Fluorocarbon resin molded body

The combination of thermally history-altered and emulsion-polymerized fluororesins in a specific mass ratio addresses the reusability and mechanical strength issues of PTFE molded products, enhancing compressive strength and creep resistance in fluororesin articles.

WO2024248103A1PCT designated stage expired Publication Date: 2024-12-05AGC INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019919
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Fluororesin molded products, particularly those made from polytetrafluoroethylene (PTFE), face challenges in reusability due to the hard and brittle nature of fired PTFE, which results in insufficient compressive strength and compression creep resistance, even when porosity is minimized.

Method used

A fluororesin molded article is created using a combination of a fluororesin with a thermal history above its melting point and a non-melt moldable fluororesin produced by emulsion polymerization, with a specific mass ratio and composition to enhance compressive strength and compression creep resistance.

Benefits of technology

The approach results in a fluororesin molded article with improved compressive strength and compression creep resistance, achieving a glossiness of 15% or more and maintaining structural integrity under deformation, while minimizing voids and improving mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

A fluorocarbon resin molded body obtained by compression-molding and firing a fluorocarbon resin composition containing a first fluorocarbon resin having a thermal history of being heated to equal to or higher than the melting point of the same and a second fluorocarbon resin not having thermal history of being heated to equal to or higher than the melting point of the same, wherein the first fluorocarbon resin is a non-melt-moldable fluorocarbon resin, the second fluorocarbon resin is a non-melt-moldable fluorocarbon resin produced by emulsion polymerization, the proportion of the first fluorocarbon resin with respect to the total mass of the first and second fluorocarbon resins is at least 40 mass%, and the glossiness at an incident angle of 60° of the molded body is at least 15%.
Need to check novelty before this filing date? Find Prior Art

Description

Fluorine resin molded body

[0001] The present invention relates to a fluororesin molded article. This application claims priority to Japanese Patent Application No. 2023-091849, filed on June 2, 2023, the contents of which are incorporated herein by reference.

[0002] Polytetrafluoroethylene resin (molding powder) obtained by suspension polymerization of tetrafluoroethylene (TFE) is compression molded and then sintered to form a molded body. The molded body obtained by sintering is processed into a molded product of the desired shape by cutting or other processes. However, once-sintered polytetrafluoroethylene resin (sintered PTFE) such as cutting chips generated during processing is hard, and even if it is crushed and compressed, it does not come together and cannot be molded. For this reason, it has been difficult to reuse it.

[0003] Patent Document 1 describes that when a powder of sintered PTFE is mixed with a PTFE dispersion (a dispersion of unsintered PTFE) obtained by emulsion polymerization of TFE, and the mixture is compression-molded and sintered to produce a molded body, the porosity after sintering decreases as the mixing ratio of unsintered PTFE increases, and the tensile strength after sintering increases. For example, it describes an example in which the porosity after sintering becomes 0% when the mixing ratio of unsintered PTFE is 100%.

[0004] Patent No. 6612001

[0005] Depending on the application of a fluororesin molded article, compressive strength and compressive creep resistance may be required. However, according to the findings of the present inventors, even if the porosity after firing is low as in the examples of Patent Document 1, voids may occur in a compression test. If many voids occur, the compressive strength and compressive creep resistance will be insufficient. The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a fluororesin molded article using a fluororesin that has a thermal history of being heated to or above its melting point, and that has good compressive strength and compressive creep resistance.

[0006] The present invention has the following aspects. [1] A molded product obtained by compression molding and sintering a fluororesin composition comprising a first fluororesin that has a thermal history of being heated to or above its melting point, and a second fluororesin that has not had a thermal history of being heated to or above its melting point, wherein the first fluororesin is a non-melt-formable fluororesin, and the second fluororesin is a non-melt-formable fluororesin produced by emulsion polymerization, the proportion of the first fluororesin relative to the total mass of the first fluororesin and the second fluororesin is 40 mass% or more, and the molded product has a gloss of 15% or more at an incident angle of 60°. [2] The fluororesin molded product according to [1], wherein the proportion of the first fluororesin relative to the total mass of the first fluororesin and the second fluororesin is 50 mass% or more. [3] The fluororesin molded product according to [1] or [2], wherein the first fluororesin and the second fluororesin are each independently fluororesins containing 99 mass% or more of tetrafluoroethylene units relative to the total mass of the fluororesins.

[0007] According to the present invention, a fluororesin molded article using a fluororesin having a thermal history of being heated to a temperature equal to or higher than its melting point can be obtained, which has good compressive strength and compressive creep resistance.

[0008] The following definitions of terms apply throughout the present specification and claims. "Monomer-based unit" is a collective term for an atomic group formed directly by polymerization of one monomer molecule and an atomic group obtained by chemically converting a portion of the atomic group. In this specification, a monomer-based unit is also simply referred to as a monomer unit. "Monomer" means a compound having a polymerizable carbon-carbon double bond. "Melting point" means the temperature corresponding to the maximum value of the melting peak measured by differential scanning calorimetry (DSC). The "to" symbol indicating a range of values ​​means that the values ​​before and after it are included as the lower and upper limits. "Average particle size" means the 50% cumulative value (median diameter, D50) in the number-based particle size distribution determined using a laser diffraction / scattering particle size distribution analyzer (e.g., HORIBA, Ltd., LA-920 measuring instrument). "Melt-moldable" means exhibiting melt fluidity. "Exhibiting melt fluidity" means that there is a temperature at which the melt flow rate is 0.1 to 1,000 g / 10 min under a load of 49 N at a temperature at least 20°C higher than the melting point of the resin. "Melt flow rate" refers to the melt mass flow rate (MFR) defined in JIS K 7210:1999 (ISO 1133:1997). "Non-melt moldable" means that the material does not exhibit the melt fluidity. "Standard specific gravity (hereinafter also referred to as "SSG")" is a value that serves as an index of average molecular weight; a larger value indicates a smaller molecular weight. It can be measured in accordance with ASTM D1457-91a and D4895-91a. "Gloss" is a value that serves as an index of gloss, and is the specular gloss value at an incident angle of 60° measured in accordance with JIS Z 8741.

[0009] <Non-melt-formable fluororesin> The fluororesin molded article of the present invention is a molded article obtained by compression molding and baking a fluororesin composition containing fluororesin 1 (hereinafter also referred to as "fluororesin 1") and fluororesin 2 (hereinafter also referred to as "fluororesin 2"). Fluororesin 1 and fluororesin 2 are both non-melt-formable fluororesins. Fluororesin 1 and fluororesin 2 may be the same or different. Fluororesin 1 and fluororesin 2 may each independently represent one type of fluororesin, or two or more types of fluororesins may be used in combination. When two or more types of fluororesins are used in combination, it is sufficient that the mixture of the two or more types of fluororesins is non-melt-formable.

[0010] As the fluororesin 1 and the fluororesin 2, a polymer having a tetrafluoroethylene unit (hereinafter also referred to as a "TFE unit") is preferable, and examples thereof include polytetrafluoroethylene (PTFE), a tetrafluoroethylene-ethylene copolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, a tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer, a tetrafluoroethylene-chlorotrifluoroethylene copolymer, a tetrafluoroethylene-ethylene-hexafluoropropylene copolymer, and a tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer.

[0011] Preferably, fluororesin 1 and fluororesin 2 are each independently PTFE. The content of TFE units in PTFE relative to the total mass of the fluororesin is preferably 99% by mass or more. The content of TFE units relative to the total mass of PTFE is more preferably 99.5% by mass or more, and may be 100% by mass.

[0012] Examples of the monomer units other than the TFE units include the above-mentioned ethylene units, hexafluoropropylene units, perfluoro(alkyl vinyl ether) units, chlorotrifluoroethylene units, vinylidene fluoride units, as well as monomer units based on perfluoro(2,2-dimethyl-1,3-dioxole), perfluoro(4-methoxy-1,3-dioxole), perfluoroalkylethylene, etc. The monomer units other than the TFE units may be one type or two or more types. By including monomer units other than the TFE units, the crystallization of PTFE is suppressed to some extent, and the tensile strength, tensile elongation, dielectric breakdown resistance, creep resistance, etc. are improved.

[0013] <Fluororesin 1> Fluororesin 1 has a thermal history of being heated to or above its melting point at least once. Fluororesin 1 can be obtained by pulverizing cuttings generated when a primary molded article produced by heating to or above its melting point is processed into a secondary molded article such as an industrial part of a desired shape, or by pulverizing an unnecessary secondary molded article. The pulverization can be performed using a pulverizer or the like. After coarse pulverization, the material may be further pulverized. An example of the heating is heating by firing required for producing a molded article. By heating to or above its melting point, the melting point of fluororesin 1 is lowered below the melting point of fluororesin 1 before being heated to or above its melting point. The fact that "fluororesin 1 has a thermal history of being heated to or above its melting point at least once" can be confirmed by differential scanning calorimetry (DSC).

[0014] The melting point of fluororesin 1 before being heated to or above its melting point is preferably 360°C or lower, more preferably 355°C or lower, and even more preferably 350°C or lower. There are no particular restrictions on the lower limit of the melting point, but it is preferably 100°C or higher, and more preferably 150°C or higher. The melting point is preferably 100 to 360°C, more preferably 100 to 355°C, and even more preferably 150 to 350°C. When the melting point is within the above range, the mechanical strength of the resulting molded article is likely to be improved.

[0015] The melting point of fluororesin 1 is preferably 335°C or lower, more preferably 330°C or lower. There is no particular limitation on the lower limit of the melting point, but it is preferably 100°C or higher, more preferably 150°C or higher. The melting point is preferably 100 to 335°C, more preferably 150 to 330°C. When the melting point is within the above range, the mechanical strength of the obtained molded article is likely to be improved.

[0016] The bulk density of fluororesin 1 is preferably 100 g / L or more, more preferably 105 g / L or more, and even more preferably 110 g / L or more. When the bulk density is equal to or greater than the lower limit, less air is carried over during the production of a molded body, resulting in excellent deaeration properties and good fusion between powder particles. Furthermore, voids are less likely to remain in the resulting molded body, and the uniformity of the molded body is also likely to be improved.

[0017] The average particle size of the fluororesin 1 is preferably 1 to 500 μm, more preferably 5 to 300 μm, and even more preferably 5 to 100 μm. When the average particle size of the fluororesin 1 is within the above range, the uniformity of the fluororesin molded article is improved.

[0018] The fluororesin 1 may be, for example, crushed pieces of a molded product obtained by a method including a step of heating a molding material containing PTFE obtained by suspension polymerization to above its melting point. PTFE obtained by suspension polymerization has an extremely high melt viscosity and exhibits non-melt moldability, which means that it cannot be molded by general thermoplastic resin molding methods such as extrusion molding and injection molding. Therefore, when molding PTFE produced by suspension polymerization (hereinafter also referred to as "molding powder"), a method is used in which the molding powder is filled into a mold, compression molded, and then sintered.

[0019] Specifically, the molding powder is molded by first filling a mold with the molding powder at room temperature and compression-molding it to form a preform, which is then heated to or above the melting point of PTFE for sintering to form a primary molded body. The molding powder may be granulated as needed and used as a granulated product. During granulation, inorganic fillers and other optional components may be added. The primary molded body is then machined, such as by cutting, to form a secondary molded body of the desired shape. Examples of secondary molded bodies include industrial components such as gaskets, linings, and insulating films, as well as square tanks that are subjected to strong acids and strong alkalis in the semiconductor industry. Powders such as shavings and scraps (hereinafter also referred to as "shavings, etc.") generated when cutting a primary molded body to form a secondary molded body, as well as powders obtained by crushing the shavings, etc., and powders obtained by crushing unwanted secondary molded bodies can be used as the fluororesin 1. In this specification, the shavings, etc. and powders are collectively referred to as "crushed material." The secondary molded body or shavings, etc. can be crushed using a crusher or the like. After the coarse crushing, it may be further pulverized. The volume of each crushed material is, for example, 50 cm 3 The following is the result.

[0020] <Fluororesin 2> Fluororesin 2 is a non-melt-moldable fluororesin produced by emulsion polymerization, and has no thermal history of being heated above its melting point. The fact that it "has no thermal history of being heated above its melting point" can be confirmed by differential scanning calorimetry (DSC). Emulsion polymerization is a polymerization method in which a monomer is polymerized in an aqueous medium containing water to obtain a dispersion containing particles of fluororesin 2 (hereinafter also referred to as "second dispersion"). Generally, emulsion polymerization is performed by a method in which a reaction liquid containing water, a polymerization initiator, and a surfactant is stirred while polymerizing the monomer in the reaction liquid. The aqueous emulsion after emulsion polymerization may be used as the second dispersion, or an aqueous dispersion obtained by blending the aqueous emulsion with a nonionic surfactant to improve storage stability may be used as the second dispersion.

[0021] From the viewpoint of suppressing coloration of the fluororesin molded article, the content of the nonionic surfactant per 100 parts by mass of the fluororesin in the second dispersion is preferably 2 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.1 parts by mass or less. Examples of nonionic surfactants will be described later.

[0022] The melting point of the fluororesin 2 is preferably 360°C or lower, more preferably 355°C or lower, and even more preferably 350°C or lower. There are no particular restrictions on the lower limit of the melting point, but it is preferably 100°C or higher, and more preferably 150°C or higher. The melting point is preferably 100 to 360°C, more preferably 100 to 350°C, and even more preferably 150 to 350°C. When the melting point is within the above range, the mechanical strength of the obtained molded article is likely to be improved.

[0023] The content of the fluororesin 2 relative to the total mass of the second dispersion is preferably from 5 to 40 mass %, more preferably from 7 to 35 mass %, and even more preferably from 10 to 30 mass %.

[0024] The average particle size of the fluororesin 2 contained in the second dispersion is preferably 0.05 to 0.5 μm, more preferably 0.08 to 0.45 μm, and even more preferably 0.10 to 0.35 μm. When the average particle size is within this range, the emulsion stability is excellent.

[0025] The fluororesin 2 preferably contains PTFE obtained by emulsion polymerization. In the method of producing PTFE by emulsion polymerization, TFE monomer is homopolymerized in the reaction solution, or TFE monomer is copolymerized with a monomer other than TFE monomer in the reaction solution to obtain a second dispersion in which PTFE particles are dispersed in a dispersion medium. For example, the second dispersion is obtained by emulsion polymerizing the TFE monomer, preferably for 1 to 20 hours, in the presence of an aqueous medium, a polymerization initiator, an anionic fluorine-containing emulsifier, and a stabilizing aid, preferably at a pressure of 0.5 to 3.0 MPa. The nonionic surfactant may also be blended. Alternatively, a dispersion may be obtained without using a fluorine-based surfactant by the methods described in WO 2021 / 085470, WO 2022 / 181662, etc.

[0026] Examples of the anionic fluorine-containing emulsifier will be described later. The amount of the anionic fluorine-containing emulsifier used in the emulsion polymerization step of TFE monomer is preferably 0.15 to 2.0 parts by mass, more preferably 0.2 to 1.0 part by mass, and even more preferably 0.2 to 0.5 part by mass, per 100 parts by mass of the PTFE to be produced.

[0027] As the stabilizing aid, paraffin wax, fluorine-based oil, fluorine-based solvent, silicone oil, etc. are preferred, with paraffin wax being more preferred. One stabilizing aid may be used alone, or two or more may be used in combination. Paraffin wax may be liquid, semi-solid, or solid at room temperature, with saturated hydrocarbons having 12 or more carbon atoms being preferred. The melting point of paraffin wax is preferably 40 to 65°C, more preferably 50 to 65°C. The amount of stabilizing aid used is preferably 0.1 to 12 parts by mass, more preferably 0.1 to 8 parts by mass, per 100 parts by mass of the aqueous medium used.

[0028] As the polymerization initiator, a water-soluble radical initiator or a water-soluble oxidation-reduction catalyst is preferably used. As the water-soluble radical initiator, persulfates such as ammonium persulfate and potassium persulfate; and water-soluble organic peroxides such as disuccinic acid peroxide, bisglutaric acid peroxide, and tert-butyl hydroperoxide are preferred. The polymerization initiator may be used alone or in combination of two or more. Oil-soluble initiators can also be used. As the polymerization initiator, disuccinic acid peroxide is more preferred. The amount of the polymerization initiator used is preferably 0.01 to 0.20 parts by mass, more preferably 0.01 to 0.15 parts by mass, per 100 parts by mass of the PTFE to be produced.

[0029] The standard specific gravity (SSG) of the PTFE contained in the second dispersion can be conceptually classified as high molecular weight PTFE when it is 2.14 or more and less than 2.22, and as low molecular weight PTFE when it is 2.22 to 2.4. Since the physical properties of PTFE decrease when the molecular weight is low, the SSG is preferably 2.14 or more and less than 2.22, and more preferably 2.14 to 2.21.

[0030] [Anionic Fluorine-Containing Emulsifier] Examples of the anionic fluorine-containing emulsifier used in emulsion polymerization include fluorine-containing emulsifiers represented by general formula (1) (hereinafter, also referred to as "fluorine-containing emulsifier (1)"). General formula (1): XCF 2 CF 2 (O) m CF 2 CF 2 OCF 2 COOA (wherein X is a hydrogen atom or a fluorine atom, and A is a hydrogen atom, an alkali metal, or NH 4 and m is 0 or 1. The fluorine-containing emulsifier (1) is preferred in that it has a good effect of stabilizing the polymerization of PTFE particles.

[0031] The X is preferably a fluorine atom in terms of polymerization stability. The m is preferably 1 in terms of polymerization stability and mechanical stability of the second dispersion. Specific examples of A include H, Li, Na, K, and NH. 4 The fluorine-containing emulsifier (1) has good solubility in water and metal ion components are unlikely to remain as impurities, and therefore, NH 4 Particularly preferred examples of the fluorine-containing emulsifier (1) are CF 3 CF 2 CF 2 CF 2 OCF 2 COONH 4 , C 2 F 5 OCF 2 CF 2 OCF 2 COONH 4 (hereinafter referred to as EEA), with EEA being more preferred.

[0032] The fluorine-containing emulsifier (1) can be produced by fluorinating an ester of a corresponding non-fluorine-containing carboxylic acid or partially fluorinated carboxylic acid by a known fluorination method such as a liquid-phase fluorination method in which the ester is reacted with fluorine in a liquid phase, a fluorination method using cobalt fluoride, or an electrochemical fluorination method, hydrolyzing the ester bond of the obtained fluorinated ester, purifying it, and then neutralizing it with ammonia.

[0033] [Nonionic fluorine-containing emulsifier] Examples of the nonionic surfactant to be blended in the aqueous emulsion obtained by emulsion polymerization include a nonionic surfactant represented by general formula (2) (hereinafter also referred to as "nonionic surfactant (2)") and a nonionic surfactant represented by general formula (3) (hereinafter also referred to as "nonionic surfactant (3)"). General formula (2): R 1 -O-D-H (wherein, R 1 is an alkyl group having 8 to 18 carbon atoms, O is an oxygen atom, and D is a polyoxyalkylene chain consisting of 5 to 20 oxyethylene groups and 1 to 2 oxypropylene groups.) General formula (3): R 2 -OE-G (wherein, R 2 is an alkyl group having 6 to 18 carbon atoms, O is an oxygen atom, E is a polyoxyalkylene chain consisting of 1 to 3 oxybutylene groups and 5 to 20 oxyethylene groups, and G is a hydrogen atom or a methyl group.) One type of nonionic surfactant may be used alone, or two or more types may be used in combination.

[0034] The nonionic surfactant contained in the second dispersion is preferably one or more selected from the group consisting of nonionic surfactants (2) and (3), and two or more of them may be used in combination. Nonionic surfactant (2) and nonionic surfactant (3) may also be used in combination.

[0035] Note that nonionic surfactants are mixtures of multiple molecules with a certain chain length distribution and a mixture of isomers, and the chain length of the polyoxyalkylene chain represents the average chain length of the multiple molecules. The number of oxyethylene groups and oxypropylene groups in the polyoxyalkylene chain is an average value. Also, when multiple types of nonionic surfactants are mixed and used, it is sufficient that the average number of oxyalkylene groups in each nonionic surfactant is within the above-mentioned range. Furthermore, each numerical value is not limited to an integer.

[0036] In the nonionic surfactant (2), R 1 The number of carbon atoms in the alkyl group represented by R is preferably in the range of 8 to 18, and more preferably 10 to 16. 1When the number of carbon atoms is equal to or greater than the lower limit of the above range, the surface tension of the second dispersion is likely to be low and the wettability is likely to be improved. When the number is equal to or less than the upper limit, the storage stability of the second dispersion is excellent. When the alkyl group, which is the hydrophobic group, has a branched structure in which it branches off midway, this is preferred in that the wettability of the second dispersion is likely to be improved. The alkyl group having a branched structure is preferably an alkyl group branched in the range from the carbon atom at the base of the alkyl group to the fifth carbon atom, and more preferably an alkyl group branched in the range from the carbon atom at the base of the alkyl group to the third carbon atom. The branched carbon atom may be a secondary carbon atom or a tertiary carbon atom, and a secondary carbon atom is preferred. The alkyl group having a branched structure includes, for example, C 10 H 21 CH (CH 3 ) CH 2 -, C 9 H 19 CH(C 3 H 7 ) -, C 6 H 13 CH(C 6 H 13 )- and the like can be exemplified.

[0037] In the nonionic surfactant (2), the hydrophilic group D is a polyoxyalkylene chain consisting of 5 to 20 oxyethylene groups and 1 to 2 oxypropylene groups. In particular, when the polyoxyalkylene chain is consisting of 7 to 12 oxyethylene groups and 1 to 2 oxypropylene groups, the properties of the second dispersion are favorable. When D contains an oxypropylene group, the defoaming property is likely to be improved. Having 2 or fewer oxypropylene groups is preferable in that it reduces the surface tension, making it easier to enhance wettability and reducing the risk of repellency during recoating. Furthermore, in D, the oxypropylene group may be present between the polyoxyethylene groups or may be bonded to the end of the polyoxyethylene chain. Bonding an oxypropylene group to the end of the polyoxyethylene chain tends to enhance the defoaming property. In particular, bonding an oxypropylene group to the molecular terminal of the polyoxyethylene chain tends to further enhance the defoaming property.

[0038] In the nonionic surfactant (2), the average number of oxyethylene groups per molecule is preferably 5 to 20, more preferably 7 to 12. When the average number of oxyethylene groups per molecule is equal to or greater than the lower limit of the above range, good storage stability is likely to be obtained. When the average number of oxyethylene groups per molecule is equal to or less than the upper limit of the above range, good wettability is likely to be obtained. As the nonionic surfactant (2), C 13 H 27 O (C 2 H 4 O) 8 C 3 H 6 OH, C 13 H 27 O (C 2 H 4 O) 9 C 3 H 6 OH, C 13 H 27 O (C 2 H 4 O) 10 (C 3 H 6 O) 2 H, C 16 H 27 O (C 2 H 4 O) 12 (C 3 H 6 O) 2 Commercially available nonionic surfactants having an average molecular structure such as H can be used.

[0039] The content of the nonionic surfactant (2) is preferably 2 to 12 parts by mass, more preferably 4 to 12 parts by mass, per 100 parts by mass of the fluororesin in the second dispersion. When the content is equal to or greater than the lower limit of the above range, good storage stability is likely to be obtained. A high content of the nonionic surfactant (2) is suitable for applications requiring thick coating, but no improvement in performance is observed even when the content exceeds the upper limit of the above range, and therefore, for economic reasons, it is preferably equal to or less than the upper limit of the above range.

[0040] In the nonionic surfactant (3), R 2The number of carbon atoms in the alkyl group represented by the formula (I) is preferably in the range of 6 to 18, more preferably 8 to 16, and even more preferably 10 to 14. When the number of carbon atoms in the alkyl group is equal to or greater than the lower limit of the above range, the surface tension of the second dispersion tends to be low and wettability tends to be enhanced. When the number of carbon atoms in the alkyl group is equal to or less than the upper limit of the above range, the second dispersion tends to have excellent storage stability. When the number of carbon atoms in the alkyl group is within the above range, the wettability and storage stability are good.

[0041] R 2 It is preferable that the alkyl group represented by the formula (I) has a branched structure, since it is easier to increase the wettability of the second dispersion. The branched carbon atom may be a secondary carbon atom or a tertiary carbon atom, and a secondary carbon atom is preferred. The alkyl group having a branched structure is preferably a C 10 H 21 CH (CH 3 ) CH 2 -, C 9 H 19 CH(C 3 H 7 ) -, C 6 H 13 CH(C 6 H 13 ) -, CH(CH 3 ) 2 CH 2 CH (CH 3 ) 2 CH 2 CH (CH (CH 3 ) 2 CH 2 - etc. can be exemplified. 2 In the alkyl group represented by the formula (I), 10% or less of the hydrogen atoms in the alkyl group may be substituted with a halogen atom such as a fluorine atom, a chlorine atom, a bromine atom, etc. The alkyl group may also contain one or two unsaturated bonds.

[0042] E in general formula (3) is a polyoxyalkylene chain consisting of 1 to 3 oxybutylene groups and 5 to 20 oxyethylene groups. The number of oxybutylene groups is preferably 1 to 2.5, more preferably 1 to 2. When it is equal to or greater than the lower limit of the above range, the defoaming properties, wettability, and viscosity properties tend to be good. When it is equal to or less than the upper limit, the viscosity increase of the second dispersion is suppressed, and good stability is likely to be obtained. When it is within the above range, properties such as viscosity, stability, defoaming properties, and wettability are good, which is preferable. The oxybutylene group may be branched or linear, with branched being preferred.

[0043] The oxybutylene group is —CH 2 -CH(C 2 H 5 )-O-,-CH(C 2 H 5 ) CH 2 -O-, -CH(CH 3 )-CH(CH 3 ) —O—, —CH 2 CH 2 -CH(CH 3 ) —O—, —CH 2 CH 2 CH 2 CH 2 Among them, —CH 2 -CH(C 2 H 5 )-O-,-CH(C 2 H 5 ) CH 2 —O—, —CH 2 CH 2 -CH(CH 3 )-O- is preferred. Examples of raw materials for the oxybutylene group include various butylene oxides, and specific examples include 1,2-butylene oxide, 2,3-butylene oxide, tetrahydrofuran, and methyloxetane.

[0044] In the nonionic surfactant (3), the number of oxyethylene groups in the polyoxyalkylene chain is 5 to 20, preferably 6 to 15, and more preferably 7 to 13. When the number is equal to or greater than the lower limit of the above range, the storage stability of the second dispersion tends to be good. When the number is equal to or less than the upper limit, the wettability tends to be good. When the number is within the above range, properties such as viscosity, stability, defoaming property, and wettability are good, which is preferable. The oxybutylene groups in the polyoxyalkylene chain may have a block structure or a random structure.

[0045] The oxybutylene group may be present at any position in the polyoxyalkylene chain, but R 2 It is preferable that the —O— group is present in the range up to 70% of the total length of the polyoxyalkylene chain, and R 2 It is more preferable that the R of the polyoxyalkylene chain is present in the range from the —O— group side to 50% of the total length of the polyoxyalkylene chain. 2 The portion bonded to the -O- group is preferably an oxybutylene group, more preferably a polyoxybutylene chain consisting of 1 to 2 oxybutylene groups. Furthermore, the portion of the polyoxyalkylene chain bonded to the G group is preferably an oxyethylene group, more preferably a polyoxyethylene chain consisting of 5 to 20 oxyethylene groups. Polyoxyalkylene chains having these preferred structures are preferred because they have better properties such as viscosity, stability, defoaming properties, and wettability. G in general formula (3) is a hydrogen atom or a methyl group, preferably a hydrogen atom.

[0046] The nonionic surfactant (3) can be obtained by addition reaction of butylene oxide and ethylene oxide with a higher alcohol by a known method. Butylene oxide and ethylene oxide may be mixed and reacted simultaneously, or butylene oxide may be reacted first and then ethylene oxide, or ethylene oxide may be reacted first and then butylene oxide. The method of reacting butylene oxide first and then ethylene oxide is preferred.

[0047] As the nonionic surfactant (3), C 13H 27 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 H、C 10 H 21 HH(H) 3 )CH 2 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 H、C 10 H 21 HH(H) 3 )CH 2 OCH(C 2 H 5 )CH 2 O(C 2 H 4 O) 8 H、C 12 H 25 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 H、C 8 H 17 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 10 H、C 12 H 25 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 10 H、C 13 H 27 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 11 H、C 13 H 27 OCH 2 CH 2 OCH 2 CH(C2 H 5 )O(C 2 H 4 O) 8 H、C 12 H 25 O(CH 2 CH(C 2 H 5 )O) 2 (C 2 H 4 O) 8 H、C 10 H 21 CH(CH 3 )CH 2 O(C 2 H 4 O) 9 CH 2 CH(C 2 H 5 )OH、C 16 H 33 OC 2 H 4 P.S. 2 H 5 )CH 2 O(C 2 H 4 O) 9 H、C 12 H 25 SO 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 CH 2 CH(C 2 H 5 )OH、C 13 H 27 P.S. 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 10 H 21 CH(CH 3 )CH 2 P.S. 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 10 H 21 CH(CH 3)CH 2 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 12 H 25 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 8 H 17 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 10 H、C 12 H 25 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 10 H、C 13 H 27 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 11 H、C 13 H 27 O(CH) 2 ) 4 O(C 2 H 4 O) 8 H、C 12 H 25 O(CH) 2 ) 4 O(C 2 H 4 O) 8 H、C 8 H 17 O(CH) 2 ) 4 O(C 2 H 4 O) 10 H、C 12 H 25 O(CH) 2 ) 4 O(C 2 H 4 O) 10 H、C 13 H27 O(CH 2 ) 4 O(C 2 H 4 O) 11 H, C 13 H 27 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 8 H, C 12 H 25 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 8 H, C 8 H 17 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 10 H, C 12 H 25 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 10 H, C 13 H 27 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 11 Examples thereof include H, etc.

[0048] When the second dispersion contains a nonionic surfactant (3), the content of the nonionic surfactant (3) is preferably 0.1 to 12 parts by mass, more preferably 0.5 to 11 parts by mass, and even more preferably 1 to 10 parts by mass, per 100 parts by mass of the fluororesin in the second dispersion. When the content is equal to or greater than the lower limit of the above range, good storage stability is likely to be obtained. In addition, cracks are less likely to occur in the fluororesin coating film, and repellency is less likely to occur. A high content of nonionic surfactant (3) is suitable for applications requiring thick coating, but no improvement in performance is observed even when the content exceeds the upper limit of the above range, and therefore, for economic reasons, it is preferable that the content be equal to or less than the upper limit of the above range.

[0049] When nonionic surfactant (2) and nonionic surfactant (3) are used in combination as a nonionic surfactant, the average number of oxybutylene groups per molecule of the nonionic surfactant as a whole is preferably 0.5 to 2, more preferably 0.7 to 1.7, and even more preferably 0.9 to 1.5. Nonionic surfactant (2) and nonionic surfactant (3) may be added separately. A mixture containing nonionic surfactant (3) and nonionic surfactant (2) by-produced during the preparation of nonionic surfactant (3) may also be used.

[0050] The second dispersion contains water as a dispersion medium for the fluororesin particles. This water may be water contained in the aqueous emulsion obtained by emulsion polymerization, or may be water prepared separately from the water in the aqueous emulsion.

[0051] The second dispersion may contain, as necessary, one or more of a pH adjuster (e.g., ammonia), an anionic surfactant, a polyethylene oxide-based thickener, a polyurethane-based thickener, a thixotropy-imparting agent, a silicone-based wettability improver, a fluorine-based wettability improver, a preservative, and the like.

[0052] Furthermore, one or more of water-soluble organic solvents, organic solvents (e.g., toluene, xylene, etc.), pigments (e.g., titanium oxide, iron oxide, carbon black, cobalt blue, etc.), glass powder, hollow glass beads, and colorants (e.g., graphite particles, silica particles, mica or titanium oxide-coated mica powder, etc.) may be blended.

[0053] <Fluororesin Composition> The fluororesin composition contains fluororesin 1 and fluororesin 2. It may further contain one or more solid components other than fluororesin 1 and fluororesin 2. Examples of other solid components include solid components used in the production process of fluororesin 1, solid components used in the production process of fluororesin 2, and solid components added after the production of fluororesin 1 and fluororesin 2. Specific examples include inorganic fillers, pigments (e.g., titanium oxide, iron oxide, carbon black, cobalt blue, etc.), colorants (e.g., graphite particles, silica particles, mica or titanium oxide-coated mica powder, etc.), and the above-mentioned additives. Examples of inorganic fillers include reinforcing fibers (e.g., glass fiber, carbon fiber, etc.), glass powder, bronze powder, graphite powder, hollow glass beads, etc. The content of other solid components is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, based on the total mass of the solid contents of the fluororesin composition. It may be zero.

[0054] A powdered fluororesin composition is used for compression molding. Examples of methods for producing a powdered fluororesin composition include the following modes (1) to (4), with mode (4) being preferred. (1) Powdered fluororesin 1 and powdered fluororesin 2 are mixed in a dry state. (2) Powdered fluororesin 1 is mixed with a dispersion in which fluororesin 2 is dispersed, and the solid in the resulting mixture is powdered. (3) The dispersion in which fluororesin 1 is dispersed is mixed with powdered fluororesin 2, and the solid in the resulting mixture is powdered. (4) The dispersion in which fluororesin 1 is dispersed is mixed with a dispersion in which fluororesin 2 is dispersed, and the solid in the resulting mixture is powdered.

[0055] The dispersion in which fluororesin 1 is dispersed (hereinafter also referred to as "first dispersion") is preferably a dispersion obtained by mixing powdered fluororesin 1 produced by the above-mentioned production method with a water-soluble organic solvent. From the viewpoint of miscibility with fluororesin 1 and water, the water-soluble organic solvent is preferably one or more water-soluble organic solvents selected from the group consisting of aprotic water-soluble organic solvents and alcohols. The alcohols may have an amino group or an alkoxy group as a substituent. The aprotic water-soluble organic solvent is preferably acetone, tetrahydrofuran, or acetonitrile. The alcohol is preferably methanol, ethanol, propanol, isopropyl alcohol, or 1-methoxy-2-propanol. Of these, isopropyl alcohol is more preferable as the water-soluble organic solvent. One type of water-soluble organic solvent may be used alone, or two or more types may be used in combination.

[0056] The content of the fluororesin 1 relative to the total mass of the first dispersion is preferably from 3 to 70 mass %, more preferably from 5 to 65 mass %, and even more preferably from 10 to 60 mass %.

[0057] The second dispersion is preferred as the dispersion having the fluororesin 2 dispersed therein. When using a powdered fluororesin 2, the powdered fluororesin 2 may be obtained by separating the fluororesin 2 from the solvent in the second dispersion by filtration, drying, or the like.

[0058] In the cases of the above embodiments (2) to (4), the mixture is stirred to aggregate fluororesin 1 and fluororesin 2, and then filtered to separate the aggregates from the dispersion medium into solid and liquid, followed by drying, to obtain a powdery fluororesin composition. The aggregates obtained by solid-liquid separation may be washed before drying. Water or an aqueous solution is preferred as the washing solvent. When the aggregates contain a water-soluble organic solvent, it is preferred to use a washing solvent whose pH is adjusted to a value that allows the water-soluble organic solvent to be removed. The aggregates may be dried by vacuum drying or atmospheric drying. It is preferred to dry the aggregates at a temperature equal to or lower than the melting point of the fluororesin for 6 hours or longer.

[0059] The glossiness of the molded body can be adjusted by the conditions of the aggregation step in which the mixture is stirred to obtain the aggregate. For example, increasing the temperature of the mixture in the aggregation step tends to decrease the glossiness. Furthermore, increasing the stirring intensity in the aggregation step tends to increase the glossiness. The stirring intensity can be adjusted by the rotation speed of the stirring blades, the shape of the stirring blades, and the number and shape of the baffles. These adjustment methods may also be combined.

[0060] In the cases of the above embodiments (2) to (4), the combined content of fluororesin 1 and fluororesin 2 relative to the total mass of the mixture is preferably 10 to 50 mass%, more preferably 12 to 45 mass%, and even more preferably 15 to 35 mass%. When the combined content of fluororesin 1 and fluororesin 2 is equal to or greater than the lower limit of the above range, fluororesin 1 and fluororesin 2 tend to aggregate, facilitating solid-liquid separation. When the combined content of fluororesin 1 and fluororesin 2 is equal to or less than the upper limit of the above range, mixing of fluororesin 1 and fluororesin 2 is likely to be promoted.

[0061] In the case of the above embodiment (4), the content of the water-soluble organic solvent relative to 100 parts by mass of water in the mixture is preferably 1 to 150 parts by mass, more preferably 3 to 140 parts by mass, and even more preferably 5 to 130 parts by mass.

[0062] The proportion of fluororesin 1 relative to the total mass of fluororesin 1 and fluororesin 2 is 40 mass% or more, preferably 45 mass% or more, more preferably 50 mass% or more, even more preferably 52 mass% or more, and particularly preferably 55 mass% or more. When the proportion of fluororesin 1 is at least the lower limit of the above range, it is easy to adjust the gloss of the molded product to 15% or more. The upper limit is not particularly limited, and is, for example, less than 100 mass%.

[0063] <Molded body> The molded body of the present invention can be obtained by compression molding the fluororesin composition and firing it. Specifically, the powdered fluororesin composition is placed in a mold and compression molded under pressure to obtain a preform, and the preform is fired to obtain a primary molded body. The shape of the primary molded body is not particularly limited. For example, it may be a block shape such as a cylindrical or polygonal pillar shape.

[0064] When the fluororesin composition is compression molded, the pressure is 100 to 350 kg / cm 2 The baking temperature after the preforming is preferably 360 to 380°C.

[0065] The obtained primary molded article may be processed by cutting or the like to produce a secondary molded article of a desired shape. Examples of uses of the secondary molded article include seals, packings, rollers, sockets, and joints.

[0066] The fluororesin molded article of the present invention may be either the primary molded article or the secondary molded article. The glossiness of the fluororesin molded article of the present invention is 15% or more, preferably 18% or more, and more preferably 20% or more. When the glossiness is equal to or greater than the above lower limit, good compressive strength and compressive creep resistance can be obtained. The upper limit of the glossiness is not particularly limited.

[0067] The reason why good compressive strength and compressive creep resistance can be obtained when the gloss of the molded product is equal to or higher than the above lower limit is thought to be because the gloss is derived from the mixing and dispersibility of fluororesin 1 and fluororesin 2.

[0068] The compressive strength of the fluororesin molded article of the present invention is preferably 3 MPa or more (1% deformation) and 12 MPa or more (10% deformation). More preferably, the compressive strength (1% deformation) is 3.3 MPa or more and the compressive strength (10% deformation) is 13 MPa or more, and even more preferably, the compressive strength (1% deformation) is 3.5 MPa or more and the compressive strength (10% deformation) is 14 MPa or more. There is no particular upper limit to the compressive strength. The compressive strength in this specification is a value obtained by the measurement method described in the Examples.

[0069] The compression creep properties of the fluororesin molded article of the present invention are preferably such that the compression creep (deformation) is 15% or less and the compression creep (permanent deformation) is 12% or less. More preferably, the compression creep (deformation) is 13% or less and the compression creep (permanent deformation) is 11% or less, and even more preferably, the compression creep (deformation) is 10% or less and the compression creep (permanent deformation) is 10% or less. There is no particular restriction on the lower limit of the compression creep. The compression creep in this specification is a value obtained by the measurement method described in the Examples.

[0070] The present invention will be explained in more detail below using examples, but the present invention is not limited to these examples.

[0071] <Measurement Method> [Melting Point] Using a differential scanning calorimeter (DSC 8500, manufactured by Perkin Elmer), the fluororesin was heated to 380° C. at a rate of 10° C. / min in an air atmosphere, and the melting point was determined from the endothermic peak. When there were multiple endothermic peaks, the peak temperature of the largest endothermic peak was used.

[0072] [Average particle size] Powdered fluororesin was dispersed in water using a laser diffraction / scattering particle size distribution analyzer (LA-920, manufactured by Horiba, Ltd.), and the particle size distribution was measured on a number basis to calculate. [Standard specific gravity (SSG)] Measured in accordance with ASTM D1457-91a and D4895-91a.

[0073] [Glossiness] 345 g of the fluororesin composition was placed in a mold with an inner diameter of 7.3 mm and subjected to a pressure of 320 kg / cm 2 A preform was obtained by pressing at 380°C. This preform was baked at 380°C for 2 hours to obtain a fluororesin molded article. The gloss was evaluated using a sheet-like molded article having a thickness of 0.5 mm obtained by skiving the obtained fluororesin molded article. The specular gloss was measured at an incident angle of 60° using a PG-IIM manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS Z 8741.

[0074] [Compression strength] A test piece was prepared as follows: 6.5 g of the fluororesin composition was placed in a mold with an inner diameter of 12.95 mm, and compressed at 320 kg / cm 2A preform was obtained by pressing at 380°C for 2 hours to obtain a test piece having a diameter of 12.7 mm and a height of 25.4 mm. The compressive strength was measured in accordance with ASTM D695 using a Tensilon universal testing machine (RTF-1350 manufactured by Orientec Co., Ltd.). The compressive strength (1% deformation) indicates the compressive stress when the strain is 1%. The larger this value, the better the compressive strength. The compressive strength (10% deformation) indicates the compressive stress when the strain is 10%. The larger this value, the better the compressive strength.

[0075] [Compression creep property] A test piece was prepared as follows: 6.5 g of the fluororesin composition was placed in a mold having an inner diameter of 12.95 mm, and subjected to a pressure of 320 kg / cm 2 A preform was obtained by pressing at 380°C for 2 hours and processed into a test specimen with a diameter of 12.7 mm and a height of 12.7 mm. Compression creep properties were measured in accordance with ASTM D621 using a creep tester (145-SV-3 manufactured by Yasuda Seiki Seisakusho). Specifically, a load of 13.7 MPa was applied to the test specimen at 24°C, and the strain after 10 seconds was considered to be the initial deformation. The strain was measured again after 24 hours, and the compression creep (deformation) was calculated using the following formula. A smaller value indicates better compression creep properties. Compression creep (deformation) = (change in height after 24 hours [mm] - initial deformation [mm]) / height of test specimen before measurement [mm] x 100. Compression creep (permanent deformation) was measured from the test specimen dimensions 24 hours after the completion of the above test using the following formula. A smaller value indicates better compression creep properties. Compression creep (permanent deformation) = height of test piece 24 hours after the end of loading [mm] / height of test piece before measurement [mm] × 100

[0076] The following Example 1 is an embodiment, and Examples 2 and 3 are comparative examples.

[0077] Example 1 Powdered fluororesin 1 was produced by the following method. A powder (molding powder, melting point before heating: 343°C) made of unsintered PTFE homopolymer obtained by suspension polymerization was preformed and sintered to obtain a molded body. The obtained molded body was pulverized to obtain PTFE with an average particle size of 40 μm or less. The melting point of the obtained PTFE was 329°C and the bulk density was 394 g / L. The obtained PTFE was not melt-moldable, as there was no temperature at which the melt flow rate was 0.1 to 1000 g / 10 min at temperatures 20°C or more higher than the melting point of the resin under a load of 49 N.

[0078] A dispersion of fluororesin 2 (second dispersion) was produced by the following method. EEA was used as the anionic fluorine-containing emulsifier (1). 36 g of EEA, 555 g of paraffin wax (melting point 55°C), and 61.3 L of deionized water were charged into a 100 L stainless steel autoclave equipped with a baffle and a stirrer. After the interior of the autoclave was purged with nitrogen and reduced pressure, TFE monomer was introduced and the temperature was raised to 62°C with stirring. TFE monomer was further injected until the internal pressure reached 1.765 MPa, and 26.3 g of disuccinic acid peroxide (concentration 80% by mass, the remainder being water) dissolved in 1 L of warm water at approximately 70°C was added.

[0079] After about 3 minutes, the internal pressure of the autoclave dropped to 1.716 MPa, so TFE monomer was injected to maintain the internal pressure at 1.765 MPa, and polymerization was allowed to proceed. During the polymerization, EEA was dissolved in warm water and a total of 53 g of EEA was injected in two batches. The autoclave temperature was gradually raised to 72 ° C., and when the amount of injected TFE monomer reached 22 kg, the reaction was terminated and the TFE in the autoclave was released into the atmosphere. The polymerization time was 105 minutes. After cooling, the paraffin wax solidified at the top was removed to obtain a second dispersion.

[0080] The content of PTFE relative to the total mass of the second dispersion was approximately 25.0 mass%, and the content of EEA relative to 100 mass parts of PTFE was 0.40 mass parts. The average particle size of PTFE particles in the second dispersion was 0.26 μm. The standard specific gravity (SSG) of PTFE was 2.21. The melting point of the obtained PTFE was 337°C. The obtained PTFE was not melt-moldable, as there was no temperature at which the melt flow rate was 0.1 to 1000 g / 10 min at a temperature 20°C or more higher than the melting point of the resin under a load of 49 N.

[0081] A powdered fluororesin composition was produced by the following method. A first dispersion was prepared by mixing 200 g of the powdered fluororesin 1 (PTFE) obtained above with 200 g of isopropanol (IPA). 798 g of the second dispersion obtained above and 802 g of water were placed in an 8-L stainless steel vessel equipped with a baffle and a stirrer. The mixture was stirred at 25°C under atmospheric pressure, and then the first dispersion was added to obtain a mixture. The fluororesin 1 accounted for 50.0 mass% of the total mass of the first dispersion. The mass ratio of PTFE in the second dispersion to the fluororesin 1 powder (PTFE) was 1:1. The mass ratio of IPA in the first dispersion to water in the second dispersion was 12:88. The total content of the fluororesin (PTFE) was 20.0 mass% of the total mass of the mixture.

[0082] Subsequently, an aggregation step was carried out. That is, the mixture was stirred at 680 rpm for 10 minutes using a stirrer at 25°C under normal pressure to aggregate the solids in the mixture. Thereafter, the aggregates were separated from the solvent by filtration using a sieve. The aggregates were washed with a large amount of water, placed in a tray, and vacuum dried at 25°C for 8 hours or more, and then dried at 200°C for 10 hours or more, thereby obtaining a powdery fluororesin composition. The proportion of fluororesin 1 relative to the total mass of fluororesin 1 and fluororesin 2 contained in the obtained fluororesin composition was 50 mass%.

[0083] The obtained fluororesin composition was placed in a mold of a predetermined shape and subjected to a pressure of 320 kg / cm 2 This preform was baked at 380° C. for 2 hours to obtain a fluororesin molded article (primary molded article) of Example 1.

[0084] The gloss, compressive strength and compressive creep properties of the fluororesin molded articles were evaluated using the methods described above. The results are shown in Table 1 (the same applies hereinafter).

[0085] <Reference Example 1> In Example 1, the molding powder (powder made of unsintered PTFE homopolymer obtained by suspension polymerization) used in Example 1 was used instead of the fluororesin composition. Except for this, a fluororesin molded article (primary molded article) was produced in the same manner as in Example 1 and evaluated.

[0086] <Example 2> In place of the fluororesin composition in Example 1, powder of fluororesin 1 was used. Except for this, an attempt was made to produce a fluororesin molded product in the same manner as in Example 1. However, the adhesion between the fluororesin particles was insufficient, and no molded product was obtained. Therefore, gloss, compressive strength, and compressive creep tests were not performed.

[0087] Example 3 In place of the fluororesin composition in Example 1, a powder of fluororesin 2 was used. That is, when producing a powdered fluororesin composition, the first dispersion was not used, and fluororesin 2 in the second dispersion was aggregated and filtered, and the resulting aggregates were vacuum-dried at 25°C for 8 hours or more and then dried at 200°C for 10 hours or more to obtain powdered fluororesin 2. Except for this, a fluororesin molded article was produced in the same manner as in Example 1. When the resulting fluororesin molded article was compressed in a compression test, numerous voids were generated.

[0088]

[0089] As shown in the results in Table 1, the fluororesin molded product of Example 1 had a glossiness of 15% or more, and despite containing fluororesin 1, which was obtained by pulverizing the baked product of suspension-polymerized PTFE, as a raw material, it exhibited compressive strength and compressive creep properties comparable to those of the fluororesin molded product of Reference Example 1, which was made from unbaked suspension-polymerized PTFE.

Claims

1. A molded product obtained by compression molding and sintering a fluororesin composition comprising a first fluororesin having a thermal history of being heated to or above its melting point and a second fluororesin having no thermal history of being heated to or above its melting point, wherein the first fluororesin is a non-melt-formable fluororesin, and the second fluororesin is a non-melt-formable fluororesin produced by emulsion polymerization, the proportion of the first fluororesin relative to the total mass of the first fluororesin and the second fluororesin is 40 mass% or more, and the gloss of the molded product at an incident angle of 60° is 15% or more.

2. A fluororesin molded article according to claim 1, wherein the first fluororesin and the second fluororesin are each independently a fluororesin containing 99% by mass or more of tetrafluoroethylene units relative to the total mass of the fluororesin.

Citation Information

Patent Citations

  • Game machine

    JP2023091849A

  • Method for producing sintered fluororesin body, sintered fluororesin body, method for producing fluororesin dispersion, method for producing sintered body, fluororesin dispersion, and sintered body

    JP6612001B1

  • Method for producing polytetrafluoroethylene aqueous dispersion

    WO2021085470A1

  • Method for producing polytetrafluoroethylene aqueous dispersion

    WO2022181662A1

  • Light diffusion cover and lighting fixture using the light diffusion cover

    JP2011171104A