Cellulose acetate powder

A cellulose acetate powder with controlled particle size distribution and specific properties addresses the challenges of productivity and thermoplasticity in conventional methods, resulting in improved processability and product quality, enabling efficient and cost-effective production.

WO2024248165A1PCT designated stage Publication Date: 2024-12-05DAICEL CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/028060
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional methods for producing cellulose acetate face challenges such as low productivity, high costs, and poor thermoplasticity, leading to material loss and thermal decomposition during thermoforming, especially when using the vacuum acetylation method.

Method used

The development of a cellulose acetate powder with a controlled particle size distribution and specific physical properties, including an acetyl substitution degree of 2.0 to 2.6 and a sulfuric acid component amount of 50 ppm or less, which improves processability and reduces unmelted particles during extrusion, thereby enhancing yield and product quality.

Benefits of technology

The cellulose acetate powder achieves improved thermoplasticity, reduced material loss, and higher quality molded products with enhanced thermal stability and melt fluidity, allowing for efficient and cost-effective production across various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024028060_05122024_PF_FP_ABST
    Figure JP2024028060_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The cellulose acetate powder is a powder comprising cellulose acetate as a main component. The cellulose acetate has a degree of acetyl substitution of 2.0-2.6 and a sulfuric acid component content of 50 ppm or less. The cellulose acetate powder has a particle size distribution in which the proportion of particles having a particle size of 1000 μm or more is 40 wt% or less.
Need to check novelty before this filing date? Find Prior Art

Description

cellulose acetate powder

[0001] The present disclosure relates to cellulose acetate powder.

[0002] In recent years, growing concern about the global environment has led to the development of biodegradable cellulose acetate as a molding material in various technical fields. The so-called acetic acid method, which uses acetic anhydride, acetic acid, and a sulfuric acid catalyst, is commonly used to produce cellulose acetate. The basic steps of the acetic acid method include a pretreatment activation step in which a pulp raw material (dissolving pulp) with a relatively high α-cellulose content is disintegrated and then mixed with acetic acid; an acetylation step in which a mixture of acetic anhydride, acetic acid, and a sulfuric acid catalyst is added to the pretreated activated pulp; an aging step (hydrolysis step) in which the highly substituted cellulose acetate obtained by acetylation is hydrolyzed to the desired degree of substitution; and a post-treatment step in which the hydrolyzed cellulose acetate is separated from the reaction solution and purified, stabilized, and dried.

[0003] The acetic acid process described above uses a single type of softwood pulp as the pulp raw material and requires a large amount of sulfuric acid catalyst and acid. Furthermore, to improve thermal stability, it is necessary to minimize the number of sulfate ester groups introduced into the glucose rings of cellulose during the reaction, and the sulfuric acid in the system is neutralized in multiple stages just before the end of the reaction. This results in low productivity, high costs, and difficulty in broadening its applications.

[0004] Patent Document 1 (JP 2018-58941 A) proposes a method for producing cellulose acetate with excellent hue using low-grade pulp as a raw material. This production method includes a hydrolysis step in which the temperature in the hydrolysis reaction system is maintained at a temperature above 80°C and not higher than 90°C for 100 to 150 minutes.

[0005] Patent Document 2 (Japanese Patent Laid-Open Publication No. 60-139701) proposes a method for producing cellulose acetate (so-called reduced pressure acetylation method) in which the pressure in the reaction system is reduced during the entire period of the acetylation reaction or during a part of the period including the initial period, and the generated gas is condensed and distilled out of the reaction system, thereby concentrating the reaction product.

[0006] The reduced pressure acetylation method uses less sulfuric acid catalyst and acid than the conventional acetic acid method, and can use a mixture of multiple tree species, such as softwood and hardwood, as pulp raw materials. Furthermore, because the amount of sulfuric acid used is small, fewer sulfate ester groups are introduced during the reaction, making the conventional multi-stage neutralization unnecessary, which is expected to reduce costs and improve productivity.

[0007] However, cellulose acetate has been known to have poor thermoplasticity. In particular, when cellulose acetate produced by the reduced pressure acetylation method is pelletized using a twin-screw extruder, problems arise, such as strand breakage making it impossible to produce the pellets or a loss of material of about 10-20% due to a low yield.

[0008] For example, in Patent Document 3 (JP 2017-52961 A), in order to facilitate thermoforming, 20 to 40 parts by weight of a plasticizer is added to 100 parts by weight of cellulose acetate powder, which is made of cellulose acetate having an acetylation degree of 53 to 56% and a 6% viscosity of 30 to 200 mPa·s, a cumulative pore volume of 0.200 ml / g or more, a ratio of particles with a particle size of 500 μm or more of 40% or less, and an angle of repose of 51° or less.

[0009] JP 2018-58941 A JP 60-139701 A JP 2017-52961 A

[0010] Although the addition of plasticizers improves the processability of cellulose acetate, for example, when thermoforming cutlery, sufficient melt fluidity cannot be obtained, and material loss due to strand breakage cannot be avoided. Changing the screw configuration or extrusion conditions to reduce strand breakage increases shear and the resin temperature, which can lead to problems such as discoloration (yellowing) and odor (acetic acid odor) due to thermal decomposition of the cellulose acetate.

[0011] An object of the present disclosure is to solve the above-mentioned problems and provide a cellulose acetate powder that is low in cost and has excellent processability.

[0012] The present inventors have discovered that unmelted particles remaining during extrusion molding of cellulose acetate are one cause of strand breakage, and have arrived at the configuration of the present disclosure by finding that controlling the particle size distribution of powder made of cellulose acetate with specific physical properties improves processability and also improves the quality of the resulting molded product.

[0013] That is, the cellulose acetate powder of the present disclosure is a powder mainly composed of cellulose acetate. The cellulose acetate has an acetyl substitution degree of 2.0 to 2.6 and a sulfuric acid content of 50 ppm or less. The cellulose acetate powder has a particle size distribution in which the proportion of particles with a particle diameter of 1000 μm or more is 40% by weight or less.

[0014] The cellulose acetate powder of the present disclosure has high production efficiency and low cost, and therefore can be used in a variety of fields that have not been applicable in the past. Moreover, the cellulose acetate powder of the present disclosure improves yield during molding processing and enables the production of high-quality molded products.

[0015] Figure 1 shows the particle size distributions of Examples and Comparative Examples on a weight basis as determined by a sieving test, and Figure 2 shows the particle size distributions of Examples and Comparative Examples on a volume basis as determined by a laser diffraction / scattering method.

[0016] An example of a preferred embodiment will be described in detail below. Each configuration and combination thereof in each embodiment is merely an example, and addition, omission, substitution, and other modifications of configurations are possible as appropriate within the scope of the present disclosure. The present disclosure is not limited by the embodiments, but only by the scope of the claims. Furthermore, each aspect disclosed in this specification can be combined with any other feature disclosed in this specification.

[0017] In this disclosure, the range "X to Y" means "X or more and Y or less." Unless otherwise noted, all test temperatures were room temperature (20°C ± 5°C), and "wt %" means weight percent, not mass concentration.

[0018] (Cellulose Acetate Powder) The cellulose acetate powder of the present disclosure is a powder mainly composed of cellulose acetate, which has an acetyl substitution degree of 2.0 to 2.6 and a sulfuric acid content of 50 ppm or less.

[0019] In this specification, the term "main component" means the component that is contained in the cellulose acetate powder at the highest content rate, and its content rate is at least 70% by weight, preferably 90% by weight or more, and more preferably 95% by weight or more.

[0020] In the present disclosure, "cellulose acetate" refers to a cellulose ester in which some or all of the hydroxyl groups of cellulose have been replaced with acetyl groups. Cellulose acetate may have substantially no substituents other than acetyl groups, but may have acyl groups other than acetyl groups to impart other properties and to the extent that the effects of the present disclosure are not impaired. Furthermore, trace amounts of sulfate groups may be introduced into cellulose acetate as a result of the use of a sulfuric acid catalyst during the production of cellulose acetate. In the present disclosure, the inclusion of sulfate groups unintentionally and unavoidably introduced during the production of cellulose acetate is permitted. Pulp, the raw material for cellulose acetate, may contain components other than cellulose, such as hemicellulose and lignin. In this specification, the term "cellulose acetate" also refers to a material containing components derived from hemicellulose and other raw materials.

[0021] In this specification, the term "powder" refers to an aggregate of a plurality of solid particles, and more specifically, is defined as an aggregate of particles of different sizes having a specific particle size distribution.

[0022] The cellulose acetate powder of the present disclosure is endowed with good thermoplasticity and thermal stability by the cellulose acetate having an acetyl substitution degree of 2.0 to 2.6 and a sulfuric acid content of 50 ppm or less. This cellulose acetate can be obtained by the low-cost method using the above-mentioned reduced pressure acetylation method.

[0023] Furthermore, the cellulose acetate powder of the present disclosure has a particle size distribution in which the proportion of particles with a particle diameter of 1000 μm or more is 40% by weight or less. When a powder with this particle size distribution is heated at the melting temperature, few particles remain unmelted. The present inventors have found that, particularly when a powder made of cellulose acetate having an acetyl substitution degree of 2.0 to 2.6 and a sulfuric acid content of 50 ppm or less is heated and melted, setting the proportion of particles with a particle diameter of 1000 μm or more to 40% by weight or less significantly reduces the number of unmelted particles and strand breakage, thereby reducing strand breakage. Furthermore, this cellulose acetate powder has superior melt fluidity compared to cellulose acetate conventionally used in industry. Therefore, it is possible to select an extruder configuration and extrusion conditions that can suppress thermal decomposition of cellulose acetate. This allows for the production of high-quality pellets and molded products with reduced yellowness and acetic acid odor. According to the present disclosure, a cellulose acetate powder with low material loss during thermoforming and excellent processability can be provided at low cost.

[0024] (Particle size distribution) In this specification, the particle size distribution of the cellulose acetate powder will be described in terms of both a weight-based particle size distribution determined by a sieving method and a volume-based particle size distribution determined by a laser diffraction / scattering method. Details of the measurement methods and conditions for each particle size distribution will be described later in the examples.

[0025] The particle size distribution based on weight by the sieving method is determined in accordance with the dry sieving test method described in JIS K0069 by sieving the cellulose acetate powder using sieves specified in JIS Z8801 (mesh openings of 4000 μm, 1700 μm, 1000 μm, 840 μm, 500 μm, 300 μm, 150 μm, and 50 μm).

[0026] In the weight-based particle size distribution measured by dry sieving, the cellulose acetate powder of the present disclosure has a proportion of particles having a particle diameter of 1000 μm or more of 40% by weight or less. From the viewpoint of improving moldability, this proportion may be 30% by weight or less, 20% by weight or less, 10% by weight or less, 5% by weight or less, or 1% by weight or less, and the lower limit may be 0.

[0027] In the particle size distribution based on weight by dry sieving, the proportion of particles having a particle diameter of 500 μm or more and less than 1000 μm may be 30% by weight or less, 20% by weight or less, 10% by weight or less, or 5% by weight or less. The proportion of particles having a particle diameter of 500 μm or more and less than 1000 μm may be 0, but may be 0.1% by weight or more.

[0028] In the weight-based particle size distribution determined by dry sieving, the proportion of particles having a particle diameter of 300 μm or more and less than 500 μm may be 10% by weight or less, or 5% by weight or less, or may be 0.1% by weight or more, or may be 0.5% by weight or more.

[0029] In the weight-based particle size distribution determined by a dry sieving method, the proportion of particles having a particle diameter of 150 μm or more and less than 300 μm may be 20% by weight or more, 25% by weight or more, or 30% by weight or more, and may be 55% by weight or less, or 50% by weight or less.

[0030] In the weight-based particle size distribution determined by a dry sieving method, the proportion of particles having a particle diameter of 50 μm or more and less than 150 μm may be 10% by weight or more, 15% by weight or more, 20% by weight or more, or 25% by weight or more, and may be 40% by weight or less, or 35% by weight or less.

[0031] In the weight-based particle size distribution determined by dry sieving, the proportion of particles with a diameter of less than 50 μm may be 25% by weight or less, or 20% by weight or less, or may be 1% by weight or more, or 5% by weight or more.

[0032] The cellulose acetate powder of the present disclosure may have a cumulative 10% particle diameter D10 in the weight-based particle size distribution measured by dry sieving of 100 μm or less, 90 μm or less, 80 μm or less, or 70 μm or less, or may be 10 μm or more, or 15 μm or more.

[0033] The cumulative 50% particle diameter D50 in the weight-based particle size distribution measured by a dry sieving method may be 200 μm or less, 180 μm or less, or 160 μm or less, or may be 80 μm or more, 90 μm or more, or 100 μm or more.

[0034] The cumulative 90% particle diameter D50 in the weight-based particle size distribution measured by a dry sieving method may be 800 μm or less, 700 μm or less, or 600 μm or less, or may be 100 μm or more, or may be 200 μm or more.

[0035] The volumetric particle size distribution determined by the laser diffraction / scattering method was determined by suspending the cellulose acetate powder in pure water and measuring the particle size distribution using a commercially available laser diffraction / scattering particle size distribution analyzer.

[0036] The cellulose acetate powder of the present disclosure may have a cumulative 10% particle diameter D10 in a volume-based particle size distribution measured by a laser diffraction / scattering method of 200 μm or less, 150 μm or less, 100 μm or less, 90 μm or less, 80 μm or less, or 70 μm or less, or may be 10 μm or more, or 20 μm or more.

[0037] The cumulative 50% particle diameter D50 in the volume-based particle size distribution measured by a laser diffraction / scattering method may be 500 μm or less, 400 μm or less, or 300 μm or less, or may be 50 μm or more, or may be 100 μm or more.

[0038] The cumulative 90% particle diameter D90 in the volume-based particle size distribution measured by a laser diffraction / scattering method may be 1000 μm or less, 900 μm or less, or 800 μm or less, or may be 300 μm or more, or may be 400 μm or more.

[0039] (Cellulose acetate) (Degree of acetyl substitution) In the present disclosure, the cellulose acetate has a degree of substitution with an acetyl group of 2.0 or more and 2.6 or less. From the viewpoint of melt moldability and facilitating the production of high-quality molded products, the degree of acetyl substitution may be 2.1 or more, 2.2 or more, or 2.5 or less. Multiple cellulose acetates with different degrees of acetyl substitution may be used in combination.

[0040] The degree of acetyl substitution of cellulose acetate can be measured by NMR as the sum of the degrees of substitution at the 2-, 3-, and 6-positions of the glucose ring of cellulose acetate according to the method of Tezuka (Tezuka, Carbonydr. Res. 273, 83 (1995)). That is, the free hydroxyl groups of cellulose acetate are acylated with a carboxylic acid anhydride in pyridine. The type of carboxylic acid anhydride used here can be selected depending on the purpose of analysis. For example, cellulose acetate is butylated with butyric anhydride, and the resulting sample is dissolved in deuterated chloroform. 13 The total degree of substitution of cellulose ester treated with carboxylic anhydride by Tezuka's method or a method based thereon is 3.0, so the sum of the areas of the carbonyl carbon signals of the acyl groups (acetyl groups) originally present in cellulose acetate and the carbonyl signals of the acyl groups (butyryl groups) introduced by butyric anhydride treatment is normalized to 3.0, and the abundance ratios of the acyl groups at the corresponding positions (in other words, the area ratios of the signals) are calculated, which can be used as the degrees of acyl substitution at the 2-, 3-, and 6-positions of the glucose ring in cellulose acetate. 13 Instead of C-NMR 1 The degree of acetyl substitution may be determined using H-NMR.

[0041] (Amount of sulfuric acid component) In the present disclosure, the cellulose acetate has a sulfuric acid component amount of 50 ppm or less. Cellulose acetate having a sulfuric acid component amount of 50 ppm or less has excellent stability during thermoforming. Molded products obtained using powder containing this cellulose acetate have reduced yellowness and acetic acid odor due to thermal decomposition. From the viewpoint of improving thermal stability, the smaller the amount of sulfuric acid component in cellulose acetate, the more preferable. For example, it may be 45 ppm or less, 40 ppm or less, or 35 ppm or less. However, when a sulfuric acid catalyst is used during the production of cellulose acetate, the lower limit is about 30 ppm.

[0042] In this specification, the amount of sulfuric acid component refers to the amount of sulfuric acid in 1 g of dried cellulose acetate, and the total sulfur content measured by combustion absorption-ion chromatography (IC) is expressed as the sulfuric acid (H 2 SO 4 The details of the measurement method and conditions will be described later in the Examples.

[0043] (Calcium Content) From the viewpoint of improving thermal stability, the calcium content of cellulose acetate may be less than 1.0 ppm, less than 0.8 ppm, or less than 0.6 ppm. Preferably, the cellulose acetate is produced by a method and under conditions in which no calcium source is intentionally added.

[0044] (Magnesium Content) The magnesium content of cellulose acetate may be 50 ppm or less, 40 ppm or less, or 1 ppm or more, or 5 ppm or more. Cellulose acetate with a magnesium content within this range has excellent thermal stability and improves the quality of the resulting molded product. The magnesium content can be adjusted by the amount of neutralizing agent added in the production process of cellulose acetate, purification conditions, etc.

[0045] The calcium and magnesium contents of cellulose acetate are measured by absorptiometry, the details of which will be described later in the Examples.

[0046] (6% Viscosity) From the viewpoint of obtaining appropriate fluidity during melt molding, the 6% viscosity of cellulose acetate may be 50 mPa·s or more, preferably 55 mPa·s or more, more preferably 65 mPa·s or more, even more preferably 70 mPa·s or more, and particularly preferably 80 mPa·s or more. Furthermore, from the viewpoint of improving the hue and mechanical properties of the obtained molded product, the 6% viscosity of cellulose acetate may be 120 mPa·s or less, preferably 110 mPa·s or less, and more preferably 100 mPa·s or less. The 6% viscosity of cellulose acetate is determined by the flow-down method using an Ostwald viscometer. Details of the measurement method and measurement conditions will be described later in the examples.

[0047] (Molecular weight and molecular weight distribution) When applied to melt molding, the weight-average molecular weight Mw of cellulose acetate is preferably 100,000 or more, more preferably 120,000 or more, from the viewpoint of obtaining molded products with excellent strength. From the viewpoint of obtaining appropriate fluidity when melted, the weight-average molecular weight Mw of cellulose acetate is preferably 1,500,000 or less, more preferably 1,200,000 or less. When biodegradability is important, the weight-average molecular weight Mw of cellulose acetate is preferably 1,000,000 or less, more preferably 800,000 or less, and even more preferably 500,000 or less, from the viewpoint of obtaining high biodegradability.

[0048] The molecular weight distribution of cellulose acetate is evaluated by the ratio of the number average molecular weight Mn to the weight average molecular weight Mw (Mw / Mn) of the cellulose acetate. From the viewpoints of processability and biodegradability, the molecular weight distribution Mw / Mn of the cellulose derivative may be 1.5 or more, 1.8 or more, or 2.0 or more, and may be 5.0 or less, 4.0 or less, or 3.0 or less.

[0049] Cellulose acetate is a semi-synthetic polymer typically obtained from cellulose. Therefore, the molecular weight and molecular weight distribution of cellulose acetate generally depend on the cellulose raw material. The molecular weight and molecular weight distribution of cellulose acetate may be adjusted by using different types of cellulose raw materials in combination.

[0050] The molecular weight and molecular weight distribution of cellulose acetate can be determined by a known method. Specifically, the molecular weight and molecular weight distribution of cellulose acetate are determined by size exclusion chromatography (GPC) measurement using the following apparatus and conditions (GPC-light scattering method). Apparatus: GPC "SYSTEM-21H" manufactured by Shodex Solvent: Acetone Column: Two GMHxl columns (Tosoh), guard column (TSKgel guard column HXL-H manufactured by Tosoh) Flow rate: 0.8 ml / min Temperature: 29°C Sample concentration: 0.25% (wt / vol) Injection volume: 100 μl Detection: MALLS (multi-angle light scattering detector) ("DAWN-EOS" manufactured by Wyatt) MALLS calibration standard: PMMA (molecular weight 27,600)

[0051] (Plasticizer) The cellulose acetate powder of the present disclosure may further contain a plasticizer. The cellulose acetate powder containing the plasticizer may be obtained by melt-kneading the cellulose acetate and the plasticizer described above.

[0052] When the cellulose acetate powder contains a plasticizer, the content thereof may be 30.0% by weight or less, 25.0% by weight or less, or 20.0% by weight or less, or 10.0% by weight or more, or 12.0% by weight or more.

[0053] The plasticizer may be any one that has the effect of improving the melt fluidity of cellulose acetate having an acetyl substitution degree of 2.0 to 2.6. In particular, when applied to molded products that come into direct contact with food, such as cutlery, tableware, and cooking utensils, from the viewpoint of safety, preferred plasticizers are selected from adipate ester compounds and citrate ester compounds. Adipate ester compounds and citrate ester compounds may be used in combination. The cellulose acetate pellets may contain plasticizers other than adipate ester compounds and citrate ester compounds, as long as the effects of the present disclosure are not impaired. When two or more plasticizers are used, it is preferable to adjust the total content to the above-mentioned content.

[0054] Specific examples of the adipate ester compound include dimethyl adipate, dibutyl adipate, diisostearyl adipate, diisodecyl adipate, diisononyl adipate, diisobutyl adipate, diisopropyl adipate, diethylhexyl adipate, dioctyl adipate, dioctyldodecyl adipate, dicapryl adipate, dihexyldecyl adipate, etc. Two or more types of adipate ester compounds may be used in combination.

[0055] Specific examples of the citrate ester compound include acetyl triethyl citrate, acetyl tributyl citrate, isodecyl citrate, isopropyl citrate, triethyl citrate, triethylhexyl citrate, tributyl citrate, etc. Two or more citrate ester compounds may be used in combination.

[0056] (Optional Components) Within the range in which the effects of the present disclosure can be obtained, the cellulose acetate powder may further contain, as optional components, known additives such as fragrances, colorants, light resistance stabilizers, antioxidants, heat stabilizers, optical property adjusters, fluorescent brighteners, flame retardants, lubricants, hydrolysis inhibitors, water repellents, etc. When the optional components are contained, it is preferable to blend the optional components so that the content of cellulose acetate in the cellulose acetate powder is at least 70 wt %.

[0057] Among the optional components, examples of flavorings include vanillin, ethyl vanillin, limonene, eugenol, ethyl acetate, benzyl alcohol, methyl salicylate, α-terpineol, etc. From the viewpoint of easily maintaining the scent after heat molding, vanillin, ethyl vanillin, eugenol, and methyl salicylate are preferred, and from the viewpoint of safety, vanillin and ethyl vanillin are more preferred.

[0058] (Method for producing cellulose acetate powder) The cellulose acetate powder of the present disclosure can be produced by the above-mentioned reduced pressure acetylation method. The reduced pressure acetylation method uses a formulation with a small amount of sulfuric acid catalyst and acid added, which enables cost reduction. Furthermore, by controlling the particle size distribution to a predetermined value, the cellulose acetate powder of the present disclosure can be obtained with excellent processability.

[0059] Specifically, the method for producing cellulose acetate powder includes a step (1) of obtaining cellulose acetate by a reduced pressure acetylation method, and a step (2) of adjusting the particle size distribution of the obtained cellulose acetate.

[0060] The process (1) for obtaining cellulose acetate by the reduced pressure acetylation method includes the steps of: (1-1) disintegrating wood pulp; (1-2) pretreating the disintegrated wood pulp by contacting it with acetic acid; (1-3) acetylating the pretreated wood pulp by reacting it with acetic anhydride under reduced pressure; (1-4) hydrolyzing the cellulose acetate obtained by acetylation; (1-5) precipitating the cellulose acetate whose degree of acetyl substitution has been adjusted by hydrolysis; and (1-6) drying the precipitated cellulose acetate.

[0061] (Wood Pulp) Examples of wood pulp include softwood pulp and hardwood pulp. Softwood pulp includes softwood pulp obtained from spruce, pine, boxwood, etc. Hardwood pulp includes eucalyptus, acacia, etc. These pulps may be used alone or in combination of two or more, and softwood pulp and hardwood pulp may be used in combination.

[0062] The α-cellulose content of the wood pulp is preferably 85% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and most preferably 100% by weight.

[0063] The α-cellulose content is calculated based on the weight of α-cellulose (insoluble portion) obtained by sequentially extracting a pulp of known weight with a 17.5% aqueous sodium hydroxide solution and then a 9.45% aqueous sodium hydroxide solution at a temperature of 25°C, oxidizing the soluble portion of the extract with potassium dichromate, determining the weight of β,γ-cellulose from the volume of potassium dichromate required for the oxidation, and subtracting the weight of β,γ-cellulose from the initial pulp weight (TAPPI T203). That is, the ratio of the weight of the insoluble portion of the pulp to the initial pulp weight is the α-cellulose content (wt %).

[0064] (Crushing) The method for crushing wood pulp may be a wet crushing method or a dry crushing method. Examples of wet crushing methods include a method in which the pulp is activated with steam and then sheared and stirred in a reactor, and a method in which the pulp is disintegrated in a dilute aqueous acetic acid solution to form a slurry, followed by repeated deliquoring and acetic acid replacement (slurry pretreatment). Examples of dry crushing methods include a method in which pulp roughly crushed in a disc refiner with pyramidal teeth is finely crushed in a disc refiner with linear teeth, and a method in which the pulp is crushed in a turbo mill equipped with a cylindrical outer box with a liner attached to the inner wall, multiple discs rotating at high speed around the center line of the outer box, and multiple blades attached between each disc in a radial direction relative to the center line. The dry crushing method is preferred, and a two-stage crushing method using a disc refiner and then a turbo mill is more preferred.

[0065] (Pretreatment) In the step of contacting disintegrated wood pulp with acetic acid to perform pretreatment (hereinafter, sometimes referred to as the "pretreatment step" or "pretreatment activation step"), the method of contacting wood pulp with acetic acid may be a method of adding acetic acid or acetic acid containing 1 to 10% by weight of sulfuric acid (sulfur-containing acetic acid) in one step, or a method of adding the acetic acid in two or more separate steps. For example, examples of the two-step addition method include a method of adding acetic acid and then adding sulfur-containing acetic acid after a certain time has elapsed, and a method of adding sulfur-containing acetic acid after a certain time has elapsed. Acetic acid may be added by spraying it onto the disintegrated wood pulp and stirring. The amount of acetic acid added is preferably 10 parts by weight or more and 500 parts by weight or less per 100 parts by weight of wood pulp. Acetic acid with a purity of 99% by weight can be used.

[0066] In this pretreatment step, after adding acetic acid and / or sulfur-containing acetic acid to the pulp, the mixture may be left to stand for 0.2 to 48 hours at a temperature of 17 to 40°C, or may be sealed and stirred for 0.1 to 24 hours at a temperature of 17 to 40°C. An inert gas may be introduced into the reaction system to control the oxygen concentration to 3% or less. Examples of inert gases that can be used include nitrogen gas, helium gas, argon gas, and neon gas. The oxygen concentration can be measured using a known oxygen concentration meter.

[0067] (Acetylation) In the step of acetylating pretreated wood pulp by reacting it with acetic anhydride (hereinafter sometimes referred to as the "acetylation step"), the acetylation reaction can be initiated by adding the pretreated wood pulp to a mixture of acetic acid, acetic anhydride, and sulfuric acid, or by adding a mixture of acetic acid and acetic anhydride and sulfuric acid to the pretreated wood pulp. Acetic acid with a purity of 99% by weight or more can be used. Sulfuric acid with a purity of 98% by weight or more is preferred. The mixture of acetic acid, acetic anhydride, and sulfuric acid is preferably temperature-adjusted in advance.

[0068] In the mixture of acetic acid, acetic anhydride, and sulfuric acid, the ratio of acetic acid to acetic anhydride is preferably 200 parts by weight or more and 400 parts by weight or less of acetic anhydride relative to 300 parts by weight or more and 600 parts by weight or less of acetic acid, and more preferably 240 parts by weight or more and 280 parts by weight or less of acetic anhydride relative to 350 parts by weight or more and 530 parts by weight or less of acetic acid.

[0069] In the acetylation step, the total amount of acetic acid and acetic anhydride is preferably 500 to 1,000 parts by weight per 100 parts by weight of wood pulp, and the amount of sulfuric acid is preferably 5 to 15 parts by weight, more preferably 7 to 13 parts by weight, and even more preferably 8 to 11 parts by weight, per 100 parts by weight of wood pulp.

[0070] The acetylation step in the present disclosure may be a so-called reduced-pressure acetylation method carried out under reduced pressure. Specifically, in the acetylation step, the degree of vacuum in the reaction system is preferably 70 Torr (9.3 kPa) or less at least at the start of the acetylation reaction. The lower limit of the degree of vacuum is not particularly limited, but is, for example, 60 Torr (8.0 kPa). This allows acetic acid in the reaction solution to evaporate, increasing the concentration of acetic anhydride consumed in the acetylation reaction and accelerating the acetylation reaction. Furthermore, the usage rate of solvents such as acetic anhydride and acetic acid is reduced, improving the productivity of cellulose acetate. Furthermore, the reduced-pressure acetylation method has the advantage of eliminating the need for cooling to suppress temperature increases associated with the acetylation reaction. Furthermore, increasing the degree of vacuum in the acetylation reaction system and reducing the pressure can reduce the oxygen concentration in the acetylation reaction system.

[0071] It is preferable to maintain the degree of vacuum in the reaction system at 70 Torr (9.3 kPa) or less from the start of the acetylation reaction until the cellulose acetate changes from a heterogeneous state to a homogeneous state, thereby suppressing the temperature rise that accompanies the acetylation reaction.

[0072] When the degree of vacuum in the acetylation reaction system is set to 70 Torr (9.3 kPa) or less, the maximum temperature reached in the acetylation reaction system is preferably 55° C. or more and 75° C. or less, and more preferably 60° C. or more and 70° C. or less. The time required for the acetylation reaction is preferably 40 minutes or more and 60 minutes or less. Here, the time required for acetylation refers to the time from the time when the wood pulp comes into contact with the solvent, acetic anhydride, and catalyst to start the reaction until the time when the neutralizing agent described below is added.

[0073] (Hydrolysis) In the cellulose acetate obtained by acetylation, almost all of the hydroxyl groups have been replaced with acetyl groups. Furthermore, the sulfuric acid used as a catalyst in the acetylation process is bound to a portion of the cellulose as sulfate esters. In the process of hydrolyzing the acetylated cellulose acetate (hereinafter referred to as the "hydrolysis process"), the cellulose acetate is hydrolyzed to adjust the degree of substitution to a desired level, and the sulfate esters are hydrolyzed and removed. Removal of the sulfate esters improves the thermal stability of the resulting cellulose acetate.

[0074] The hydrolysis step can be carried out by adding a neutralizing agent to a reaction mixture containing acetylated cellulose acetate. Examples of the neutralizing agent include water (including steam), dilute acetic acid, or carbonates, acetates, hydroxides, or oxides of magnesium, iron, aluminum, zinc, or the like. Magnesium acetate or an aqueous magnesium acetate solution is preferably used. An aqueous magnesium acetate solution having a concentration of 5% by weight or more and 30% by weight or less is preferred.

[0075] Furthermore, if the sulfate ion concentration in the reaction mixture containing cellulose acetate is high, sulfate esters cannot be removed efficiently. Therefore, it is preferable to lower the sulfate ion concentration by adding an aqueous solution of magnesium acetate or the like or an acetic acid-water mixed solution to form an insoluble sulfate salt. It is preferable to adjust the sulfate ion concentration in the reaction mixture containing cellulose acetate to 1 part by weight or more and 6 parts by weight or less per 100 parts by weight of cellulose acetate (in cellulose equivalent).

[0076] In the hydrolysis step, the oxygen concentration in the hydrolysis reaction system may be adjusted to 3% or less, more preferably 1% or less. When hydrolysis is carried out at high temperatures using steam (high-temperature aging), it is preferable to adjust the oxygen concentration in the hydrolysis reaction system to 3% at least before blowing in steam. By introducing an inert gas into the hydrolysis reaction system, the oxygen concentration can be adjusted to 3% or less, more preferably 1% or less.

[0077] (Precipitation) In the step of precipitating cellulose acetate (hereinafter referred to as the "precipitation step"), a reaction mixture containing cellulose acetate adjusted to a desired degree of acetyl substitution is mixed with a precipitant such as water or dilute acetic acid to precipitate the cellulose acetate as a solid. The precipitate may be separated and washed with water to remove free metal components, sulfuric acid components, etc. Dilute acetic acid is preferred as the precipitant used to obtain the cellulose acetate precipitate.

[0078] In particular, after the hydrolysis step (complete neutralization), in order to enhance the thermal stability of cellulose acetate, it is preferred to add an alkali metal compound and / or an alkaline earth metal compound as a stabilizer to the water used for washing with water, and magnesium acetate is preferred as this stabilizer.

[0079] (Drying) In the step of drying the precipitated cellulose acetate (hereinafter referred to as the "drying step"), the method for drying the cellulose acetate is not particularly limited, and known methods such as air drying, drying under reduced pressure, hot air drying, etc. The drying conditions can be appropriately selected based on the moisture content of the cellulose acetate separated in the precipitation step.

[0080] (Particle Size Adjustment) Step (2) of adjusting the particle size distribution of the cellulose acetate obtained by the reduced pressure acetylation method is a step of adjusting the particle size distribution of the cellulose acetate obtained by the drying step described above so that the proportion of particles with a particle diameter of 1000 μm or more is 40% by weight or less. For example, the particle size distribution may be adjusted by pulverizing the dried cellulose acetate, by classifying the dried cellulose acetate, or by pulverizing the dried cellulose acetate and then classifying it. The pulverization method, pulverization conditions, and classification method can be selected using the particle size distribution based on weight as determined by the dry sieving test method described above as an index. This step yields the cellulose acetate powder of the present disclosure.

[0081] The method for producing cellulose acetate powder according to the present disclosure may further include a step (3) of mixing the cellulose acetate having an adjusted particle size distribution with a plasticizer. The plasticizers described above can be appropriately selected and used. The optional components described above may be further mixed with the plasticizer. This step provides a cellulose acetate powder containing the plasticizer and, if desired, the optional components.

[0082] (Molded Article) The molded article of the present disclosure is formed from the cellulose acetate powder described above. The molded article of the present disclosure may be formed from cellulose acetate powder containing a plasticizer. The shape of the molded article may be a film, plate, rod, cylinder, polygonal pillar, or the like, and can be appropriately selected depending on the application or purpose. Pellets made of cellulose acetate powder produced by melt kneading using an extruder may be used as the molded article of the present disclosure. The size of the pellets is appropriately selected depending on the application, but for use in cutlery, cylindrical pellets with a diameter of 2 to 3 mm and a length of 3 to 3.5 mm are preferred. The molded article and pellets may contain the plasticizer in the amount described above.

[0083] The molded article can be produced by a conventional molding method, such as injection molding, injection compression molding, injection press molding, extrusion compression molding, extrusion molding, rotational molding, press molding, compression molding, inflation molding, etc. For example, the molded article of the present disclosure can be obtained by melting and injection molding the cellulose acetate powder or pellets made of the cellulose acetate powder.

[0084] (Applications) The cellulose acetate powder of the present disclosure can be used, for example, as a material for tableware, packaging containers, trays, agricultural materials, fishing materials, office automation parts, construction materials, medical parts, home appliance parts, automotive components, daily necessities, stationery, eyeglass frames, etc. In particular, the cellulose acetate powder of the present disclosure can be thermoformed with a small amount of plasticizer, so the plasticizer content in the molded product is low. Therefore, the amount of plasticizer leaching during use meets the leaching standards of the Food Sanitation Act, making it suitable for applications that come into direct contact with food, such as cutlery, tableware, and cooking utensils.

[0085] The effects of the present disclosure will be clarified below by examples, but the present disclosure should not be interpreted as being limited based on the description of these examples.

[0086] [Test 1] [Comparative Example 1] Sulfite-process dissolving pulp (a mixture of softwood and hardwood, containing 96.5% α-cellulose) was used as the cellulose raw material and disintegrated using a disintegrator. 35 parts by weight of acetic acid was added to 100 parts by weight of the disintegrated pulp (5% moisture content), and the mixture was pretreated and activated at 40°C for 30 minutes. A mixture of 247 parts by weight of acetic anhydride and 438 parts by weight of acetic acid, previously heated to 40°C, was added to an acetylation reactor and stirred and mixed with the entire amount of pretreated activated pulp. The vacuum pump connected to the acetylation reactor was then operated to reduce the pressure inside the reaction system to an absolute pressure of 428 kPa. A mixture of 3.8 parts by weight of sulfuric acid and 100 parts by weight of acetic acid (sulfur-containing acetic acid), adjusted to 40°C, was then added to the reactor to initiate the acetylation reaction. The mixture was then stirred and mixed under reduced pressure for approximately 20 minutes to carry out the acetylation reaction, after which the vacuum pump was stopped and the reaction system was returned to normal pressure. After the addition of the sulfur-containing acetic acid, the temperature of the reaction solution in the system rose to about 54° C., and after 20 minutes the temperature of the reaction solution was about 51° C. By stirring and mixing for an additional 12 minutes under normal pressure, the temperature of the reaction solution reached about 53° C. One minute later, 16 parts by weight of an aqueous magnesium acetate solution with a concentration of 38% by weight was added and mixed to the reaction solution, completely neutralizing the sulfuric acid in the system and obtaining a reaction mixture containing an excess of magnesium acetate.

[0087] The reaction mixture in the acetylation reactor was then transferred to an aging tank, where it was heated to 150°C over 90 minutes, held at 150°C for 30 minutes, and then cooled to 110°C over 20 minutes to obtain a reaction mixture containing cellulose acetate. The resulting reaction mixture was mixed with a dilute aqueous acetic acid solution under vigorous stirring to precipitate cellulose acetate. The precipitate was separated, washed with water, dehydrated, and dried to obtain the cellulose acetate powder of Comparative Example 1.

[0088] Example 1 The cellulose acetate powder of Comparative Example 1 was pulverized using a Makino pulverizer (manufactured by Makino Sangyo Co., Ltd., model number DD-2-3.7) (rotation conditions: 2450 rpm, screen diameter φ0.5 mm) to obtain the cellulose acetate powder of Example 1.

[0089] Comparative Example 2: Sulfite-process dissolving pulp (softwood, α-cellulose content 93.0%) was used as the cellulose raw material and disintegrated using a disintegrator. 29 parts by weight of acetic acid was added to 100 parts by weight of the disintegrated pulp (moisture content 5%), and the mixture was pretreated and activated at 35°C for 60 minutes. 503 parts by weight of a 45% by weight acetic anhydride-acetic acid solution, 13 parts by weight of 98% by weight sulfuric acid, and 29 parts by weight of 99% by weight acetic acid were mixed and cooled to -17°C. This cooled mixture and the entire amount of pretreated activated pulp were charged into an acetylation reactor and stirred. An additional 18 parts by weight of the 45% by weight acetic anhydride-acetic acid solution was then added to the acetylation reactor to initiate the acetylation reaction. The temperature was then adjusted to approximately 48°C in approximately 45 minutes due to the heat of the acetylation reaction, and the reaction was carried out for approximately 30 minutes. After the reaction was completed, 45 parts by weight of a 24% by weight aqueous magnesium acetate solution was added to the reaction mixture and mixed to partially neutralize the sulfuric acid in the system and hydrolyze the acetic anhydride.

[0090] The reaction mixture in the acetylation reactor was then transferred to an aging tank, where an aging reaction (hydrolysis reaction) was carried out at 85°C for 110 minutes. During the reaction, 10 parts by weight of a 24% by weight aqueous magnesium acetate solution was added to partially neutralize the sulfuric acid in the system. Furthermore, 17 parts by weight of water was added to adjust the concentration. After the aging reaction was completed, 16 parts by weight of a 24% by weight aqueous magnesium acetate solution was added and mixed to completely neutralize the sulfuric acid in the system, and 58 parts by weight of water was added to adjust the concentration. The resulting reaction mixture was mixed with a dilute aqueous acetic acid solution under vigorous stirring to precipitate cellulose acetate. The precipitate was washed with water, immersed in a dilute aqueous calcium hydroxide solution (20 ppm), filtered, and dried.

[0091] The obtained dried product was pulverized (rotation conditions: 2450 rpm, screen diameter φ0.5 mm) using a Makino type pulverizer (manufactured by Makino Sangyo Co., Ltd., model number DD-2-3.7) to obtain cellulose acetate powder of Comparative Example 2.

[0092] Comparative Example 3: Prehydrolyzed kraft pulp (hardwood, α-cellulose content 98.4%) was used as a cellulose raw material and crushed into a flocculent state using a disc refiner. 26.8 parts by weight of acetic acid was added to 100 parts by weight of the crushed pulp (moisture content 8%), and the mixture was stirred and then allowed to stand for 60 hours to perform pretreatment activation. This activated pulp was added to a mixture (5°C) consisting of 323 parts by weight of acetic acid, 245 parts by weight of acetic anhydride, and 13.1 parts by weight of sulfuric acid to form a reaction solution. The temperature of the reaction solution was then adjusted from 5°C to 40°C over 40 minutes, and the acetylation reaction was carried out for 90 minutes from the time the pulp was added to the mixture.

[0093] Thereafter, a 24 wt% magnesium acetate aqueous solution was added over 3 minutes to adjust the amount of sulfuric acid in the reaction solution to 2.5 parts by weight. Furthermore, the reaction solution was heated to 75°C, and water was added to adjust the water concentration in the reaction solution to 5 mol%. This water concentration was calculated by multiplying the molar ratio of water to acetic acid in the reaction solution by 100, and expressed in mol%. Then, an aging reaction was carried out at 85°C for 100 minutes, and the sulfuric acid was neutralized with magnesium acetate to obtain a reaction mixture containing cellulose acetate.

[0094] 400 parts by weight of the resulting reaction mixture and 1,200 parts by weight of 10% diluted acetic acid were added to a commercial mixer (manufactured by Panasonic, model number MX-152SP-W) and stirred for 4 seconds to precipitate cellulose acetate. The precipitate was washed with water, immersed in a diluted aqueous calcium hydroxide solution (20 ppm), filtered, and dried.

[0095] The obtained dried product was pulverized (rotation conditions: 2450 rpm, screen diameter φ0.5 mm) using a Makino type pulverizer (manufactured by Makino Sangyo Co., Ltd., model number DD-2-3.7) to obtain cellulose acetate powder of Comparative Example 3.

[0096] Comparative Example 4 In Comparative Example 4, commercially available cellulose acetate (manufactured by Eastman Chemical Co.) was used.

[0097] Comparative Example 5 As Comparative Example 5, commercially available cellulose acetate (manufactured by Push Corporation) was used.

[0098] (Physical Property Evaluation) The acetyl substitution degree, 6% viscosity, calcium content, magnesium content, sulfuric acid content, and particle size distribution (sieving test method and laser diffraction / scattering method) of the examples and comparative examples were measured by the following methods. Hereinafter, the term "sample" is appropriately referred to as cellulose acetate powder. The obtained results are shown in Table 1 below. In Table 1, "Ca" represents the calcium content (ppm), "Mg" represents the magnesium content (ppm), "Total S" represents the total sulfur content (ppm), "D50(1)" represents the 50% cumulative particle size (μm) in the weight-based particle size distribution, and "D10(2)", "D50(2)", and "D90(2)" represent the 10% cumulative particle size (μm), the 50% cumulative particle size (μm), and the 90% cumulative particle size (μm) in the volume-based particle size distribution, respectively. Furthermore, "1000 μm or more" refers to the proportion (wt%) of particles in a sample that have a particle diameter of 1000 μm or more, "500-1000 μm" refers to the proportion (wt%) of particles in a sample that have a particle diameter of 500 μm or more but less than 1000 μm, "300-500 μm" refers to the proportion (wt%) of particles in a sample that have a particle diameter of 300 μm or more but less than 500 μm, "150-300 μm" refers to the proportion (wt%) of particles in a sample that have a particle diameter of 150 μm or more but less than 300 μm, "50-150 μm" refers to the proportion (wt%) of particles in a sample that have a particle diameter of 50 μm or more but less than 150 μm, and "50 μm or less" refers to the proportion (wt%) of particles in a sample that have a particle diameter of less than 50 μm.

[0099] (Degree of Acetyl Substitution) The degree of acetyl substitution was measured according to the method of Tezuka (Tezuka, Carbonydr. Res. 273, 83 (1995)), by propionylating the free hydroxyl groups in cellulose acetate with propionic anhydride in pyridine, dissolving the obtained sample in deuterated chloroform, and 13 The C-NMR spectrum was measured, and the degree of acetyl substitution at the 2-, 3-, and 6-positions was determined from the area ratio of the carbon signals of the acetyl group appearing in the order of 2-, 3-, and 6-positions from the high magnetic field in the region from 169 ppm to 171 ppm, and the sum of the degrees of substitution was calculated as the degree of acetyl substitution.

[0100] (6% Viscosity) 3.00 g of dried cellulose acetate powder and 39.90 g of 95% acetone aqueous solution were placed in an Erlenmeyer flask, sealed, and stirred for approximately 1.5 hours. The flask was then shaken for approximately 1 hour on a rotary shaker to completely dissolve the solution. The resulting 6 wt / vol% solution was transferred to the marked line of an Ostwald viscometer and allowed to warm to 25±1°C for approximately 15 minutes. The flow time between the time marks was measured, and the 6% viscosity was calculated using the following formula (1): 6% viscosity (mPa s) = flow time (s) × viscometer coefficient (1)

[0101] The viscometer coefficient was determined by measuring the flow time in the same manner as above using a standard solution for viscometer calibration (manufactured by Showa Sekiyu K.K., trade name "JS-200" (compliant with JIS Z 8809)) and using the following formula (2): Viscometer coefficient = {absolute viscosity of standard solution (mPa s) × density of solution (0.827 g / cm)} 3 )} / {density of standard solution (g / cm 3 ) × number of seconds the standard solution flows (s)) ... (2)

[0102] (Calcium and Magnesium Contents) 3.0 g of undried sample was weighed into a crucible, carbonized on an electric heater, and then incinerated for approximately 2 hours in an electric furnace at 750°C to 850°C. After cooling for approximately 30 minutes, 25 mL of 0.07% hydrochloric acid solution was added and dissolved by heating at 220°C to 230°C. After cooling, the solution was diluted to 200 mL with distilled water. This was used as a test solution, and the absorbance was measured using an atomic absorption spectrophotometer along with a standard solution to determine the calcium (Ca) and magnesium (Mg) concentrations of the test solution, which were then converted into the calcium (Ca) and magnesium (Mg) contents of the sample. The moisture content of the undried sample was measured using a Kett moisture meter (METTLER TOLEDO HB43). Approximately 2.0 g of the wet sample was placed on the aluminum tray of the Kett moisture meter and heated at 120°C until the weight no longer changed. The moisture content (wt%) in the sample was calculated from the change in weight before and after heating.

[0103] (Amount of sulfuric acid component) The amount of sulfuric acid component in the sample was measured by combustion absorption-ion chromatography (IC). Specifically, about 30 mg of a dried sample was combusted at a combustion temperature of 1000°C using a combustion apparatus (trade name "AQF-2100H" manufactured by Mitsubishi Chemical Analytech Co., Ltd.), and the generated gas component was dissolved in 10 ml of an absorption liquid (H 2 O 2 The resulting absorbed solution was subjected to ion chromatography under the following measurement conditions: Apparatus: Thermo Fisher Scientific ion chromatograph, product name "Integrion" Main column: AS-12, Pre-column: AG-12 Eluent: 3 mM K 2 CO 3 Suppressor: "ADRS" (recycle mode) manufactured by Thermo Fisher Scientific Flow rate: 1.2 ml / min Detector: electrical conductivity detector Column temperature: 35°C Injection volume: 100 μl

[0104] The total sulfur content was determined from the measurement results of ion chromatography, and this total sulfur content was calculated using sulfuric acid (H 2 SO 4 The amount of sulfuric acid component (ppm) in 1 g of bone-dry cellulose acetate powder was calculated by converting the amount of sulfuric acid component (ppm) in 1 g of bone-dry cellulose acetate powder.

[0105] (Particle Size Distribution 1: Sieving Test Method) In accordance with the dry sieving test method described in JIS K0069, cellulose acetate powder was sieved using sieves specified in JIS Z8801 to determine weight-based particle size distribution 1. Specifically, 100 g of a sample was shaken for 5 minutes using sieves with openings of 4000 μm, 1700 μm, 1000 μm, 840 μm, 500 μm, 300 μm, 150 μm, and 50 μm in a Rotap type sieve shaker (manufactured by Iida Seisakusho, tapping: 156 times / min, rolling: 290 times / min), and the weight of the sample remaining on each sieve was measured, and the ratio (cumulative weight percentage) of each sample to the total sample tested was calculated to obtain particle size distribution 1. The particle size distribution 1 obtained in Example 1 and Comparative Examples 1 and 2 is shown in FIG.

[0106] (Particle size distribution 2: laser diffraction / scattering method) A volume-based particle size distribution 2 was determined by dynamic light scattering. Specifically, dried cellulose acetate powder was added to pure water in an amount to give a concentration of about 100 ppm, and a suspension was formed using an ultrasonic vibration device. This suspension was measured using a laser diffraction / scattering particle size distribution measuring device (manufactured by Horiba, Ltd., trade name "LA-960") under the following conditions: ultrasonic treatment: 15 minutes, refractive index: 1.500, medium: water (refractive index 1.333), to obtain particle size distribution 2. The particle size distributions 2 obtained in Example 1 and Comparative Examples 1, 2, 4, and 5 are shown in FIG. 2.

[0107]

[0108] [Test 2] [Example 2] 79.6 parts by weight of the cellulose acetate powder of Example 1 and 19.8 parts by weight of a citrate ester plasticizer (triethyl citrate manufactured by Morimura Shoji Co., Ltd.) were sequentially charged into an extruder (trade name "TEM58-SSG" manufactured by Toshiba Corporation) and extrusion-molded at a temperature of 240°C to obtain pellets (2.5 mm diameter) of Example 2. The extrusion rate (kg / hr) when the extrusion conditions were a cylinder temperature of 180 to 240°C and a screw rotation speed of 250 to 350 rpm is shown in Table 2 below.

[0109] Pellets (2.5 mm diameter) of Comparative Examples 6 to 10 were obtained in the same manner as in Example 2, except that the cellulose acetate powder of Comparative Examples 1 to 5 was used instead of the cellulose acetate powder of Example 1. The extrusion rates (kg / hr) under the extrusion conditions of a cylinder temperature of 180 to 240°C and a screw rotation speed of 250 to 350 rpm are shown in Table 2 below.

[0110] (Melt fluidity) Using an extrusion-type plastometer (trade name "Melt Flow Index Tester D4002" manufactured by Yasuda Seiki Seisakusho Co., Ltd.), the melt flow rates (g / 10 min) of the examples and comparative examples were measured at a temperature of 220°C and a load of 10.4 kg in accordance with the description of JIS K 7210. The measurement results are shown in Table 2 below.

[0111] (Tensile Test) The pellets of the Examples and Comparative Examples were each injection molded at a temperature of 220 to 250°C to prepare a sheet having a thickness of 3.0 mm. This sheet was punched out to prepare rectangular test pieces (No. 1 dumbbells). A tensile test was conducted in accordance with ASTM-D 638 at a pulling rate of 5 mm / min to measure the tensile elongation (%). The results are shown in Table 2 below.

[0112] (YI Value) The YI value (yellow index value) of the reflected light of the pellet was measured in accordance with ASTM E313-73. The instrument used was a spectrophotometer CM-5 manufactured by Konica Minolta, and the measurement conditions selected were a measurement diameter of 30 mm, a D65 light source, a 10° field of view, and SCE. A calibration glass for petri dish measurement, CM-A212, was fitted into the measurement section, and a zero calibration box, CM-A124, was placed on top of it to perform zero calibration, followed by white calibration using the built-in white calibration plate. Measurement was performed using the white calibration plate, CM-A210, and the L * is 99.16±0.05, a * is -0.07±0.02, b * It was confirmed that the YI was 0.02±0.01 and the YI was -0.02±0.01. The pellets were measured in a cylindrical glass container with an inner diameter of 30 mm and a height of 50 mm, and the pellets were packed to a depth of about 40 mm. The average values ​​of three measurements are shown in Table 2 below. The smaller the YI value, the less yellowish the product is and the better the hue.

[0113]

[0114] [Test 3] [Example 3] 79.6 parts by weight of the cellulose acetate powder of Example 1, 19.8 parts by weight of a citrate ester plasticizer (triethyl citrate manufactured by Morimura Shoji Co., Ltd.), and 0.1 parts by weight of vanillin (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a flavoring were sequentially charged into an extruder (trade name "TEM58-SSG" manufactured by Toshiba Corporation) and extrusion-molded at a temperature of 240°C to obtain pellets (2.5 mm diameter) of Example 3.

[0115] Pellets (2.5 mm diameter) of Comparative Example 11 were obtained in the same manner as in Example 3, except that the cellulose acetate powder of Comparative Example 1 was used. During extrusion molding of Comparative Example 1, a material loss of 10 to 20% by weight occurred due to strand breakage caused by unmelted particles.

[0116] (Sensory Test) Immediately after production, 50 g of the sample (pellets) was sealed in a container (size 115 mm x 90 mm, thickness 28 mm) and stored at room temperature for one week. The container was then opened, and five panelists conducted a sensory evaluation of the acetic acid odor and fragrance inside the container. The test was conducted at a room temperature of 20°C and a relative humidity of 60%. The sample was compared with a control product, Example 2 (which had the same composition as Example 3 except that it did not contain vanillin), and the results were ranked according to the following evaluation criteria. The results are shown in Table 3 below as the average of the five panelists. Evaluation Criteria (Acetic Acid Odor Reduction Effect) 1: The control product is significantly more effective. 2: The control product is slightly more effective. 3: The effects are equivalent. 4: The test product is slightly more effective. 5: The test product is significantly more effective. Evaluation Criteria (Overall Aroma Evaluation): 1: The control product is significantly more effective. 2: The control product is slightly more effective. 3: The effects are equivalent. 4: The test product is slightly more effective. 5: The test product is significantly more effective.

[0117] (Measurement of Acetic Acid Concentration) Immediately after production, 50 g of the sample (pellets) was sealed in a container (size 115 mm x 90 mm, thickness 28 mm) and stored at room temperature for one week. Thereafter, the acetic acid concentration in the container was measured using a gas detection tube method. The measurement results are shown in Table 3 below.

[0118]

[0119] As shown in Table 1-3, the cellulose acetate powders of the Examples were rated higher than those of the Comparative Examples.

[0120] For example, comparing Example 2 (Example 1) with Comparative Example 6 (Comparative Example 1), in Example 2, the twin-screw extrusion throughput increased from 250 kg / hr to 350 kg / hr, which is expected to result in an approximately 40% improvement in productivity in the extrusion process. Furthermore, since no strand breakage occurred in Example 2, material loss was also reduced. Furthermore, the tensile elongation of Example 2 was approximately twice that of Comparative Example 6, confirming that the mechanical properties of the resulting molded product were improved. Furthermore, comparing Example 3 (Example 1) with Comparative Example 11 (Comparative Example 1), it was confirmed that Example 3 also reduced the acetic acid odor and produced a molded product with a high fragrance effect.

[0121] Furthermore, when Example 2 (Example 1) is compared with Comparative Example 7 (Comparative Example 2), it is found that the melt flow rate (MFR) is about 1.2 times that of Example 2 (Example 1), and that the processability is improved. From the above evaluation results, the superiority of the present disclosure is clear.

[0122] Disclosed Items Each of the following items discloses a preferred embodiment.

[0123] [Item 1] A powder containing cellulose acetate as a main component, wherein the cellulose acetate has an acetyl substitution degree of 2.0 to 2.6, an amount of sulfuric acid component of 50 ppm or less, and a particle size distribution in which the proportion of particles having a particle diameter of 1000 μm or more is 40% by weight or less.

[0124] [Item 2] The cellulose acetate powder according to Item 1, having a particle size distribution in which the proportion of particles having a particle diameter of 1000 μm or more is 10% by weight or less.

[0125] [Item 3] The cellulose acetate powder according to Item 1 or 2, wherein the cumulative 50% particle diameter D50 in a volume-based particle size distribution determined by a laser diffraction / scattering method is 500 μm or less.

[0126] [Item 4] The cellulose acetate powder according to any one of Items 1 to 3, wherein the cumulative 50% particle diameter D50 in the weight-based particle size distribution determined by a dry sieving method is 200 μm or less.

[0127] [Item 5] The cellulose acetate powder according to any one of Items 1 to 4, wherein the proportion of particles having a particle diameter of 500 μm or more and less than 1000 μm in the particle size distribution is 30% by weight or less.

[0128] [Item 6] The cellulose acetate powder according to any one of Items 1 to 5, wherein the proportion of particles having a particle diameter of 300 μm or more and less than 500 μm in the particle size distribution is 10% by weight or less.

[0129] [Item 7] The cellulose acetate powder according to any one of Items 1 to 6, wherein the proportion of particles having a particle diameter of 150 μm or more and less than 300 μm in the particle size distribution is 20% by weight or more.

[0130] [Item 8] The cellulose acetate powder according to any one of Items 1 to 7, wherein the proportion of particles having a particle diameter of 50 μm or more and less than 150 μm in the particle size distribution is 10% by weight or more.

[0131] [Item 9] The cellulose acetate powder according to any one of Items 1 to 8, wherein in the particle size distribution, the proportion of particles having a particle diameter of less than 50 μm is 25% by weight or less.

[0132] [Item 10] The cellulose acetate powder according to any one of Items 1 to 9, wherein the cellulose acetate has a calcium content of less than 1.0 ppm.

[0133] [Item 11] The cellulose acetate powder according to any one of Items 1 to 10, further comprising a plasticizer.

[0134] [Item 12] The cellulose acetate powder according to Item 11, wherein the plasticizer is selected from the group consisting of an adipic acid ester compound and a citrate ester compound.

[0135] [Item 13] A molded article formed by containing the cellulose acetate powder according to any one of items 1 to 12.

[0136] [Item 14] A pellet formed containing the cellulose acetate powder according to any one of items 1 to 12.

[0137] The cellulose acetate powder according to the present disclosure can be used as a molding material in various fields.

Claims

1. A powder mainly composed of cellulose acetate, the cellulose acetate having an acetyl substitution degree of 2.0 or more and 2.6 or less, an amount of sulfuric acid component of 50 ppm or less, and a particle size distribution in which the proportion of particles having a particle diameter of 1000 μm or more is 40 weight % or less.

2. The cellulose acetate powder according to claim 1, having a particle size distribution in which the proportion of particles having a particle diameter of 1000 μm or more is 10% by weight or less.

3. The cellulose acetate powder according to claim 1, having a cumulative 50% particle diameter D50 of 500 μm or less in a volume-based particle size distribution measured by a laser diffraction / scattering method.

4. The cellulose acetate powder according to claim 1, having a cumulative 50% particle diameter D50 in a weight-based particle size distribution as determined by a dry sieving method of 200 μm or less.

5. The cellulose acetate powder according to claim 1, wherein the proportion of particles having a particle diameter of 500 μm or more and less than 1000 μm in the particle size distribution is 30% by weight or less.

6. The cellulose acetate powder according to claim 1, wherein the proportion of particles having a particle diameter of 300 μm or more and less than 500 μm in the particle size distribution is 10% by weight or less.

7. The cellulose acetate powder according to claim 1, wherein the proportion of particles having a particle diameter of 150 μm or more and less than 300 μm in the particle size distribution is 20% by weight or more.

8. The cellulose acetate powder according to claim 1, wherein the proportion of particles having a particle diameter of 50 μm or more and less than 150 μm in the particle size distribution is 10% by weight or more.

9. The cellulose acetate powder according to claim 1, wherein in the particle size distribution, the proportion of particles with a diameter of less than 50 μm is 25% by weight or less.

10. The cellulose acetate powder according to claim 1, wherein the cellulose acetate has a calcium content of less than 1.0 ppm.

11. The cellulose acetate powder of claim 1, further comprising a plasticizer.

12. The cellulose acetate powder according to claim 11, wherein the plasticizer is selected from the group consisting of adipate compounds and citrate compounds.

13. A molded article formed containing the cellulose acetate powder according to claim 1.

14. A pellet formed containing the cellulose acetate powder of claim 1.

Citation Information

Patent Citations

  • Production of cellulose acetate

    JP1985139701A

  • Production of cellulose acetate

    JP1991205401A

  • Process for initiating acetylation and equipment therefor

    JP1997216901A

  • Method for reaction control and apparatus therefor

    JP1997272701A

  • 6-position-highly acetylated cellulose acetate and method for producing the same

    JP2009019123A