composite process, it has been proposed to use a binder, and microfibrillated fibers, heat-fusible fibers, heat-fusible resin powders, etc. have been used as binders (Patent Documents 1 to 3). Furthermore, it has been reported that when a carboxymethylcellulose ammonium salt is used as a binder in producing a molded body of activated carbon, a molded body with high mechanical strength and excellent water resistance can be obtained (Patent Document 4).

[0003] Japanese Patent Laid-Open No. 07-256239 Japanese Patent Laid-Open No. 2003-334544 Japanese Patent Laid-Open No. 2020-163269 Japanese Patent Laid-Open No. 03-093615

[0004]

[0003] By making the zeolite particles finer, the specific surface area increases, thereby enhancing the lead removal ability. However, zeolite particles with small particle sizes are difficult to adhere to activated carbon particles, which leads to problems such as a loss of stability during production and the zeolite particles detaching from the activated carbon when water is passed through the composition. In light of these circumstances, an object of the present invention is to provide an activated carbon-containing composite composition that is stable during production and in which the zeolite is unlikely to detach from the activated carbon, and a method for producing the same.

[0005] As a result of extensive research, the present inventors have discovered that the above-mentioned problems can be solved even when small-sized zeolite particles are used by using carboxymethylcellulose ammonium salt as a binder for fixing zeolite particles to activated carbon, and have thus completed the present invention.

[0006] That is, the present invention is as follows. [1] An activated carbon-containing composite composition (hereinafter also referred to as the composition of the present invention) containing activated carbon particles, zeolite particles, and carboxymethylcellulose ammonium salt. [2] The activated carbon-containing composite composition according to [1], wherein the zeolite particles have a particle size of 0.5 to 10 μm. [3] The activated carbon-containing composite composition according to [1] or [2], wherein the activated carbon particles have a particle size of 180 to 5000 μm. [4] The activated carbon-containing composite composition according to any one of [1] to [3], having a size of 20 mesh pass and 50 mesh on. [5] A method for producing an activated carbon-containing composite composition (hereinafter also referred to as the production method of the present invention), comprising the steps of mixing activated carbon particles, zeolite particles, and carboxymethylcellulose ammonium salt to obtain a mixture, and heating the mixture to 150°C or higher. [6] The production method according to [5], wherein the zeolite particles have a particle size of 0.5 to 10 μm. [7] The production method according to [5] or [6], wherein the activated carbon particles have a particle size of 180 to 5000 μm. [8] The manufacturing method according to any one of [5] to [7], further comprising a step of recovering an activated carbon-containing composite composition having a size of 20 mesh pass and 50 mesh on after the heating step. [9] The manufacturing method according to any one of [5] to [8], wherein 8 to 12 parts by weight of the carboxymethyl cellulose ammonium salt is mixed with 100 parts by weight of the activated carbon particles.

[10] A water purification composition containing the activated carbon-containing composite composition according to any one of [1] to [4] or the activated carbon-containing composite composition manufactured by the manufacturing method according to any one of [5] to [9].

[11] A water purification cartridge comprising the water purification composition according to

[10] .

[0007] According to the present invention, even when small-sized zeolite particles are used in the composite with activated carbon, a composite composition is provided which is excellent in stability during production, the zeolite is less likely to be released, and has high mechanical strength. The activated carbon-containing composite composition of the present invention has excellent lead removal ability and is therefore suitable for use in water purification applications, and is expected to be applied to water purification cartridges, etc.

[0008] Graph showing residual lead concentration (ppb) after passing water through an activated carbon-containing composition. Graph showing residual lead concentration (ppb) after passing water through an activated carbon-containing composition.

[0009] The present invention will now be described in detail. However, the present invention is not limited to the following embodiments and can be freely modified within the scope of the present invention.

[0010] The composition of the present invention contains activated carbon particles, zeolite particles, and carboxymethyl cellulose. These components are not simply mixed in the composition of the present invention, but are bonded to each other to form a composite. Usually, carboxymethyl cellulose and / or its esterified crosslinked product derived from carboxymethyl cellulose ammonium salt added during production adhere the activated carbon particles and zeolite particles, and these are molded to form a composite composition.

[0011] The activated carbon in the present invention may be obtained by carbonizing and / or activating a carbonaceous material. The activated carbon particles are preferably several hundred micrometers in diameter from the viewpoint of the adsorption capacity of harmful substances such as trihalomethanes. 2 The specific surface area in this specification may be a value calculated by the BET method from a nitrogen adsorption isotherm.

[0012] Examples of the carbonaceous material include plant-based materials such as wood, sawdust, charcoal, fruit shells such as coconut shells and walnut shells, fruit seeds, pulp manufacturing by-products, lignin, and blackstrap molasses; mineral-based materials such as peat, grass peat, lignite, brown coal, lapilli, anthracite, coke, coal tar, coal pitch, petroleum distillation residue, and petroleum pitch; synthetic materials such as phenol, saran, and acrylic resin; and natural materials such as recycled fiber (rayon).

[0013] From the viewpoints of harmful substance removal performance, pressure loss during water flow, and ease of molding (granulation), the particle size of the activated carbon particles is preferably 180 μm or more and 5000 μm or less, more preferably 250 μm or more and 2000 μm or less, and most preferably 300 μm or more and 850 μm or less, as measured by the particle size measurement method according to JIS K1474:2014. The particle size in this specification may be a value measured using a laser diffraction / scattering particle size distribution analyzer. Furthermore, unless otherwise specified, the particle size in this specification may be the major axis. The shape of the activated carbon particles is not particularly limited and may be spherical, approximately spherical, plate-like, acicular, or amorphous.

[0014] Zeolites in the present invention may include aluminosilicates and metallosilicates.

[0015] As the aluminosilicate, A-type or X-type aluminosilicate can be preferably used because of its large ion exchange capacity. Furthermore, the metallosilicate is an aluminosilicate in which the aluminum atoms are substituted with other metal atoms, and may be represented by the following general formula (1): x(MIO m/2 )y(MIIO n/2 )z(SiO 2 ) (1) In general formula (1), MI is at least one element selected from Na, K, Ca, Mg, and H, MII is at least one metal atom selected from Ti, Zn, Al, B, P, Fe, Ga, Cu, V, and Cr, x, y, and z represent the number of moles of each compound, where x > 0, y > 0, and z > 0, and m and n represent the valences of the MI and MII elements, respectively, and z / y > 1. The MII metal in the metallosilicate compound is preferably titanium (Ti), and z / y is preferably 2.5 to 25, and more preferably 3 to 7.

[0016] In this embodiment, the zeolite particles are 300 m in diameter from the viewpoint of lead adsorption capacity. 2 Preferably, the specific surface area is 1 / g or more.

[0017] From the viewpoint of lead adsorption performance (adsorption rate and adsorption amount), the particle size of the zeolite particles is preferably 0.5 to 10 μm, more preferably 0.5 to 3 μm, as measured by a particle size distribution method using a laser diffraction scattering method. In the composition of the present invention, since the zeolite particles are unlikely to be detached from the activated carbon particles, even zeolite particles having such a small particle size can be used, thereby making it possible to obtain an activated carbon-containing composite composition with high lead adsorption capacity.

[0018] The shape of the zeolite particles is not particularly limited, and may be spherical, approximately spherical, plate-like, needle-like, or irregular.

[0019] Commercially available zeolite particles can be used, for example, "Zeomic H010N" and "Zeomic LH210N" commercially available from Sinanen Zeomic Co., Ltd.

[0020] The carboxymethyl cellulose in the composition of the present invention may contain a crosslinked product. The carboxymethyl cellulose ammonium salt added as a binder in the production method of the present invention described below is a carboxymethyl cellulose in which an ammonium group is bonded to the end of the carboxyl methyl group. It decomposes upon heating and converts into carboxymethyl cellulose having a free carboxyl group. The carboxymethyl cellulose having a free carboxyl group can form an ester bond with a hydroxyl group in a neighboring carboxymethyl cellulose molecule to form a crosslinked structure and bond the molecules together. Therefore, carboxymethyl cellulose and its esterified crosslinked product make the activated carbon-containing composite composition less soluble in water, harder, and less likely to release zeolite particles from the activated carbon.

[0021] The carboxymethyl cellulose and / or carboxymethyl cellulose ammonium salt in the present invention may be one which, when made into a 1% aqueous solution, has a viscosity of preferably 1 to 2000 cps, more preferably 1 to 500 cps, as measured at 25°C and 60 rpm using a Brookfield viscometer.

[0022] The carboxymethylcellulose ammonium salt may be commercially available, for example, "CMC Ammonium Salt DN10L" available from Daicel Millize Co., Ltd.

[0023] From the viewpoint of lead adsorption capacity and strength, the composition of the present invention preferably has a size of 20 mesh pass and 50 mesh on. In this specification, 20 mesh refers to a mesh size of 0.850 mm, and 50 mesh refers to a mesh size of 0.300 mm. Furthermore, 10 mesh described in the examples refers to a mesh size of 2.000 mm, and 30 mesh refers to a mesh size of 0.600 mm. The shape of the composition of the present invention is not particularly limited, and may be spherical, approximately spherical, plate-like, acicular, or irregular.

[0024] The composition of the present invention preferably contains 8 to 12 parts by weight of carboxymethyl cellulose per 100 parts by weight of activated carbon particles. If the amount of carboxymethyl cellulose as a binder is too large, the activated carbon may be coated, resulting in a decrease in water purification ability. If the amount is too small, the zeolite particles may be easily detached from the activated carbon.

[0025] The composition of the present invention preferably contains 4 to 12 parts by weight of zeolite particles per 100 parts by weight of activated carbon particles, and within this range, sufficient lead adsorption capacity can be achieved.

[0026] The composition of the present invention can be preferably produced by the production method of the present invention, i.e., a method including the steps of mixing activated carbon particles, zeolite particles, and carboxymethylcellulose ammonium salt to obtain a mixture, and heating the mixture to 150°C or higher, preferably 150 to 250°C, more preferably 180 to 220°C. The activated carbon particles, zeolite particles, and carboxymethylcellulose ammonium salt are the same as those described above for the composition of the present invention. In the step of obtaining the mixture, water may be added in addition to the activated carbon particles, zeolite particles, and carboxymethylcellulose ammonium salt. The amount of water added is preferably 80 to 120 parts by weight per 100 parts by weight of activated carbon particles. The resulting mixture may be molded or granulated into pellets or the like before the subsequent heating step. Molding or granulation can be performed by any known method, such as pressing or extrusion. The resulting mixture may also be dried to reduce the moisture content before the subsequent heating step. The drying step may be performed after the molding or granulation step of the mixture. The mixture is heated at a temperature of 150° C. or higher, preferably 150 to 250° C., more preferably 180 to 220° C., for preferably 60 minutes or longer, more preferably 120 minutes or longer. As described above, the heating step causes the carboxymethyl cellulose ammonium salt to thermally decompose, forming an esterified crosslinked structure of carboxymethyl cellulose, making the activated carbon-containing composite composition less soluble in water, hard, and less likely to release zeolite particles from the activated carbon.

[0027] In the production method of the present invention, it is preferable to mix 8 to 12 parts by weight of carboxymethyl cellulose ammonium salt with 100 parts by weight of activated carbon particles. Also, in the production method of the present invention, it is preferable to mix 4 to 12 parts by weight of zeolite particles with 100 parts by weight of activated carbon particles. The explanation of these ranges is in accordance with the explanation of the composition of the present invention described above.

[0028] The production method of the present invention may further include, after the heating step, a step of recovering the activated carbon-containing composite composition having a size of 20 mesh pass and 50 mesh on.

[0029] The composition of the present invention or the activated substance-containing composite composition obtained by the manufacturing method of the present invention can adsorb and remove harmful substances such as lead and trihalomethanes from water, and therefore can be incorporated into a water purification composition. In addition to the activated carbon-containing composite composition of the present invention, the water purification composition may optionally contain other components such as activated carbon and excipients. Such a water purification composition can be filled into a column container or the like to form a water purification cartridge, or can be formed into a molded product enclosed in a nonwoven fabric, or can be in any form suitable for water flow. The water purification composition is preferably provided in these forms in a water purifier.

[0030] The present invention will be explained in more detail below using examples, but the present invention is not limited to these examples.

[0031] [Test Example 1] Investigation of binders and granulation conditions A search was made for a binder suitable for compositing activated carbon particles and zeolite particles. The activated carbon-containing composite compositions produced in the following production examples were evaluated as follows.

[0032] <Hardness Evaluation> The hardness was evaluated according to the following procedure (hardness measurement method described in JIS K1474:2014). Fifteen 12.7 mm diameter steel balls and fifteen 9.5 mm diameter steel balls were placed in a circular metal hardness test dish with a diameter of 20 cm and a depth of 5 cm. 100 mL of the sieved sample (20 mesh pass and 50 mesh on, or 10 mesh pass and 30 mesh on, excluding samples outside the specified sieve size) was measured and weighed (S). This was placed in the hardness test dish and shaken for 30 minutes using a sieve shaker. The entire amount was then sieved through a 50 mesh or 30 mesh sieve, and the weight (W) of the mesh-on sample, i.e., the sample remaining in the hardness test dish after shaking, was measured. The hardness was calculated by applying each weight to the following formula: Hardness H (%) = W / S × 100

[0033] <Evaluation of Moldability> After kneading predetermined materials, the strength and moldability of the mixture were observed when it was molded.

[0034] <Evaluation after immersion in water> 10 g of the produced activated carbon-containing composite composition was put into 200 mL of water at room temperature, and the state after leaving it to stand for 30 minutes was observed.

[0035] (Production Example 1) Bentonite The materials shown in Table 1 were kneaded and molded into pellets using a disk pelleter (φ4 mm), and then dried at 150°C for 4 hours. After drying, the crushed pellets were sieved to obtain pellets that passed 20 mesh and were on 50 mesh. The hardness of the obtained composition was very low. Furthermore, a large amount of binder was required for molding.

[0036]

[0037] (Production Example 2) Polyolefin, Carboxymethylcellulose Ammonium Salt The materials shown in Table 2 were kneaded and molded into pellets using a disk pelleter (φ4 mm). The pellets were dried at 150°C for 4 hours, and the weights were measured before and after drying. After drying, the crushed pellets were sieved to obtain pellets that passed 20 mesh and were on 50 mesh. When polyolefin was used as the binder, moldability was very poor. On the other hand, when carboxymethylcellulose ammonium salt was used as the binder, moldability was excellent. Furthermore, the amount of binder required for molding could be made smaller than that of bentonite. However, when immersed in water, some of the binder gelled, causing the composition to disintegrate.

[0038]

[0039] (Production Example 3) Study of Heat Treatment 1 The materials shown in Table 3 were kneaded and molded into pellets using a disk pelleter (φ4 mm), which were then dried at 80°C for 4 hours, and the weights were measured before and after drying. The dried pellets were then heat-treated under the conditions shown in Table 3, crushed, and sieved to obtain pellets that passed 20 mesh and were on 50 mesh. The heat treatment prevented dissolution and gelation of the binder when immersed in water, and prevented the composition from collapsing.

[0040]

[0041] (Production Example 4) Study of Heat Treatment 2 The materials shown in Table 4 were kneaded and molded into pellets using a disk pelletizer (φ4 mm). The pellets were then dried at 80°C for 4 hours, and the weights were measured before and after drying. The dried pellets were then heat-treated under the conditions shown in Table 4, crushed, and sieved to obtain pellets with a 20-mesh pass and a 50-mesh pass. It is believed that the dissolution of the carboxymethylcellulose ammonium salt in the composition in water is influenced by the dissociation of the ammonia moiety due to reaction with the alkali content of the activated carbon. Therefore, the use of activated carbon that had been pre-washed with acid to remove the alkali content (acid-washed carbon) prevented the composition from collapsing. However, the use of unwashed activated carbon after heat treatment at 200°C also prevented the composition from collapsing.

[0042]

[0043] (Production Example 5) Carboxymethylcellulose ammonium salt, acrylic polymer The materials shown in Table 5 were kneaded and molded into pellets using a disk pelletizer (φ4 mm), which were then dried at 150°C for 4 hours, and the weights were measured before and after drying. The dried pellets were then heat-treated under the conditions shown in Table 5, crushed, and sieved to obtain pellets that passed 20 mesh and were on 50 mesh. When an acrylic polymer was used as a binder, the viscosity was high during kneading and dispersibility was poor, resulting in very poor moldability. Furthermore, when an acrylic polymer and carboxymethylcellulose ammonium salt were used in combination as binders, moldability was improved and disintegration of the composition when immersed in water was prevented.

[0044]

[0045] (Production Example 6) Investigation of Granule Size The materials shown in Table 6 were kneaded and molded into pellets using a disk pelleter (φ4 mm), followed by drying at 80°C for 4 hours. The dried pellets were further heat-treated at 200°C for 2 hours, crushed, and sieved to obtain pellets that passed 10 mesh and were on 30 mesh, or pellets that passed 20 mesh and were on 50 mesh. When an acrylic polymer and carboxymethylcellulose ammonium salt were used in combination as a binder, the viscosity was high during kneading, making stable moldability impossible, and in some cases, the pellets were not suitable for molding using a disk pelleter. When carboxymethylcellulose ammonium salt was used alone as a binder, the composition exhibited excellent moldability, was prevented from collapsing when immersed in water, and sufficient hardness was obtained.

[0046]

[0047] Test Example 2: Investigation of zeolite release from activated carbon-containing composite composition The materials shown in Table 7 were mixed and formed into pellets using a disk pelleter (φ4 mm), and then dried at 80°C for 4 hours. The dried pellets were further heat-treated at 200°C for 2 hours, crushed, and then sieved to obtain pellets that passed 10 mesh and were on 30 mesh, or pellets that passed 20 mesh and were on 50 mesh. The zeolite release rate of the obtained activated carbon-containing composite composition was evaluated using the following procedure.

[0048] <Evaluation of Desorption Rate> The mesh-on sample (the sample that remained uncrushed by shaking in the hardness test dish) and the mesh-pass sample obtained when sieved through a 30-mesh or 50-mesh sieve in the hardness test described above were each thoroughly combusted to remove activated carbon. The ash after combustion was recovered and weighed, and the weight ratio of the ash of the over-sieve sample to the ash of the under-sieve sample was taken as the zeolite weight ratio. The closer this weight ratio between the over-sieve sample and the under-sieve sample is to 1, the less zeolite was desorbed.

[0049] As shown in Table 7, it was found that the smaller the particle size of the zeolite particles, the less the zeolite particles were released from the composition.

[0050]

[0051] [Test Example 3] Investigation of Lead Removal Ability 1 The materials shown in Table 8 were kneaded and formed into pellets using a disk pelleter (φ4 mm) and dried at 80°C for 4 hours. The dried pellets were further heat-treated at 200°C for 2 hours, crushed, and sieved to obtain pellets that passed 20 mesh and were on 50 mesh. These were used as the granules of Examples 1 to 3. The granules of Examples 1 to 3 were mixed with powdered activated carbon to prepare Samples 1 to 3, each with the composition shown in Table 9. Comparative samples of powdered activated carbon were also prepared, and each sample was packed into a column. Lead was dissolved in tap water at a concentration of 0.15 ppm to prepare a test solution. The test solution was passed through the column packed with each sample at room temperature at a rate of 20 mL / min using a Smoothflow Pump (manufactured by Takumina Corporation). After the start of water flow, the test solution was collected at predetermined intervals, and the residual lead concentration was measured by flameless atomic absorption spectrometry.

[0052]

[0053]

[0054] The results are shown in Figure 1. Zeolite particles with smaller particle sizes had a higher lead adsorption rate than those with larger particle sizes.

[0055] [Test Example 4] Investigation of lead removal ability 2 The materials shown in Table 10 were kneaded and molded into pellets using a disk pelleter (φ4 mm), and then dried at 80°C for 4 hours. The dried pellets were further heat-treated at 200°C for 2 hours, crushed, and sieved to obtain pellets that passed 10 mesh and were on 30 mesh, or pellets that passed 20 mesh and were on 50 mesh for each of Examples 4 to 6. Samples 4 to 9 were prepared by mixing the granulated materials of Examples 4 to 6 with powdered activated carbon, each having the composition shown in Table 11. Additionally, powdered activated carbon alone was prepared as a comparative sample. A water flow test was performed on each sample in the same manner as in Test Example 3, and the residual lead concentration after the test was measured.

[0056]

[0057]

[0058] The results are shown in Figure 2. The higher the content of zeolite particles and the lower the content of binder, the better the lead removal ability. Furthermore, the smaller the particle size of the activated carbon-containing composite composition (20 mesh pass and 50 mesh on) was, the better the lead adsorption rate.

[0059] Test Example 5: Strength Study The activated carbon-containing composite compositions of Examples 1 to 3 prepared in Test Example 3, or samples containing only powdered activated carbon, were observed for disintegration when immersed in water to evaluate the strength of the compositions. Each sample was washed with water to remove residual dust that could cause initial turbidity, and then 1 g of each was added to 70 mL of tap water and allowed to stand at room temperature for 14 days. After 14 days, the samples were gently stirred, and the supernatant was recovered and the light transmittance was measured. Furthermore, the immersion liquid after 14 days was shaken horizontally (80 rpm) for 2 hours in a shaker, and the supernatant was recovered and the light transmittance was measured. Note that adding the activated carbon-containing composite composition to tap water did not result in water repellency.

[0060] The results are shown in Table 12. It was found that the use of zeolite particles with larger particle sizes resulted in a composition that was more prone to collapse and had poorer strength.

[0061]

Claims

1. An activated carbon-containing composite composition comprising activated carbon particles, zeolite particles, and carboxymethyl cellulose.

2. The activated carbon-containing composite composition according to claim 1, wherein the zeolite particles have a particle size of 0.5 to 10 μm.

3. The activated carbon-containing composite composition according to claim 1, wherein the activated carbon particles have a particle size of 180 to 5000 μm.

4. The activated carbon-containing composite composition according to claim 1, having a size of 20 mesh pass and 50 mesh on.

5. A method for producing an activated carbon-containing composite composition, comprising: mixing activated carbon particles, zeolite particles, and carboxymethylcellulose ammonium salt to obtain a mixture; and heating the mixture to 150° C. or higher.

6. The method according to claim 5, wherein the zeolite particles have a particle size of 0.5 to 10 μm.

7. The method according to claim 5, wherein the particle size of the activated carbon particles is 180 to 5000 μm.

8. The method of claim 5, further comprising the step of recovering the activated carbon-containing composite composition having a size of 20 mesh pass and 50 mesh on after said heating step.

9. The method according to claim 5, wherein 8 to 12 parts by weight of the carboxymethylcellulose ammonium salt is mixed with 100 parts by weight of the activated carbon particles.

10. A water purification composition comprising the activated carbon-containing composite composition according to any one of claims 1 to 4, or the activated carbon-containing composite composition produced by the production method according to any one of claims 5 to 9.

11. A water purification cartridge comprising the water purification composition according to claim 10.

Citation Information

Patent Citations

  • Adsorbent for gas

    JP1985235637A

  • Production of formed carbon material

    JP1991093615A

  • Deodorizing material

    JP1997154927A

  • Deodorizing body

    JP1997192205A

  • Porous absorbing material and its manufacturing method

    JP2001219061A