Resin substrate, light guide plate, optical member for eyewear, and wearable device

The use of a resin substrate with specific density and refractive index, combined with a diffraction grating, addresses the issue of residual stress-induced birefringence in resin light guide plates, achieving lightweight and high-image-clarity solutions for augmented reality wearable devices.

WO2024248093A1PCT designated stage expired Publication Date: 2024-12-05HOYA CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019889
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Resin light guide plates for augmented reality wearable devices face challenges in achieving lightweight designs with high image clarity due to residual stress-induced birefringence, which blurs images, despite using resins with improved refractive indices.

Method used

A resin substrate with a thickness of 0.1 to 1.5 mm, density of 0.93 to 2.10 g/cm³, and refractive index of 1.60 or more, where the retardation value is 30 nm or less, and the A/B ratio of retardation differences is 3.5 or less, is used, along with a diffraction grating, to minimize residual stress and enhance image clarity.

Benefits of technology

The solution results in lightweight resin substrates and light guide plates that provide excellent image reproducibility and reduced haze, maintaining image clarity even after accelerated weathering tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019889_05122024_PF_FP_ABST
    Figure JP2024019889_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a resin substrate for forming an optical member, the resin substrate containing a resin, wherein the thickness of the resin substrate is 0.1 to 1.5 mm, the density of the resin is 0.93 to 2.10 g / cm3, the refractive index of the resin substrate is 1.60 or more, a retardation value of the resin substrate is 30 nm or less, and the following formula (1) is satisfied, where A is the difference between a maximum value and a minimum value of the retardation measured on a straight line in a uniaxial direction of the resin substrate, and B is the difference between a maximum value and a minimum value of the retardation measured on a straight line in a direction substantially orthogonal to the uniaxial direction. (1)…A / B≤3.5
Need to check novelty before this filing date? Find Prior Art

Description

Resin substrates, light guide plates, optical components for eyewear, and wearable devices

[0001] The present disclosure relates to a resin substrate, a light guide plate, an optical member for eyewear, and a wearable device.

[0002] In augmented reality (AR) wearable devices such as head-mounted displays, it has been proposed to use a light guide plate made of a high-refractive index glass substrate in order to expand the field of view (FOV) (for example, Patent Document 1).

[0003] The projected light emitted from this type of AR wearable device passes through a light guide plate and travels to the field of vision of the device wearer, where it is focused using a diffraction grating or the like, and transmitted light from outside is delivered to the field of vision of the device wearer together with the projected light.

[0004] JP 2022-97824 A

[0005] High density (3.0-5.5 g / cm 3 While selecting a glass composition that is high enough to increase the refractive index of a glass substrate can hinder the weight reduction of wearable devices and reduce the manufacturing yield and processability of the glass substrate. Therefore, efforts have been made to manufacture light guide plates using resin compositions with low density and high refractive index. However, when molding a thin resin light guide plate with a thickness of 0.1 to 1.5 mm, residual stress can occur in the resin substrate (light guide plate) due to the dispersion state of the inorganic filler, as well as the molding pressure and cooling time. This can cause birefringence in the light passing through the light guide plate, resulting in blurred or smeared edges of images passing through the light guide plate. As a result, even when a resin with an improved refractive index is used, it has not been possible to achieve the required performance as a light guide plate. Therefore, the present disclosure aims to provide a resin substrate, light guide plate, eyewear optical component, and wearable device that are lightweight and exhibit excellent image clarity.

[0006] A resin substrate according to an embodiment of the present disclosure is a resin substrate for forming an optical member, the resin substrate comprising a resin, wherein the thickness of the resin substrate is 0.1 to 1.5 mm, and the density of the resin is 0.93 to 2.10 g / cm 3 The resin substrate has a refractive index of 1.60 or more, a retardation value of 30 nm or less, and, when the difference between the maximum and minimum values ​​of retardation measured on a straight line in one axial direction of the resin substrate is A and the difference between the maximum and minimum values ​​of retardation measured on a straight line in a direction substantially perpendicular to the one axial direction is B, the relationship of the following formula (1) is satisfied: A / B≦3.5 (1)

[0007] A light guide plate according to an embodiment of the present disclosure includes: a substrate containing a resin; and a diffraction grating formed on at least a portion of the substrate, wherein the thickness of the substrate is 0.1 to 1.5 mm, and the density of the resin is 0.93 to 2.10 g / cm. 3 The refractive index of the substrate is 1.60 or more, the retardation value of the substrate is 30 nm or less, and when the difference between the maximum and minimum values ​​of retardation measured on a line in one axial direction of the substrate is A and the difference between the maximum and minimum values ​​of retardation measured on a line in a direction approximately perpendicular to the one axial direction is B, the relationship of the following formula (1) is satisfied: A / B≦3.5 (1)

[0008] An eyewear optical element according to one embodiment of the present disclosure includes: a resin translucent substrate; and a light guide plate according to any one of claims 10 to 17, wherein at least one light guide plate is integrally held by the light-transmitting substrate; and the refractive index (RW) of the light guide plate is greater than the refractive index (RT) of the light-transmitting substrate.

[0009] A wearable device according to one embodiment of the present disclosure includes the above-described optical member for eyewear.

[0010] The present disclosure can provide a resin substrate, a light guide plate, an optical member for eyewear, and a wearable device that are lightweight and exhibit excellent image reproducibility.

[0011] Fig. 1 is a schematic cross-sectional view showing one embodiment of a light guide plate according to this embodiment. Fig. 2 is a drawing showing the outline of a resin substrate according to this embodiment. Fig. 3 is a flow chart of a cast polymerization method. Fig. 4 is a flow chart of an injection molding method. Fig. 5 is a schematic diagram showing the measurement range of the retardation value and A / B in a resin substrate.

[0012] Hereinafter, an embodiment of the present disclosure (hereinafter referred to as "the present embodiment") will be described in detail, but the present invention is not limited thereto, and various modifications are possible without departing from the gist of the present invention. In this specification, for example, when a numerical range is expressed as "1 to 100," it is intended to include both the lower limit "1" and the upper limit "100." The same applies to other numerical ranges.

[0013] 1 is a schematic cross-sectional view showing an embodiment of a light guide plate according to the present invention. The light guide plate 1 includes a substrate 10 containing a resin, a diffraction grating 52, and a diffraction grating 32. The diffraction grating 52 and the diffraction grating 32 are each formed on one main surface of the substrate 10. Light of each wavelength is introduced into the diffraction grating 52 from the image display device 24.

[0014] The image display element 24 is, for example, a transmissive liquid crystal (LCD T-LCOS) panel driven by a field sequential method. The image display element 24 modulates light of each wavelength in accordance with an image signal generated by an image engine (not shown) of the signal processing device 5. The light of each wavelength modulated by the pixels in the effective area of ​​the image display element 24 is incident on the light guide plate 10 with a predetermined luminous flux cross section (approximately the same shape as the effective area). Note that the image display element 24 can also be replaced with other types of display elements, such as a DMD (Digital Mirror Device), a reflective liquid crystal (LCOS) panel, a MEMS (Micro Electro Mechanical Systems), an organic EL (Electro-Luminescence), or an inorganic EL.

[0015] 1, a diffraction grating 52 is laminated on the second surface 10b of the substrate 10. The diffraction grating 52 may have, for example, an interference fringe pattern pitch formed thereon.

[0016] The light of each wavelength modulated by the image display element 24 is sequentially incident on the first surface 10a into the substrate 10.

[0017] The diffraction grating 52 diffracts the light of each wavelength incident sequentially at a predetermined angle to guide it to the wearer's eye. The light of each wavelength diffracted by the diffraction grating 52 is repeatedly totally reflected at the interface between the substrate 10 and air, propagates within the substrate 10, and is then incident on the diffraction grating 32.

[0018] The light of each wavelength incident on the diffraction grating 32 is diffracted by the diffraction grating 32 and sequentially emitted approximately perpendicularly to the outside from the second surface 10b of the light guide plate 10. The light of each wavelength thus emitted as approximately parallel light is focused on the wearer's retina as a virtual image I of the image generated by the image display element 24.

[0019] <Substrate> The substrate 10 in the light guide plate 1 according to this embodiment contains a resin. By using a substrate containing a resin as the base material, it is possible to use a material that has a high refractive index but a relatively low density, making it possible to reduce the weight of the wearable device. The thickness of the substrate 10 is preferably 0.1 to 1.5 mm, more preferably 0.2 to 1.2 mm, and even more preferably 0.3 to 1.0 mm. The thickness of the resin substrate or the substrate of the light guide plate can be measured using an ultrasonic thickness gauge.

[0020] The density of the resin used in the substrate 10 is preferably 0.93 to 2.10 g / cm 3 and more preferably 1.20 to 1.80 g / cm 3 and more preferably 1.30 to 1.50 g / cm 3 The density of the resin can be measured by the underwater displacement method in accordance with JIS K7112-1:2023.

[0021] The refractive index of the substrate 10 is preferably 1.60 or more, more preferably 1.65 or more, and even more preferably 1.70 or more. The upper limit of the refractive index of the substrate is not particularly limited, but is, for example, 2.00 or less. By setting the refractive index of the substrate within this range, the viewing angle can be widened. The refractive index can be measured in accordance with JIS K7142:2014.

[0022] The retardation value of the substrate is preferably 30 nm or less, more preferably 15 nm or less, and even more preferably 10 nm or less. The lower limit of the retardation value of the substrate is not particularly limited, but is, for example, 0.1 nm or more.

[0023] "Retardation" is the phase difference between light in the direction of the molecular main chain and light perpendicular to it. Generally, polymers can be molded into any shape by heating and melting them, and it is known that retardation occurs due to the stress and molecular orientation that occurs during the heating and cooling process. In this specification, "retardation" refers to in-plane retardation unless otherwise specified.

[0024] The retardation value can be within the aforementioned range by reducing the residual stress in the resin substrate (light guide plate) through appropriate material selection, pressure control during molding, and cooling conditions. However, even when the residual stress is reduced, variations in the pressure distribution during molding of the resin substrate, the molecular structure of the resin that increases the refractive index of the resin substrate, or the molecular orientation of the inorganic filler can cause differences in the retardation value distribution depending on the location on the resin substrate or resin light guide plate. This causes variations in the light passing through the light guide plate, making it difficult to adequately control the image and reducing image clarity. Therefore, in addition to lowering the retardation value, we also need to reduce variations in the residual stress distribution to achieve the A / B range described below.

[0025] When the difference between the maximum and minimum retardation values ​​measured along a line in one axial direction of the substrate 10 is A and the difference between the maximum and minimum retardation values ​​measured along a line in a direction substantially perpendicular to the uniaxial direction is B, it is preferable to satisfy the relationship of the following formula (1). By satisfying this A / B range, variation in the residual stress distribution is reduced, preventing a decrease in the intensity and clarity of image light due to optical transmission loss. A / B≦3.5 (1) A / B is preferably 1.0 to 3.0, more preferably 1.1 to 2.5, even more preferably 1.1 to 1.8, even more preferably 1.1 to 1.6, even more preferably 1.1 to 1.5, and even more preferably 1.1 to 1.2. To achieve A / B within this range, the retardation value is set to 30 nm or less, and internal stress is further removed. Specifically, to eliminate variation in the residual stress distribution, internal stress can be removed by polishing or annealing the entire resin substrate. A lower retardation value tends to increase the A / B value, so even if the retardation value is reduced, the variation in birefringence can be reduced by preventing anisotropy from occurring in the substrate.

[0026] 0.75 W / m 2 The haze of the light guide plate after 200 hours of accelerated weathering test in a cycle of 5 hours of UV light irradiation and 5 hours of humid 95% RH is preferably 1.8% or less, more preferably 1.0% or less, and even more preferably 0.8% or less. In accordance with JIS K 7373:2006, the test was conducted using a QUV accelerated weathering tester QUV / SE (manufactured by Q-LAB) after 4 hours of UV light irradiation (0.20 W / m 2 The sample is subjected to an accelerated weathering test for 168 hours, with a cycle of 95% RH and 95% RH humidity for 4 hours, and the haze is measured in accordance with JIS K7136.

[0027] The ratio (R / D) of the refractive index (R) of the substrate to the density (D) of the substrate is preferably 1.00 to 1.30, more preferably 1.10 to 1.30, and even more preferably 1.13 to 1.26. By satisfying this R / D range, a light guide plate that is lightweight and has a high refractive index can be obtained. The R / D value is calculated from the refractive index (R) of the resin substrate or resin light guide plate obtained by the above measurement method and the density (D) of the resin substrate or resin light guide plate.

[0028] Examples of resins used for the substrate include at least one selected from the group consisting of urethane resins, episulfide resins, polycarbonate resins, acrylic resins, epoxy resins, and nitrogen-containing aromatic polymer resins.

[0029] (Urethane-based resin) Urethane-based resin is the cured product of the polymerizable composition that comprises isocyanate component and active hydrogen compound component.As urethane-based resin, there can be mentioned the thiourethane resin that comprises the polymerization site of isocyanate component and polythiol component; the thiourethane resin that is the polymerization site of isocyanate component and polyol component; and the urethane-urea resin that has the polythiourethane site that is the polymerization site of isocyanate component and thiol component and the polyurea site that is the polymerization product of isocyanate component and polyamine component.

[0030] Examples of the isocyanate component include bis(isocyanatomethyl)bicyclo[2.2.1]heptane, bis(isocyanatomethyl)cyclohexane, bis(isocyanatomethyl)benzene, tolylene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and pentamethylene diisocyanate.

[0031] Examples of the active hydrogen compound component include toluenediamine, pentaerythritol tetrakismercaptoacetate, pentaerythritol tetrakismercaptopropionate, trimethylolpropane trismercaptoacetate, trimethylolpropane trismercaptopropionate, bis(mercaptoethylthio)mercaptopropane, bis(mercaptomethyl)-3,6,9-trithiaundecanedithiol, dimercaptoethyl sulfide, and bis(mercaptomethyl)dithiane. Among these, it is preferable to use polythiol components such as pentaerythritol tetrakismercaptoacetate, pentaerythritol tetrakismercaptopropionate, trimethylolpropane trismercaptoacetate, trimethylolpropane trismercaptopropionate, bis(mercaptoethylthio)mercaptopropane, bis(mercaptomethyl)-3,6,9-trithiaundecanedithiol, dimercaptoethyl sulfide, and bis(mercaptomethyl)dithiane.

[0032] The equivalent ratio of the active hydrogen groups of the active hydrogen compound component to the isocyanato groups of the polyisocyanate component (active hydrogen groups / isocyanato groups) is preferably 40 / 60 to 60 / 40, more preferably 45 / 55 to 55 / 45. Examples of the active hydrogen groups include hydroxy groups, mercapto groups, and —NH groups.

[0033] (Episulfide Resin) The episulfide resin is a cured product of a polymerizable composition containing an epithio compound. Here, the polymerizable composition may contain other monomers.

[0034] Examples of epithio compounds include bis-(β-epithiopropyl) sulfide and bis-(β-epithiopropyl) disulfide. In addition to the epithio compound, other polymerizable components such as the polyisocyanate component and polythiol component described above may be added to the polymerizable composition. The content of the epithio compound in the polymerizable composition is preferably 50 to 98% by mass, more preferably 60 to 96% by mass, and even more preferably 70 to 96% by mass.

[0035] The polymerizable composition preferably further contains sulfur in combination with the epithio compound. The sulfur content in the polymerizable composition is preferably 1 to 30% by mass, more preferably 5 to 20% by mass, and even more preferably 10 to 20% by mass or more.

[0036] The polymerizable composition preferably further contains a polythiol compound in combination with the epithio compound. Examples of the polythiol compound include the compounds exemplified above. When used in combination with the epithio compound, the content of the polythiol compound in the polymerizable component is preferably 2 to 50% by mass or more, more preferably 4 to 30% by mass, and even more preferably 5 to 10% by mass.

[0037] When the polymerizable composition contains a polyisocyanate component and a polythiol component, or an epithio compound, it preferably contains a polymerization catalyst, such as a tin compound (e.g., dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dichloride, dimethyltin dichloride), a tertiary amine, a quaternary ammonium salt, an imidazole compound, or a pyrazole compound.

[0038] When the polymerizable composition contains an isocyanate component and an active hydrogen compound component, the amount of the polymerization catalyst added in the polymerizable composition is preferably 0.001 to 2 parts by mass, more preferably 0.005 to 1 part by mass, and even more preferably 0.007 to 0.5 parts by mass or more, relative to 100 parts by mass of the total amount of the isocyanate component and the active hydrogen compound component.

[0039] When an epithio compound is contained, the amount of the polymerization catalyst added in the polymerizable composition is preferably 0.001 to 2 parts by mass, more preferably 0.005 to 1 part by mass, and still more preferably 0.007 to 0.5 parts by mass, relative to 100 parts by mass of the total amount of the polymerizable components.

[0040] (Polycarbonate Resin) The polycarbonate resin is preferably a cured product of a polymerizable composition containing diethylene glycol bisallyl carbonate. The polymerizable composition preferably contains diethylene glycol bisallyl carbonate, more preferably diethylene glycol bisallyl carbonate, benzyl methacrylate, diallyl phthalate, and an alkyl methacrylate in which the alkyl group has 1 to 4 carbon atoms.

[0041] The amount of diethylene glycol bisallyl carbonate blended is preferably 5 to 100% by mass, more preferably 10 to 80% by mass, and even more preferably 20 to 50% by mass, based on the total amount of monomers in the polymerizable composition. When used in combination with benzyl methacrylate, diallyl phthalate, and an alkyl methacrylate having an alkyl group of 1 to 4 carbon atoms, the amount of diethylene glycol bisallyl carbonate blended is more preferably 5 to 40% by mass, more preferably 10 to 35% by mass, and even more preferably 20 to 40% by mass, based on the total amount of monomers in the polymerizable composition.

[0042] The amount of benzyl methacrylate to be blended is preferably 5 to 40% by mass, more preferably 10 to 30% by mass, and even more preferably 15 to 25% by mass, based on the total amount of monomers in the polymerizable composition.

[0043] The diallyl phthalate may be one or two selected from the group consisting of diallyl isophthalate and diallyl terephthalate.

[0044] The amount of diallyl phthalate to be blended is preferably 14 to 88% by mass, more preferably 20 to 70% by mass, and even more preferably 30 to 60% by mass, based on the total amount of monomers in the polymerizable composition.

[0045] Examples of alkyl methacrylates having an alkyl group with 1 to 4 carbon atoms include at least one selected from the group consisting of methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, iso-propyl methacrylate, n-butyl methacrylate, sec-butyl methacrylate, iso-butyl methacrylate, and tert-butyl methacrylate.

[0046] The amount of alkyl methacrylate to be added is preferably 1 to 6% by mass, more preferably 2 to 5% by mass, and even more preferably 3 to 5% by mass, based on the total amount of monomers in the polymerizable composition.

[0047] Examples of the radical initiator used in the polymerization include 1,1-azobiscyclohexane carbonate, diisopropyl peroxycarbonate, 1,1'-azobiscyclohexane nitrate, di-tert-butyl peroxide, etc. The amount of the radical initiator to be added is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 8 parts by mass, and even more preferably 1.0 to 5 parts by mass, relative to 100 parts by mass of the monomers in the polymerizable composition.

[0048] (Acrylic Resin) The acrylic resin is a cured product of a polymerizable composition containing an acrylic compound. The polymerizable composition may contain other monomers.

[0049] Examples of the acrylic compound include a polyfunctional (meth)acrylate compound having an aromatic ring, a polyalkylene glycol di(meth)acrylate, a monofunctional acrylate, etc. Among these, it is preferable to include a polyfunctional (meth)acrylate compound having an aromatic ring and a polyalkylene glycol di(meth)acrylate.

[0050] Examples of polyfunctional (meth)acrylate compounds having an aromatic ring include alkylene oxide-modified bisphenol A having (meth)acrylloyl groups at both terminals, and alkylene oxide-modified and urethane-modified bisphenol A having (meth)acrylloyl groups at both terminals. Among these, alkylene oxide-modified bisphenol A having (meth)acrylloyl groups at both terminals is preferred. Examples of alkylene oxide-modified bisphenol A having (meth)acrylloyl groups at both terminals include 2,2-bis[4-[2-((meth)acryloxy)ethoxy]phenyl]propane and 2,2-bis[4-[2-((meth)acryloxy)ethoxy]-3,5-dibromophenyl]propane.

[0051] The content of the polyfunctional (meth)acrylate compound having an aromatic ring in the polymerizable composition is preferably 40 to 90 mass %, more preferably 50 to 80 mass %, and even more preferably 55 to 70 mass % or more.

[0052] Examples of polyalkylene glycol di(meth)acrylates include diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, dibutylene glycol di(meth)acrylate, tributylene glycol di(meth)acrylate, and tetrabutylene glycol di(meth)acrylate.

[0053] The content of the polyalkylene glycol di(meth)acrylate in the polymerizable composition is preferably 10 to 60% by mass, more preferably 20 to 50% by mass, and even more preferably 30 to 45% by mass or more.

[0054] Examples of monofunctional (meth)acrylates include phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, 3-phenoxy-2-hydroxypropyl (meth)acrylate, 2-phenylphenyl (meth)acrylate, 4-phenylphenyl (meth)acrylate, 3-(2-phenylphenyl)-2-hydroxypropyl (meth)acrylate, 3-(4-phenylphenyl)-2-hydroxypropyl (meth)acrylate, 1-naphthyloxyethyl (meth)acrylate, 2-naphthyloxyethyl (meth)acrylate, 2,4,6-tribromophenyl (meth)acrylate, 2,4,6-tribromophenoxyethyl (meth)acrylate, 2,4,6-tribromophenyl-di(oxyethyl)-(meth)acrylate, and 2,4,6-tribromobenzyl (meth)acrylate.

[0055] When the polymerizable composition contains an acrylic compound, it preferably contains a radical polymerization initiator. Examples of the radical polymerization initiator include an energy ray-sensitive polymerization initiator and a heat-sensitive polymerization initiator.

[0056] The amount of the radical polymerization initiator added is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.5 to 3 parts by mass, relative to 100 parts by mass of the total amount of the acrylic compounds.

[0057] (Nitrogen-Containing Aromatic Polymer Resin) The nitrogen-containing aromatic polymer resin can be synthesized as a hyperbranched polymer having a melamine structure by, for example, polymerizing a resin obtained from a raw material containing cyanuric chloride and a triazine-based diamine, polymerizing cyanuric chloride and an aromatic diamine, polymerizing a triazine-containing aromatic triamine and triazine dichloride, or polymerizing an aromatic tricarboxylic acid and a triazine-containing aromatic diamine.

[0058] The substrate may contain other additives such as an ultraviolet absorber, a release agent, a colorant, an antioxidant, a refractive index adjuster, a birefringence adjuster, a coloring inhibitor, a fluorescent brightener, etc. These may be used alone or in combination of two or more.

[0059] The substrate preferably contains an ultraviolet absorber or an antioxidant. By containing an ultraviolet absorber or an antioxidant, the weather resistance of the resin substrate and the resin light guide plate can be improved, deterioration over time and yellowing can be prevented, and transparency during use can be maintained. Specifically, it is preferable to adjust the amount of the ultraviolet absorber or antioxidant so that the haze of the resin substrate or the resin light guide plate after a QUV accelerated weathering test is 1.8% or less.

[0060] Examples of ultraviolet absorbers include benzophenone compounds, benzotriazole compounds, dibenzoylmethane, and 4-tert-butyl-4'-methoxybenzoylmethane.

[0061] Examples of benzophenone compounds include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-n-octoxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, and 2,2'-dihydroxy-4-methoxybenzophenone.

[0062] Examples of benzotriazole compounds include 2-ethylhexyl 2-(2-hydroxy-4-ethoxyphenyl)-2H-benzotriazole-5-carboxylate, 2-(2-hydroxy-5-methylphenyl)-2H-benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chloro-2H-benzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chloro-2H-benzotriazole, 2-(2-hydroxy-3,5-di-tert-butyl-5-methylphenyl)-5-chloro-2H-benzotriazole, and benzotriazole compounds such as 2-(2-hydroxy-3,5-di-tert-butylphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)-2H-benzotriazole, and 2-(2-hydroxy-4-octyloxyphenyl)-2H-benzotriazole. These may be used alone or in combination of two or more.

[0063] The amount of the ultraviolet absorber added is preferably 0.01 to 5% by mass, more preferably 0.05 to 3% by mass, and even more preferably 0.1 to 2% by mass, based on the total amount of the substrate. Furthermore, by adding 0.01 to 5 parts by mass of a hindered amine light stabilizer together with the ultraviolet absorber, it is possible to prevent an increase in the haze value and a decrease in transparency when used as a light guide plate.

[0064] Examples of antioxidants include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants.

[0065] Examples of phenol-based antioxidants include 2,6-di-t-butyl-4-methylphenol and phenol. Examples of sulfur-based antioxidants include dilauryl 3,3'-thiodipropionate. Examples of phosphorus-based antioxidants include phosphite compounds such as triphenyl phosphite, trioctyl phosphite, and tridecyl phosphite. Antioxidants can be used alone or in combination of two or more.

[0066] The amount of antioxidant added is preferably 0.01 to 5% by mass, more preferably 0.05 to 3% by mass, and even more preferably 0.1 to 2% by mass, based on the total mass of the substrate.

[0067] The substrate preferably contains a refractive index adjuster. By containing a refractive index adjuster, even when a resin with a low refractive index is used, the refractive index of the resin light guide plate can be improved, thereby enabling a wider viewing angle. Examples of refractive index adjusters include inorganic particles. Examples of inorganic particle materials include silica, alumina, zirconia, titania, and zeolite. The inorganic particles are preferably surface-modified with a silane coupling agent, and preferably have a particle size of 100 nm or less. The particle size of the inorganic particles is preferably 5 to 40 nm, more preferably 10 to 35 nm, and even more preferably 10 to 30 nm. The particle size of the inorganic particles is the average particle size.

[0068] If the amount of refractive index adjuster added is large, the density of the material for the entire substrate increases, making it difficult to achieve a lightweight light guide plate. Furthermore, if inorganic particles are added as a refractive index adjuster at a ratio of 20 parts by mass or more per 100 parts by mass of the substrate resin, the fluidity of the resin itself decreases and internal stress occurs due to the orientation of the material, causing birefringence. Therefore, the amount of refractive index adjuster added is preferably 0.1 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.1 to 5 parts by mass per 100 parts by mass of the substrate resin.

[0069] The substrate preferably contains a birefringence adjuster. By containing a birefringence adjuster, it becomes easier to adjust the retardation value to 30 nm or less. Examples of birefringence adjusters include triazine-based birefringence adjusters and birefringence adjusters made of compounds having a fluorene skeleton. Examples of triazine-based birefringence adjusters include 2-hydroxyphenyl-s-triazine derivatives. Commercially available triazine-based birefringence adjusters include Tinuvin 1600, Tinuvin 460, Tinuvin 477, Tinuvin 479, and Tinuvin 1577 from BASF, and LA-F70 and LA46 from ADEKA.

[0070] The amount of birefringence adjuster added is preferably 1 to 30 parts by mass, more preferably 5 to 20 parts by mass, and even more preferably 10 to 15 parts by mass, per 100 parts by mass of the resin of the substrate.

[0071] The shape of the substrate of the light guide plate is not particularly limited, but may be a quadrilateral plate.

[0072] The flatness of the light guide plate substrate is preferably 25.0 μm or less, more preferably 20.0 μm or less, even more preferably 12.0 μm or less, and even more preferably 10.0 μm or less. The lower limit of the flatness is not particularly limited, but is, for example, 0.1 μm or more. The flatness is measured by measuring the flatness of one surface of the substrate, and tends to be higher when the substrate is curved or warped. The flatness can be measured using a flatness tester (FT-15) manufactured by Nidek Co., Ltd. By removing residual stress, it is possible to adjust the flatness value of the resin substrate or the light guide plate substrate to a smaller value.

[0073] The TTV of the substrate of the light guide plate is preferably 1 μm or less, more preferably 0.9 μm or less, and even more preferably 0.8 μm or less. The lower limit of the TTV is not particularly limited, but is, for example, 0.01 μm or more. TTV refers to the difference between the maximum and minimum values ​​of the thickness (i.e., the distance between the first surface 10 a and the second surface 10 b of the substrate of the light guide plate) (i.e., TTV (Total Thickness Variation)). TTV can be measured using a Bow / Warp measurement device SBW-331ML / d manufactured by Kobelco Research Institute, Ltd.

[0074] [Resin Substrate] The above-mentioned substrate may be prepared by molding a resin into a desired shape, or by cutting it out from a resin substrate. That is, the resin substrate according to this embodiment is a resin substrate for forming an optical member, and contains a resin, the thickness of the resin substrate is 0.1 to 1.5 mm, and the density of the resin is 0.93 to 2.10 g / cm. 3 The resin substrate has a refractive index of 1.60 or more, a retardation value of 30 nm or less, and, when the difference between the maximum and minimum values ​​of retardation measured on a line in one axial direction of the resin substrate is A and the difference between the maximum and minimum values ​​of retardation measured on a line in a direction substantially perpendicular to the one axial direction is B, the relationship of the following formula (1) is satisfied: A / B<3.5 (1)

[0075] The examples and preferred ranges of the resin, additive, thickness, density, refractive index, retardation value, A / B, and flatness of the resin substrate according to this embodiment are the same as those of the substrate described above, and therefore will not be described here. However, the retardation value and the range of A / B are within the ranges described in the examples.

[0076] The resin substrate according to this embodiment may have a disk-like shape, but is not particularly limited thereto. The diameter of the disk is also not particularly limited, but may be, for example, 50 mm to 450 mm, or 60 mm to 150 mm. The resin substrate according to this embodiment may have a shape that does not have a base curve, such as a convex or concave surface, like a lens substrate, and may be, for example, a flat plate shape.

[0077] The resin substrate according to this embodiment will now be described in more detail. Fig. 2 is a diagram showing the outline of the resin substrate according to this embodiment. The resin substrate 100 has a disk shape. A base material 10 of a light guide plate is cut out from the resin substrate 100 and used.

[0078] The resin substrate according to this embodiment can be produced by, for example, a cast polymerization method in which a resin substrate is obtained by cast-polymerizing a polymerizable composition, or an injection molding method in which a molten resin is injected into a mold.

[0079] As shown in FIG. 3 , in the case of the cast polymerization method, the method for producing a resin substrate includes a cast polymerization step of obtaining a resin substrate by cast-polymerizing a polymerizable composition, and may further include a slicing step of slicing the resin substrate to obtain resin substrates having a desired thickness. The method may also include an annealing step of removing residual stress by heat treatment and a polishing step of polishing the resin substrate with a polishing device, for the purposes of providing the resin substrate with predetermined roughness and flatness and further reducing variations in the distribution of residual stress.

[0080] Specifically, a resin substrate raw material liquid is poured into a cavity formed by two molds arranged at a predetermined distance. A resin substrate is formed by a curing reaction of the raw material liquid, and then released from the mold. The released resin substrate is then sliced ​​to a predetermined thickness of 0.3 to 2.0 mm using a wire saw, and then polished with a polishing device with sufficient removal allowance until the wire saw marks disappear, resulting in a resin substrate with a thickness of 0.1 to 1.5 mm. Note that the released resin substrate may be cut at its periphery to create a smooth surface, if necessary, and then sliced ​​with a wire saw.

[0081] The polishing device may be any device capable of polishing without imparting anisotropy to the substrate surface, and specifically, a lapping device is preferably used. A resin substrate is placed on a flat surface plate, and a slurry such as alumina or silica is poured onto the surface plate. The surface plate and the resin substrate are rotated relative to each other while being pressed with a predetermined pressure, thereby removing scratches and residual stress from the resin substrate surface. Either a single-sided polishing device or a double-sided polishing device can be used to polish resin substrates. These devices can uniformly remove wire saw marks and other processing marks and residual stresses on both sides of the substrate, thereby minimizing flatness.

[0082] By the above steps, a resin substrate having a retardation value within a desired range and an A / B ratio within a desired range can be manufactured.

[0083] As shown in FIG. 4, in the case of an injection molding method, the manufacturing method of a resin substrate includes an injection molding step in which a thermoplastic molten resin is injected into a mold to obtain a resin substrate. The resin substrate may also include an annealing step in which the resin substrate is annealed to achieve a predetermined dimensional accuracy and flatness, and to reduce variations in the distribution of residual stress. Specifically, to form a resin substrate, molten resin is injected into a cavity having a predetermined shape and cooled in the mold. The resin substrate is then removed from the mold and annealed to remove residual stress. The annealing conditions can be set appropriately depending on the type of resin used. Depending on the type of resin, the annealing treatment may be performed at a temperature above the glass transition temperature and below the melting point, for example, at 120 to 210°C for 3 to 20 hours, followed by cooling for a time equal to or longer than the heating time, thereby reducing internal strain and removing residual stress. The resin substrate may then be shaped by surface polishing.

[0084] By the above steps, a resin substrate having a retardation value within a desired range and an A / B ratio within a desired range can be manufactured.

[0085] A substrate to be used for a light guide plate is cut out from the resin substrate according to this embodiment.

[0086] The light guide plate according to this embodiment is used in an augmented reality (AR) wearable device, etc. More specifically, the light guide plate according to this embodiment is used in an eyewear optical member (for example, a spectacle lens type display display unit) used in a wearable device.

[0087] [Optical Component for Eyewear] The optical component for eyewear according to this embodiment includes a resin light-transmitting substrate and the light guide plate according to this embodiment. At least one of the light guide plates is integrally held in the light guide plate. The refractive index (RW) of the light guide plate is greater than the refractive index (RT) of the light-transmitting substrate. The difference (RW - RT) between the refractive index (RW) of the light guide plate and the refractive index (RT) of the light-transmitting substrate is preferably 0.2 to 1.0, more preferably 0.3 to 0.8, and even more preferably 0.3 to 0.5.

[0088] The term "translucent substrate" refers to a substrate through which the opposite surface can be seen.

[0089] The eyewear optical component is not particularly limited as long as it is applicable to wearable devices, but may be, for example, a spectacle lens applied to a spectacle-type wearable device. In this case, the light-transmitting substrate has the shape of a spectacle lens substrate. The spectacle lens substrate does not necessarily have to have a spherical surface, but may be a flat plate shaped to fit into a spectacle frame.

[0090] [Wearable Device] An example of a wearable device using the light guide plate according to this embodiment is a head-mounted display. The head-mounted display includes, for example, a spectacle-type frame worn on the head of a wearer and an eyewear optical element according to this embodiment attached to the frame. The spectacle-type frame may be equipped with a backlight for illuminating images, a signal processing device for displaying images, a speaker for reproducing sound, and the like.

[0091] As described above, the present disclosure provides the following embodiments. <1> A resin substrate for forming an optical element, the resin substrate having a thickness of 0.1 to 1.5 mm, and a density of the resin of 0.93 to 2.10 g / cm 3A resin substrate having a refractive index of 1.60 or more, a retardation value of 30 nm or less, and satisfying the relationship of the following formula (1), where A is the difference between the maximum and minimum values ​​of retardation measured on a straight line in one axial direction of the resin substrate, and B is the difference between the maximum and minimum values ​​of retardation measured on a straight line in a direction approximately perpendicular to the one axial direction. A / B≦3.5 (1) <2> 0.75 W / m 2 The resin substrate according to <1>, wherein the haze of the resin substrate after a 200-hour accelerated weathering test consisting of a cycle of 5 hours of UV light irradiation and 5 hours of humid 95% RH is 1.8% or less. <3> The resin substrate according to <1> or <2>, wherein the ratio (R / D) of the refractive index (R) of the resin substrate to the density (D) of the resin substrate is 1.00 to 1.30. <4> The resin substrate according to any one of <1> to <3>, wherein the resin contains at least one resin selected from the group consisting of urethane-based resins, episulfide resins, polycarbonate resins, acrylic resins, epoxy resins, and nitrogen-containing aromatic polymer resins. <5> The resin substrate according to any one of <1> to <4>, wherein the resin substrate contains an ultraviolet absorber or an antioxidant. <6> The resin substrate according to any one of <1> to <5>, wherein the resin substrate contains a refractive index adjuster. <7> The resin substrate according to any one of <1> to <6>, wherein the resin substrate contains a birefringence adjuster. <8> The resin substrate according to any one of <1> to <7>, wherein the resin substrate is a disk. <9> The resin substrate according to any one of <1> to <8>, wherein the resin substrate has a flatness of 25.0 μm or less. <10> A resin substrate comprising: a substrate containing resin; and a diffraction grating formed on at least a part of the substrate, wherein the thickness of the substrate is 0.1 to 1.5 mm, and the density of the resin is 0.93 to 2.10 g / cm. 3A light guide plate, wherein the refractive index of the substrate is 1.60 or more, the retardation value of the substrate is 30 nm or less, and the relationship of the following formula (1) is satisfied, where A is the difference between the maximum and minimum values ​​of retardation measured on a line in one axial direction of the substrate, and B is the difference between the maximum and minimum values ​​of retardation measured on a line in a direction approximately perpendicular to the one axial direction. A / B≦3.5 (1) <11> 0.75 W / m 2 The light guide plate according to <10>, wherein the haze of the light guide plate after 200 hours of accelerated weathering testing, which includes a cycle of 5 hours of UV light irradiation and 5 hours of humid 95% RH, is 1.8% or less. <12> The light guide plate according to <10> or <11>, wherein the ratio (R / D) of the refractive index (R) of the substrate to the density (D) of the substrate is 1.00 to 1.30. <13> The light guide plate according to any one of <10> to <12>, wherein the resin includes at least one selected from the group consisting of urethane resins, episulfide resins, polycarbonate resins, acrylic resins, epoxy resins, and nitrogen-containing aromatic polymer resins. <14> The light guide plate according to any one of <10> to <13>, wherein the substrate contains an ultraviolet absorber or an antioxidant. <15> The light guide plate according to any one of <10> to <14>, wherein the substrate contains a refractive index adjuster. <16> The light guide plate according to any one of <10> to <15>, wherein the substrate contains a birefringence adjuster. <17> The light guide plate according to any one of <10> to <16>, wherein the substrate has a flatness of 25.0 μm or less. <18> An eyewear optical element comprising: a resin light-transmitting substrate; and the light guide plate according to any one of <10> to <17>, wherein at least one light guide plate is integrally held by the light-transmitting substrate, and wherein a refractive index (RW) of the light guide plate is greater than a refractive index (RT) of the light-transmitting substrate. <19> A wearable device comprising the eyewear optical element according to <18>.

[0092] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the following examples.

[0093] [Retardation Value] The retardation value of the resin substrate or light guide plate substrate was measured using a birefringence measurement device PA100 manufactured by Photonic Lattice Co., Ltd. <Light Guide Plate> The retardation value is obtained by drawing a circle centered on the centroid of the shape represented by the periphery of the resin light guide plate, drawing a circle tangent to the periphery, and calculating the average retardation value measured within the circle. <Resin Substrate> The retardation value of the resin substrate is measured within an area excluding the periphery of the resin substrate. For example, as shown in Figure 5, the retardation value is obtained by drawing a circle centered on the centroid A of the shape represented by the periphery O of the resin substrate (if the periphery of the resin substrate is circular, the circle centered on the centroid coincides with the periphery of the resin substrate), drawing a concentric circle C inside the circle whose diameter is 90% of the original length, and calculating the average retardation value measured within the inner concentric circle. The reason why the values ​​obtained within the range of the inner concentric circle are used as described above is that the outer periphery of the resin substrate is prone to residual stress during molding and processing, resulting in locally high retardation values. On the other hand, since the resin substrate is cut out from it and used as a resin light guide plate, the outer periphery of the resin substrate is not used as a resin light guide plate and is discarded, so there is no need to consider the retardation value.

[0094] [Method for Measuring A / B] The retardation distribution A / B was measured using the following method. Measurements were made along two lines α and β that intersect approximately at right angles at the center of gravity (centroid) of the resin substrate or light guide plate substrate. The center of gravity is determined by drawing two lines that bisect the area of ​​the plan view, assuming the thickness and density of the substrate are constant, and their intersection is the center of gravity (centroid). Here, "approximately perpendicular" refers to an angle range of 90°±5°. This assumes that it may be difficult to align the measurement reference lines perfectly perpendicularly depending on the settings of the measurement equipment, and measurements were made at any position within this range. The retardation values ​​for the line α and the line α that pass through the center of gravity were measured within the range inside the intersection with the outer periphery of the resin substrate or light guide plate substrate. <Resin Substrate> Measurements were made according to the following criteria for resin substrates. As shown in Figure 5, when the length of the line segments between the intersections of lines α and β with the periphery of the resin substrate is set to 100, the difference A between the maximum and minimum values ​​of line α and the difference B between the maximum and minimum values ​​of line β are calculated from the values ​​measured within a 75% length range from the centroid. Lines α and β can be drawn at any position as long as they intersect at the center of gravity, and the value at the point where A / B is largest is taken as the value of A / B. However, A > B must be satisfied. Therefore, the value of A / B is preferably closer to 1 within the range of 1 to 3.5 (which reduces the variation and distribution of retardation values ​​in the substrate and light guide plate). The measurement range is set to 90% from the center of gravity because birefringence due to external stress is likely to occur near the periphery, making it difficult to obtain accurate measurements. This is why the variation in retardation distribution is evaluated by excluding this area. Furthermore, while high residual stress due to processing occurs particularly near the periphery of the resin substrate, when a light guide plate is cut out of the resin substrate and used, this area is cut and removed and therefore not used, so it is not subject to evaluation. <Light guide plate> The light guide plate was measured according to the following criteria: For a rectangular light guide plate, lines α and β were drawn at the center of gravity, and the value at the point where A / B was the largest was taken as the value of A / B, provided that A>B was satisfied.

[0095] [Haze] According to JIS K 7373:2006, the haze was measured by irradiating the sample with UV light for 4 hours (0.20 W / m) using a QUV accelerated weathering tester QUV / SE (manufactured by Q-LAB).2 The resin substrate and the resin light guide plate were subjected to an accelerated weathering test for 168 hours, with a cycle of 4 hours at room temperature and 95% RH. The haze of the resin substrate and the resin light guide plate was measured in accordance with JIS K7136.

[0096] Example 1: A polymerizable composition for a resin substrate (a polymerizable composition containing raw materials for a polythiourethane resin) was injected into a cavity formed by two molds spaced apart at a predetermined distance. The resin substrate was formed by a curing reaction of the raw material liquid and then released from the mold. The released resin substrate was then sliced ​​using a wire saw to obtain multiple resin substrates with a thickness of 1.1 mm. To remove residual stress caused by slicing due to scratches during processing, the multiple resin substrates were stacked with spacers interposed between them and annealed at 170°C for 3 hours. Subsequently, the resin substrates were polished to a predetermined retardation value using a double-side lapping machine at a pressure of 6 kPa using an alumina slurry with an average particle size of 0.5 μm. A 1.0 mm-thick resin substrate was formed using the above method. The refractive index of the resin substrate was 1.67 and the density was 1.34 g / cm. 3 The flatness of the resin substrate was 3.5 μm, and the TTV of the resin substrate was 0.8 μm. The haze value before the accelerated weathering test was 0.3%, and the haze value after the accelerated weathering test was 1.5%.

[0097] [Example 2] A resin substrate having a thickness of 1.0 mm was formed in the same manner as in Example 1, except that the average particle size of the alumina slurry was 1.0 μm and the pressure during polishing was 4 kPa. The flatness of the resin substrate was 10.8 μm, and the total thickness variation (TTV) of the resin substrate was 0.8 μm.

[0098] [Example 3] A resin substrate having a thickness of 1.0 mm was formed in the same manner as in Example 1, except that the average particle size of the alumina slurry was 1.0 μm, the pressure during polishing was 5 kPa, and the rotation speed of the platen of the polishing apparatus was set to 1.2 times that of Example 1. The flatness of the resin substrate was 18.2 μm, and the TTV of the resin substrate was 0.9 μm.

[0099] [Example 4] A resin substrate having a thickness of 1.0 mm was formed in the same manner as in Example 1, except that the average particle size of the alumina slurry was set to 5.0 μm, the pressure during polishing was set to 6 kPa, and the rotation speed of the platen of the polishing apparatus was set to 1.3 times that of Example 1. The flatness of the resin substrate was 24.3 μm, and the TTV of the resin substrate was 1.0 μm.

[0100] A resin substrate having a thickness of 1.0 mm was formed in the same manner as in Example 1, except that the average particle size of the alumina slurry was 8.0 μm, the pressure during polishing was 2 kPa, and the rotation speed of the platen of the polishing apparatus was set to 1.1 times that of Example 1. The flatness of the resin substrate was 27.5 μm, and the TTV of the resin substrate was 1.0 μm.

[0101] Comparative Example 2 A resin substrate having a thickness of 1.0 mm was formed in the same manner as in Example 1, except that the average particle size of the alumina slurry was 5.0 μm, the pressure during polishing was 6 kPa, the rotation speed of the platen of the polishing apparatus was set to 1.3 times that of Example 1, and no annealing treatment was performed. The flatness of the resin substrate was 28.1 μm, and the TTV of the resin substrate was 1.3 μm.

[0102]

[0103] In Examples 1 and 2, the retardation value of the resin substrate and the A / B value, which is the variation in the retardation distribution, are both low values, and when used as a light guide plate, there is no bleeding or blurring of the image contours, and no dark areas occur in parts of the image, resulting in good light guide properties with no uneven brightness.

[0104] In Example 3, slight blurring of the image is observed compared to Examples 1 and 2, but there is no unevenness in brightness and a clear image can be displayed.

[0105] In Example 4, as in Example 3, slight bleeding was observed in the image, and it was also confirmed that dark areas were generated in parts of the image.

[0106] In Comparative Example 1, the residual stress on the surface of the resin substrate was not sufficiently removed, so the retardation value exceeded the predetermined range, and it was confirmed that this caused blurring at the contours of the image.

[0107] In Comparative Example 2, the wire saw marks could not be sufficiently removed by polishing, and therefore residual stress caused by the wire saw marks during slicing remains in the form of streaks in a certain direction, resulting in uneven brightness and dark areas in some parts of the image.

[0108] Example 5 To form a resin substrate, a molten thermoplastic resin (acrylic resin with 3 parts by weight of a hindered amine-based light stabilizer and 5 parts by weight of a phenol-based antioxidant added) was injected into a cavity having a predetermined shape. The mold was allowed sufficient time to cool, with the initial temperature set to 80°C. 150 seconds after injection, the mold temperature was lowered using water cooling so that the molded product would be below the ejection temperature. After removal from the mold, the product was annealed to remove residual stress. The annealing conditions can be adjusted appropriately depending on the resin material. For example, heating at 150°C for 3 hours followed by cooling for a period longer than the heating time reduced internal strain and removed residual stress. The surface was then polished to a desired shape, resulting in a 1.0 mm thick resin substrate. The resin substrate had a refractive index of 1.60 and a density of 1.25 g / cm. 3 The flatness of the resin substrate was 5.8 μm, and the TTV of the resin substrate was 0.7 μm. The haze value before the accelerated weathering test was 0.25%, and the haze value after the accelerated weathering test was 0.8%.

[0109] Example 6 A resin substrate having a thickness of 1.0 mm was prepared by injection molding in the same manner as in Example 5, except that titanium oxide particles having an average particle size of 40 nm were added to 100 parts by weight of the thermoplastic resin in an amount of 15 parts by weight. The refractive index of the resin substrate was 1.67 and the density was 1.47 g / cm. 3 The flatness of the resin substrate was 9.7 μm, and the total thickness variation (TTV) of the resin substrate was 0.9 μm.

[0110] Example 7 A resin substrate having a thickness of 1.0 mm was prepared by injection molding in the same manner as in Example 5, except that titanium oxide particles having an average particle size of 40 nm were added to 100 parts by weight of the thermoplastic resin in an amount of 50 parts by weight. The refractive index of the resin substrate was 1.76 and the density was 1.77 g / cm. 3 The flatness of the resin substrate was 16.8 μm, and the total thickness variation (TTV) of the resin substrate was 0.8 μm.

[0111] Comparative Example 3: A resin substrate having a thickness of 1.0 mm was prepared by injection molding in the same manner as in Example 5, except that titanium oxide particles having an average particle size of 40 nm were added in an amount of 30 parts by weight per 100 parts by weight of thermoplastic resin. The resin substrate had a flatness of 21.5 μm and a total thickness variation (TTV) of 1.2 μm.

[0112]

[0113] In Examples 5 to 7, the retardation value of the resin substrate is reduced by annealing. However, the fluidity and orientation are affected by the resin and its additives used in injection molding, and the A / B value, which represents the variation in the retardation distribution, increases.

[0114] Therefore, when the resin substrate in Example 5, which is made of a thermoplastic resin to which titanium oxide, a refractive index adjuster, is not added, is used as a light guide plate, there is no bleeding or blurring of the image contours, and furthermore, there is no occurrence of dark areas in parts of the image, and good light guiding properties with no unevenness in brightness can be obtained. On the other hand, it can be confirmed that in Examples 6 and 7, dark areas are generated in parts of the image, causing unevenness in brightness.

[0115] In Comparative Example 3, since no annealing treatment was performed, it can be seen that blurring occurs at the contours of the image, brightness unevenness occurs, and dark areas appear in parts of the image.

[0116] REFERENCE SIGNS LIST 1 light guide plate 10 substrate 24 image display device 32, 52 diffraction grating

Claims

1. A resin substrate for forming an optical member, comprising a resin, the thickness of the resin substrate being 0.1 to 1.5 mm, and the density of the resin being 0.93 to 2.10 g / cm 3 A resin substrate having a refractive index of 1.60 or more, a retardation value of 30 nm or less, and satisfying the relationship of the following formula (1), where A is a difference between the maximum and minimum values ​​of retardation measured on a straight line in one axial direction of the resin substrate, and B is a difference between the maximum and minimum values ​​of retardation measured on a straight line in a direction approximately perpendicular to the one axial direction. A / B≦3.5 (1) 2. 0.75 W / m 2 2. The resin substrate according to claim 1, wherein the haze of the resin substrate after 200 hours of accelerated weathering test with a cycle of 5 hours of UV light exposure and 5 hours of humid 95% RH is 1.8% or less.

3. The resin substrate according to claim 1, wherein the ratio (R / D) of the refractive index (R) of the resin substrate to the density (D) of the resin substrate is 1.00 to 1.

30.

4. The resin substrate according to claim 1, wherein the resin comprises at least one selected from the group consisting of urethane resins, episulfide resins, polycarbonate resins, acrylic resins, epoxy resins, and nitrogen-containing aromatic polymer resins.

5. The resin substrate according to claim 1, further comprising an ultraviolet absorbing agent or an antioxidant.

6. The resin substrate according to claim 1, wherein the resin substrate contains a refractive index adjusting agent.

7. The resin substrate according to claim 1, wherein the resin substrate contains a birefringence adjusting agent.

8. The resin substrate according to claim 1, wherein the resin substrate is a disk.

9. The resin substrate according to claim 1, wherein the flatness of the resin substrate is 25.0 μm or less.

10. A method for manufacturing a diffraction grating comprising the steps of: a substrate containing a resin; and a diffraction grating formed on at least a part of the substrate, the substrate having a thickness of 0.1 to 1.5 mm, and the resin having a density of 0.93 to 2.10 g / cm. 3A light guide plate in which the refractive index of the substrate is 1.60 or more, the retardation value of the substrate is 30 nm or less, and, when the difference between the maximum and minimum values ​​of retardation measured on a line in one axial direction of the substrate is A and the difference between the maximum and minimum values ​​of retardation measured on a line in a direction approximately perpendicular to the one axial direction is B, the relationship of the following formula (1) is satisfied: A / B≦3.5 (1) 11. 0.75 W / m 2 11. The light guide plate of claim 10, wherein the haze of the light guide plate is 1.8% or less after 200 hours of accelerated weathering with cycles of 5 hours UV light exposure and 5 hours humid 95% RH.

12. The light guide plate according to claim 10, wherein the ratio (R / D) of the refractive index (R) of the substrate to the density (D) of the substrate is 1.00 to 1.

30.

13. The light guide plate according to claim 10, wherein the resin includes at least one selected from the group consisting of urethane resins, episulfide resins, polycarbonate resins, acrylic resins, epoxy resins, and nitrogen-containing aromatic polymer resins.

14. The light guide plate according to claim 10, wherein the substrate contains an ultraviolet absorbing agent or an antioxidant.

15. The light guide plate according to claim 10, wherein the substrate contains a refractive index adjusting agent.

16. The light guide plate according to claim 10, wherein the substrate contains a birefringence adjusting agent.

17. The light guide plate according to claim 10, wherein the flatness of the substrate is 25.0 μm or less.

18. An optical component for eyewear, comprising: a resin translucent substrate; and a light guide plate according to any one of claims 10 to 17, wherein at least one of the light guide plates is integrally held by the light-transmitting substrate, and the refractive index (RW) of the light guide plate is greater than the refractive index (RT) of the light-transmitting substrate.

19. A wearable device comprising the eyewear optical member according to claim 18.

Citation Information

Patent Citations

  • Light guide plate

    JP2022097824A

  • Multi-layer diffractive eyepiece

    JP2019528474A

  • Image display light guide plate

    JP2020126239A

  • Resin light guide body for head mount display

    JP2021162621A

  • Wearable devices

    JP2021504760A