Anode active material for lithium secondary battery, manufacturing method therefor and lithium secondary battery comprising same
The use of natural graphite with enhanced particle strength and a low-crystalline carbon coating in lithium secondary batteries addresses the degradation issues, resulting in improved charging output and lifespan by optimizing the structural and electrical properties of the anode active material.
Patent Information
- Application Number
- PCT/KR2024/007026
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Lithium secondary batteries face challenges with the degradation of charging output and lifespan due to dendrite formation and irreversible reactions, particularly in natural graphite anode active materials used in electric vehicles and energy storage systems, which require improved charging characteristics and longevity.
A negative electrode active material for lithium secondary batteries is developed using natural graphite that satisfies specific physical properties, including high particle strength achieved through oxidation treatment and high-density spheronization, along with a coating layer of low-crystalline carbon materials to enhance lithium ion conductivity and reduce side reactions.
The solution significantly improves both charging output characteristics and lifespan of lithium secondary batteries by increasing particle strength, reducing porosity, and enhancing lithium ion conductivity, leading to better electrochemical performance and extended battery life.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Negative active material for lithium secondary battery, method for producing same, and lithium secondary battery including same
[0001] The present invention relates to an anode active material for a lithium secondary battery, a method for producing the same, and a lithium secondary battery comprising the same, and more specifically, to an anode active material for a lithium secondary battery comprising natural graphite, a method for producing the same, and a lithium secondary battery comprising the same.
[0002]
[0003] As the price of energy sources rises due to the depletion of fossil fuels and concerns about environmental pollution grow, eco-friendly alternative energy sources are becoming an essential factor for future life.
[0004] In particular, as technological development and demand for mobile devices increase, the demand for secondary batteries as an energy source is rapidly increasing, and recently, the use of secondary batteries as a power source for electric vehicles (xEV) and energy storage systems (ESS) is becoming a reality.
[0005] The above secondary battery has traditionally used lithium metal as a cathode, but as problems have arisen regarding battery short-circuiting due to dendrite formation and the risk of explosion due to this, the use of carbon-based active materials that enable reversible lithium ion intercalation and deintercalation and maintain structural and electrical properties has emerged.
[0006] As the above carbon-based active material, various forms of carbon-based materials such as artificial graphite, natural graphite, and hard carbon have been applied, and among these, graphite-based active materials are the most widely used because they can guarantee the life characteristics of lithium secondary batteries with excellent reversibility. Since the graphite-based active material has a low discharge voltage of -0.2 V compared to lithium, a battery using the graphite-based active material can exhibit a high discharge voltage of 3.6 V, thereby providing many advantages in terms of energy density of lithium batteries.
[0007] Among these, natural graphite in particular has the advantage of exhibiting higher output and capacity than other carbon-based active materials such as artificial graphite, and has excellent adhesive strength, allowing for reduced use of binders and the implementation of high-capacity, high-density negative electrodes.
[0008] In particular, lithium secondary batteries used in electric vehicles require rapid charging characteristics, enabling rapid charging, and long-life characteristics, ensuring excellent retention of discharge capacity over repeated charging and discharging. Therefore, there is a pressing need to develop technologies that can further improve the charge output and lifespan characteristics of existing natural graphite anode active materials.
[0009]
[0010] Accordingly, one object of the present invention is to provide a negative electrode active material for a lithium secondary battery having improved charge output characteristics and lifespan characteristics, a method for producing the same, and a lithium secondary battery including the same.
[0011]
[0012] One embodiment of the present invention provides a negative active material for a lithium secondary battery, which includes natural graphite, and wherein the natural graphite satisfies the following formula 1.
[0013] [Formula 1]
[0014] P 1.7 - P 1.3 ≥ 1200 kg·f / ㎠
[0015] In the above equation 1, P 1.7 is the applied pressure when the pellet density becomes 1.7 g / cc, and P 1.3 is the applied pressure when the pellet density becomes 1.3 g / cc.
[0016]
[0017] The above natural graphite can satisfy the following equation 2.
[0018] [Formula 2]
[0019] P 1.6 - P 1.3 ≥ 850 kg·f / ㎠
[0020] In the above equation 2, P 1.6 is the applied pressure when the pellet density becomes 1.6 g / cc, and P 1.3 is the applied pressure when the pellet density becomes 1.3 g / cc.
[0021]
[0022] The above natural graphite can satisfy the following equation 3.
[0023] [Formula 3]
[0024] P 1.5 - P 1.3 ≥ 550 kg·f / ㎠
[0025] In the above equation 3, P 1.5 is the applied pressure when the pellet density becomes 1.5 g / cc, and P 1.3 is the applied pressure when the pellet density becomes 1.3 g / cc.
[0026]
[0027] The above natural graphite can satisfy the following equation 4.
[0028] [Formula 4]
[0029] P 1.4 - P 1.3 ≥ 250 kg·f / ㎠
[0030] In the above equation 4, P 1.4 is the applied pressure when the pellet density becomes 1.4 g / cc, and P 1.3 is the applied pressure when the pellet density becomes 1.3 g / cc.
[0031]
[0032] The above natural graphite may have an orientation peak intensity ratio (I110 / I004) of 0.50 or more when analyzing an XRD pattern.
[0033] The above natural graphite may have a sphericity of 0.85 or more.
[0034]
[0035] The negative active material for the above lithium secondary battery is disposed on the natural graphite and may further include a coating layer containing a low-crystalline carbon material.
[0036] The above low-crystalline carbon material may be soft carbon, hard carbon, or a combination thereof.
[0037] The content of the coating layer may be 1 to 20 wt% based on the total weight of the natural graphite.
[0038] The above negative active material for lithium secondary batteries has a tap density of 1.1 g / cm 3 It could be strange.
[0039] The above negative active material for a lithium secondary battery may have a SPAN value of 1 to 1.5.
[0040] The above negative active material for a lithium secondary battery may have an average particle diameter (D50) of 12 to 20 μm.
[0041]
[0042] Another embodiment of the present invention provides a method for producing a negative active material for a lithium secondary battery, comprising the steps of: preparing natural graphite powder; oxidizing the natural graphite powder; and forming the oxidized natural graphite powder into a high-density spheroid.
[0043] The above oxidation treatment can be performed at a temperature of 500 to 700°C.
[0044] The above oxidation treatment can be performed for 1 to 5 hours.
[0045] The above oxidation treatment can be performed in air or oxygen atmosphere.
[0046] The above high-density spheroidization can be performed by a mechanical spheroidization method.
[0047] The above mechanical spheroidization method can be performed by one or more methods selected from the group consisting of air classifying milling, spheronizing milling, grinding milling, mechanofusion milling, planetary milling, hybridization milling, shape milling, and high speed milling.
[0048] After the step of forming the oxidized natural graphite powder into high-density spheroids, a step of mixing a low-crystalline carbon material precursor and then heat-treating the mixture to form a coating layer containing a low-crystalline carbon material may be further included.
[0049] The above low-crystalline carbon precursor may be petroleum pitch, coal pitch, mesophase pitch, heavy oil, light oil, polyvinyl alcohol (PVA), polyvinyl chloride (PVC), sucrose, phenol resin, furan resin, furfuryl alcohol, polyacrylonitrile, cellulose, styrene, polyimide, epoxy resin, glucose, or a combination thereof.
[0050]
[0051] Another embodiment of the present invention provides a negative electrode for a lithium secondary battery comprising the above-described negative electrode active material.
[0052] Another embodiment of the present invention provides a lithium secondary battery including the negative electrode.
[0053]
[0054] A negative active material for a lithium secondary battery according to one embodiment of the present invention can improve the charge output characteristics and life characteristics of the battery.
[0055]
[0056] The terms first, second, and third, etc., are used to describe, but are not limited to, various parts, components, regions, layers, and / or sections. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.
[0057] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.
[0058] When a part is referred to as being "on" or "over" another part, it can be directly on or over the other part, or there may be other parts intervening. Conversely, when a part is referred to as being "directly on" another part, there are no other parts intervening.
[0059] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.
[0060] Also, unless otherwise stated, % means weight%, and 1 ppm is 0.0001 weight%.
[0061] In this specification, the term "combination(s) thereof" described in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including any one or more selected from the group consisting of said components.
[0062] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.
[0063]
[0064] 1. Negative active material
[0065] The present inventors have conducted repeated research to improve both the charging output and lifespan characteristics of a natural graphite negative electrode active material, and have thus completed the present invention by discovering that the above effects can be preferably achieved when the negative electrode active material satisfies properties such as Equation 1 below.
[0066] One embodiment of the present invention provides a negative active material for a lithium secondary battery, which includes natural graphite, and wherein the natural graphite satisfies the following formula 1.
[0067] [Formula 1]
[0068] P 1.7 - P 1.3 ≥ 1200 kg·f / ㎠
[0069] In the above equation 1, P 1.7 is the applied pressure when the pellet density of the negative electrode active material becomes 1.7 g / cc, and P 1.3 is the applied pressure when the pellet density of the negative active material becomes 1.3 g / cc.
[0070] In this specification, “pellet density” refers to the density of active material powder measured when a load is applied in the height direction after a specific mass and specific area of active material powder sample is placed in a cylinder and pressure is applied. That is, Equation 1 above refers to the additional applied pressure required to increase the pellet density of the active material powder from 1.3 g / cc to 1.7 g / cc, and the greater the additional applied pressure, the stronger the rigidity of the active material powder. In other words, the natural graphite according to the present invention has very high particle strength.
[0071] Since the negative active material for a lithium secondary battery according to one embodiment of the present invention satisfies Equation 1, both the charge output characteristics and life characteristics of the battery can be improved.
[0072] More specifically, the inventors of the present invention have discovered that a natural graphite active material having a high particle strength satisfying Equation 1 can be more easily obtained by oxidizing natural graphite powder and then forming it into a high-density spheroid.
[0073] At this time, when natural graphite powder is oxidized, the carbon atoms on the graphite surface react with oxygen to form carbon dioxide, and some of the planes forming the layered structure of the natural graphite are decomposed, which can form new lithium ion channels. Accordingly, since lithium ions can pass through both the lithium ion channels in the direction parallel to the planes forming the layered structure, which are the original lithium ion movement paths, and the lithium ion channels newly formed by the above process, the charging output characteristics of the battery can be improved. In addition, when natural graphite is sphericalized into a high-density shape, the directionality of the graphite layer edges within the graphite particles can be diversified, allowing for smoother movement of lithium ions. Accordingly, the charging output characteristics of the battery can be improved.
[0074] Meanwhile, the inventors of the present invention have discovered that when the negative active material satisfies Equation 1, not only the charge output characteristics of the battery but also the lifespan characteristics are improved. This is believed to be because the oxidation-high-density spheroidization process maximizes the effectiveness of high-density spheroidization and minimizes the porosity within the graphite, thereby reducing the irreversible lithium consumption due to additional SEI formation between the electrolyte / graphite interface during the lifespan, which is known to be a major lifespan degradation mechanism.
[0075] More specifically, the value of Formula 1 of the above natural graphite may be 1250 kg·f / ㎠ or more.
[0076]
[0077] In one embodiment, the natural graphite may satisfy the following equation 2.
[0078] [Formula 2]
[0079] P 1.6 - P 1.3 ≥ 850 kg·f / ㎠
[0080] In the above equation 2, P 1.6 is the applied pressure when the pellet density becomes 1.6 g / cc, and P 1.3is the applied pressure when the pellet density becomes 1.3 g / cc.
[0081] More specifically, the value of Formula 2 of the above natural graphite may be 870 kg·f / ㎠ or more.
[0082]
[0083] In one embodiment, the natural graphite may satisfy the following equation 3.
[0084] [Formula 3]
[0085] P 1.5 - P 1.3 ≥ 550 kg·f / ㎠
[0086] In the above equation 3, P 1.5 is the applied pressure when the pellet density becomes 1.5 g / cc, and P 1.3 is the applied pressure when the pellet density becomes 1.3 g / cc.
[0087] More specifically, the value of Formula 3 of the above natural graphite may be 570 kg·f / ㎠ or more.
[0088]
[0089] In one embodiment, the natural graphite may satisfy the following equation 4.
[0090] [Formula 4]
[0091] P 1.4 - P 1.3 ≥ 250 kg·f / ㎠
[0092] In the above equation 4, P 1.4 is the applied pressure when the pellet density becomes 1.4 g / cc, and P 1.3 is the applied pressure when the pellet density becomes 1.3 g / cc.
[0093] More specifically, the value of Formula 4 of the above natural graphite may be 280 kg·f / ㎠ or more.
[0094]
[0095] The technical significance of the negative active material satisfying the above equations 2 to 4 is the same as equation 1 described above, and is therefore omitted.
[0096]
[0097] Meanwhile, the natural graphite may have an orientation peak intensity ratio (I110 / I004) of 0.50 or more when analyzing the XRD pattern, and more specifically, may be 0.51 or more and 0.70 or less.
[0098] In this specification, the orientation peak intensity ratio (I110 / I004) means a value obtained by dividing the area obtained by integrating the peak intensities of the (110) plane and (004) plane measured by XRD of the (110) plane and (004) plane. Specifically, the (110) plane represents a range of 76.5 degrees < 2θ < 78.5 degrees, and the (004) plane represents a range of 53.5 < 2θ < 56.0 degrees, and 2θ represents a diffraction angle.
[0099] As the orientation peak intensity ratio (I110 / I004) of natural graphite satisfies the above range, the orientation of the edge portion of the graphite layer within the graphite particles can be diversified, so that the movement of lithium ions can occur more smoothly, and thus the charging output characteristics of the battery can be improved.
[0100]
[0101] The above natural graphite may have a sphericity of 0.85 or more, and more specifically, 0.90 or more.
[0102] In this specification, sphericity is a numerical expression of the degree to which a particle is close to a sphere, and refers to the value obtained by dividing the perimeter of a circle having the same area as the particle projection shape by the actual perimeter of the particle projection shape using a flow particle analysis device. This sphericity can be measured using an analyzer for optical image acquisition (Fluid Imaging Technologies, Flowcam 8100) and analysis S / W (visual spreadsheet).
[0103] As natural graphite satisfies the above sphericity range, the density and orientation of the spherical natural graphite particles increase together, so that when applied to a negative electrode active material, uniform surface coating becomes possible, electrode energy density can be improved, and the output characteristics of the battery can be improved.
[0104] The above-described orientation peak intensity ratio (I110 / I004) and sphericity range can be more easily obtained through a high-density sphericity process in the manufacturing method.
[0105]
[0106] The above-described negative active material for a lithium secondary battery is disposed on the natural graphite and may further include a coating layer containing a low-crystalline carbon material. By further including the coating layer on the surface of the natural graphite, side reactions of the natural graphite with the electrolyte are suppressed, thereby reducing irreversible reactions and improving lithium ion conductivity, thereby improving electrochemical characteristics such as battery output and lifespan.
[0107] The above low-crystalline carbon material is not particularly limited. For example, the low-crystalline carbon material may be, but is not limited to, soft carbon, hard carbon, or a combination thereof. The graphitizable carbon may be an amorphous carbon-based material manufactured by carbonizing coke, needle coke, coal pitch, petroleum pitch, mesophase pitch, or a combination thereof. The non-graphitizable carbon may be an amorphous carbon-based material manufactured by pyrolyzing phenol resin, furan resin, furfuryl alcohol, polyacrylonitrile, styrene, polyimide, epoxy resin, or a combination thereof.
[0108] The content of the coating layer may be 1 to 20 wt% based on the total weight of the natural graphite, and more specifically, 2 to 16 wt%, 3 to 12 wt%, or 4 to 10 wt%. When the content of the coating layer satisfies the above range, the natural graphite and the coating layer can be effectively bonded, and the output and life characteristics of the lithium secondary battery can be improved by reducing side reactions and improving lithium ion conductivity.
[0109]
[0110] The above negative active material for lithium secondary batteries has a tap density of 1.1 g / cm 3 It can be ideal. As the tap density of the negative active material satisfies the above range, the electrode energy density can be improved. In the present specification, the tap density can be measured by a method generally used in the art for measuring the degree of filling of a sample per unit volume. For example, it can be the density (sample weight / volume) calculated through the change in volume after a measuring container containing a sample is mechanically dropped (tapped) from a fixed height a fixed number of times in accordance with the measuring device and method specified in ASTM B527.
[0111] The above-described negative electrode active material for a lithium secondary battery may have a SPAN value of 1 to 1.5. When the SPAN value of the negative electrode active material satisfies the above range, there may be advantages of improved swelling characteristics due to reduced electrode resistance caused by fine particles and coarse particles and reduced electrode expansion. More specifically, if the SPAN value of the negative electrode active material is too small, there may be problems such as local electrode expansion due to a relatively wide particle size distribution, and if the SPAN value of the negative electrode active material is too large, there may be problems of reduced electrode rollability and increased porosity within the electrode. In the present specification, the SPAN value means a value obtained by calculating the particle size [particle size (D90) - particle size (D10)] / particle size (D50), and particle size (D90), particle size (D50), and particle size (D10) may be defined as particle sizes corresponding to 90%, 50%, and 10% of the volume accumulation amount in the particle size distribution curve, respectively. Each of the above particle sizes can be measured, for example, using the laser diffraction method.
[0112] The above-described negative electrode active material for a lithium secondary battery may have an average particle size (D50) of 12 to 20 μm. When the average particle size of the negative electrode active material satisfies the above range, there may be advantages in securing maximum electrode adhesion and rollability, as well as securing electrochemical reversible capacity and realizing initial efficiency. More specifically, if the average particle size of the negative electrode active material is too small, there may be a problem of decreasing the initial charge / discharge Coulombic efficiency due to an increase in the specific surface area, and if the average particle size of the negative electrode active material is too large, there may be a problem of increasing electrode resistance and electrode expansion rate. In the present specification, the average particle size (D50) may be defined as a particle size corresponding to 50% of the volume accumulation amount in the particle size distribution curve of the particles.
[0113]
[0114] 2. Method for manufacturing negative active material
[0115] Another embodiment of the present invention provides a method for producing a negative active material for a lithium secondary battery, comprising the steps of: preparing natural graphite powder; oxidizing the natural graphite powder; and forming the oxidized natural graphite powder into a high-density spheroid.
[0116] Hereinafter, a method for manufacturing a negative electrode active material for a lithium secondary battery according to another embodiment of the present invention will be described step by step.
[0117]
[0118] First, prepare natural graphite powder.
[0119] At this time, the prepared natural graphite may be a primary spherical form of natural graphite raw material powder.
[0120] The above first spheroidization may be performed by a general method of spheroidizing plate-shaped natural graphite raw material powder in order to use spheroidized graphite material in the manufacture of negative electrode active materials.
[0121]
[0122] Next, the natural graphite powder is subjected to oxidation treatment.
[0123] Through the above oxidation process, carbon atoms and oxygen atoms on the graphite surface react to produce carbon dioxide, which in turn decomposes some of the planes forming the graphite's layered structure, forming new lithium ion channels. Furthermore, as described in the high-density spheroidization process described below, this process further enhances the particle strength of the active material.
[0124] The above oxidation treatment can be performed at a temperature of 500 to 700°C. If the oxidation treatment temperature is too low, the oxidation reaction may not proceed, resulting in a problem of minimal oxidation effect as described above. On the other hand, if the oxidation treatment temperature is too high, excessive oxidation of the graphite surface layer may cause an increase in surface roughness and an increase in the specific surface area, resulting in a decrease in the reversible discharge capacity and initial charge / discharge coolant efficiency.
[0125] The above oxidation treatment can be performed for 1 to 5 hours. If the oxidation treatment time is too short, there may be a problem in that the aforementioned oxidation effect is minimal, and if the oxidation treatment time is too long, there may be a problem in that the surface roughness increases and the specific surface area increases due to excessive oxidation of the graphite surface layer, resulting in a decrease in the reversible discharge capacity and the initial charge / discharge coolant efficiency.
[0126] The above oxidation treatment can be performed in air or oxygen atmosphere.
[0127]
[0128] Next, the above-mentioned oxidized natural graphite powder is formed into high-density spheroids.
[0129] The above high-density spheroidization can be performed by a mechanical spheroidization method.
[0130] The above mechanical spheroidization method can be performed by one or more methods selected from the group consisting of air classifying milling, spheronizing milling, grinding milling, mechanofusion milling, planetary milling, hybridization milling, shape milling, and high speed milling.
[0131] The above secondary re-sphericization step can be performed at a rotation speed of 500 to 4000 rpm, and more specifically, can be performed at a rotation speed of 700 to 2000 rpm or 800 to 1500 rpm. By performing sphericization at a rotation speed within the above range, cracking and destruction of the graphite raw material can be minimized, and natural graphite with an appropriate degree of sphericity can be formed.
[0132] The above secondary re-sphericization step can be performed for 5 to 40 minutes, more specifically for 8 to 25 minutes or 10 to 20 minutes. By performing sphericization for a time within the above range, natural graphite having an appropriate degree of sphericity can be formed.
[0133] In particular, the method for manufacturing a negative active material according to the present invention can further strengthen the particle strength of the negative active material and form the interior of the graphite particles more densely as high-density spheroidization progresses after oxidation treatment compared to when only high-density spheroidization progresses. Accordingly, the values of Equations 1 to 4 described above can further increase. This is because some of the planes forming the layer structure of the graphite are decomposed by the oxidation treatment, and graphite with shorter planes are more densely aggregated by high-density spheroidization.
[0134]
[0135] Through the above oxidation treatment and high-density spheroidization process, the properties of the obtained negative active material, such as Equations 1 to 4, orientation peak intensity ratio (I110 / I004), and spheroidization degree, can be appropriately obtained within the range according to the present invention.
[0136]
[0137] Next, after the step of forming the oxidized natural graphite powder into high-density spheroids, a step of mixing a low-crystalline carbon material precursor and then heat-treating the mixture to form a coating layer containing a low-crystalline carbon material may be further included.
[0138] The above low-crystalline carbon precursor may be petroleum pitch, coal pitch, mesophase pitch, heavy oil, light oil, polyvinyl alcohol (PVA), polyvinyl chloride (PVC), sucrose, phenol resin, furan resin, furfuryl alcohol, polyacrylonitrile, cellulose, styrene, polyimide, epoxy resin, glucose, or a combination thereof.
[0139] The above mixing can be performed by a mechanical mixing method. At this time, the mechanical mixing method can be performed by at least one method selected from the group consisting of ball milling, mechanofusion milling, shaker milling, planetary milling, attritor milling, shape milling, nauta milling, nobilta milling, high speed mixing, paddle mixing, ribbon mixing, Henschel mixing, corn type mixing, thinky mixing, homo mixing, and a stirrer.
[0140] The above mechanical mixing method can be performed at a rotation speed of 500 to 3000 rpm.
[0141] The above heat treatment can be performed in an atmosphere of hydrogen, nitrogen, argon, or a mixed gas thereof at a temperature of 600 to 1500°C.
[0142]
[0143] 3. Cathode and lithium secondary battery
[0144] Another embodiment of the present invention provides a negative electrode for a lithium secondary battery comprising the above-described negative electrode active material.
[0145] According to another embodiment of the present invention, a negative electrode for a lithium secondary battery may more specifically include: a negative electrode current collector; and a negative electrode active material layer positioned on the negative electrode current collector and including the above-described negative electrode active material for a lithium secondary battery.
[0146] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0147] The above negative electrode active material layer may optionally include a binder and / or a conductive material together with the negative electrode active material.
[0148] The above binder serves to improve the adhesion between negative electrode active material particles and the adhesive strength between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the negative electrode active material layer.
[0149] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types of these may be used. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the negative electrode active material layer.
[0150] A negative electrode for a lithium secondary battery according to one embodiment of the present invention can be manufactured according to a conventional negative electrode manufacturing method, except that the negative electrode active material described above is used.
[0151] Specifically, the composition for forming a negative electrode active material layer, including the aforementioned negative electrode active material and optionally a binder, a conductive agent, and a solvent, can be applied onto a negative electrode current collector, followed by rolling and drying. At this time, the types and contents of the negative electrode active material, binder, and conductive agent are as described above.
[0152] The solvent may be a solvent generally used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the negative electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the negative electrode.
[0153] Alternatively, the negative electrode may be manufactured by casting the composition for forming the negative electrode active material layer on a separate support, then peeling the film from the support and laminating the resulting film on a negative electrode current collector.
[0154]
[0155] Another embodiment of the present invention provides a lithium secondary battery including the negative electrode.
[0156] A lithium secondary battery according to another embodiment of the present invention may more specifically include a positive electrode, a negative electrode positioned opposite the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.
[0157] The above cathode is as described above.
[0158] In addition, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of a positive electrode, a negative electrode, and a separator, and a sealing member that seals the battery container.
[0159]
[0160] The above positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and the positive electrode active material layer may include a positive electrode active material.
[0161] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesion of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0162] The positive electrode active material may be a compound capable of reversibly intercalating and deintercalating lithium (a lithiated intercalation compound). Specifically, one or more of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used. A specific example thereof may be a compound represented by one of the following chemical formulas:
[0163] Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c(In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α T α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α T2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α T α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-αT2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Fe2(PO4)3(0 ≤ f ≤ 2); and LiFePO4.
[0164] In the above chemical formula, A is Ni, Co, Mn or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof; D is O, F, S, P or a combination thereof; E is Co, Mn or a combination thereof; T is F, S, P or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; I is Cr, V, Fe, Sc, Y or a combination thereof; J may be V, Cr, Mn, Co, Ni, Cu or a combination thereof.
[0165] Of course, it is also possible to use a compound having a coating layer on the surface of the compound or a mixture of the compound and a compound having a coating layer.
[0166] The above coating layer may include at least one coating element compound selected from the group consisting of an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, and a hydroxycarbonate of a coating element. The compounds forming these coating layers may be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The coating layer forming process may use any coating method as long as it can coat the compound with these elements by a method (e.g., spray coating, dipping, etc.) that does not adversely affect the physical properties of the positive electrode active material. Since this is well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0167] The above-described positive electrode active material layer may further include a binder and / or a conductive material together with the above-described positive electrode active material.
[0168]
[0169] The above binder serves to improve the adhesion between positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one kind alone or a mixture of two or more kinds thereof may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0170] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any particular restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types may be used among these, but the present invention is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0171] The above anode can be manufactured according to a conventional anode manufacturing method.
[0172] Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, including a positive electrode active material and optionally a binder, a conductive agent, or a solvent, onto a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.
[0173] The solvent may be a solvent generally used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.
[0174] Alternatively, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.
[0175]
[0176] The above separator separates the positive and negative electrodes and provides a passage for lithium ions to move. Any separator commonly used as a separator in lithium secondary batteries can be used without any particular restrictions. In particular, a separator having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.
[0177]
[0178] The above electrolyte may include, but is not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0179] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.
[0180] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.
[0181] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0182] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.
[0183]
[0184] Example 1
[0185] (1) Manufacturing of negative electrode active material
[0186] (Preparation of natural graphite powder) Primary spherical natural graphite powder with an average particle diameter (D50) of 16 μm was prepared.
[0187] (After oxidation treatment), the natural graphite powder was subjected to oxidation treatment in a continuous rotary kiln at 600°C in an air atmosphere for 3 hours.
[0188] (High-density spheroidization) Afterwards, the above-mentioned oxidized natural graphite powder was subjected to high-density spheroidization treatment at 1000 rpm for 25 minutes in a spheronizer, and fine and coarse particles were removed through air classification and sieve classification.
[0189] (Coating) After that, the high-density spherical natural graphite powder was mixed with petroleum pitch as a base material at a weight ratio of 100:8, and then mechanically mixed in a high-speed stirrer at 2000 rpm for 10 minutes to form a uniform mixture. The mixture was placed in a container, heat-treated at 1200°C for 5 hours in a nitrogen atmosphere, and then classified through a 75 μm sieve to produce natural graphite having a coating layer formed thereon.
[0190] (2) Cathode manufacturing
[0191] The above-mentioned negative active material and conductive agent, styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a mass ratio of 96.6:1:1.3:1.1, and then dispersed in deionized distilled water to prepare a negative active material layer composition. The composition was applied to a Cu-foil current collector, and then dried and rolled to obtain an electrode density of 1.50±0.05 and 1.70±0.05 g / cm. 3 The cathode was manufactured.
[0192] (3) Lithium secondary battery manufacturing
[0193] A coin-type 2032 half-cell was manufactured using the above-mentioned cathode as a working electrode and metallic lithium as a counter electrode. At this time, a separator made of a porous polypropylene film was inserted between the working electrode and the counter electrode, and the electrolyte used was a 7:3 volume ratio mixed solution of diethyl carbonate (DEC) and ethylene carbonate (EC) in which 1 M concentration of LiPF6 was dissolved.
[0194]
[0195] Example 2
[0196] A negative electrode active material, a negative electrode, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that natural graphite powder was mixed with petroleum pitch in a weight ratio of 100:8.8.
[0197]
[0198] Comparative Example 1
[0199] A negative electrode active material, a negative electrode, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the high-density spheroidization and coating steps were not performed.
[0200]
[0201] Comparative Example 2
[0202] A negative electrode active material, a negative electrode, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the high-density spheroidization step was not performed.
[0203]
[0204] Comparative Example 3
[0205] A negative active material, a negative electrode, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the oxidation treatment step was not performed.
[0206]
[0207] Comparative Example 4
[0208] A negative active material, a negative electrode, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the oxidation treatment and high-density spheroidization steps were not performed.
[0209]
[0210] Table 1 below summarizes the manufacturing process of the positive electrode active materials of the examples and comparative examples.
[0211] Oxidized high-density spherical coating Example 1○○○ Example 2○○○ Comparative example 1○--Comparative example 2○-○ Comparative example 3-○○ Comparative example 4--○
[0212]
[0213] Experimental Example 1: Evaluation of Active Material Properties
[0214] The properties of the negative active materials manufactured according to the examples and comparative examples were evaluated as follows, and the results are shown in Tables 2 and 3.
[0215] (1) Evaluation of particle size (D10, D50, D90, Dmax) and SPAN values
[0216] For the active material powder, particle size (D10, D50, D90, Dmax) and SPAN values were derived using the laser diffraction method. The SPAN value was derived by calculating [particle size (D90) - particle size (D10)] / particle size (D50). Particle size (Dmax), particle size (D90), particle size (D10), and particle size (D50) can be defined as particle sizes corresponding to 100%, 90%, 10%, and 50% of the volume accumulation amount in the particle size distribution curve, respectively.
[0217] (2) Surface area evaluation
[0218] For the active material powder, the specific surface area was measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020).
[0219] (3) Tap density evaluation
[0220] Based on ASTM B527, 15 g of active material powder was placed in a 50 mL container and tapped at 3000 cycles @ 284 cycles / min to measure the packing density.
[0221] (4) Orientation evaluation
[0222] The area ratio (I110 / I004) was calculated by integrating the peak intensities of the XRD spectrum attributed to the (110) plane and (004) plane of the graphite crystal in the XRD pattern obtained from the X-ray diffraction measurement. More specifically, the XRD measurement conditions are as follows.
[0223] - Target: Cu(Kα-ray) graphite monochromator
[0224] - Slit: Diverging slit = 1 degree, Receiving slit = 0.1 mm, Scatter slit = 1 degree
[0225] - Measurement area and step angle / measurement time:
[0226] - (110) Surface: 76.5 degrees < 2θ < 78.5 degrees, 0.1 degrees / 4.2 seconds
[0227] - (004) Surface: 53.5 degrees < 2θ < 56.0 degrees, 0.1 degrees / 4.2 seconds, where 2θ represents the diffraction angle.
[0228] (5) Evaluation of sphericity
[0229] The sphericity was evaluated by dividing the perimeter of a circle with the same area as the particle projection shape by the actual perimeter of the particle projection shape using a flow-type particle analysis device. At this time, the measurement was performed using an analyzer for optical image acquisition (Fluid Imaging Technologies, Flowcam 8100) and analysis S / W (visual spreadsheet).
[0230] (6) Evaluation of pellet density according to applied pressure, evaluation of Equations 1 to 4
[0231] For the active material powder, the pellet density of the active material powder was measured according to the applied pressure.
[0232] D10(μm)D50(μm)D90(μm)Dmax(μm)SpanSpecific surface area(m) 2 / g)Tap density (g / cc)Orientation (I110 / I004)SphericityExample 16.216.727621.251.91.160.5170.92Example 26.317.428621.251.81.170.6460.92Comparative example 111.119.835741.215.20.820.1550.91Comparative example 210.718.361.762.32.81.80.990.3390.91Comparative example 310.6172652.30.911.71.180.6010.94Comparative example 410.318.152.152.22.311.81.050.4340.87
[0233] Pellet density applied pressure (kg·f / ㎠) Formula 1 Formula 2 Formula 3 41.3 g / cc 1.4 g / cc 1.5 g / cc 1.6 g / cc 1.7 g / cc Example 1 298 59 7 8 9 5 1 1 9 5 1 5 9 5 1 2 9 7 8 9 7 5 9 7 2 9 9 Example 2 29 5 5 7 8 9 5 1 1 9 5 1 5 9 5 1 3 0 0 9 0 6 0 0 3 0 2 Comparative Example 1 1 0 0 1 6 5 2 5 5 3 5 5 4 9 8 3 9 8 2 5 5 1 5 6 5 Comparative Example 2 25 0 3 9 7 5 9 8 9 5 1 0 9 5 8 4 5 6 4 5 3 4 8 1 4 7 Comparative Example 3 20 0 4 0 7 0 1 0 5 1 3 1 0 1 1 0 8 0 5 5 0 2 0 Comparative Example 42203976558451195975625435177
[0234] Referring to Tables 2 and 3, in the case of Examples 1 and 2, in which both the oxidation treatment and the high-density spheroidization process were performed, it was confirmed that the orientation and spheroidization degrees were excellent and the tap density was high. In addition, the values of Equations 1 to 4 were all large, confirming that the particle rigidity was excellent. On the other hand, in the case of Comparative Examples 1, 2, and 4, in which the high-density spheroidization process was not performed, it was confirmed that the orientation degree was inferior and the spheroidization degree was small. In addition, it was confirmed that the values of Equations 1 to 4 were small, confirming that the particle rigidity was inferior.
[0235] Meanwhile, in the case of Comparative Example 3, which performed a high-density spheroidization process but did not perform an oxidation treatment process, the orientation, spheroidization, and tap density were good at similar levels to those of the examples, but it was confirmed that the values of Equations 1 to 4 were lower than those of the examples, and it was confirmed that the particle rigidity was somewhat inferior.
[0236]
[0237] Experimental Example 2: Evaluation of Electrochemical Characteristics of Lithium Secondary Battery
[0238] The electrochemical characteristics of lithium secondary batteries manufactured according to the examples and comparative examples were evaluated and are shown in Table 4 below.
[0239] (1) Evaluation of charging output characteristics (SOC 10% → 80%)
[0240] The manufactured lithium secondary battery was charged at 0.1C to 4.2V / 0.005C under constant current / constant voltage (CC / CV) conditions at 25℃, then discharged at 0.1C to 2.5V under constant current (CC) conditions to complete the formation process, and then charged at 0.1C to 10% of the cell capacity (SOC 10%). From this point on, the battery was charged at each C-rate (2.0C, 2.5C, 3.0C, 3.5C, 4.0C, 4.5C, 5.0C, 6.0C) under constant current / constant voltage (CC / CV) conditions, and the time required to charge to 80% of the cell capacity (SOC 80%) was measured.
[0241] (2) Life characteristics evaluation (3C / 0.5C)
[0242] The manufactured lithium secondary battery was charged at 0.1C to 4.2V / 0.005C under constant current / constant voltage (CC / CV) conditions at 25℃, and then discharged at 0.1C to 2.5V under constant current (CC) conditions to complete the formation process. Then, it was charged at 3C-rate to 4.2V / 0.005C under constant current / constant voltage (CC / CV) conditions, and then discharged at 0.5C to 2.5V under constant current (CC) conditions to measure the discharge capacity retention rate of the 100th cycle cell.
[0243] SOC 10% -> 80% Charge Time (min)Cycle Retention (%, 3C, 100cycle)2C3C4C5C6CExample 12114.512.411.611.393.20%Example 22114.612.311.811.292.10%Comparative Example 122.11715.815.415.291.50%Comparative Example 221.315.714.113.613.591.00%Comparative Example 321.215.11312.312.182.60%Comparative Example 421.820.62020.521.974.10%
[0244] Referring to Table 4, it was confirmed that in the case of Examples 1 and 2, where the properties of the negative active material, such as Formula 1, were sufficiently large, the charge output characteristics and lifespan characteristics at high rates of 2C or more were both very excellent. On the other hand, in the case of Comparative Examples 1 to 4, where the properties of the negative active material, such as Formula 1, were small, the charge output characteristics and lifespan characteristics were inferior to those of the Examples.
[0245]
[0246] Although the preferred embodiments of the present invention have been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the patent claims, the detailed description of the invention, and the attached drawings, and it is obvious that this also falls within the scope of the present invention.
[0247] Accordingly, the actual scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Contains natural graphite, The above natural graphite is an anode active material for a lithium secondary battery satisfying the following formula 1: [Formula 1] P.S 1.7 - P.S 1.3 ≥ 1200 kg·f / ㎠ In the above equation 1, P 1.7 is the applied pressure when the pellet density of the negative active material becomes 1.7 g / cc, and P 1.3 is the applied pressure when the pellet density of the negative active material becomes 1.3 g / cc.
2. In paragraph 1, The above natural graphite is an anode active material for a lithium secondary battery satisfying the following formula 2: [Formula 2] P.S 1.6 - P.S 1.3 ≥ 850 kg·f / ㎠ In the above equation 2, P 1.6 is the applied pressure when the pellet density of the negative electrode active material becomes 1.6 g / cc, and P 1.3 is the applied pressure when the pellet density of the negative active material becomes 1.3 g / cc.
3. In paragraph 1, The above natural graphite is an anode active material for a lithium secondary battery satisfying the following formula 3: [Formula 3] P.S 1.5 - P.S 1.3 ≥ 550 kg·f / ㎠ In the above equation 3, P 1.5 is the applied pressure when the pellet density of the negative active material becomes 1.5 g / cc, and P 1.3 is the applied pressure when the pellet density of the negative active material becomes 1.3 g / cc.
4. In paragraph 1, The above natural graphite is an anode active material for a lithium secondary battery satisfying the following formula 4: [Formula 4] P.S 1.4 - P.S 1.3 ≥ 250 kg·f / ㎠ In the above equation 4, P 1.4 is the applied pressure when the pellet density of the negative active material becomes 1.4 g / cc, and P 1.3 is the applied pressure when the pellet density of the negative active material becomes 1.3 g / cc.
5. In paragraph 1, The above natural graphite is a negative electrode active material for a lithium secondary battery having an orientation peak intensity ratio (I110 / I004) of 0.50 or more when analyzed by XRD pattern.
6. In paragraph 1, The above natural graphite is a negative electrode active material for a lithium secondary battery having a sphericity of 0.85 or higher.
7. In paragraph 1, The above natural graphite is an oxidized negative active material for a lithium secondary battery.
8. In paragraph 1, A negative active material for a lithium secondary battery, which is disposed on the above natural graphite and further includes a coating layer containing a low-crystalline carbon material.
9. In paragraph 8, A negative electrode active material for a lithium secondary battery, wherein the content of the coating layer is 1 to 20 wt% based on the total weight of the natural graphite.
10. In paragraph 1, Tap density is 1.1 g / cm 3 A negative electrode active material for a lithium secondary battery.
11. In paragraph 1, A negative active material for a lithium secondary battery having a SPAN value of 1 to 1.
5.
12. In paragraph 1, A negative active material for a lithium secondary battery having an average particle diameter (D50) of 12 to 20 μm.
13. Step for preparing natural graphite powder; A step of oxidizing the above natural graphite powder; and A step of forming the above oxidized natural graphite powder into a high-density spheroid, A method for manufacturing a negative electrode active material for a lithium secondary battery.
14. In paragraph 13, A method for producing a negative active material for a lithium secondary battery, wherein the above oxidation treatment is performed at a temperature of 500 to 700°C.
15. In paragraph 13, A method for manufacturing a negative active material for a lithium secondary battery, wherein the above oxidation treatment is performed for 1 to 5 hours.
16. In paragraph 13, A method for manufacturing a negative active material for a lithium secondary battery, wherein the above oxidation treatment is performed in an air or oxygen atmosphere.
17. In paragraph 13, After the step of forming the above-mentioned oxidized natural graphite powder into high-density spheroids, A method for manufacturing a negative active material for a lithium secondary battery, further comprising a step of mixing a low-crystalline carbon material precursor and then heat-treating the mixture to form a coating layer containing a low-crystalline carbon material.
18. A negative electrode for a lithium secondary battery comprising the negative electrode active material of any one of claims 1 to 12.
19. A lithium secondary battery comprising the negative electrode for a lithium secondary battery of Article 18.
Citation Information
Patent Citations
Negative electrode material for nonaqueous electrolyte secondary battery, negative electrode using the same, and nonaqueous electrolyte secondary battery
JP2010251126A
Negative electrode material for non-aqueous secondary battery, negative electrode for non-aqueous secondary battery, and non-aqueous secondary battery
JP2019175775A
Carbonaceous material for cell and cell containing thecarbonaceous material
KR1020010080071A
Negative electrode active material for rechargeable lithium battery, method for preparing the same, negative electrode including the same, and rechargeable lithium battery including the negative electrode
KR1020140140952A
Negative electrode material for lithium ion secondary battery, production method for negative electrode material for lithium ion secondary battery, negative electrode material slurry for lithium ion secondary battery, negative electrode for lithium ion secondary battery, and lithium ion secondary battery
US20210083288A1