Ferroelectric nitride field effect transistors

WO2024249498A1PCT designated stage expired Publication Date: 2024-12-05THE RGT UNIV OF MICHIGAN
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/031445
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-29
Publication Date
2024-12-05

Smart Images

  • Figure US2024031445_05122024_PF_FP_ABST
    Figure US2024031445_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A device includes a substrate and a heterostructure supported by the substrate. The heterostructure includes a gate dielectric layer comprising a III-nitride alloy, the III-nitride alloy comprising a Group IIIB element, and a channel layer adjacent to the gate dielectric layer. The channel layer is transparent at an operational wavelength of the device. The III-nitride alloy is ferroelectric.
Need to check novelty before this filing date? Find Prior Art

Description

FERROELECTRIC NITRIDE FIELD EFFECT TRANSISTORSCROSS-REFERENCE TO RELATED APPLICATION

[0001] This application claims the benefit of U.S. provisional application entitled “Ferroelectric Nitride Field Effect Transistors,” filed May 29, 2023, and assigned Serial No. 63 / 469,500, the entire disclosure of which is hereby expressly incorporated by reference.BACKGROUND OF THE DISCLOSUREField of the Disclosure

[0002] The disclosure relates generally to ferroelectric Group Ill-nitride materials.Brief Description of Related Technology

[0003] Non-volatile memory (NVM) technologies have advanced to address the huge surge in data centric computing and the difficulty of traditional dimensional scaling to meet escalating demands. In this context, the discovery of ferroelectricity in HfO2 has invoked renewed interest in ferroelectric field effect transistors (FeFET), in which the polarization switching of a ferroelectric gate barrier is harnessed to control the channel conductance, giving rise to fast read / write operations. The unique functionalities offered by a ferroelectric material can be harnessed to produce in-memory architectures with diffused boundaries between memory and logic, while exceeding the performance gains previously offered by device scaling. Although HfO2 has been extensively studied for FeFET technology, HfO2 faces challenges in terms of ON / OFF ratio, memory window, wake-up time, retention loss, operating voltage, and device variability.

[0004] Meanwhile, transistor scaling has led to ultrathin channel materials, attracting considerable attention to two-dimensional (2D) van der Waals materials. However, these materials have several inherent limitations like propensity to form traps at the interface, high contact resistance at metal / semiconductor interface, and more significantly, a CMOS incompatible growth process.

[0005] Recently, Indium Tin Oxide (ITO), a material traditionally used as a transparent contact layer, has emerged as a prospective alternative material for an ultrathin channel,showing excellent compatibility with CMOS back end-of-line technologies. Thickness scaling and HfO2-based ferroelectric gating has been shown to be effective in enhancing the controllability of such a high-carrier density channel.SUMMARY OF THE DISCLOSURE

[0006] In accordance with one aspect of the disclosure, a device includes a substrate and a heterostructure supported by the substrate. The heterostructure includes a gate dielectric layer including a Ill-nitride alloy, the Ill-nitride alloy including a Group II IB element, and a channel layer adjacent to the gate dielectric layer. The channel layer is transparent at an operational wavelength of the device. The Ill-nitride alloy is ferroelectric.

[0007] In accordance with another aspect of the disclosure, a device includes a substrate and a heterostructure supported by the substrate. The heterostructure includes a gate dielectric layer including a Ill-nitride alloy, the Ill-nitride alloy including a Group 11 IB element, and a channel layer adjacent to the gate dielectric layer. The channel layer includes an oxide material. The Ill-nitride alloy is ferroelectric.

[0008] In accordance with another aspect of the disclosure, a device includes a substrate and a heterostructure including a gate layer supported by the substrate, a gate dielectric layer supported by the gate layer, the gate dielectric layer including a Ill-nitride alloy, the Ill- nitride alloy including a Group 111 B element, and a channel layer supported by the gate dielectric layer. The gate dielectric layer is monocrystalline and ferroelectric.

[0009] In accordance with yet another aspect of the disclosure, a method of fabricating a device, the method including providing a gate layer on a substrate, implementing a nonsputtered, epitaxial growth procedure to form a gate dielectric layer supported by the gate layer, the gate dielectric layer including a Ill-nitride alloy, the Ill-nitride alloy including a Group 111 B element, depositing a channel layer across the gate dielectric layer, the channel layer being transparent at an operational wavelength of the device, and forming source / drain contacts that overlap the channel layer. The non-sputtered, epitaxial growth procedure is configured such that the gate dielectric layer is monocrystalline and ferroelectric.

[0010] In connection with any one of the aforementioned aspects, the devices and / or methods described herein may alternatively or additionally include or involve any combination of one or more of the following aspects or features. The channel layer includes an oxide material. The gate dielectric layer is monocrystalline. The heterostructure further includes a buried gate layer in contact with the Ill-nitride alloy of the gate dielectric layer.The buried gate layer includes a Ill-nitride semiconductor material. The Ill-nitride alloy of thegate dielectric layer is in contact with the buried gate layer. The device further includes a source contact and a drain contact. The source and drain contacts are spaced apart from one another to define a channel of the channel layer. The source and drain contacts overlap the channel layer. The channel layer is thinner in the channel and thicker underneath the source and drain contacts to reduce contact resistance. The heterostructure is configured such that a normalized memory window of the device exceeds about 0.4 Volts per nanometer of gate dielectric layer thickness. The gate dielectric layer has a polarization range greater than 50 pC / cm2. The Ill-nitride alloy of the gate dielectric layer is in contact with the channel layer. The gate dielectric layer is monocrystalline. The heterostructure further includes a buried gate layer in contact with the Ill-nitride alloy of the gate dielectric layer. The buried gate layer includes a Ill-nitride semiconductor material. The channel layer is transparent at an operational wavelength of the device. The heterostructure further includes a buried gate layer in contact with the Ill-nitride alloy of the gate dielectric layer. The buried gate layer includes a Ill-nitride semiconductor material. The method further includes etching the channel layer in between the source / drain contacts. Ambient exposure of the gate dielectric layer prior to depositing the channel layer is controlled to limit surface oxidation to about 1 nm or less.BRIEF DESCRIPTION OF THE DRAWING FIGURES

[0011] For a more complete understanding of the disclosure, reference should be made to the following detailed description and accompanying drawing figures, in which like reference numerals identify like elements in the figures.

[0012] Figure 1 depicts (a) a schematic representation of a device heterostructure in accordance with one example, along with a top-view SEM image showing an example channel length Lchof about 2 pm, (b) a fabrication flow diagram of ScAIN / ITO FeFET device in accordance with one example, (c) a graphical plot of height profile of an ITO film obtained from AFM before and after etching, and (d) a graphical plot of TLM results of 10 nm ITO underneath Ni (inset shows an SEM image of TLM patterns).

[0013] Figure 2 depicts (a) a schematic illustration of an example ScAIN capacitor used for evaluation of ferroelectric response of a 100 nm ScAIN layer, (b) a graphical plot of normalized C-V loop of the ScAIN capacitor measured at an ac-voltage of 200 mV, frequency of about 2 MHz with 50 mV steps, (c) a graphical plot of voltage dependent P-E loops measured at 20 kHz and room temperature showing saturation behavior, and (d) agraphical plot of E-field dependent PUND measurements using triangular pulses (P.W.= 0.1 ms and delay time of 1 s) showing saturated remnant polarization of about 128 pC / cm2.

[0014] Figure 3 depicts graphical plots of (a) log-scale transfer characteristics of an example FeFET device (tCh = 5 nm, Lch= 2 pm and Wch= 5 pm) at two different drain bias (Vds = 0.5 V and 0.1 V); transfer curve of the FeFET before thinning the ITO channel shows the ferroelectric ScAIN is unable to sufficiently modulate the 10 nm ITO channel, (b) linear scale transfer characteristics showing the threshold voltage in the two branches (Vthiand Vth2) and extraction of the memory window, Vthi-Vth2 of about 42 V, (c) output characteristics at different gate bias with the highest Id of about 135 pA / pm at Vds= 3 V, and (d) calculated sheet carrier concentration in the ON and OFF states of the FeFET device showing polarization induced carrier modulation.

[0015] Figure 4 depicts graphical plots of (a) endurance measurements showing lon / loff ratio as a function of poling cycles with maximum lon / loff ~ 106, (b) memory window and threshold voltages with a maximum memory window of 42 V, (c) retention characteristics showing distinct ON and OFF states till 105s, and (d) performance benchmarking of example FeFET devices (shown as red star) against recently reported ferroelectric FETs (shown as blue triangular and circular symbols). The memory window is normalized with respect to ferroelectric layer thickness.

[0016] Figure 5 is a schematic view of a device (e.g., FeFET device) having a ferroelectric gate dielectric layer and channel layer configured in accordance with one example.

[0017] Figure 6 is a flow diagram of a method of fabricating a device (e.g., FeFET device) having a ferroelectric gate dielectric layer and channel layer configured in accordance with one example.

[0018] Figure 7 depicts graphical plots of performance of an 18 nm ScAIN FeFET device in accordance with one example, including: (a) a CV curve (1 MHz, 200 mV) measured from a 18 nm ScAIN capacitor with a top drive electrode diameter of 20pm (shown in inset), (b) a transfer curve of the FeFET device fabricated from the 18 nm ScAIN capacitor showing clear counterclockwise hysteresis, and (c) extraction of threshold voltage (Vn = -3.8 V and Vt2= - 0.6 V) and associated memory window (3.2 V) from the linear plot of the transfer characteristics.

[0019] The embodiments of the disclosed devices and methods may assume various forms. Specific embodiments are illustrated in the drawing and hereafter described with the understanding that the disclosure is intended to be illustrative. The disclosure is not intended to limit the invention to the specific embodiments described and illustrated herein.DETAILED DESCRIPTION OF THE DISCLOSURE

[0020] Devices having a ferroelectric gate dielectric layer are described. The ferroelectric gate dielectric layer includes an epitaxial (e.g., fully epitaxial) ferroelectric Ill-nitride alloy, such as ScAIN. Past issues with HfO2 are addressed by the use of such ferroelectric materials. For instance, Sc-alloyed wurtzite Ill-nitrides (e.g., ScAIN) exhibit large tunable coercive fields (1 .6-5 MV cm-1), remarkable switchable polarization greater than 50 pC / cm2(e.g., 80-120 pC / cm2), and robust ferroelectric properties. The giant switchable polarization and large tunable coercive field of such oxide-free ferroelectric materials are combined with a channel layer to achieve enhanced channel carrier modulation and large memory window in a field-effect transistor device. The channel layers are configured and integrated as described herein to achieve high-performance FeFET devices. Methods of fabricating such devices are also described.

[0021] In some cases, the channel layer of the disclosed devices is composed of, or otherwise includes, indium tin oxide (ITO). Examples described herein exhibit the integration of an ITO-based or other oxide-based channel with an epitaxially grown ferroelectric ScAIN gate dielectric layer to realize high-performance FeFET devices. The example devices show a high ON state current of about 10-4A, remarkable ON / OFF ratio greater than 106and a large, normalized memory window greater than 0.4 V per nm of gate dielectric layer thickness (e.g., 0.42 V / nm). Furthermore, the disclosed devices can withstand repeated program / erase cycling and show excellent retention characteristics, all of which are useful characteristics for transistor-memory functionalities.

[0022] Although the disclosed devices are described in connection with non-volatile memory applications, the disclosed devices and methods are useful in a wide variety of contexts and applications. For instance, the transparency of the channel and other layers of the heterostructure may be useful in connection with various electronic and optoelectronic devices and applications, such as transistor, photovoltaic and photodetection devices.

[0023] The disclosed methods are configured to incorporate scandium (Sc) or other group 111 B elements into the wurtzite crystal structure of the Ill-nitride material. Molecular beam epitaxy (MBE), metal-organic chemical vapor deposition (MOCVD), hydride vapor phase epitaxy (HVPE), pulsed laser deposition (PLD), and other non-sputtered epitaxial growth procedures may be used to realize the ferroelectric Ill-nitride alloy layers. The disclosed methods may or may not include implementation of a post-growth annealing procedure.

[0024] The disclosed devices and structures exhibit ferroelectric switching in one or more single-crystal, or monocrystalline, epitaxially grown layers of an alloy of a Ill-nitride material,e.g., in ScxAli.xN films. The films may be grown by molecular beam epitaxy (MBE) or other non-sputtered, epitaxial procedures (e.g., MOCVD, HVPE, and PLD). In some cases, the layers are grown on GaN templates or other Ill-nitride semiconductor layers. Alternatively, the layers are grown on a metal layer, such as molybdenum. The disclosed methods and devices show the feasibility of controlling the electrical polarization of lll-V semiconductors grown by MBE and other non-sputtered epitaxial growth procedures. The use of epitaxial growth procedures enables thickness scaling (e.g., into the nanometer regime). Epitaxial growth may accordingly be useful in fabricating devices having a broad range of applications in electronic, photonic, optoelectronic, and memory contexts.

[0025] In some examples, ScxAli.xN films were grown using a Veeco GENXpolar MBE system equipped with a radio-frequency (RF) plasma source. In these examples, a Si- doped GaN layer was first grown on a GaN / sapphire template, which may be used as a bottom or buried gate layer, as described herein. Subsequently, a ScxAli.xN layer was grown. The Sc content may be varied by tuning the Sc / AI flux ratio, which may be further confirmed by energy dispersive x-ray spectroscopy (EDS).

[0026] Although described in connection with examples of epitaxially grown ScxAli.xN layers, the disclosed methods and devices may be applied to a wide variety of Ill-nitride alloys. The disclosed methods and devices may thus include or involve the incorporation of scandium into other Ill-nitride wurtzite structures. For instance, the disclosed methods and devices may include or involve one or more epitaxially grown ScxAlyGai-x.yN layers, ScxGai-XN layers, or Scxlni.xN layers. The configuration, construction, fabrication, and other characteristics of the heterostructures may also vary from the examples described. For instance, the heterostructures may include any number of epitaxially grown layers of ferroelectric and non-ferroelectric nature. The disclosed methods and devices are not limited to Ill-nitride alloys including scandium. For instance, the Ill-nitride alloys may include additional or alternative group 111 B elements, such as yttrium (Y) and lanthanum (La).

[0027] Although described in connection with examples having the Ill-nitride alloy layer adjacent to (e.g., epitaxially grown on) Ill-nitride semiconductor layers, the disclosed methods and devices are not limited to heterostructures including Ill-nitride semiconductor layers as a template, base, or other component. For instance, a number of examples are described in which the Ill-nitride alloy layer is grown on or otherwise supported by a metal layer, such as a molybdenum or aluminum layer. Additional or alternative other types of materials may also be used in the heterostructures, including, for instance, other semiconductor materials.

[0028] Although the disclosed methods are described in connection with MBE growth procedures, additional or alternative non-sputtered epitaxial growth procedures may be used. For instance, metal-organic chemical vapor deposition (MOCVD), hydride vapor phase epitaxy (HVPE), atomic layer deposition (ALD), and atomic layer epitaxy (ALE) growth procedures may be used. Still other procedures may be used, including, for instance, pulsed laser deposition procedures.

[0029] Example ScAIN / n+-GaN heterostructures were grown by a Veeco GENxplor molecular beam epitaxy system. In these examples, a 200 nm-thick Si-doped n+-GaN (with an electron concentration of about 1019cm'3) was grown on commercial GaN / sapphire substrates, following which a 100 nm ScAIN film was grown under N-rich conditions. The Sc content in the ScAIN films was measured at about 20%. Further details on the epitaxial growth conditions, procedures, and related morphology of similar films are set forth in WO 2023 / 022768 ("Epitaxial Nitride Ferroelectronics"), International Application No. PCT / US23 / 13727 ("Epitaxial Nitride Ferroelectronic Devices" filed February 23, 2023), P. Wang, et al., "Fully epitaxial ferroelectric ScAIN grown by molecular beam epitaxy," Applied Physics Letters, vol. 118, p. 223504 (2021), and D. Wang et al., "An Epitaxial Ferroelectric ScAIN / GaN Heterostructure Memory," Advanced Electronic Materials, p. 2200005 (2022), the entire disclosures of which are hereby incorporated by reference.

[0030] Figure 1 , part a, shows a schematic cross-section of an example FeFET device 100 and SEM images of an actual device with an enlarged view 102 of the channel region, showing a channel length Lchof about 2 pm. Further details about the device 100 and the fabrication thereof are shown in the flow diagram of Figure 1 , part b.

[0031] The example device 100 of Figure 1 includes an ITO channel 104. The as- deposited ITO layer 104 (about 10 nm) is highly conductive with a bulk doping concentration of 3 x 1019cm'3and a Hall mobility of 18.4 cm2 / V s. To establish effective gate controllability, the thickness of the ITO layer 104 was reduced to about 5 nm by wet etching (about 3.7% HCI at an etch rate of 1 nm / s). The height profile obtained from AFM shown in Figure 1 , part c, confirms the thickness of the ITO channel 104 before and after etching to be about 10 nm and about 5 nm, respectively. Wet etching is performed in the last step to form a recessed channel configuration, in which thicker ITO underneath source / drain contacts 106, 108 helps reduce the contact resistance. TLM measurements were performed to extract the resistance (R) versus length characteristics of the 10 nm thick ITO channel 104 underneath the contacts 106, 108 as shown in Figure 1 , part d. A low contact resistance of0.8 Q-mm and a low contact resistivity of 5.07 x 10-6Q / cm2were extracted for the source / drain contacts 106, 108.

[0032] The ferroelectric response of a 100 nm ScAIN thin film 110 of the device 100 was evaluated by making example capacitor devices 200 as shown in the schematic of Figure 2, part a. The capacitor devices 200 were driven from a top electrode 202 on the ScAIN film 204, with a diameter of 40 pm. The clear butterfly shaped CV characteristics in Figure 2, part b, and the box shaped P-E loops with saturated polarization, as shown in Figure 2, part c, confirms the ferroelectricity in the epitaxially grown ScAIN film 204. From the voltage dependent P-E loops shown in Figure 2, part c, a clear saturation is observed in the negative branch of the P-E loop; however, the saturation in the positive branch is less clear, which indicates that it is difficult to completely compensate the contribution of leakage current in the ScAIN film 204.

[0033] Figure 2, part d, illustrates the remnant polarization recorded from electric field dependent PUND measurements for the capacitor devices 200. The saturated remnant polarization is extracted to be about 128 pC / cm2which is consistent with previously reported values in ScAIN films with a similar Sc content. Usually, the initial poling pulse in the PUND measurements compensates the non-switching current from resistive leakage and dielectric responses, thus verifying the presence of saturated remnant polarization in ferroelectrics. However, the slight increase observed in the remnant polarization indicates that it is yet difficult to completely compensate the contribution of leakage current in the ScAIN films 204.

[0034] The transfer characteristics (Id vs Vg) of the fabricated transistor devices 100 (see, e.g., Figure 1) were measured using a dual sweep gate bias. As can be seen in Figure 3, part a, the ITO channel conductivity cannot be effectively modulated by the ferroelectric layer for the as-deposited 10 nm ITO channel. However, after thinning down the channel to about 5 nm, the transfer characteristics of the FeFET device (shown as Vds = 0.1 V and 0.5 V in Figure 3a) show distinct ON and OFF states and large counterclockwise hysteresis.

[0035] The threshold voltage of the example devices was extracted using extrapolation in the linear region, which is a commonly used threshold voltage extraction method in field effect transistors. From the linear plot of transfer characteristics in Figure 3, part b, an increase in gate bias is seen, and the drain current starts increasing drastically around about 17 V (Vthi). This is associated with the enhanced accumulation of electrons in the ITO channel owing to the switching of polarization direction of the ScAIN gate dielectric, i.e., the polarization direction, initially facing away from the channel, reorients to face towards the channel. Next, as the gate bias is decreased from 40 V, the drain current drops sharplyaround -25 V (Vth2). This sudden drop can be associated with the pinch-off of the electrons in the channel due to large negative gate voltage. Further negative poling leads to ferroelectric switching and sets the device to the OFF state.

[0036] The resultant hysteresis loop gives rise to a large memory window, calculated as Vthi-Vth2, with the maximum being about 42 V. The origin of this hysteresis loop is the ferroelectric polarization switching in the ScAIN barrier and not the interface trapped charges. Often, ferroelectric FET devices suffer from a memory window collapse due to the depolarization field induced instability of the polarization states. However, the large coercive field and remnant polarization of the epitaxially grown ScAIN thin film facilitates a large window of operation, in which the ON and OFF states can be clearly distinguished. Also, the counterclockwise direction of the hysteresis loop rules out other trapping dominated phenomenon, which generally induces clockwise hysteresis behavior in an electron type transistor.

[0037] The maximum ON / OFF current ratio of the Fe-FETs was about 106 at a read-out voltage of Vg= -20 V, with the drain current (Id) in the OFF state being in the same range as that of the gate current (lg). This leakage current may originate due to the large area of the contacts and the global back gate architecture in the example devices.

[0038] The output characteristics (Id vs Vd) of the FeFET device shown in Figure 3, part c, exhibit linear behavior with a high current density of about 135 pA / pm at a drain bias of 3 V. Such a high ON current can be attributed to the polarization charges induced by the ferroelectric ScAIN film. As shown in Figure 3, part d, the ferroelectric polarization of the ScAIN film, when facing towards the channel (ON state), leads to enhancement of carriers in the channel (as compared to Hi obtained from Hall), whereas, polarization direction facing away from the channel (OFF state), leads to a depletion of charge carriers in the ITO channel. The calculated sheet carrier modulation in the ITO channel induced by the ferroelectric polarization in the ON state was about +1.1 x 1013cm-2and about -1 .3 x 1013cm2in the OFF state.

[0039] To analyze the memory behavior and reliability of the example FeFET devices, endurance and retention tests were performed. Figure 4, part a, shows the ON / OFF current ratio extracted from switching the device between ON and OFF states over 105cycles, with the highest ON / OFF ratio at about 106. Repeated cycling results in increased contribution from gate leakage, thus increasing the OFF-state current, whereas the ON current gradually degrades with cycling due to the formation of new defect centers. The ON / OFF current ratio was maintained at greater than 100 even after 105cycles, beyond which the devicesundergo breakdown owing to sudden increase in gate leakage. Also, the counterclockwise hysteresis loop is clearly observed even after 105cycles, which corroborates the robust ferroelectric properties of the epitaxially grown ScAIN film.

[0040] Figure 4, part b, shows the gradual shift in threshold voltage and the associated progression of the memory window with cycling. It is observed that Vth2 shifts towards higher positive voltages, while Vthiremains almost constant. Such a positive shift of threshold voltage may be attributed to charge injection due to generation of deep trap levels with cycling, while the unequal shift in the two branches may result from the asymmetric screening of the polarization charges. The highest memory window is found to be about 42 V at the first cycle. The collapse of the memory window is often attributed to the depolarization in the ferroelectric layer, however, the large remnant polarization in the ScAIN film preserves the memory window at about 20 V even after 105cycles.

[0041] The remnant ON and OFF current was obtained at different read-out time intervals as shown in Figure 4, part c. It is observed that the ON and OFF state currents do not show any appreciable degradation until 104seconds, while the two polarization states can be clearly distinguished for more than 105seconds. Given the high retention resistance of the ScAIN film, the degradation is likely due to trapping related processes instead of polarization degradation in the ScAIN film.

[0042] Figure 4, part d, presents a benchmarking of the normalized memory window versus ON / OFF current ratios. The triangular and circular points in blue represent state-of-the art FeFET devices recently reported in literature, whereas the star-shaped red point denotes an example of the disclosed devices. It should be noted that the FeFET indicated in Figure 4 as reference 11 (X. Liu et al., "Post-CMOS compatible aluminum scandium nitride / 2D channel ferroelectric field-effect-transistor memory," Nano Letters, vol. 21 , pp. 3753-3761 , 2021) used a 100 nm ferroelectric ScAIN as the gate dielectric in a back-gate configuration, however, the ScAIN was sputter deposited and M0S2 was used as the channel material. A saturated remanent polarization of 80 pC / cm2was observed in that ferroelectric ScAIN film. In contrast, the example of the disclosed device achieved a remnant polarization of about 128 pC / cm2from the electric field dependent PUND measurements with a pulse width of 0.1 ms and delay time of 1 second. The higher remnant polarization in the epitaxially grown ferroelectric ScAIN film results in a much lower depolarization field, because of which, the memory window can be sustained for a greater range of bias. Overall, it can be observed that the performance of the example ScAIN-based FeFET devices described herein clearly surpasses other devices in terms of the normalized memory window, while simultaneouslyachieving a high ON / OFF ratio. Such performance may be useful in, for instance, 1 - transistor NVM technologies.

[0043] The material quality as well as the interface between the ferroelectric layer and the channel layer may be optimized for better endurance and retention characteristics.Furthermore, thickness scaling of the ScAIN film may be used to epitaxially grow ScAIN films down to 5 nm. Further details are set forth in D. Wang et al., “Thickness scaling down to 5 nm of ferroelectric ScAIN on CMOS compatible molybdenum grown by molecular beam epitaxy", Applied Physics Letters, vol. 122, p. 052101 (2023), the entire disclosure of which is hereby incorporated by reference. Scaling down the thickness of the ferroelectric ScAIN may result in a decreased operational bias, and hence comparatively lower read-out voltages. Therefore, FeFET devices having a scaled down ferroelectric ScAIN layer as the gate dielectric layer may be integrated with channel materials such as ITO to realize devices useful for next generation electronics, going beyond the memory-logic interconnect bottlenecks implemented by dimensional scaling and von-Neumann architectures. Further details regarding an example device having a scaled-down ferroelectric ScAIN layer are set forth in connection with Figure 7 below.

[0044] The examples disclosed herein demonstrate high-performance FeFET devices with an ITO channel and ScAIN as the ferroelectric gate dielectric material. The devices exhibited a large programmable window of about 0.42 V / nm with an lOn / lOff ratio of about 106. The ferroelectric ScAIN film is robust enough to withstand repeated cycling without considerable degradation in the memory window while achieving an ON / OFF current ratio of about 100 even after 105cycles. Moreover, the ferroelectric polarization showed excellent retention characteristics as the two states can be distinctly read-out even after 105seconds. The example FeFET devices described herein provide are useful in a wide variety of computing paradigms.

[0045] Figure 5 shows a FeFET device 500 in accordance with one example. The FeFET device 500 includes a substrate 502 and a heterostructure 504 supported by the substrate 502. The substrate 502 may be composed of, or otherwise include, sapphire. Alternative or additional materials may be used, including, for instance, silicon, bulk GaN, bulk AIN, or other semiconductor material. Still other materials may be used, including, for instance, silicon carbide.

[0046] The heterostructure 504 includes a gate dielectric layer 506 composed of, or otherwise including, a Ill-nitride alloy. As described herein, the Ill-nitride alloy is ferroelectric. In some cases, the gate dielectric layer 506 is monocrystalline. The Ill-nitride alloy includesa Group 11 IB element, such as scandium. In some cases, the Ill-nitride alloy is ScAIN. Other materials may be used as described herein.

[0047] The heterostructure 504 further includes a channel layer 508 adjacent to (e.g., on top of) the gate dielectric layer 506. In this example, the channel layer 508 is supported by the gate dielectric layer 506. Accordingly, the layers of the heterostructure 504 may be arranged in a back-gate configuration or architecture. The arrangement of the layers may vary in other cases. For example, the channel may reside on the lateral surfaces of the nanowire gate dielectric (e.g., in a FIN structure), or the channel may be surrounded by a gate dielectric layer. In some cases, the Ill-nitride alloy of the gate dielectric layer 506 is in contact with the channel layer 508 as shown.

[0048] In some cases, the channel layer 508 is transparent at an operational wavelength of the device 500. Alternatively or additionally, the channel layer 508 is composed of, or otherwise includes, an oxide material, such as ITO, ZnO, InO, and GaO.

[0049] In the example of Figure 5, the heterostructure 504 further includes a buried or back gate layer 510 adjacent the gate dielectric layer 506. In some cases, the buried gate layer 510 is composed of, or otherwise includes, a Ill-nitride semiconductor material, such as n- type doped GaN. Other materials may be used as described herein. The Ill-nitride alloy of the gate dielectric layer 506 may be in contact with the buried gate layer 510 as shown.

[0050] The FeFET device 500 further includes a source contact 512 and a drain contact 514 spaced apart from one another to define a channel of the channel layer 508. In this example, the source and drain contacts 512, 514 overlap the channel layer 508. The channel layer 508 may be thinner in the channel region as shown to establish a recessed channel configuration.

[0051] The gate dielectric layer 506 has a polarization range such that a normalized memory window of the device 500 exceeds about 0.4 Volts per nanometer of gate dielectric layer thickness.

[0052] Figure 6 depicts a method 600 of fabricating a device having a ferroelectric gate dielectric layer in accordance with one example. The device may be a FeFET device, such as the FeFET device 500 of Figure 5, or another FeFET device.

[0053] The method 600 may begin with an act 602 in which a substrate is prepared and / or otherwise provided. In some cases, the act 602 includes providing a sapphire substrate in an act 604. Alternative or additional materials may be used, including, for instance, silicon, bulk GaN, bulk AIN, or other semiconductor material. Still other materials may be used,including, for instance, silicon carbide. The substrate may be cleaned in an act 606. In some cases, a native or other oxide layer may be removed from a substrate surface in an act 608. In the example of Figure 6 (e.g., sapphire examples), the act 602 may include implementing a nitridation procedure in an act 609. Additional or alternative processing may be implemented in other cases, including, for instance, doping or deposition procedures. The substrate thus may or may not have a uniform composition. The substrate may be a uniform or composite structure.

[0054] In an act 610, one or more growth templates, buffer, or other layers are formed. The layer(s) are thus formed on, or otherwise supported by, the substrate. The layer(s) may or may not be in contact with the substrate. In some cases, the layer(s) are composed of, or otherwise include, a semiconductor material. For instance, the act 610 may include an act 612 in which a semiconductor layer is formed. For example, a Ill-nitride layer, such as a GaN layer, may be grown or otherwise formed on the substrate. Other compound or other semiconductor materials may be used, including, for instance, AIGaN. The semiconductor layer(s) may be N-polar or metal-polar. The semiconductor layer(s) may form a part of the heterostructure underlying the ferroelectric layer to be grown. The semiconductor layer be undoped or doped (e.g., Si-doped). The act 612 may thus be implemented before (e.g., in preparation for) implementing an epitaxial growth procedure in which a wurtzite structure is formed. The wurtzite structure may thus be formed on the semiconductor layer. The semiconductor layer may be configured or used as a growth template for the wurtzite structure and / or other elements of the heterostructure. In some cases, the act 612 may include growing the semiconductor layer in an epitaxial growth chamber in which the epitaxial growth procedure for the wurtzite structure is implemented. As a result, the substrate may remain within, e.g., is not removed from, the epitaxial growth chamber between forming the semiconductor layer and implementing the epitaxial growth procedure for growing the wurtzite structure.

[0055] Alternatively or additionally, the act 610 includes an act 614 in which one or more metal or other conductive layers are deposited and patterned. For example, an aluminum layer may be deposited on a silicon substrate in preparation for the epitaxial growth of the wurtzite structure.

[0056] The method 600 may include an act 616 in which one or more electrodes or contacts or other layers are formed. The layer(s) may form a part of the heterostructure underlying the ferroelectric layer to be grown. Examples of the underlying layer(s) include a gate electrode or layer of the heterostructure. The nature of the underlying layer(s) may vary with the device being fabricated. The Si-doped layer may or may not be grown on top of thetemplate or buffer layer formed in the act 610. In the example of Figure 6, the act 616 includes growing a silicon-doped GaN layer in an act 618. The Si-doped GaN layer may be N-polar or metal-polar. Other materials may be used. For instance, the underlying layer(s) may be composed of, or otherwise include, AIGaN, I n AIN , InGaN, or InAIGaN. Still other materials may be used. For instance, a channel layer may be composed of, or otherwise include, other types of semiconductors, e.g., Ga2Os, diamond, Si, SiGe, GaAs, InGaAs, or InP, in addition to one or more of the above-referenced Ill-nitride alloys. The Si-doped GaN layer may act as a gate electrode of a device, such as a memory device.

[0057] Still other materials may be formed and configured as the gate layer. For example, in an act 620, a metal layer may be deposited or otherwise formed. The metal layer may be composed of, or otherwise include, a metal such as molybdenum. Further details regarding the incorporation and use of a metal layer in a heterostructure having a ferroelectric layer are set forth in P. Wang et al., " Ferroelectric Nitride Heterostructures on CMOS Compatible Molybdenum for Synaptic Memristors," ACS Appl. Mater. Interfaces, 15, 14, 18022-18031 (2023). The act 620 may include one or more procedures for preparing the metal layer for epitaxial growth of a ferroelectric layer, such as oxide removal via, e.g., an anneal procedure in vacuum.

[0058] In an act 622, a non-sputtered epitaxial growth procedure is implemented at a growth temperature to form a wurtzite structure supported by the substrate. As described herein, the wurtzite structure is composed of, or otherwise includes, an alloy of a Ill-nitride material. For instance, the Ill-nitride material may be AIN. Additional or alternative Ill-nitride materials may be used, including, for instance, gallium nitride (GaN), indium nitride (InN), and their alloys. As also described herein, the epitaxial growth procedure is configured to incorporate scandium and / or another group 111 B element into the alloy of the Ill-nitride material. The alloy may thus be ScxAli.xN, for example. In some cases, the act 622 includes an act 624 in which an MBE procedure is implemented. In other cases, an MOCVD or other non-sputtered epitaxial growth procedure is implemented in an act 626.

[0059] The act 622 may constitute a continuation, or part of a sequence, of growth procedures. The growth procedures may be implemented in a common, or same, growth chamber. The act 622 may thus include an act 628 in which epitaxial growth is continued in the same chamber in which one or more other layers of the heterostructure were grown. For instance, one or more of the growth template and the underlying semiconductor layer(s) formed in the acts 610 and 616 may be formed in the same chamber as the ferroelectric layer. Sequential layers of the heterostructure may thus be grown without exposure to the ambient. The quality of the interface between the layers may accordingly be improved.

[0060] The growth temperature may be at a level such that the wurtzite structure exhibits a breakdown field strength greater than a ferroelectric coercive field strength of the wurtzite structure. Ferroelectric switching and other behavior may thus be achieved.

[0061] The growth temperature is at a level lower than what would be expected given the Ill-nitride material. In some examples, the growth temperature level is significantly less than the temperature at which the Ill-nitride material would typically be grown. For instance, the growth temperature level may be such that attempts to grow a structure composed of the Ill- nitride material (i.e., without scandium) at the growth temperature level would not be worthwhile. The resulting structure would be of such poor quality (e.g., possess far too many defects) to be useful. Growth of a single crystal of the scandium-including alloy (e.g., a monocrystalline layer of the alloy) at the growth temperature level may nonetheless be achieved. For example, in some cases, a ScxAli.xN alloy may be epitaxially grown at a growth temperature of about 650 degrees Celsius or about 750 degrees Celsius despite that the corresponding (scandium-free) Ill-nitride material, AIN, is conventionally grown at much higher temperatures, e.g., about 1000 degrees Celsius. Conversely, attempts to grow AIN at about 650 degrees Celsius, about 750 degrees Celsius, or lower than about 650 or 750 degrees Celsius, would result in structures of such poor quality so as to be useless. In contrast, the epitaxially grown ScxAli.xN layer grown at such low temperatures is unexpectedly monocrystalline and of high quality.

[0062] Growth of the ScxAli.xN layer at the conventional AIN growth temperature (and other temperatures above the upper bound) unexpectedly results in the formation of dislocations and / or other leakage paths in the ScxAli.xN layer. With the leakage paths, the ScxAli.xN layer has a breakdown field strength level too low (e.g., below the ferroelectric coercive field strength level). The layer accordingly does not exhibit ferroelectric behavior.

[0063] In some cases, the growth temperature may be about 650 degrees Celsius or less or about 750 degrees Celsius or less. The growth temperature may correspond with the temperature measured at a thermocouple in the growth chamber. The growth temperature at the epitaxial surface may be slightly different. The growth temperature is accordingly approximated via the temperature measurement at the thermocouple.

[0064] The upper bound of the growth temperature range may vary in accordance with the alloy and / or the epitaxial growth technique. For instance, in other cases, the upper bound on the growth temperature may be higher, such as about 680 degrees Celsius, or about 690 degrees Celsius. In still other cases, the upper bound may be lower, including, for instance, about 600 degrees Celsius or about 620 degrees Celsius.

[0065] At each level within the above-described ranges of suitable growth temperatures, the resulting wurtzite structure is monocrystalline. The resulting wurtzite structure is monocrystalline to a degree not realizable via, for instance, sputtering-based procedures for forming ScxAli.xN layers. Such procedures are only capable of producing structures with x- ray diffraction rocking curve line widths on the order of a few degrees at best. In contrast, the structures grown by the disclosed methods exhibit x-ray diffraction rocking curve line widths on the order of a few hundred arc-seconds or less, well over an order of magnitude less. In this manner, leakage current paths are minimized or otherwise sufficiently reduced so that the resulting wurtzite structure has a suitably high breakdown field strength level, e.g., sufficiently greater than the ferroelectric coercive field strength.

[0066] The above-noted differences in crystal quality evidenced via x-ray diffraction rocking curve line widths may also be used to distinguish between monocrystalline and polycrystalline structures. As used herein, the term "polycrystalline" refers to structures having x-ray diffraction rocking curve line widths on the order of a few degrees or higher. As used herein, the term "monocrystalline" refers to structures having x-ray diffraction rocking curve line widths at least one order of magnitude lower than the order of a few degrees.

[0067] Comparing the wurtzite structures of the layers grown by MBE or other nonsputtered techniques (e.g., MOCVD or HVPE) with sputtering deposition techniques, the microstructure of the former techniques is more uniform with highly ordered stacking sequence of atoms. In sputter deposited layers, domains with cubic phase or domains with in-plane mis-orientation are readily observed. The existence of these mis-aligned domains suppresses the complete switching of polarization, and further results in the fast loss of polarization during fatigue testing. Regarding phase purity, the highly crystallographic orientation of layers grown by MBE or other non-sputtered techniques exhibits more repeatable ferroelectric switching, which is useful in a number of device applications.

[0068] The wurtzite structure of the ferroelectric layer may be nitrogen-polar (N-polar) or metal-polar. The polarity of an underlying layer formed in the act 610 and / or the act 616 may be used to establish the polarity of the ferroelectric layer formed in the act 622. The polarity of the underlying layer may, in turn, be established by a characteristic of the substrate. The polarity may continue across the interface between the underlying layer and the ferroelectric layer. Either N- or metal-polarity may thus persist as the composition changes from the underlying layer to the ferroelectric layer.

[0069] The wurtzite structure may then be annealed in an act 632. The annealing may be implemented at a temperature greater than the growth temperature. In some cases, theannealing temperature falls in a range from about 700 Celsius to about 1500 degrees Celsius. Examples of films prepared with such annealing exhibited stable polarization switching with further reduced leakage current relative to non-annealed films. Film or device uniformity was also improved via the annealing, thereby further improving the polarization switching behavior of the ferroelectric Sc-lll-N alloys. The underlying mechanism for the improved performance and uniformity with annealing is attributed to the reduced threading dislocation density and defect density, which usually act as electric leakage paths. Such usefulness of the post-growth annealing is realized despite past concerns that high processing temperatures can lead to a loss of ferroelectricity.

[0070] Such post-growth high-temperature annealing of ScxAli.xN may be performed in-situ in the same growth chamber (e.g., the same MBE chamber) in an act 634. In other cases, the annealing is performed ex-situ in a chamber directed to annealing procedures.

[0071] The annealing process may be implemented under high vacuum in an act 636 (e.g., in-situ in the growth chamber). In other cases, the annealing may be implemented either with nitrogen plasma radiation or under nitrogen gas flow in an act 638.

[0072] The above-described annealing procedure may be implemented in connection with films grown under any of the above-described growth conditions. For instance, the annealing procedure may be implemented after growth under slightly to moderately N-rich conditions at a growth temperature at or below about 650 degrees Celsius, or at or below about 750 degrees Celsius. The annealing procedure may also be implemented after growth under unbalanced flux ratios (e.g., N-rich or extreme N-rich conditions) at growth temperatures above about 650 degrees Celsius or above about 750 degrees Celsius.

[0073] The method 600 include one or more acts directed to forming additional features of the device. In the example of Figure 6, the method 600 includes an act 640 in which a device isolation layer, such as a field oxide layer, is deposited and patterned. The device isolation layer may be composed of, or otherwise include, SiO2. The patterning may include reactive ion etching (RIE) and / or other procedures. The patterning may be directed to forming openings in the device isolation layer for a gate contact and a channel of the device.

[0074] In an act 642, a gate contact of the device is formed. A deposition procedure may be used. In some cases, the gate contact is composed of, or otherwise includes, one or more metal layers, such as titanium and gold.

[0075] The method 600 includes an act 644 in which a channel layer is formed. A sputtering and / or other deposition procedure may be used. The channel layer may becomposed of, or otherwise include, ITO in some cases. The composition of the channel layer may vary as described herein.

[0076] The act 644 may be implemented in a manner that minimizes or otherwise reduces the surface oxidation of the ferroelectric gate dielectric layer. For instance, the heterostructure may be transferred from the growth chamber in a manner that minimizes or reduces the amount of time during which the ferroelectric gate dielectric layer is exposed to the ambient. In some cases, the exposure time is on the order of minutes or less than one minute. In these and other cases, the surface oxidation may be limited to about 1 nm or less. Alternatively or additionally, the surface may be covered by one or more layers of materials, e.g., GaN, to minimize surface oxidation.

[0077] In the example of Figure 6, source and drain contacts are formed in an act 646. The source and drain contacts may be composed of, or otherwise include, nickel, but alternative or additional materials may be used. The formation of the contacts may include a deposition procedure and a patterning procedure.

[0078] Following the formation of the source and drain contacts, the channel layer may be thinned in an act 648. In some cases, the channel layer may be etched (e.g., wet etched). For example, an HCI-based etch procedure may be implemented.

[0079] The method 600 may include one or more additional acts. For example, one or more acts may be implemented to form other conductive layers or structures.

[0080] The order of the acts of the method 600 may differ from the example shown in Figure 6. For example, the act in which the gate contact is formed may be implemented at a different point in the fabrication sequence.

[0081] A number of different types of devices may be fabricated by the method 600 of Figure 6, including, for instance, various types of nonvolatile memory devices (e.g., FeFET, memristors, and FeSFET devices), various types of reconfigurable electronic and other devices, and various types of photodetection, photovoltaic and optoelectronic devices (e.g., self-driven photodetector and solar cell devices).

[0082] Figure 7 depicts a FeFET device having a thinner (scaled down) ferroelectric gate barrier in accordance with one example. While the 100 nm ScAIN FeFET example devices described above exhibit useful device characteristics, the operational voltage is significantly high, owing to the large coercive field of the 100 nm ScAIN ferroelectric gate barrier. That operational voltage may present an operational challenge for memory devices that operate at relatively low input voltages. The thickness of the ferroelectric gate barrier may be scaleddown to address this challenge. In one example, a ScAIN / ITO FeFET device having a similar back-gate configuration to the examples described above has a recessed 5 nm ITO channel and a ferroelectric ScAIN barrier scaled down to about 18 nm (rather than, e.g., 100 nm). Clear butterfly shaped CV characteristics shown in Figure 7, part a, confirmed the ferroelectricity in the epitaxially grown 18 nm ScAIN thin films. The transfer characteristics of the ScAIN FeFET device shown in Figure 7, part b, exhibit clear channel modulation and a large counterclockwise hysteresis achieved by the ferroelectric barrier. Figure 7, part c, shows the extraction of threshold voltages Vn = - 3.8 V and Vt2= -0.6 V and the associated memory window, M.W. = 3.2 V for the example device.

[0083] Described herein are examples of ferroelectric field effect transistor (FeFET) devices having a back-gate configuration. The devices harness the polarization switching characteristics of epitaxially grown ferroelectric Scandium Aluminum Nitride (ScAIN) to control the conductance of an ITO (Indium-Tin Oxide) channel. The ferroelectric transistors exhibit a large memory window of about 0.42 V / nm. A high ON current along with a large ON / OFF current ratio of about 106is observed owing to ferroelectric polarization induced carrier modulation in the ITO channel. The distinct ON / OFF states and the memory window were preserved even after 105cycles while simultaneously showing retention time greater than 105seconds. The integration of a nitride ferroelectric material (e.g., ScAIN) with a promising channel material (ITO), as demonstrated in the example devices, allows high- performance FeFET devices to be realized for in-memory computing, edge intelligent applications, and a variety of other applications.

[0084] The term "about" is used herein in a manner to include deviations from a specified value that would be understood by one of ordinary skill in the art to effectively be the same as the specified value due to, for instance, the absence of appreciable, detectable, or otherwise effective difference in operation, outcome, characteristic, or other aspect of the disclosed methods and devices.

[0085] The present disclosure has been described with reference to specific examples that are intended to be illustrative only and not to be limiting of the disclosure. Changes, additions and / or deletions may be made to the examples without departing from the spirit and scope of the disclosure.

[0086] The foregoing description is given for clearness of understanding only, and no unnecessary limitations should be understood therefrom.

Claims

What is Claimed is:

1. A device comprising: a substrate; and a heterostructure supported by the substrate, the heterostructure comprising: a gate dielectric layer comprising a Ill-nitride alloy, the Ill-nitride alloy comprising a Group 111 B element; and a channel layer adjacent to the gate dielectric layer; wherein: the channel layer is transparent at an operational wavelength of the device; and the Ill-nitride alloy is ferroelectric.

2. The device of claim 1 , wherein the channel layer comprises an oxide material.

3. The device of claim 1 , wherein the gate dielectric layer is monocrystalline.

4. The device of claim 1 , wherein the heterostructure further comprises a buried gate layer in contact with the Ill-nitride alloy of the gate dielectric layer.

5. The device of claim 4, wherein the buried gate layer comprises a Ill-nitride semiconductor material.

6. The device of claim 4, wherein the Ill-nitride alloy of the gate dielectric layer is in contact with the buried gate layer.

7. The device of claim 1 , further comprising a source contact and a drain contact, wherein: the source and drain contacts are spaced apart from one another to define a channel of the channel layer; and the source and drain contacts overlap the channel layer.

8. The device of claim 7, wherein the channel layer is thinner in the channel and thicker underneath the source and drain contacts to reduce contact resistance.

9. The device of claim 1 , wherein the heterostructure is configured such that a normalized memory window of the device exceeds about 0.4 Volts per nanometer of gate dielectric layer thickness.

10. The device of claim 1 , wherein the gate dielectric layer has a polarization range greater than 50 pC / cm2.

11. The device of claim 1 , wherein the 11 l-nitride alloy of the gate dielectric layer is in contact with the channel layer.

12. A device comprising: a substrate; and a heterostructure supported by the substrate, the heterostructure comprising: a gate dielectric layer comprising a Ill-nitride alloy, the Ill-nitride alloy comprising a Group 111 B element; and a channel layer adjacent to the gate dielectric layer; wherein: the channel layer comprises an oxide material; and the Ill-nitride alloy is ferroelectric.

13. The device of claim 12, wherein the gate dielectric layer is monocrystalline.

14. The device of claim 12, wherein the heterostructure further comprises a buried gate layer in contact with the Ill-nitride alloy of the gate dielectric layer.

15. The device of claim 14, wherein the buried gate layer comprises a Ill-nitride semiconductor material.

16. A device comprising: a substrate; and a heterostructure comprising: a gate layer supported by the substrate; a gate dielectric layer supported by the gate layer, the gate dielectric layer comprising a Ill-nitride alloy, the Ill-nitride alloy comprising a Group I IIB element; and a channel layer supported by the gate dielectric layer; wherein the gate dielectric layer is monocrystalline and ferroelectric.

17. The device of claim 16, wherein the channel layer is transparent at an operational wavelength of the device.

18. The device of claim 17, wherein: the heterostructure further comprises a buried gate layer in contact with the Ill-nitridealloy of the gate dielectric layer; and the buried gate layer comprises a Ill-nitride semiconductor material.

19. A method of fabricating a device, the method comprising: providing a gate layer on a substrate; implementing a non-sputtered, epitaxial growth procedure to form a gate dielectric layer supported by the gate layer, the gate dielectric layer comprising a Ill-nitride alloy, the Ill-nitride alloy comprising a Group II IB element; depositing a channel layer across the gate dielectric layer, the channel layer being transparent at an operational wavelength of the device; and forming source / drain contacts that overlap the channel layer; wherein the non-sputtered, epitaxial growth procedure is configured such that the gate dielectric layer is monocrystalline and ferroelectric.

20. The method of claim 19, further comprising etching the channel layer in between the source / drain contacts.

21. The method of claim 19, wherein ambient exposure of the gate dielectric layer prior to depositing the channel layer is controlled to limit surface oxidation to about 1 nm or less.

Citation Information

Patent Citations

  • Post CMOS Compatible Ferroelectric Field Effect Transistor With AIScN Dielectric And 2D Material Channel