Fluorine resin composition, molded body, and production method for fluorine resin composition

The fluororesin composition, combining thermally treated and untreated PTFE, achieves enhanced compressive strength and workability by controlling metal impurities, addressing the compressive strength issues in PTFE molded articles.

WO2024248095A1PCT designated stage expired Publication Date: 2024-12-05AGC INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019895
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing methods for producing fluororesin molded articles using polytetrafluoroethylene (PTFE) result in products with inferior compressive strength due to the inclusion of metal impurities from thermal history, making reuse difficult and affecting mechanical properties.

Method used

A fluororesin composition comprising a first fluororesin with a thermal history heated above its melting point and a second fluororesin without such history, both being non-melt moldable, is compression molded and fired at 380°C for 2 hours, with a metal elution limit of 5 ng/g or less to enhance compressive strength and workability.

Benefits of technology

The approach results in molded articles with improved compressive strength and recycling efficiency by minimizing metal impurities, thereby overcoming the limitations of previous methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

A fluorine resin composition according to the present invention includes a first fluorine resin that has a heat history of being heated to at least the melting point thereof and a second fluorine resin that does not have a heat history of being heated to at least the melting point thereof. The first fluorine resin and the second fluorine resin are non-melt-moldable resins. When a preliminary molded body obtained by compression molding the fluorine resin composition is fired for at least 2 hours at 380°C to make a micro-dumbbell-shaped test piece that is 16×45 mm and 0.5 mm thick and the test piece is left for 24 hours at 23°C in 3.6 mass% hydrochloric acid, the metal elution amount relative to the total mass of the test piece is no more than 5 ng / g.
Need to check novelty before this filing date? Find Prior Art

Description

Fluororesin composition, molded article, and method for producing fluororesin composition

[0001] The present invention relates to a fluororesin composition, a molded article, and a method for producing a fluororesin composition. This application claims priority to Japanese Patent Application No. 2023-091850, filed on June 2, 2023, the contents of which are incorporated herein by reference.

[0002] Polytetrafluoroethylene resin (molding powder) obtained by suspension polymerization of tetrafluoroethylene (TFE) is compression molded and then sintered to form a molded body. The molded body obtained by sintering is processed into a molded product of the desired shape by cutting or other processes. However, once-sintered polytetrafluoroethylene resin (sintered PTFE) such as cutting chips generated during processing is hard, and even if it is crushed and compressed, it does not come together and cannot be molded. For this reason, it has been difficult to reuse it.

[0003] Patent Document 1 describes that when a powder of sintered PTFE is mixed with a PTFE dispersion (a dispersion of unsintered PTFE) obtained by emulsion polymerization of TFE, and the mixture is compression-molded and sintered to produce a molded body, the porosity after sintering decreases and the tensile strength after sintering increases as the mixing ratio of unsintered PTFE increases. For example, the document describes an example in which the porosity after sintering becomes 0% when the mixing ratio of unsintered PTFE is 100%.

[0004] Patent No. 6612001

[0005] However, when the present inventors conducted an investigation using the method described in Patent Document 1, it was confirmed that the resulting molded body had inferior compressive strength compared to a molded body produced using only the molding powder.

[0006] An object of the present invention is to provide a fluororesin composition which can give a molded article having high compressive strength and excellent processability even when using a fluororesin having a thermal history of being heated to or above its melting point, a molded article of the fluororesin composition, and a method for producing the fluororesin composition.

[0007] The present invention has the following aspects. [1] A fluororesin composition comprising a first fluororesin having a thermal history of being heated to or above its melting point, and a second fluororesin having no thermal history of being heated to or above its melting point, wherein the first fluororesin and the second fluororesin are non-melt-formable fluororesins, and the fluororesin composition is compression-molded to obtain a preform, which is baked at 380°C for 2 hours or more to form a microdumbbell-shaped test piece having a thickness of 0.5 mm and a size of 16 mm x 45 mm. When the test piece is allowed to stand in 3.6 mass% hydrochloric acid at 23°C for 24 hours, the test piece has a metal elution amount of 5 ng / g or less relative to the total mass of the test piece. [2] The fluororesin composition according to [1], wherein the first fluororesin has tetrafluoroethylene units, and the content of the tetrafluoroethylene units relative to the total mass of the first fluororesin is 99 mass% or more. [3] The fluororesin composition according to [1] or [2], wherein the second fluororesin has tetrafluoroethylene units, and the content of the tetrafluoroethylene units relative to the total mass of the second fluororesin is 99 mass% or more. [4] The fluororesin composition according to any of [1] to [3], wherein the content of the first fluororesin relative to the total mass of the first fluororesin and the second fluororesin is 10 mass% or more. [5] A molded product of the fluororesin composition according to any of [1] to [4]. [6] A method for producing the fluororesin composition according to any of [1] to [4], comprising washing a mixture containing the first fluororesin and the second fluororesin.

[0008] According to the present invention, it is possible to provide a fluororesin composition which can give a molded article having high compressive strength and excellent processability even when using a fluororesin having a thermal history of being heated to or above its melting point, a molded article of the fluororesin composition, and a method for producing the fluororesin composition.

[0009] The following definitions of terms apply throughout the present specification and claims. "Monomer-based unit" is a collective term for an atomic group formed directly by polymerization of one monomer molecule and an atomic group obtained by chemically converting a portion of the atomic group. In this specification, a monomer-based unit is also simply referred to as a monomer unit. "Monomer" means a compound having a polymerizable carbon-carbon double bond. "Melting point" means the temperature corresponding to the maximum value of the melting peak measured by differential scanning calorimetry (DSC). The "to" symbol indicating a range of values ​​means that the values ​​before and after it are included as the lower and upper limits. "Average particle size" means the 50% cumulative value (median diameter, D50) in the number-based particle size distribution determined using a laser diffraction / scattering particle size distribution analyzer (e.g., HORIBA, Ltd., LA-920 measuring instrument). "Melt-moldable" means exhibiting melt fluidity. "Exhibiting melt fluidity" means that there is a temperature at which the melt flow rate is 0.1 to 1000 g / 10 min at a temperature 20°C or more higher than the melting point of the resin under a load of 49 N. "Melt flow rate" refers to the melt mass flow rate (MFR) defined in JIS K 7210:1999 (ISO 1133:1997). "Non-melt moldable" means that the material does not exhibit the melt fluidity. "Standard specific gravity (hereinafter also referred to as "SSG")" is a value that serves as an index of average molecular weight, with a larger value indicating a smaller molecular weight. It can be measured in accordance with ASTM D1457-91a and D4895-91a. The amount of metal elution can be measured by inductively coupled plasma mass spectrometry.

[0010] <Fluororesin Composition> The fluororesin composition of this embodiment comprises a first fluororesin (hereinafter also referred to as "fluororesin 1") that has a thermal history of being heated to or above its melting point, and a second fluororesin (hereinafter also referred to as "fluororesin 2") that does not have a thermal history of being heated to or above its melting point. Fluororesin 1 and fluororesin 2 are non-melt-formable fluororesins. A preform obtained by compression molding the fluororesin composition is baked at 380°C for 2 hours or more to form a microdumbbell-shaped test piece having a thickness of 0.5 mm and a size of 16 mm x 45 mm. The test piece is left to stand in 3.6 mass% hydrochloric acid at 23°C for 24 hours, and the amount of metal elution relative to the total mass of the test piece is 5 ng / g or less.

[0011] The amount of metal elution is 5 ng / g or less, preferably 2 ng / g or less, and more preferably 1 ng or less. The lower limit of the amount of metal elution is not particularly limited, but may be 0 ng / g, or may be, for example, 0.01 ng / g or more, or 0.1 ng / g or more. The upper limit and the lower limit can be arbitrarily combined. When the amount of metal elution is the upper limit or less, the compressive strength of the obtained molded body is likely to be improved. Examples of metals include iron, chromium, nickel, and copper.

[0012] <Non-melt-formable fluororesin> Both fluororesin 1 and fluororesin 2 are non-melt-formable fluororesins. Fluororesin 1 and fluororesin 2 may be the same or different. Fluororesin 1 and fluororesin 2 may each independently be one type of fluororesin, or two or more types of fluororesins may be used in combination. When two or more types of fluororesins are used in combination, it is sufficient that the mixture of the two or more types of fluororesins is non-melt-formable.

[0013] As the fluororesin 1 and the fluororesin 2, a polymer having a tetrafluoroethylene unit (hereinafter also referred to as a "TFE unit") is preferable, and examples thereof include polytetrafluoroethylene (PTFE), a tetrafluoroethylene-ethylene copolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, a tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer, a tetrafluoroethylene-chlorotrifluoroethylene copolymer, a tetrafluoroethylene-ethylene-hexafluoropropylene copolymer, and a tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer.

[0014] Preferably, fluororesin 1 and fluororesin 2 are each independently PTFE. The content of TFE units in PTFE relative to the total mass of the fluororesin is preferably 99% by mass or more. The content of TFE units relative to the total mass of PTFE is more preferably 99.5% by mass or more, and may be 100% by mass.

[0015] Examples of the monomer units other than the TFE units include the above-mentioned ethylene units, hexafluoropropylene units, perfluoro(alkyl vinyl ether) units, chlorotrifluoroethylene units, vinylidene fluoride units, as well as monomer units based on perfluoro(2,2-dimethyl-1,3-dioxole), perfluoro(4-methoxy-1,3-dioxole), perfluoroalkylethylene, etc. The monomer units other than the TFE units may be one type or two or more types. By including monomer units other than the TFE units, the crystallization of PTFE is suppressed to some extent, and the tensile strength, tensile elongation, dielectric breakdown resistance, creep resistance, etc. are improved.

[0016] (Fluororesin 1) Fluororesin 1 has a thermal history of being heated to or above its melting point at least once. Fluororesin 1 can be obtained by pulverizing cuttings generated when a primary molded body produced by heating to or above its melting point is processed into a secondary molded body such as an industrial part of a desired shape, or by pulverizing an unnecessary secondary molded body. The pulverization can be performed using a pulverizer or the like. After coarse pulverization, the material may be further pulverized. An example of the heating is heating by firing required for producing a molded body. By heating to or above its melting point, the melting point of fluororesin 1 is lowered below the melting point of fluororesin 1 before being heated to or above its melting point. The fact that "has a thermal history of being heated to or above its melting point at least once" can be confirmed by differential scanning calorimetry (DSC).

[0017] The melting point of fluororesin 1 before being heated to or above its melting point is preferably 360°C or lower, more preferably 355°C or lower, and even more preferably 350°C or lower. There are no particular restrictions on the lower limit of the melting point, but it is preferably 100°C or higher, and more preferably 150°C or higher. The melting point is preferably 100 to 360°C, more preferably 100 to 355°C, and even more preferably 150 to 350°C. When the melting point is within the above range, the mechanical strength of the resulting molded article is likely to be improved.

[0018] The melting point of fluororesin 1 is preferably 335°C or lower, more preferably 330°C or lower. There is no particular limitation on the lower limit of the melting point, but it is preferably 100°C or higher, more preferably 150°C or higher. The melting point is preferably 100 to 335°C, more preferably 150 to 330°C. When the melting point is within the above range, the mechanical strength of the obtained molded article is likely to be improved.

[0019] The bulk density of fluororesin 1 is preferably 100 g / L or more, more preferably 105 g / L or more, and even more preferably 110 g / L or more. When the bulk density is equal to or greater than the lower limit, less air is carried over during the production of a molded body, resulting in excellent deaeration properties and good fusion between powder particles. Furthermore, voids are less likely to remain in the resulting molded body, and the uniformity of the molded body is also likely to be improved.

[0020] The average particle size of the fluororesin 1 is preferably 1 to 500 μm, more preferably 5 to 300 μm, and even more preferably 5 to 100 μm. When the average particle size of the fluororesin 1 is within the above range, the uniformity of the obtained molded article is improved.

[0021] The fluororesin 1 may be, for example, crushed pieces of a molded product obtained by a method including a step of heating a molding material containing PTFE obtained by suspension polymerization to above its melting point. PTFE obtained by suspension polymerization has an extremely high melt viscosity and exhibits non-melt moldability, which means that it cannot be molded by general thermoplastic resin molding methods such as extrusion molding and injection molding. Therefore, when molding PTFE produced by suspension polymerization (hereinafter also referred to as "molding powder"), a method is used in which the molding powder is filled into a mold, compression molded, and then sintered.

[0022] Specifically, the molding powder is molded by first filling a mold with the molding powder at room temperature and compression-molding it to form a preform, which is then heated to or above the melting point of PTFE for sintering to form a primary molded body. The molding powder may be granulated as needed and used as a granulated product. During granulation, inorganic fillers and other optional components may be added. The primary molded body is then machined, such as by cutting, to form a secondary molded body of the desired shape. Examples of secondary molded bodies include industrial components such as gaskets, linings, and insulating films, and square tanks that are subjected to strong acids and strong alkalis in the semiconductor industry. Powders such as shavings, scraps, etc. (hereinafter also referred to as "shavings, etc.") generated when cutting a primary molded body to form a secondary molded body, as well as powders obtained by crushing the shavings, etc., and powders obtained by crushing unwanted secondary molded bodies can be used as the fluororesin 1. In this specification, the shavings, etc. and powders are collectively referred to as "crushed material." The secondary molded body or shavings, etc. can be crushed using a crusher or the like. After the coarse crushing, it may be further pulverized. The volume of each crushed material is, for example, 50 cm 3 The following is the result.

[0023] In this embodiment, the crushed material may be washed. Examples of washing liquids for washing the crushed material include water, organic solvents, surfactants, and the like. Alternatively, a washing liquid such as an aqueous solution containing two or more of these may be used. The amount of washing liquid used relative to 100 parts by mass of the crushed material is preferably 10 to 5,000 parts by mass, more preferably 50 to 4,000 parts by mass, and even more preferably 100 to 3,000 parts by mass. Washing may be performed by Method 1, in which the crushed material is immersed in the washing liquid and allowed to stand, Method 2, in which the crushed material is stirred, or Method 3, in which the washing liquid is poured over the crushed material. The immersion time is preferably longer than 0 hours and shorter than 100 hours, more preferably longer than 0 hours and shorter than 80 hours, and even more preferably longer than 0 hours and shorter than 60 hours. The temperature of the washing liquid is preferably 0 to 200°C, more preferably 10 to 150°C. In Methods 1 and 2, the crushed material and the washing liquid are then preferably subjected to solid-liquid separation by filtration or the like, followed by drying. In Method 1 and Method 2, when the process from adding a washing solution to the mixture to solid-liquid separation is counted as one washing, washing is preferably carried out 1 to 30 times, more preferably 1 to 25 times, and even more preferably 2 to 20 times. Similarly, washing in Method 3 is preferably carried out multiple times.

[0024] The crushed material to be washed may be crushed material such as shavings directly generated during the production of a secondary molded body, or may be crushed powder obtained by pulverizing a secondary molded body or shavings, etc. From the viewpoint of operability, crushed material such as shavings directly generated during the production of a secondary molded body is preferred.

[0025] (Fluororesin 2) Fluororesin 2 has no thermal history of being heated above its melting point. The melting point of fluororesin 2 is preferably 360°C or lower, more preferably 355°C or lower, and even more preferably 350°C or lower. The lower limit of the melting point is not particularly limited, but is preferably 100°C or higher, and more preferably 150°C or higher. The melting point is preferably 100 to 360°C, more preferably 100 to 350°C, and even more preferably 150 to 350°C. When the melting point is within the above range, the mechanical strength of the obtained molded article is likely to be improved. The fact that "has no thermal history of being heated above its melting point" can be confirmed by differential scanning calorimetry (DSC).

[0026] The fluororesin 2 may be, for example, a fluororesin produced by emulsion polymerization. Emulsion polymerization is a polymerization method in which a monomer is polymerized in an aqueous medium containing water to obtain a dispersion containing particles of the fluororesin 2. In general, emulsion polymerization is performed by a method in which a reaction liquid containing water, a polymerization initiator, and a surfactant is polymerized in the reaction liquid while the reaction liquid is stirred.

[0027] From the viewpoint of suppressing coloration of the resulting molded article, the content of the nonionic surfactant is preferably 2 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.1 parts by mass or less, per 100 parts by mass of the fluororesin in the dispersion. Examples of nonionic surfactants will be described later.

[0028] The content of the fluororesin 2 in the dispersion is preferably from 5 to 40% by mass, more preferably from 7 to 35% by mass, and even more preferably from 10 to 30% by mass.

[0029] The average particle size of the fluororesin 2 contained in the dispersion is preferably 0.05 to 0.5 μm, more preferably 0.08 to 0.45 μm, and even more preferably 0.10 to 0.35 μm. When the average particle size is within this range, the emulsion stability is excellent.

[0030] The fluororesin 2 preferably contains PTFE obtained by emulsion polymerization. In the method of producing PTFE by emulsion polymerization, TFE monomer is homopolymerized in the reaction solution, or TFE monomer is copolymerized with a monomer other than TFE monomer in the reaction solution to obtain a dispersion in which PTFE particles are dispersed in a dispersion medium. For example, in the presence of an aqueous medium, a polymerization initiator, an anionic fluorine-containing emulsifier, and a stabilizing aid, the TFE monomer is emulsion-polymerized, preferably over 1 to 20 hours, at a pressure of preferably 0.5 to 3.0 MPa, to obtain a dispersion. The nonionic surfactant may also be blended. Alternatively, a dispersion may be obtained without using a fluorine-based surfactant by the methods described in WO 2021 / 085470, WO 2022 / 181662, etc.

[0031] Examples of the anionic fluorine-containing emulsifier will be described later. The amount of the anionic fluorine-containing emulsifier used in the emulsion polymerization step of TFE monomer is preferably 0.15 to 2.0 parts by mass, more preferably 0.2 to 1.0 part by mass, and even more preferably 0.2 to 0.5 part by mass, per 100 parts by mass of the PTFE to be produced.

[0032] As the stabilizing aid, paraffin wax, fluorine-based oil, fluorine-based solvent, silicone oil, etc. are preferred, with paraffin wax being more preferred. One stabilizing aid may be used alone, or two or more may be used in combination. Paraffin wax may be liquid, semi-solid, or solid at room temperature, with saturated hydrocarbons having 12 or more carbon atoms being preferred. The melting point of paraffin wax is preferably 40 to 65°C, more preferably 50 to 65°C. The amount of stabilizing aid used is preferably 0.1 to 12 parts by mass, more preferably 0.1 to 8 parts by mass, per 100 parts by mass of the aqueous medium used.

[0033] As the polymerization initiator, a water-soluble radical initiator or a water-soluble oxidation-reduction catalyst is preferably used. As the water-soluble radical initiator, persulfates such as ammonium persulfate and potassium persulfate; and water-soluble organic peroxides such as disuccinic acid peroxide, bisglutaric acid peroxide, and tert-butyl hydroperoxide are preferred. The polymerization initiator may be used alone or in combination of two or more. Oil-soluble initiators can also be used. As the polymerization initiator, disuccinic acid peroxide is more preferred. The amount of the polymerization initiator used is preferably 0.01 to 0.20 parts by mass, more preferably 0.01 to 0.15 parts by mass, per 100 parts by mass of the PTFE to be produced.

[0034] The standard specific gravity (SSG) of the PTFE resin contained in the dispersion is an index of the average molecular weight of PTFE, and it can be conceptually classified as high molecular weight PTFE when the SSG is 2.14 or more but less than 2.22, and low molecular weight PTFE when the SSG is 2.22 to 2.4. Since the physical properties of PTFE decrease when the molecular weight is low, the SSG is preferably 2.14 or more but less than 2.22, and more preferably 2.14 to 2.21.

[0035] (Anionic Fluorine-Containing Emulsifier) ​​Examples of the anionic fluorine-containing emulsifier used in emulsion polymerization include fluorine-containing emulsifiers represented by general formula (1) (hereinafter also referred to as "fluorine-containing emulsifier (1)"). General formula (1): XCF 2 CF 2 (O) m CF 2 CF 2 OCF 2 COOA (wherein X is a hydrogen atom or a fluorine atom, and A is a hydrogen atom, an alkali metal, or NH 4 and m is 0 or 1. The fluorine-containing emulsifier (1) is preferred in that it has a good effect of stabilizing the polymerization of PTFE particles.

[0036] The X is preferably a fluorine atom in terms of polymerization stability. The m is preferably 1 in terms of polymerization stability and mechanical stability of the dispersion. Specific examples of A include H, Li, Na, K, and NH. 4 The fluorine-containing emulsifier (1) has good solubility in water and metal ion components are unlikely to remain as impurities, and therefore, NH 4 Particularly preferred examples of the fluorine-containing emulsifier (1) are CF 3 CF 2 CF 2 CF 2 OCF 2 COONH 4 , C 2 F 5 OCF 2 CF 2 OCF 2 COONH 4 (hereinafter referred to as EEA), with EEA being more preferred.

[0037] The fluorine-containing emulsifier (1) can be produced by fluorinating an ester of a corresponding non-fluorine-containing carboxylic acid or partially fluorinated carboxylic acid by a known fluorination method such as a liquid-phase fluorination method in which the ester is reacted with fluorine in a liquid phase, a fluorination method using cobalt fluoride, or an electrochemical fluorination method, hydrolyzing the ester bond of the obtained fluorinated ester, purifying it, and then neutralizing it with ammonia.

[0038] (Nonionic Fluorine-Containing Emulsifier) ​​Examples of the nonionic surfactant to be blended in the aqueous emulsion obtained by emulsion polymerization include a nonionic surfactant represented by general formula (2) (hereinafter also referred to as "nonionic surfactant (2)") and a nonionic surfactant represented by general formula (3) (hereinafter also referred to as "nonionic surfactant (3)"). General formula (2): R 1 -O-D-H (wherein, R 1 is an alkyl group having 8 to 18 carbon atoms, O is an oxygen atom, and D is a polyoxyalkylene chain consisting of 5 to 20 oxyethylene groups and 1 to 2 oxypropylene groups.) General formula (3): R 2 -OE-G (wherein, R 2 is an alkyl group having 6 to 18 carbon atoms, O is an oxygen atom, E is a polyoxyalkylene chain consisting of 1 to 3 oxybutylene groups and 5 to 20 oxyethylene groups, and G is a hydrogen atom or a methyl group.) One type of nonionic surfactant may be used alone, or two or more types may be used in combination.

[0039] The nonionic surfactant contained in the dispersion is preferably one or more selected from the group consisting of nonionic surfactants (2) and (3), and two or more may be used in combination. Nonionic surfactants (2) and (3) may also be combined.

[0040] Note that nonionic surfactants are mixtures of multiple molecules with a certain chain length distribution and a mixture of isomers, and the chain length of the polyoxyalkylene chain represents the average chain length of the multiple molecules. The number of oxyethylene groups and oxypropylene groups in the polyoxyalkylene chain is an average value. Also, when multiple types of nonionic surfactants are mixed and used, it is sufficient that the average number of oxyalkylene groups in each nonionic surfactant is within the above-mentioned range. Furthermore, each numerical value is not limited to an integer.

[0041] In the nonionic surfactant (2), R 1 The number of carbon atoms in the alkyl group represented by R is preferably in the range of 8 to 18, and more preferably 10 to 16. 1When the number of carbon atoms is equal to or greater than the lower limit of the above range, the surface tension of the dispersion is likely to be low and the wettability is likely to be improved. When the number of carbon atoms is equal to or less than the upper limit, the storage stability of the dispersion is excellent. When the alkyl group, which is the hydrophobic group, has a branched structure in which it branches off midway, this is preferred in that it is easier to improve the wettability of the dispersion. The alkyl group having a branched structure is preferably an alkyl group branched in the range from the carbon atom at the base of the alkyl group to the fifth carbon atom, and more preferably an alkyl group branched in the range from the carbon atom at the base of the alkyl group to the third carbon atom. In addition, the branched carbon atom may be a secondary carbon atom or a tertiary carbon atom, and a secondary carbon atom is preferred. The alkyl group having a branched structure includes, for example, C 10 H 21 CH (CH 3 ) CH 2 -, C 9 H 19 CH(C 3 H 7 ) -, C 6 H 13 CH(C 6 H 13 )- and the like can be exemplified.

[0042] In the nonionic surfactant (2), the hydrophilic group D is a polyoxyalkylene chain consisting of 5 to 20 oxyethylene groups and 1 to 2 oxypropylene groups. In particular, a polyoxyalkylene chain consisting of 7 to 12 oxyethylene groups and 1 to 2 oxypropylene groups results in favorable properties of the second dispersion. When D contains an oxypropylene group, defoaming properties are likely to be improved. Having 2 or fewer oxypropylene groups is preferred in that it reduces surface tension, facilitates wettability, and reduces repelling during recoating. Furthermore, in D, the oxypropylene group may be present between the polyoxyethylene groups or may be bonded to the end of the polyoxyethylene chain. Bonding an oxypropylene group to the end of the polyoxyethylene chain facilitates enhanced defoaming properties. In particular, bonding an oxypropylene group to the molecular terminal of the polyoxyethylene chain facilitates enhanced defoaming properties.

[0043] In the nonionic surfactant (2), the average number of oxyethylene groups per molecule is preferably 5 to 20, more preferably 7 to 12. When the average number of oxyethylene groups per molecule is equal to or greater than the lower limit of the above range, good storage stability is likely to be obtained. When the average number of oxyethylene groups per molecule is equal to or less than the upper limit of the above range, good wettability is likely to be obtained. As the nonionic surfactant (2), C 13 H 27 O (C 2 H 4 O) 8 C 3 H 6 OH, C 13 H 27 O (C 2 H 4 O) 9 C 3 H 6 OH, C 13 H 27 O (C 2 H 4 O) 10 (C 3 H 6 O) 2 H, C 16 H 27 O (C 2 H 4 O) 12 (C 3 H 6 O) 2 Commercially available nonionic surfactants having an average molecular structure such as H can be used.

[0044] The content of the nonionic surfactant (2) is preferably 2 to 12 parts by mass, more preferably 4 to 12 parts by mass, per 100 parts by mass of the fluororesin in the dispersion. When the content is equal to or greater than the lower limit of the above range, good storage stability is likely to be obtained. A high content of the nonionic surfactant (2) is suitable for applications requiring thick coating, but no improvement in performance is observed even when the content exceeds the upper limit of the above range, and therefore, for economic reasons, it is preferably equal to or less than the upper limit of the above range.

[0045] In the nonionic surfactant (3), R 2The number of carbon atoms in the alkyl group represented by the formula (I) is preferably in the range of 6 to 18, more preferably 8 to 16, and even more preferably 10 to 14. When the number of carbon atoms in the alkyl group is equal to or greater than the lower limit of the above range, the surface tension of the dispersion tends to be low and wettability tends to be increased. When the number of carbon atoms in the alkyl group is equal to or less than the upper limit of the above range, the dispersion tends to have excellent storage stability. When the number of carbon atoms in the alkyl group is within the above range, the wettability and storage stability are good.

[0046] R 2 The alkyl group represented by the formula (I) preferably has a branched structure, since it is easier to increase the wettability of the dispersion. The branched carbon atom may be a secondary carbon atom or a tertiary carbon atom, and a secondary carbon atom is preferred. The alkyl group having a branched structure is preferably a C 10 H 21 CH (CH 3 ) CH 2 -, C 9 H 19 CH(C 3 H 7 ) -, C 6 H 13 CH(C 6 H 13 ) -, CH(CH 3 ) 2 CH 2 CH (CH 3 ) 2 CH 2 CH (CH (CH 3 ) 2 CH 2 - etc. can be exemplified. 2 In the alkyl group represented by the formula (I), 10% or less of the hydrogen atoms in the alkyl group may be substituted with a halogen atom such as a fluorine atom, a chlorine atom, a bromine atom, etc. The alkyl group may also contain one or two unsaturated bonds.

[0047] E in general formula (3) is a polyoxyalkylene chain consisting of 1 to 3 oxybutylene groups and 5 to 20 oxyethylene groups. The number of oxybutylene groups is preferably 1 to 2.5, more preferably 1 to 2. When it is equal to or greater than the lower limit of the above range, the defoaming properties, wettability, and viscosity properties tend to be good. When it is equal to or less than the upper limit, the viscosity increase of the dispersion is suppressed, and good stability is likely to be obtained. When it is within the above range, properties such as viscosity, stability, defoaming properties, and wettability are good, which is preferable. The oxybutylene group may be branched or linear, with branched being preferred.

[0048] The oxybutylene group is —CH 2 -CH(C 2 H 5 )-O-,-CH(C 2 H 5 ) CH 2 -O-, -CH(CH 3 )-CH(CH 3 ) —O—, —CH 2 CH 2 -CH(CH 3 ) —O—, —CH 2 CH 2 CH 2 CH 2 Among them, —CH 2 -CH(C 2 H 5 )-O-,-CH(C 2 H 5 ) CH 2 —O—, —CH 2 CH 2 -CH(CH 3 )-O- is preferred. Examples of raw materials for the oxybutylene group include various butylene oxides, and specific examples include 1,2-butylene oxide, 2,3-butylene oxide, tetrahydrofuran, and methyloxetane.

[0049] In the nonionic surfactant (3), the number of oxyethylene groups in the polyoxyalkylene chain is 5 to 20, preferably 6 to 15, and more preferably 7 to 13. When the number is equal to or greater than the lower limit of the above range, the storage stability of the dispersion tends to be good. When the number is equal to or less than the upper limit, the wettability tends to be good. When the number is within the above range, properties such as viscosity, stability, defoaming property, and wettability are good, which is preferable. The oxybutylene groups in the polyoxyalkylene chain may have a block structure or a random structure.

[0050] The oxybutylene group may be present at any position in the polyoxyalkylene chain, but R 2 It is preferable that the —O— group is present in the range up to 70% of the total length of the polyoxyalkylene chain, and R 2 It is more preferable that the R of the polyoxyalkylene chain is present in the range from the —O— group side to 50% of the total length of the polyoxyalkylene chain. 2 The portion bonded to the -O- group is preferably an oxybutylene group, more preferably a polyoxybutylene chain consisting of 1 to 2 oxybutylene groups. Furthermore, the portion of the polyoxyalkylene chain bonded to the G group is preferably an oxyethylene group, more preferably a polyoxyethylene chain consisting of 5 to 20 oxyethylene groups. Polyoxyalkylene chains having these preferred structures are preferred because they have better properties such as viscosity, stability, defoaming properties, and wettability. G in general formula (3) is a hydrogen atom or a methyl group, preferably a hydrogen atom.

[0051] The nonionic surfactant (3) can be obtained by addition reaction of butylene oxide and ethylene oxide with a higher alcohol by a known method. Butylene oxide and ethylene oxide may be mixed and reacted simultaneously, or butylene oxide may be reacted first and then ethylene oxide, or ethylene oxide may be reacted first and then butylene oxide. The method of reacting butylene oxide first and then ethylene oxide is preferred.

[0052] As the nonionic surfactant (3), C 13 H27 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 H、C 10 H 21 HH(H) 3 )CH 2 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 H、C 10 H 21 HH(H) 3 )CH 2 OCH(C 2 H 5 )CH 2 O(C 2 H 4 O) 8 H、C 12 H 25 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 H、C 8 H 17 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 10 H、C 12 H 25 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 10 H、C 13 H 27 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 11 H、C 13 H 27 OCH 2 CH 2 OCH 2 CH(C2 H 5 )O(C 2 H 4 O) 8 H、C 12 H 25 O(CH 2 CH(C 2 H 5 )O) 2 (C 2 H 4 O) 8 H、C 10 H 21 CH(CH 3 )CH 2 O(C 2 H 4 O) 9 CH 2 CH(C 2 H 5 )OH、C 16 H 33 OC 2 H 4 P.S. 2 H 5 )CH 2 O(C 2 H 4 O) 9 H、C 12 H 25 SO 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 CH 2 CH(C 2 H 5 )OH、C 13 H 27 P.S. 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 10 H 21 CH(CH 3 )CH 2 P.S. 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 10 H 21 CH(CH 3)CH 2 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 12 H 25 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 8 H 17 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 10 H、C 12 H 25 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 10 H、C 13 H 27 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 11 H、C 13 H 27 O(CH) 2 ) 4 O(C 2 H 4 O) 8 H、C 12 H 25 O(CH 2 ) 4 O(C 2 H 4 O) 8 H、C 8 H 17 O(CH) 2 ) 4 O(C 2 H 4 O) 10 H、C 12 H 25 O(CH) 2 ) 4 O(C 2 H 4 O) 10 H、C 13 H27 O(CH 2 ) 4 O(C 2 H 4 O) 11 H, C 13 H 27 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 8 H, C 12 H 25 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 8 H, C 8 H 17 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 10 H, C 12 H 25 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 10 H, C 13 H 27 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 11 Examples thereof include H, etc.

[0053] When the dispersion contains nonionic surfactant (3), the content of nonionic surfactant (3) is preferably 0.1 to 12 parts by mass, more preferably 0.5 to 11 parts by mass, and even more preferably 1 to 10 parts by mass, per 100 parts by mass of the fluororesin in the dispersion. When the content is equal to or greater than the lower limit of the above range, good storage stability is likely to be obtained. In addition, cracks are less likely to occur in the fluororesin coating film, and repellency is less likely to occur. A high content of nonionic surfactant (3) is suitable for applications requiring thick coating, but no improvement in performance is observed even when the content exceeds the upper limit of the above range, and therefore, for economic reasons, it is preferable that the content be equal to or less than the upper limit of the above range.

[0054] When nonionic surfactant (2) and nonionic surfactant (3) are used in combination as a nonionic surfactant, the average number of oxybutylene groups per molecule of the nonionic surfactant as a whole is preferably 0.5 to 2, more preferably 0.7 to 1.7, and even more preferably 0.9 to 1.5. Nonionic surfactant (2) and nonionic surfactant (3) may be added separately. A mixture containing nonionic surfactant (3) and nonionic surfactant (2) by-produced during the preparation of nonionic surfactant (3) may also be used.

[0055] The dispersion contains water as a dispersion medium for the fluororesin particles. This water may be water contained in the aqueous emulsion obtained by emulsion polymerization, or water prepared separately from the water in the aqueous emulsion. The dispersion may optionally contain one or more of a pH adjuster (e.g., ammonia), an anionic surfactant, a polyethylene oxide thickener, a polyurethane thickener, a thixotropic agent, a silicone wettability improver, a fluorine wettability improver, a preservative, etc. Furthermore, the dispersion may contain one or more of a water-soluble organic solvent, an organic solvent (e.g., toluene, xylene, etc.), a pigment (e.g., carbon black, etc.), a glass powder, hollow glass beads, and a colorant (e.g., graphite particles, silica particles, mica, etc.).

[0056] (Composition) The fluororesin composition may contain one or more solid components other than fluororesin 1 and fluororesin 2. Examples of other solid components include solid components used in the production process of fluororesin 1, solid components used in the production process of fluororesin 2, and solid components added after the production of fluororesin 1 and fluororesin 2. Specific examples include inorganic fillers, pigments (e.g., carbon black), colorants (e.g., graphite particles, silica particles, mica), and the above-mentioned additives. Examples of inorganic fillers include reinforcing fibers (e.g., glass fiber, carbon fiber), glass powder, bronze powder, graphite powder, hollow glass beads, and the like. The content of other solid components is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, based on the total mass of the solid contents of the fluororesin composition. It may be zero.

[0057] The total content of fluororesin 1 and fluororesin 2 relative to the total mass of the solid content of the fluororesin composition is preferably 30 to 100 mass%, more preferably 40 to 100 mass%, and even more preferably 50 to 100 mass%. The fluororesin composition is preferably solid, more preferably powdered. The content of fluororesin 1 relative to the total mass of fluororesin 1 and fluororesin 2 is preferably 10 mass% or more, more preferably 10 to 90 mass%, even more preferably 15 to 85 mass%, and particularly preferably 20 to 80 mass%. When the content of fluororesin 1 is equal to or greater than the lower limit of the above range, recycling efficiency is improved when fluororesin 1 is derived from cuttings or the like during the production of the above-mentioned secondary molded body (in the case of recycled fluororesin). When the content of fluororesin 1 is equal to or less than the upper limit of the above range, the compressive strength of the resulting molded body is likely to be improved.

[0058] <<Method for Producing Fluororesin Composition>> The method for producing the fluororesin composition of the present embodiment includes washing a mixture containing the first fluororesin and the second fluororesin.

[0059] <Method for producing the mixture> The mixture can be obtained by mixing fluororesin 1 and fluororesin 2. Examples of the mixing method include the following modes (1) to (4), with mode (4) being preferred. (1) Dry mixing of powdered fluororesin 1 and powdered fluororesin 2. (2) Mixing of powdered fluororesin 1 and a dispersion in which fluororesin 2 is dispersed. (3) Mixing of a dispersion in which fluororesin 1 is dispersed with powdered fluororesin 2. (4) Mixing of a dispersion in which fluororesin 1 is dispersed with a dispersion in which fluororesin 2 is dispersed.

[0060] The dispersion in which the fluororesin 1 is dispersed is preferably a dispersion obtained by mixing the powdered fluororesin 1 produced by the above-described production method with a water-soluble organic solvent. From the viewpoint of miscibility with the fluororesin 1 and water, the water-soluble organic solvent is preferably one or more water-soluble organic solvents selected from the group consisting of aprotic water-soluble organic solvents and alcohols. The alcohols may have an amino group or an alkoxy group as a substituent. The aprotic water-soluble organic solvent is preferably acetone, tetrahydrofuran, or acetonitrile. The alcohol is preferably methanol, ethanol, propanol, isopropyl alcohol, or 1-methoxy-2-propanol. Of these, isopropyl alcohol is more preferable as the water-soluble organic solvent. One type of water-soluble organic solvent may be used alone, or two or more types may be used in combination.

[0061] The content of Fluororesin 1 relative to the total mass of the dispersion in which Fluororesin 1 is dispersed is preferably from 3 to 70 mass %, more preferably from 5 to 65 mass %, and even more preferably from 10 to 60 mass %.

[0062] The dispersion in which the fluororesin 2 is dispersed is preferably a dispersion in which the fluororesin 2 is dispersed by the above-mentioned emulsion polymerization. A dispersion in which a nonionic surfactant has been blended into the dispersion to improve storage stability may also be used. When using powdered fluororesin 2, the powdered fluororesin 2 may be obtained by separating the fluororesin 2 from the solvent by filtration, drying, or the like from the dispersion in which the fluororesin 2 is dispersed.

[0063] The content of the fluororesin 2 relative to the total mass of the dispersion in which the fluororesin 2 is dispersed is preferably from 5 to 40 mass %, more preferably from 7 to 35 mass %, and even more preferably from 10 to 30 mass %.

[0064] In the cases of the above embodiments (2) to (4), the combined content of fluororesin 1 and fluororesin 2 relative to the total mass of the mixture is preferably 10 to 50 mass%, more preferably 12 to 45 mass%, and even more preferably 15 to 35 mass%. When the combined content of fluororesin 1 and fluororesin 2 is equal to or greater than the lower limit of the above range, fluororesin 1 and fluororesin 2 tend to aggregate, facilitating solid-liquid separation. When the combined content of fluororesin 1 and fluororesin 2 is equal to or less than the upper limit of the above range, mixing of fluororesin 1 and fluororesin 2 is likely to be promoted.

[0065] In the case of the above embodiment (4), the content of the water-soluble organic solvent relative to 100 parts by mass of water in the mixture is preferably 2 to 150 parts by mass, more preferably 5 to 140 parts by mass, and even more preferably 10 to 130 parts by mass.

[0066] The metal content relative to the total mass of the solid content of the mixture is preferably 0 to 10 mg / g, more preferably 0 to 5 mg / g, and even more preferably 0 to 1 mg / g. When the metal content is equal to or greater than the lower limit of the above range, the method for producing a fluororesin composition of this embodiment can be suitably employed. When the metal content is equal to or less than the upper limit of the above range, the compressive strength of the obtained molded article is likely to be improved.

[0067] (Method for washing the mixture) The mixture can be washed by adding a washing liquid to a mixture containing powdered fluororesin 1 and fluororesin 2. In the above embodiments (2) to (4), the mixture is stirred and agglomerated to obtain an agglomerate. The agglomerate is filtered to separate the agglomerate and the solvent, and the agglomerate is washed with a large amount of water. Thereafter, by drying, a mixture containing powdered fluororesin 1 and fluororesin 2 can be obtained.

[0068] Examples of cleaning liquids used to wash the mixture include water and organic solvents. Alternatively, cleaning liquids such as aqueous solutions containing two or more of these may be used. The amount of cleaning liquid used is preferably 10 to 5,000 parts by mass, more preferably 50 to 4,000 parts by mass, and even more preferably 100 to 3,000 parts by mass, relative to 100 parts by mass of the solid content of the mixture. Washing may be performed by Method 1, in which the mixture is immersed in the cleaning liquid and allowed to stand, Method 2, in which the mixture is stirred, or Method 3, in which the cleaning liquid is poured over the mixture. The immersion time is preferably more than 0 hours and not more than 100 hours, more preferably more than 0 hours and not more than 80 hours, and even more preferably more than 0 hours and not more than 60 hours. The temperature of the cleaning liquid is preferably 0 to 200°C, more preferably 10 to 150°C. In Methods 1 and 2, the mixture and the cleaning liquid are then preferably subjected to solid-liquid separation by filtration or the like, followed by drying. In Method 1 and Method 2, when the process from adding a washing solution to the mixture to solid-liquid separation is counted as one washing, washing is preferably carried out 1 to 30 times, more preferably 1 to 25 times, and even more preferably 2 to 20 times. Similarly, washing in Method 3 is preferably carried out multiple times.

[0069] <Molded body> The molded body of this embodiment can be obtained by compression molding the powdered fluororesin composition described above and firing it. Specifically, the powdered fluororesin composition is placed in a mold and compression molded under pressure to obtain a preform, and the preform obtained is fired to obtain a primary molded body. The shape of the primary molded body is not particularly limited. For example, it may be a block shape such as a cylindrical or polygonal pillar shape.

[0070] When the fluororesin composition is compression molded, the pressure is 100 to 350 kg / cm 2 The baking temperature after the preforming is preferably 360 to 380°C.

[0071] The obtained primary molded article may be processed by cutting or the like to produce a secondary molded article of a desired shape. Examples of uses of the secondary molded article include seals, packings, rollers, sockets, and joints.

[0072] The molded article of this embodiment may be the primary molded article or the secondary molded article.

[0073] <Mechanism of Action> The fluororesin composition of the present invention contains fluororesin 1 having a thermal history of being heated to or above its melting point. When fluororesin 1 originates from chips or the like during the production of the aforementioned secondary molded article, it may be contaminated with metals from the cutting machine used in the cutting process or the pulverizer used in the pulverization process. The present inventors have found for the first time that such metal contamination impairs the compressive strength of molded articles obtained from the fluororesin composition. They then found that a preform obtained by compression molding the fluororesin composition was baked at 380°C for 2 hours or more to form a microdumbbell-shaped test specimen measuring 0.5 mm in thickness and 16 mm x 45 mm. The test specimen was then left to stand in 3.6% by mass hydrochloric acid at 23°C for 24 hours, and the amount of metal elution relative to the total mass of the test specimen was kept at 5 ng / g or less, thereby suppressing the decrease in compressive strength and increasing the recycling efficiency of the fluororesin.

[0074] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the following examples, Example 1 is an example, Examples 2 and 3 are comparative examples, and Example 4 is a reference example.

[0075] <Evaluation Method> (Melting Point) Using a differential scanning calorimeter (DSC 8500, manufactured by Perkin Elmer), the fluororesin was heated to 380° C. at a rate of 10° C. / min in an air atmosphere, and the melting point was determined from the endothermic peak. When there were multiple endothermic peaks, the peak temperature of the largest endothermic peak was used.

[0076] (Average Particle Diameter) Using a laser diffraction / scattering particle size distribution analyzer (LA-920, manufactured by Horiba, Ltd.), powdered fluororesin was dispersed in water, and the particle size distribution was measured on a number basis to calculate the average particle diameter.

[0077] (Standard Specific Gravity) Measured in accordance with ASTM D1457-91a and D4895-91a.

[0078] (Metal elution test) 50 g of 3.6 mass % hydrochloric acid was added to 10 g of molded body 1B, 2B, or 4B obtained in Examples 1, 2, and 4, and the mixture was allowed to stand at 23°C for 24 hours. Thereafter, solid-liquid separation was performed, and the amount of metal in the resulting solution was measured by inductively coupled plasma mass spectrometry (ICP-MS, Agilent 7900 ICP-MS). The amount of metal elution was determined by dividing the obtained amount of metal by the mass of molded body 1B, 2B, or 4B.

[0079] (Evaluation of Compressive Strength) The compressive strength of the molded articles 1A to 4A obtained in Examples 1 to 4 described below was measured in accordance with ASTM D695 using a Tensilon universal material testing machine (RTF-1350 manufactured by Orientec Co., Ltd.).

[0080] Compressive strength (0.2% yield strength) is the stress level at a strain of 0.2%. A larger value indicates better compressive strength. Evaluation was performed according to the following criteria: A: Compressive strength (0.2% yield strength) is 7 MPa or more; B: Compressive strength (0.2% yield strength) is less than 7 MPa.

[0081] The compressive stress at a compressive strain of 10% (stress at 10% deformation) indicates the compressive stress when the strain is 10%. The larger this value, the better the compressive strength. Evaluation was performed according to the following criteria. A: Compressive strength (stress at 10% deformation) is 16 MPa or more. B: Compressive strength (stress at 10% deformation) is less than 16 MPa.

[0082] (Production Example 1) A powdery fluororesin A (molding powder) consisting of only TFE units was produced by suspension polymerization. The fluororesin A was a fluororesin that had no thermal history of being heated above its melting point.

[0083] (Production Example 2) Fluororesin A was preformed and then baked at or above its melting point to produce a primary molded body. The offcuts and scraps obtained when a secondary molded body was cut out of the resulting primary molded body were pulverized to obtain powdered fluororesin B with an average particle size of 40 μm or less. Fluororesin B is a fluororesin with a thermal history of being heated to or above its melting point. The melting point of the resulting fluororesin B was 329°C. The resulting fluororesin B was non-melt-moldable, as it did not exhibit a temperature at which the melt flow rate was 0.1 to 1000 g / 10 min at a temperature 20°C or more higher than the melting point of the resin under a load of 49 N. 200 g of fluororesin B and 200 g of isopropanol were mixed to obtain dispersion B. The content of fluororesin B relative to the total mass of dispersion B was 50 mass%.

[0084] (Production Example 3) 36 g of EEA, 555 g of paraffin wax (melting point 55 ° C), and 61.3 L of deionized water were charged into a 100 L stainless steel autoclave equipped with a baffle and a stirrer. After the interior of the autoclave was purged with nitrogen and reduced pressure, TFE was introduced and the temperature was raised to 62 ° C with stirring. TFE was further injected until the internal pressure reached 1.765 MPa, and 26.3 g of disuccinic acid peroxide (concentration 80 mass%, remainder water) was dissolved in 1 L of warm water at about 70 ° C and injected. After about 3 minutes, the internal pressure of the autoclave dropped to 1.716 MPa, so TFE was injected to maintain the internal pressure at 1.765 MPa, and polymerization was allowed to proceed. During the polymerization, EEA was dissolved in warm water and a total of 53 g of EEA was injected in two batches. The autoclave temperature was gradually raised to 72°C, and the reaction was terminated when the amount of TFE injected reached 22 kg, and the TFE in the autoclave was released into the atmosphere. The polymerization time was 105 minutes. After cooling, the solidified paraffin wax on top was removed, yielding Dispersion C, in which fluororesin C composed solely of TFE units produced by emulsion polymerization was dispersed. The content of fluororesin C relative to the total mass of Dispersion C was approximately 25.0 mass%, and the EEA concentration was 0.40 mass parts per 100 mass parts of fluororesin C. The average particle size of fluororesin C in Dispersion C was 0.26 μm. The standard specific gravity (SSG) of fluororesin C was 2.21. The melting point of fluororesin C was 337°C. The resulting fluororesin C was non-melt-moldable, as there was no temperature at which the melt flow rate was 0.1 to 1,000 g / 10 min at temperatures 20°C or more higher than the melting point of the resin under a load of 49 N.

[0085] Example 1 798 g of Dispersion C and 802 g of water were placed in an 8-L stainless steel vessel equipped with a baffle and a stirrer and stirred. 400 g of Dispersion B was added to the stirred Dispersion C to obtain Dispersion D, a mixture containing fluororesin B and fluororesin C. The mass ratio of fluororesin B to fluororesin C in Dispersion D (fluororesin B:fluororesin C) was 1:1. The mass ratio of IPA to water in Dispersion D (IPA:water) was 12:88. The combined content of fluororesin B and fluororesin C relative to the total mass of Dispersion D was 20.0 mass%. The mixture was stirred at 680 rpm for 10 minutes using a stirrer to aggregate the solids in Dispersion D, and the solvent was separated by filtration to obtain Aggregate 1 before washing. The filtered Aggregate 1 was transferred to a stainless steel vessel, and 300 parts by mass of water per 100 parts by mass of Aggregate 1 was added and stirred, followed by filtration and a washing process. The washing step was repeated three times to obtain washed aggregate 2. The obtained aggregate 2 was placed in a tray, vacuum dried at 25°C for 2 hours or more, and then dried at 200°C for 10 hours or more to obtain fluororesin composition 1, which was a mixture of powdered fluororesin B and powdered fluororesin C. 6.5 g of the obtained fluororesin composition 1 was placed in a mold with a diameter of 12.95 mm and subjected to a pressure of 320 kg / cm. 2 This preform was baked at 380°C for 2 hours to obtain a molded body 1A of Example 1. 345 g of the obtained fluororesin composition 1 was placed in a mold with a diameter of 7.3 mm, and a pressure of 320 kg / cm was applied. 2 A preform was obtained by pressing at 380°C for 2 hours. This preform was then fired at 380°C for 2 hours to obtain a molded body. The obtained molded body was skived to produce a sheet with a thickness of 0.5 mm, and a microdumbbell-shaped test piece measuring 16 mm x 45 mm was punched out to obtain molded body 1B of Example 1 (a microdumbbell-shaped test piece). The above-mentioned evaluations were carried out using molded bodies 1A and 1B. The results are shown in Table 1 (the same applies to Examples 2 to 4 below).

[0086] Example 2 The unwashed agglomerate 1 filtered off in Example 1 was transferred to a stainless steel tank, and 100 parts by mass of water was added to 100 parts by mass of agglomerate 1, followed by stirring. The water was then separated by filtration to obtain washed agglomerate 3. The obtained agglomerate 3 was placed in a tray, vacuum dried at 25°C for 2 hours or more, and then dried at 200°C for 10 hours or more to obtain fluororesin composition 2, which was a mixture of powdered fluororesin B and powdered fluororesin C. A molded body was prepared in the same manner as in Example 1, except that fluororesin composition 2 was used instead of fluororesin composition 1, to obtain molded bodies 2A and 2B of Example 2 (microdumbbell-shaped test pieces).

[0087] (Example 3) A molded body was produced in the same manner as in Example 1, except that fluororesin B was used instead of fluororesin composition 1, to obtain molded body 3A of Example 3. On the other hand, when fluororesin B was used, skiving could not be performed, and molded body 3B (a test piece in the shape of a microdumbbell) could not be molded.

[0088] (Example 4) Molded bodies 4A and 4B (microdumbbell-shaped test pieces) of Example 4 were obtained in the same manner as in Example 1, except that fluororesin A was used instead of fluororesin composition 1.

[0089]

[0090] It was found that the molded article of Example 1, in which the amount of metal elution was 5 ng / g or less, had excellent compressive strength.

Claims

1. A fluororesin composition comprising a first fluororesin having a thermal history of being heated to or above its melting point, and a second fluororesin having no thermal history of being heated to or above its melting point, wherein the first fluororesin and the second fluororesin are non-melt-formable fluororesins, and the fluororesin composition is compression-molded to obtain a preform, which is baked at 380°C for 2 hours or more to obtain a microdumbbell-shaped test piece having a thickness of 0.5 mm and a size of 16 mm x 45 mm. The test piece is left to stand in 3.6% by mass hydrochloric acid at 23°C for 24 hours, and the amount of metal eluted relative to the total mass of the test piece is 5 ng / g or less.

2. A fluororesin composition according to claim 1, wherein the first fluororesin has tetrafluoroethylene units, and the content of the tetrafluoroethylene units relative to the total mass of the first fluororesin is 99 mass% or more.

3. A fluororesin composition according to claim 2, wherein the second fluororesin has tetrafluoroethylene units, and the content of the tetrafluoroethylene units relative to the total mass of the second fluororesin is 99 mass% or more.

4. A fluororesin composition according to any one of claims 1 to 3, wherein the content of the first fluororesin relative to the total mass of the first fluororesin and the second fluororesin is 10 mass% or more.

5. A molded article of the fluororesin composition according to any one of claims 1 to 3.

6. A method for producing a fluororesin composition according to any one of claims 1 to 3, comprising washing a mixture containing the first fluororesin and the second fluororesin.

Citation Information

Patent Citations

  • Game machine

    JP2023091850A

  • Method for producing sintered fluororesin body, sintered fluororesin body, method for producing fluororesin dispersion, method for producing sintered body, fluororesin dispersion, and sintered body

    JP6612001B1

  • Method for producing polytetrafluoroethylene aqueous dispersion

    WO2021085470A1

  • Method for producing polytetrafluoroethylene aqueous dispersion

    WO2022181662A1

  • Molded body of polytetrafluoroethylene, mixed powder and method for producing molded body

    JP2009242710A